Microplasma electrochemical method for recycling waste lithium-ion battery cathodes

The microplasma electrochemical method using a deep eutectic solvent and microplasma electrochemistry rapidly and efficiently recycles metals from spent lithium-ion batteries, addressing the inefficiencies and environmental concerns of existing methods.

WO2026240300A1PCT designated stage Publication Date: 2026-11-19SEOUL NATIONAL UNIVERSITY R&DB FOUNDATION
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2026/000012
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-14
Filing Date
2026-01-02
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Existing methods for recycling metals from spent lithium-ion batteries, such as wet and dry smelting, are energy-intensive, complex, and environmentally harmful due to the use of hazardous chemicals.

Method used

A microplasma electrochemical method combining a deep eutectic solvent (DES) and microplasma electrochemistry (MIPEC) is used to extract metals like lithium, cobalt, nickel, and manganese from spent lithium-ion batteries under room temperature and atmospheric pressure.

Benefits of technology

This method achieves rapid and efficient metal extraction with high leaching efficiency, reducing energy consumption and environmental impact, and avoids the use of toxic chemicals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2026000012_19112026_PF_FP_ABST
    Figure KR2026000012_19112026_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a microplasma electrochemical method for recycling waste lithium-ion battery cathodes, the microplasma electrochemical method comprising the steps of: (a) mixing waste lithium-ion battery cathode materials and a deep eutectic solvent (DES), and leaching important metals by using microplasma electrochemistry (MIPEC); and (b) recovering important metals from the leachate obtained in step (a). The present invention provides an eco-friendly and economical method whereby important metals such as lithium, cobalt, nickel, and manganese can be rapidly extracted and recycled from waste lithium-ion batteries under room temperature and atmospheric pressure conditions by combining a DES and MIPEC.
Need to check novelty before this filing date? Find Prior Art

Description

Microplasma electrochemical method for recycling spent lithium-ion battery cathodes

[0001] The present invention relates to a microplasma electrochemical method for recycling spent lithium-ion battery cathodes, and more specifically, to an environmentally friendly and economical method that combines a deep eutectic solvent (DES) and microplasma electrochemistry (MIPEC) to rapidly extract and recycle important metals such as lithium, cobalt, nickel, and manganese from spent lithium-ion batteries under conditions of room temperature and atmospheric pressure.

[0002] Lithium-ion batteries are rechargeable secondary batteries that have a high energy density relative to their weight and a high operating voltage, resulting in excellent charge and discharge cycles and low power loss due to self-discharge. Additionally, they have the characteristic of being able to be charged without being completely discharged because they do not have a memory effect, and they are widely used in mobile phones, laptop computers, digital cameras, and electric vehicles.

[0003] Recently, as the electric vehicle market has grown rapidly, the industry for recovering important metals such as lithium, nickel, cobalt, and manganese from spent lithium-ion batteries is gradually developing. Although much research is being conducted on the recovery and reuse of important metals from spent lithium-ion batteries, existing methods for recovering and reusing important metals from spent lithium-ion batteries (e.g., wet smelting methods, dry smelting methods, etc.) have problems such as high energy consumption, complex extraction processes, and environmental pollution caused by the use of hazardous compounds such as acid or alkali solutions.

[0004] In this regard, Korean Published Patent No. 10-2024-0139566 comprises an electrolytic cell, a separator that partitions the interior of the electrolytic cell to separate it into a first space and a second space, an oxidation electrode located in the first space, and a reduction electrode located in the second space opposite to the oxidation electrode, wherein the first space contains lithium ions (Li + A leaching solution, which is a liquid having ) conductivity, is filled, and the oxidation electrode is immersed in the leaching solution, and the second space contains the lithium ions (Li + A lithium recovery system is disclosed, characterized in that a recovery solution, which is a liquid capable of precipitating in the form of a lithium compound, is filled, and the reduction electrode is immersed in the recovery solution. However, a method that combines a eutectic solvent and microplasma electrochemistry to rapidly and economically recover important metals under conditions of room temperature and atmospheric pressure, as in the present invention, is not disclosed.

[0005] The objective of the present invention is to provide an environmentally friendly and economical method for rapidly extracting and recycling important metals such as lithium, cobalt, nickel, and manganese from spent lithium-ion batteries under room temperature and atmospheric pressure conditions by combining a eutectic solvent and a microplasma electrochemical method.

[0006] To achieve the above objective, the present invention provides a microplasma electrochemical method for recycling spent lithium-ion battery cathodes, comprising the steps of: (a) mixing a spent lithium-ion battery cathode material with a deep eutectic solvent (DES) and leaching a key metal using microplasma electrochemistry (MIPEC); and (b) recovering the key metal from the leaching solution obtained in step (a).

[0007] In addition, according to the present invention, a method is provided in which, in step (a), the waste lithium-ion battery cathode material is selected from one or more of the group consisting of lithium cobalt oxide (LCO), lithium manganese oxide (LMO), lithium iron phosphate (LFP), lithium nickel manganese cobalt oxide (NMC), and NMC black mass.

[0008] In addition, according to the present invention, a method is provided in which, in step (a), the eutectic solvent is selected from the group consisting of choline chloride (ChCl)-glycerol, ChCl-p-toluenesulfonic acid (pTSA), ChCl-oxalic acid, ChCl-acetic acid, ChCl-malonic acid, ChCl-ethylene glycol, and ChCl-urea.

[0009] In addition, according to the present invention, a method is provided in which the step of leaching an important metal using a microplasma electrochemical method in step (a) is performed for 0.5 to 4 hours under conditions of room temperature and atmospheric pressure.

[0010] In addition, according to the present invention, a method is provided in which, in step (a), the microplasma electrochemistry is performed using a microplasma anode working electrode made of a conductive capillary having a hollow structure (e.g., a hollow stainless-steel capillary), and a mesh-type counter electrode made of a conductive metal selected from the group consisting of platinum, molybdenum, tungsten, copper, silver, and zinc.

[0011] In addition, according to the present invention, a method is provided in which, in step (a), the important metal is selected from the group consisting of lithium, cobalt, nickel, manganese, iron, phosphorus, sodium, aluminum, copper, and carbon.

[0012] In addition, according to the present invention, a method is provided in which step (b) is performed using electrochemical deposition or precipitation.

[0013] According to the microplasma electrochemical method for recycling waste lithium-ion battery cathodes of the present invention, an environmentally friendly and economical method is provided that enables the rapid extraction and recycling of important metals such as lithium, cobalt, nickel, and manganese from waste lithium-ion batteries under conditions of room temperature and atmospheric pressure.

[0014] In addition, compared to conventional wet smelting methods or dry smelting methods, the present invention has the advantage of not requiring high temperatures and not using toxic chemical substances such as high concentrations of acid, alkali, or reducing agents.

[0015] In addition, the present invention can be effectively applied in various fields such as lithium cobalt oxide (LCO), lithium manganese oxide (LMO), lithium iron phosphate (LFP), lithium nickel manganese cobalt oxide (NMC), and NMC black mass.

[0016] However, the effects of the present invention are not limited to those mentioned above, and other unmentioned effects will be clearly understood by those skilled in the art from the description below.

[0017] FIG. 1 is a diagram showing the results of testing the leaching performance according to one embodiment of the present invention.

[0018] FIG. 2 is a diagram showing the characteristics and analysis results of a mechanism according to one embodiment of the present invention.

[0019] FIG. 3 is a diagram showing the characteristics and analysis results of a product obtained according to one embodiment of the present invention.

[0020] Figure 4 is a diagram showing the results of testing the leaching performance according to another embodiment of the present invention.

[0021] The present invention will be described in more detail below with reference to the attached drawings.

[0022] One aspect of the present invention relates to a microplasma electrochemical method for recycling spent lithium-ion battery cathodes, comprising the steps of: (a) mixing a spent lithium-ion battery cathode material with a deep eutectic solvent (DES) and leaching a key metal using microplasma electrochemistry (MIPEC); and (b) recovering the key metal from the leaching solution obtained in step (a).

[0023] More specifically, in step (a) of the present invention, the waste lithium-ion battery cathode material may be selected from one or more of the group consisting of, for example, lithium cobalt oxide (LCO), lithium manganese oxide (LMO), lithium iron phosphate (LFP), lithium nickel manganese cobalt oxide (NMC), and NMC black mass.

[0024] In step (a) of the present invention, the waste lithium-ion battery cathode material is mixed with a eutectic solvent, wherein the eutectic solvent refers to a substance that exists in a solution phase at 40 to 50°C or lower, with a lowered melting point when two naturally derived substances (liquid / solid or solid / solid) are mixed in a certain molar ratio at room temperature.

[0025] The above eutectic solvent is generally composed of a mixture of a hydrogen bond acceptor (HBA) and a hydrogen bond donor (HBD), and the chemical and physical properties of the eutectic solvent are determined according to the combination of the HBA and HBD.

[0026] In the present invention, the eutectic solvent may be selected from the group consisting of, for example, choline chloride (ChCl)-glycerol, ChCl-p-toluenesulfonic acid (pTSA), ChCl-oxalic acid, ChCl-acetic acid, ChCl-malonic acid, ChCl-ethylene glycol, and ChCl-urea.

[0027] In addition, in step (a) of the present invention, a critical metal is leached from a spent lithium-ion battery cathode using a microplasma electrochemical method. As in the present invention, when a critical metal is leached by combining a eutectic solvent (DES) and a microplasma electrochemical method (MIPEC), it is desirable to be able to efficiently leach the critical metal very quickly, that is, within 0.5 to 4 hours, under mild conditions, namely room temperature and atmospheric pressure.

[0028] More specifically, when leaching cobalt from spent lithium-ion batteries, conventional wet smelting methods are known to take about 18 to 24 hours, and in particular, DES leaching smelting methods are known to require heating to a high temperature such as about 220°C or to be carried out for more than about 24 hours, but according to the present invention, important metals can be leached very quickly within 0.5 to 4 hours under mild conditions such as room temperature and atmospheric pressure.

[0029] In addition, when leaching cobalt from spent lithium-ion battery materials, in terms of efficiency, compared to leaching with only a pure eutectic solvent (Pure DES leaching) or leaching with a eutectic solvent (DES) combined with an electrochemical method (Electrochemical leaching in DES), leaching with DES combined with MIPEC as in the present invention has the advantage of exhibiting leaching efficiency that is approximately 2,281 times and approximately 12,657 times higher, respectively.

[0030] In addition, the microplasma electrochemical method in step (a) of the present invention may be performed using a microplasma anode working electrode made of a conductive capillary having a hollow structure (e.g., a hollow stainless-steel capillary), and a mesh-type counter electrode made of a conductive metal selected from the group consisting of platinum, molybdenum, tungsten, copper, silver, and zinc.

[0031] In addition, according to the present invention, a method is provided in which, in step (a), the important metal is selected from the group consisting of lithium, cobalt, nickel, manganese, iron, phosphorus, sodium, aluminum, copper, and carbon.

[0032] Meanwhile, step (b) of the present invention is a step of recovering important metals from the leaching solution obtained in step (a).

[0033] More specifically, the above step (b) can be performed, for example, using electrochemical deposition or precipitation.

[0034]

[0035] The present invention will be explained in more detail below through examples. However, these examples are intended to illustrate the invention and the scope of the invention is not limited to these examples.

[0036]

[0037] Example 1: Experimental Method

[0038] 1-1. DES Synthesis

[0039] Choline chloride (HOC2H4N[CH3]3Cl; ChCl; ≥98%; Sigma-Aldrich) and ethylene glycol (HOCH2CH2OH, anhydrous; EG; ≥98%; Sigma-Aldrich) were used as the hydrogen bond acceptor (HBA) and hydrogen bond donor (HBD), respectively, with a molar ratio of 1:2. ChCl was dried in a vacuum oven at 80°C for 24 hours and then transferred to a glove box (less than 2 ppm O2 and H2O). The ChCl / EG mixture was continuously stirred at 400 rpm and heated in the glove box to 80°C until a uniform, transparent liquid was formed (ChCl / EG DES).

[0040]

[0041] 1-2. Metal Extraction Using MIPEC

[0042] For metal extraction, 0.6 g of LCO powder (98%; Energy Chemical) was added to 30 g of ChCl / EG DES and mixed in an electrolytic cell. A microplasma electrode (hollow stainless-steel capillary; outer diameter 1.60 mm, inner diameter 0.25 mm) and a Pt mesh (1.5 x 1.5 mm; 99.99%) were used as the working electrode and counter electrode, respectively (Fig. 1a). The microplasma was ignited by applying a DC voltage (DC power supply, Dong Wen High Voltage Company) along with an argon flow (purity 99.0%). Simultaneously, a resistor (~50 kΩ) was used to ensure a stable discharge. After MIPEC treatment at specific time intervals, approximately 0.5 mL of the cathode material + DES leaching solution was extracted using a syringe, filtered through a membrane filter (diameter 10 mm, pore size 0.45 µm), and used for characterization.

[0043]

[0044] 1-3. Leaching Efficiency

[0045] The leaching efficiency was calculated by the following equation.

[0046]

[0047] Here, C is the metal concentration of the solution (mgL) -1 ) and V represents the initial volume of the solution (L), and m x represents the initial amount of metal ions (mg) in the cathode material.

[0048]

[0049] 1-4. Metal Recovery

[0050] After metal extraction, approximately 10 ml of Na2CO3 (20 wt% in deionized water) was added to 4 ml of the leaching solution. The mixture was centrifuged and washed several times with deionized water until no cloud formed when an AgNO3 solution was added to the liquid supernatant. The purified precipitate powder was dried in an oven at 90°C for 24 hours and then calcined at 500°C for 6 hours.

[0051]

[0052] Example 2: Results and Discussion

[0053] 2-1. Extraction of Important Metals from Waste LIBs

[0054] The leaching behavior of Li and Co in spent LIBs was investigated using lithium cobalt(III) oxide (LiCoO2, LCO) powder as an initial model compound. A DES composed of ChCl and EG in a molar ratio of 1:2 was used as the leaching agent and the reducing agent. An argon-induced microplasma was used as the working electrode, and a Pt mesh was used as the counter electrode (see Fig. 1a). For the cathode material dissolution experiment, approximately 0.6 g of LCO powder was mixed with 30 g of the ChCl / EG DES solution. The well-mixed solution was electrolyzed for various reaction times at a current of 20 mA using the microplasma as the anode and continuously mixed at 400 rpm.

[0055] The MIPEC-DES approach according to the present invention was found to be an ultrafast dissolution strategy. Indeed, after approximately 30 minutes of electrolysis, the color of the DES solution turned transparent blue, which is Co 2+This is interpreted as indicating an increase in concentration. As can be seen in Fig. 1b, the concentrations of Li and Co leached into the DES were highly dependent on the electrolysis time, and when MIPEC was used as the anode, the leaching efficiencies of Li and Co reached 100% and 91.4%, respectively, within approximately 180 minutes. Although the efficiency was close to that of general wet smelting methods, such as 100% for Co, the reaction time to reach this efficiency was much shorter than that of conventional wet smelting leaching (18–24 hours) or DES smelting leaching methods (>24 hours). Previous studies have reported using DES for high-efficiency leaching, but such methods generally require heating the DES to high temperatures, such as approximately 220°C, which is significantly higher than the room temperature used in the present invention. As a result, it was found that recycling 0.1g of LCO using the MIPEC-DES method according to the present invention (20W for 180 minutes) can achieve similar leaching efficiency while saving 1 / 400 of the energy compared to DES leaching at 220℃ (using a 1kW heating plate for 24 hours).

[0056] To find the cause of the high efficiency of the MIPEC-DES method according to the present invention, the effects of MIPEC and DES were studied separately. When Li and Co were extracted using only ChCl / EG DES at room temperature without MIPEC treatment, almost no leaching occurred. As shown in Fig. 1c, even when the leaching time was extended from 180 minutes to 24 hours, the leaching efficiency was only 0.33% for Li and 0.04% for Co. This suggests that MIPEC is necessary for DES leaching under mild conditions, i.e., at room temperature.

[0057] Next, to investigate the effects of plasma and electrochemistry in the MIPEC method, an electrochemical (EC) leaching method was tested in ChCl / EG DES. The microplasma anode was replaced with a conventional Pt mesh electrode, and the same current was applied to the solution. Although no apparent leaching occurred, the concentration of Li was too low to be detected by ICP-AES even after 24 hours, and the leaching efficiency of Co was only 0.01%. This demonstrates that electrochemistry alone cannot operate and that plasma plays a more important role.

[0058] In addition, since microplasma can function as both an anode and a cathode, the performance of the microplasma acting as a cathode was also tested due to the differing reaction environments. After a 180-minute experiment, the leaching efficiency was 3.29% for Li and 1.88% for Co, which was significantly higher than that of DES chemical leaching and EC leaching methods, demonstrating the effectiveness of plasma chemistry. However, it was still incomparable to microplasma anode leaching. The leaching efficiency of Co using a microplasma anode was 2,281 times, 12,657 times, and 47 times higher than that of pure DES leaching, electrochemical leaching from DES, and using a microplasma cathode, respectively. These results indicate that plasma plays a key role and that fabrication can be achieved more efficiently by controlling the electrochemical input.

[0059]

[0060] 2-2. Mechanism Analysis

[0061] In lithium cobalt(III) oxide (LiCoO2) powder, Co(III) is the dominant oxidation state but is insoluble and remains stable in acidic solutions at room temperature. Therefore, converting Co from the insoluble high-oxidation state Co(III) to the much more soluble low-oxidation state Co(II) is a key factor in improving leaching efficiency and reaction kinetics in conventional wet smelting processes. In the MIPEC-DES method, tetrachlorocobaltate(ii) anion ([CoCl4]2- ) was formed, which can be confirmed by ultraviolet-visible (UV-vis) spectroscopy. [CoCl4] 2- The triplet characterization peak of was clearly observed in the 600-700 nm range and increased with longer reaction times. At the same time, SEM images showed that the layered structure of the LCO powder was gradually corroded. These results indicate that the leaching mechanism of this method is also based on the reduction of Co(III).

[0062] The reduction mechanism of Co(III) in the MIPEC-DES process according to the present invention was investigated. Ethylene glycol in DES can act as a reducing agent during the LCO dissolution process, and the presence of oxygen acceptors in the eutectic mixture appears to be essential for digesting oxides because it facilitates the cleavage of metal oxide bonds. However, the reducing power of ethylene glycol is somewhat limited, and to effectively extract important elements from spent LIBs, the extraction reaction must be operated at 220°C for 24 hours. As shown in Fig. 1c, it was confirmed that DES leaching at room temperature does not show a clear effect. This indicates that a new reaction pathway is at work due to the presence of MIPEC.

[0063] In recently reported contact-electro-catalysis (CEC) methods, ROS generated by contact electrocatalysis can not only directly reduce metals but also significantly improve leaching efficiency by generating H2O2 to further leach the metals. Therefore, in this invention, radicals generated under various conditions were tested. As shown in Fig. 2a, superoxide ·O2 in the MIPEC-DES system - ... was detected. The EPR spectrum obtained when the LCO-DES mixture was treated with microplasma as an anode was ·O2 - Provided a signal. When microplasma was used as a cathode ·O2 -The signal was much weaker but still present. When only LCO was introduced into the DES without microplasma, no signal was observed.

[0064] Meanwhile, ·O2 - Regarding where this originates, previous reports indicate that microplasmas can generate radicals in water and organic solvents, particularly in air, but have not been studied in DES solvents. The effect of oxygen was first investigated in different atmospheres under two air conditions under N2 protection. As shown in Fig. 2b, Li in air + Wa Co 2+ The concentration was slightly higher than during N2 protection. The above results indicate that oxygen affects the leaching behavior of the microplasma anode in DES to some extent. Since DES consists of a hydrogen bond acceptor (HBA) and a hydrogen bond donor (HBD), the role of HBD in the leaching process was verified using ChCl / Urea DES. In the same MIPEC-DES process, the leaching capacity of ChCl / Urea DES was incomparable to that of ChCl / EG DES, and the leaching efficiencies of Li and Co were 3.28% and 1.84%, respectively, over 180 minutes. Additionally, no ROS signal was detected in the EPR. The above results indicate that the type of HBD has a significant impact on LCO leaching in the MIPEC-DES process.

[0065] Based on the above results, it is presumed that the reaction mechanism of the MIPEC-DES method according to the present invention is related to both plasma chemistry and electrochemistry. When a microplasma anode is used, EG(C2H6O2) becomes C2H5O + Cations, superoxide, and H + It forms to change the solution to an acidic environment (Equation (1)). Then ·O2 - It can directly contribute to the reduction of the metal as indicated in equation (2). The oxygen generated in this step and the oxygen in the air can produce more ·O2 through plasma chemistry. -It can be activated to form.

[0066]

[0067]

[0068]

[0069] On the other hand, during the electrochemical reaction, ChCl(C5H 14 ClNO) also decomposes and is oxidized to C5H 13 It can be ClNO, which is ·O2 as described in equations (4) and (5). - It reacts with and is converted back to ChCl. At this stage, hydrogen peroxide (H2O2) accumulates and helps to leach the metal with H2O2, as in an acid-leaching reaction (i.e., a wet smelting process) (Equation (6)). In this reaction, ·O2 - By effectively producing and utilizing H2O2, the MIPEC-DES method exhibited high extraction efficiency. When using a microplasma cathode, there were few high-energy particles in the plasma, and the electrochemical reaction often provided electrons to the system, making it difficult to induce the reaction in equations (1) and (4). Therefore, as shown in FIG. 1c, the extraction efficiency was much lower than that of a microplasma anode.

[0070]

[0071]

[0072]

[0073] The point to note is C2H5O + It is possible to form EG by reacting with H2O2. Using equations (1)(4)(5)(7), EG and ChCl are not consumed.

[0074]

[0075] This can be confirmed by the NMR results (Fig. 2d). After treatment with a microplasma anode for 180 minutes, the spectra of ChCl / EG DES at 2.75 ppm and 2.50 ppm did not show distinct changes, and the color of DES remained clear. In the presence of an LCO cathode material, ·O2 as in equations (2) and (6). - Since it can react with H2O2, the recovery of ChCl / EG DES is slightly affected, and some byproducts are generated. However, overall, NMR results indicate that the structure of DES is similar at the beginning and end of the MIPEC-DES process, suggesting the stability of DES and that the MIPEC-DES method is environmentally friendly.

[0076] In addition, Density Functional Theory (DFT) was used to identify the leaching behavior and interactions between solvent molecules and metal ions. Electron donation from the solvent molecule's most occupied (HOMO) orbital to the metal ion's empty orbital is an interaction during the leaching process. Furthermore, the smaller the band gap (the energy difference between HOMO and LUMO), the more stable the binding between DES and Li / Co. As can be seen in Figures 2e and 2f, Co had a narrower band gap (5.31 eV) compared to Li (6.32 eV). The binding energy of the DES-Li / Co interaction was calculated using the following equation to determine the metal ion affinity of DES.

[0077]

[0078] In general, the absolute value of binding energy reflects the leaching ability of the solvent. The higher the binding energy, the stronger the interaction, and the greater the affinity and binding stability between DES and metal ions. The calculated binding energies for DES-Li and DES-Co are 4.71 eV and 16.75 eV, respectively. This result indicates that DES prefers to form a stable complex with Co, which is consistent with the bandgap analysis. Furthermore, as can be seen from the HOMO orbital results, the adsorption between DES and Li / Co is Cl - It absorbs the surroundings, which matches the UV-vis spectrum.

[0079]

[0080] 2-3. Recovery Strategy

[0081] In the present invention, electrochemical deposition or precipitation was performed on the leaching solution to recover Co and separate metal ions.

[0082] In the present invention, Co was recovered using a 3-electrode system for the electrochemical deposition. After MIPEC-anode treatment, the LCO-DES solution was exposed to a constant current set to -4.5 mA for 1 hour for 180 minutes. The deposits plated on the electrode surface were characterized by SEM, and energy dispersive X-ray spectroscopy (EDS) results suggested that cobalt was recovered as Co3O4 or Co(OH)2.

[0083] In the present invention, for the precipitation, the leaching solution was diluted using Na2CO3 and then calcined to obtain Co3O4, which can be further processed to manufacture a lithium-ion battery. As shown in Figs. 3a and b, the product obtained from calcination exhibited uniform spherical particles in which Co and O were evenly distributed throughout the product. Furthermore, the powder obtained after calcining at 500°C for 6 hours showed Co3O4 signals in the XRD pattern (Fig. 3c), specifically appearing at 36.8, 44.5, 58.9, and 64.90, which are (311), (400), (511), and (440) phase peaks (PDF#43-1003). Fig. 3d shows Co2p with peaks at 779.5, 781.1, and 782.5 eV. 3 / 2 It shows the XPS curve fitting of the band, which also corresponds to the combination.

[0084]

[0085] 2-4. Applicability

[0086] To verify the applicability of the MIPEC-DES method according to the present invention to various cathode materials, in addition to layered LCO, the olivine cathode material LFP (chemical formula LiFePO4), the spinel cathode material LMO (chemical formula LiMn2O4), and the ternary cathode material NMC (chemical formula LiNi 1 / 3 Mn 1 / 3 Co 1 / 3This study was extended by observing the behavior regarding O2. Various cathode materials were exposed to the MIPEC-DES system for 180 minutes, and it was observed that the MIPEC-DES method exhibited good performance for all three types of cathode materials (Figs. 4a-c). For all major elements in LFP and LMO, and for Li in NMC, the leaching efficiency reached nearly 80% within 120 minutes. The 180-minute leaching efficiencies for Li, Fe, and P in LFP were 87.3%, 100%, and 84.0%, respectively; for Li and Mn in LMO, it was 100%; and for Li, Co, Ni, and Mn in NMC, it was 99.4%, 56.5%, 100%, and 51.2%, respectively. Furthermore, the feasibility of the MIPEC-DES method for actual battery electrode recycling applications was also tested on NMC black mass. The 180-minute leaching efficiencies of Li, Co, Ni, and Mn on NMC black mass were 69.8%, 52.7%, 85.6%, and 60.7%, respectively (Fig. 4d). The decrease in leaching efficiency is presumed to have been caused by impurities introduced due to decomposition. The excellent performance of MIPEC-DES demonstrated advantages, including applicability to major common cathode materials on the market.

[0087]

[0088] 2-5. Conclusion

[0089] As such, it has been demonstrated that it is possible to recycle important metals from waste LIBs by utilizing microplasma electrochemistry and a DES reaction medium according to the present invention.

[0090] More specifically, the leaching efficiencies of Li and Co from the LCO cathode material were up to 100% and 91.4%, respectively, within 180 minutes at room temperature. The above mechanism involves the reduction of EG during MIPEC treatment to produce superoxide (·O2 - It has been verified that it can generate ) and additionally generate H2O2. ·O2 -Both and H2O2 can reduce insoluble Co(III) to soluble Co(II) and improve leaching ability.

[0091] In addition, the MIPEC-DES method according to the present invention has demonstrated excellent universality and efficiency for other binary batteries (LMO and LFP) and ternary batteries (NMC and NMC black mass) at room temperature. Furthermore, in addition to reporting the dissolution of the cathode material, a complete recovery process has been demonstrated in which the dissolved ions are precipitated and the obtained solid is calcined to recover the metal into a useful product.

[0092] In conclusion, the MIPEC-DES method according to the present invention offers promising prospects for battery utilization and recycling in terms of economic feasibility, environmental impact, technology, and safety, and provides notable advantages of environmental friendliness, high efficiency, and excellent commonality for LIB recycling.

[0093] From the foregoing description, those skilled in the art to which the present invention pertains will understand that the present invention may be implemented in other specific forms without altering its technical concept or essential features. In this regard, the embodiments described above should be understood as illustrative in all respects and not restrictive. The scope of the present invention should be interpreted as including all modifications or variations derived from the meaning and scope of the claims set forth below and their equivalents, rather than from the detailed description above.

Claims

1. A microplasma electrochemical method for recycling spent lithium-ion battery cathodes comprising the following steps: (a) a step of mixing spent lithium-ion battery cathode material with a deep eutectic solvent (DES) and leaching important metals using microplasma electrochemistry (MIPEC); and (b) A step of recovering important metals from the leaching solution obtained in step (a) above.

2. A method according to claim 1, wherein in step (a), the waste lithium-ion battery cathode material is selected from the group consisting of lithium cobalt oxide (LCO), lithium manganese oxide (LMO), lithium iron phosphate (LFP), lithium nickel manganese cobalt oxide (NMC), and NMC black mass.

3. A method according to claim 1, wherein in step (a), the eutectic solvent is selected from the group consisting of choline chloride (ChCl)-glycerol, ChCl-p-toluenesulfonic acid (pTSA), ChCl-oxalic acid, ChCl-acetic acid, ChCl-malonic acid, ChCl-ethylene glycol, and ChCl-urea.

4. A method according to claim 1, wherein the step of leaching an important metal using a microplasma electrochemical method in step (a) is performed for 0.5 to 4 hours under conditions of room temperature and atmospheric pressure.

5. A method according to claim 1, wherein in step (a), the microplasma electrochemistry is performed using a microplasma anode working electrode made of a conductive capillary having a hollow structure, and a mesh-type counter electrode made of a conductive metal selected from the group consisting of platinum, molybdenum, tungsten, copper, silver, and zinc.

6. A method according to claim 1, wherein in step (a), the important metal is selected from the group consisting of lithium, cobalt, nickel, manganese, iron, phosphorus, sodium, aluminum, copper, and carbon.

7. A method according to claim 1, wherein step (b) is performed using electrochemical deposition or precipitation.