Novel lactate-substituted hydroxyapatite compound and preparation method therefor

The synthesis of lactate-substituted hydroxyapatite addresses the limitation of organic anion integration in apatite materials, enhancing biocompatibility and functionality, enabling applications in UV blocking, flame retardancy, and multiphase formulations.

WO2026240452A1PCT designated stage Publication Date: 2026-11-19METIMEDI PHARMA CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2026/006089
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2026-05-11
Filing Date
2026-05-14
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Existing apatite materials lack the integration of organic anions, limiting their applications and properties, particularly in terms of biocompatibility and functional capabilities.

Method used

A method is developed to synthesize lactate-substituted hydroxyapatite by reacting calcium organic compounds, phosphate salt compounds, and carbonate salt compounds in a liquid phase, forming a compound with the formula Ca₁₀(PO₄)₆(OH)₂-X(C₃H₅O₃)ₓ, where x is an integer, which introduces organic anions into the apatite structure.

Benefits of technology

The resulting lactate-substituted hydroxyapatite exhibits enhanced biocompatibility and functional properties, including UV blocking, flame retardancy, and stability in both aqueous and oil phases, making it suitable for various applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2026006089_19112026_PF_FP_ABST
    Figure KR2026006089_19112026_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to: a method for preparing a lactate-substituted hydroxyapatite compound, comprising a step of reacting an organic calcium compound, a phosphate compound and a carbonate compound in a liquid phase; an anion-substituted hydroxyapatite compound prepared using the preparation method; and uses of the compound for cosmetics, paints and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Novel lactate-substituted hydroxyapatate compound and method for preparing the same

[0001] The present invention relates to a novel lactate-substituted hydroxyapatate compound and a method for preparing the same.

[0002] Apatite is a substance that exists in nature in various structures and forms. Fundamentally, apatite is one of the phosphate minerals with the chemical formula Ca5(PO4)3(F, Cl, OH). Depending on the composition, OH - In many cases, hydroxyapatite, Cl - In many cases, Chlorapatite, F - In many cases, it is named Fluorapatite. Basic apatite has a specific gravity of 3.0 or higher and a hexagonal crystal structure. Apatite is one of the minerals utilized by living organisms and has the advantage of excellent biocompatibility.

[0003] [Prior Art]

[0004] Republic of Korea Patent Publication No. 1020110010910

[0005] The present invention was conceived in response to the above necessity, and the objective of the present invention is to provide a novel apatite material.

[0006] Another objective of the present invention is to provide a method for manufacturing the novel Apatite material.

[0007] To achieve the above objective, the present invention provides a method for preparing a lactate-substituted hydroxyapatite compound comprising the step of reacting a calcium organic compound, a phosphate salt compound, and a carbonate salt compound in a liquid phase.

[0008] In one embodiment of the present invention, the calcium organic compound is preferably calcium lactate, the phosphate salt compound is sodium phosphate monobasic, and the carbonate salt compound is sodium bicarbonate, but is not limited thereto.

[0009] In another embodiment of the present invention, the reaction is preferably carried out within a pH range of 6.8 to 8.0, and the reaction is preferably carried out within a pH range of 6.8 to 7.4.

[0010] The above reaction is preferably carried out within a pH range of 7.2 to 7.8, but is not limited thereto.

[0011] In another embodiment of the present invention, the reaction is preferably a spontaneous endothermic reaction, but is not limited thereto.

[0012] In addition, the present invention provides a lactate-substituted hydroxyapatate compound produced by the manufacturing method of the present invention.

[0013] In one embodiment of the present invention, the chemical formula of the compound is Ca 10 (PO4)6(OH) 2-X (C3H5O3) X With the structural formula, where x is preferably an integer but is not limited thereto.

[0014] In addition, the present invention is Ca 10 (PO4)6(OH) 2-X (An - ) X With the structural formula of where x is an integer, and An - It provides a compound meaning an organic anion integrated into the HA grid.

[0015] The present invention provides a composition comprising the compound of the present invention.

[0016] In one embodiment of the present invention, the composition is preferably, but not limited to, a cosmetic composition, a paint composition, a paper composition, or an additive composition for automobiles, ships, electronics, construction, or household goods.

[0017] Regarding the use of the composition of the compound of the present invention, it is well described in the specifications of International Patent Application No. PCT / KR2026 / 005263 and Korean Patent Application No. 10-2025-0050948, which are patents among the applicant's previously filed patents regarding the substantial use of the compound of the present invention, and in particular regarding its use in cosmetics, etc., it is cited here.

[0018] In the embodiments of the compound of the present invention in this application specification, the dispersion effect, etc. of the compound of the present invention is described.

[0019] The composition of the present invention utilizes plate-shaped particles to have an absorption or reflection effect of wavelengths in the ultraviolet region, thereby acting as an electromagnetic wave blocking / blocking booster (UV filter / booster), and

[0020] It has a flame-retardant effect that delays or extinguishes fire by forming charcoal, and by absorbing the measurement spectrum and converting it into thermal energy to induce a phase change of the solvent at a very rapid rate, it can be used in UV-blocking cosmetics, UV-blocking boosters, flame-retardant water-based or oil-based paints, photodegradation inhibitors, flame-retardant urethanes, heating hot water additives, fire retardants, high-efficiency cogeneration additives, high-altitude food additives, UV-blocking paper, flame-retardant paper, interior wallpaper, and archival paper.

[0021] The present invention will be described below.

[0022] The present invention relates to a novel substance, Lactate-substituted hydroxyapatite (hereinafter LSH), which is a type of apatite formed by the combination of calcium and phosphate.

[0023] The present invention introduces the characteristics and synthesis method of lactate-substituted hydroxyapatite produced by substituting a negative charge with lactate.

[0024] As can be seen from the present invention, the present invention has identified a method for preparing a lactate-substituted hydroxyapatite compound comprising the step of reacting a calcium organic compound, a phosphate salt compound, and a carbonate salt compound in a liquid phase, the conditions of the method, and the characteristics of the compound prepared by the method.

[0025] Figure 1 is a figure showing the equilibrium of each phosphate ion,

[0026] Photographs in Fig. 2 show the liquid state, after drying at room temperature, and a micrograph of lactate-substituted hydroxyapatite magnified 100 times.

[0027] FIG. 3 is an SEM image of the lactate-substituted hydroxyapatite of the present invention (top photo), and the middle and bottom photos are SEM images of 50 nm hydroxyapatite and 3000 nm hydroxyapatite, respectively.

[0028] FIG. 4 is a graph confirming the binding characteristics of functional groups via FT-IR, FIG. 4 is a graph of the lactate-substituted hydroxyapatite of the present invention, and FIG. 5 and 6 are graphs of 50 nm hydroxyapatite and 3000 nm hydroxyapatite, respectively.

[0029] Figure 7 shows the concentration (turbidity) of lactate-substituted hydroxyapatite, Figure 8 shows the Z-average (average diameter) of lactate-substituted hydroxyapatite, Figure 9 shows the intensity size (major particle size) of lactate-substituted hydroxyapatite, and Figure 10 shows the Zeta-potential (surface charge) of lactate-substituted hydroxyapatite.

[0030] FIG. 11 is a figure showing the characteristics of a compound of the present invention (hereinafter referred to as 'MEDI-25' in the figure) applicable to both aqueous and oil phase formulations.

[0031] It can be stably dispersed in both the water phase and the oil phase, and superior oil adsorption characteristics compared to HA were confirmed, and it can be seen that it contributes to suppressing phase separation and maintaining viscosity.

[0032] Figure 12 shows the realization of a 20 wt% water dispersion of 10 CI-listed metal oxides, and

[0033] Figure 13 shows the analysis of the aggregated structure of metal oxides based on MEDI-25 (SEM).

[0034] Figures 14 to 16 show the EDS elemental distributions of Red Iron Oxide-MEDI-25, Yellow Iron Oxide-MEDI-25, and Brown Iron Oxide-MEDI-25, respectively.

[0035]

[0036] The present invention will be further explained below through non-limiting embodiments. However, the following embodiments are described for the purpose of illustrating the present invention, and the scope of the present invention shall not be interpreted as being limited by the following embodiments.

[0037] Example 1. Reaction-participating substances

[0038] The basic composition of apatite consists of calcium and phosphate. Therefore, sources of calcium and phosphate are required, and additionally, a buffer substance is needed to support chemical equilibrium. A total of three compounds are used in the reaction, and the characteristics of each compound are explained in the subsections.

[0039] 1.1. Calcium

[0040] Calcium is an alkaline earth metal element belonging to Group 2 of the periodic table. Its atomic weight is 40, and as a positively charged metal ion, it forms ionic bonds with negatively charged elements. Additionally, calcium can enhance its stability through coordinate bonding. A general characteristic of Group 1 and Group 2 alkali metals is that they react violently with water.

[0041] 1.1.1. Calcium Source

[0042] Calcium atoms exist as 2+ cations, lacking two electrons in their outermost shell. Therefore, according to the octet rule, two electrons are required for the calcium atom to be stabilized. Anionic molecules, elements, functional groups, or radicals that provide electrons can form ionic bonds with calcium. Due to this characteristic, a certain amount dissociates when dissolved in water. A representative compound is calcium chloride (CaCl2).

[0043] The novel substance synthesizes lactate-substituted hydroxyapatite by utilizing calcium lactate pentahydrate. Calcium lactate is calcium (Ca 2+ It has a structure in which one lactate (C3H5O3) group is attached to two lactate groups. Because it is biologically very stable, it can be used for food and is a substance used in various industrial fields.

[0044] 1.1.2. Organic Calcium and Inorganic Calcium

[0045] Calcium exists in various forms around us by forming ionic bonds with negative charges. When it combines with negatively charged organic substances, it is called organic calcium, and when it combines with negatively charged inorganic substances, it is called inorganic calcium.

[0046] Organic calcium compounds include aryl, allyl, and alkyl derivatives, metallocenes, amides, hydrides, and fluorides. Representative compounds include calcium lactate, calcium citrate, calcium gluconate, calcium acetate, calcium ascorbate, and calcium pyruvate.

[0047] Inorganic calcium exists in the form of calcium carbonate, calcium phosphate, calcium fluoride, calcium sulfate, and calcium chloride, and is primarily found in the form of bones or minerals.

[0048] 1.2. Phosphate

[0049] Phosphorus is a nitrogen group element belonging to Group 15 of the periodic table. Its atomic weight is 30.973, and isotopes can be synthesized artificially. Due to its high reactivity in nature, it is extremely rare to find it existing as pure phosphorus. Three allotropes exist (white phosphorus, red phosphorus, and black phosphorus), with white and red phosphorus being the most abundant. Phosphorus is present in phosphates and in the cells of all living organisms.

[0050] 1.2.1. Phosphate Source

[0051] Phosphorus atoms have five electrons in their outermost shell. To be stabilized, phosphorus atoms form covalent bonds with oxygen to become phosphoric acid, which has the chemical formula H3PO4. Phosphoric acid is a weak acid and a colorless solid crystal. The ion commonly referred to as phosphate is an orthophosphate derivative, PO4. 3- It is. Hydrogen is H2PO4 through acid-base equilibrium. - and HPO4 2- It produces [it]. Thanks to these characteristics, it exhibits high solubility in water and is used as a buffer solution.

[0052] The equilibrium of each ion is as shown in Fig. 1.

[0053] The new material synthesizes lactate-substituted hydroxyapatite using sodium phosphate monobasic. Sodium phosphate monobasic is sodium (Na + It has a structure in which ions and dihydrogen phosphate ions (H2PO4) are attached.

[0054] 1.2.2. The Role of Phosphate

[0055] Phosphoric acid combined with sodium is primarily used in precipitation experiments due to its high degree of ionization and reactivity. It forms ionic bonds not only with sodium but also with cationic metals such as magnesium and aluminum. Phosphorus and calcium form calcium hydrogen phosphate and hydroxyapatite. Except when combined with sodium, most compounds are poorly soluble in water and therefore precipitate in the form of solid crystals. Sodium phosphate monobasic forms the main framework of apatite together with the calcium of calcium lactate.

[0056] 1.3. Carbonate

[0057] Carbonate is a carbonate, CO3 2- It refers to a dissociated form. Carbonates are derived from carbonic acid, which has the chemical formula H2CO3. Carbonic acid is unstable and has a strong tendency to decompose into water and carbon dioxide. Although carbon dioxide dissolves well in water, physical degassing occurs when it encounters rough surfaces or porous objects. Such surfaces act as nuclei for bubble generation, rapidly removing carbon dioxide. Representative examples include sodium bicarbonate, produced by a 1:1 reaction between carbonic acid and sodium hydroxide, and sodium carbonate, produced by a 1:2 reaction; calcium carbonate is formed when carbonic acid reacts with calcium hydroxide.

[0058] 1.3.1. Role of Carbonate

[0059] Carbonates react with metal ions to form insoluble carbonate precipitates. They can also store carbon dioxide and release it upon contact with acid. Carbon capture is known as mineral carbonation and is viewed as a technology for addressing climate change. Due to these characteristics, they are primarily used in the environmental industry. Precipitates formed from carbonates are eco-friendly, and calcium carbonate is directly utilized or consumed by living organisms.

[0060] 1.3.2. pH Control of Carbonate

[0061] The most important characteristic of carbonates is their role as buffers in acid-base reactions. Like the second substance, phosphate, they act as buffers and exist in three chemical equilibrium states. The chemical equilibrium steps and pKa values ​​are shown in Table 1 below.

[0062] Step Chemical Formula Description Equilibrium Constant (at 25℃) 1 CO2 (g) ↔ CO2 (aq) Gaseous CO2 dissolves in water Henry's Law: kH ≈ 3.4 x 10⁻⁶ -2 mol / (L·atm)2CO2(aq) + H2O ↔ H2CO3 Conversion of CO2 to carbonic acid (slow reaction) Very small (almost in the state of CO₂) 3H2CO3 ↔ H + + HCO3 1st dissociation (weak acid) K a1 ≈ 4.3 x 10 -7 (pKa₁≒ 6.35)4HCO3 - ↔ H + + CO3 2- Secondary dissociation (weaker acid) K a2 ≈ 5.6 x 10 -11 (pKa₂≒ 10.33)

[0063] In typical aqueous solutions, it exists mostly as CO2(aq), but its main form changes depending on the pH. It is H2CO3 when the pH is 6 or lower, and HCO3 when the pH is 6 to 10. - , CO3 when pH is 10 or higher 2- is dominant.

[0064] Sodium bicarbonate is used in this reaction. Sodium bicarbonate adjusts the pH and converts apatite into hydroxyapatite by donating OH- to it.

[0065] Example 2. Chemical reaction equation and chemical formula of the product

[0066] The products of the three substances are small particles ranging in size from nano to micro. It is a very rapid chemical reaction, and the particles precipitate after formation. These particles fundamentally possess apatite characteristics; typically, hydroxyl substitution is referred to as hydroxyapatite. Phosphate can be substituted with one or more other anions. Due to these characteristics, one of the conditions describing apatite is the calcium / phosphate ratio. Generally, the Ca / P ratio is 1.66, and when the proportion of Ca is low, it is called calcium-deficient hydroxyapatite. Since this is not a fixed ratio, the Ca / P ratio varies depending on the synthesis method or the type of anion; known anions include hydroxyl groups, fluorine, and chloride. Furthermore, organic substances can also be substituted using the same principle.

[0067] 2.1. Nomenclature

[0068] The basic characteristic of the resulting compound is that it is apatite. The name given to apatite varies depending on the method of synthesis. Primary apatite is formed by attaching F, Cl, and OH to X in the general chemical formula Ca5(PO4)3(X) described in the overview. Primary apatite is as shown in Table 2 below.

[0069] Name Chemical Formula X Ionic Characteristics FluorapatiteCa5(PO4)3FF - Chlorapatite, the most stable and common form of tooth and bone component, Calcium 5(PO4)3Cl₂ -Rarely found in high-temperature environments Hydroxylapatite Cal5(PO4)3OHOH - Major components of living organism bones and teeth

[0070] Because ion substitution occurs relatively easily in the apatite structure, secondary apatites exist as shown in Table 3 below.

[0071] Name, Substitution Ion or Structural Change, Characteristics and Uses, Carbonate-apatite, Some PO4 3- -> CO3 2- Common in organism bones / teeth, biocompatible Strontium-apatite, some Ca 2+ -> Sr 2+ Formed in a geological environment, currently under radiation therapy research. Manganese-apatite, some Ca 2+ -> Mn 2+ Reported in rare, geological environments Lead-apatite Partially or entirely Ca 2+ -> Pb 2+ Lead-containing, structural similarity to compounds related to the LK-99 controversy: Cadmium-apatite, some Ca 2+ -> Cd 2+ Used in research on environmental purification adsorbents. Rare-earth-apatite some Ca 2+ -> Rare Earth Ions (RE 3+ Etc. Important as a raw ore for rare earth resources.

[0072] Apatite synthesized in vivo or used for medical purposes is as shown in Table 4 below.

[0073] Name, Characteristics, and Description: Carbonate-hydroxyapatite, found in actual bones / teeth, OH - and PO4 3- partially CO3 2- Synthetic Bioapatite replacement artificial bone, used as implant material, high biocompatibility

[0074] Finally, minerals of the apatite series with similar structures exist as shown in Table 5.

[0075] Name Chemical Formula Main Substitution Ion Description Mimetite Pb5(AsO4)3CIAsO4 3- , Pb 2+ Lead-arsenic apatite-like mineral Pyromorphite Pb5(PO4)3CIPb 2+ Lead-containing phosphate mineral Vanadinite (Pb5(VO4)3CIVO4) 3- , Pb 2+ Rare mineral resources including vanadium

[0076] As shown above, apatite exists in various forms, and these are the forms known to date. Most apatite series either substitute cations or do not have organic matter in the anion. On the other hand, the new material substitutes an organic matter in the anion.

[0077] The substance produced by this method is named [Organic-substituted hydroxyapatite]. For example, apatite produced using calcium lactate is named [Lactate-substituted hydroxyapatite].

[0078] 2.2. Aqueous de novosynthesis: KSC method

[0079] The process of generating organic-substituted hydroxyapatite using calcium organic compounds is a new type of synthesis method known as de novosynthesis. Experimental results show that ionizable calcium organic compounds produce apatite-series particles when they come into contact with phosphate compounds and carbonate compounds. Therefore, all reactions in this synthesis process that produce apatite by reacting calcium organic compounds, phosphate compounds, and carbonate compounds in the liquid phase are named the [KSC method].

[0080] 2.3. Equilibrium of Phosphate and Carbonate

[0081] The concept of chemical equilibrium, which refers to a state where the forward and reverse reaction rates are equal, appears in sections 1.2.1 and 1.3.2 of the preceding section. Depending on the chemical properties of phosphate and carbonate, chemical equilibrium is achieved according to pH when in an ionized state. A characteristic of organic-substituted hydroxyapatite is that apatite is formed differently depending on which phosphate and hydroxy groups are attached to calcium under a specific equilibrium state. According to experimental results, the formation rate of organic-substituted hydroxyapatite is very slow under low pH conditions (approximately pH 7 or lower); when exposed to air, CO2 in the air dissolves in water and shifts to a basic state, slowly forming organic-substituted hydroxyapatite.

[0082] The novel substance utilizes sodium phosphate monobasic and sodium bicarbonate. Although the pH varies depending on the concentration and mixing ratio of the two substances, it generally results in a buffer solution with a pH between 6.8 and 7.4. When mixed in a 1:1 ratio based on 0.1M, a pH of approximately 7.0–7.2 is formed; a higher proportion of sodium phosphate monobasic lowers the pH, while a higher proportion of sodium bicarbonate raises the pH. When the novel substance is produced, the size and shape of the organic-substituted hydroxyapatite differ depending on the pH.

[0083] 2.4. Process of Carbonic Acid and Carbon Dioxide Formation

[0084] When sodium phosphate monobasic and sodium bicarbonate are dissolved in excess in an aqueous solution, a small amount of CO2 gas is generated. Additionally, it was confirmed that an excess amount of CO2 is produced when calcium lactate is added. This phenomenon occurs when CO2, which is dissociated in the aqueous solution after the reaction, encounters the irregular surface of organic-substituted hydroxyapatite, resulting in degassing or the physical nucleation of CO2.

[0085] When organic-substituted hydroxyapatite is formed, the hydroxyl group is taken from the bicarbonate, and H2CO3 is converted to CO2(aq). CO2(aq) is degassed and undergoes a phase change to CO2(g) and is released into the air.

[0086] 2.5. Thermodynamic Reactions

[0087] General spontaneous precipitation reactions are exothermic. Thermodynamically, spontaneous precipitation occurs when the change in Gibbs free energy (△G) is negative. In the free energy formula △G = △HT△S, energy is generally released when ions combine to form a crystal structure, so △H < ​​0. Since precipitation is a process in which the disorder of the solution decreases, △S generally has a value of < 0. Furthermore, at a specific temperature, a precipitate forms if the ion product (Q) is greater than the solubility product (Ksp), while all ions exist in a dissolved state if the ion product is smaller than the solubility product.

[0088] However, the KSC method is a spontaneous endothermic reaction. The case in which a solid is formed by the spontaneous endothermic reaction of ions is as follows. In the free energy formula, △G = △HT△S, since it is an endothermic reaction, △H is positive. Because △G must be negative, a high temperature or a very large change in entropy at -T△S is required.

[0089] The KSC method is a reaction performed at room temperature, in which entropy decreases due to precipitation formation. In this specific case, the entropy of the entire system increases when hydrated ions are separated and water molecules become free in a complex reaction accompanied by dissolution, while gas release into the air occurs simultaneously. Consequently, the condition T△S > △H is established, allowing for the formation of organic-substituted hydroxyapatite.

[0090] 2.6. Chemical formula of organic-substituted hydroxyapatite

[0091] Organic-substituted hydroxyapatite is basically [Ca 10 (PO4)6(OH) 2-X (An - ) X It has a ] structure, and the number of phosphate groups can be adjusted according to the synthesis conditions of the KSC method. Accordingly, it can be a carbonate, hydrate, or (An - ) can be added or removed.

[0092] 2.6.1. Substitution of the Hydroxyl Group of Apatite with Lactate

[0093] Organic-substituted hydroxyapatite is formed according to the principle described above. Specifically, lactate-substituted hydroxyapatite was produced using calcium lactate, sodium phosphate monobasic, and sodium bicarbonate. The chemical formula of the product is Ca 10 (PO4)6(OH) 2-X (C3H5O3) X It has the structural formula. In the following text, Lactate-substituted hydroxyapatite is referred to by the abbreviation LSH, and the characteristics and applications of LSH are described.

[0094] Example 3. Verification of LSH through Analytical Chemistry

[0095] The micromorphology of lactate-substituted hydroxyapatite was examined, and analytical chemistry techniques were used to confirm that it belongs to the apatite family. When generated in a liquid phase, lactate-substituted hydroxyapatite takes the form of white nano to micro-scale particles and sinks because it is heavier than water. When water is dried to crystallize it, it forms hard white crystals. For comparison with general hydroxyapatite, Hydroxyapatite Nanopowder / Nanoparticles 50 nm (NG10SM0104) and Hydroxyapatite Micron powder 3000 nm (NG04EO072386), purchased from nanografi, were compared.

[0096] Lactate-substituted hydroxyapatite was prepared by dissolving 160 mg / 10 ml of sodium phosphate monobasic, 400 mg / 10 ml of sodium bicarbonate, and 616.58 mg / ml of calcium lactate in water in that order. Sodium phosphate monobasic and sodium bicarbonate are highly soluble in water and exist as clear aqueous solutions. When calcium lactate is added to the aqueous solution containing dissolved sodium phosphate monobasic and sodium bicarbonate, an endothermic reaction occurs immediately, producing lactate-substituted hydroxyapatite along with CO2 generation.

[0097] 3.1. Photograph of the actual product

[0098] Lactate-substituted hydroxyapatite produces an opaque solution. Figure 2 shows the liquid state, after drying at room temperature, and a micrograph of the lactate-substituted hydroxyapatite magnified 100 times.

[0099] As can be seen in Figure 2, when Lactate-substituted hydroxyapatite dispersed in water is dried, the surface is completely covered with white crystals, and when viewed under a microscope, it is filled with Lactate-substituted hydroxyapatite without any gaps.

[0100] 3.2. Product Analysis via SEM-EDS

[0101] SEM-EDS was performed to confirm the unique phenomenon of lactate-substituted hydroxyapatite. The morphology of lactate-substituted hydroxyapatite was confirmed using a SEM microscope, and elemental analysis was confirmed using EDS (Fig. 3).

[0102] As can be seen in Figure 3, when magnified 300 times using SEM, a picture like the top left image is obtained. When the lactate-substituted hydroxyapatite is dried, it appears as a plate covering the bottom, filling it completely without gaps. When magnified up to 5000 times, it showed the appearance as the top right image, with granules protruding from the plate.

[0103] Generally, hydroxyapatite has a sand-like appearance at a size of 50 nm, as shown in the middle photo, and hydroxyapatite at a size of 3000 nm has a spherical shape, as shown in the bottom photo.

[0104] When elemental analysis was performed on lactate-substituted hydroxyapatite, the results shown in Table 6 below were obtained.

[0105] Spectrum 3ElementSignalTypeLineApparentConcentrationK RatioWt%Wt%SigmaAtomic%StandardNameFactoryStandardStandardizationDaterCEDSKseries15.090.1508621.520.3033.16C VitYesOEDSKSeries71.010.2389734.820.2540.29SiO2YesNaEDSKseries60.440.2550719.870.1516.00AIbiteYesPEDSKseries23.290.13026 6.620.093.96GaPYesCaEDSKseries33.260.2971713.520.136.24WollastoniteYesPtEDSMseries6.430.064343.640.260.35PtYesTotal100100

[0106] 3.3. Analysis of Functional Groups via FT-IR

[0107] After elemental analysis, functional groups and bonding characteristics were confirmed through FT-IR. As a result of the IR analysis, a graph as shown in Figure 4 was obtained.

[0108] As can be seen in Fig. 4, the graph of lactate-substituted hydroxyapatite was more complex than that of single hydroxyapatite. Hydroxyapatite has a unique fingerprint region pattern, and peaks with the same pattern were observed in lactate-substituted hydroxyapatite as well. The parts other than the hydroxyapatite peak appear to be lactate. The results of the IR spectrum analysis are shown in Table 7 below.

[0109] WavenumberIntensityType of bond3305.1Strong, very broadO-H2982.22,2939.07MediumC-HC=O2208.03WeakP=O(Inorgainc)1918.96WeakCaCO3(Reference)1578.51-1268.05Strong, mediumC-OC=O1117.72-559.89Strong, mediumApatite

[0110] As can be seen from the table above, the analysis results showed that in the IR spectrum graph, lactate functional groups appeared in the basic apatite structure of lactate-substituted hydroxyapatite.

[0111] Example 4. LSH Synthesis Conditions

[0112] Organic-substituted hydroxyapatite takes on various forms depending not only on anion substitution conditions but also on synthesis conditions. Since it is not possible to define all variables in this article, three representative factors that influence the shape and structure of the particles are introduced.

[0113] 4.1. Differences in product according to pH conditions (pH 7.4, pH 8)

[0114] In the preparation of organic-substituted hydroxyapatite, dissolving sodium phosphate monobasic and sodium bicarbonate in water results in a pH value between 7.3 and 7.5. If the pH decreases to become acidic, particles do not form due to the equilibrium state. Conversely, if the pH increases to become basic, the particle size increases and the crystal structure of the product changes. Generally, particles formed between pH 7.2 and 7.8 undergo nucleation through heterogeneous nucleation, which allows them to adhere well to surfaces such as the bottom. Conversely, if the pH rises to approximately 8 or higher, nucleation occurs through homogeneous nucleation. The size of the resulting particles is smaller and more uniform when formed between pH 7.2 and 7.8 compared to when formed at pH 8 or higher.

[0115] Example 5. Characteristics of LSH

[0116] Organic-substituted hydroxyapatite produced by the KSC method exhibits different physicochemical properties depending on the specific substance. A brief introduction to the properties of lactate-substituted hydroxyapatite, which was used in the experiment, is provided below.

[0117] 5.1. Visual / Tactile / Gastronomic Characteristics of LSH

[0118] Lactate-substituted hydroxyapatite is formed immediately in solution upon contact with sodium phosphate, sodium bicarbonate, and calcium lactate. It turns the solution opaque white, and if left at rest for a long period, the lactate-substituted hydroxyapatite precipitates. When the liquid dries, it takes on a white crystalline form and adheres to surfaces, coating them like a thin film.

[0119] In solution, the texture is almost identical to water, and it does not feel rough due to the small particle size. In the solid state, lactate-substituted hydroxyapatite resembles chalk and is not rough. In the solid state, it has a slightly sour and salty taste.

[0120] 5.2. Physical Properties of LSH (Size and z-potential in liquid state)

[0121] Dynamic Light Scattering (DLS) was used to measure the approximate size and surface charge of lactate-substituted hydroxyapatite. The reaction is very fast when lactate-substituted hydroxyapatite is prepared at concentrations of 160 mg / 10 ml of sodium phosphate monobasic, 400 mg / 10 ml of sodium bicarbonate, and 616.58 mg / ml of calcium lactate. By adjusting the concentrations, DLS measurements were performed at 8 mg / 10 ml of sodium phosphate monobasic, 20 mg / 10 ml of sodium bicarbonate, and 7.7 mg / ml of calcium lactate.

[0122] As can be seen in Figures 7 to 10, the experimental results show that the solution becomes opaque within 10 minutes depending on the concentration of calcium lactate. The reaction appears to conclude within 10 minutes. Within one hour, it grows into lactate-substituted hydroxyapatite with a size of 3000 nm and grows to a size of 4000–6000 nm at a slow rate. The surface charge of the lactate-substituted hydroxyapatite is negative, and the surface charge tended to decrease as the size increased.

[0123] Example 6: MEDI-25 is a multiphase adaptable material applicable to both aqueous and oil-phase formulations

[0124] FIG. 11 is a figure showing the characteristics of the compound of the present invention (described as 'MEDI-25' in the figure) applicable to both aqueous and oil phase formulations,

[0125] It can be stably dispersed in both the water phase and the oil phase, and superior oil adsorption characteristics compared to HA were confirmed, and it can be seen that it contributes to suppressing phase separation and maintaining viscosity.

[0126] The characteristics of the compound of the present invention are due to its porous structure, which provides an oil porosity effect on the surface and internal microspaces, and is attributed to a structural stabilization effect within the oil phase.

[0127] Example 7: Acting as a highly stable metal oxide dispersant

[0128] This embodiment is an example demonstrating that the compound (MEDI-25) of the present invention can serve as a stable metal oxide transport platform based on an inorganic nanostructure.

[0129] A 20 wt% water dispersion of the 10 CI-listed metal oxides listed in Table 8 below was produced.

[0130] As can be seen in Figure 12, it was possible to maintain a uniform color even in the solid state, enable reversible conversion between powder and dispersion, and confirm redispersion characteristics without structural collapse.

[0131] In addition, through the figures in Figures 13 to 16, it was possible to confirm the uniform coexistence of the Fe-rich core and the Ca-P network.

[0132] No. Color Product Name Compound Name CI #INCI Name Chemical Formula 1 Red Red Iron Oxide Iron(III) oxide, red iron oxide 77491 Ferric oxide e2O2 2 Brown Brown Iron Oxide Red iron oxide, yellow iron oxide, black iron oxide 77491 77492 77499 Ferric oxide, Hydrated ferric oxide or Iron oxide monohydrate or Ferrous-Ferric oxide Fe2O3 or Fe2O3·H2O or FeO(OH)·nH2O or Fe3O4 3 Yellow Yellow Iron Oxide Iron(III) oxide hydrate, yellow iron oxide 77492 Hydrated ferric oxide or Iron oxide monohydrate Fe2O3·H2O or FeO(OH)·nH2O 4 Green Chromium Green Oxide Chromium(III) oxide 77288 Chromium oxide green Cr2O3 5 Blue Ultramarine Blue Green Oxide (Pigment Blue 29) Complex sodium aluminum sulfosilicate 77007 Ultramarines Na 6·8 Al6Si6O 24 S 2·4 6 Ultramarine Violet Complex Sodium Aluminum Sulfosilicate 77007 UltramarinesH x Na 4~6 Al6Si6O 24 S27 Purple Manganese Violet (Pigment Violet 16) Ammonium Manganese(III) Pyrophosphate 77742 Manganese Violet NH4MnP2O78 Black Iron Oxide Iron(II, III), Black Iron Oxide 77499 Ferrous-Ferric Oxide Fe3O49 White Titanium Oxide Titanium Dioxide 77891 Titanium Dioxide TiO210 White Zinc Oxide Zinc Oxide 77947 Zinc oxide ZnO

Claims

1. A method for preparing a lactate-substituted hydroxyapatite compound comprising the step of reacting a calcium organic compound, a phosphate salt compound, and a carbonate salt compound in a liquid phase.

2. A method for preparing a lactate-substituted hydroxyapatate compound according to claim 1, wherein the calcium organic compound is calcium lactate, the phosphate salt compound is sodium phosphate monobasic, and the carbonate salt compound is sodium bicarbonate.

3. A method for preparing a lactate-substituted hydroxyapatate compound according to claim 1, characterized in that the reaction is performed within a pH range of 6.8 to 8.

0.

4. A method for preparing a lactate-substituted hydroxyapatate compound according to claim 1, characterized in that the reaction is performed within a pH range of 6.8 to 7.

4.

5. A method for preparing a lactate-substituted hydroxyapatate compound according to claim 1, characterized in that the reaction is performed within a pH range of 7.2 to 7.

8.

6. A method for preparing a lactate-substituted hydroxyapatate compound according to claim 1, characterized in that the reaction is a spontaneous endothermic reaction.

7. A lactate-substituted hydroxyapatate compound prepared by the method of any one of claims 1 to 6.

8. In claim 7, the chemical formula of the above compound is Ca 10 (PO4)6(OH) 2-X (C3H5O3) X A compound characterized by having the structural formula where x is an integer. 9.Ca 10 (PO4)6(OH) 2-X (An - ) X It has the structural formula of, where x is an integer and An - is a compound meaning an organic anion integrated into the HA grid.

10. A composition comprising the compound of claim 7 or 9.