Method for patterned electrodeposition coating of polyimide on cryogenic cooling piping
A patterned polyimide electrodeposition method for cryogenic pipes enhances cooling performance by increasing the Leidenfrost point and reducing thermal shrinkage, addressing inefficiencies in existing coating methods.
Patent Information
- Application Number
- PCT/KR2025/095458
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-13
- Filing Date
- 2025-07-16
- Publication Date
- 2026-11-19
AI Technical Summary
Existing methods for coating cryogenic transfer pipes with polymers are inefficient and prone to damage from thermal shrinkage, and they do not effectively enhance cooling performance due to limitations in applying uniform coatings on long, thin pipes.
A method for electrodepositing a patterned polyimide coating inside cryogenic cooling pipes using a masking sheet and polyimide precursor solution, followed by electrodeposition and heat treatment to form a polyimide layer, which reduces thermal shrinkage and enhances cooling performance.
The method improves cooling rate by increasing the Leidenfrost point, reduces refrigerant consumption, and minimizes damage from thermal shrinkage, enabling rapid cooling of cryogenic equipment.
Smart Images

Figure KR2025095458_19112026_PF_FP_ABST
Abstract
Description
Polyimide pattern electrodeposition coating method for cryogenic cooling piping
[0001] The present invention relates to a method for electrodepositing a polyimide pattern for cryogenic cooling pipes, and more specifically, to a technology for improving cooling speed and efficiency by electrodepositing polyimide in a patterned form inside a cryogenic cooling pipe.
[0002]
[0003] Initial cooling using cryogenic fluids is an essential technology in various scientific and industrial fields. Systems requiring cryogenic environments utilize cryogenic fluids such as liquid helium, liquid nitrogen, and liquid hydrogen to lower the temperature from room temperature to cryogenic temperatures at a sufficient rate.
[0004] In the aerospace field, liquid oxygen and liquid hydrogen are utilized as oxidizers and propellants, respectively, due to their high energy density and efficient combustion characteristics. For these cryogenic fuels, cryogenic storage tanks with vacuum insulation structures to minimize evaporation during storage, as well as cryogenic transfer piping for stable supply, are essential. Cryogenic infrared sensors are used in space exploration and astronomical research. Infrared sensors require maintaining a temperature lower than the target being measured to minimize thermal noise and accurately detect faint signals from space; therefore, maintaining a cryogenic environment of several Kelvin is necessary. These cryogenic infrared sensors are applied to observation instruments such as the James Webb Space Telescope.
[0005] Cryogenic fluids are essential for cooling superconducting devices. Superconductors possess the characteristic of having zero electromotive force below their critical temperature, and a cryogenic environment is required to realize this. Liquid helium and liquid nitrogen are primarily used for initial cooling, which rapidly lowers the temperature of superconductors below their critical point. In the medical field, MRI systems use low-temperature superconductors to generate strong magnetic fields; to achieve this, liquid helium is used to lower the temperature to approximately 4.2 K, thereby maintaining the superconducting state. In the power sector, there are superconducting power cables capable of high-efficiency, high-capacity transmission. To transmit power while maintaining the superconducting phenomenon, they are operated within supercooled liquid nitrogen circulating in a closed circuit.
[0006] Furthermore, as global interest in climate change and environmental pollution issues has recently increased, the demand for eco-friendly transportation equipment is surging. With the emphasis on the need to address climate change and reduce carbon emissions, high-efficiency electric propulsion aircraft combining liquid hydrogen and superconducting motors, as well as LNG and liquid hydrogen vessels, are attracting attention, rather than traditional internal combustion engines that emit large amounts of greenhouse gases such as carbon dioxide. Once a means of transportation operates in an ultra-low temperature environment, the temperature rises to ambient temperature when operation is stopped, requiring re-cooling to resume operation.
[0007] To supply cryogenic fluids to such applications, cryogenic transfer piping with a vacuum insulation structure is required. If the insulation performance of the transfer piping is insufficient and the fluid is not sufficiently cooled to its saturation temperature, pressure rises due to evaporation during supply, hindering the stable supply of refrigerant to the cryogenic application equipment.
[0008] If the time required for initial cooling from ambient temperature to cryogenic temperatures is prolonged, heat loss due to continuous external heat intrusion and the consumption of cryogenic refrigerant increase. Rapid initial cooling allows the application device to reach the target temperature quickly, thereby reducing overall operating time, minimizing heat loss, and enabling efficient operation by shortening the work cycles that require repeated cooling and warm-up cycles. In particular, for expensive refrigerants such as liquid helium and liquid neon, it is important to reduce refrigerant consumption, and for liquid hydrogen and liquid oxygen, which pose an explosion risk, the amount released into the atmosphere during initial cooling can be reduced.
[0009] In common fluids such as water, surface roughness is increased to reduce the contact angle at the interface, thereby improving boiling heat transfer performance. However, since cryogenic fluids such as liquid nitrogen have very low contact angles, the change in heat transfer performance due to surface roughness is negligible.
[0010] One method to improve the initial cooling rate is to thinly coat metal surfaces with polymers having low thermal conductivity. Existing studies utilize dip coating or spray coating using Teflon, but these processes are difficult to apply to actual applications such as transfer pipes due to length limitations. Furthermore, there is a complete lack of research on pattern coatings, which can enhance cooling performance while reducing the risk of damage caused by thermal shrinkage, as they are difficult to apply to thin, long pipes. Therefore, it is necessary to identify a coating process capable of coating polymers onto thin, long pipes and to analyze the cooling performance resulting from the pattern coating within the pipes under flow boiling conditions.
[0011]
[0012] The present invention aims to provide a method for electrodepositing polyimide in a patterned form inside a pipe for cryogenic cooling.
[0013] The technical problems that the present invention aims to solve are not limited to those mentioned above, and other unmentioned technical problems will be clearly understood by those skilled in the art from the description below.
[0014]
[0015] To achieve the above objective, the present invention provides a polyimide pattern electrodeposition coating method for cryogenic cooling pipes, characterized by comprising: a step of cutting a masking sheet into a pattern shape; a step of attaching the cut pattern masking sheet to the inside of a pipe; a step of installing the pipe with the attached pattern masking sheet into a pipe coating device; a step of filling the inside of the pipe with the attached pattern masking sheet with a polyimide precursor solution and applying power to perform electrodeposition coating to form a polyimide coating layer; and a step of removing the masking sheet attached to the inside of the pipe with the formed polyimide coating layer.
[0016] The material of the masking sheet may be one or more selected from the group consisting of Teflon, polyimide, and silicone.
[0017] The pattern shape of the pattern masking sheet above is any one of a square, a circle, a triangle, a hexagon, and an irregular shape, and the pattern shape may be arranged continuously or discontinuously.
[0018] The coating ratio of the above polyimide may be 20 to 80% relative to the internal area of the pipe.
[0019] The coating thickness of the above polyimide may be 3 to 100 μm.
[0020] The step of forming a polyimide coating layer by filling the inside of the above pipe with a polyimide precursor solution and applying power to perform electrodeposition coating can be performed by forming a polyimide precursor coating layer through electrodeposition coating and then heat-treating at 200 to 300 ℃ to form a polyimide coating layer through imidization.
[0021] In addition, the present invention provides a cryogenic cooling pipe coated with a polyimide pattern by the above method.
[0022] In addition, the present invention provides a superconductor cooling device comprising the above-mentioned cryogenic cooling pipe.
[0023]
[0024] By means of the solution to the above problem, the present invention can provide a method for polyimide pattern electrodeposition coating for cryogenic cooling pipes.
[0025] In addition, the polyimide pattern electrodeposition coating method for cryogenic cooling pipes according to the present invention can improve the cooling rate by coating polyimide on a metal surface to increase the Leidenfrost point, thereby rapidly transitioning film boiling to transient boiling.
[0026] In addition, the polyimide pattern electrodeposition coating method for cryogenic cooling pipes according to the present invention can rapidly cool cryogenic application equipment from room temperature to operating temperature, thereby reducing the time required for system operation.
[0027] In addition, the polyimide pattern electrodeposition coating method for cryogenic cooling pipes according to the present invention has an economic advantage in that the consumption of cryogenic refrigerant required to cool cryogenic application equipment to the operating temperature is reduced.
[0028] In addition, the polyimide pattern electrodeposition coating method for cryogenic cooling pipes according to the present invention is advantageous against damage caused by the difference in thermal shrinkage between the metal and the polyimide during the cooling process, as the polyimide coating on the metal surface is discontinuous.
[0029] The effects of the present invention are not limited to those mentioned above, and other unmentioned effects will be clearly understood by those skilled in the art from the description in the claims.
[0030]
[0031] Figure 1 shows a schematic diagram of an electrodeposition coating process for polyimide coating.
[0032] Figure 2 shows a schematic diagram of the pattern coating process on the inner surface of a pipe.
[0033] Figure 3 shows the shape of a masking sheet according to the coating ratio. (a) 25%, (b) 44%, (c) 69%
[0034] Figure 4 shows the pattern coating arrangement on the inner surface of the pipe for each coating ratio. (a) 25%, (b) 44%, (c) 69%
[0035] Figure 5 shows the results of scanning electron microscope (SEM) measurements of electrodeposition coating layers coated with thicknesses of (a) 5.4 μm, (b) 27.3 μm, and (c) 49.1 μm.
[0036] Figure 6 shows (a) a schematic diagram of the flow boiling experiment apparatus setup and (b) a schematic diagram of the test section used for the cooling experiment.
[0037] Figure 7 shows the results of the cooling performance evaluation of the bare piping at various mass flow rates. (a) 3.7 g / s, (b) 7.5 g / s, (c) 11.2 g / s
[0038] Figure 8 shows the temperature change according to coating thickness of 100% coated piping at various mass flow rates. (a) 3.7 g / s, (b) 7.5 g / s, (c) 11.2 g / s
[0039] Figure 9 shows the temperature change according to the coating ratio of a 49.1 μm coated pipe at various mass flow rates. (a) 3.7 g / s, (b) 7.5 g / s, and (c) 11.2 g / s
[0040] Figure 10 shows the reduction in cooling time of pattern-coated tubing compared to bare tubing at various mass flow rates. (a) 3.7 g / s, (b) 7.5 g / s, and (c) 11.2 g / s
[0041] Figure 11 shows (a) the change in heat flux according to coating thickness of a 100% coated pipe and (b) the change in heat flux according to coating ratio of a 49.1 μm coated pipe at a mass flow rate of 7.5 g / s.
[0042] Figure 12 shows (a) boiling curves according to coating thickness of a 100% coated pipe and (b) boiling curves according to coating ratio of a 49.1 μm coated pipe at a mass flow rate of 7.5 g / s.
[0043] Figure 13 schematically illustrates the bubble dynamics in a superheated state in (a) a bare pipe and (b) a pattern-coated pipe.
[0044]
[0045] The terms used in this invention have been selected based on currently widely used general terms, taking into account their functions within the invention; however, these terms may vary depending on the intent of those skilled in the art, case law, the emergence of new technologies, etc. Additionally, in specific cases, terms have been arbitrarily selected by the applicant, and in such cases, their meanings will be described in detail in the relevant description of the invention. Therefore, the terms used in this invention should be defined not merely by their names, but based on their meanings and the overall content of the invention.
[0046] Unless otherwise defined, all terms used herein, including technical or scientific terms, have the same meaning as generally understood by those skilled in the art to which the present invention pertains. Terms such as those defined in commonly used dictionaries should be interpreted as having a meaning consistent with their meaning in the context of the relevant technology, and should not be interpreted in an ideal or overly formal sense unless explicitly defined in this application.
[0047] When a part of a specification is described as “comprising” a certain component, this means that, unless specifically stated otherwise, it does not exclude other components but may include additional components.
[0048] Embodiments of the present invention are described below with reference to the attached drawings so that those skilled in the art can easily implement them. However, the present invention may be embodied in various different forms and is not limited to the embodiments described herein.
[0049]
[0050] The present invention will be described in detail below.
[0051]
[0052] The present invention provides a polyimide pattern electrodeposition coating method for cryogenic cooling pipes, characterized by comprising: a step of cutting a masking sheet into a pattern shape; a step of attaching the cut pattern masking sheet to the inside of a pipe; a step of installing the pipe with the attached pattern masking sheet into a pipe coating device; a step of filling the inside of the pipe with the attached pattern masking sheet with a polyimide precursor solution and applying power to perform electrodeposition coating to form a polyimide coating layer; and a step of removing the masking sheet attached to the inside of the pipe with the formed polyimide coating layer.
[0053] The reason polymer-coated metal specimens exhibit rapid cooling completion times during cooling via boiling heat transfer is that they possess a Leidenfrost point at a superheat higher than bare, causing low-heat flux film boiling to rapidly transition to transient boiling. It is assumed that film boiling mostly consists of a dry zone with low heat flux, where a vapor film forms at the solid-liquid interface due to the generation of numerous bubbles, although a conduction zone where the liquid comes into direct contact with the solid occasionally occurs. In this case, for general metals with high heat capacity and thermal diffusivity, heat diffuses rapidly even when liquid conduction occurs, resulting in minimal surface temperature changes; consequently, the surface is quickly covered by a new vapor film, returning to stable film boiling. However, if a conduction zone occurs on a polymer with low heat capacity and thermal diffusivity on the metal surface, heat cannot diffuse between the metal and the adjacent polymer. Consequently, a localized temperature drop occurs at the polymer surface in contact with the liquid, and the vapor film fails to recover, creating an unstable vapor film. When the local temperature drop on the polymer surface reaches the transition temperature that causes transition boiling, a transition and nucleation boiling region begins where the heat flux increases, resulting in a larger Leidenfrost point and a faster cooling rate than that of a bare specimen.
[0054] Polymer coatings, such as PTFE, are typically applied to metal surfaces using dip coating or spray coating methods. While these conventional methods are effective for simple shapes like rods, they are not suitable for achieving a uniform coating on the inner surface of long, narrow tubes due to limitations in thickness control and coating uniformity. To overcome these limitations, the present invention fabricated a patterned polymer coating on the inner surface of a long, narrow tube using electrophoretic deposition (EPD). EPD is an electrochemical technique that precisely and uniformly coats (electrodeposits) charged colloidal polymer particles onto a conductive substrate under an applied electric field, enabling conformal coating even on geometrically complex surfaces. Polyimide (PI) was selected as the coating material because it exhibits excellent mechanical strength, thermal stability, and dielectric properties at cryogenic temperatures, making it highly suitable for superconducting and cryogenic applications.
[0055] Figure 1 shows a schematic diagram of an electrodeposition coating process for polyimide coating. Electrodeposition is a thin film coating method that forms a film by moving and accumulating charged colloidal particles onto a conductive substrate under an electric field.
[0056] In this invention, polyamic acid (PAA), a precursor of polyimide, is dispersed in water to generate negatively charged colloidal particles, which are then used as a coating solution. The coating process begins by injecting the polyamic acid colloidal solution into an electrochemical cell, followed by the application of a DC voltage between a stainless steel tube (anode) and a counter electrode (cathode). The negatively charged colloidal particles migrate to the anode via electrophoresis, and hydrogen ions (H₂) generated by the electrolysis of water on the anode surface +It interacts with ). This local pH reduction lowers the solubility of polyamic acid, causing particle aggregation and film formation on the tube walls. At the same time, electroosmotic flow promotes the removal of water through microporous pathways within the coating layer, thereby improving the density and adhesion of the coating layer. After electrodeposition, the polyamic acid coating layer is thermally imidized through heat treatment, transforming into a mechanically robust and thermally stable polyimide film suitable for cryogenic applications.
[0057] In the present invention, a customized masking process was developed to produce a patterned PI coating on the inner surface of a metal tube and integrated with an electrodeposition coating process.
[0058] Figure 2 shows a schematic diagram of the pattern coating process on the inner surface of the pipe.
[0059] First, a step of cutting the masking sheet into a pattern shape can be performed.
[0060] Masking sheets must meet criteria such as electrical insulation to prevent unintended electrodeposition of coating solution, chemical resistance to polyamic acid solution, thermal stability against high-temperature imidization, and mechanical durability that allows insertion and removal without tearing or deformation.
[0061] The material of the masking sheet may be one or more selected from the group consisting of Teflon, polyimide, and silicone. Preferably, it may be Teflon, but is not limited thereto.
[0062] When inserting the above pattern masking sheet into the pipe, an auxiliary sheet may be attached to the above pattern masking sheet for structural stability.
[0063] The pattern shape of the masking sheet above is any one of a square, a circle, a triangle, a hexagon, and an irregular shape, and the pattern shape may be arranged continuously or discontinuously.
[0064] Next, the step of attaching the cut pattern masking sheet to the inside of the pipe can be performed.
[0065] Insert the above pattern masking sheet into the pipe and attach it to the inner surface of the pipe, then press it with a fixing rod to ensure close contact, and then remove the auxiliary sheet to leave only the pattern masking sheet.
[0066] Next, the step of installing the pipe with the pattern masking sheet attached to it into a pipe coating device can be performed.
[0067] The electrode can be positioned to be concentric with the pipe to which the pattern masking sheet is attached. If the concentricity between the pipe and the electrode is insufficient, it may be difficult to achieve a uniform coating in the radial direction.
[0068] The pipe with the above-mentioned pattern masking sheet attached is positioned vertically on a pipe coating device.
[0069] Next, a step can be performed to form a polyimide coating layer by filling the inside of the pipe to which the pattern masking sheet is attached with a polyimide precursor solution and applying power to perform electrodeposition coating.
[0070] The above polyimide coating is applied only to the exposed area where the pattern masking sheet is not attached.
[0071] The above polyimide precursor may be polyamic acid (PAA).
[0072] The coating ratio of the polyimide may be 20 to 80% relative to the internal area of the pipe. Preferably, the coating ratio of the polyimide may be 20 to 50% relative to the internal area of the pipe, but is not limited thereto. The coating ratio of the polyimide can be controlled through the size and number of pattern shapes of the pattern masking sheet.
[0073] The coating thickness of the polyimide may be 3 to 100 μm. Preferably, it may be 3 to 60 μm, but is not limited thereto.
[0074] The coating thickness of the above polyimide can be controlled by controlling the diameter of the electrode, voltage, and current flow time.
[0075] The voltage applied during the above electrodeposition coating is preferably in the range of 1 to 20 V. Below 1 V, it is undesirable because it takes a very long time for the electrodeposition coating to be completed or the coating thickness is thin, resulting in a film formation that is not dense. Furthermore, under a voltage exceeding 20 V, bubble generation due to the electrolysis of water increases significantly, causing bubble defects within the coating layer and making it difficult to form a dense and uniform film, which is also undesirable. Therefore, it is preferable to perform the electrodeposition coating within the range of 1 to 20 V. The voltage application time can be adjusted according to the above applied voltage.
[0076] The step of forming a polyimide coating layer by filling the inside of the above pipe with a polyimide precursor solution and applying power to perform electrodeposition coating can be performed by forming a polyimide precursor coating layer through electrodeposition coating and then heat-treating at 200 to 300 ℃ to form a polyimide coating layer through imidization.
[0077] Finally, a step of removing the masking sheet attached to the inside of the pipe on which the polyimide coating layer is formed can be performed.
[0078] By coating polyimide on the inner surface of a cryogenic cooling pipe using the polyimide pattern electrodeposition coating method according to the present invention, the cooling speed can be improved, and by coating in a patterned form, the possibility of damage due to thermal shrinkage during the cooling process is reduced and the cooling speed can be improved more quickly.
[0079] In addition, the present invention provides a cryogenic cooling pipe coated with a polyimide pattern by the above method.
[0080] In addition, the present invention provides a superconductor cooling device comprising the above-mentioned cryogenic cooling pipe.
[0081]
[0082] Hereinafter, the present invention will be described in detail with reference to examples to specifically explain the invention. However, the embodiments according to the present invention may be modified in various different forms, and the scope of the present invention is not to be interpreted as being limited to the embodiments described below. The embodiments of this specification are provided to more completely explain the present invention to those with average knowledge in the art.
[0083]
[0084] <Preparation Example> Synthesis of Polyimide Precursor
[0085] Polyamic acid was prepared by dissolving 17.5 parts by weight of pyromellitic dianhydride, 12.8 parts by weight of 4,4'-diaminophenyl ether, and 17.2 parts by weight of diaminosilicone in a solvent consisting of dimethyl sulfoxide, acetone, and ethyl alcohol to a solid content of 20 wt%, and reacting at room temperature for 3 hours under a nitrogen atmosphere. Subsequently, triethanolamine and trihexylamine were added and mixed for about 16 hours to prepare a polyamic acid salt. Then, a polymer colloidal dispersion was prepared by adding 150 parts by weight of distilled water based on 100 parts by weight of polyamic acid.
[0086]
[0087] <Example> Polyimide pattern electrodeposition coating
[0088] Stainless steel, widely used in cryogenic transfer lines, was used as the piping material. The outer diameter of the specimen was 12.7 mm, the inner diameter was 10.92 mm, and the length was 380 mm. The polyimide coating thickness was adjusted to 5.4 μm, 27.2 μm, and 49.1 μm. The coatings were fabricated with surface coverage rates of 0%, 25%, 44%, 69%, and 100%. Initial cooling performance was experimentally evaluated using 2 bar liquid nitrogen (LN2) under forced flow boiling conditions at mass flow rates of 3.7 g / s, 7.5 g / s, and 11.2 g / s.
[0089]
[0090] 1. Masking and cutting of the pattern shape
[0091] A 0.18 mm thick Teflon sheet was selected as the masking material. Square patterns were used to manufacture masking sheets with various coating ratios (24%, 44%, and 69%), and the parameters of the patterned coatings are summarized in Table 1 below. 80 squares were produced for the low ratio of 25%, the medium ratio of 44%, and the high ratio of 69%, and specimens were produced using smaller squares for the same 44% ratio pattern coating. The drawings of the patterned masking sheets are shown in Fig. 3. Figs. 3(a)–(c) show the drawings of masking sheets with coating ratios of 25%, 44%, and 69%, respectively.
[0092] The masking sheet was cut into a pattern shape, and an auxiliary sheet was attached.
[0093] Classification Coating Ratio 25% 44% 69% Number of Squares (pieces) 160 160 160 Side Length (mm) 4.5 67.5 Number of Radial Patterns (pieces) 44 4 Number of Length Patterns (pieces) 40 40 40
[0094] Figures 4(a)-(c) show the pattern coating arrangement on the inner surface of the pipe for each coating ratio.
[0095] 2. Attach masking sheets to the inside of the pipes
[0096] The piping material used was stainless steel, which is widely used in cryogenic transfer lines, and a long, narrow pipe with an outer diameter of 12.7 mm, an inner diameter of 10.92 mm, and a length of 380 mm was used.
[0097] After removing the release liner from the masking sheet, it was inserted into the pipe and attached to the inner surface, then pressed with a fixing rod to ensure a tight seal. The auxiliary sheet was carefully removed, leaving only the patterned Teflon masking sheet.
[0098] 3. Removal of electroplating and masking sheet
[0099] Subsequently, to ensure a uniform coating inside the pipe, the pipe was installed in a device designed to maintain concentricity between the electrode and the pipe while preventing leakage of the coating solution. After filling the pipe with a polyimide precursor solution for electrodeposition coating, power was applied between the pipe (anode) and the internal electrode rod (cathode) to perform electrodeposition coating. To induce an imidation reaction in the polyimide precursor, the coated pipe was heated in a furnace to a maximum of 250°C to cure the coating layer and ensure stable adhesion. The electrodeposited PAA layer was thermally imidized to form a stable polyimide film. Finally, the masking sheet was removed to obtain the pattern-coated pipe. A total of three coating thicknesses were prepared: 5.4 μm, 27.3 μm, and 49.1 μm.
[0100]
[0101] <Comparative Example 1> 100% Coated Pipe
[0102] It was manufactured in the same manner as Example 1, except for the masking process.
[0103]
[0104] <Comparative Example 2> 0% coated (bare) pipe
[0105] Pipes without electroplating were prepared.
[0106]
[0107] <Experimental Example 1> Evaluation of Masking Sheet Materials for Electrodeposition Coating
[0108] Coating solution experiments and heating furnace experiments were conducted on masking sheets of different materials.
[0109] Table 2 below shows the experimental results of masking materials for polyimide electrodeposition coating, and finally, a Teflon tape was selected that guarantees both chemical resistance and heat resistance.
[0110] Classification Chemical resistance in colloidal solutions Heat resistance during drying Tensile strength High heat-resistant masking tape OX Low Kapton tape OO Low PVC sheet XX Low PET sheet OX Low General masking tape OX High Polyester tape OX Low Teflon sheet OO High
[0111]
[0112] <Experimental Example 1> SEM Analysis
[0113] Figure 5 shows the coating thickness of the inner surface of the tube measured using a scanning electron microscope (SEM). Electrodeposited coating layers with three thicknesses of 5.4 μm, 27.3 μm, and 49.1 μm can be observed.
[0114]
[0115] <Experimental Example 2>
[0116] Fluid boiling experimental apparatus
[0117] Initial cooling experiments were performed using liquid nitrogen (LN2) under flow boiling conditions. To ensure accurate and repeatable cooling measurements, it was essential to provide a stable supply of saturated LN2 to the test section. The experimental setup is shown in Fig. 6(a). Since connecting the liquid nitrogen deurer directly to the test section would make pressure regulation difficult, the liquid nitrogen was instead first transferred to a vacuum-insulated storage tank. Helium gas was supplied via a pressure regulator to maintain a stable pressure in the storage tank. To prevent overpressure during rapid vaporization during initial cooling, a safety relief valve was installed in the storage tank, and a buffer tank was integrated into the helium supply line. During the transfer of liquid nitrogen to the test zone, partial vaporization may occur due to heat input from the surrounding environment and the heat capacity of the supply piping. To prevent gaseous inflow, a supercooling heat exchanger was used to condense all vapor into the liquid phase. The initial unsaturated fluid was purged using a bypass valve. Once a stable flow of the saturated liquid was secured, the bypass was quickly closed to redirect the flow to the test section. The test section was installed inside a vacuum-insulated chamber to minimize the thermal load. Using a vacuum pump, 10 -4 A high vacuum of less than torr was maintained. Liquid nitrogen passing through the test section was completely vaporized in an atmospheric heat exchanger and then passed through a flow meter. System pressure was measured upstream of the bypass valve.
[0118] Figure 6(b) shows a schematic diagram of the test section used for the cooling experiment. The total length of the piping is 500 mm, and the coating piping is 380 mm. Custom ConFlat flanges with Lok fittings at both ends were fabricated to maintain vacuum insulation while connecting to the cryogenic pipeline. The vacuum chamber was equipped with NW ports and flexible bellows to facilitate assembly and sealing. Surface temperatures were measured using high-speed response thermocouples with fine bead tips. Six thermocouples were installed at the midpoint and the outlet, at two axial positions. Three sensors were placed circumferentially at each axial position on the bottom, side, and top of the outer surface of the tube to measure the radial heat distribution during cooling.
[0119] The test piping was made of stainless steel with an outer diameter of 12.7 mm, an inner diameter of 10.92 mm, and a length of 380 mm. Polyimide (PI), which exhibits excellent mechanical and thermal stability at cryogenic temperatures, was used as the coating material. Coating thicknesses of 5.4 μm, 27.3 μm, and 49.1 μm were applied, and the coating ratios were varied to 0%, 25%, 44%, 69%, and 100%. All experiments were conducted at an inlet pressure of 2 bar at three mass flow rates of 3.7 g / s, 7.5 g / s, and 11.2 g / s.
[0120]
[0121] Results of flow boiling experiment in liquid nitrogen
[0122] 1) Cooling curve of bare piping (0% coating ratio)
[0123] Prior to evaluating the cooling performance of the coated piping, the cooling performance of the bare piping was evaluated at various mass flow rates as shown in Fig. 7. At all mass flow rates, the temperature profile at each sensor location follows well-known boiling heat transfer regions, namely film boiling, transition boiling, and flow boiling combined with fluid flow. The saturated liquid nitrogen supplied to the test zone passes through the supercooling heat exchanger but does not immediately occupy the entire pipe cross-section. Instead, the liquid gradually accumulates from bottom to top, cooling sequentially from the bottom of the pipe to the sides, and finally to the top. In the axial direction, the outlet cools more slowly than the midpoint because it takes longer for the liquid to reach the downstream location. Although cooling begins almost simultaneously at both axial locations, it should be noted that the outlet may experience a cooling delay due to axial heat conduction in the flange area exposed to ambient conditions. As expected, increasing the mass flow rate accelerates the cooling rate, indicating that increased liquid nitrogen supply improves convective heat removal.
[0124] 2) Cooling curve of the coated tube
[0125] As can be seen in Figure 7, the upstream and downstream regions begin to cool simultaneously, but the downstream region exhibits a relatively slower cooling rate. This can be attributed to axial heat conduction at the vacuum insulation chamber outlet and the thermal capacity of the flange components. To minimize the influence of these boundary effects, the temperature of the bottom surface at the midpoint was selected as a representative variable for evaluating cooling performance.
[0126] Figure 8 shows the temperature change of a 100% coated tube according to coating thickness at three mass flow rates. In all cases, the initial cooling phase remains in the film boiling region, during which both the coated and bare tubes exhibit similar cooling curves. However, the 100% coated tube reaches the film boiling region earlier and transitions to the transient boiling region more quickly, accelerating the overall cooling process. Importantly, the film boiling region increases with increasing coating thickness, allowing for a faster exit from the film boiling region. At a mass flow rate of 3.7 g / s, the Leidenfrost point (LFP) of the coated tube begins significantly earlier and at a higher temperature compared to the bare tube. For the bare tube, the LFP is observed at 266 seconds and 123 K. However, as the coating thickness increases, LFP shifts to 117 seconds at 167K for the 5.4μm coating, 105 seconds at 174K for the 27.3μm coating, and 95 seconds at 182K for the 49.1μm coating. At a mass flow rate of 7.5g / s, LFP in the bare tubing appears at 184 seconds and 119K. LFP shifts to 93 seconds at 163K for the 5.4μm coating, 77 seconds at 179K for the 27.3μm coating, and 64 seconds at 190K for the 49.1μm coating. At a mass flow rate of 11.2g / s, LFP in the bare tubing appears at 127 seconds and 126K. For the 5.4μm coating, the LFP moves to 90 seconds at 163K, for the 27.3μm coating to 67 seconds at 175K, and for the 49.1μm coating to 64 seconds at 194K.
[0127] When the mass flow rate is 3.7 g / s, a thin coating of 5.4 μm significantly improves cooling performance, but the effect becomes negligible when the thickness is increased. Conversely, as the mass flow rate increases, the influence of coating thickness becomes greater, and as the coating thickness increases, the cooling rate becomes increasingly faster.
[0128] Figure 9 compares the cooling rates of tubes with a coating thickness of 49.1 μm at various pattern coating ratios. The pattern-coated piping exhibits a significantly steeper temperature gradient compared to the uncoated piping and the 100% coated piping, indicating improved heat transfer and accelerated cooling performance. Furthermore, no LFP was observed in the cooling curves of the pattern-coated piping. In particular, even at a coating ratio of 69%, cooling performance was significantly improved compared to the 100% coated piping, and the total cooling time was also greatly reduced. Additionally, when the coating ratios were low at 25% and 44%, superior cooling performance was observed compared to when the coating ratio was high. These results indicate that pattern coating offers superior cooling performance compared to 100% coating and that an optimal pattern coating ratio exists. This characteristic was consistently observed across all test cases.
[0129] 3) Effect of Pattern Coating on Cooling Rate Improvement and Cooling Time Reduction
[0130] Figure 10 shows the results of comparing the normalized cooling time reduction rate of the coated piping with that of the coated piping at various mass flow rates (MFA). Cooling time is defined as the time it takes for the pipe wall temperature to decrease from 300K to 88.0K, which corresponds to 98% of the total temperature drop from 2 bar (83.6K) to the liquid nitrogen saturation point.
[0131] At all flow rates, the 49.1 μm, 25% pattern-coated pipe, which had the thickest coating thickness and the lowest coating ratio, showed the greatest reduction in cooling time, exhibiting a maximum reduction of 88% at 3.7 g / s. On the other hand, the pipe with a 100% coating area showed a lower reduction in cooling time at all flow rates, exhibiting a maximum reduction of 60% when the coating thickness was the thickest.
[0132] 4) Heat transfer characteristics of various coated pipes
[0133] Since surface temperature alone is insufficient to fully analyze the underlying heat transfer mechanism, the present invention evaluated cooling performance and boiling regions through heat flux analysis. Heat flux serves as a clear and quantitative indicator for evaluating the influence of coating conditions on transient cooling characteristics. In particular, analyzing heat flux through superheating allows for the distinction of various boiling regions, such as film boiling, transition boiling, and nucleation boiling, and enables the quantitative comparison of heat transfer behavior across various coating configurations. Figure 11 shows the change in heat flux of a coated pipe at a mass flow rate of 7.5 g / s. (a) shows the effect of coating thickness on a 100% coated pipe, and (b) shows the effect of the coating ratio at a thickness of 49.1 μm. In Figure 11(a), the bare pipe exhibits prolonged film boiling due to vapor film formation, resulting in low heat flux over most of the cooling process, followed by a sharp peak when the surface passes through the LFP. Conversely, the coated pipe with increased thickness shows an early termination of the film boiling region and transitions more quickly to a more efficient boiling mode. However, during film boiling, the heat flux remains similar to that of the bare pipe. Figure 11(b) shows distinct behavior in the patterned-coated pipe. Unlike the bare and 100% coated pipes, the patterned coating generates a high heat flux from the initial cooling phase, making it difficult to distinguish the film boiling region.
[0134] Figure 12 shows the boiling curves of the coated tubing. Figure 12(a) shows the boiling curves of the 100% coated tubing at various coating thicknesses. For the bare tubing, LFP occurs at a relatively low superheat of 40K. However, as the coating thickness increases, LFP shifts to higher superheat levels, reaching up to 110K for the thickest coating (49.1 μm). This accelerated onset of transition boiling reduces the duration of film boiling, enabling a faster cooling process. Figure 12(b) shows the boiling curves of the patterned coated tubing with a fixed coating thickness of 49.1 μm and different coating ratios applied. Unlike the 100% coated tubing and the bare tubing, the patterned coated tubing exhibits a relatively high heat flux even at high superheats, making it difficult to clearly distinguish LFP. This behavior suggests that the patterned coating improves overall heat transfer performance throughout the boiling process by increasing film instability and bubble interference.
[0135] According to the results presented in Figures 11 and 12, the patterned coated piping exhibited superior initial cooling performance compared to both bare and 100% coated piping. In particular, the patterned coated piping showed a higher heat flux even under high superheat conditions where film boiling is generally dominant, which suggests fundamentally different bubble behavior.
[0136] Figure 13 schematically illustrates the bubble kinetics in the superheated state of bare and pattern-coated piping. As can be seen in Figure 13(a), the bare piping experiences stable film boiling at high superheats, and a vapor film forms between the liquid and solid surfaces. This vapor film hinders heat transfer, resulting in a prolonged period of low heat flux until the surface cools sufficiently to transition to a nucleation state.
[0137] As can be seen in Fig. 13(b), the patterned coated tube makes the vapor film more unstable due to the structure of the coating's μm height under high superheat conditions, thereby increasing the contact between the solid and the liquid. As a result, high heat transfer occurs from the beginning of cooling, and it appears that film boiling is almost suppressed.
[0138] As cooling progresses, the coated surface cools faster than the bare surface due to localized temperature drops. Due to this characteristic, under low superheat conditions, bubbles generated by nucleation on the coated surface graze the bare surface, which still possesses a vapor film due to film boiling, as they follow the liquid flow. The vapor film on the bare surface is disrupted by interference from the nucleation bubbles, increasing solid-liquid contact and enhancing heat transfer. Pattern coatings are known to improve initial cooling performance by significantly increasing the heat flux during the initial cooling process, utilizing this superposition phenomenon where unstable film boiling formation and bubbles generated in different boiling regions coexist and interact.
[0139]
[0140] In this invention, a patterned polyimide coating was applied to the inner surface of a stainless steel pipe using electrodeposition coating. Initial cooling performance was evaluated according to various coating thicknesses, coating ratios, and mass flow rates of liquid nitrogen. The main results are as follows.
[0141] In the case of 100% coated piping, the cooling rate increased as the coating thickness increased. The cooling time was reduced by 28–60% compared to uncoated piping. This improvement is due to the increase in LFP with increasing coating thickness, which shortens the film boiling time and accelerates the transition to transition boiling, as confirmed by the boiling curve.
[0142] As the mass flow rate increased, the total cooling time decreased. However, the relative benefit of increasing coating thickness diminished at high flow rates, suggesting that thick coatings are less effective under high flow rate conditions. This implies that thin coatings are sufficient to improve cooling performance at low flow rates.
[0143] Patterned coated piping demonstrated superior performance compared to 100% coated piping under all conditions. In particular, at low coating ratios (25% and 44%), patterned coated piping exhibited the fastest cooling rates, reducing cooling time by up to 88% compared to bare piping. Notably, patterned coated piping displayed high heat flux even under high superheated conditions, indicating that bubble interactions between the bare piping and the coated area destabilize the vapor film and promote an early transition to efficient boiling. This bubble interaction mechanism is considered a key factor in the superior cooling performance of the patterned coating.
[0144] These results demonstrate the potential of patterned polyimide coatings as a highly effective and practical thermal strengthening technology for cryogenic transfer lines and components requiring rapid initial cooling.
[0145]
[0146] Specific embodiments of the present invention have been examined so far. Those skilled in the art will understand that the present invention may be embodied in modified forms without departing from the essential characteristics of the invention. Therefore, the disclosed embodiments should be considered in an illustrative rather than a restrictive sense. The scope of the present invention is defined by the claims, not by the foregoing description, and all variations within the scope of equivalents should be interpreted as being included in the present invention.
Claims
1. A step of cutting the masking sheet into a pattern shape; A step of attaching the above-detailed pattern masking sheet to the inside of the pipe; A step of installing the pipe with the above-mentioned pattern masking sheet attached to a pipe coating device; A step of forming a polyimide coating layer by filling the inside of a pipe to which the above-mentioned pattern masking sheet is attached with a polyimide precursor solution and applying power to perform electrodeposition coating; and A method for polyimide pattern electrodeposition coating for cryogenic cooling pipes, characterized by including the step of removing a masking sheet attached to the inside of a pipe on which the polyimide coating layer is formed.
2. In Paragraph 1, A polyimide pattern electrodeposition coating method for cryogenic cooling pipes, characterized in that the material of the masking sheet is one or more selected from the group consisting of Teflon, polyimide, and silicone.
3. In Paragraph 1, A method for applying a polyimide pattern electrodeposition coating for cryogenic cooling pipes, characterized in that the pattern shape of the pattern masking sheet is any one of a square, a circle, a triangle, a hexagon, and an irregular shape, and the pattern shape is arranged continuously or discontinuously.
4. In Paragraph 1, A polyimide pattern electrodeposition coating method for cryogenic cooling pipes, characterized in that the coating ratio of the above polyimide is 20 to 80% relative to the internal area of the pipe.
5. In Paragraph 1, A polyimide pattern electrodeposition coating method for cryogenic cooling pipes, characterized in that the coating thickness of the polyimide is 3 to 100 μm.
6. In Paragraph 1, The step of forming a polyimide coating layer by filling the inside of the above-mentioned pipe with a polyimide precursor solution and applying power to perform electrodeposition coating is: A polyimide pattern electrodeposition coating method for cryogenic cooling pipes, characterized by forming a polyimide precursor coating layer through the above electrodeposition coating and then forming a polyimide coating layer through imidization by heat treatment at 200 to 300 ℃.
7. Cryogenic cooling pipe with a polyimide pattern electrodeposited and coated by the method of claim 1.