Electrolyte for secondary battery and secondary battery comprising same
The electrolyte composition for lithium secondary batteries, featuring specific additives, addresses performance degradation issues by forming a protective film to inhibit metal leaching and stabilize the electrolyte, enhancing lifespan and capacity retention.
Patent Information
- Application Number
- PCT/KR2026/005703
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-12
- Filing Date
- 2026-04-29
- Publication Date
- 2026-11-19
Smart Images

Figure KR2026005703_19112026_PF_FP_ABST
Abstract
Description
Electrolyte for secondary batteries and secondary batteries including the same
[0001] The present invention relates to an electrolyte for a secondary battery and a secondary battery containing the same.
[0002]
[0003] With the recent rapid proliferation of battery-powered electronic devices such as mobile phones, laptop computers, and electric vehicles, the demand for high-energy-density, high-capacity rechargeable batteries is increasing rapidly. Consequently, research and development aimed at improving the performance of rechargeable batteries is actively underway.
[0004] A lithium secondary battery is a battery comprising a positive electrode and a negative electrode containing an active material capable of lithium ion intercalation and deintercalation, and an electrolyte, which produces electrical energy through oxidation and reduction reactions when lithium ions are intercalated or deintercalated from the positive and negative electrodes.
[0005] The electrolyte for these lithium secondary batteries consists of a lithium salt dissolved in a non-aqueous organic solvent. The characteristics of a lithium secondary battery are determined by complex reactions between the anode and the electrolyte, and between the cathode and the electrolyte. Therefore, the use of an appropriate electrolyte is one of the important variables for improving the performance of a lithium secondary battery.
[0006]
[0007] One embodiment provides an electrolyte for a secondary battery that offers a room temperature life, a low resistance increase rate after high-temperature storage, a high capacity retention rate after high-temperature storage, and an effect of suppressing transition metal leaching after high-temperature storage.
[0008] Another embodiment provides a secondary battery comprising the above electrolyte.
[0009]
[0010] One embodiment provides an electrolyte for a secondary battery.
[0011] 1. An electrolyte for a secondary battery comprises a non-aqueous organic solvent; a lithium salt; and an additive, wherein the additive comprises a mixture of (I) and (II):
[0012] (I)(a) One or more alkali metal salts or alkaline earth metal salts of metaphosphoric acid (HPO3), or
[0013] (b) one or more of lithium borate or lithium phosphate,
[0014] (II) Compounds represented by the following chemical formula 1:
[0015] [Chemical Formula 1]
[0016]
[0017] (In the above chemical formula 1,
[0018] R 11 , R 12 , R 13 , R 14 and R 15 is the same as defined in the description of the invention below).
[0019] In 2.1, R in Chemical Formula 1 above 11 , R 12 , R 13 , and R 14 Electrolyte for a secondary battery, each independently hydrogen or a substituted or unsubstituted C1 to C5 alkyl group.
[0020] In 3.1 to 2, R in Chemical Formula 1 15 An electrolyte for a secondary battery, wherein is a methoxy group, an ethoxy group, an n-propoxy group, an iso-propoxy group, an n-butoxy group, an iso-butoxy group, a tert-butoxy group, an n-pentoxy group, or an iso-pentoxy group.
[0021] 4.1 to 3, an electrolyte for a secondary battery wherein the compound represented by Chemical Formula 1 is one or more of the following Chemical Formulas 1-2 to 1-5:
[0022] [Chemical Formula 1-2]
[0023]
[0024] [Chemical Formula 1-3]
[0025]
[0026] [Chemical Formula 1-4]
[0027]
[0028] [Chemical Formula 1-5]
[0029] .
[0030] 5.1 to 4, an electrolyte for a secondary battery comprising one or more of the alkali metal salt of the metaphosphoric acid, LiPO3, NaPO3, and KPO3.
[0031] 6.1 to 5, an electrolyte for a secondary battery wherein one or more of the lithium borate or lithium phosphate are represented by the following chemical formula 2:
[0032] [Chemical Formula 2]
[0033]
[0034] R 21 C1 to C10 alkylene groups formed by single bonds or substituted or unsubstituted bonds,
[0035] A is boron (B) or phosphorus (P), and
[0036] X is a halogen element, and
[0037] n is an integer from 0 to 2, and
[0038] m is an integer from 1 to 3, and
[0039] If A is boron (B), then n + m = 2 is satisfied, and
[0040] If A is P, then n + m = 3 is satisfied).
[0041] 7.1 to 6, an electrolyte for a secondary battery wherein one or more of the lithium borate or lithium phosphate are represented by any one of the following chemical formulas 2-1 to 2-5:
[0042] [Chemical Formula 2-1]
[0043]
[0044] [Chemical Formula 2-2]
[0045]
[0046] [Chemical Formula 2-3]
[0047]
[0048] [Chemical Formula 2-4]
[0049]
[0050] [Chemical Formula 2-5]
[0051]
[0052] 8.1 to 7, wherein (I) : (II) is an electrolyte for a secondary battery included in the electrolyte in a weight ratio of 1 : 0.1 to 1 : 10.
[0053] 9.1 to 8, an electrolyte for a secondary battery, wherein (II) is included in an amount of 0.01 to 5 weight% with respect to the total amount of the electrolyte, and (I) is included in an amount of 0.01 to 5 weight% with respect to the total amount of the electrolyte.
[0054] 10.1 to 9, an electrolyte for a secondary battery, wherein the additive is included in an amount of 0.01 to 10 weight% relative to the total amount of the electrolyte.
[0055] 11.1 to 10, the electrolyte for a secondary battery, wherein the non-aqueous organic solvent is a mixture containing ethylene carbonate (EC): ethylmethyl carbonate (EMC): dimethyl carbonate (DMC) in a volume ratio of 10 to 30: 20 to 50: 20 to 50.
[0056] 12.1 to 11, an electrolyte for a secondary battery, wherein the concentration of the lithium salt in the electrolyte is 0.1M to 3.0M.
[0057] 13.1 to 12, the lithium salt is one or more selected from the group consisting of LiPF6, LiClO4, LiBF4, (lithium bis(fluorosulfonyl)imide (LiFSI), LiTFSI, LiSO3CF3, LiBOB, LiFOB, LiDFBP, LiTFOP, LiPO2F2, LiSbF6, LiAsF6, LiAlO2, LiAlCl4, LiCl, LiI, LiN(SO3C2F5)2, Li(FSO2)2N, and LiC4F9SO3, an electrolyte for a secondary battery.
[0058] 14.1 to 13, an electrolyte for a secondary battery comprising at least 95% by weight of the total additive of the electrolyte.
[0059] Another embodiment provides a secondary battery.
[0060] 15. A secondary battery comprises a positive electrode including a positive active material; a negative electrode including a negative active material; and an electrolyte, wherein the electrolyte comprises the electrolytes of 1 to 14.
[0061] In 16.15, the positive electrode active material comprises one or more of a lithium iron phosphate-based compound, a lithium manganese iron phosphate-based compound, a lithium nickel cobalt manganese-based oxide, and a lithium nickel cobalt aluminum-based oxide, in a secondary battery.
[0062] 17.15 A secondary battery wherein the negative electrode active material comprises at least one of graphite and a Si composite.
[0063]
[0064] An electrolyte according to one embodiment can have the effect of improving lifespan characteristics and reliability when activating a secondary battery in a secondary battery.
[0065]
[0066] FIG. 1 is a conceptual diagram briefly illustrating a secondary battery according to one embodiment of the present invention.
[0067] FIGS. 2 and FIGS. 3 are cross-sectional views schematically illustrating a secondary battery according to one embodiment.
[0068]
[0069] In order to fully understand the structure and effects of the present invention, preferred embodiments of the present invention are described with reference to the attached drawings. However, the present invention is not limited to the embodiments disclosed below, but can be implemented in various forms and various modifications can be made. The description of these embodiments is provided merely to ensure that the disclosure of the present invention is complete and to fully inform those skilled in the art of the scope of the invention.
[0070] In this specification, when a component is described as being on another component, it means that it may be formed directly on the other component or that a third component may be interposed between them. Additionally, in the drawings, the thicknesses of the components are exaggerated for the effective description of the technical content. Throughout the specification, parts indicated by the same reference numeral represent the same components.
[0071] Unless otherwise specified in this specification, the singular form may also include the plural. Additionally, unless otherwise specified, "A or B" may mean "comprising A, comprising B, or comprising A and B." As used herein, "comprises" and / or "comprising" do not exclude the presence or addition of one or more other components to the mentioned components.
[0072] In this specification, "combination of these" may mean a mixture of components, a laminate, a composite, a copolymer, an alloy, a blend, and a reaction product, etc.
[0073] In this specification, "substitution" means that, unless otherwise defined, at least one hydrogen of a substituent or compound is substituted with a deuterium, a halogen group, a hydroxyl group, an amino group, a C1 to C30 amine group, a nitro group, a C1 to C40 silyl group, a C1 to C30 alkyl group, a C1 to C10 alkylsilyl group, a C6 to C30 arylsilyl group, a C3 to C30 cycloalkyl group, a C3 to C30 heterocycloalkyl group, a C6 to C30 aryl group, a C2 to C30 heteroaryl group, a C1 to C20 alkoxy group, a C1 to C10 fluoroalkyl group, a cyano group, or a combination thereof.
[0074] Specifically, "substitution" may mean that at least one hydrogen in the substituent or compound is substituted with deuterium, a halogen group, a C1 to C30 alkyl group, a C1 to C10 alkylsilyl group, a C6 to C30 arylsilyl group, a C3 to C30 cycloalkyl group, a C3 to C30 heterocycloalkyl group, a C6 to C30 aryl group, a C2 to C30 heteroaryl group, a C1 to C10 fluoroalkyl group, or a cyano group. For example, "substitution" may mean that at least one hydrogen in the substituent or compound is substituted with deuterium, a halogen group, a C1 to C20 alkyl group, a C6 to C30 aryl group, a C1 to C10 fluoroalkyl group, or a cyano group. Alternatively, "substitution" may mean that at least one hydrogen in the substituent or compound is substituted with a deuterium, a halogen group, a C1 to C5 alkyl group, a C6 to C18 aryl group, a C1 to C5 fluoroalkyl group, or a cyano group. For example, "substitution" may mean that at least one hydrogen in the substituent or compound is substituted with a deuterium, a cyano group, a halogen group, a methyl group, an ethyl group, a propyl group, a butyl group, a phenyl group, a biphenyl group, a terphenyl group, a trifluoromethyl group, or a naphthyl group.
[0075] Unless otherwise defined in this specification, "*" indicates a part connected to the same or different atoms or chemical formulas. Unless specifically mentioned otherwise in the chemical formulas described in this specification, hydrogen may be bonded in the structure of the chemical formula. Unless otherwise defined in this specification, the halogen may be F, Cl, Br, or I.
[0076] FIG. 1 is a conceptual diagram briefly illustrating a secondary battery according to embodiments of the present invention. Referring to FIG. 1, the secondary battery may include a positive electrode (10), a negative electrode (20), a separator (30), and an electrolyte (ELL).
[0077] The positive electrode (10) and the negative electrode (20) may be spaced apart from each other with a separator (30) in between. The separator (30) may be placed between the positive electrode (10) and the negative electrode (20). The positive electrode (10), the negative electrode (20), and the separator (30) may come into contact with an electrolyte (ELL). The positive electrode (10), the negative electrode (20), and the separator (30) may be impregnated within the electrolyte (ELL).
[0078] The electrolyte (ELL) may be a medium for transferring lithium ions between the positive electrode (10) and the negative electrode (20). Within the electrolyte (ELL), the lithium ions may pass through a separator (30) and move toward the positive electrode (10) or the negative electrode (20).
[0079] positive electrode (10)
[0080] A positive electrode (10) for a secondary battery may include a current collector (COL1) and a positive electrode active material layer (AML1) formed on the current collector (COL1). The positive electrode active material layer (AML1) may include a positive electrode active material and may further include a binder and / or a conductive material.
[0081] For example, the anode (10) may further include an additive that can serve as a sacrificial anode.
[0082] The content of the positive active material in the positive active material layer (AML1) may be 90% to 99.5% by weight with respect to 100% by weight of the positive active material layer (AML1). The content of the binder and the conductive material may each be 0.5% to 5% by weight with respect to 100% by weight of the positive active material layer (AML1).
[0083] The above binder serves to adhere the positive active material particles well to each other and also to adhere the positive active material well to the current collector (COL1). Representative examples of binders include, but are not limited to, polyvinyl alcohol, carboxymethylcellulose, hydroxypropylcellulose, diacetylcellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polymers containing ethylene oxide, polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, (meth)acrylated styrene-butadiene rubber, epoxy resin, (meth)acrylic resin, polyester resin, nylon, etc.
[0084] The above conductive material is used to impart conductivity to the electrode, and any electronically conductive material that does not cause chemical changes can be used in the battery being constructed. Examples of conductive materials include carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, carbon nanofiber, carbon nanotube; metal-based materials in the form of metal powder or metal fibers containing copper, nickel, aluminum, silver, etc.; conductive polymers such as polyphenylene derivatives; or mixtures thereof.
[0085] Al can be used as the current collector (COL1), but is not limited thereto.
[0086] positive electrode active material
[0087] As the positive active material in the positive active material layer (AML1), a compound capable of reversible intercalation and deintercalation of lithium (a lithated intercalation compound) may be used. Specifically, one or more composite oxides of lithium and a metal selected from cobalt, manganese, nickel, and combinations thereof may be used.
[0088] The above composite oxide may be a lithium transition metal composite oxide, and specific examples include a lithium nickel-based oxide, a lithium cobalt-based oxide, a lithium manganese-based oxide, a lithium iron phosphate-based compound, a cobalt-free nickel-manganese-based oxide, or a combination thereof.
[0089] As an example, a compound represented by any one of the following chemical formulas may be used. Li a A 1-b X b O 2-c D c (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05); Li a Mn 2-b X b O 4-c D c (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05); Li a Ni 1-b-c Co b X c O 2-α D α (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.5, 0<α<2); Li a Ni 1-b-c Mn b X c O 2-α D α (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.5, 0<α<2); Li a Ni b Co c L 1 d G e O2(0.90≤a≤1.8, 0≤b≤0.9, 0≤c≤0.5, 0≤d≤0.5, 0≤e≤0.1); Li aNiG b O2(0.90≤a≤1.8, 0.001≤b≤0.1); Li a CoG b O2(0.90≤a≤1.8, 0.001≤b≤0.1); Li a Mn 1-b G b O2(0.90≤a≤1.8, 0.001≤b≤0.1); Li a Mn2G b O4(0.90≤a≤1.8, 0.001≤b≤0.1); Li a Mn 1-g G g PO4(0.90≤a≤1.8, 0≤g≤0.5); Li (3-f) Fe2(PO4)3(0≤f≤2); Li a FePO4(0.90≤a≤1.8).
[0090] In the above chemical formula, A is Ni, Co, Mn, or a combination thereof; X is Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, a rare earth element, or a combination thereof; D is O, F, S, P, or a combination thereof; G is Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V, or a combination thereof; L 1 is Mn, Al, or a combination thereof.
[0091] For example, the above-mentioned positive electrode active material may be a high-nickel positive electrode active material in which the nickel content relative to 100 mol% of the metal excluding lithium in the lithium transition metal composite oxide is 80 mol% or more, 85 mol% or more, 90 mol% or more, 91 mol% or more, or 94 mol% or more and 99 mol% or less. The high-nickel positive electrode active material can achieve high capacity and can be applied to high-capacity, high-density secondary batteries.
[0092] Negative electrode (20)
[0093] The negative electrode (20) for a secondary battery includes a current collector (COL2) and a negative active material layer (AML2) located on the current collector (COL2). The negative active material layer (AML2) includes a negative active material and may further include a binder and / or a conductive material.
[0094] For example, the negative electrode active material layer (AML2) may contain 90% to 99% by weight of negative electrode active material, 0.5% to 5% by weight of binder, and 0% to 5% by weight of conductive material.
[0095] The above binder serves to effectively bond the negative electrode active material particles to each other and also to effectively bond the negative electrode active material to the current collector (COL2). As the binder, a non-aqueous binder, an aqueous binder, a dry binder, or a combination thereof may be used.
[0096] Examples of the above-mentioned non-aqueous binders include polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene propylene copolymer, polystyrene, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polyamide imide, polyimide, or combinations thereof.
[0097] The above-mentioned water-based binder may be selected from styrene-butadiene rubber, (meth)acrylated styrene-butadiene rubber, (meth)acrylonitrile-butadiene rubber, (meth)acrylic rubber, butyl rubber, fluororubber, polyethylene oxide, polyvinylpyrrolidone, polyepichlorohydrin, polyphosphazene, poly(meth)acrylonitrile, ethylenepropylenediene copolymer, polyvinylpyridine, chlorosulfonated polyethylene, latex, polyester resin, (meth)acrylic resin, phenolic resin, epoxy resin, polyvinyl alcohol, and combinations thereof.
[0098] When a water-based binder is used as the above-mentioned cathode binder, a cellulose-based compound capable of imparting viscosity may be further included. As this cellulose-based compound, one or more types such as carboxymethyl cellulose, hydroxypropylmethyl cellulose, methyl cellulose, or alkali metal salts thereof may be mixed and used. Na, K, or Li may be used as the alkali metal.
[0099] The above dry binder is a polymer material capable of fiberization, and may be, for example, polytetrafluoroethylene, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, polyethylene oxide, or a combination thereof.
[0100] The above conductive material is used to impart conductivity to the electrode, and any electronically conductive material that does not cause chemical changes can be used in the battery being constructed. Specific examples include carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjenblack, carbon fiber, carbon nanofiber, carbon nanotube; metal-based materials in the form of metal powder or metal fibers including copper, nickel, aluminum, silver, etc.; conductive polymers such as polyphenylene derivatives; or mixtures thereof.
[0101] As the current collector (COL2), copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, a polymer substrate coated with a conductive metal, and combinations thereof may be used.
[0102] cathode active material
[0103] The negative electrode active material in the negative electrode active material layer (AML2) comprises a material capable of reversibly intercalating / deintercalating lithium ions, lithium metal, an alloy of lithium metal, a material capable of doping and dedoping lithium, or a transition metal oxide.
[0104] A material capable of reversibly intercalating / deintercalating the above lithium ions may be a carbon-based negative electrode active material, such as crystalline carbon, amorphous carbon, or a combination thereof. Examples of the crystalline carbon include graphite such as amorphous, plate-like, flake-like, spherical, or fibrous natural graphite or artificial graphite, and examples of the amorphous carbon include soft carbon or hard carbon, mesophase pitch carbide, calcined coke, etc.
[0105] As the above lithium metal alloy, an alloy of lithium and a metal selected from Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al, and Sn may be used.
[0106] As a material capable of doping and undoping the above lithium, a Si-based negative electrode active material or a Sn-based negative electrode active material may be used. The Si-based negative electrode active material may be silicon, a silicon-carbon composite, SiOx (0 < x < 2), a Si-Q alloy (wherein Q is selected from alkali metals, alkaline earth metals, group 13 elements, group 14 elements (excluding Si), group 15 elements, group 16 elements, transition metals, rare earth elements, and combinations thereof), or a combination thereof. The Sn-based negative electrode active material may be Sn, SnO2, a Sn-based alloy, or a combination thereof.
[0107] The silicon-carbon composite may be a composite of silicon and amorphous carbon. According to one embodiment, the silicon-carbon composite may be in the form of silicon particles and amorphous carbon coated on the surface of the silicon particles. For example, it may include a secondary particle (core) assembled from silicon primary particles and an amorphous carbon coating layer (shell) located on the surface of the secondary particle. The amorphous carbon may also be located between the silicon primary particles, so that, for example, the silicon primary particles may be coated with amorphous carbon. The secondary particles may be dispersed in an amorphous carbon matrix.
[0108] The silicon-carbon composite may further include crystalline carbon. For example, the silicon-carbon composite may include a core comprising crystalline carbon and silicon particles and an amorphous carbon coating layer located on the surface of the core.
[0109] The above Si-based or Sn-based negative electrode active material can be used in combination with a carbon-based negative electrode active material.
[0110] Separator (30)
[0111] Depending on the type of secondary battery, a separator (30) may be present between the positive electrode (10) and the negative electrode (20). As such a separator (30), polyethylene, polypropylene, polyvinylidene fluoride, or a multilayer film of two or more layers thereof may be used, and of course, a mixed multilayer film such as a polyethylene / polypropylene two-layer separator, a polyethylene / polypropylene / polyethylene three-layer separator, or a polypropylene / polyethylene / polypropylene three-layer separator may be used.
[0112] The separator (30) may include a porous substrate and a coating layer comprising an organic material, an inorganic material, or a combination thereof located on one or both sides of the porous substrate.
[0113] The porous substrate may be a polymer membrane formed from any one of the following: polyolefins such as polyethylene and polypropylene; polyesters such as polyethylene terephthalate and polybutylene terephthalate; polyacetal; polyamide; polyimide; polycarbonate; polyetherketone; polyaryletherketone; polyetherimide; polyamideimide; polybenzimidazole; polyethersulfone; polyphenylene oxide; cyclic olefin copolymer; polyphenylene sulfide; polyethylene naphthalate; glass fiber; Teflon; and polytetrafluoroethylene, or a copolymer or mixture of two or more of these.
[0114] The above organic material may include a polyvinylidene fluoride-based polymer or a (meth)acrylic-based polymer.
[0115] The above inorganic materials are Al2O3, SiO2, TiO2, SnO2, CeO2, MgO, NiO, CaO, GaO, ZnO, ZrO2, Y2O3, It may include, but is not limited to, inorganic particles selected from SrTiO3, BaTiO3, Mg(OH)2, boehmite, and combinations thereof.
[0116] The above organic and inorganic materials may exist mixed in a single coating layer, or may exist in a stacked form with a coating layer containing organic materials and a coating layer containing inorganic materials.
[0117] Electrolyte (ELL)
[0118] The electrolyte (ELL) for secondary batteries contains a non-aqueous organic solvent and a lithium salt.
[0119] The above-mentioned non-aqueous organic solvent serves as a medium through which ions involved in the electrochemical reaction of the battery can move.
[0120] The above-mentioned non-aqueous organic solvent may be a carbonate-based, ester-based, ether-based, ketone-based, or alcohol-based solvent, an aprotic solvent, or a combination thereof.
[0121] The above carbonate-based solvents may include dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methylpropyl carbonate (MPC), ethylpropyl carbonate (EPC), ethylmethyl carbonate (EMC), ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), etc.
[0122] Ester-based solvents such as methyl acetate, ethyl acetate, n-propyl acetate, dimethyl acetate, methylpropionate, ethylpropionate, decanolide, mevalonolactone, valerolactone, and caprolactone may be used.
[0123] As ether-based solvents, dibutyl ether, tetraglame, diglame, dimethoxyethane, 2-methyltetrahydrofuran, 2,5-dimethyltetrahydrofuran, tetrahydrofuran, etc. may be used. Additionally, as ketone-based solvents, cyclohexanone, etc. may be used. As alcohol-based solvents, ethyl alcohol, isopropyl alcohol, etc. may be used, and as aprotic solvents, nitriles such as R-CN (where R is a straight-chain, branched, or cyclic hydrocarbon group having 2 to 20 carbon atoms and may include a double bond, an aromatic ring, or an ether group); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane, 1,4-dioxolane; sulfolanes, etc. may be used.
[0124] The above-mentioned non-aqueous organic solvent can be used alone or in a mixture of two or more types.
[0125] In addition, when using a carbonate-based solvent, a mixture of cyclic carbonates and chain carbonates can be used, and the cyclic carbonates and chain carbonates can be mixed in a volume ratio of 1:1 to 1:9.
[0126] The above lithium salt is a substance that dissolves in an organic solvent and acts as a source of lithium ions within the battery, enabling the basic operation of the secondary battery and facilitating the movement of lithium ions between the anode and cathode. Representative examples of lithium salts include LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiAlO2, LiAlCl4, LiPO2F2, LiCl, LiI, LiN(SO3C2F5)2, Li(FSO2)2N (lithium bis(fluorosulfonyl)imide, LiFSI), LiC4F9SO3, and LiN(C x F 2x+1 SO2)(C y F 2y+1 It may include one or more selected from SO2)(x and y are integers from 1 to 20), lithium trifluoromethane sulfonate, lithium tetrafluoroethane sulfonate, lithium difluorobis(oxalate)borate (LiDFOB), lithium difluorobis(oxalate)phosphate (LiDFOP), and lithium bis(oxalate)borate (LiBOB).
[0127] secondary battery
[0128] Secondary batteries can be classified into cylindrical, prismatic, pouch, coin, etc., depending on their shape. FIGS. 2 and FIGS. 3 are schematic diagrams illustrating a secondary battery according to one embodiment, where FIG. 2 is a cylindrical battery shape and FIG. 3 is a prismatic battery shape. Referring to FIGS. 2 and FIGS. 3, the secondary battery (100) may include an electrode assembly (40) with a separator (30) interposed between a positive electrode (10) and a negative electrode (20), and a case (50) in which the electrode assembly (40) is housed. The positive electrode (10), the negative electrode (20), and the separator (30) may be impregnated with an electrolyte (not shown). The secondary battery (100) may include a sealing member (60) that seals the case (50) as in FIG. 2. In addition, in FIG. 3, the secondary battery (100) may include a positive lead tab (11) and a positive terminal (12), a negative lead tab (21) and a negative terminal (22).
[0129] [Electrolyte]
[0130] Hereinafter, an electrolyte for a secondary battery according to one embodiment of the present invention will be described in more detail.
[0131] An electrolyte for a secondary battery according to one embodiment comprises the above-described non-aqueous organic solvent; a lithium salt; and an additive, wherein the additive comprises an additive to be described below.
[0132] The above electrolyte can be prepared by dissolving a lithium salt in a non-aqueous organic solvent, adding the above additive, and then performing a mixing process. The process of mixing the electrolyte is widely known in the field of electrolyte manufacturing, and a person skilled in the art can appropriately select and use it.
[0133] A non-aqueous organic solvent according to one embodiment of the present invention may include one or more of the non-aqueous organic solvents described above.
[0134] In one embodiment, the non-aqueous organic solvent may be a mixture containing ethylene carbonate (EC): ethyl methyl carbonate (EMC): dimethyl carbonate (DMC) in a volume ratio of 10 to 30: 20 to 50: 20 to 50. Here, the volume ratio is a value based on 100 volume% of the total of ethylene carbonate (EC): ethyl methyl carbonate (EMC): dimethyl carbonate (DMC). Within the above range, the effect of providing improved room temperature life, a low resistance increase rate after high-temperature storage, and a high capacity retention rate after high-temperature storage by the additive to be described later may be significant. Additionally, within the above range, the effect of providing improved room temperature life, a low resistance increase rate after high-temperature storage, and a high capacity retention rate after high-temperature storage in a secondary battery containing the cathode active material to be described later may be significant.
[0135] For example, the above volume ratio can be EC : EMC : DMC = 10 to 20 : 30 to 50 : 30 to 50.
[0136] A lithium salt according to one embodiment of the present invention may include one or more selected from the group consisting of LiPF6, LiClO4, LiBF4, lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), LiSO3CF3, LiBOB, LiFOB, LiDFBP, LiTFOP, LiPO2F2, LiSbF6, LiAsF6, LiAlO2, LiAlCl4, LiCl, LiI, LiN(SO3C2F5)2, Li(FSO2)2N, and LiC4F9SO3. According to one embodiment, the lithium salt may be LiPF6.
[0137] The concentration of the lithium salt in the above electrolyte may be 0.1M to 3.0M. Specifically, the concentration of the lithium salt may be 0.5M or higher and 1.0M or higher. The concentration of the lithium salt may be 3.0M or lower, 2.5M or lower, and 2.0M or lower. In the present invention, when the concentration of the lithium salt is 0.1M to 2.0M, the conductivity and viscosity of the electrolyte can be appropriately maintained.
[0138] additives
[0139] An additive according to one embodiment of the present invention comprises a mixture of (I) and (II):
[0140] (I)(a) One or more alkali metal salts or alkaline earth metal salts of metaphosphoric acid (HPO3), or
[0141] (b) one or more of lithium borate or lithium phosphate,
[0142] (II) Compounds represented by the following chemical formula 1:
[0143] [Chemical Formula 1]
[0144]
[0145] (In the above chemical formula 1,
[0146] R 11 , R 12, R 13 , R 14 and R 15 is the same as defined in the description of the invention below).
[0147] Additive according to the first embodiment
[0148] An additive according to one embodiment of the present invention comprises an alkali metal salt or alkaline earth metal salt of metaphosphoric acid (HPO3); and a mixture of compounds represented by the following chemical formula 1.
[0149] The alkali metal salt or alkaline earth metal salt of methane phosphate consists of an inorganic component relative to the compound represented by Chemical Formula 1 below. When the alkali metal salt or alkaline earth metal salt of methane phosphate is combined with the compound represented by Chemical Formula 1 below, the effect of inhibiting transition metal leaching can be enhanced by forming an organic-inorganic film on the electrode surface. The compound represented by Chemical Formula 1 below can significantly enhance the effect of inhibiting transition metal leaching by the alkali metal salt or alkaline earth metal salt of methane phosphate. In particular, the compound represented by Chemical Formula 1 below can significantly enhance the effect of inhibiting transition metal leaching by the alkali metal salt or alkaline earth metal salt of methane phosphate after high-temperature storage. Furthermore, when the alkali metal salt or alkaline earth metal salt of methane phosphate is combined with the compound represented by Chemical Formula 1 below, it can significantly enhance the improvement effect of high-temperature life and room-temperature life by providing a low resistance increase rate after high-temperature storage and a high capacity retention rate at room temperature and high temperature. In addition, since both the alkali metal or alkaline earth metal salt of methane phosphate and the compound represented by the following chemical formula 1 contain a phosphorus element, the effect of neutralizing transition metals leached from the anode can be enhanced.
[0150] Additives containing alkali metal salts or alkaline earth metal salts of metaphosphoric acid and not containing compounds of Formula 1 may have lower high-temperature and room-temperature lifespans and increased resistance after high-temperature storage.
[0151] Additives containing the compound of Chemical Formula 1 and not containing alkali metal salts or alkaline earth metal salts of metaphosphoric acid may have a reduced effect in inhibiting transition metal leaching.
[0152] Here, "transition metal" may include, but is not limited to, cobalt, manganese, iron, nickel, copper, zinc, etc. The above transition metal may be derived from the positive electrode active material.
[0153] The compound represented by Chemical Formula 1 below has an aromatic ring-type phosphite structure, where P has a lone pair of electrons. Additionally, an alkoxy group is bonded to P in the phosphite structure. Therefore, the compound represented by Chemical Formula 1 has a significantly high ability to act as a Lewis base, thereby stabilizing reactive substances, particularly Lewis acids, generated within the electrolyte during repeated charging and discharging of the battery, which improves the room-temperature life of the battery and provides a low resistance increase rate and a high capacity retention rate even after high-temperature storage of the battery. Furthermore, the compound represented by Chemical Formula 1 can bond to the anode due to the lone pair of electrons in P, thereby suppressing the leaching of metal from the anode and improving the room-temperature life of the battery. Additionally, the compound represented by Chemical Formula 1 has strong oxidizing properties due to the aromatic ring connected to the phosphite structure, which allows it to form a film through oxidation at the anode interface, thereby providing an anode protection effect.
[0154] The compound represented by Chemical Formula 1 can provide significant effects in improving the room-temperature life of the battery, lower resistance growth rate after high-temperature storage, and high capacity retention rate in an electrolyte containing LiPF6 as a lithium salt. LiPF6 has a low melting point and high solubility in low dielectric constant solvents, and is excellent in ionic conductivity, dissociation, anion mobility, thermal stability, and anode stability. However, LiPF6 forms PF5 gas, a strong acid, through a hydration reaction. As a Lewis acid, PF5 can permanently damage the anode active material by opening the ring of non-aqueous organic solvents or by generating HF through a continued hydration reaction. On the other hand, the compound represented by Chemical Formula 1 can provide the aforementioned effects by stabilizing PF5 through acting as a Lewis base for PF5.
[0155] The compound represented by Chemical Formula 1 contains LiPF6 as a lithium salt, and in an electrolyte containing a mixture of ethylene carbonate (EC): ethylmethyl carbonate (EMC): dimethyl carbonate (DMC) as a non-aqueous organic solvent in a volume ratio of 10 to 30: 20 to 50: 20 to 50, the effect of improving the room temperature life of the battery, a low resistance increase rate after high-temperature storage of the battery, and a high capacity retention rate may be significant.
[0156] The compound represented by Chemical Formula 1 can reduce side reactions at the cathode interface by forming a film SEI on the cathode surface through easy decomposition at the cathode interface.
[0157] The compound represented by Chemical Formula 1 is represented by the following Chemical Formula 1.
[0158] [Chemical Formula 1]
[0159]
[0160] (In the above chemical formula 1
[0161] R 11 , R 12 , R 13 and R 14Each is independently hydrogen, a halogen, a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C1 to C20 alkoxy group, a substituted or unsubstituted C2 to C20 alkenyl group, a substituted or unsubstituted C2 to C20 alkynyl group, a substituted or unsubstituted C3 to C20 cycloalkyl group, a substituted or unsubstituted C6 to C20 aryl group, or a substituted or unsubstituted C2 to C20 heteroaryl group, and
[0162] R 15 is a substituted or unsubstituted C1 to C20 alkoxy group).
[0163] In one specific example, R 11 , R 12 , R 13 , and R 14 Each may independently be hydrogen, a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C2 to C20 alkenyl group, or a substituted or unsubstituted C2 to C20 alkenyl group. For example, R 11 , R 12 , R 13 , and R 14 Each may independently be hydrogen or a substituted or unsubstituted C1 to C5 alkyl group.
[0164] In one specific example, R 15 may be an unsubstituted C1 to C10 alkoxy group, or an unsubstituted C1 to C5 alkoxy group, or an unsubstituted C1 to C3 alkoxy group. For example, R 15 It can be a methoxy group, ethoxy group, n-propoxy group, iso-propoxy group, n-butoxy group, iso-butoxy group, tert-butoxy group, n-pentoxy group, or iso-pentoxy group, etc.
[0165] For example, the above compound may be one or more of the following chemical formulas 1-2 to 1-5:
[0166] [Chemical Formula 1-2]
[0167]
[0168] [Chemical Formula 1-3]
[0169]
[0170] [Chemical Formula 1-4]
[0171]
[0172] [Chemical Formula 1-5]
[0173] .
[0174] The compound of Chemical Formula 1 above can be synthesized using ordinary methods known to those skilled in the art.
[0175] Alkali metal salts or alkaline earth metal salts of metaphosphoric acid can easily decompose at the cathode interface and form a film SEI on the cathode surface, thereby suppressing side reactions at the cathode interface.
[0176] Alkali metal salts or alkaline earth metal salts of metaphosphate are metaphosphate anions PO3 - It is a salt composed of an alkali metal cation or an alkaline earth metal cation. Here, the alkali metal can be lithium, sodium, potassium, rubidium, cesium, or francium.
[0177] In one embodiment, the alkali metal salt of metaphosphoric acid may include one or more of LiPO3, NaPO3, KPO3, CsPO3, and RbPO3.
[0178] In one embodiment, the additive may be included in an amount of 95% or more by weight of the total additive of the electrolyte, for example, 95 to 100% by weight or 100% by weight. Within this range, the effect of the additive described above is realized, and side reactions of the electrolyte can be suppressed.
[0179] The above additive may be included in an amount of 0.01 to 10 weight% relative to the total amount of the electrolyte. Within this range, the effect of the additive can be realized. Specifically, the additive may be included in an amount of 0.05 to 5 weight%, 0.05 to 3 weight%, 0.1 to 3 weight%, or 0.1 to 2.5 weight% relative to the total amount of the electrolyte. Within this range, the effect of the additive is significantly enhanced, and there may be an additional effect of not increasing the resistance of the battery.
[0180] The alkali metal or alkaline earth metal salt of the metaphosphoric acid: the compound represented by Chemical Formula 1 may be included in the electrolyte in a weight ratio of 1:0.1 to 1:10. Within this range, the improvement in effect due to the combination of the two types of additives may be significant. For example, the weight ratio may be 1:0.1 to 1:8 or 1:0.2 to 1:5.
[0181] The compound represented by Chemical Formula 1 above may be included in an amount of 0.01 to 5 weight% relative to the total amount of the electrolyte. Within this range, high-temperature life and room-temperature life can be improved without affecting the transition metal leaching inhibitory effect of the alkali metal salt or alkaline earth metal salt of the metaphosphoric acid. For example, the compound may be included in an amount of 0.01 to 1 weight%, 0.1 to 5 weight%, 0.1 to 3 weight%, or 0.1 to 2 weight% relative to the total amount of the electrolyte.
[0182] The alkali metal salt or alkaline earth metal salt of the metaphosphoric acid may be included in an amount of 0.01 to 5 weight% relative to the total amount of the electrolyte. Within this range, the transition metal leaching inhibition effect can be achieved, and the high-temperature life and room-temperature life can be improved by the compound represented by Formula 1. For example, the compound may be included in an amount of 0.01 to 1 weight%, 0.1 to 5 weight%, 0.1 to 3 weight%, or 0.1 to 2 weight% relative to the total amount of the electrolyte.
[0183] Additive according to the second embodiment
[0184] An additive according to one embodiment of the present invention comprises one or more of lithium borate or lithium phosphate; and a mixture of compounds represented by the chemical formula 1.
[0185] One or more of lithium borate or lithium phosphate is one of the lithium salts in the electrolyte. The compound represented by Chemical Formula 1 above can provide room temperature life, low temperature life, high temperature life, low resistance increase rate after high temperature storage, high capacity retention rate after high temperature storage, and low gas generation rate after high temperature storage by combining with one or more of lithium borate and lithium phosphate.
[0186] The compound represented by Chemical Formula 1 has an aromatic ring-type phosphite structure, where P has a lone pair of electrons. Additionally, an alkoxy group is bonded to P in the phosphite structure. Therefore, the compound represented by Chemical Formula 1 has a significantly high ability to act as a Lewis base, thereby stabilizing reactive substances, particularly Lewis acids, generated within the electrolyte during repeated charging and discharging of the battery. This improves the room-temperature life of the battery and provides a low resistance increase rate and a high capacity retention rate even after high-temperature storage of the battery. Furthermore, the compound represented by Chemical Formula 1 can bond to the anode due to the lone pair of electrons in P, thereby suppressing the leaching of metal from the anode and improving the room-temperature life of the battery. Moreover, the compound represented by Chemical Formula 1 has strong oxidizing properties due to the aromatic ring connected to the phosphite structure, which allows it to form a film through oxidation at the anode interface, thereby providing an anode protection effect.
[0187] The compound represented by Chemical Formula 1 above can provide significant effects in improving the room-temperature life of a battery, a low resistance increase rate after high-temperature storage, and a high capacity retention rate in an electrolyte containing LiPF6 as a lithium salt. LiPF6 has a low melting point and high solubility in low dielectric constant solvents, and is excellent in ionic conductivity, dissociation degree, anion mobility, thermal and anode stability. However, LiPF6 forms PF5 gas, a strong acid, through a hydration reaction. As a Lewis acid, PF5 can permanently damage the anode active material by opening the ring of a non-aqueous organic solvent or by generating HF through a continued hydration reaction. On the other hand, the compound represented by Chemical Formula 1 can provide the aforementioned effects by stabilizing PF5 through acting as a Lewis base for PF5.
[0188] The compound represented by Chemical Formula 1 above may have a significant effect of improving the room temperature life of the battery, providing a low resistance increase rate and a high capacity retention rate after high-temperature storage of the battery in an electrolyte comprising a mixture containing LiPF6 as a lithium salt and ethylene carbonate (EC) : ethylmethyl carbonate (EMC) : dimethyl carbonate (DMC) as a non-aqueous organic solvent in a volume ratio of 10 to 30 : 20 to 50 : 20 to 50.
[0189] The compound represented by the above chemical formula 1 is represented by the following chemical formula 1.
[0190] [Chemical Formula 1]
[0191]
[0192] (In the above chemical formula 1,
[0193] R 11 , R 12 , R 13 and R 14 Each is independently hydrogen, a halogen, a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C1 to C20 alkoxy group, a substituted or unsubstituted C2 to C20 alkenyl group, a substituted or unsubstituted C2 to C20 alkynyl group, a substituted or unsubstituted C3 to C20 cycloalkyl group, a substituted or unsubstituted C6 to C20 aryl group, or a substituted or unsubstituted C2 to C20 heteroaryl group, and
[0194] R 15 is a substituted or unsubstituted C1 to C20 alkoxy group).
[0195] The detailed description of the compound represented by Chemical Formula 1 is substantially the same as that described in the additive according to the first embodiment. Therefore, the detailed description of the compound represented by Chemical Formula 1 is omitted.
[0196] The above lithium borate or lithium phosphate is a different substance from the above lithium salt.
[0197] The above lithium borate or lithium phosphate can be represented by the following chemical formula 2:
[0198] [Chemical Formula 2]
[0199]
[0200] R 21 C1 to C10 alkylene groups formed by single bonds or substituted or unsubstituted bonds,
[0201] A is boron (B) or phosphorus (P), and
[0202] X is a halogen element, and
[0203] n is an integer from 0 to 2, and
[0204] m is an integer from 1 to 3, and
[0205] If A is boron (B), then n + m = 2 is satisfied, and
[0206] If A is P, then n + m = 3 is satisfied).
[0207] In one example, in the above chemical formula 2, R 21 ... is a single bond, and A can be boron (B). The above additive can enhance the effect of the electrolyte as a lithium boron oxalate salt.
[0208] In one example, the lithium borate or lithium phosphate may include one or more of the following chemical formulas 2-1 to 2-5:
[0209] [Chemical Formula 2-1]
[0210]
[0211] [Chemical Formula 2-2]
[0212]
[0213] [Chemical Formula 2-3]
[0214]
[0215] [Chemical Formula 2-4]
[0216]
[0217] [Chemical Formula 2-5]
[0218]
[0219] In one embodiment, the additive may include one or more of the chemical formulas 2-1 and 2-2.
[0220] The above additive can be manufactured by conventional methods known to those skilled in the art.
[0221] In one embodiment, the additive may be included in an amount of 95% or more by weight of the total additive of the electrolyte, for example, 95 to 100% by weight or 100% by weight. Within this range, the effect of the additive described above is realized, and side reactions of the electrolyte can be suppressed.
[0222] The above additive may be included in an amount of 0.01 to 10 weight% relative to the total amount of the electrolyte. Within this range, the effect of the additive can be realized. Specifically, the additive may be included in an amount of 0.05 to 5 weight%, 0.05 to 3 weight%, 0.1 to 3 weight%, or 0.1 to 2.5 weight% relative to the total amount of the electrolyte. Within this range, the effect of the additive is significantly enhanced, and there may be an additional effect of not increasing the resistance of the battery.
[0223] One or more of the above lithium borate and lithium phosphate: A compound represented by Chemical Formula 1 may be included in the above electrolyte in a weight ratio of 1:0.1 to 1:10. Within the above range, the improvement in effect by the combination of the two types of additives may be significant. For example, the above weight ratio may be 1:0.1 to 1:8 or 1:0.1 to 1:5.
[0224] The compound represented by Chemical Formula 1 above may be included in an amount of 0.01 to 5 weight% relative to the total amount of the electrolyte. Within this range, high-temperature life and room-temperature life can be improved without affecting the effects of one or more of the lithium borate and lithium phosphate. For example, the compound may be included in an amount of 0.1 to 5 weight%, 0.1 to 3 weight%, or 0.1 to 2 weight% relative to the total amount of the electrolyte.
[0225] One or more of the above lithium borate and lithium phosphate may be included in an amount of 0.01 to 5 weight% relative to the total amount of the electrolyte. Within this range, a gas generation reduction effect can be achieved, and high-temperature life and room-temperature life can be improved by the compound represented by Chemical Formula 1. For example, the compound may be included in an amount of 0.1 to 5 weight%, 0.1 to 3 weight%, or 0.1 to 2 weight% relative to the total amount of the electrolyte.
[0226] [Rechargeable Battery]
[0227] In another embodiment of the present invention, a secondary battery is provided comprising: a positive electrode comprising a positive active material; a negative electrode comprising a negative active material; and an electrolyte, wherein the electrolyte comprises a non-aqueous organic solvent; a lithium salt; and an additive, and the additive comprises a mixture of (I) and (II).
[0228] (I)(a) One or more alkali metal salts or alkaline earth metal salts of metaphosphoric acid (HPO3), or
[0229] (b) one or more of lithium borate or lithium phosphate,
[0230] (II) A compound represented by the above chemical formula 1.
[0231] The above secondary battery may be applied to automobiles, mobile phones, and / or various types of electric devices, etc., but the present invention is not limited thereto.
[0232] The above-mentioned positive electrode active material may be a lithium transition metal composite oxide, and specific examples of the above-mentioned positive electrode active material may include a lithium nickel-based oxide, a lithium cobalt-based oxide, a lithium manganese-based oxide, a lithium iron phosphate-based compound, a cobalt-free nickel-based oxide, or a combination thereof.
[0233] As an example, the above-mentioned positive active material may use a compound represented by any one of the following chemical formulas. Li a A 1-b X b O 2-c D c (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05); Li a Mn 2-b X b O 4-c D c (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05); Li a Ni 1-b-c Co b X c O 2-α D α (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.5, 0<α<2); Li a Ni 1-b-c Mn b X c O 2-α D α (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.5, 0<α<2); Li a Ni b Co c L 1 d G e O2(0.90≤a≤1.8, 0≤b≤0.9, 0≤c≤0.5, 0≤d≤0.5, 0≤e≤0.1); Li a NiG b O2(0.90≤a≤1.8, 0.001≤b≤0.1); Li a CoG b O2(0.90≤a≤1.8, 0.001≤b≤0.1); Li a Mn 1-b G bO2(0.90≤a≤1.8, 0.001≤b≤0.1); Li a Mn2G b O4(0.90≤a≤1.8, 0.001≤b≤0.1); Li a Mn 1-g G g PO4(0.90≤a≤1.8, 0≤g≤0.5); Li (3-f) Fe2(PO4)3(0≤f≤2); Li a FePO4(0.90≤a≤1.8).
[0234] In the above chemical formula, A is Ni, Co, Mn, or a combination thereof; X is Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, a rare earth element, or a combination thereof; D is O, F, S, P, or a combination thereof; G is Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V, or a combination thereof; L 1 is Mn, Al, or a combination thereof.
[0235] The above positive active material may include one or more of a lithium iron phosphate-based compound, a lithium nickel cobalt manganese-based oxide, and a lithium nickel cobalt aluminum-based oxide.
[0236] The above positive active material may include, for example, a lithium nickel-based oxide represented by the following chemical formula 3, a lithium cobalt-based oxide represented by the following chemical formula 4, a lithium iron phosphate-based compound represented by the following chemical formula 5, a cobalt-free lithium nickel-based oxide represented by the chemical formula 6, or a combination thereof.
[0237] [Chemical Formula 3]
[0238] Li a1 Ni x1 M 1 y1 M 2 z1 O 2-b1 X b1
[0239] In the above chemical formula 3, 0.9≤a1≤1.8, 0.3≤x1≤1, 0≤y1≤0.7, 0≤z1≤0.7, 0.9≤x1+y1+z1≤1.1, and 0≤b1≤0.1, and M 1 and M 2 Each is independently one or more elements selected from the group consisting of Al, B, Ba, Ca, Ce, Co, Cr, Cu, Fe, Mg, Mn, Mo, Nb, Si, Sn, Sr, Ti, V, W, and Zr, and X is one or more elements selected from the group consisting of F, P, and S.
[0240] In the above Chemical Formula 3, 0.6≤x1≤1, 0≤y1≤0.4, and 0≤z1≤0.4, or 0.8≤x1≤1, 0≤y1≤0.2, and 0≤z1≤0.2. In one embodiment, M in the above Chemical Formula 3 1 is Co and M 2 It can be Mn or Al.
[0241] [Chemical Formula 4]
[0242] Li a2 Co x2 M 3 y2 O 2-b2 X b2
[0243] In the above chemical formula 4, 0.9≤a2≤1.8, 0.7≤x2≤1, 0≤y2≤0.3, 0.9≤x2+y2≤1.1, and 0≤b2≤0.1, and M 3 is one or more elements selected from the group consisting of Al, B, Ba, Ca, Ce, Cr, Cu, Fe, Mg, Mn, Mo, Ni, Se, Si, Sn, Sr, Ti, V, W, Y, Zn and Zr, and X is one or more elements selected from the group consisting of F, P, and S.
[0244] [Chemical Formula 5]
[0245] Li a3 Fe x3 M 4 y3 PO4-b3 X b3
[0246] In the above chemical formula 5, 0.9≤a3≤1.8, 0.6≤x3≤1, 0≤y3≤0.4, and 0≤b3≤0.1, and M 4 is one or more elements selected from the group consisting of Al, B, Ba, Ca, Ce, Co, Cr, Cu, Mg, Mn, Mo, Ni, Se, Si, Sn, Sr, Ti, V, W, Y, Zn and Zr, and X is one or more elements selected from the group consisting of F, P, and S.
[0247] [Chemical Formula 6]
[0248] Li a4 Ni x4 Mn y4 M 5 z4 O 2-b4 X b4
[0249] In the above chemical formula 6, 0.9≤a4≤1.8, 0.8≤x4<1, 0 <y4≤0.2, 0≤z4≤0.2, 0.9≤x4+y4+z4≤1.1, 및 0≤b4≤0.1이고 M 5 is one or more elements selected from the group consisting of Al, B, Ba, Ca, Ce, Cr, Fe, Mg, Mo, Nb, Si, Sn, Sr, Ti, V, W, and Zr, and X is one or more elements selected from the group consisting of F, P, and S.
[0250] It is possible to have a coating layer on the surface of the above-mentioned lithium composite oxide, or to use a mixture of the above-mentioned lithium composite oxide and a compound having a coating layer. This coating layer may include at least one coating element compound selected from the group consisting of oxides of coating elements, hydroxides of coating elements, oxyhydroxides of coating elements, oxycarbonates of coating elements, and hydroxycarbonates of coating elements. The compounds forming these coating layers may be amorphous or crystalline. As coating elements included in the above-mentioned coating layer, Mg, Al, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr, or mixtures thereof may be used. For the coating layer formation process, any coating method may be used as long as the compound can be coated using these elements in a way that does not adversely affect the physical properties of the cathode active material (e.g., spray coating, immersion method, etc.). Since this is a matter that is well understood by those skilled in the art, a detailed explanation is omitted.
[0251] In a specific embodiment, the negative electrode active material may include at least one of graphite and a Si composite.
[0252] When the above-mentioned cathode active material includes a Si composite and graphite together, the Si composite and graphite may be included in the form of a mixture, in which case the Si composite:graphite may be included in a weight ratio of 1:99 to 50:50 based on a total of 100 parts by weight. More specifically, the Si composite:graphite may be included in a weight ratio of 3:97 to 20:80, 4:96 to 20:80, or 5:95 to 20:80.
[0253] The above Si composite comprises a core containing Si-based particles and an amorphous carbon coating layer, for example, the Si-based particles are a Si-C composite, SiO xIt may include one or more of (0 < x ≤ 2) and Si alloys. For example, the Si-C composite may include a core containing Si particles and crystalline carbon and an amorphous carbon coating layer located on the surface of the core. The crystalline carbon may include, for example, graphite, and more specifically, natural graphite, artificial graphite, or a mixture thereof.
[0254] When the positive electrode contains one or more of the following as positive electrode active materials: a lithium iron phosphate-based compound, a lithium manganese iron phosphate-based compound, a lithium nickel cobalt manganese-based oxide, and a lithium nickel cobalt aluminum-based oxide, and the negative electrode contains graphite as a negative electrode active material, the effect of improving high-temperature stability of the secondary battery can be maximized.
[0255] The operating voltage of the above secondary battery is at least 2.5V, and it may operate even at a high voltage of 4.2V or higher.
[0256] In one embodiment, the secondary battery may be a cylindrical battery.
[0257]
[0258] Examples and comparative examples of the present invention are described below. However, the following examples are merely one example of the present invention, and the present invention is not limited to the following examples.
[0259]
[0260] Preparation Example:
[0261] A solution of 10 g of 2-Chloro-1,3,2-benzodioxanephosphole and 17 g of methanol was stirred at 70°C for 24 hours. After the reaction was finished, the reaction mixture was fractionally distilled under reduced pressure to obtain a compound represented by the following chemical formula 1-2, and it was confirmed by 1H NMR that chemical formula 1-2 was prepared.
[0262] [Chemical Formula 1-2]
[0263]
[0264] 1H NMR (400 MHz, CDCl3): 3.35 (d, 3H), 7.00~7.05 (m, 2H), 7.10~7.15 (m, 2H); 31P NMR (162 MHz, CDCl3): 128.
[0265]
[0266] Examples 1 to 8 and Comparative Examples 1 to 2
[0267] (1) Preparation of electrolyte
[0268] An electrolyte was prepared by dissolving 1.5 M LiPF6 in a carbonate-based solvent mixed with ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) in a volume ratio of 20:40:40 (based on a total volume of 100 volumes), adding an additive, and mixing. Specifically, the amount of additive used is shown in Table 1 below.
[0269] The molar concentration (M) of LiPF6 in the above electrolyte refers to the amount (number of moles) of lithium salt dissolved per 1 L of electrolyte. The content of the additive (unit: weight%) in Table 1 below refers to the weight of the additive relative to 100 weight% of the total electrolyte (lithium salt + non-aqueous organic solvent + additive).
[0270] The above additives used were the following chemical formulas 1-2, LiPO3, NaPO3, and KPO3.
[0271] [Chemical Formula 1-2]
[0272]
[0273]
[0274] (2) Manufacturing of secondary batteries
[0275] Manufacturing of the cathode
[0276] A cathode slurry was prepared by mixing 98 wt% of a cathode active material, in which a graphite and Si composite was mixed in a weight ratio of 95.8:4.2, 1 wt% of styrene-butadiene rubber (SBR), and 1 wt% of carboxymethylcellulose (CMC), adding the mixture to distilled water, and stirring for 60 minutes using a mechanical stirrer. The slurry was applied to a thickness of about 60 μm on a 10 μm thick copper foil using a doctor blade, dried in a hot air dryer at 100 °C for 0.5 hours, dried once more under vacuum conditions at 120 °C for 4 hours, and then rolled to produce a cathode.
[0277] Manufacturing of anodes
[0278] LiNi as a positive electrode active material 0.80 Co 0.10 Al 0.10 An anode slurry was prepared by mixing O297 wt%, artificial graphite powder as a conductive material, 1.0 wt% carbon black (Ketjenblack), and 1.5 wt% polyvinylidene fluoride (PVdF) as a binder, adding the mixture to N-methyl-2-pyrrolidone, and stirring for 30 minutes using a mechanical stirrer. The slurry was applied to a thickness of about 60 μm on a 20 μm thick aluminum foil using a doctor blade, dried in a hot air dryer at 100 ℃ for 0.5 hours, dried once more under vacuum conditions at 120 ℃ for 4 hours, and then rolled to produce an anode.
[0279] Battery manufacturing
[0280] An electrode assembly was manufactured by assembling the above positive electrode and the above negative electrode with a separator made of polyethylene material with a thickness of 16 μm, and a circular (4.2 V class) secondary battery was manufactured by injecting the above electrolyte.
[0281] Evaluation 1: Room Temperature Life Cycle Characteristics Evaluation (Unit: %)
[0282] Room temperature charge-discharge characteristics were evaluated for secondary batteries according to the examples and comparative examples. To this end, 1,000 charge-discharge cycles of the secondary batteries were performed under conditions of 25°C, 0.5C charging (CC / CV, 4.2V, 0.2C Cut-off) / 0.5C discharging (CC, 2.5V Cut-off). The capacity retention rate (unit: %) was calculated according to the following formula.
[0283] Capacity retention rate (%) = (Discharge capacity after 1,000 cycles / Discharge capacity after 1 cycle) × 100.
[0284] Evaluation 2: Capacity retention rate after high-temperature storage (Unit: %)
[0285] The secondary batteries of the examples and comparative examples were subjected to 0.33C CC / CV charging (4.2V, 0.02C CUT-OFF) and 0.33C CC discharging (2.5V CUT-OFF) at 25°C twice, and the second discharge capacity C1 was measured. The charged secondary batteries were stored at 60°C for 60 days, then left at room temperature for an additional 30 minutes, and discharged at 0.33C CC (2.5V CUT-OFF) to measure the discharge capacity C2. The capacity retention rate was calculated as follows.
[0286] Capacity retention rate (%) = C2 / C1 × 100.
[0287] Evaluation 3: High-Temperature Storage Characteristics Evaluation - DCIR (Direct Current Internal Resistance) Increase Rate (Unit: %)
[0288] For the secondary batteries according to the examples and comparative examples, the initial DC resistance (unit: mΩ) was measured using the △V / △I (change in voltage / change in current) value, the maximum energy state inside the battery was made to a fully charged state (SOC 100%), and after storing it at 60°C for 60 days in this state, the DC resistance (unit: mΩ) was measured in the same way, and the DCIR increase rate (%) was calculated as follows.
[0289] DCIR growth rate (%) = (DCIR after 60 days at 60℃ / Initial DCIR) × 100.
[0290] Evaluation 4: Transition metal leaching amount after high-temperature storage (Unit: ppm)
[0291] After charging the secondary batteries of the examples and comparative examples at 0.33C CC / CV (4.2V, 0.02C CUT-OFF) at 25℃, the charged secondary batteries were stored at 60℃ for 60 days, and then left at room temperature for an additional 30 minutes.
[0292] Afterward, the electrolyte inside the cell was collected by centrifugation, and an appropriate amount of the electrolyte was mixed with nitric acid to completely ionize it, and then diluted with distilled water to prepare an analytical sample. The total content of directly contained transition metal ions (transition metal leaching amount) was measured using an ICP-MS analyzer.
[0293] The results of the above evaluation are shown in Table 1 below.
[0294] LiPO3NaPO3KPO3 Chemical Formula 1-2 Room Temperature Life High Temperature Life DCIR Increase Rate After High Temperature Storage Transition Metal Leaching Amount After High Temperature Storage Comparative Example 1000063.758.1197.23341 Comparative Example 20.500080.481.5140.22010 Example 10.50000.584.485.1125.51674 Example 20.1000.592.393.5115.11211 Example 30.5000.189.488.1120.71487 Example 40.25000.2588.785.6124.21530 Example 50.500285.183.5130.01500 Example 62000.584.983.0131.41549 Example 700.500.580.782.3135.11541 Example 8000.50.580.080.1133.71533
[0295] synthesis
[0296] Referring to Table 1 above, the electrolyte of the example had excellent room temperature life, low resistance increase rate after high-temperature storage, high capacity retention rate after high-temperature storage, and transition metal leaching inhibition effect after high-temperature storage.
[0297] However, Comparative Example 1, which does not include both types of the additives of the present invention, and Comparative Example 2, which does not include the compound of Formula 1 of the present invention, had inferior effects compared to the example.
[0298]
[0299] Examples 9 to 13 and Comparative Examples 3 to 4
[0300] (1) Preparation of electrolyte
[0301] An electrolyte was prepared by dissolving 1.5 M LiPF6 in a carbonate-based solvent mixed with ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) in a volume ratio of 20:40:40 (based on a total volume of 100 volumes), adding an additive, and mixing. Specifically, the amount of additive used is shown in Table 2 below.
[0302] The molar concentration (M) of LiPF6 in the above electrolyte refers to the amount (number of moles) of lithium salt dissolved per 1 L of electrolyte. The content of additives (unit: weight%) in Table 2 below refers to the weight of the additives relative to 100 weight% of the total electrolyte (lithium salt + non-aqueous organic solvent + additives). The additives used are those with the following chemical formulas 1-2 and 2-1.
[0303] [Chemical Formula 1-2]
[0304]
[0305] [Chemical Formula 2-1]
[0306]
[0307] (2) Manufacturing of secondary batteries
[0308] Manufacturing of the cathode
[0309] A cathode slurry was prepared by mixing 98 wt% of a cathode active material, in which a graphite and Si composite was mixed in a weight ratio of 95.8:4.2, 1 wt% of styrene-butadiene rubber (SBR), and 1 wt% of carboxymethylcellulose (CMC), adding the mixture to distilled water, and stirring for 60 minutes using a mechanical stirrer. The slurry was applied to a thickness of about 60 μm on a 10 μm thick copper foil using a doctor blade, dried in a hot air dryer at 100 °C for 0.5 hours, dried once more under vacuum conditions at 120 °C for 4 hours, and then rolled to produce a cathode.
[0310] Manufacturing of anodes
[0311] A cathode slurry was prepared by mixing 497 wt% of LiFePO4 as a cathode active material, 0.5 wt% of artificial graphite powder and 1.0 wt% of carbon black (Ketjen black) as a conductive material, and 1.5 wt% of polyvinylidene fluoride (PVdF) as a binder, adding the mixture to N-methyl-2-pyrrolidone, and stirring for 30 minutes using a mechanical stirrer. The slurry was applied to a thickness of about 60 μm on a 20 μm thick aluminum foil using a doctor blade, dried in a hot air dryer at 100 ℃ for 0.5 hours, dried once more under vacuum conditions at 120 ℃ for 4 hours, and then rolled to produce a cathode.
[0312] Battery manufacturing
[0313] An electrode assembly was manufactured by assembling the above positive electrode and the above negative electrode with a separator made of polyethylene material with a thickness of 16 μm, and a circular (3.8 V class) secondary battery was manufactured by injecting the above electrolyte.
[0314] Evaluation 5: Room Temperature Life Cycle Characteristics Evaluation
[0315] Room temperature charge-discharge characteristics were evaluated for secondary batteries according to the examples and comparative examples. To this end, 1,000 charge-discharge cycles of the secondary batteries were performed under conditions of 25°C, 0.5C charging (CC / CV, 3.8V, 0.2C Cut-off) / 0.5C discharging (CC, 2.5V Cut-off). The capacity retention rate (unit: %) was calculated according to the following formula.
[0316] Capacity retention rate (%) = (Discharge capacity after 1,000 cycles / Discharge capacity after 1 cycle) × 100.
[0317] Evaluation 6: Low-temperature life cycle characteristics evaluation
[0318] Low-temperature charge-discharge characteristics were evaluated for secondary batteries according to the examples and comparative examples. To this end, 400 charge-discharge cycles of the secondary batteries were performed under conditions of -10℃, 0.5C charging (CC / CV, 3.8V, 0.2C Cut-off) / 0.5C discharging (CC, 2.5V Cut-off). The capacity retention rate (unit: %) was calculated according to the following formula.
[0319] Capacity retention rate (%) = (Discharge capacity after 400 cycles / Discharge capacity after 1 cycle) × 100.
[0320] Evaluation 7: Capacity retention rate after high-temperature storage
[0321] After charging the secondary batteries of the examples and comparative examples at 0.33C CC / CV (3.8V, 0.02C CUT-OFF) at 25℃, the charged secondary batteries were stored at 60℃ for 60 days, then left at room temperature for an additional 30 minutes, and discharged at 0.33C CC (2.5V CUT-OFF) to measure the discharge capacity C2. The capacity retention rate was calculated as follows.
[0322] Capacity retention rate (%) = C2 / C1 × 100.
[0323] Evaluation 8: Increase rate of DCIR (direct current internal resistance) after high-temperature storage
[0324] For the secondary batteries according to the examples and comparative examples, the initial DC resistance (unit: mΩ) was measured using the △V / △I (change in voltage / change in current) value, the maximum energy state inside the battery was made to a fully charged state (SOC 100%), and after storing it at 60°C for 60 days in this state, the DC resistance (unit: mΩ) was measured, and the DCIR increase rate (%) was calculated as follows.
[0325] DCIR growth rate (%) = (DCIR after 60 days at 60℃ / Initial DCIR) × 100.
[0326] The results of the above evaluation are shown in Table 2 below.
[0327] Chemical Formula 1-2 Chemical Formula 2-1 Room Temperature Life Low Temperature Life Capacity Retention Rate After High Temperature Storage DCIR Increase Rate After High Temperature Storage Comparative Example 3 00 85.1 24.1 92.4 118.4 Comparative Example 4 00 58 5.0 70 59 2.0 105.2 Example 9 0 50 58 9.8 74.3 94.2 101.1 Example 10 0 10 58 6.3 48.8 93.3 110.6 Example 11 0 50 19 2.1 88.3 95 798.4 Example 12 0 25 0.2 59 3.3 90 0 95 595.1 Example 13 2.0 0 58 5.9 80.4 90 897.8
[0328] synthesis
[0329] Referring to Table 2 above, the electrolyte of the example had a high room temperature life, low temperature life, and capacity retention rate after high temperature storage, and a low resistance increase rate after high temperature storage.
[0330] On the other hand, Comparative Example 3, which does not contain the two types of additives of the present invention, and Comparative Example 4, which does not contain the compound of Formula 1 of the present invention, had higher room temperature lifespan, low temperature lifespan, and capacity retention rate after high-temperature storage compared to the example, and showed inferior effects in the resistance increase rate after high-temperature storage.
[0331]
[0332] Examples 14 to 18 and Comparative Examples 5 to 6
[0333] (1) Preparation of electrolyte
[0334] An electrolyte was prepared by dissolving 1.15 M LiPF6 in a carbonate-based solvent mixed with ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) in a volume ratio of 20:40:40 (based on a total volume of 100 volumes), adding an additive, and mixing. Specifically, the amount of additive used is shown in Table 3 below.
[0335] The molar concentration (M) of LiPF6 in the above electrolyte refers to the amount (number of moles) of lithium salt dissolved per 1 L of electrolyte. The content of the additive (unit: weight%) in Table 3 below refers to the weight of the additive relative to 100 weight% of the total electrolyte (lithium salt + non-aqueous organic solvent + additive). The above additives used are the above Chemical Formula 1-2 and the following Chemical Formula 2-2.
[0336] [Chemical Formula 2-2]
[0337]
[0338]
[0339] (2) Manufacturing of secondary batteries
[0340] Manufacturing of the cathode
[0341] A cathode slurry was prepared by mixing 98 wt% of a cathode active material, in which a graphite and Si composite was mixed in a weight ratio of 95.8:4.2, 1 wt% of styrene-butadiene rubber (SBR), and 1 wt% of carboxymethylcellulose (CMC), adding the mixture to distilled water, and stirring for 60 minutes using a mechanical stirrer. The slurry was applied to a thickness of about 60 μm on a 10 μm thick copper foil using a doctor blade, dried in a hot air dryer at 100 °C for 0.5 hours, dried once more under vacuum conditions at 120 °C for 4 hours, and then rolled to produce a cathode.
[0342] Manufacturing of anodes
[0343] LiNi as a positive electrode active material 0.80 Co 0.10 Mn 0.10 An anode slurry was prepared by mixing O297 wt%, artificial graphite powder as a conductive material, 1.0 wt% carbon black (Ketjenblack), and 1.5 wt% polyvinylidene fluoride (PVdF) as a binder, adding the mixture to N-methyl-2-pyrrolidone, and stirring for 30 minutes using a mechanical stirrer. The slurry was applied to a thickness of about 60 μm on a 20 μm thick aluminum foil using a doctor blade, dried in a hot air dryer at 100 ℃ for 0.5 hours, dried once more under vacuum conditions at 120 ℃ for 4 hours, and then rolled to produce an anode.
[0344] Battery manufacturing
[0345] An electrode assembly was manufactured by assembling the above positive electrode and the above negative electrode with a separator made of polyethylene material with a thickness of 16 μm, and a prismatic (4.2 V class) secondary battery was manufactured by injecting the above electrolyte.
[0346] Evaluation 9: Increase rate of DCIR (direct current internal resistance) after high-temperature storage
[0347] For the secondary batteries according to the examples and comparative examples, the initial DC resistance (unit: mΩ) was measured using the △V / △I (change in voltage / change in current) value, the maximum energy state inside the battery was made to a fully charged state (SOC 100%), and after storing it at 60°C for 60 days in this state, the DC resistance (unit: mΩ) was measured, and the DCIR increase rate (%) was calculated as follows.
[0348] DCIR growth rate (%) = (DCIR after 60 days at 60℃ / Initial DCIR) × 100.
[0349] Evaluation 10: Capacity retention rate after high-temperature storage
[0350] The secondary batteries of the Examples and Comparative Examples were charged at 0.33C CC / CV (4.2V, 0.02C CUT-OFF) and discharged at 0.33C CC (2.5V CUT-OFF) at 25°C. After storing the charged secondary batteries at 60°C for 60 days, they were additionally left at room temperature for 30 minutes, and discharged at 0.33C CC (2.5V CUT-OFF) to measure the discharge capacity C2 (unit: Ah). The capacity retention rate was calculated as follows.
[0351] Capacity retention rate (%) = C2 / C1 × 100.
[0352] Evaluation 11: High-temperature storage characteristics Gas generation amount (unit: mL) and gas growth rate (unit: %)
[0353] High-temperature gas generation characteristics were evaluated for secondary batteries according to the examples and comparative examples. To this end, the maximum energy state inside the battery was set to a fully charged state (SOC 100%), and the amount of gas generated (unit: mL) was evaluated in this state, both initially (before storage at high temperature (60℃)) and after storage at high temperature (60℃) for 7 days. The ratio of gas generation was calculated by measuring the volume change before and after high-temperature storage and converting it into a change in mass using Archimedes' method. The gas increase rate was calculated as (amount of gas generated after storage at high temperature for 7 days) / (initial amount of gas generated) x 100.
[0354] Evaluation 12: Evaluation of Room Temperature Charge / Discharge Cycle Characteristics
[0355] Room temperature charge-discharge characteristics were evaluated for secondary batteries according to the examples and comparative examples. To this end, 200 charge-discharge cycles of the secondary batteries were performed under conditions of 25°C, 0.33C charging (CC / CV, 4.2V, 0.2C Cut-off) / 1C discharging (CC, 2.5V Cut-off). The capacity retention rate (unit: %) was calculated according to the following formula.
[0356] Capacity retention rate (%) = (Discharge capacity after 200 cycles / Discharge capacity after 1 cycle) × 100.
[0357] The results of the above evaluation are shown in Tables 4 and 5 below.
[0358] Chemical Formula 1-2 Chemical Formula 2-2 Comparative Example 500 Comparative Example 600.5 Example 140.250.5 Example 150.10.5 Example 160.11.0 Example 170.50.5 Example 180.51.0
[0359] Initial DCIR DCIR after high-temperature storage DCIR Increase Rate Initial Capacity Capacity after high-temperature storage Capacity Retention Rate Comparison Example 5 10.90 13.47 124 6.09 5.59 91.8 Comparison Example 6 11.17 13.50 121 6.105.49 90 Example 14 13.27 13.72 103 6.06 5.64 93 Example 15 12.46 13.59 109 6.105.58 91 Example 16 12.50 13.83 111 6.07 5.54 91 Example 17 13.03 13.49 104 6.08 5.529 0.8 Example 18 13.33 13.85 104 6.015.51 92
[0360] Initial Gas Generation Amount Gas Generation Amount After High-Temperature Storage Gas Growth Rate Capacity Retention Rate Comparison Example 5 10.93 13.03 11996.3 Comparison Example 6 10.95 12.89 11896.6 Example 14 10.43 10.98 10599.3 Example 15 11.08 12.44 11297 Example 16 11.05 12.39 11298 Example 17 10.88 11.98 11097.8 Example 18 10.85 11.88 10998.5
[0361] synthesis
[0362] Referring to Tables 4 and 5 above, the electrolyte of the example had high room temperature life, high temperature life, and capacity retention rate after high temperature storage, and low resistance increase rate and gas generation rate after high temperature storage.
[0363] On the other hand, Comparative Example 5, which does not contain the two types of additives of the present invention, and Comparative Example 6, which does not contain the compound of Formula 1 of the present invention, showed inferior effects compared to the example in terms of room temperature life, high temperature life, capacity retention rate after high temperature storage, resistance increase rate after high temperature storage, and gas generation rate after high temperature storage.
[0364]
[0365] Although preferred embodiments of the present invention have been described above, the present invention is not limited thereto and can be implemented with various modifications within the scope of the claims, the detailed description of the invention, and the attached drawings, and it is obvious that such modifications also fall within the scope of the present invention.
Claims
1. A non-aqueous organic solvent; a lithium salt; and an additive, comprising, The above additive is an electrolyte for a secondary battery comprising a mixture of (I) and (II): (I)(a) One or more alkali metal salts or alkaline earth metal salts of metaphosphoric acid (HPO3), or (b) one or more of lithium borate or lithium phosphate, (II) Compounds represented by the following chemical formula 1: [Chemical Formula 1] (In the above chemical formula 1, R 11 , R 12 , R 13 and R 14 Each is independently hydrogen, a halogen, a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C1 to C20 alkoxy group, a substituted or unsubstituted C2 to C20 alkenyl group, a substituted or unsubstituted C2 to C20 alkynyl group, a substituted or unsubstituted C3 to C20 cycloalkyl group, a substituted or unsubstituted C6 to C20 aryl group, or a substituted or unsubstituted C2 to C20 heteroaryl group, and R 15 is a substituted or unsubstituted C1 to C20 alkoxy group).
2. In claim 1, R in the above chemical formula 1 11 , R 12 , R 13 , and R 14 Electrolyte for a secondary battery, each independently hydrogen or a substituted or unsubstituted C1 to C5 alkyl group.
3. In claim 1, R in the above chemical formula 1 15 An electrolyte for a secondary battery, wherein is a methoxy group, an ethoxy group, an n-propoxy group, an iso-propoxy group, an n-butoxy group, an iso-butoxy group, a tert-butoxy group, an n-pentoxy group, or an iso-pentoxy group.
4. An electrolyte for a secondary battery according to claim 1, wherein the compound is one or more of the following chemical formulas 1-2 to 1-5: [Chemical Formula 1-2] [Chemical Formula 1-3] [Chemical Formula 1-4] [Chemical Formula 1-5] .
5. An electrolyte for a secondary battery according to claim 1, wherein the alkali metal salt of the metaphosphoric acid comprises one or more of LiPO3, NaPO3, and KPO3.
6. An electrolyte for a secondary battery according to claim 1, wherein one or more of the lithium borate or lithium phosphate are represented by the following chemical formula 2: [Chemical Formula 2] R 21 C1 to C10 alkylene groups formed by single bonds or substituted or unsubstituted bonds, A is boron (B) or phosphorus (P), and X is a halogen element, and n is an integer from 0 to 2, and m is an integer from 1 to 3, and If A is boron (B), then n + m = 2 is satisfied, and If A is P, then n + m = 3 is satisfied).
7. An electrolyte for a secondary battery according to claim 1, wherein one or more of the lithium borate or lithium phosphate are represented by any one of the following chemical formulas 2-1 to 2-5: [Chemical Formula 2-1] [Chemical Formula 2-2] [Chemical Formula 2-3] [Chemical Formula 2-4] [Chemical Formula 2-5] .
8. In paragraph 1, the above (I) : (II) is an electrolyte for a secondary battery included in the above electrolyte in a weight ratio of 1 : 0.1 to 1 :
10.
9. An electrolyte for a secondary battery according to claim 1, wherein (II) is included in an amount of 0.01 to 5 weight% with respect to the total amount of the electrolyte, and (I) is included in an amount of 0.01 to 5 weight% with respect to the total amount of the electrolyte.
10. An electrolyte for a secondary battery according to claim 1, wherein the additive is included in an amount of 0.01 to 10 weight% with respect to the total amount of the electrolyte.
11. An electrolyte for a secondary battery according to claim 1, wherein the non-aqueous organic solvent is a mixture comprising ethylene carbonate (EC): ethylmethyl carbonate (EMC): dimethyl carbonate (DMC) in a volume ratio of 10 to 30: 20 to 50: 20 to 50.
12. An electrolyte for a secondary battery according to claim 1, wherein the concentration of the lithium salt in the electrolyte is 0.1M to 3.0M.
13. An electrolyte for a secondary battery according to claim 1, wherein the lithium salt is one or more selected from the group consisting of LiPF6, LiClO4, LiBF4, (lithium bis(fluorosulfonyl)imide (LiFSI), LiTFSI, LiSO3CF3, LiBOB, LiFOB, LiDFBP, LiTFOP, LiPO2F2, LiSbF6, LiAsF6, LiAlO2, LiAlCl4, LiCl, LiI, LiN(SO3C2F5)2, Li(FSO2)2N, and LiC4F9SO3.
14. An electrolyte for a secondary battery according to claim 1, wherein the additive comprises 95% by weight or more of the total additive of the electrolyte.
15. Anode comprising a positive active material; A cathode comprising a cathode active material; and A secondary battery comprising an electrolyte according to any one of claims 1 to 14.
16. A secondary battery according to claim 15, wherein the positive electrode active material comprises one or more of a lithium iron phosphate-based compound, a lithium manganese iron phosphate-based compound, a lithium nickel cobalt manganese-based oxide, and a lithium nickel cobalt aluminum-based oxide.
17. A secondary battery according to claim 15, wherein the negative electrode active material comprises at least one of graphite and a Si composite.