Positive electrode active material for lithium secondary battery, method for preparing same, positive electrode including same, and lithium secondary battery including same

A single-crystal cathode active material with 80-98% nickel and controlled thermal decomposition characteristics, manufactured via multi-step heat treatment, improves structural stability and capacity retention in lithium secondary batteries.

WO2026240313A1PCT designated stage Publication Date: 2026-11-19NINGBO RONBAY LITHIUM BATTERY MATERIAL CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2026/001951
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-12
Filing Date
2026-02-03
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Lithium secondary batteries face issues with reduced capacity and capacity retention due to microcracks caused by poor structural stability in polycrystalline cathode active materials, especially when nickel content is increased.

Method used

A single-crystal positive electrode active material with a nickel content of 80-98 mol% and specific thermal decomposition characteristics, manufactured through a multi-step heat treatment process, is developed to enhance structural stability and capacity retention.

Benefits of technology

The single-crystal cathode active material exhibits excellent structural stability and high capacity retention, addressing the limitations of polycrystalline materials by maintaining performance even with higher nickel content.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2026001951_19112026_PF_FP_ABST
    Figure KR2026001951_19112026_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed are a positive electrode active material for a lithium secondary battery, a method for preparing same, a positive electrode including same, and a lithium secondary battery including same. The positive electrode active material for a lithium secondary battery according to an embodiment may be a single-crystal positive electrode active material composed of single particles, wherein the nickel content on the basis of the components other than lithium and oxygen is more than 80 mol% and less than 98 mol%, and the thermogravimetric analysis (TGA) results satisfy Expression 1: [Equation 1] 0.35 ≤ A / B ≤ 0.80. Here, A is △W300(wt%)·300(K) / Tonset(K) when analyzed by TGA in an oxygen (O2) atmosphere, B is △W300(wt%)·300(K) / Tonset(K) when analyzed by TGA in a nitrogen (N2) or argon (Ar) atmosphere, Tonset(K) is onset Kelvin temperature (K) in a first stage structural breakdown region of the positive electrode active material, △W300(wt%) = Wonset (wt%) - Wonset+300K(wt%), Wonset(wt%) is the wt% at Tonset(K) relative to the initial weight, and Wonset+300K(wt%) is the wt% at Tonset(K) + 300(K) relative to the initial weight.
Need to check novelty before this filing date? Find Prior Art

Description

A positive electrode active material for a lithium secondary battery, a method for manufacturing the same, a positive electrode including the same, and a lithium secondary battery including the same

[0001] The present invention relates to a positive electrode active material for a lithium secondary battery, a method for manufacturing the same, a positive electrode including the same, and a lithium secondary battery including the same. More specifically, the invention relates to a positive electrode active material for a lithium secondary battery having excellent structural stability and high capacity and capacity retention rate in a battery, wherein the single-crystal positive electrode active material composed of a single particle has specific thermal decomposition characteristics, a method for manufacturing the same, a positive electrode including the same, and a lithium secondary battery including the same.

[0002] Various cathode active materials are used in lithium secondary batteries applied in fields such as electric vehicles (EVs) and energy storage systems (ESS). Among these cathode active materials for lithium secondary batteries, lithium composite metal oxides containing nickel as a main component and one or more components from cobalt, manganese, and aluminum are widely used as cathode active materials.

[0003] In the case of a polycrystalline (multi-particle) cathode active material composed of multiple primary particles, the above lithium composite metal oxide needs to address the problem of reduced capacity and capacity retention rate caused by microcracks occurring during the charging and discharging process in the battery, which is attributed to poor structural stability. Additionally, in the case of a single-crystal cathode active material composed of a single particle that has improved the structural stability problem of the polycrystalline cathode active material, it is necessary to further improve structural stability as the nickel content is further increased to enhance capacity.

[0004] (Prior Art Literature)

[0005] (Patent Document 1) Published Patent Application No. 10-2019-0069073 (June 19, 2019)

[0006] (Patent Document 2) Published Patent Application No. 10-2019-0046425 (May 7, 2019)

[0007] The problem that the present invention aims to solve is to provide a cathode active material for a lithium secondary battery having excellent structural stability and high capacity and capacity retention rate in a battery, a method for manufacturing the same, a cathode including the same, and a lithium secondary battery including the same.

[0008] A first aspect of the present invention for solving the above problem provides a positive electrode active material for a lithium secondary battery. This positive electrode active material is a single-crystal positive electrode active material composed of a single particle, wherein the nickel content among the remaining components excluding lithium and oxygen is greater than 80 mol% and less than 98 mol%, and the thermogravimetric analysis (TGA) results satisfy the following Equation 1:

[0009] [Mathematical Formula 1] 0.35 ≤ A / B ≤ 0.80.

[0010] Here, A is △W when analyzing using oxygen (O2) as the atmosphere gas in TGA. 300 (wt%)·300(K) / T onset (K) and B is △W when analyzing using nitrogen (N2) or argon (Ar) as the atmosphere gas in TGA. 300 (wt%)·300(K) / T onset (K) is.

[0011] Here, T onset (K) is the onset Kelvin temperature (K) in the first stage structural collapse region of the cathode active material, and △W 300 (wt%) = W onset (wt%) - W onset+300K (wt%) and W onset (wt%) is T relative to initial weight onset It is the weight percentage (wt%) at (K), and W onset+300K (wt%) is T relative to initial weight onset It is the weight percentage (wt%) at (K) + 300(K).

[0012] In this aspect, the nickel content may be greater than 90 mol% and less than 98 mol%.

[0013] In one embodiment, the positive electrode active material may include a lithium complex transition metal oxide having nickel and one or more components selected from the group consisting of cobalt, manganese, and aluminum.

[0014] A second aspect of the present invention provides a method for manufacturing a positive electrode active material for a lithium secondary battery. The method may include, as steps for manufacturing a positive electrode active material for a lithium secondary battery, a) a precursor manufacturing step for manufacturing a precursor for a positive electrode active material, b) a step of manufacturing a primary positive electrode active material by performing a primary heat treatment on a material containing the manufactured precursor, and c) a step of manufacturing a secondary positive electrode active material by performing a secondary heat treatment on a material containing the primary positive electrode active material.

[0015] In one embodiment, after step c), step d) may further include a step of preparing a third positive active material by heat-treating a material containing a second positive active material.

[0016] A third aspect of the present invention provides a positive electrode for a lithium secondary battery comprising the positive electrode active material of the first aspect.

[0017] A fourth aspect of the present invention provides a lithium secondary battery comprising a positive electrode of the third aspect.

[0018] According to embodiments of the present invention, a single-crystal cathode active material composed of a single particle has specific thermal decomposition characteristics, thereby providing a cathode active material for a lithium secondary battery that has excellent structural stability and high capacity and capacity retention rate in the battery.

[0019] In addition, a method can be provided to manufacture a cathode active material for a lithium secondary battery with excellent structural stability by making a single-crystal cathode active material composed of a single particle have specific thermal decomposition characteristics through stepwise heat treatment.

[0020] In addition, a positive electrode for a lithium secondary battery comprising the above positive electrode active material can be provided.

[0021] In addition, a lithium secondary battery with high capacity and capacity retention rate including the above-mentioned positive electrode can be provided.

[0022] Figures 1a to 1c are schematic diagrams for explaining TGA graphs.

[0023] Figure 2 shows △W of Equation 1. 300 (wt%) and T onset This is a schematic diagram to explain (K).

[0024] Figure 3 is a graph showing the correlation between A / B of Equation 1 and discharge capacity (mAh / g, @100 cycle).

[0025] Preferred embodiments of the present invention will be described below with reference to the attached drawings. Embodiments of the present invention may be modified in various different forms, and the scope of the present invention is not limited to the embodiments described below. Embodiments of the present invention are provided to more fully explain the present invention to those with average knowledge in the art. Accordingly, the shapes and sizes of elements in the drawings may be exaggerated for clearer explanation, and elements indicated by the same reference numerals in the drawings are the same elements. In the present invention, the expressions "first" or "second" do not imply order or importance, but are merely for distinguishing components.

[0026] The first aspect of the present invention provides a positive electrode active material for a lithium secondary battery. This positive electrode active material is a single-crystal positive electrode active material composed of a single particle, and the thermogravimetric analysis (TGA) results satisfy the following Equation 1. The positive electrode active material of this aspect has specific thermal decomposition characteristics, which can improve the capacity and capacity retention rate of a lithium secondary battery.

[0027] [Mathematical Formula 1] 0.35 ≤ A / B ≤ 0.80,

[0028] Here, A is △W when analyzing using oxygen (O2) as the atmosphere gas in TGA. 300 (wt%)·300(K) / Tonset (K) and B is △W when analyzing using nitrogen (N2) or argon (Ar) as the atmosphere gas in TGA. 300 (wt%)·300(K) / T onset (K) is.

[0029] Here, T onset (K) is the onset Kelvin temperature (K) in the first stage structural collapse region of the cathode active material, and △W 300 (wt%) = W onset (wt%) - W onset+300K (wt%) and W onset (wt%) is T relative to initial weight onset It is the weight percentage (wt%) at (K), and W onset+300K (wt%) is T relative to initial weight onset It is the weight percentage (wt%) at (K) + 300(K).

[0030] In one embodiment, the positive electrode active material may be a lithium composite metal oxide having nickel and comprising one or more components selected from the group consisting of cobalt, manganese, and aluminum.

[0031] The positive electrode active material may have a nickel content of more than 80 mol% and less than 98 mol% among the remaining components excluding lithium and oxygen. In other words, among the remaining components excluding lithium and oxygen, the nickel content may be more than 80 mol% and less than 98 mol% among the total components including the main component (e.g., one or more components among nickel, cobalt, manganese, and aluminum), the doping material, the coating material, and other additive materials.

[0032] Furthermore, in order to achieve a higher capacity in the cathode active material, the nickel content may be greater than 90 mol% and less than 98 mol%.

[0033] Thermogravimetric Analysis (TGA)

[0034] In the present invention, the TGA conditions for the positive electrode active material may be as follows.

[0035] ① Temperature range: Room temperature to 1,200℃

[0036] ② Heating rate: 5℃ / min

[0037] ③ Atmosphere gas: For A in Equation 1 - Oxygen (O2), for B in Equation 1 - Nitrogen (N2) or Argon (Ar)

[0038] ④ Gas supply flow rate: 20 mL / min

[0039] To explain the thermal decomposition characteristics of the cathode active material, a TGA graph for a typical lithium composite metal oxide cathode active material is shown in Figure 1a.

[0040] Referring to Fig. 1a, the temperature ranges in the TGA graph can be divided into I to IV.

[0041] In section I, the weight may decrease mainly because moisture adsorbed on the positive active material is removed.

[0042] In section II, the weight may decrease mainly due to the decomposition of lithium hydroxide formed on the surface of the positive electrode active material.

[0043] In section III, the weight may decrease mainly due to oxygen release caused by the first-stage structural collapse of the positive active material, and some may decrease due to carbon dioxide emission caused by the decomposition of lithium carbonate present on the surface of the positive active material.

[0044] In section IV, weight may decrease mainly due to oxygen release caused by the two-stage structural breakdown of the positive active material.

[0045] However, depending on the type of cathode active material, in the TGA graph up to 1,200°C, there may be cases where only the process of the first stage of structural decay of the cathode active material proceeds, as shown in Fig. 1b, and the temperature range is divided into I to III, or cases where more decay stages appear than in Fig. 1a, as shown in Fig. 1c, and the temperature range is divided into I to V.

[0046] The extent to which lithium carbonate on the surface of the positive electrode active material affects weight loss in the TGA graph can be explained as follows using Fig. 1a.

[0047] Assuming that the amount of lithium carbonate formed on the surface of the cathode active material is typically 5,000 ppm or less according to the titration method, and that the amount of lithium carbonate decomposed in section III of Fig. 1a is also 5,000 ppm or less, and considering that the weight loss ratio when lithium carbonate decomposes into lithium oxide while emitting carbon dioxide is approximately 60% and the temperature at which lithium carbonate decomposes is approximately 700 to 1,000°C, the weight loss due to the decomposition of lithium carbonate in section III can be expected to be approximately 0.3 wt% (5,000 ppm x 60%) or less. That is, considering that the difference between W11, which is the wt% at T11, the temperature at which the first stage of structural decay of the cathode active material begins in Figure 1a, and W21, which is the wt% at T21, the temperature at which the first stage of structural decay ends, is approximately 6 wt%, it can be estimated that among the 6 wt% weight loss in section III, the loss due to structural decay of the cathode active material is approximately 5.7 wt% (95% of the total 6 wt%) or more, and the loss due to decomposition of lithium carbonate is approximately 0.3 wt% (5% of the total 6 wt%) or less.

[0048] In summary, in the case of Fig. 1a, more than 95% of the weight loss in section III where the positive active material collapses is due to the collapse of the positive active material, and less than 5% is due to the decomposition of lithium carbonate present on the surface of the positive active material. Thus, the weight loss in the section where the positive active material collapses in TGA can be attributed to the release of oxygen due to the structural collapse of the positive active material itself.

[0049] Differences in TGA based on atmospheric gas

[0050] In the present invention, when an analysis of the cathode active material is performed according to the above TGA conditions, even for the same cathode active material, T in Equation 1 is relatively... when oxygen is used as the atmosphere gas compared to when nitrogen or argon is used. onset (K) is increasing and △W 300 (wt%) decreases, resulting in △W 300 (wt%)·300(K) / T onset We discovered the phenomenon of (K) becoming smaller and proposed this patent.

[0051] T in TGA depending on the atmosphere gas onset (K) and △W 300 The reason for the change in (wt%) is believed to be that the lithium composite metal oxide, which is the cathode active material of the present invention, is a metal oxide, i.e., contains oxygen elements in its constituent components, thus exhibiting excellent oxidation resistance, and that this property is more stable in oxygen gas compared to nitrogen or argon gas in terms of structural stability.

[0052] In TGA, when the atmosphere gas is oxygen and when it is nitrogen or argon, T onset (K) and △W 300 (wt%) changes, i.e., △W 300 (wt%)·300(K) / T onset (K) changes, and the degree of change varies depending on the cathode active materials. A / B in Equation 1 is expressed to reflect this difference in change, and Equation 1 was developed through the evaluation of the correlation between A / B in Equation 1 and the capacity characteristics in the battery.

[0053] The characteristics of the positive active material according to the range of mathematical formula 1 are described in detail below.

[0054] Overview of Mathematical Formula 1

[0055] [Mathematical Formula 1] 0.35 ≤ A / B ≤ 0.80,

[0056] Here, A is △W when analyzing using oxygen (O2) as the atmosphere gas in TGA.300 (wt%)·300(K) / T onset (K) and B is △W when analyzing using nitrogen (N2) or argon (Ar) as the atmosphere gas in TGA. 300 (wt%)·300(K) / T onset (K) is.

[0057] Here, T onset (K) is the onset Kelvin temperature (K) in the first stage structural collapse region of the cathode active material, and △W 300 (wt%) = W onset (wt%) - W onset+300K (wt%) and W onset (wt%) is T relative to initial weight onset It is the weight percentage (wt%) at (K), and W onset+300K (wt%) is T relative to initial weight onset It is the weight percentage (wt%) at (K) + 300(K).

[0058] Mathematical formula 1 reflects the following contents.

[0059] 1) △W in Equation 1 300 (wt%)·300(K) / T onset (K) is related to the structural stability of the positive electrode active material,

[0060] 2) In mathematical formula 1, A / B is related to the structural stability of the positive electrode active material,

[0061] 3) T onset When using the weight loss at a temperature increased by 300K starting from (K), better results can be obtained in terms of correlation with the electrochemical characteristics of the positive electrode active material.

[0062] 4) T onset When applying the temperature of (K) as Kelvin temperature (K) rather than Celsius temperature (°C), better results can be obtained in terms of correlation with the electrochemical properties of the positive electrode active material.

[0063] T for A and B in mathematical equation 1 onset(K) and △W 300 (wt%) is explained using Figure 2 as follows.

[0064] T in mathematical formula 1 onset (K) is the temperature at which the first stage of structural collapse of the positive active material begins, as shown in Fig. 2, and T relative to the initial weight onset wt% in (K) is W in Fig. 2 onset It corresponds to (wt%).

[0065] T in Fig. 2 onset (K) + 300K is T onset Representing a temperature increased by 300K from (K), and T relative to initial weight onset (K) The wt% at 300K is W in Fig. 2 onset+300K It corresponds to (wt%).

[0066] T in mathematical formula 1 onset (K) can be 773.15K (500℃) to 1173.15K (900℃).

[0067] △W of mathematical formula 1 300 (wt%) is W in Fig. 2 onset W relative to (wt%) onset+300K It represents the weight change of (wt%).

[0068] △W of mathematical formula 1 300 (wt%)·300(K) is T in Fig. 2 onset T in (K) onset Change in weight (△W) when increased to (K) + 300K 300 It reflects (wt%) and the temperature change amount (300K) together, and corresponds to the rectangular area in Fig. 2.

[0069] T11 to T13, which are the starting temperatures of section III in FIGS. 1a to 1c, and T in FIG. 2 onset (K) can be determined using the inflection point of the DTG (derivative TG) curve, which is the first derivative graph of the TGA graph.

[0070] Range of Mathematical Formula 1

[0071] In mathematical formula 1, when the A / B ratio of the positive active material is 0.35 to 0.80, the crystal structure of the positive active material is stable and the degree of deformation of the crystal structure is low, so excellent characteristics such as capacity and capacity retention rate in the battery can be exhibited.

[0072] The major factors affecting A / B in mathematical formula 1 may be the following cases.

[0073] 1) Heat treatment conditions for manufacturing the primary cathode active material of the present invention

[0074] 2) Doping conditions for manufacturing the primary cathode active material of the present invention

[0075] Specifically, in the case of 1) above, when manufacturing the primary cathode active material of the present invention, differences may occur in the crystal structure, crystallinity, density, and strength of the cathode active material depending on the heat treatment conditions (heating rate, maximum temperature, holding time at the maximum temperature, atmosphere gas), and such differences may affect A / B of Equation 1 of the secondary (or tertiary if necessary) cathode active material, which is the final cathode active material.

[0076] In addition, in case 2) above, when manufacturing the primary cathode active material of the present invention, there may be differences in the crystal structure, crystallinity, density, and strength of the cathode active material depending on the components and content of the doping material, and such differences may affect A / B of Equation 1 of the secondary (or tertiary if necessary) cathode active material, which is the final cathode active material.

[0077] In mathematical formula 1, A / B can be reduced by the following ① and ②.

[0078] ① Increase in maximum temperature and / or increase in holding time at maximum temperature under primary heat treatment conditions when manufacturing the primary cathode active material of the present invention,

[0079] ② Increase in the mixing ratio of the doping material relative to the anode active material when manufacturing the primary anode active material of the present invention.

[0080] As the maximum temperature and / or the holding time at the maximum temperature in ① above increases, and as the mixing ratio of the doping material in ② above increases, A / B in Equation 1 can become smaller.

[0081] According to ① and / or ② above, the positive active material may have an A / B of Equation 1 of less than 0.35. This positive active material is a case where the layered structure, which is the crystal structure of the positive active material, collapses according to ① above and / or the layered structure is deformed according to ② above. This causes problems with the movement of lithium ions within the positive active material and ultimately may result in a decrease in capacity and capacity retention rate in the battery.

[0082] In mathematical formula 1, A / B can be increased by the following ①' and ②'.

[0083] ① Reduction of maximum temperature and / or reduction of holding time at maximum temperature under primary heat treatment conditions when manufacturing the primary cathode active material of the present invention

[0084] ② Reduction in the mixing ratio of doping material relative to the cathode active material when manufacturing the primary cathode active material of the present invention.

[0085] As the maximum temperature and / or the holding time at the maximum temperature in ①' above gradually decreases, and as the mixing ratio of the doping material in ②' above gradually decreases, A / B in Equation 1 can become larger.

[0086] According to ①' and / or ②' above, the positive active material may have an A / B ratio of Equation 1 greater than 0.80. This positive active material is a case where structural stability is reduced according to ①' and / or ②' above. This is because the structural stability in the battery is reduced, leading to relatively severe microcracks, and ultimately, the capacity and capacity retention rate in the battery may decrease.

[0087] In summary, for a positive electrode active material in which A / B of Equation 1 is 0.35 to 0.80, it has optimal structural stability and can ultimately exhibit excellent characteristics in terms of capacity and capacity retention rate in the battery.

[0088] A detailed explanation of the above 1) and 2), which are major factors affecting A / B in mathematical formula 1, is provided in the method for manufacturing a positive electrode active material, which is the second aspect of the present invention.

[0089] In addition, differences in the physical properties of the precursor according to the manufacturing method when manufacturing the precursor of the present invention may affect A / B of Equation 1. That is, depending on the manufacturing method, there may be differences in the composition, component distribution (co-shell, concentration gradient), crystal structure, density, specific surface area, particle size, and particle size distribution of the precursor, and these differences may affect the structural stability of the cathode active material.

[0090] Physical properties of the positive electrode active material

[0091] The particle size of a single-crystal cathode active material composed of a single particle is the average particle size (D 50 ) may be 2μm to 7μm. However, it is not limited to this.

[0092] The particle shapes of a single-crystal cathode active material composed of a single particle may include spherical, elliptical, rhomboidal, rectangular, cuboidal, random, and mixtures thereof. However, it is not limited thereto.

[0093] A second aspect of the present invention provides a method for manufacturing a positive electrode active material for a lithium secondary battery according to the first aspect. This method may include: 1) a precursor manufacturing step for manufacturing a precursor for a positive electrode active material; 2) a step of manufacturing a primary positive electrode active material by first heat treating a material containing the manufactured precursor; 3) a step of manufacturing a secondary positive electrode active material by second heat treating a material containing the primary positive electrode active material; and 4) optionally, a step of manufacturing a tertiary positive electrode active material by third heat treating a material containing the secondary positive electrode active material.

[0094] 1) Preparation of precursors for positive electrode active materials

[0095] The precursor for the positive electrode active material may be a precursor prepared by a co-precipitation method.

[0096] Depending on the method of preparation, a precursor prepared by a co-precipitation method may include: 1) a precursor prepared by a continuous method; 2) a precursor prepared by a batch method; 3) a precursor in which the content ratio of the components constituting the precursor is uniform within the precursor particles; 4) a precursor in which the content ratio of the components constituting the precursor is non-uniform within the precursor particles (e.g., a precursor having a concentration gradient or a precursor having a core-shell structure); 5) a precursor containing a doping substance among the components constituting the precursor; and 6) a precursor not containing a doping substance among the components constituting the precursor.

[0097] In these co-precipitation methods, precursors according to each manufacturing method may have different physical properties, and these differences in physical properties may affect A / B of Equation 1 of the cathode active material.

[0098] The precursor for the positive electrode active material of the present invention can be manufactured by a method other than the co-precipitation method.

[0099] Methods other than the co-precipitation method may include wet mixing, dry mixing, spray drying, and spray thermal decomposition methods. The wet mixing method may be characterized by dissolving part or all of the cathode active material components in a solvent and then drying them while stirring. The dry mixing method may be characterized by mixing part or all of the cathode active material components in a solid state and then uniformly grinding the solid-state mixed components through a milling process. The spray drying method may be characterized by dissolving part or all of the cathode active material components in a solvent and then spray drying them. The spray thermal decomposition method may be characterized by dissolving part or all of the cathode active material components in a solvent and then spray thermal decomposing them at a high temperature.

[0100] Precursors prepared by manufacturing methods other than the co-precipitation method may each have different physical properties, and these differences in physical properties may affect A / B of Equation 1 of the cathode active material.

[0101] In addition, precursors prepared by methods other than the co-precipitation method may require different processes for manufacturing the cathode active material, and these differences in manufacturing processes may affect A / B of Equation 1 of the cathode active material.

[0102] 2) Preparation of positive electrode active material

[0103] The following describes a process for manufacturing an anode active material using a precursor prepared by a co-precipitation method (excluding precursors containing doping materials).

[0104] 2.1) Preparation of Primary Cathode Active Material

[0105] A material prepared by mixing a material containing a precursor, a lithium compound, and a doping material, performing a primary heat treatment, and then undergoing grinding, classification, washing, filtration, drying, classification, and iron removal processes can be called a primary cathode active material.

[0106] The composition and content of the doping material and the primary heat treatment conditions affect A / B of Equation 1 of the primary cathode active material and ultimately affect A / B of Equation 1 of the secondary (or tertiary if necessary) cathode active material.

[0107] doping substances

[0108] The components of the doping material used in the primary cathode active material manufacturing process may include at least one selected from the group consisting of Mg, Ca, Sr, Ba, Ti, V, Cr, Fe, Cu, Zn, B, Al, Si, Sn, P, Sb, Bi, S, F, Zr, Nb, Mo, Hf, Ta, W, Sc, Y, La, and Ce.

[0109] The content of the doping material is preferably 5.0 mol% or less among the remaining components of the positive active material excluding lithium and oxygen. If the content of the doping material exceeds 5.0 mol%, the A / B of Equation 1 of the positive active material decreases due to the deformation of the crystal structure of the positive active material, and in some cases, it may become 0.35 or less.

[0110] 1st heat treatment conditions

[0111] The main factors affecting A / B of Equation 1 of the cathode active material under the primary heat treatment conditions of the primary cathode active material manufacturing process are the maximum temperature of the primary heat treatment process and the holding time at the maximum temperature.

[0112] In the first heat treatment process, the maximum temperature may preferably be between 750°C and 950°C. If the maximum temperature is below 750°C, the sintering of the positive active material is insufficient, the structural stability of the positive active material decreases, and the A / B of Equation 1 of the positive active material increases, and in some cases, may exceed 0.80. On the other hand, if the maximum temperature exceeds 950°C, the sintering of the positive active material is excessive, and due to the collapse of the crystal structure of the positive active material, the A / B of Equation 1 of the positive active material decreases, and in some cases, may become less than 0.35.

[0113] In the first heat treatment process, the holding time at the maximum temperature may be 10 to 30 hours. If less than 10 hours, the sintering of the positive active material is insufficient, the structural stability of the positive active material decreases, and the A / B of Equation 1 of the positive active material increases, and in some cases, may exceed 0.80. On the other hand, if more than 30 hours, the sintering of the positive active material is excessive, and due to the breakdown of the crystal structure of the positive active material, the A / B of Equation 1 of the positive active material decreases, and in some cases, may fall below 0.35.

[0114] 2.2) Preparation of secondary cathode active material

[0115] A material prepared by mixing a material containing a primary positive active material and a coating material, performing a secondary heat treatment, and then undergoing grinding, classification, and iron removal processes can be called a secondary positive active material.

[0116] coating material

[0117] In the manufacturing process of the secondary cathode active material, the components that can be used as coating materials may include at least one selected from the group consisting of Li, N, Mg, Ca, Sr, Ba, Ti, V, Cr, Mn, Fe, Co, Cu, Zn, B, Al, Si, Sn, P, Sb, Bi, S, F, Zr, Nb, Mo, Hf, Ta, W, Sc, Y, La, and Ce.

[0118] The content of the coating material is preferably 5.0 mol% or less of the remaining components of the positive electrode active material excluding lithium and oxygen. If the content of the coating material exceeds 5.0 mol%, the nickel content of the positive electrode active material becomes relatively low, and the movement of lithium ions is hindered, which may result in a decrease in capacity, capacity retention rate, and output characteristics.

[0119] 2.3) Preparation of tertiary cathode active material

[0120] A material obtained by performing a third heat treatment on a second positive active material can be called a third positive active material. The third heat treatment can be performed selectively if necessary. That is, the second positive active material may not satisfy the conditions of the positive active material of the present invention, in which case a positive active material satisfying the present invention can be manufactured through a third heat treatment.

[0121] For example, if the A / B of the secondary cathode active material does not satisfy the range of Equation 1, a third cathode active material satisfying the range of Equation 1 can be manufactured by mixing the secondary cathode active material and the coating material and performing a third heat treatment.

[0122] In addition, when using two or more coating materials, the two or more coating materials may be manufactured by applying them together in a secondary heat treatment process, but in some cases, the coating materials may be manufactured by applying them separately in secondary and tertiary heat treatments.

[0123] Second (or third if necessary) heat treatment conditions

[0124] The secondary (or tertiary if necessary) heat treatment conditions of the secondary (or tertiary if necessary) cathode active material manufacturing process may be as follows.

[0125] In the second (or third if necessary) heat treatment process, the maximum temperature may preferably be between 350°C and 650°C. If the maximum temperature is below 350°C, the coating material may not be properly formed on the surface of the positive active material, and if the maximum temperature exceeds 650°C, the coating material may penetrate from the surface of the positive active material into the interior.

[0126] In the second (or third if necessary) heat treatment process, the holding time at the maximum temperature may be 5 to 20 hours. If less than 5 hours, the coating material may not be properly formed on the surface of the positive active material, and if more than 20 hours, the coating material may penetrate from the surface of the positive active material into the interior.

[0127] A third aspect of the present invention may be a positive electrode for a lithium secondary battery comprising a positive electrode active material of the front side. The positive electrode of this aspect may include a positive electrode current collector and a positive electrode active material layer formed on the positive electrode current collector. The positive electrode active material layer may include a positive electrode active material on the front side of the positive electrode.

[0128] Aluminum thin films may be used as the positive current collector, but are not limited thereto. The positive active material layer may include a positive active material, a binder, and a conductive material. The positive active material layer may include a positive active material according to the present invention. The binder may include a polymer having a fluorine (F) component, for example, polyvinyl fluoride (PVF), polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), and modifications thereof. The conductive material is used to impart conductivity to the electrode, and any electronically conductive material that does not cause chemical changes in the battery may be used. For example, natural graphite, artificial graphite, carbon black, acetylene black, ketjen black, carbon fiber, etc. may be used.

[0129] A fourth aspect of the present invention may be a lithium secondary battery comprising a positive electrode on the front side.

[0130] The lithium secondary battery of this aspect may include a positive electrode, a negative electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte on the front side.

[0131] The cathode may include a cathode current collector and a cathode active material layer formed on the current collector. A copper thin film may be used as the cathode current collector, but is not limited thereto. The cathode active material layer may include a cathode active material, a binder composition, and / or a conductive material.

[0132] The separator is inserted between the anode and the cathode to separate them, and may be one that has low resistance to the movement of electrolyte ions and excellent electrolyte wettability. For example, it may be selected from glass fiber, polyester, Teflon, polyethylene, polypropylene, polytetrafluoroethylene, or combinations thereof, and may be in the form of a nonwoven or woven fabric.

[0133] The electrolyte can be prepared by dissolving a lithium salt in an organic solvent. Any organic solvent and lithium salt that can be generally used as an organic solvent in the relevant technical field may be used. In addition, solid electrolytes such as organic solid electrolytes and inorganic solid electrolytes may be used as the electrolyte. When a solid electrolyte is used, the solid electrolyte may also serve as a separator.

[0134] Hereinafter, the present invention will be described in detail with reference to examples to specifically explain the invention. However, the embodiments according to the present invention may be modified in various different forms, and the scope of the present invention should not be interpreted as being limited to the embodiments described below. The embodiments of the present invention are provided to more completely explain the invention to those with average knowledge in the art.

[0135] 1. Preparation of precursors

[0136] 1) Preparation of Precursor 1

[0137] As shown below, the chemical formula is Ni in a continuous method 0.93 Co 0.02 Mn 0.05 A precursor 1 of (OH)2 was prepared.

[0138] ① Nickel sulfate, cobalt sulfate, and manganese sulfate were dissolved in deionized water to prepare a solution with a molar ratio of Ni:Co:Mn = 0.93:0.02:0.05.

[0139] ② Deionized water was filled into a continuous reactor, the water temperature of the reactor was set to 60℃, stirring was started, ammonia water was added to adjust the ammonia concentration to 3.0-3.3 g / L, sodium hydroxide solution was added to adjust the pH to 11.2-11.4, and nitrogen was injected (injected until the end of the co-precipitation reaction) to remove dissolved oxygen.

[0140] ③ The solution of ①, ammonia water, and sodium hydroxide solution were introduced into a reactor to start a co-precipitation reaction, at which time the ammonia concentration in the reactor was maintained at 3.0-3.3 g / L and the pH at 11.2-11.4.

[0141] ④ While continuously maintaining the state of ③ above, when the average particle size of the particles in the solution overflowing from the reactor becomes ~3.5 μm, the co-precipitation reaction is stopped, and then spherical precursor 1 is prepared through filtration, washing, drying, sieving, and iron removal processes.

[0142] 2) Preparation of Precursor 2

[0143] As shown below, the chemical formula is Ni in a continuous method 0.93 Mn 0.07 A precursor 2, which is (OH)2, was prepared.

[0144] ① Nickel sulfate and manganese sulfate were dissolved in deionized water to prepare a solution with a molar ratio of Ni:Mn = 0.93:0.07.

[0145] ② Subsequently, spherical precursor 2 was prepared by carrying out the same steps ② through ④ of the preparation of precursor 1.

[0146] 3) Preparation of Precursor 3

[0147] As shown below, the chemical formula is Ni in a continuous method 0.93 Co 0.07 A precursor 3, which is (OH)2, was prepared.

[0148] ① Nickel sulfate and manganese sulfate were dissolved in deionized water to prepare a solution with a molar ratio of Ni:Co = 0.93:0.07.

[0149] ② Subsequently, spherical precursor 3 was prepared by carrying out the same steps ② through ④ of the preparation of precursor 1.

[0150] 4) Preparation of Precursor 4

[0151] As shown below, by the spray drying method, the chemical formula is Ni 0.93 Co 0.02 Mn 0.05 A precursor 4, which is (OH)2, was prepared.

[0152] ① A solution was prepared by dissolving nickel nitrate, cobalt nitrate, and manganese nitrate in deionized water to a molar ratio of Ni:Co:Mn = 0.93:0.02:0.05, and then adding a small amount of citric acid.

[0153] ② The solution of ① above was spray-dried instantaneously using hot air while spraying it into small droplet shapes using a spray drying device to pulverize it, and then a primary powder was produced using a centrifugal device.

[0154] ③ The primary powder obtained in ② above was heat-treated in a kiln at 450°C for 3 hours in an oxygen atmosphere to remove residual moisture and citric acid.

[0155] ④ The heat-treated primary powder of ③ and deionized water were placed in a ball mill and milled to produce a slurry.

[0156] ⑤ The slurry prepared in ④ was secondarily spray-dried using a spray drying device to produce spherical precursor 4 with an average particle size of 3.7 μm.

[0157] 2. Preparation of positive electrode active material

[0158] In the preparation of the following positive electrode active material, the mixing molar ratios for the materials are based on the metal (or main component), and the results of the mixing molar ratios are shown in the experimental formulas in "Table 1 of 3. Evaluation" below.

[0159] 1) Preparation of positive electrode active material 1-1

[0160] A positive electrode active material 1-1 was prepared as follows using the above-prepared precursor 1.

[0161] ① The above precursor 1, lithium hydroxide, and zirconium oxide as a doping material were added to a mixing container in a molar ratio of 1.00 to 1.03 to 0.01 and mixed uniformly.

[0162] ② The mixed powder of ① was subjected to primary heat treatment in a box kiln under the following conditions.

[0163] - Atmosphere gas: Oxygen

[0164] - Heating rate: Heating from room temperature to 700℃ at a rate of 2℃ / min

[0165] - Holding time: Maintain at 700℃ for 20 hours

[0166] - Cooling method: Natural cooling

[0167] ③ The primary heat-treated material of ② was crushed and classified, then subjected to washing, filtration, drying, classification, and iron removal processes.

[0168] ④ The primary positive active material obtained in ③ above, titanium oxide as coating material 1, and aluminum oxide as coating material 2 were added to a mixing container in a molar ratio of 1.00 to 0.005 to 0.005 and mixed uniformly.

[0169] ⑤ The mixed powder of ④ was subjected to secondary heat treatment in a box kiln under the following conditions.

[0170] - Atmosphere gas: Oxygen

[0171] - Heating rate: Heating from room temperature to 550℃ at a rate of 2℃ / min

[0172] - Holding time: Hold at 550℃ for 10 hours

[0173] - Cooling method: Natural cooling

[0174] ⑥ The secondary heat-treated material of ⑤ was crushed and classified, and then subjected to a deironing process to produce the cathode active material 1-1.

[0175] 2) Preparation of positive electrode active material 1-2

[0176] Anode active material 1-2 was prepared by keeping the rest the same except that the primary heat treatment conditions of ② in the preparation of anode active material 1-1 were changed as in ②' below.

[0177] ②' The mixed powder of ① was subjected to primary heat treatment in a box kiln under the following conditions.

[0178] - Atmosphere gas: Oxygen

[0179] - Heating rate: Heating from room temperature to 800℃ at a rate of 2℃ / min

[0180] - Holding time: Maintain at 800℃ for 20 hours

[0181] - Cooling method: Natural cooling

[0182] 3) Preparation of positive electrode active material 1-3

[0183] Anode active material 1-3 was prepared by keeping the rest the same except that the primary heat treatment conditions of ② in the preparation of anode active material 1-1 were changed as in ②' below.

[0184] ②' The mixed powder of ① was subjected to primary heat treatment in a box kiln under the following conditions.

[0185] - Atmosphere gas: Oxygen

[0186] - Heating rate: Heating from room temperature to 850℃ at a rate of 2℃ / min

[0187] - Holding time: Hold at 850℃ for 5 hours

[0188] - Cooling method: Natural cooling

[0189] 4) Preparation of positive electrode active material 1-4

[0190] Anode active material 1-4 was prepared by keeping the rest the same except that the primary heat treatment conditions of ② in the preparation of anode active material 1-1 were changed as in ②' below.

[0191] ②' The mixed powder of ① was subjected to primary heat treatment in a box kiln under the following conditions.

[0192] - Atmosphere gas: Oxygen

[0193] - Heating rate: Heating from room temperature to 850℃ at a rate of 2℃ / min

[0194] - Holding time: Hold at 850℃ for 20 hours

[0195] - Cooling method: Natural cooling

[0196] 5) Preparation of positive electrode active material 1-5

[0197] Anode active material 1-5 was prepared by keeping the rest the same except that the primary heat treatment conditions of ② in the preparation of anode active material 1-1 were changed as in ②' below.

[0198] ②' The mixed powder of ① was subjected to primary heat treatment in a box kiln under the following conditions.

[0199] - Atmosphere gas: Oxygen

[0200] - Heating rate: Heating from room temperature to 850℃ at a rate of 2℃ / min

[0201] - Holding time: Hold at 850℃ for 40 hours

[0202] - Cooling method: Natural cooling

[0203] 6) Preparation of positive electrode active material 1-6

[0204] Anode active material 1-6 was prepared by keeping the rest the same except that the primary heat treatment conditions of ② in the preparation of anode active material 1-1 were changed as in ②' below.

[0205] ②' The mixed powder of ① was subjected to primary heat treatment in a box kiln under the following conditions.

[0206] - Atmosphere gas: Oxygen

[0207] - Heating rate: Heating from room temperature to 900℃ at a rate of 2℃ / min

[0208] - Holding time: Maintain at 900℃ for 20 hours

[0209] - Cooling method: Natural cooling

[0210] 7) Preparation of positive electrode active material 1-7

[0211] Anode active material 1-7 was prepared by keeping the rest the same except that the primary heat treatment conditions of ② in the preparation of anode active material 1-1 were changed as in ②' below.

[0212] ②' The mixed powder of ① was subjected to primary heat treatment in a box kiln under the following conditions.

[0213] - Atmosphere gas: Oxygen

[0214] - Heating rate: Heating from room temperature to 1,000℃ at a rate of 2℃ / min

[0215] - Holding time: Maintain at 1,000℃ for 20 hours

[0216] - Cooling method: Natural cooling

[0217] 8) Preparation of positive electrode active material 2-1

[0218] A positive electrode active material 2-1 was prepared as follows using the above-prepared precursor 2.

[0219] ① The above precursor 2 and lithium hydroxide were added to a mixing container in a molar ratio of 1.00 to 1.03 and mixed uniformly.

[0220] ② The mixed powder of ① was subjected to primary heat treatment in a box kiln under the following conditions.

[0221] - Atmosphere gas: Oxygen

[0222] - Heating rate: Heating from room temperature to 850℃ at a rate of 2℃ / min

[0223] - Holding time: Hold at 850℃ for 20 hours

[0224] - Cooling method: Natural cooling

[0225] ③ The primary heat-treated material of ② was crushed and classified, then subjected to washing, filtration, drying, classification, and iron removal processes.

[0226] ④ The primary positive active material obtained in ③ above, titanium oxide as coating material 1, and aluminum oxide as coating material 2 were added to a mixing container in a molar ratio of 1.00 to 0.005 to 0.005 and mixed uniformly.

[0227] ⑤ The mixed powder of ④ was subjected to secondary heat treatment in a box kiln under the following conditions.

[0228] - Atmosphere gas: Oxygen

[0229] - Heating rate: Heating from room temperature to 550℃ at a rate of 2℃ / min

[0230] - Holding time: Hold at 550℃ for 10 hours

[0231] - Cooling method: Natural cooling

[0232] ⑥ The secondary heat-treated material of ⑤ was crushed and classified, and then subjected to a deironing process to produce the cathode active material 2-1.

[0233] 9) Preparation of positive electrode active material 2-2

[0234] Anode active material 2-2 was prepared by keeping the rest the same except that the mixing ratio of ① in the preparation of anode active material 2-1 was changed as in ①' below.

[0235] ① The above precursor 2, lithium hydroxide, and zirconium oxide as a doping material were added to a mixing container in a molar ratio of 1.00 to 1.03 to 0.0025 and mixed uniformly.

[0236] 10) Preparation of positive electrode active material 2-3

[0237] Anode active material 2-3 was prepared by keeping the rest the same except that the mixing ratio of ① in the preparation of anode active material 2-1 was changed as in ①' below.

[0238] ① The above precursor 2, lithium hydroxide, and zirconium oxide as a doping material were added to a mixing container in a molar ratio of 1.00 to 1.03 to 0.005 and mixed uniformly.

[0239] 11) Preparation of positive electrode active material 2-4

[0240] Anode active material 2-4 was prepared by keeping the rest the same except that the mixing ratio of ① in the preparation of anode active material 2-1 was changed as in ①' below.

[0241] ① The above precursor 2, lithium hydroxide, and zirconium oxide as a doping material were added to a mixing container in a molar ratio of 1.00 to 1.03 to 0.01 and mixed uniformly.

[0242] 12) Preparation of positive electrode active material 2-5

[0243] Anode active material 2-5 was prepared by keeping the rest the same except that the mixing ratio of ① in the preparation of anode active material 2-1 was changed as in ①' below.

[0244] ① The above precursor 2, lithium hydroxide, and zirconium oxide as a doping material were added to a mixing container in a molar ratio of 1.00 to 1.03 to 0.02 and mixed uniformly.

[0245] 13) Preparation of positive electrode active material 2-6

[0246] Anode active material 2-6 was prepared by keeping the rest the same except that the mixing ratio of ① in the preparation of anode active material 2-1 was changed as in ①' below.

[0247] ① The above precursor 2, lithium hydroxide, and zirconium oxide as a doping material were added to a mixing container in a molar ratio of 1.00 to 1.03 to 0.04 and mixed uniformly.

[0248] 14) Preparation of positive electrode active material 2-7

[0249] Anode active material 2-7 was prepared by keeping the rest the same except that the mixing ratio of ① in the preparation of anode active material 2-1 was changed as in ①' below.

[0250] ① The above precursor 2, lithium hydroxide, and zirconium oxide as a doping material were added to a mixing container in a molar ratio of 1.00 to 1.03 to 0.06 and mixed uniformly.

[0251] 15) Preparation of Cathode Active Material 3-1

[0252] A positive electrode active material 3-1 was prepared as follows using the above-prepared precursor 3.

[0253] ① The above precursor 3, lithium hydroxide, and aluminum oxide as a doping material were added to a mixing container in a molar ratio of 1.00 to 1.03 to 0.01 and mixed uniformly.

[0254] ② The mixed powder of ① was subjected to primary heat treatment in a box kiln under the following conditions.

[0255] - Atmosphere gas: Oxygen

[0256] - Heating rate: Heating from room temperature to 700℃ at a rate of 2℃ / min

[0257] - Holding time: Maintain at 700℃ for 20 hours

[0258] - Cooling method: Natural cooling

[0259] ③ The primary heat-treated material of ② was crushed and classified, then subjected to washing, filtration, drying, classification, and iron removal processes.

[0260] ④ Titanium oxide was added to the primary positive active material and coating material obtained in ③ above in a molar ratio of 1.00 to 0.005 and mixed uniformly.

[0261] ⑤ The mixed powder of ④ was subjected to secondary heat treatment in a box kiln under the following conditions.

[0262] - Atmosphere gas: Oxygen

[0263] - Heating rate: Heating from room temperature to 550℃ at a rate of 2℃ / min

[0264] - Holding time: Hold at 550℃ for 10 hours

[0265] - Cooling method: Natural cooling

[0266] ⑥ The secondary heat-treated material of ⑤ was crushed and classified, and then subjected to a deironing process.

[0267] ⑦ Aluminum oxide was added to the secondary positive active material obtained in ⑥ and coating material 2 in a molar ratio of 1.00 to 0.005 and mixed uniformly.

[0268] ⑧ The mixed powder of ⑦ was subjected to a third heat treatment in a box kiln under the following conditions.

[0269] - Atmosphere gas: Oxygen

[0270] - Heating rate: Heating from room temperature to 550℃ at a rate of 2℃ / min

[0271] - Holding time: Hold at 550℃ for 10 hours

[0272] - Cooling method: Natural cooling

[0273] The cathode active material 3-1 was prepared by crushing and classifying the 3rd heat-treated material of ⑨ and ⑧, followed by a deironing process.

[0274] 16) Preparation of Cathode Active Material 3-2

[0275] Anode active material 3-2 was prepared by keeping the rest the same except that the primary heat treatment conditions of ② in the preparation of anode active material 3-1 were changed as follows.

[0276] - Atmosphere gas: Oxygen

[0277] - Heating rate: Heating from room temperature to 800℃ at a rate of 2℃ / min

[0278] - Holding time: Maintain at 800℃ for 20 hours

[0279] - Cooling method: Natural cooling

[0280] 17) Preparation of positive electrode active material 3-3

[0281] Anode active material 3-3 was prepared by keeping the rest the same except that the primary heat treatment conditions of ② in the preparation of anode active material 3-1 were changed as follows.

[0282] - Atmosphere gas: Oxygen

[0283] - Heating rate: Heating from room temperature to 850℃ at a rate of 2℃ / min

[0284] - Holding time: Hold at 850℃ for 5 hours

[0285] - Cooling method: Natural cooling

[0286] 18) Preparation of positive electrode active material 3-4

[0287] Anode active material 3-4 was prepared by keeping the rest the same except that the primary heat treatment conditions of ② in the preparation of anode active material 3-1 were changed as follows.

[0288] - Atmosphere gas: Oxygen

[0289] - Heating rate: Heating from room temperature to 850℃ at a rate of 2℃ / min

[0290] - Holding time: Hold at 850℃ for 20 hours

[0291] - Cooling method: Natural cooling

[0292] 19) Preparation of positive electrode active material 3-5

[0293] Anode active material 3-5 was prepared by keeping the rest the same except that the primary heat treatment conditions of ② in the preparation of anode active material 3-1 were changed as follows.

[0294] - Atmosphere gas: Oxygen

[0295] - Heating rate: Heating from room temperature to 850℃ at a rate of 2℃ / min

[0296] - Holding time: Hold at 850℃ for 40 hours

[0297] - Cooling method: Natural cooling

[0298] 20) Preparation of positive electrode active material 3-6

[0299] Anode active material 3-6 was prepared by keeping the rest the same except that the primary heat treatment conditions of ② in the preparation of anode active material 3-1 were changed as follows.

[0300] - Atmosphere gas: Oxygen

[0301] - Heating rate: Heating from room temperature to 900℃ at a rate of 2℃ / min

[0302] - Holding time: Maintain at 900℃ for 20 hours

[0303] - Cooling method: Natural cooling

[0304] 21) Preparation of positive electrode active material 3-7

[0305] Anode active material 3-7 was prepared in the same manner as in Example 3-1, except that the primary heat treatment conditions of ② were changed as follows.

[0306] - Atmosphere gas: Oxygen

[0307] - Heating rate: Heating from room temperature to 1,000℃ at a rate of 2℃ / min

[0308] - Holding time: Maintain at 1,000℃ for 20 hours

[0309] - Cooling method: Natural cooling

[0310] 22) Preparation of Cathode Active Material 4-1

[0311] A positive electrode active material 4-1 was prepared as follows using the above-prepared precursor 4.

[0312] ① The above precursor 4 and lithium hydroxide were added to a mixing container in a molar ratio of 1.00 to 1.03 and mixed uniformly.

[0313] ② The mixed powder of ① was subjected to primary heat treatment in a box kiln under the following conditions.

[0314] - Atmosphere gas: Oxygen

[0315] - Heating rate: Heating from room temperature to 850℃ at a rate of 2℃ / min

[0316] - Holding time: Hold at 850℃ for 20 hours

[0317] - Cooling method: Natural cooling

[0318] ③ The primary heat-treated material of ② was crushed and classified, then subjected to washing, filtration, drying, classification, and iron removal processes.

[0319] ④ The primary positive active material obtained in ③ above, titanium oxide as coating material 1, and aluminum oxide as coating material 2 were added to a mixing container in a molar ratio of 1.00 to 0.005 to 0.005 and mixed uniformly.

[0320] ⑤ The mixed powder of ④ was subjected to secondary heat treatment in a box kiln under the following conditions.

[0321] - Atmosphere gas: Oxygen

[0322] - Heating rate: Heating from room temperature to 550℃ at a rate of 2℃ / min

[0323] - Holding time: Hold at 550℃ for 10 hours

[0324] - Cooling method: Natural cooling

[0325] ⑥ The secondary heat-treated material of ⑤ was crushed and classified, and then subjected to a deironing process to produce the cathode active material 4-1.

[0326] 23) Preparation of Cathode Active Material 4-2

[0327] Anode active material 4-2 was prepared by keeping the rest the same except that the mixing ratio of ① in the preparation of anode active material 4-1 was changed as in ①' below.

[0328] ① The above precursor 4, lithium hydroxide, and zirconium oxide as a doping material were added to a mixing container in a molar ratio of 1.00 to 1.03 to 0.0025 and mixed uniformly.

[0329] 24) Preparation of positive electrode active material 4-3

[0330] Anode active material 4-3 was prepared by keeping the rest the same except that the mixing ratio of ① in the preparation of anode active material 4-1 was changed as in ①' below.

[0331] ① The above precursor 4, lithium hydroxide, and zirconium oxide as a doping material were added to a mixing container in a molar ratio of 1.00 to 1.03 to 0.005 and mixed uniformly.

[0332] 25) Preparation of positive electrode active material 4-4

[0333] Anode active material 4-4 was prepared by keeping the rest the same except that the mixing ratio of ① in the preparation of anode active material 4-1 was changed as in ①' below.

[0334] ① The above precursor 4, lithium hydroxide, and zirconium oxide as a doping material were added to a mixing container in a molar ratio of 1.00 to 1.03 to 0.01 and mixed uniformly.

[0335] 26) Preparation of positive electrode active materials 4-5

[0336] Anode active material 4-5 was prepared by keeping the rest the same except that the mixing ratio of ① in the preparation of anode active material 4-1 was changed as in ①' below.

[0337] ① The above precursor 4, lithium hydroxide, and zirconium oxide as a doping material were added to a mixing container in a molar ratio of 1.00 to 1.03 to 0.02 and mixed uniformly.

[0338] 27) Preparation of positive electrode active material 4-6

[0339] Anode active material 4-6 was prepared by keeping the rest the same except that the mixing ratio of ① in the preparation of anode active material 4-1 was changed as in ①' below.

[0340] ① The above precursor 4, lithium hydroxide, and zirconium oxide as a doping material were added to a mixing container in a molar ratio of 1.00 to 1.03 to 0.04 and mixed uniformly.

[0341] 28) Preparation of positive electrode active material 4-7

[0342] Anode active material 4-7 was prepared by keeping the rest the same except that the mixing ratio of ① in the preparation of anode active material 4-1 was changed as in ①' below.

[0343] ① The above precursor 2, lithium hydroxide, and zirconium oxide as a doping material were added to a mixing container in a molar ratio of 1.00 to 1.03 to 0.06 and mixed uniformly.

[0344] 3. Evaluation

[0345] 1) Component analysis of the cathode active material

[0346] Elemental analysis of the above-prepared cathode active materials was performed using an ICP-OES analyzer. For the ICP-OES analysis, the major components were analyzed using an Agilent 5800 (RF power 1200W) analyzer, and trace elements such as doping and coating materials were analyzed using a Perkin Elmer Avio550 (RF power 1300W).

[0347] Table 1 shows the experimental chemical formulas for the positive electrode active materials of the above examples and comparative examples, and the analytical chemical formulas obtained using ICP-OES.

[0348] Cathode active material experiment, chemical formula analysis, chemical formula 1-1Li 1.03 [(Ni 0.93 Co 0.02 Mn 0.05 )-(Zr 0.01 )-(Ti 0.005 Al 0.005 )]O (>2) Li 1.007 [(Ni 0.909 Co 0.020 Mn 0.050 Zr 0.010 Ti 0.005Al 0.006 )]O (>2) 1-2Li 1.005 [(Ni 0.910 Co 0.020 Mn 0.048 Zr 0.011 Ti 0.005 Al 0.006 )]O (>2) 1-3Li 1.004 [(Ni 0.910 Co 0.020 Mn 0.050 Zr 0.010 Ti 0.005 Al 0.005 )]O (>2) 1-4Li 1.006 [(Ni 0.912 Co 0.018 Mn 0.049 Zr 0.010 Ti 0.005 Al 0.006 )]O (>2) 1-5Li 1.005 [(Ni 0.910 Co 0.021 Mn 0.049 Zr 0.009 Ti 0.005 Al 0.006 )]O (>2) 1-6Li 1.004 [(Ni 0.912 Co 0.019 Mn 0.049 Zr 0.010 Ti 0.005 Al 0.005 )]O (>2) 1-7Li 1.003 [(Ni 0.910 Co 0.021 Mn 0.051 Zr 0.009 Ti 0.004 Al 0.005 )]O (>2) 2-1Li 1.03 [(Ni 0.93 Mn 0.07 (Ti) 0.005 Al 0.005 )]O (>2) Li 1.006 [(Ni 0.920 Mn 0.069 Ti 0.005 Al 0.006 )]O (>2) 2-2Li 1.03 [(Ni0.93 Mn 0.07 (Zr) 0.0025 (Ti) 0.005 Al 0.005 )]O (>2) Li 1.005 [(Ni 0.920 Mn 0.069 Zr 0.002 Ti 0.004 Al 0.005 )]O (>2) 2-3Li 1.03 [(Ni 0.93 Mn 0.07 (Zr) 0.005 (Ti) 0.005 Al 0.005 )]O (>2) Li 1.006 [(Ni 0.915 Mn 0.070 Zr 0.005 Ti 0.004 Al 0.006 )]O (>2) 2-4Li 1.03 [(Ni 0.93 Mn 0.07 (Zr) 0.01 (Ti) 0.005 Al 0.005 )]O (>2) Li 1.004 [(Ni 0.912 Mn 0.069 Zr 0.010 Ti 0.004 Al 0.005 )]O (>2) 2-5Li 1.03 [(Ni 0.93 Mn 0.07 (Zr) 0.02 (Ti) 0.005 Al 0.005 )]O (>2) Li 1.004 [(Ni 0.902 Mn 0.070 Zr 0.018 Ti 0.004 Al 0.006 )]O (>2) 2-6Li 1.03 [(Ni 0.93 Mn 0.07 (Zr) 0.04 (Ti) 0.005 Al 0.005 )]O (>2) Li1.005 [(Ni 0.885 Mn 0.067 Zr 0.039 Ti 0.004 Al 0.005 )]O (>2) 2-7Li 1.03 [(Ni 0.93 Mn 0.07 (Zr) 0.06 (Ti) 0.005 Al 0.005 )]O (>2) Li 1.004 [(Ni 0.870 Mn 0.066 Zr 0.056 Ti 0.004 Al 0.004 )]O (>2) 3-1Li 1.03 [(Ni 0.93 Co 0.07 (Al) 0.01 (Ti) 0.005 (Al) 0.005 )]O (>2) Li 1.006 [(Ni 0.911 Co 0.070 Al 0.014 Ti 0.005 )]O (>2) 3-2Li 1.003 [(Ni 0.910 Co 0.070 Al 0.015 Ti 0.005 )]O (>2) 3-3Li 1.004 [(Ni 0.912 Co 0.068 Al 0.015 Ti 0.005 )]O (>2) 3-4Li 1.005 [(Ni 0.910 Co 0.068 Al 0.016 Ti 0.006 )]O (>2) 3-5Li 1.003 [(Ni 0.911 Co 0.069 Al 0.014 Ti 0.006 )]O (>2) 3-6Li 1.005 [(Ni 0.909 Co 0.071 Al 0.016 Ti0.004 )]O (>2) 3-7Li 1.004 [(Ni 0.912 Co 0.069 Al 0.014 Ti 0.005 )]O (>2) 4-1Li 1.03 [(Ni 0.93 Co 0.02 Mn 0.05 (Ti) 0.005 (Al) 0.005 )]O (>2) Li 1.005 [(Ni 0.920 Co 0.020 Mn 0.050 Ti 0.005 Al 0.005 )]O (>2) 4-2Li 1.03 [(Ni 0.93 Co 0.02 Mn 0.05 (Zr) 0.0025 (Ti) 0.005 (Al) 0.005 )]O (>2) Li 1.004 [(Ni 0.919 Co 0.020 Mn 0.048 Zr 0.003 Ti 0.005 Al 0.005 )]O (>2) 4-3Li 1.03 [(Ni 0.93 Co 0.02 Mn 0.05 (Zr) 0.005 (Ti) 0.005 (Al) 0.005 )]O (>2) Li 1.005 [(Ni 0.916 Co 0.019 Mn 0.049 Zr 0.005 Ti 0.005 Al 0.005 )]O (>2) 4-4Li 1.03 [(Ni 0.93 Co 0.02 Mn 0.05 (Zr) 0.01 (Ti) 0.005 (Al) 0.005 )]O (>2) Li1.005 [(Ni 0.912 Co 0.020 Mn 0.049 Zr 0.009 Ti 0.005 Al 0.005 )]O (>2) 4-5Li 1.03 [(Ni 0.93 Co 0.02 Mn 0.05 (Zr) 0.02 (Ti) 0.005 (Al) 0.005 )]O (>2) Li 1.003 [(Ni 0.902 Co 0.019 Mn 0.049 Zr 0.019 Ti 0.006 Al 0.005 )]O (>2) 4-6Li 1.03 [(Ni 0.93 Co 0.02 Mn 0.05 (Zr) 0.04 (Ti) 0.005 (Al) 0.005 )]O (>2) Li 1.003 [(Ni 0.887 Co 0.018 Mn 0.050 Zr 0.037 Ti 0.004 Al 0.004 )]O (>2) 4-7Li 1.03 [(Ni 0.93 Co 0.02 Mn 0.05 (Zr) 0.06 (Ti) 0.005 (Al) 0.005 )]O (>2) Li 1.004 [(Ni 0.869 Co 0.018 Mn 0.047 Zr 0.057 Ti 0.005 Al 0.004 )]O (>2)

[0349] In Table 1, the "Experimental" chemical formulas are based on the molar ratio values ​​used in the manufacturing method, while the "Analytical" chemical formulas represent the remaining components (components shown in the chemical formulas), excluding lithium and oxygen, based on a 1.0 molar standard. Referring to Table 1, it can be confirmed that the experimental and analytical values ​​match well for the components other than lithium. In the case of lithium, the analytical value is lower than the experimental value, which is because lithium compounds present on the surface of the cathode active material are removed during the cleaning process in the primary cathode active material manufacturing process.

[0350] 2) Particle size analysis of cathode active material

[0351] Particle size analysis of the cathode active materials prepared in the examples and comparative examples was performed using a particle size analyzer (Master Sizer 3000), and the results are shown in Table 2.

[0352] Positive active material D 50 (μm)Span1-13.71.381-23.91.381-34.11.361-44.01.391-53.91.351-64.21.331-74 .01.342-13.71.422-23.81.392-33.71.412-43.51.432-53.31.402-63.41.412-74.2 1.393-13.61.343-23.41.353-33.61.363-43.71.333-53.51.373-63.51.383-73.61.354-14.31.424-24.51.434-34.61.394-44.51.434-54.81.414-64.71.444-74.91.45

[0353] Referring to Table 2, there is no difference in the average particle size and particle size distribution according to the examples and comparative examples. From this, it can be confirmed that the average particle size and particle size distribution are not affected by the heat treatment temperature and doping material content during the manufacture of the cathode active material.3) Analysis of the amount of residual lithium on the surface of the cathode active material

[0354] The content of residual lithium (lithium hydroxide and lithium carbonate) present on the surface of the cathode active material prepared in the examples and comparative examples was evaluated as follows by titration using a 905 Titrado instrument. Specifically, 10 g of the cathode active material was dispersed in 100 mL of water and then titrated with 0.1 M HCl to obtain a pH titration result, and the content of lithium hydroxide and lithium carbonate present on the surface of the cathode active material was measured using the result. The results are shown in Table 3 and Figure 3.

[0355] Cathode Active Material LiOH (ppm) Li2CO3 (ppm) 1 - 14 226 36 25 1 - 24 45 43 35 7 1 - 34 0 5 7 28 5 0 1 - 43 7 35 25 4 1 1 - 5 3 3 10 24 3 5 1 - 6 3 5 7 226 1 2 1 - 7 2 9 6 1 2 4 5 3 2 - 14 4 5 23 6 7 0 2 - 24 3 4 0 24 2 1 2 - 3 4 3 5 6 23 2 9 2 - 4 3 7 3 4 25 6 1 2 - 5 3 6 6 5 24 5 2 2 - 6 3 0 10 2 3 22-7314521833-1361526283-2361025533-3332622603-4314320413-5288319203-6278818593-7263216374-1394229894-2385028814-3361428524-4305123664-5312524424-6298021804-726571875

[0356] Referring to Table 3, it can be confirmed that the lithium carbonate content in the residual lithium of the cathode active materials is 5,000 ppm or less according to the appropriate method, which indicates that the influence of lithium carbonate decomposition on the weight loss in the cathode active material decomposition section is negligible. 4. TGA of Cathode Active Materials

[0357] TGA was performed on the cathode active materials of the examples and comparative examples in the following manner. A NETZSCH STA 2500 TGA instrument was used, the evaluation temperature range was from room temperature to 1,200°C, the heating rate was 5°C / min, oxygen gas was used as the atmosphere gas for the first analysis and nitrogen gas for the second analysis, and the gas supply flow rate for each was 20 mL / min.

[0358] The TGA results for the cathode active materials of the examples and comparative examples are T shown in Fig. 2 onset (K) and △W 300 Calculated and organized based on (wt%), Table 4 shows the results when oxygen was used as the atmosphere gas, and Table 5 shows the results when nitrogen was used as the atmosphere gas.

[0359] Positive active material T onset (K)△W 300 (wt%)·300(K)△W 300 (wt%)·300(K) / T onset (K)1-1967.525542.641-2981.916991.731-3971.123012.371-4986.711051.121-5996.91500.151-6992.34270.431-7999.1600.06 2-1986.627522.792-2994.419691.982-3996.214271.432-4997.09170.922-51004.05120.512-61006.34230.422-71016.01120.11 3-11000.918721.873-21016.08840.873-31009.114431.433-41018.08550.843-51031.44230.413-61027.84620.453-71035.11350.134-1938.929103.104-2944.322762.414-3947.415921.684-4949.411391.204-5950.84180.444-6954.51340.144-7962.2960.10

[0360] Positive active material T onset (K)△W 300 (wt%)·300(K)△W 300 (wt%)·300(K) / T onset(K)1-1924.229103.151-2936.421902.341-3927.326702.881-4941.417101.821-5952.54200.441-6947.06900.731-7957.42100. 222-1937.930903.292-2944.224602.612-3946.523402.472-4948.719202.022-5954.313501.412-6958.45400.562-7963.83300. 343-1947.325502.693-2960.418901.973-3952.525502.683-4965.415901.653-5974.86600.683-6971.28400.863-7985.53900.404-1897.532103.584-2904.426402.924-3907.019502.154-4908.517101.884-5911.910801.184-6917.63900.434-7925.23300.36

[0361] Referring to Tables 4 and 5, even with the same cathode active material, T is relatively higher when using oxygen as the atmosphere gas compared to using nitrogen. onset (K) is increasing and △W 300 (wt%)·300(K) indicates a decreasing result. △W in Table 4, which is A in Equation 1 300 (wt%)·300(K) / T onset (K) and △W in Table 5, which is B in Equation 1 300 (wt%)·300(K) / T onset (K) and the calculated A / B are shown together in Table 6.

[0362] Cathode active material ABA / B1-12.643.150.841-21.732.340.741-32.372.880.821-41.121.820.621-50.150.440.341-60.430.730.591-70.060.220.272-12.793.290.852-21.982.610.762-31.432.470.582-40.922.020.462-50.511.410.362-60.420.560.752-70.110.34 0.323-11.872.690.703-20.871.970.443-31.432.680.533-40.841.650.513-50.410.680.603-60.450.860.523-70.130.400.334-13.103.580.874-22.412.920.834-31.682.150.784-41.201.880.644-50.441.180.374-60.140.430.334-70.100.360.28

[0363] Referring to Table 6, it is shown that the maximum temperature in the primary heat treatment process and the content of the doping material mixed relative to the cathode active material during the manufacture of the primary cathode active material of the present invention affect A / B in Equation 1.

[0364] 5. Evaluation of battery performance of cathode active material

[0365] To evaluate the battery performance of the cathode active materials of the examples and comparative examples, a cathode and a lithium battery (coin half-cell) were manufactured using the following method.

[0366] A positive electrode was prepared in which a positive electrode active material layer composed of the respective positive electrode active material of the example and comparative example, carbon conductive material (Super P), and PVDF binder in a weight ratio of 97:1.5:1.5 was formed on an aluminum thin film current collector.

[0367] A coin half-cell was manufactured using the above anode, a lithium metal cathode, a polyethylene separator, and an electrolyte (composed of a mixed solution of ethylene carbonate (EC), dimethyl carbonate (DMC), ethylmethyl carbonate (EMC), and lithium hexafluorophosphate (LiPF6)).

[0368] The capacity characteristics were evaluated as follows using each of the above-manufactured coin half-cells.

[0369] The coin half-cell was initially charged to 4.4V with a constant current of 0.2C and a cut-off of 0.01C at 45℃, and initially discharged to 3.0V with a constant current of 0.2C. Subsequently, the coin half-cell was charged to 4.4V with a constant current of 0.5C and a cut-off of 0.05C at 45℃, and discharged to 3.0V with a constant current of 0.5C. This was repeated 100 times, with this as one cycle. The results are shown in Table 7.

[0370] Cathode Active Material Initial Charge Capacity (mAh / g) Initial Discharge Capacity (mAh / g) Efficiency (%) Discharge Capacity (mAh / g, @100cycle) Capacity Retention Rate (%, @100cycle) 1-1239.8209.687.4176.284.11-2240.6213.788.8190.789.21-3239.6209.087.2172.382.41-4241.6216.389.5198.591.81-5235.0203.286.5170.884.11-6237.5208.687.8186.289.31-7231.2196.484.91 61.182.02-1242.7215.088.6175.081.42-2242.4217.789.8189.387.02-3242.1216.389.3192.288.92-4241.8215.489.1196.791.32-5240.0212.788.6193.390.92-6237.3209.288.2186.489.12-7235.5197.783.9164. 483.23-1240.0214.189.2187.387.53-2241.4217.890.2198.591.13-3239.6215.389.9191.188.83-4242.2219.390.5202.192.23-5238.2211.888.9188.489.03-6239.1214.789.8189.488.23-7233.3201.886.5168.38 3.44-1236.7205.486.8166.981.34-2235.8206.487.5173.584.14-3237.2210.688.8192.791.54-4237.4211.889.2194.491.84-5235.8209.588.8194.492.84-6232.5198.585.4166.383.84-7228.5191.483.8158.282.7

[0371] Figure 3 shows a graph illustrating the correlation between A / B in Table 6 and the discharge capacity (mAh / g, @100 cycle) in Table 7. Referring to Figure 3, it can be seen that the discharge capacity at 100 cycles is superior when the A / B of the positive active material is between 0.35 and 0.80 compared to other positive active materials with an A / B of less than 0.35 or greater than 0.80.

[0372] Referring to Table 6 and Figure 3, for positive electrode active materials with excellent discharge capacity at 100 cycles, i.e., A / B ratio of 0.35 to 0.80, A is shown to have a value in the range of 0.38 (wt%) to 2.00 (wt%), and B is shown to have a value in the range of 0.70 (wt%) to 3.00 (wt%). This is due to the result that when oxygen is used as the atmosphere gas in the TGA of the positive electrode active material compared to when nitrogen or argon is used, the temperature at which structural breakdown of the positive electrode active material begins increases relatively, and the weight change amount with a 300K temperature increase relative to the temperature at which structural breakdown begins decreases relatively.

[0373] The present invention relates to the correlation between the TGA results of a positive electrode active material, which indicates relative structural stability, and the results of capacity characteristics in a battery. Generally, there is a difficulty in having to fabricate and evaluate a battery to observe the capacity characteristics of a positive electrode active material, but by using Equation 1 of the present invention, the capacity characteristics in a battery can be predicted based solely on the TGA results of the positive electrode active material.

[0374] In conclusion, through the precursor for a positive electrode active material and the method for manufacturing a positive electrode active material presented in the present invention, a positive electrode active material having high capacity and improved structural stability can be manufactured. Furthermore, the capacity characteristics of such a positive electrode active material can be easily predicted in a battery through TGA, and a lithium secondary battery with excellent capacity and capacity retention rate can be manufactured using a positive electrode active material having these characteristics.

[0375] The terms used in this invention are intended to describe specific embodiments and are not intended to limit the invention. Unless otherwise evident from the context, singular expressions should be understood to include a plural meaning. Terms such as "comprising" or "having" mean that the features, numbers, steps, actions, components, or combinations thereof described in the specification exist, not that they are excluded.

[0376] The present invention is not limited by the embodiments described above and the attached drawings, but is intended to be limited by the attached claims. Accordingly, various substitutions, modifications, and changes may be made by those skilled in the art within the scope of the technical concept of the present invention as described in the claims, and such should also be considered to fall within the scope of the present invention.

Claims

1. It is a single-crystal cathode active material composed of a single particle, and Among the remaining components excluding lithium and oxygen, the nickel content is greater than 80 mol% and less than 98 mol%, and A cathode active material for a lithium secondary battery whose thermogravimetric analysis (TGA) results satisfy the following mathematical formula 1: [Mathematical Formula 1] 0.35 ≤ A / B ≤ 0.80, Here, A is △W when analyzing using oxygen (O2) as the atmosphere gas in TGA. 300 (wt%)·300(K) / T onset (K) and B is △W when analyzing using nitrogen (N2) or argon (Ar) as the atmosphere gas in TGA. 300 (wt%)·300(K) / T onset (K) and T onset (K) is the onset Kelvin temperature (K) in the first stage structural breakdown region of the positive active material, which is a temperature within the range of 773.15K (500℃) to 1173.15K (900℃), and △W 300 (wt%) = W onset (wt%) - W onset+300K (wt%) and W onset (wt%) is T relative to initial weight onset wt%(wt%) at (K), and W onset+300K (wt%) is T relative to initial weight onset wt%(wt%) at (K) + 300(K), and In the case where oxygen (O2) is used as the atmosphere gas for analysis in the above TGA, the oxygen (O2) gas supply flow rate is 20 mL / min, the analysis temperature range is from room temperature to 1,200℃, and the heating rate is 5℃ / min. In the case where nitrogen (N2) or argon (Ar) is used as the atmosphere gas for analysis in the above TGA, the nitrogen (N2) or argon (Ar) gas supply flow rate is 20 mL / min, the analysis temperature range is from room temperature to 1,200℃, and the heating rate is 5℃ / min. The first stage structural collapse section of the above positive active material is a section where the structure of the above positive active material collapses and weight reduction occurs.

2. In Paragraph 1, A positive electrode active material for a lithium secondary battery having a nickel (Ni) content of more than 90 mol% and less than 98 mol%.

3. In Paragraph 1, A positive electrode active material for a lithium secondary battery, wherein the above A is 0.38 (wt%) to 2.00 (wt%).

4. In Paragraph 1, A positive electrode active material for a lithium secondary battery, wherein the above B is 0.50 (wt%) to 2.75 (wt%).

5. In Paragraph 1, The above positive active material comprises nickel and one or more selected from the group consisting of cobalt, manganese, and aluminum, for a lithium secondary battery.

6. A method for manufacturing the positive electrode active material of any one of claims 1 to 5, a) a precursor manufacturing step for manufacturing a precursor for a positive electrode active material; b) a step of producing a primary positive active material by performing a primary heat treatment on a material containing the manufactured precursor; and c) a step of manufacturing a secondary positive active material by performing a secondary heat treatment on a material containing the primary positive active material; A method for manufacturing a positive electrode active material for a lithium secondary battery, comprising 7. In Paragraph 6, c) After step, d) a step of manufacturing a tertiary positive active material by performing a tertiary heat treatment on a material containing the above secondary positive active material; A method for manufacturing a positive electrode active material for a lithium secondary battery, further comprising 8. A positive electrode for a lithium secondary battery comprising the positive electrode active material of any one of paragraphs 1 to 5.

9. A lithium secondary battery comprising the positive electrode of paragraph 8.