Anti-pollution coating technique based on low-temperature process
A low-temperature coating process using a cross-linked PDMS derivative and organic solvent addresses the challenge of achieving durable water and oil repellency on heat-sensitive plastics, ensuring effective adhesion and preventing thermal deformation.
Patent Information
- Application Number
- PCT/KR2026/001009
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-16
- Filing Date
- 2026-01-16
- Publication Date
- 2026-11-19
AI Technical Summary
Plastics with low surface energy, such as PP and ABS, face challenges in achieving durable water and oil repellency due to low adhesion of fluorosilane-based coatings and require high-temperature processes that can deform heat-sensitive substrates.
A low-temperature coating method using a cross-linked PDMS derivative and an organic solvent, such as pentane, hexane, or heptane, applied in a specific ratio, effectively imparts water and oil repellency without complex pretreatment, adhering well to plastic substrates.
The method achieves durable water and oil repellency on plastics, ensuring strong adhesion and preventing thermal deformation, enhancing product performance and durability.
Smart Images

Figure KR2026001009_19112026_PF_FP_ABST
Abstract
Description
Low-temperature process-based anti-fouling coating technology
[0001] The present invention relates to a low-temperature process-based anti-fouling coating technology that can impart water-repellent and oil-repellent anti-fouling functions to heat-sensitive substrates, such as plastics, without deformation. The formed coating exhibits excellent resistance to water, oil, dust, biological contaminants, etc. The present invention includes a surface activation step and a step of depositing a functional coating layer at a low temperature. The method according to the present invention may be useful for indoor and outdoor home appliances, kitchen appliances, automobiles, motorcycles, aviation, aerospace, vapor recovery devices, vapor recovery facilities, pipes, hoods, hood components, etc.
[0002] Plastics are widely used across modern industries due to their various advantages, such as lightweight properties, ease of processing, and durability. However, most plastics have low surface energy or, due to specific chemical structures, are prone to wetting by liquids like water or oil. This can lead to various problems, including product contamination, corrosion, and functional degradation. For example, moisture penetration into electronic device housings can cause corrosion or malfunction of internal components, while automotive exterior parts may suffer damage to their appearance or performance degradation due to contamination by rainwater or oil. In the case of medical devices, surface contamination increases the risk of infection, and in food packaging, it can lead to spoilage of contents or a decline in the functionality of the packaging itself. Therefore, imparting hydrophobicity and oleophobicity to plastic substrates is a critical technical challenge for improving product performance, durability, reliability, and user convenience.
[0003] Water and oil repellency on a surface is determined by the relationship between the surface energy of the coated substrate and the surface tension of the liquid in contact. For a liquid to remain in droplet form without wetting the surface, the surface energy of the substrate must be significantly lower than the surface tension of the liquid. To quantitatively evaluate the water and oil repellency performance of a coating, the contact angle and contact angle hysteresis are primarily measured. The contact angle is the angle formed between a liquid droplet placed on a solid surface and the surface, and it is the most fundamental indicator of surface wettability. A larger contact angle means that it is more difficult for the liquid to wet the surface; generally, a contact angle of 90° or greater for water is classified as hydrophobic, and 150° or greater as superhydrophobic. Similarly, a high contact angle for oil is considered to indicate excellent oleophobic properties. The contact angle hysteresis refers to the minimum angle at which a liquid droplet begins to slide on an inclined surface. A low contact hysteresis angle indicates that liquid droplets do not adhere well to the surface and can be easily removed, which is closely related to self-cleaning properties.
[0004] Polypropylene (PP) is a nonpolar polymer with no polar groups in its molecular structure and has very low surface energy. As a result, liquid coating agents do not wet the surface well, and the adhesion is very weak. In addition, due to its crystalline or semicrystalline characteristics, solvent penetration is difficult, which is disadvantageous for forming an adhesion mechanism, and low molecular weight substances or additives may leach out from the surface, forming a weak boundary layer.
[0005] ABS (Acrylonitrile Butadiene Styrene) is an amorphous terpolymer with generally low surface energy. Although it offers better adhesion properties than polyolefins, surface treatment is recommended for applications where durability is critical.
[0006] Fluorosilane-based coating agents are known to impart water and oil repellency, but they are known to present challenges in ensuring durability due to their low reactivity with the substrate and pose environmental pollution issues. To ensure durability, binder / pretreatment processes, complex substrate surface modifications, or high sintering temperatures are required. For a coating agent to effectively wet the substrate surface and form strong adhesion, the surface energy of the substrate must generally be higher than or similar to the surface tension of the coating solution (or melt). Directly applying fluorosilane-based coating agents with low surface energy to plastics with low surface energy, particularly PP or ABS, violates this principle, making it very difficult to secure adhesion.
[0007] Accordingly, the inventors discovered that a fluorine-free silane-based coating agent (Chemical Formula 1) adheres well to a plastic substrate through a low-temperature coating process without complex pretreatment or surface modification, thereby imparting water repellency and oil repellency, and completed the present invention.
[0008] The object of the present invention is to provide a coating composition for imparting oil-repellent and water-repellent properties to the surface of a plastic substrate.
[0009] Another objective of the present invention is to provide a plastic substrate coated with the coating composition.
[0010] Another objective of the present invention is to provide a low-temperature coating method for imparting oil-repellent and water-repellent properties to the surface of a plastic substrate.
[0011] In order to achieve the above objective,
[0012] The present invention is,
[0013] A cross-linked PDMS (Polydimethylsiloxane) derivative represented by Chemical Formula 1; and
[0014] Includes one organic solvent selected from pentane, hexane, heptane, and octane;
[0015] A composition comprising 0.01 to 0.1 parts by weight of a cross-linked PDMS (Polydimethylsiloxane) derivative represented by the above chemical formula 1, based on 1 part by weight of an organic solvent,
[0016] A coating composition for imparting oil-repellent and water-repellent properties to the surface of a plastic substrate is provided.
[0017] [Chemical Formula 1]
[0018]
[0019] (In the above Chemical Formula 1, x and y are each integers from 1 to 30, preferably integers from 1 to 15, and more preferably integers from 1 to 10.)
[0020]
[0021] In addition, the present invention provides a plastic substrate coated with a coating composition for imparting oil-repellent and water-repellent properties.
[0022]
[0023] Furthermore, the present invention,
[0024] A step of coating a plastic substrate with the coating composition of claim 1 (Step 1); and
[0025] A step of curing at 60-90℃ for 10-100 minutes (Step 2); comprising
[0026] A low-temperature coating method is provided to impart oil-repellent and water-repellent properties to the surface of a plastic substrate.
[0027]
[0028] The coating composition according to the present invention can impart water repellency and oil repellency to a plastic substrate by using a cross-linked PDMS derivative represented by Formula 1 and an organic solvent in a specific mixing ratio, and can be useful for indoor and outdoor home appliances, kitchen products, automobiles, motorcycles, aviation, aerospace, oil vapor recovery devices, oil vapor recovery equipment, pipes, hoods, hood parts, etc.
[0029] Figure 1 shows the results of summarizing the water contact angle measurements of the coated PP of the example.
[0030] Figure 2 shows the results of summarizing the water contact hysteresis angle measurements of the coated PP of the example.
[0031] Figure 3 shows the results of summarizing the water contact angle measurements of the coated ABS of the example.
[0032] Figure 4 shows the results of summarizing the water contact hysteresis angle measurements of the coated ABS of the example.
[0033] Figure 5 shows the results of summarizing the oil contact angle measurements of the coated PP of the example.
[0034] Figure 6 shows the results of summarizing the oil contact history angle measurements of the coated PP of the example.
[0035] Figure 7 shows the results of summarizing the contact angle measurements of the coated ABS oil of the example.
[0036] Figure 8 shows the results of summarizing the oil contact history angle measurements of the coated ABS of the example.
[0037] The present invention is,
[0038] A cross-linked PDMS (Polydimethylsiloxane) derivative represented by Chemical Formula 1; and
[0039] Includes one organic solvent selected from pentane, hexane, heptane, and octane;
[0040] A composition comprising 0.01 to 0.1 parts by weight of a cross-linked PDMS (Polydimethylsiloxane) derivative represented by the above chemical formula 1, based on 1 part by weight of an organic solvent,
[0041] A coating composition for imparting oil-repellent and water-repellent properties to the surface of a plastic substrate is provided.
[0042] [Chemical Formula 1]
[0043]
[0044] (In the above Chemical Formula 1, x and y are each integers from 1 to 30, preferably integers from 1 to 15, and more preferably integers from 1 to 10.)
[0045]
[0046] Based on 1 part by weight of the above organic solvent, 0.01-0.1 parts by weight of a crosslinked PDMS (Polydimethylsiloxane) derivative represented by Chemical Formula 1, preferably 0.02-0.1 parts by weight, 0.03-0.1 parts by weight, 0.04-0.1 parts by weight, or 0.05-0.1 parts by weight may be included.
[0047] If the content of the cross-linked PDMS derivative represented by the above chemical formula 1 falls outside the above range, there may be a problem with reduced oil and water repellency or insufficient uniformity of the coating.
[0048]
[0049] The coating composition according to the present invention is characterized by not including a PDMS (Polydimethylsiloxane) derivative represented by the following chemical formula 2.
[0050] [Chemical Formula 2]
[0051]
[0052] (In the above Chemical Formula 2, m is an integer from 1 to 100, preferably an integer from 1 to 80, and more preferably an integer from 1 to 60.)
[0053]
[0054] The coating composition according to the present invention may be used by methods such as drop coating, dip coating, and spin coating, but is not limited thereto.
[0055]
[0056] Among the above organic solvents, hexane was used as an example in the present invention, but pentane, heptane, and octane can also be used.
[0057]
[0058] The plastic substrate includes PP (Polypropylene), ABS (Acrylonitrile Butadiene Styrene), PC (Polycarbonate), PC / ABS alloy, HIPS (High Impact Polystyrene), PBT (Polybutylene Terephthalate), PPO (Polyphenylene Oxide), POM (Polyoxymethylene), PPA (Polyphthalamide), PET (Polyethylene Terephthalate), Plastics such as PU (Polyurethane), PA (Polyamide), HDPE (High-Density Polyethylene), PEEK (Polyetheretherketone), PEI (Polyetherimide), PPS (Polyphenylene Sulfide), PTFE (Polytetrafluoroethylene), PI (Polyimide), and PMI (Polymethacrylimide) can be used.
[0059]
[0060] In addition, the present invention provides a plastic substrate coated with a coating composition for imparting oil-repellent and water-repellent properties.
[0061] The coating composition according to the present invention can be used in the electronic and optoelectronic industries, such as indoor and outdoor home appliances, insulation coverings for wires and cables, printed circuit boards, semiconductor manufacturing process components, display panel protective films, connectors, sockets, etc.
[0062] It may also be used in the automotive and aerospace industries, such as automotive interior, exterior, and engine room parts, aircraft and spacecraft parts, etc., and
[0063] It can be used in the medical and healthcare device industry, such as catheters, guidewires, endoscopes, surgical instruments, implants, drug delivery systems, medical device housings, etc., and
[0064] It can be used in the food processing industry, such as cooking equipment, food processing facilities, vapor recovery devices, hoods, etc., and
[0065] It may also be used in the textile and clothing industry for outdoor clothing, sportswear, workwear, carpets, etc.
[0066] It can be used in the construction and building industries, such as for building exterior materials and roofing materials, and
[0067] It may also be used in the chemical industry for pipes, tanks, valves, etc., and
[0068] It can be used in the energy industry, such as wind turbine components, solar panels, battery components, and small nuclear reactors, and
[0069] It can be used in household goods, various industrial machinery, parts protection coatings, packaging industries, and more.
[0070]
[0071] Furthermore, the present invention,
[0072] A step of coating a plastic substrate with the coating composition of claim 1 (Step 1); and
[0073] A step of curing at 60-90℃ for 10-100 minutes (Step 2); comprising
[0074] A low-temperature coating method is provided to impart oil-repellent and water-repellent properties to the surface of a plastic substrate.
[0075]
[0076] In one embodiment of the present invention, when PP (Polypropylene) is used as the plastic substrate, the coating agent is used in a weight ratio of organic solvent:Chemical Formula 1 = 1:0.05-0.1 and can be cured at 60-90°C (preferably 70-80°C) for 10 to 50 minutes.
[0077] In another aspect of the present invention, when ABS (Acrylonitrile Butadiene Styrene) is used as the plastic substrate, the coating agent is used in a weight ratio of organic solvent:Chemical Formula 1 = 1:0.05-0.1, and can be cured at 60-90°C (preferably 60-65°C) for 10 to 50 minutes (preferably 30 to 50 minutes).
[0078] The present invention will be explained in more detail below through the following examples. However, the following examples are merely illustrative of the present invention, and the scope of the present invention is not limited by the following examples.
[0079]
[0080] <Example> Preparation of a plastic substrate coated with a water-repellent and oil-repellent coating agent
[0081] As an example of a plastic substrate, PP (Polypropylene) or ABS (Acrylonitrile Butadiene Styrene) was used as the substrate to be coated. Since the heat distortion temperature of PP is 80-110°C and the heat distortion temperature of ABS is 85-105°C, high-temperature coating cannot be applied, so low-temperature coating must be applied.
[0082] Specifically, as a coating agent, a hexane solvent and SYLGARD 184 Silicon Elastomer Curing Agent (manufacturer: Dow Chemical Company), a cross-linked PDMS derivative represented by Chemical Formula 1, were mixed in a weight ratio of 1:0.01, 1:0.05, or 1:0.1. A PP or ABS substrate was coated onto the coating agent by a dip coating method.
[0083] Next, the dip-coated substrate from above was heat-treated at a low temperature in an oven to complete the curing. The heat treatment temperature was 60, 70, 80, 90, or 100°C, and the heat treatment time was 10, 30, 50, or 100 minutes.
[0084] [Chemical Formula 1: Curing agent]
[0085]
[0086] In the above chemical formula 1, x and y are integers from 1 to 30, respectively.
[0087]
[0088] <Comparative Example 1> Preparation of bare PP (Polypropylene) substrate
[0089] A PP (Polypropylene) substrate that was not treated with a coating agent was prepared as Comparative Example 1.
[0090]
[0091] <Comparative Example 2> Preparation of bare ABS (Acrylonitrile Butadiene Styrene) substrate
[0092] An ABS (Acrylonitrile Butadiene Styrene) substrate that was not treated with a coating agent was prepared as Comparative Example 2.
[0093]
[0094] <Comparative Example 3> Preparation of a PP substrate coated with a coating agent having a composition of Hexane:(Base+Curing agent) = 1:0.05
[0095] Mixture A was prepared in a weight ratio of Base (Chemical Formula 2):Curing agent (Chemical Formula 1) = 10:1, and then a coating agent with a composition of hexane:mixture A = 1:0.05 was prepared and coated on a PP substrate in the same manner as in the example. At this time, the curing treatment conditions were 70°C for 30 minutes.
[0096]
[0097] <Comparative Example 4> Preparation of an ABS substrate coated with a coating agent having a composition of Hexane:(Base+Curing agent) = 1:(0.05+0.05)
[0098] Mixture A was prepared in a weight ratio of Base (Chemical Formula 2):Curing agent (Chemical Formula 1) = 10:1, and then a coating agent with a composition of hexane:mixture A = 1:0.05 was prepared and coated on a PP substrate in the same manner as in the example. At this time, the curing treatment conditions were 60°C for 30 minutes.
[0099]
[0100] <Experimental Example 1> Evaluation of Water Repellency and Coating Curing
[0101] First, to evaluate water repellency, water (purified water) was dropped onto the surfaces of the examples and comparative examples, respectively, and the contact angle and contact history angle were evaluated.
[0102] Next, to determine if any uncured residual coating material remained on the surface after the coating curing treatment, the time required to wash away the dripping coating material was measured by spraying approximately 0.8 mL of water per second. In other words, the less uncured residual coating material remains on the surface, the shorter the washing time.
[0103] The results of measuring the contact angle, contact history angle, and cleaning time are shown in Tables 1 to 6 below.
[0104] Here, 'contact angle hysteresis' refers to the angle at which water or oil begins to flow down after placing a sample on a stage of a device capable of finely adjusting the tilt, dropping water or oil onto the sample, and gradually applying a tilt to the stage. In other words, the lower the contact angle hysteresis, the better the water / oil repellency, allowing for the expectation of a self-cleaning effect. For example, if the contact angle hysteresis is 1°, water or oil flows down even when the sample is tilted only 1°, whereas if the contact angle hysteresis is 90°, water or oil does not flow down even when the sample is held upright at 90°.
[0105]
[0106]
[0107]
[0108]
[0109]
[0110]
[0111]
[0112]
[0113]
[0114]
[0115]
[0116]
[0117]
[0118] In Tables 1 to 12 above,
[0119] The measured water contact angle and contact hysteresis angle of the coated PP of the example are shown in FIGS. 1 and FIGS. 2, respectively.
[0120] The measured water contact angle and contact hysteresis angle of the coated ABS of the example are shown in FIGS. 3 and FIGS. 4, respectively.
[0121] The measured oil contact angle and contact hysteresis angle of the coated PP of the example are shown in FIGS. 5 and FIGS. 6, respectively.
[0122] The measured contact angle and contact hysteresis angle of the coated ABS oil of the example are shown in Figures 7 and 8, respectively.
[0123]
[0124] The optimal coating conditions for imparting water repellency to the PP substrate were confirmed from the above Figures 1 and 2.
[0125] Specifically, for the PP substrate, using a coating agent composition in the range of hexane:Chemical Formula 1 = 1:0.05-0.1 showed a tendency for excellent water repellency. While the 1:0.01 coating agent composition showed good results in water contact angle under some low-temperature coating conditions, it did not show a significant improvement in water repellency compared to the bare PP substrate (Comparative Example 1) in water contact hysteresis angle. Overall, it was found that low-temperature coating conditions preferably involve treatment at 60-90°C for 10 to 50 minutes. Meanwhile, at 100°C, thermal deformation of the PP substrate occurred as the treatment time increased. On the other hand, in the case of Comparative Example 3, the water contact angle was 102.54 ± 1.27°, which was a negligible effect on improving water repellency compared to the bare PP substrate (Comparative Example 1, 101.89°), and the water contact hysteresis angle was 22.78 ± 0.83°, which was a result showing a decrease in water repellency compared to the bare PP substrate (Comparative Example 1, 19.61°).
[0126]
[0127] The optimal coating conditions for imparting water repellency to the ABS substrate were confirmed from the above Figures 3 and 4.
[0128] Specifically, for the ABS substrate, using a coating agent composition in the range of hexane:Chemical Formula 1 = 1:0.05-0.1 showed a tendency for excellent water repellency. The 1:0.01 coating agent composition showed good results in water contact angle and water contact hysteresis angle under some low-temperature coating conditions, but under most low-temperature coating conditions, no significant improvement in water repellency was observed compared to the bare ABS substrate (Comparative Example 2). Overall, it was found that low-temperature coating conditions preferably involve treatment at 60-90°C for 10 to 50 minutes. Meanwhile, at 100°C, thermal deformation of the ABS substrate occurred as the treatment time increased. On the other hand, in the case of Comparative Example 4, the water contact angle was 95.74 ± 1.31°, which was lower than that of the bare ABS substrate (Comparative Example 2, 96.56°), and the water contact hysteresis angle was 21.48 ± 1.13°, which was a negligible effect of improving water repellency compared to the bare ABS substrate (Comparative Example 2, 21.73°).
[0129]
[0130] The optimal coating conditions for imparting oil repellency to the PP substrate were confirmed from the above Figures 5 and 6.
[0131] Specifically, for the PP substrate, using a coating agent composition in the range of hexane:Chemical Formula 1 = 1:0.05-0.1 showed a tendency for excellent oil repellency, and while the 1:0.01 coating agent composition showed good results in oil contact hysteresis angle under some low-temperature coating conditions, no significant improvement in oil repellency was observed compared to the bare PP substrate (Comparative Example 1) under most low-temperature coating conditions. Overall, it was found that low-temperature coating conditions preferably involve treatment at 70-80°C for 10 to 50 minutes. Meanwhile, at 100°C, thermal deformation of the PP substrate occurred as the treatment time increased. On the other hand, in the case of Comparative Example 3, the oil contact angle was 27.04 ± 0.67°, which was a negligible effect on improving oil repellency compared to the bare PP substrate (Comparative Example 1, 26.59°), and the oil contact hysteresis angle was 27.98 ± 0.73°, which was a result showing a decrease in oil repellency compared to the bare PP substrate (Comparative Example 1, 26.21°).
[0132]
[0133] The optimal coating conditions for imparting oil repellency to the ABS substrate were confirmed from the above Figures 7 and 8.
[0134] Specifically, in the case of the ABS substrate, using a coating agent composition in the range of hexane:Chemical Formula 1 = 1:0.05-0.1 showed a tendency for excellent oil repellency, while the 1:0.01 coating agent composition did not show a significant improvement in oil repellency compared to the bare ABS substrate (Comparative Example 2) in terms of oil contact hysteresis angle. Overall, it was found that low-temperature coating conditions were preferably treated at 60-65°C for 30 to 100 minutes. Meanwhile, at 100°C, thermal deformation of the ABS substrate occurred as the treatment time increased. On the other hand, in the case of Comparative Example 4, the oil contact angle was 28.11 ± 1.26°, which was lower than that of the bare ABS substrate (Comparative Example 2, 28.81°), and the oil contact hysteresis angle was 20.21 ± 0.93°, which was a negligible improvement in water repellency compared to the bare ABS substrate (Comparative Example 2, 20.83°).
[0135]
[0136] Overall, it was confirmed that the optimal coating agent composition for imparting water and oil repellency is preferably mixed in a weight ratio of hexane:Chemical Formula 1 = 1:0.05-0.1.
[0137]
[0138] The present invention has been described above with reference to its preferred embodiments. Those skilled in the art will understand that the present invention may be embodied in modified forms without departing from the essential characteristics of the invention. Therefore, the disclosed embodiments should be considered in an illustrative rather than a restrictive sense. The scope of the invention is defined not by the foregoing description but particularly by the claims, and all variations within the equivalent scope should be interpreted as being included in the invention.
[0139] The coating composition according to the present invention can impart water repellency and oil repellency to a plastic substrate by using a cross-linked PDMS derivative represented by Formula 1 and an organic solvent in a specific mixing ratio, and can be useful for indoor and outdoor home appliances, kitchen products, automobiles, motorcycles, aviation, aerospace, oil vapor recovery devices, oil vapor recovery equipment, pipes, hoods, hood parts, etc.
Claims
1. A cross-linked PDMS (Polydimethylsiloxane) derivative represented by Chemical Formula 1; and Includes one organic solvent selected from pentane, hexane, heptane, and octane; A composition comprising 0.01 to 0.1 parts by weight of a cross-linked PDMS (Polydimethylsiloxane) derivative represented by the above chemical formula 1, based on 1 part by weight of an organic solvent, Coating composition for imparting oil-repellent and water-repellent properties to the surface of a plastic substrate. [Chemical Formula 1] (In Chemical Formula 1 above, x and y are integers from 1 to 30, respectively.) 2. In Paragraph 1, A coating composition for imparting oil-repellent and water-repellent properties to the surface of a plastic substrate, comprising 0.02 to 0.1 parts by weight of a cross-linked PDMS (Polydimethylsiloxane) derivative represented by the above chemical formula 1, based on 1 part by weight of an organic solvent.
3. In Paragraph 2, A coating composition for imparting oil-repellent and water-repellent properties to the surface of a plastic substrate, comprising 0.03 to 0.1 parts by weight of a cross-linked PDMS (Polydimethylsiloxane) derivative represented by the above chemical formula 1, based on 1 part by weight of an organic solvent.
4. In Paragraph 3, A coating composition for imparting oil-repellent and water-repellent properties to the surface of a plastic substrate, comprising 0.04 to 0.1 parts by weight of a cross-linked PDMS (Polydimethylsiloxane) derivative represented by the above chemical formula 1, based on 1 part by weight of an organic solvent.
5. In Paragraph 4, A coating composition for imparting oil-repellent and water-repellent properties to the surface of a plastic substrate, comprising 0.05 to 0.1 parts by weight of a cross-linked PDMS (Polydimethylsiloxane) derivative represented by the above chemical formula 1, based on 1 part by weight of an organic solvent.
6. In Paragraph 1, A coating composition for imparting oil-repellent and water-repellent properties to a plastic substrate surface, which does not contain a PDMS (Polydimethylsiloxane) derivative represented by the following chemical formula 2. [Chemical Formula 2] (In Chemical Formula 2 above, m is an integer from 1 to 100.) 7. In Paragraph 1, A coating composition for imparting oil-repellent and water-repellent properties to a plastic substrate surface, wherein the organic solvent is hexane.
8. In Paragraph 1, A coating composition for imparting oil-repellent and water-repellent properties to the surface of a plastic substrate, wherein the plastic substrate is any one selected from the group consisting of PP (Polypropylene), ABS (Acrylonitrile Butadiene Styrene), PC (Polycarbonate), PC / ABS alloy, HIPS (High Impact Polystyrene), PBT (Polybutylene Terephthalate), PPO (Polyphenylene Oxide), POM (Polyoxymethylene), PPA (Polyphthalamide), PET (Polyethylene Terephthalate), PU (Polyurethane), PA (Polyamide), HDPE (High-Density Polyethylene), PEEK (Polyetheretherketone), PEI (Polyetherimide), PPS (Polyphenylene Sulfide), PTFE (Polytetrafluoroethylene), PI (Polyimide), and PMI (Polymethacrylimide).
9. A plastic substrate coated with the coating composition of claim 1, imparted with oil-repellent and water-repellent properties.
10. A step of coating a plastic substrate with the coating composition of claim 1 (Step 1); and A step of curing at 60-90℃ for 10-100 minutes (Step 2); comprising Low-temperature coating method for imparting oil-repellent and water-repellent properties to the surface of a plastic substrate.