Quantum dot composition, cured film, and display device

A quantum dot composition with a ligand mixture and solvent-free formulation addresses efficiency degradation, ensuring high brightness and stability in display devices by improving dispersibility and luminance ratios.

WO2026240379A1PCT designated stage Publication Date: 2026-11-19SAMSUNG SDI CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2026/005683
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-12
Filing Date
2026-04-29
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Quantum dot compositions face challenges in maintaining photoelectric efficiency and external quantum efficiency during thermal processes, leading to degradation and reduced performance in display devices.

Method used

A quantum dot composition with a specific ligand mixture of compounds (Formula 1 and Formula 2) and a solvent-free formulation, including photocurable monomers and light scattering agents, enhances dispersibility and stability, improving frontal and side luminance ratios.

Benefits of technology

The composition maintains high external quantum efficiency and photoconversion retention, enhancing display device performance by improving brightness uniformity and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2026005683_19112026_PF_FP_ABST
    Figure KR2026005683_19112026_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a quantum dot composition, a cured film, and a display device. Specifically, provided are a quantum dot composition, a cured film, and a display device, the quantum dot composition comprising quantum dot having ligands, wherein the ligands comprise a compound of chemical formula 1 and a compound of chemical formula 2.
Need to check novelty before this filing date? Find Prior Art

Description

Quantum dot composition, cured film, and display device

[0001] This relates to a quantum dot composition, a cured film, and a display device.

[0002]

[0003] Quantum dot compositions containing quantum dots (QDs) are required to have good patternability while preventing the degradation of photoelectric efficiency of quantum dots during thermal processes, exposure, development, washing, deposition, and subsequent thermal processes, and to increase productivity. The cured film formed from the above composition may experience a decrease in the external quantum efficiency and photoelectric conversion retention rate of the quantum dots as it undergoes subsequent thermal processes.

[0004] A cured film is desirable in which the external quantum efficiency and photoconversion retention rate of the cured film can be maintained even after undergoing thermal curing and subsequent thermal processes following photocuring.

[0005]

[0006] The invention provides a quantum dot composition that offers improved dispersibility of quantum dots.

[0007] The present invention provides a quantum dot composition that improves frontal luminance and improves the ratio of side luminance to frontal luminance.

[0008]

[0009] According to one embodiment, a quantum dot composition is provided.

[0010] 1. A quantum dot composition comprises quantum dots having ligands, wherein the ligand comprises a mixture of a compound of Formula 1 below and a compound of Formula 2 below:

[0011] [Chemical Formula 1]

[0012]

[0013] (In the above chemical formula 1,

[0014] L 11 , L 12 , L 13 , R 1 and n are the same as defined in the description of the invention below).

[0015] [Chemical Formula 2]

[0016]

[0017] (In the above chemical formula 2,

[0018] L 21 , L 22 , L 23 and n are the same as defined in the description of the invention below).

[0019] In 2.1, in the above chemical formula 2, L 22 A quantum dot composition having a straight-chain or branched-chain alkylene group having 1 to 10 carbon atoms.

[0020] 3.1 to 2, wherein the compound of Formula 2 is a compound of Formula 2-1 below, a quantum dot composition:

[0021] [Chemical Formula 2-1]

[0022]

[0023] 4.1 to 3, wherein the compound of Formula 1 is a compound of Formula 1-11 below, quantum dot composition:

[0024] [Chemical Formula 1-11]

[0025]

[0026] (n is an integer from 1 to 10).

[0027] 5.1 to 4, wherein the compound of Formula 1 is included in an amount of 30 to 90 weight percent of the total ligands of the quantum dots.

[0028] 6.1 to 5, wherein the compound of Formula 2 is included in an amount of 10 to 70 weight% of the total ligands of the quantum dots.

[0029] 7.1 to 6, wherein the quantum dot composition further comprises one or more of a photocurable monomer having unsaturated bonds and an initiator.

[0030] 8.1 to 7, wherein the composition is a solvent-free composition, a quantum dot composition.

[0031] 9.1 to 8, wherein the composition further comprises one or more of a light scattering agent and a polymerization inhibitor.

[0032] 10.1 to 9, wherein the quantum dots are non-cadmium light-emitting materials comprising one or more of InP / ZnS and InP / ZnSe / ZnS, a quantum dot composition.

[0033] 11.1 to 10, wherein the quantum dot comprises a core comprising Ag, In, Ga and S; and a shell comprising at least two selected from the group consisting of Ag, Ga, Zn and S.

[0034] According to another embodiment, a hardened film is provided.

[0035] The above-mentioned cured film comprises a cured product of the quantum dot compositions 1 to 11.

[0036] According to another embodiment, a display device is provided.

[0037] The above display device includes the above cured film.

[0038]

[0039] A uniform light dispersion effect was provided by providing improved dispersibility of the quantum dots.

[0040] The screen quality of the display device can be improved by improving front brightness and improving the ratio of side brightness to front brightness.

[0041]

[0042] FIG. 1 is a conceptual diagram of a display device according to one embodiment.

[0043] Figures 2, 3, and 4 are the results of the dispersibility evaluation of quantum dots of Example 1, Example 2, and Comparative Example 1, respectively.

[0044]

[0045] Embodiments of the present application will be described in more detail with reference to the attached drawings. However, the technology disclosed in the present application is not limited to the embodiments described herein and may be embodied in other forms. The embodiments introduced herein are provided merely to ensure that the disclosed content is thorough and complete and to ensure that the spirit of the present application is sufficiently conveyed to those skilled in the art. In the drawings, the dimensions, such as the width or thickness of the components, are shown slightly enlarged to clearly represent the components of each device, and the dimensions, such as the width or thickness of the components, are not limited to the scope of the present invention. In a plurality of drawings, the same reference numerals refer to substantially identical components.

[0046] The terms used herein are for describing exemplary embodiments only and are not intended to limit the invention. The singular expression includes the plural expression unless the context clearly indicates otherwise.

[0047] In this specification, "upper" and "lower" are defined based on the drawings, and depending on the viewing perspective, "upper" may be changed to "lower" and "lower" to "upper." Additionally, terms referred to as "on" or "on" may include not only the direct upper portion but also cases where other structures are interposed in between. Conversely, terms referred to as "directly on," "immediately on," or "directly formed" indicate the absence of other structures, such as intermediate bodies.

[0048] Unless otherwise specifically stated in this specification, "alkyl group" means a C1 to C20 alkyl group, "alkenyl group" means a C2 to C20 alkenyl group, "cycloalkenyl group" means a C3 to C20 cycloalkenyl group, "heterocycloalkenyl group" means a C3 to C20 heterocycloalkenyl group, "aryl group" means a C6 to C20 aryl group, "arylalkyl group" means a C6 to C20 arylalkyl group, "alkylene group" means a C1 to C20 alkylene group, "arylene group" means a C6 to C20 arylene group, "alkylarylene group" means a C6 to C20 alkylarylene group, "heteroarylene group" means a C3 to C20 heteroarylene group, and "alkoxylene group" means a C1 to C20 alkoxylene group It means.

[0049] Unless specifically stated in this specification, "substitution" means that at least one hydrogen atom is a halogen atom (F, Cl, Br, I), a hydroxyl group, a C1 to C20 alkoxy group, a nitro group, a cyano group, an amine group, an imino group, an azido group, an amidino group, a hydrazino group, a hydrazono group, a carbonyl group, a carbamyl group, a thiol group, an ester group, an ether group, a carboxyl group or a salt thereof, a sulfonic acid group or a salt thereof, a phosphoric acid or a salt thereof, a C1 to C20 alkyl group, a C2 to C20 alkenyl group, a C2 to C20 alkynyl group, a C6 to C20 aryl group, a C7 to C20 arylalkyl group, a C3 to C20 cycloalkyl group, a C3 to C20 cycloalkenyl group, a C3 to C20 cycloalkynyl group, a C2 to C20 heterocycloalkyl group, or C2 to C20 It means being substituted with a heterocycloalkenyl group, a C2 to C20 heterocycloalkenyl group, a C3 to C20 heteroaryl group, or a combination thereof.

[0050] Additionally, unless otherwise specifically stated in this specification, "(meth)acrylate" means that both "acrylate" and "methacrylate" are possible, and "(meth)acrylic acid" means that both "acrylic acid" and "methacrylic acid" are possible.

[0051] Unless otherwise specified herein, "combination" means mixing or copolymerization.

[0052] Unless otherwise defined in the chemical formulas within this specification, if a chemical bond is not depicted at a position where a chemical bond should be depicted, it means that a hydrogen atom is bonded at said position.

[0053] In the present specification, when describing a numerical range, "X to Y" means X or greater and Y or less (X ≤ and ≤Y).

[0054] According to one embodiment, a quantum dot composition with improved dispersibility of quantum dots is provided. This can provide a uniform light dispersion effect.

[0055] According to one embodiment, a quantum dot composition is provided that improves front brightness and improves the ratio of side brightness to front brightness. This can improve the screen quality of a display device.

[0056] According to one embodiment, the quantum dot composition may preferably have a viscosity of 5 to 27 cps at 25°C. Within this range, inkjetting properties are excellent, allowing for the formation of a uniform cured film and improving processability.

[0057] According to one embodiment, the quantum dot composition may be solvent-free. Although the composition is solvent-free, it may have excellent inkjet jetting properties.

[0058] According to one embodiment, a quantum dot composition comprises a quantum dot having a ligand, and said ligand comprises a compound of Formula 1 below:

[0059] [Chemical Formula 1]

[0060]

[0061] (In the above chemical formula 1,

[0062] R 1 is a substituted or unsubstituted C1 to C10 alkyl group or a substituted or unsubstituted C6 to C20 aryl group, and

[0063] L 11 to L 13 Each is an independently substituted or unsubstituted C1 to C10 alkylene group, ester group, or ether group, and

[0064] n is an integer from 1 to 20).

[0065] In the above chemical formula 1, L 12 ga is an ester group and at the same time L 13 When this is an unsubstituted C1 to C10 alkylene group, n can be an integer from 4 to 20.

[0066] In the above chemical formula 1, L 11 and L 13 is each independently a substituted or unsubstituted C1 to C10 alkylene group, and L 12 It can be an ester group (*-C(=O)O-* or *-O(C=O)-*) or an ether group (*-O-*).

[0067] The compound represented by the above chemical formula 1 may include at least one selected from the group consisting of the following chemical formulas 1-1 to 1-10, but is not necessarily limited thereto.

[0068] [Chemical Formula 1-1]

[0069]

[0070] [Chemical Formula 1-2]

[0071]

[0072] [Chemical Formula 1-3]

[0073]

[0074] [Chemical Formula 1-4]

[0075]

[0076] [Chemical Formula 1-5]

[0077]

[0078] [Chemical Formula 1-6]

[0079]

[0080] [Chemical Formula 1-7]

[0081]

[0082] [Chemical Formula 1-8]

[0083]

[0084] [Chemical Formula 1-9]

[0085]

[0086] [Chemical Formula 1-10]

[0087]

[0088] For example, the compound of Chemical Formula 1 above may be a compound of Chemical Formula 1-11 below:

[0089] [Chemical Formula 1-11]

[0090]

[0091] (n is an integer from 1 to 10).

[0092] The compound of Chemical Formula 1 above can contribute to increasing external quantum efficiency after photocuring and subsequent processes of the quantum dot composition.

[0093] In one embodiment, the compound of Formula 1 may be included in an amount of 30 to 90 weight percent of the total ligands of the quantum dots. Within this range, the external quantum efficiency of the quantum dot composition can be increased, and a brightness improvement effect can be provided. For example, the compound of Formula 1 may be included in an amount of 30 to 70 weight percent of the total ligands of the quantum dots.

[0094] A cured film formed from a quantum dot composition containing quantum dots having the compound of Chemical Formula 1 as a ligand may not have an insufficient effect on improving frontal brightness, and the ratio of lateral brightness to frontal brightness may not be sufficiently high. The compound of Chemical Formula 1 is a compound having a primary thiol group (-SH) as shown in Chemical Formula 1. Therefore, when a quantum dot composition containing the compound of Chemical Formula 1 as a ligand is cured, the quantum dots and the photocurable monomer are separated from each other, causing the quantum dots to aggregate independently of the photocurable monomer. This lowers frontal brightness by blocking the transmission of light emitted from a light source, and

[0095] Here, 'photocurable monomer' may refer to a monomer that disperses quantum dots in a quantum dot composition and forms a matrix that forms the cured film. The photocurable monomer may be a photocurable monomer having unsaturated bonds as described below.

[0096] The above quantum dot comprises, in addition to the compound of Formula 1, a compound of Formula 2 as a ligand:

[0097] [Chemical Formula 2]

[0098]

[0099] (In the above chemical formula 2,

[0100] L 21 Silver oxygen,

[0101] L 22 is a straight-chain or branched-chain alkylene group having 1 to 20 carbon atoms,

[0102] L 23 Silver hydrogen or methyl group,

[0103] n is an integer from 1 to 10)

[0104] Quantum dots having a mixture of the compound of Formula 1 and the compound of Formula 2 as ligands can improve frontal brightness and improve the ratio of side brightness to frontal brightness. This is because the compound of Formula 2 simultaneously possesses a phosphoric acid group capable of binding to quantum dots and a (meth)acrylate group capable of reacting with the photocurable monomer. Therefore, by directly participating in the curing reaction of the photocurable monomer, the compound of Formula 2 prevents the aggregation of quantum dots within the cured film, thereby improving the transmission of light emitted from the light source and enabling the realization of maximum frontal brightness while satisfying the optimal frontal-side brightness ratio.

[0105] With respect to the ratio of side luminance to front luminance, in a display device having a cured film formed of the quantum dot composition, the RL (ratio of luminance) value of Formula 1 below may be 75 to 85%:

[0106] [Equation 1]

[0107] RL value = [(530T) / (450A)] x 100.

[0108] (In the above Equation 1,

[0109] 530T is the light transmittance at a wavelength of 530 nm (unit: %) when driving a display device equipped with the above-mentioned cured film,

[0110] 450A is the absorption rate at a wavelength of 450 nm (unit: %) when driving a display device equipped with the above-mentioned cured film.

[0111] When the above RL value is 75 to 85%, the front brightness can be increased and the ratio of side brightness to front brightness can be increased.

[0112] In one embodiment, in the above formula 2, L 22 It may be a straight-chain or branched-chain alkylene group having 1 to 10 carbon atoms, or a straight-chain or branched-chain alkylene group having 1 to 5 carbon atoms.

[0113] In one specific example, in the above chemical formula 2, n may be an integer from 1 to 5.

[0114] For example, the compound of Chemical Formula 2 above may be the compound of Chemical Formula 2-1 below:

[0115] [Chemical Formula 2-1]

[0116]

[0117] The compound of Formula 2 above may be included in an amount of 10 to 70 weight percent of the total ligands of the quantum dot. Within this range, the frontal brightness can be increased and the ratio of lateral brightness to frontal brightness can be increased. For example, the compound of Formula 2 above may be included in an amount of 30 to 70 weight percent of the total ligands of the quantum dot.

[0118] The total sum of the compound of Formula 1 and the compound of Formula 2 may be included in an amount of 95% or more by weight, for example, 95 to 100% by weight, or 100% by weight, of the total ligands of the quantum dot.

[0119] The above quantum dots can have a maximum fluorescence emission wavelength at 500 nm to 680 nm.

[0120] Surface modification of quantum dots by the compound of Formula 1 and the compound of Formula 2 can be performed by referring to methods known to those skilled in the art.

[0121] In the case where the quantum dot composition according to one embodiment is a solvent-free quantum dot composition, the quantum dots may be included in an amount of 5 to 60 weight%, for example, 10 to 60 weight%, 20 to 60 weight%, or 30 to 50 weight%. When the quantum dots are included within the above range, high light retention rate and light efficiency can be achieved even after curing.

[0122] In the case where the quantum dot composition according to one embodiment is a quantum dot composition containing a solvent, the quantum dots may be included in an amount of 1 to 40 weight%, for example, 3 to 30 weight%, relative to the total amount of the quantum dot composition. When the quantum dots are included within the above range, the photoconversion rate is excellent, and excellent processability can be achieved without impairing pattern characteristics and development characteristics.

[0123] The above quantum dots absorb light in a wavelength range of 360 nm to 780 nm, for example, a wavelength range of 400 nm to 780 nm, and emit fluorescence in a wavelength range of 500 nm to 700 nm, for example, 500 nm to 580 nm, or 600 nm to 680 nm. That is, the above quantum dots have a maximum fluorescence emission wavelength (fluorescence λ) at 500 nm to 680 nm. em Can have ).

[0124] Each of the above quantum dots can independently have a full width at half maximum (FWHM) of 20 nm to 100 nm, for example, 20 nm to 50 nm. When the quantum dots have a full width at half maximum within the above range, the color purity is high, so when used as a color material in a color filter, there is an effect of increasing the color reproduction rate.

[0125] Each of the above quantum dots may independently be organic, inorganic, or a hybrid of organic and inorganic materials.

[0126] The above quantum dots may each independently be composed of a core and a shell surrounding the core, and the core and shell may each independently have structures such as a core, core / shell, core / first shell / second shell, alloy, alloy / shell, etc., composed of Group II-IV, Group III-V, etc., but are not limited thereto.

[0127] For example, the core may comprise at least one material selected from the group consisting of CdS, CdSe, CdTe, ZnS, ZnSe, ZnTe, HgS, HgSe, HgTe, GaN, GaP, GaAs, InP, InAs, and alloys thereof, but is not necessarily limited thereto. The shell surrounding the core may comprise at least one material selected from the group consisting of CdSe, ZnSe, ZnS, ZnTe, CdTe, PbS, TiO, SrSe, HgSe, and alloys thereof, but is not necessarily limited thereto.

[0128] In one embodiment, as global interest in the environment has recently increased significantly and regulations on toxic substances are being strengthened, an environmentally friendly non-cadmium light-emitting material (InP / ZnS, InP / ZnSe / ZnS, etc.) with a somewhat lower quantum yield was used instead of a light-emitting material having a cadmium-based core, but it is not necessarily limited to this.

[0129] In one embodiment, the core of the quantum dot comprises a core comprising Ag, In, Ga, and S; and a shell comprising at least two selected from the group consisting of Ag, Ga, Zn, and S. The quantum dot may have one or more ligands, and the first ligand may include a halide, and the second ligand may include an alkyl group or an alkoxyamine, but is not necessarily limited thereto.

[0130] In the case of the above-mentioned core / shell structured quantum dots, the size (average particle size) of each of the total quantum dots including the shell may be 1 nm to 15 nm, for example, 5 nm to 15 nm.

[0131] For example, the above quantum dots may each independently include red quantum dots, green quantum dots, or a combination thereof. Each of the above red quantum dots may each independently have an average particle size of 10 nm to 15 nm. Each of the above green quantum dots may each independently have an average particle size of 5 nm to 8 nm.

[0132] Meanwhile, to ensure the dispersion stability of the quantum dots, the quantum dot composition according to one embodiment may further include a dispersant. The dispersant helps to uniformly disperse a photoconversion material, such as quantum dots, within the quantum dot composition, and may be a nonionic, anionic, or cationic dispersant. Specifically, polyalkylene glycol or esters thereof, polyoxyalkylene, polyhydric alcohol ester alkylene oxide adduct, alcohol alkylene oxide adduct, sulfonic acid ester, sulfonic acid salt, carboxylic acid ester, carboxylic acid salt, alkylamide alkylene oxide adduct, alkyl amine, etc., may be used, and these may be used alone or in a mixture of two or more. The dispersant may be used in an amount of 0.1% to 100% by weight, for example, 10% to 20% by weight, relative to the solid content of the photoconversion material, such as quantum dots.

[0133] Photocurable monomer having unsaturated bonds

[0134] The above quantum dot composition comprises a photocurable monomer containing unsaturated bonds. For example, the photocurable monomer may be a photocurable monomer having a carbon-carbon double bond at the terminal.

[0135] The above photocurable monomer may be included in an amount of 30 to 70 weight%, for example 40 to 70 weight%, 45 to 65 weight%, or 45 to 60 weight% based on the total amount (e.g., based on solid content) of the above quantum dot composition. Within the above range, it is possible to manufacture a composition having a viscosity that allows for inkjet jetting, particularly a solvent-free quantum dot composition, and also the quantum dots in the manufactured composition, particularly the solvent-free quantum dot composition, may have excellent dispersibility, thereby improving optical properties.

[0136] The above photocurable monomer may have a molecular weight of 150 g / mol to 1,000 g / mol. Within this range, it may be advantageous for ink-jetting as it does not increase the viscosity of the composition without impairing the optical properties of the quantum dots.

[0137] The above photocurable monomer may be represented by the following chemical formula 3, but is not necessarily limited thereto:

[0138] [Chemical Formula 3]

[0139]

[0140] (In the above chemical formula 3,

[0141] R 1 and R 2 Each is independently a hydrogen atom or a substituted or unsubstituted C1 to C10 alkyl group, and

[0142] L 41 and L 43 Each is an independently substituted or unsubstituted C1 to C10 alkylene group, and

[0143] L 42 is a substituted or unsubstituted C1 to C10 alkylene or ether group (*-O-*).

[0144] For example, the above photocurable monomer may include one or more of the following chemical formulas 3-1 and 3-2, but is not necessarily limited thereto.

[0145] [Chemical Formula 3-1]

[0146]

[0147] [Chemical Formula 3-2]

[0148]

[0149] For example, in addition to the compounds represented by Chemical Formula 3-1 and Chemical Formula 3-2, the above photocurable monomer comprises ethylene glycol diacrylate, triethylene glycol diacrylate, 1,4-butanediol diacrylate, 1,6-hexanediol diacrylate, neopentyl glycol diacrylate, pentaerythritol diacrylate, pentaerythritol triacrylate, dipentaerythritol diacrylate, dipentaerythritol triacrylate, dipentaerythritol pentaacrylate, pentaerythritol hexaacrylate, bisphenol A diacrylate, trimethylolpropane triacrylate, novolac epoxyacrylate, ethylene glycol dimethacrylate, triethylene glycol dimethacrylate, propylene glycol dimethacrylate, 1,4-butanediol dimethacrylate, It may further include 1,6-hexanediol dimethacrylate or a combination thereof.

[0150] Initiator

[0151] A curable composition according to one embodiment may further include an initiator, such as a photopolymerization initiator, a thermal polymerization initiator, or a combination thereof.

[0152] The above photopolymerization initiator is an initiator capable of initiating a polymerization reaction by light, and examples include acetophenone-based compounds, benzophenone-based compounds, thioxantone-based compounds, benzoin-based compounds, triazine-based compounds, oxime-based compounds, aminoketone-based compounds, etc., but are not necessarily limited thereto.

[0153] Examples of the above acetophenone-based compounds include 2,2'-diethoxyacetophenone, 2,2'-dibutoxyacetophenone, 2-hydroxy-2-methylpropiophenone, pt-butyltrichloroacetophenone, pt-butyldichloroacetophenone, 4-chloroacetophenone, 2,2'-dichloro-4-phenoxyacetophenone, 2-methyl-1-(4-(methylthio)phenyl)-2-morpholinopropan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butan-1-one, etc.

[0154] Examples of the above benzophenone compounds include benzophenone, benzoyl benzoic acid, methyl benzoyl benzoate, 4-phenyl benzophenone, hydroxybenzophenone, acrylated benzophenone, 4,4'-bis(dimethylamino)benzophenone, 4,4'-bis(diethylamino)benzophenone, 4,4'-dimethylaminobenzophenone, 4,4'-dichlorobenzophenone, 3,3'-dimethyl-2-methoxybenzophenone, etc.

[0155] Examples of the above thioxanthonic compounds include thioxanthon, 2-methylthioxanthon, isopropylthioxanthon, 2,4-diethylthioxanthon, 2,4-diisopropylthioxanthon, 2-chlorothioxanthon, etc.

[0156] Examples of the above-mentioned benzoin compounds include benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin isobutyl ether, benzyl dimethyl ketal, etc.

[0157] Examples of the above triazine compounds include 2,4,6-trichloro-s-triazine, 2-phenyl-4,6-bis(trichloromethyl)-s-triazine, 2-(3',4'-dimethoxystyryl)-4,6-bis(trichloromethyl)-s-triazine, 2-(4'-methoxynaphthyl)-4,6-bis(trichloromethyl)-s-triazine, 2-(p-methoxyphenyl)-4,6-bis(trichloromethyl)-s-triazine, 2-(p-tolyl)-4,6-bis(trichloromethyl)-s-triazine, 2-biphenyl-4,6-bis(trichloromethyl)-s-triazine, and bis(trichloromethyl)-6-styryl-s-triazine. Examples include 2-(naphtho-1-yl)-4,6-bis(trichloromethyl)-s-triazine, 2-(4-methoxynaphtho-1-yl)-4,6-bis(trichloromethyl)-s-triazine, 2-4-bis(trichloromethyl)-6-piperonyl-s-triazine, 2-4-bis(trichloromethyl)-6-(4-methoxystyryl)-s-triazine, etc.

[0158] Examples of the above oxime compounds include O-acyloxime compounds, 2-(O-benzoyloxime)-1-[4-(phenylthio)phenyl]-1,2-octanedione, 1-(O-acetyloxime)-1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazole-3-yl]ethanolone, O-ethoxycarbonyl-α-oxyamino-1-phenylpropan-1-one, etc. Specific examples of the above O-acyloxime compounds include 1,2-octanedione, 2-dimethylamino-2-(4-methylbenzyl)-1-(4-morpholine-4-yl-phenyl)-butan-1-one, 1-(4-phenylsulfanylphenyl)-butan-1,2-dione-2-oxime-O-benzoate, 1-(4-phenylsulfanylphenyl)-octan-1,2-dione-2-oxime-O-benzoate, 1-(4-phenylsulfanylphenyl)-octan-1-one-oxime-O-acetate, and 1-(4-phenylsulfanylphenyl)-butan-1-one-oxime-O-acetate.

[0159] Examples of the above aminoketone compounds include 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1 (2-Benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1).

[0160] In addition to the above compounds, the above photopolymerization initiator may use carbazole compounds, diketone compounds, sulfonium borate compounds, diazo compounds, imidazole compounds, non-imidazole compounds, etc.

[0161] The above photopolymerization initiator may also be used together with a photosensitizer that causes a chemical reaction by absorbing light, becoming excited, and then transferring that energy.

[0162] Examples of the above-mentioned photosensitizers include tetraethylene glycol bis-3-mercaptopropionate, pentaerythritol tetrakis-3-mercaptopropionate, dipentaerythritol tetrakis-3-mercaptopropionate, etc.

[0163] Examples of the above-mentioned thermal polymerization initiators include peroxides, specifically benzoyl peroxide, dibenzoyl peroxide, lauryl peroxide, di-lauryl peroxide, di-tert-butyl peroxide, cyclohexane peroxide, methyl ethyl ketone peroxide, hydroperoxides (e.g., tert-butyl hydroperoxide, cumene hydroperoxide), dicyclohexyl peroxydicarbonate, 2,2-azobis(isobutyronitrile), t-butyl perbenzoate, etc., and 2,2'-azobis-2-methylpropionitrile, etc., but are not necessarily limited thereto, and any that is widely known in the art may be used.

[0164] The above initiator may be included in an amount of 0.1 to 5 weight%, for example, 1 to 4 weight%, relative to the total amount of the quantum dot composition (e.g., based on solid content). When included within the above range, sufficient curing occurs during photolithography or thermal curing, thereby obtaining excellent reliability, and the decrease in transmittance caused by unreacted initiator can be prevented, thereby preventing the degradation of the optical properties of the quantum dots.

[0165] Mining agent

[0166] A quantum dot composition according to one embodiment may further include a light scattering agent.

[0167] The light scattering agent may include barium sulfate (BaSO4), calcium carbonate (CaCO3), titanium dioxide (TiO2), zirconia (ZrO2), or a combination thereof.

[0168] The light scattering agent above reflects light that is not absorbed by the aforementioned quantum dots and enables the quantum dots to reabsorb the reflected light. That is, the light scattering agent increases the amount of light absorbed by the quantum dots, thereby increasing the light conversion efficiency of the quantum dot composition.

[0169] The above light scattering agent has an average particle size (D 50 The average particle size of the light diffusing agent may be 150 nm to 250 nm, and specifically, 180 nm to 230 nm. When the average particle size of the light diffusing agent is within the above range, it may have a superior light diffusing effect and increase light conversion efficiency.

[0170] The light scattering agent may be included in an amount of 1 to 20 weight%, e.g., 2 to 15 weight%, e.g., 3 to 10 weight%, relative to the total amount of the quantum dot composition (e.g., based on solid content). Within this range, an improvement in light conversion efficiency due to the use of the light scattering agent can be expected, and the problem of quantum dot sedimentation may not occur.

[0171] additives

[0172] To improve the stability and dispersibility of the above quantum dots, the solvent-free quantum dot composition according to one embodiment may further include a polymerization inhibitor.

[0173] The polymerization inhibitor may include hydroquinone-based compounds, catechol-based compounds, or combinations thereof, but is not necessarily limited thereto. As the solvent-free quantum dot composition according to one embodiment further includes the hydroquinone-based compounds, catechol-based compounds, or combinations thereof, crosslinking at room temperature can be prevented during exposure after printing (coating) the solvent-free quantum dot composition.

[0174] For example, the above hydroquinone-based compound, catechol-based compound, or combination thereof may include hydroquinone, methyl hydroquinone, methoxyhydroquinone, t-butyl hydroquinone, 2,5-di-t-butyl hydroquinone, 2,5-bis(1,1-dimethylbutyl) hydroquinone, 2,5-bis(1,1,3,3-tetramethylbutyl) hydroquinone, catechol, t-butyl catechol, 4-methoxyphenol, pyrogallol, 2,6-di-t-butyl-4-methylphenol, 2-naphthol, tris(N-hydroxy-N-nitrosophenylaminato-O,O')aluminium, or combinations thereof, but are not necessarily limited thereto.

[0175] The above hydroquinone-based compound, catechol-based compound, or a combination thereof may be used in the form of a dispersion, and the polymerization inhibitor in the form of the dispersion may be included in an amount of 0.001% to 3% by weight, for example, 0.1% to 2% by weight, based on the total amount of the solvent-free quantum dot composition. When the polymerization inhibitor is included within the above range, the problem of deterioration over time at room temperature can be solved, while simultaneously preventing a decrease in sensitivity and surface peeling.

[0176] The solvent in the above composition may be included in an amount of 2 parts by weight or less, for example, 0 to 2 parts by weight per 100 parts by weight based on the solid content of the above composition.

[0177] In addition, the quantum dot composition according to one embodiment may further include malonic acid; 3-amino-1,2-propanediol; a silane-based coupling agent; a leveling agent; a fluorine-based surfactant; or a combination thereof to improve heat resistance and reliability.

[0178] For example, the quantum dot composition according to one embodiment may further include a silane-based coupling agent having reactive substituents such as vinyl groups, carboxyl groups, methacrylate groups, isocyanate groups, and epoxy groups to improve adhesion to a substrate.

[0179] Examples of the above-mentioned silane coupling agents include trimethoxysilyl benzoic acid, γ-methacryloxypropyl trimethoxysilane, vinyltriacetoxysilane, vinyltrimethoxysilane, γ-isocyanate propyl triethoxysilane, γ-glycidoxypropyl trimethoxysilane, β-epoxycyclohexyl ethyltrimethoxysilane, etc., and these may be used alone or in a mixture of two or more.

[0180] The above silane-based coupling agent may be included in an amount of 0.01 to 10 parts by weight per 100 parts by weight of the quantum dot composition. When the silane-based coupling agent is included within the above range, adhesion, storage stability, etc. are excellent.

[0181] In addition, the solvent-free quantum dot composition may further include a surfactant, such as a fluorine-based surfactant, as needed to improve coating properties and prevent defect formation, i.e., to improve leveling performance. The fluorine-based surfactant may have a low weight-average molecular weight of 4,000 g / mol to 10,000 g / mol, specifically a weight-average molecular weight of 6,000 g / mol to 10,000 g / mol. Additionally, the fluorine-based surfactant may have a surface tension of 18 mN / m to 23 mN / m (measured in a 0.1% propylene glycol monomethyl ether acetate (PGMEA) solution). When the weight-average molecular weight and surface tension of the above-mentioned fluorine-based surfactant are within the above range, leveling performance can be further improved, staining can be prevented during high-speed coating, and since there is less bubble generation and fewer film defects, excellent characteristics are imparted to slit coating, a high-speed coating method.

[0182] In addition, the quantum dot composition according to one embodiment may use a silicone-based surfactant together with the aforementioned fluorine-based surfactant. Specific examples of the silicone-based surfactant include, but are not limited to, TSF400, TSF401, TSF410, and TSF4440 of Toshiba Silicon.

[0183] The surfactant, including the above-mentioned fluorine-based surfactant, etc., may be included in an amount of 0.01 to 5 parts by weight, for example, 0.1 to 2 parts by weight, per 100 parts by weight of the above-mentioned solvent-free quantum dot composition. When the above-mentioned surfactant is included within the above range, the phenomenon of foreign matter occurring in the sprayed composition is reduced.

[0184] In addition, the quantum dot composition according to one embodiment may further include a certain amount of other additives, such as antioxidants, within a range that does not impair physical properties.

[0185] Another aspect provides a cured film manufactured using the above quantum dot composition, and a display device including the above cured film.

[0186] According to one embodiment, the cured film comprises a cured product of the quantum dot composition.

[0187] One of the methods for manufacturing the above-described cured film comprises the step of forming a pattern by applying the above-described quantum dot composition onto a substrate using an inkjet jetting method (S1); and the step of curing the pattern (S2).

[0188] (S1) Step of forming a pattern

[0189] It is preferable to apply the above quantum dot composition onto a substrate with a thickness of 0.5 to 20 μm using an inkjet jetting method. The inkjet jetting can form a pattern by spraying only a single color per nozzle and repeatedly spraying according to the required number of colors, or it can form a pattern by simultaneously spraying the required number of colors through each inkjet nozzle to reduce the process.

[0190] The above inkjet jetting method may use an inkjet printer having an inkjet head equipped with a piezo-type nozzle that applies pressure according to voltage.

[0191] More specifically, the quantum dot composition is ejected onto a substrate from the nozzle of an inkjet head. At this time, the amount of the composition ejected may be 1 to 80 pL / time, for example, 1 to 30 pL / time, or as another example, 1 to 20 pL / time.

[0192] The aperture of the inkjet head may be 5 to 100 μm, for example, 10 to 80 μm, in order to minimize nozzle clogging and improve ejection precision, but is not limited thereto.

[0193] The ejection pressure of the inkjet head is 1,000 to 100,000s based on the shear rate. -1It may be, but is not limited to this.

[0194] The temperature at the time of discharge is not particularly limited, but from the viewpoint of suppressing crystallization of the material included in the ink composition, it may be 10 to 120°C, for example, 15 to 60°C, as another example, 15 to 40°C, and as yet another example, 20 to 35°C.

[0195] (S2) Curing step

[0196] Pixels can be obtained by curing the pattern obtained above. At this time, a photocuring process can be applied as a method for curing. The photocuring process irradiates active rays such as UV rays with a wavelength of 190 nm to 450 nm, for example, 200 nm to 500 nm. As light sources used for irradiation, low-pressure mercury lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, metal halide lamps, argon gas lasers, etc., can be used, and in some cases, X-rays, electron beams, etc., can also be used.

[0197] Another method for manufacturing the above-mentioned cured film is to manufacture the cured film using a lithography method with the aforementioned quantum dot composition, and the manufacturing method is as follows.

[0198] (1) Coating and film formation step

[0199] The aforementioned quantum dot composition is applied to a substrate that has undergone a predetermined pretreatment using a spin or slit coating method, a roll coating method, a screen printing method, an applicator method, etc., to a desired thickness, for example, 2 μm to 10 μm, and then a film is formed by removing the solvent by heating at a temperature of 70°C to 90°C for 1 minute to 10 minutes.

[0200] (2) Exposure step

[0201] After interposing a mask of a predetermined shape to form a pattern required on the above-mentioned coating film, active rays such as UV light of 190 nm to 450 nm, for example 200 nm to 500 nm, are irradiated. As a light source used for irradiation, a low-pressure mercury lamp, a high-pressure mercury lamp, an ultra-high-pressure mercury lamp, a metal halide lamp, an argon gas laser, etc., may be used, and in some cases, X-rays, electron beams, etc., may also be used.

[0202] The exposure amount varies depending on the type, mixing amount, and dry film thickness of each component of the quantum dot composition, but, for example, when using a high-pressure mercury lamp, it is 500 mJ / cm² 2  It is less than (based on a 365 nm sensor).

[0203] (3) Phenomenon stage

[0204] Following the above exposure step, an alkaline aqueous solution is used as a developer to dissolve and remove unnecessary parts, thereby leaving only the exposed areas to form an image pattern. That is, when developed with an alkaline developer, the unexposed areas are dissolved, and an image color filter pattern is formed.

[0205] (4) Post-processing step

[0206] The image pattern obtained by the above phenomenon can be cured by reheating or irradiating with active rays to obtain a pattern that is excellent in terms of heat resistance, light resistance, adhesion, crack resistance, chemical resistance, high strength, storage stability, etc.

[0207] Another perspective display device includes the above-mentioned hardened film.

[0208] According to one embodiment, the display device includes a color filter layer comprising the cured film. According to one embodiment, the display device may be a light-emitting element display device including an organic light-emitting display device.

[0209] FIG. 1 is a cross-sectional view of a light-emitting element display device according to one embodiment.

[0210] Referring to FIG. 1, a display device (11) according to one embodiment comprises a first substrate (111), two or more first electrodes (112) formed on the first substrate (111), a pixel defining film (113) formed between adjacent first electrodes (112), an organic light-emitting layer (120) formed on each of the first electrodes (112) and emitting a first light, a second electrode layer (114) formed on the organic light-emitting layer (120), and a first flattening layer (115) formed on the second electrode layer (114); a sealing layer (119) formed on the first flattening layer (115), a second flattening layer (118) formed on the sealing layer (119), and quantum dots (3, 3r, 3g) formed on the second flattening layer (118) that convert the first light into at least one of a different second light and a third light. It includes a color filter layer (130) and a second substrate (116) formed on the color filter layer (130).

[0211] In a display device (11) according to one embodiment, the organic light-emitting layer (120) may be defined as a first pixel area, a second pixel area, and a third pixel area, and each pixel area is spaced apart by a pixel defining film (113) at a predetermined interval. In one embodiment, the unit layer belonging to the first to third pixel areas among the organic light-emitting layer (120) is defined as the first to third organic light-emitting layers (120a to 120c), respectively.

[0212] The color filter layer (130) is formed to cover the space between adjacent light-blocking members (117). The color filter layer (130) includes first to third color filters (130r, 130g, 130b) formed at positions that overlap with the aforementioned first to third pixel regions, respectively.

[0213] In one embodiment, the first color filter (130r) may emit a second light different from the first light, the second color filter (130g) may emit a third light different from the first light, and the third color filter (130b) may emit the first light. For example, the first light may be blue light, the second light may be red light, and the third light may be green light.

[0214] Although not shown in FIG. 1, the display device may further include a color conversion layer.

[0215]

[0216] Hereinafter, the structure and operation of the present invention will be explained in more detail through preferred embodiments of the present invention. However, these are presented as preferred examples of the present invention and should not be interpreted in any way as limiting the present invention.

[0217]

[0218] The detailed specifications of the components used in the examples and comparative examples are as follows.

[0219] (Preparation of quantum dot composition)

[0220] (A) Quantum dot: Surface-modified quantum dot

[0221] (B) Photocurable monomer having an unsaturated double bond; 1,6-hexanediol diacrylate (HDDA, Miwon Specialty Chemical Co.)

[0222] (C) Photopolymerization initiator: TPO-L (Polynetran)

[0223] (D) Light scattering agent: Titanium dioxide dispersion (rutile type TiO2; D50 (180 nm), solid content 50 wt%, Iridos Co., Ltd.)

[0224] (E) Polymerization inhibitor: Methylhydroquinone (TOKYO CHEMICAL)

[0225]

[0226] Example 1

[0227] Preparation of surface-modified quantum dots

[0228] A magnetic bar is placed in a three-necked round-bottom flask, and a green quantum dot dispersion solution (InP / ZnSe / ZnS, core / first shell / second shell, Hansol Chemical; quantum dot solid content 23 wt%) is added.

[0229] In the above flask, the compound of Chemical Formula 1-10 and the compound of Chemical Formula 2-1 are added in a weight ratio of 70:30 out of a total of 100 parts by weight, catalyst zinc acetate is added, and the mixture is stirred for 10 hours at 80°C under a nitrogen atmosphere. At this time, the total amount of the compound of Chemical Formula 1-10 and the compound of Chemical Formula 2-1 is 30 parts by weight and the catalyst is 3 parts by weight, relative to 100 parts by weight of the quantum dots.

[0230] After the reaction is finished, the solution is cooled to room temperature (23°C), and then the quantum dot reaction solution obtained by the above reaction is added to cyclohexane to obtain a precipitate. The precipitate and cyclohexane are separated by centrifugation, and the precipitate is sufficiently dried in a vacuum oven for one day to obtain green quantum dots surface-modified with the two compounds above.

[0231] [Chemical Formula 1-10]

[0232]

[0233] [Chemical Formula 2-1]

[0234]

[0235] Based on solid content, 41 parts by weight of the surface-modified green quantum dots prepared above and 51.95 parts by weight of a photocurable monomer having unsaturated double bonds are mixed and stirred at room temperature for 12 hours. 0.05 parts by weight of a polymerization inhibitor are added and stirred at room temperature for 5 minutes. Subsequently, 3 parts by weight of a photopolymerization initiator and 4 parts by weight of a light scattering agent are added and mixed to prepare a solvent-free quantum dot composition.

[0236]

[0237] Example 2

[0238] A quantum dot composition was prepared in the same manner as in Example 1, except that the compound of Formula 1-10 and the compound of Formula 2-1 were added in a weight ratio of 30:70 out of a total of 100 parts by weight in Example 1.

[0239]

[0240] Comparative Example 1

[0241] A quantum dot composition was prepared in the same manner as in Example 1, except that in Example 1, the compound of Formula 1-10 and the compound of Formula 2-1 were added in a weight ratio of 100:0 out of a total of 100 parts by weight.

[0242]

[0243] Comparative Example 2

[0244] A quantum dot composition was prepared in the same manner as in Example 1, except that the compound of Formula 2-1 was not used in Example 1, and instead, the compound of Formula 1-10 and the compound of Formula 4 below were added in a weight ratio of 70:30 out of a total of 100 parts by weight.

[0245] [Chemical Formula 4]

[0246]

[0247]

[0248] Comparative Example 3

[0249] In Comparative Example 2, a quantum dot composition was prepared in the same manner as in Example 1, except that the compound of Formula 1-10 and the compound of Formula 4 below were added in a weight ratio of 30:70 out of a total of 100 parts by weight.

[0250] [Chemical Formula 4]

[0251]

[0252] The properties of the manufactured quantum dot compositions in Table 1 below were evaluated, and the results are shown in Table 1 and Figures 2 to 4 below.

[0253]

[0254] (1) Absorption rate, light transmittance, and RL value

[0255] Each quantum dot composition corresponding to the examples and comparative examples was coated to a thickness of 15 μm on yellow photoresist (YPR) using a spin coater (Mikasa, opticoat MS-A150, 800 rpm, 5 sec), and UV exposure was applied at 5000 mJ / cm² in an exposure unit (wavelength 395 nm) under a nitrogen atmosphere. 2 A single film (2 cm x 2 cm) was produced by exposure to light (83℃, 10 seconds).

[0256] Subsequently, the above film is cured (POB) for 30 minutes in a hot air circulating drying oven in a nitrogen atmosphere at 180°C for 30 minutes, and then cooled for 1 hour. Afterward, the absorption rate at a wavelength of 450 nm and the light transmittance at a wavelength of 530 nm were measured for the above film using an integrating hemisphere quantum efficiency meter (Otsuka, QE-2100), and the RL value was calculated according to Equation 1. When the RL value is 75 to 85%, the frontal brightness can be increased and the ratio of side brightness to frontal brightness can be increased.

[0257] (2) Frontal luminance (unit: cd / m²) 2 )

[0258] A single film was manufactured using the method of (1) and attached to an OLED display device having a light-emitting unit. The display device was driven. The luminance value was measured using a luminance measuring instrument CS2000 (Konica Minolta). The luminance value measured from the front was measured and is shown in Table 1 below.

[0259] (3) Dispersibility of quantum dots

[0260] The morphology of the cross-section of the film and the dispersibility of quantum dots were analyzed using a focused ion beam (FIB) scanning electron microscope (SEM) at a magnification of 50,000x for a film obtained using the manufactured quantum dot composition, and the results are shown in Figures 2 to 4 below. In addition, based on the above morphology, if the quantum dots are well dispersed, it was evaluated as good, and if the quantum dots are not well dispersed, it was evaluated as poor.

[0261]

[0262] Ligand RL Front View Luminance Quantum Dot Dispersibility Quantum Dot Dispersibility Chemical Formula 1-10 Chemical Formula 2-1 Chemical Formula 4 Comparative Example 1 1000080499 9.9°C 4 Defective Comparative Example 2 700307449 4.9 Unspecified Defective Comparative Example 3 300707350 9.9 Unspecified Defective Example 1 7030081514.9°C 2 Good Example 2 3070083529.9°C 3 Good

[0263]

[0264] As shown in Table 1 and Figures 2 and 3 above, the specimen prepared with the quantum dot composition of the example provides a uniform light dispersion effect by providing improved dispersibility of the quantum dots and can improve front brightness. In addition, according to Table 1 above, since the specimen prepared with the quantum dot composition of the example has an RL value of 75 to 85%, it is expected that the screen quality of the display device can be improved by improving the ratio of side brightness to front brightness.

[0265] However, as shown in Table 1 and Figure 4 above, the specimen prepared with the quantum dot composition of the comparative example had poor dispersibility of quantum dots and low frontal brightness. In addition, since the specimen prepared with the quantum dot composition of the comparative example did not have an RL value of 75 to 85%, it is expected that the improvement effect of the ratio of side brightness to frontal brightness will be weak.

[0266]

[0267] Simple variations or modifications of the present invention can be easily implemented by those skilled in the art, and all such variations or modifications are considered to be included within the scope of the present invention.

Claims

1. Includes quantum dots having ligands, The above ligand is a quantum dot composition comprising a mixture of a compound of Chemical Formula 1 below and a compound of Chemical Formula 2 below: [Chemical Formula 1] (In the above chemical formula 1, R 1 is a substituted or unsubstituted C1 to C10 alkyl group or a substituted or unsubstituted C6 to C20 aryl group, and L 11 to L 13 Each is an independently substituted or unsubstituted C1 to C10 alkylene group, ester group, or ether group, and n is an integer from 1 to 20, provided that L 12 ga is an ester group and at the same time L 13 When this is an unsubstituted C1 to C10 alkylene group, n is an integer from 4 to 20). [Chemical Formula 2] (In the above chemical formula 2, L 21 Silver oxygen, L 22 is a straight-chain or branched-chain alkylene group having 1 to 20 carbon atoms, L 23 Silver hydrogen or methyl group, n is an integer from 1 to 10).

2. In claim 1, in the above chemical formula 2, L 22 A quantum dot composition having a straight-chain or branched-chain alkylene group having 1 to 10 carbon atoms.

3. A quantum dot composition according to claim 1, wherein the compound of Chemical Formula 2 is a compound of Chemical Formula 2-1 below: [Chemical Formula 2-1] .

4. A quantum dot composition according to claim 1, wherein the compound of Chemical Formula 1 is a compound of Chemical Formula 1-11 below: [Chemical Formula 1-11] (n is an integer from 1 to 10).

5. A quantum dot composition according to claim 1, wherein the compound of Formula 1 is included in an amount of 30 to 90 weight percent of the total ligands of the quantum dot.

6. A quantum dot composition according to claim 1, wherein the compound of formula 2 is included in an amount of 10 to 70 weight percent of the total ligands of the quantum dot.

7. The quantum dot composition of claim 1, wherein the quantum dot composition further comprises one or more of a photocurable monomer having unsaturated bonds and an initiator.

8. In claim 1, the quantum dot composition is a solvent-free composition.

9. A quantum dot composition according to claim 1, wherein the composition further comprises one or more of a light scattering agent and a polymerization inhibitor.

10. A quantum dot composition according to claim 1, wherein the quantum dots comprise one or more of InP / ZnS and InP / ZnSe / ZnS as non-cadmium light-emitting materials.

11. A quantum dot composition according to claim 1, wherein the quantum dot comprises a core comprising Ag, In, Ga and S; and a shell comprising at least two selected from the group consisting of Ag, Ga, Zn and S.

12. A cured film comprising a cured product of a quantum dot composition according to any one of claims 1 to 11.

13. A display device comprising the cured film of paragraph 12.