Silicon-carbon composite for negative electrode active material of secondary battery and method for preparing same

A silicon-carbon composite with a carbon coating on silicon particles via low-temperature CVD addresses stability and reactivity issues, enhancing discharge capacity and lifespan by maintaining small silicon crystal grains and suppressing silicon carbide formation.

WO2026240403A1PCT designated stage Publication Date: 2026-11-19OCI CO LTD(KR)
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2026/005868
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-13
Filing Date
2026-05-07
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Silicon-based negative electrode materials for secondary batteries face challenges such as reduced lifespan stability due to volume expansion, structural cracking, and reactivity with water, leading to decreased conductivity and manufacturing difficulties.

Method used

A silicon-carbon composite is manufactured with a carbon-containing coating layer on silicon particles using low-temperature chemical vapor deposition (CVD) to protect the silicon surface and control crystal grain size, suppressing excessive silicon carbide formation and maintaining mechanical flexibility.

Benefits of technology

The silicon-carbon composite improves discharge capacity, initial efficiency, and lifespan characteristics by stabilizing the silicon particles, reducing viscosity issues, and enhancing the mechanical flexibility of the negative electrode material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2026005868_19112026_PF_FP_ABST
    Figure KR2026005868_19112026_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a silicon-carbon composite for use as a negative electrode active material for a secondary battery, and a method for preparing same. More specifically, the present invention relates to: a silicon-carbon composite in which a carbon-containing coating layer is formed at a low temperature on the surface of a core containing silicon (Si) particles by a chemical vapor deposition (CVD) process to protect the surface of the silicon and keep the silicon grain size at or below 10 nm, and which can simultaneously improve the discharge capacity, initial efficiency, and capacity retention rate of a secondary battery; and a method for preparing same.
Need to check novelty before this filing date? Find Prior Art

Description

Silicon-carbon composite for secondary battery negative electrode active material and method for manufacturing the same

[0001] The present invention relates to a silicon-carbon composite for use as a negative electrode active material for a secondary battery and a method for manufacturing the same. More specifically, the invention relates to a silicon-carbon composite and a method for manufacturing the same, which can simultaneously improve the discharge capacity, initial efficiency, and capacity retention rate of a secondary battery by forming a coating layer containing carbon on the surface of a core containing silicon (Si) particles using a chemical vapor deposition (CVD) process at a low temperature to protect the surface of the silicon while maintaining the silicon crystal grain size at 10 nm or less.

[0002] The performance improvement of secondary batteries is based on the components of the cathode material, anode active material, and electrolyte.

[0003] Among the above components, graphite-based materials, which are mainly used as negative electrode active materials, are commercially available due to their excellent electrochemical performance and low cost, but they have limitations in being applied to high-capacity secondary batteries because their theoretical capacity is limited to 370 mAh / g.

[0004] To overcome the aforementioned limitations, non-graphite cathode active materials such as silicon, tin, and germanium are emerging as alternative materials. Among them, silicon is gaining attention as a material to replace graphite because it has a theoretical capacity of 4,000 to 4,200 mAh / g, can store a very large amount of lithium per unit weight, and exhibits a high capacity nearly 10 times greater than that of graphite. However, despite its high theoretical capacity, it has the disadvantage of reduced lifespan stability due to a large volume expansion of approximately 400% during the charge and discharge process, which causes problems such as structural cracking, destruction, and pulverization of silicon particles and reduced conductivity, as well as the continuous formation of a solid electrolyte interface (SEI) layer.

[0005] In addition, due to the high water-based reactivity of silicon particles, phenomena such as a decrease in pH and a decrease in viscosity may occur when manufacturing a cathode slurry using them, which can act as a factor causing difficulties in the manufacturing process and further degradation of battery performance.

[0006] For example, there is a need to develop a high-quality silicon-carbon composite for secondary battery negative electrode active materials and a method for manufacturing the same, which can further improve the initial discharge capacity, initial efficiency, and lifespan characteristics of secondary batteries by controlling the structural properties of a composite containing silicon particles and carbon.

[0007] The first objective of the present invention is to provide a silicon-carbon composite in which silicon does not react with water by covering the surface of a core containing silicon particles with a carbon-containing coating layer through low-temperature carbon CVD coating technology to improve problems such as silicon reacting with water and the viscosity of the cathode slurry decreasing.

[0008] The second objective of the present invention is to provide a method for manufacturing a silicon-carbon composite that can suppress the excessive generation of silicon carbide (SiC) without increasing the size of silicon crystal grains by coating the surface of a core containing silicon particles through a carbon CVD coating technology carried out at a low temperature of 800°C or lower.

[0009] The objectives of the present invention are not limited to those mentioned above, and other objectives and advantages of the present invention not mentioned may be understood from the following description and will be more clearly understood by the embodiments of the present invention. Furthermore, it will be readily apparent that the objectives and advantages of the present invention can be realized by the means and combinations thereof set forth in the claims.

[0010] According to one aspect of the present invention, a method for manufacturing a silicon-carbon composite comprises: (S1) introducing a core containing silicon particles into a chemical vapor deposition (CVD) reactor; (S2) supplying a mixed gas containing a carbon source gas into the CVD reactor; (S3) reacting the core containing silicon particles and the carbon source gas under a temperature condition greater than 600°C and less than 700°C to chemically vapor deposit a coating layer containing carbon on the surface of the core; and (S4) precipitating the result of step (S3) as a solid to obtain a silicon-carbon composite.

[0011] According to one aspect of the present invention, the step (S1) and / or (S2) may be performed under an inert gas atmosphere to provide a method for manufacturing a silicon-carbon composite.

[0012] According to one embodiment of the present invention, a method for manufacturing a silicon-carbon composite can be provided in which the inert gas is one or more selected from the group consisting of argon gas, helium gas, and nitrogen gas.

[0013] According to one aspect of the present invention, a method for manufacturing a silicon-carbon composite can be provided in which the mixed gas containing the carbon source gas comprises the carbon source gas and the inert gas, and the flow rate ratio of the carbon source gas and the inert gas is carbon source gas : inert gas = 1:3 to 1:30.

[0014] According to one embodiment of the present invention, a method for manufacturing a silicon-carbon composite can be provided in which the carbon source gas is one or more selected from the group consisting of acetylene (C2H2), ethylene, propylene, methane, ethane, and propane.

[0015] According to one embodiment of the present invention, a method for manufacturing a silicon-carbon composite can be provided, wherein the thickness of the coating layer containing carbon is 10 to 30 nm.

[0016] According to one embodiment of the present invention, a method for manufacturing a silicon-carbon composite can be provided in which the reaction time in step (S3) is 3 to 6 hours.

[0017] According to one aspect of the present invention, a silicon-carbon composite manufactured according to the method for manufacturing the silicon-carbon composite can be provided.

[0018] According to one aspect of the present invention, a silicon-carbon composite can be provided in which the size of silicon crystal grains measured by X-ray diffraction (XRD) analysis within the silicon-carbon composite is 10 nm or less.

[0019] According to one aspect of the present invention, a negative electrode active material comprising the silicon-carbon composite can be provided.

[0020] According to one embodiment of the present invention, a secondary battery comprising the negative electrode active material can be provided.

[0021] The silicon-carbon composite according to the present invention can improve the lifespan of a secondary battery when used as a negative electrode active material by maintaining the size of the silicon crystal grains at 10 nm or less and effectively protecting the surface of the silicon through low-temperature carbon CVD coating technology, thereby coating the surface of the core containing silicon particles.

[0022] According to the method for manufacturing a silicon-carbon composite of the present invention, SiC is not excessively generated within the silicon-carbon composite, thereby providing a silicon-carbon composite with improved expression capacity, discharge capacity, etc. in a secondary battery.

[0023] According to the method for manufacturing a silicon-carbon composite according to the present invention, the problem of reduced viscosity of the negative electrode slurry can be effectively solved by blocking the water-based reactivity of silicon in the silicon-carbon composite, and a silicon-based negative electrode active material with greatly improved stability can be realized by maintaining the mechanical flexibility of amorphous silicon and effectively suppressing damage caused by volume change of silicon during charging and discharging.

[0024] In addition to the effects described above, the effects of the present invention are described together with the details for implementing the invention below.

[0025] FIG. 1 shows silicon grain size measurement data through XRD analysis of silicon-carbon composites (or negative electrode active materials) according to Comparative Examples 1 to 3 and Example 1 (Measurement Example 1).

[0026] FIG. 2 shows data measuring the change in viscosity over time in a cathode slurry prepared using silicon-carbon composites (or cathode active materials) according to Comparative Examples 1 and 2 and Example 1 (Experimental Example 1).

[0027] FIG. 3 shows experimental data on the capacity recovery ratio according to the evaluation of coin pool cells using silicon-carbon composites (or negative electrode active materials) according to Comparative Examples 1 and 4 and Example 1 (Experimental Example 3).

[0028] The aforementioned objectives, features, and advantages are described in detail below with reference to the description of the invention, and accordingly, a person skilled in the art to which the invention pertains will be able to easily implement the technical concept of the invention. In describing the invention, detailed descriptions of known technologies related to the invention are omitted if it is determined that such descriptions may unnecessarily obscure the essence of the invention. The terms described below are terms used in consideration of their functions and operations in the invention, and the meaning of each term should be interpreted based on the content throughout this specification.

[0029] As used in this specification, singular expressions include plural expressions unless the context clearly indicates otherwise.

[0030] Where terms such as "comprising," "having," "consisting of," "containing," or "having" are used for a component in this specification, other parts may be added unless "only" is used. Where a component is expressed in the singular, it includes cases where it is included in the plural unless specifically stated otherwise.

[0031] In this specification, where it is stated that one component is "connected," "coupled," or "connected" to another component, it should be understood that the components may be directly connected or connected to each other, but that another component may be "interposed" between each component, or that each component may be "connected," "coupled," or "connected" through another component.

[0032] In interpreting the components in this specification, they are interpreted to include an error range even if there is no separate explicit description.

[0033] In this specification, the standard for units is based on weight unless otherwise specifically stated. For example, if "%" is indicated, it is interpreted as weight % (wt.%).

[0034] The present invention will be described in more detail below.

[0035] Method for manufacturing silicon-carbon composites

[0036] According to one embodiment of the present invention, a method for manufacturing a silicon-carbon composite comprises: (S1) introducing a core containing silicon particles into a chemical vapor deposition (CVD) reactor; (S2) supplying a mixed gas containing a carbon source gas into the CVD reactor; (S3) reacting the core containing silicon particles and the carbon source gas under a temperature condition greater than 600°C and less than 700°C to chemically vapor deposit a coating layer containing carbon on the surface of the core; and (S4) precipitating the result of step (S3) as a solid to obtain a silicon-carbon composite.

[0037] The low-temperature CVD carbon coating method according to the method for manufacturing a silicon-carbon composite of the present invention can achieve the objectives of the present invention, such as making the silicon crystal grain size 10 nm or less by suppressing, to the maximum extent, the thermal crystallization of Si particles caused by high-temperature thermal energy that may occur during the CVD process. In the case of general CVD-based carbon coating, the silicon crystal grain size can generally increase significantly after coating due to thermal crystallization of silicon particles caused by thermal energy, and this can be largely dependent on the reaction temperature.

[0038] The applicant completed the present invention by conducting heat treatment temperature screening through XRD measurements of silicon-carbon composites obtained via a CVD process at 600°C to 700°C, and by discovering that the optimal temperature condition for the low-temperature CVD process of the present invention is a temperature condition greater than 600°C and less than 700°C. When a coating layer containing carbon is deposited on a core containing silicon particles via a CVD process under the above temperature conditions, the size of the silicon crystal grains can be maintained at 10 nm or less through XRD analysis after coating. In addition, excessive SiC formation within the final silicon-carbon composite can be suppressed. Under temperature conditions of 700°C or higher, excessive thermal crystallization of Si particles occurs, causing the Si crystal grain size to exceed 10 nm, and under temperature conditions of 600°C or lower, carbon coating on the surface of the Si / C composite may not proceed well. The above temperature conditions may be, for example, 610°C or higher, 620°C or higher, or 630°C or higher, and 690°C or lower, 680°C or lower, or 670°C or lower.

[0039] According to one embodiment of the present invention, steps (S1) and / or (S2) may be performed under an inert gas atmosphere. The mixed gas containing the carbon source gas in step (S2) may include an inert gas.

[0040] According to one embodiment of the present invention, the inert gas may be one or more selected from the group consisting of argon, nitrogen, and helium gases. The inert gas acts as a carrier and does not react with the carbon source gas (such as acetylene), thereby suppressing the formation of byproducts.

[0041] According to one embodiment of the present invention, the carbon source gas may be one or more selected from the group consisting of acetylene (C2H2), ethylene, propylene, methane, ethane, and propane.

[0042] According to one embodiment of the present invention, the mixed gas containing the carbon source gas comprises the carbon source gas and the inert gas, and the flow rate ratio of the carbon source gas to the inert gas in the mixed gas containing the carbon source gas may be carbon source gas : inert gas = 1:3 to 1:30, and preferably 1:10 to 1:20. If the lower limit is exceeded, there may be a problem in that the carbon source gas (acetylene, etc.) at a high concentration is excessively decomposed, thereby forming a large amount of byproducts, and if the upper limit is exceeded, there may be a problem in that the decomposition rate drops significantly due to the extremely low concentration of the carbon source gas (acetylene, etc.), so that the coating layer is not formed. To ensure stable decomposition of the carbon source gas (acetylene, etc.), the carbon concentration must be controlled by introducing it together with about 10 to 30 times the amount of inert gas so that the formation of byproducts due to carbon decomposition can be suppressed during carbon coating.

[0043] According to one embodiment of the present invention, the reaction time in step (S3) may be 3 to 6 hours. If the lower limit is exceeded, there may be a problem in that the carbon coating is not sufficiently applied and the Si anode active material cannot be effectively protected, and if the upper limit is exceeded, there may be a problem in that the capacity and ICE (Initial Coulombic Efficiency) of the anode active material decrease due to an excessive amount of carbon coating.

[0044] According to one embodiment of the present invention, the rotation speed of the reaction substrate in step (S3) may be 2.0 to 4.0 rpm. If the lower limit is exceeded, there may be a problem of not being able to achieve a uniform coating due to the almost non-flow of silicon and / or composite particles, and if the upper limit is exceeded, there may be a problem of particles being released outside the reactor along with the reaction gas due to excessive scattering of silicon and / or composite particles.

[0045] Silicon-Carbon Composite

[0046] According to one embodiment of the present invention, a silicon-carbon composite manufactured according to the method for manufacturing a silicon-carbon composite according to one embodiment of the present invention can be provided.

[0047] In one embodiment of the present invention, the size of silicon crystal grains measured by X-ray diffraction (XRD) analysis within the silicon-carbon composite may be 10 nm or less. The size of silicon crystal grains measured by the XRD analysis may correspond to the average value of the entire silicon. The size of the silicon crystal grains may be the size of the crystal grains in the surface silicon layer. For example, the size of the crystal grains may be 9 nm or less, 8 nm or less, or 7 nm or less. There is no specific lower limit, but for example, the size of the crystal grains may be 1.0 nm or more. If the upper limit is exceeded, the stress caused by volume change during charging and discharging of the silicon negative electrode active material cannot be suppressed, which may lead to a problem of reduced lifespan characteristics.

[0048] When a negative electrode slurry is prepared using a silicon-carbon composite having silicon crystal grains maintained at 10 nm or less according to one embodiment of the present invention as a negative electrode active material, the decrease in viscosity of the negative electrode slurry can be minimized. For example, in a measurement of the change in viscosity of the negative electrode slurry over about one week, the decrease in viscosity can be maintained within 5%. If a core containing silicon particles is not surface-treated with a coating layer containing carbon according to the manufacturing method of the present invention, the viscosity of the negative electrode slurry decreases, and consequently, the coating properties of the negative electrode plate may be reduced.

[0049] According to one embodiment of the present invention, the silicon-carbon composite may have an average particle size (D50) of 3 to 7 μm. If the value exceeds the lower limit, there may be a problem of reduced ICE due to excessive side reactions caused by the high surface area, and if the value exceeds the upper limit, there may be a problem of reduced lifespan characteristics due to cracking of the composite particles.

[0050] When a silicon-carbon composite according to one embodiment of the present invention is used as a negative electrode active material for a secondary battery, the reduction in discharge capacity can be minimized. For example, the reduction in discharge capacity may be within 10%.

[0051] In a silicon-carbon composite according to one embodiment of the present invention, the thickness of the carbon-containing coating layer may be 10 to 30 nm, preferably 15 to 25 nm or 15 to 20 nm. If the thickness exceeds the lower limit, there may be a problem where the lifespan characteristics are reduced due to insufficient carbon coating, and if the thickness exceeds the upper limit, there may be a problem where conductivity decreases and ICE is degraded due to an excessively thick carbon coating. The carbon-containing coating layer applied in the present invention may be an amorphous-based carbon layer. Since an amorphous-based carbon layer may have low conductivity and high reactivity with the electrolyte, ICE may be degraded if it is excessively coated. As a result of diligent efforts, the inventors have determined the appropriate thickness of the carbon-containing coating layer as described above and have completed the present invention.

[0052] A silicon-carbon composite according to one embodiment of the present invention can improve lifespan performance when used as a negative electrode active material for a secondary battery.

[0053] According to one embodiment of the present invention, a negative electrode active material comprising the silicon-carbon composite can be provided. According to one embodiment of the present invention, a secondary battery comprising the negative electrode active material can be provided.

[0054] According to one embodiment of the present invention, the secondary battery may have an initial charge capacity (ICC; initial charge capacity) of 2200 to 2500 mAh / g. In addition, the secondary battery may have an initial coulombic efficiency (ICE; discharge amount relative to initial charge amount) of 90 to 95% at 1.5 V. In addition, the secondary battery may have an initial discharge capacity (IDC; initial discharge capacity) of 2000 to 2200 mAh / g at 1.5 V.

[0055] The structure and operation of the present invention will be described in more detail below through preferred embodiments. However, these are presented as preferred examples of the present invention and should not be interpreted in any way as limiting the present invention.

[0056] I. Preparation Example: Preparation of a Silicon-Carbon Composite

[0057] Example 1

[0058] A core containing silicon particles with a grain size of 1.7 nm (XRD analysis) was prepared by chemical vapor deposition (CVD) of silicon and carbon onto a porous carbon-based structure. The porous carbon-based structure was prepared by spheroidizing, activating, and carbonizing carbon using Carbon Black (DC3501) produced by OCI. The particle size of the prepared porous carbon-based structure was approximately 3-7 μm, and a first pore volume with an average pore size of 50 nm or less was 0.27 cc / g, and a second pore volume with an average pore size of 50 nm or more and 350 nm or less was 1.26 cc / g.

[0059] 50 g of the above core was placed inside a Rotary Kiln reactor and heated at 650°C.

[0060] Acetylene gas and argon gas were injected into a reaction apparatus heated to 650°C at a ratio of 0.05 slm : 1.95 slm (total 2.0 slm) under atmospheric pressure, and the reaction was carried out for 4 hours with the rotation speed of the reaction substrate at 3.0 rpm to form a carbon-containing coating layer on the surface of the core, and then cooled to room temperature to produce a final silicon-carbon composite with a solid content.

[0061] Comparative Example 1

[0062] The core of Example 1 was used without undergoing the CVD process.

[0063] Comparative Example 2

[0064] A silicon-carbon composite was prepared in the same manner as in Example 1, except that the reaction temperature was set to 600°C.

[0065] Comparative Example 3

[0066] A silicon-carbon composite was prepared in the same manner as in Example 1, except that the reaction temperature was set to 700°C.

[0067] Comparative Example 4

[0068] The procedure was carried out in the same manner as in Example 1, but argon gas was injected at 2.0 slm under atmospheric pressure into a reaction device heated to 650°C, and heat treatment was performed for 4 hours at a rotation speed of 3.0 rpm of the reaction substrate, after which the solid was recovered by cooling to room temperature.

[0069] II. Measurement of Physical Properties of Silicon-Carbon Composites

[0070] Measurement Example 1. XRD Analysis

[0071] The size of silicon crystal grains in the silicon-carbon composites of Comparative Examples 1 to 3 and Example 1 was measured by XRD analysis under the following conditions.

[0072] Analytical Instrument: Panalytical’s Empyrean

[0073] Analysis conditions: 40 kV / 30 mA

[0074] X-ray source : Cu Ka1

[0075] Silicon grain size: Uses the value obtained through the Scherrer equation in the software.

[0076] The results of the above measurement example 1 are listed in Table 1.

[0077] Si grain size (nm) Comparative Example 11.7 Comparative Example 21.8 Example 15.8 Comparative Example 311.7

[0078] In the case of the 600℃ carbon CVD coating (Comparative Example 2), no crystalline silicon peak (around 2θ = 28º) was observed, and in the case of 650℃ (Example 1), the grain size was found to be about 6 nm (5.8 nm), and in the case of 700℃ (Comparative Example 3), it was found to be at the level of 11.7 nm.

[0079] It was confirmed that a core composed of silicon particles is structurally more flexible and better able to withstand volume changes occurring during charging and discharging when in an amorphous state. It was also confirmed that higher flexibility can be expected as the size of the silicon crystal grains decreases, particularly when it is 10 nm or less.

[0080] Measurement Example 2. Analysis of Low-Temperature Carbon CVD Coating Layer

[0081] The C content of the original sample was measured by analyzing CO and CO2 generated by burning the sample using an analytical instrument (ELTRA GmBH CS-2000), and the average value was used after three measurements.

[0082] The results of the above measurement example 2 are listed in Table 2.

[0083] O (wt%)(ONH)C (wt%)(C / S)Si (wt%) Comparative Example 10.5 38.0 61.5 Comparative Example 20.5 38.5 61.0 Example 10.5 39.0 60.5 Comparative Example 30.5 39.7 59.8

[0084] It was confirmed that after carbon CVD coating at 600℃ (Comparative Example 2) / 650℃ (Example 1) / 700℃ (Comparative Example 3), the weight percentage of carbon in the composite increased by 0.5% / 1.0% / 1.7%, respectively, compared to Ref (Comparative Example 1). It was found that this was because the amount of carbon CVD coating increased with increasing reaction temperature.

[0085] As shown in Tables 1 and 2 above, under the same conditions, the amount of carbon-containing coating varied depending on the reaction temperature, which could be confirmed by the change in C weight%. It was confirmed that at 600°C, the carbon coating was not sufficient, and at 700°C, although a large amount of carbon coating was formed, the grain size grew excessively.

[0086] III. Performance Evaluation of Silicon-Carbon Composites

[0087] Experimental Example 1. Cathode Slurry Viscosity Test

[0088] Cathode Slurry Recipe

[0089] A cathode slurry was prepared by using the silicon-carbon composites of Comparative Examples 1 to 3 and Example 1 as cathode active materials and mixing the materials with a sinker in the weight and weight ratios as described in Table 3 below.

[0090] Weight (g) Ratio (Wet%) Cathode Active Material Silicon-Carbon Composite 5.5 9 5.8 Graphite 21.9 Carbon Black 0.2 9 1.0 CMC (sodium salt of carboxymethyl cellulose) 0.4 9 1.7 SBR (styrene-butadiene rubber) 0.8 6 1.5 DI Water 3 4.5 9 - Weight % of Cathode Active Material in Cathode Slurry 43.2

[0091] Slurry viscosity test method

[0092] After placing the above cathode slurry in a 60 mL vial, the viscosity value at 20 rpm was measured using a viscometer (brookfield viscometer dv-ii +pro / SC4-31 Spindles).

[0093] 1 L of cathode slurry was placed in a container and run overnight at 150 rpm using a ball mill, and the change in viscosity was measured daily.

[0094] The results of the above slurry viscosity test are shown in Figure 2 and Table 4.

[0095] Slurry viscosity change rate (%) (@ 7 days) Comparative Example 1-79 Comparative Example 2-66 Example 1-1 Comparative Example 3-0.5

[0096] As a result of the cathode slurry viscosity test, Comparative Example 1 had a portion of the silicon surface exposed, making it prone to reaction with water; consequently, the reaction between silicon and water caused a decrease in pH, creating an acidic environment. In an acidic state, the binding strength of the CMC binder weakens, leading to a decrease in the viscosity of the cathode slurry. The 600°C CVD coated sample (Comparative Example 2) experienced a decrease in cathode slurry viscosity because the low reaction temperature prevented proper protection of the surface silicon. It was confirmed that the 650°C CVD coated sample (Example 1) suppressed the decrease in slurry viscosity by effectively protecting the surface silicon with an appropriate surface coating.

[0097] Experimental Example 2: Evaluation of 100% Si / C Half Cell

[0098] To prepare a cathode slurry, a conductive material was prepared by mixing conductive carbon black (Super P) and carbon nanotubes (SWCNT) (Super P : SWCNT = 9.9 : 0.1, weight ratio), and a binder was prepared by mixing CMC (sodium salt of carboxymethyl cellulose) and SBR (styrene-butadiene rubber) (CMC : SBR = 3 : 7, weight ratio). The cathode active material, conductive material, and binder prepared above were mixed using a sinker mixer (cathode active material : conductive material : binder = 8 : 1 : 1, weight ratio) to obtain a cathode slurry.

[0099] The above cathode slurry was applied to a cathode current collector (copper foil, 18 μm), dried at 80°C for 1 hour, and then heat-treated in a vacuum oven at 100°C for 12 hours to obtain a cathode plate.

[0100] The fabricated negative electrode plate was punched to 16 mmΦ to obtain a negative electrode plate for a coin cell, and coin cell fabrication and electrochemical evaluation were carried out using the negative electrode plate and a Li-metal counter electrode. The charge and discharge conditions for the initial 1-2 cycles (Formation cycle) were charge CC / CV: 0.005 V / 0.005 C, discharge CC: 1.0 V, and the rate limit was 0.1 C.

[0101] Using the half-cell device TOSCAT-3100, the initial coulombic efficiency (ICE; discharge amount relative to initial charge amount), initial charge capacity (ICC; initial charge capacity), and initial discharge capacity (IDC; initial discharge capacity) were measured and are shown in Table 5 below.

[0102] ICC (mAh / g) ICE (@ 1.5 V)(%) IDC (@ 1.5 V)(mAh / g) Capacity reduction ratio (%) relative to IDC of Comparative Example 1 Comparative Example 1 246692.922900 Comparative Example 2 231692.621466 Example 1 230492.321277 Comparative Example 3 225091.3205410

[0103] In the case of carbon CVD coating, it was confirmed that there was a slight decrease in ICC and ICE compared to the REF sample (Comparative Example 1). The decrease in ICC can be interpreted as a result of the decrease in the weight percentage of silicon in the composite due to the introduced carbon coating layer, and the decrease in ICE is presumed to be due to the low electrical conductivity of the carbon coating layer introduced through the CVD process.

[0104] Due to these effects, the 700℃ CVD coated sample (Comparative Example 3) showed a high reduction rate of 10% compared to the IDC capacity of the REF sample (Comparative Example 1).

[0105] Experimental Example 3: Evaluation of Coin Full Cell Lifespan

[0106] A cathode material was prepared by mixing 9 wt% of the silicon-carbon composite prepared in Comparative Examples 1 and 4 and Example 1, respectively, with 91 wt% of graphite by weight. Separately, a conductive material was prepared by mixing conductive carbon black (Super P) and carbon nanotube conductive material (SWCNT) (Super P : SWCNT = 9 : 1 by weight ratio). Separately, a binder was prepared by mixing CMC (sodium salt of carboxymethyl cellulose) and SBR (styrene-butadiene rubber) (CMC : SBR = 3 : 7 by weight ratio).

[0107] The cathode material, conductive material, and binder prepared above were mixed with a sinker (cathode material : conductive material : binder = 95.8 : 1 : 3.2, weight ratio) to obtain a cathode slurry.

[0108] The above cathode slurry was applied to a copper foil with a thickness of 18 μm and dried at 80°C for 1 hour. Then, it was rolled and heat-treated in a vacuum oven at 100°C for 12 hours, and then punched to 16 mmΦ to manufacture a cathode plate.

[0109] The anode was manufactured by mixing the anode material NCM622, conductive carbon black (Super P), and PVDF in a weight ratio of 92:4:4 and punching the electrode plate to 14mmΦ.

[0110] A coin full cell (CR2032) was manufactured using the above cathode and anode, and its electrochemical characteristics were verified. The charge / discharge conditions for the initial 1-2 cycles (cycle formation) were set with a charge CC / CV of 4.25 V / 0.05 C, a discharge CC of 2.5 V, and a rate limit of 0.1 C. Subsequently, for 100 cycles, charge and discharge were performed with only the rate limit changed to 0.5 C to measure the life characteristics.

[0111] The results of the lifespan evaluation of the above coin pool cell are shown in Figure 3 and Table 6.

[0112] Capacity Recovery Ratio (CRR, %) (@ 100 cycles) Comparative Example 187 Comparative Example 490 Example 198

[0113] In the case of 650°C C-CVD (Example 1), the lifetime characteristics were effectively improved, which was confirmed to be due to the annealing effect and the role of another surface coating layer (a coating layer containing carbon). Due to this carbon-containing coating layer, it was confirmed that Example 1 showed an increased lifetime improvement effect compared to the REF sample (Comparative Example 1) and the sample that underwent only heat treatment (Comparative Example 4). This can be interpreted as the low-temperature CVD coating technology of the present invention effectively contributing to the improvement of the lifetime characteristics of the cathode active material.

[0114] Although an embodiment of the present invention has been described above, this specification is not necessarily limited to such embodiment. Those skilled in the art may modify and change the present invention in various ways by adding, changing, deleting, or adding components, etc., without departing from the spirit of the invention as described in the claims, and such modifications and changes are also to be included within the scope of the rights of the present invention.

Claims

1. A method for manufacturing a silicon-carbon composite, (S1) A step of introducing a core containing silicon particles into a Chemical Vapor Deposition (CVD) reactor; (S2) A step of supplying a mixed gas containing a carbon source gas into the above CVD reactor; (S3) A step of chemically vaporizing a coating layer containing carbon on the surface of the core by reacting the core containing the silicon particles and a carbon source gas at a temperature condition greater than 600℃ and less than 700℃; and (S4) A step of precipitating the product of step (S3) as a solid to obtain a silicon-carbon composite; comprising Method for manufacturing a silicon-carbon composite.

2. In Paragraph 1, The above (S1) and / or (S2) steps are performed under an inert gas atmosphere, Method for manufacturing a silicon-carbon composite.

3. In Paragraph 2, The above inert gas is one or more selected from the group consisting of argon gas, helium gas, and nitrogen gas, Method for manufacturing a silicon-carbon composite.

4. In Paragraph 1, The mixed gas containing the carbon source gas comprises a carbon source gas and an inert gas, wherein the flow rate ratio of the carbon source gas and the inert gas is carbon source gas : inert gas = 1:3 to 1:

30. Method for manufacturing a silicon-carbon composite.

5. In Paragraph 1, The above carbon source gas is one or more selected from the group consisting of acetylene (C2H2), ethylene, propylene, methane, ethane, and propane, Method for manufacturing a silicon-carbon composite.

6. In Paragraph 1, A method for manufacturing a silicon-carbon composite, wherein the thickness of the coating layer containing the carbon is 10 to 30 nm.

7. In Paragraph 1, The reaction time in the above step (S3) is 3 to 6 hours, Method for manufacturing a silicon-carbon composite.

8. A silicon-carbon composite manufactured according to a method for manufacturing a silicon-carbon composite according to any one of claims 1 to 7.

9. In Paragraph 8, The silicon grain size measured by X-ray diffraction (XRD) analysis within the above silicon-carbon composite is 10 nm or less, Silicon-carbon composite.

10. A negative electrode active material comprising a silicon-carbon composite according to claim 8.

11. A secondary battery comprising a negative electrode active material according to paragraph 10.