Ceramic substrate unit and manufacturing method of ceramic substrate unit

The ceramic substrate unit with directly bonded cooling fins addresses thermal and manufacturing issues in power modules by enhancing heat dissipation and reducing weight, ensuring reliable and efficient operation in high-power environments.

WO2026240500A1PCT designated stage Publication Date: 2026-11-19AMOGREENTECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2026/096068
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-15
Filing Date
2026-04-20
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Conventional heat dissipation structures in power modules for electric vehicles and industrial inverters suffer from increased thermal resistance, complexity, weight, and reliability issues due to intermediate layers and differences in thermal expansion, leading to performance degradation and manufacturing challenges.

Method used

A ceramic substrate unit with cooling fins directly bonded to the lower surface of a ceramic substrate, using Ag-Cu alloy brazing or sintering, eliminates intermediate layers, shortens heat conduction paths, and maintains bonding reliability, thereby enhancing heat dissipation and reducing weight and manufacturing complexity.

Benefits of technology

The solution improves heat dissipation efficiency, reduces module thickness and weight, and ensures stable operation under high-power conditions, minimizing thermal stress and delamination, while lowering manufacturing costs and meeting miniaturization demands.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2026096068_19112026_PF_FP_ABST
    Figure KR2026096068_19112026_PF_FP_ABST
Patent Text Reader

Abstract

Provided are a ceramic substrate unit and a manufacturing method of said ceramic substrate unit. The ceramic substrate unit according to the present invention is for a power module and comprises: a ceramic substrate; an upper metal layer formed on the upper surface of the ceramic substrate and formed such that a substrate-mounting component can be mounted thereon; a flat bottom metal layer formed on the bottom surface of the ceramic substrate; and cooling pins directly bonded to the bottom surface of the bottom metal layer, wherein the plurality of cooling pins are independently formed without being connected to one another and are bonded to the bottom metal layer by brazing or sinter bonding.
Need to check novelty before this filing date? Find Prior Art

Description

Ceramic substrate unit and method for manufacturing the ceramic substrate unit

[0001] The present invention relates to a ceramic substrate unit, and more particularly to a ceramic substrate unit capable of exhibiting improved heat dissipation performance in high current and high voltage environments and enabling miniaturization and weight reduction of the substrate unit, and a method for manufacturing the ceramic substrate unit.

[0002] Power modules applied to electric vehicles (EVs) and industrial inverters operate in high-voltage and high-current environments; accordingly, a highly reliable heat dissipation structure is essential to effectively release the high-temperature heat generated during device operation. To meet these requirements, a structure in which a heatsink made of a high thermal conductivity metal material is bonded to the underside of a ceramic substrate has conventionally been widely adopted.

[0003] However, such conventional heat dissipation structures entail the following technical problems.

[0004] First, heatsinks typically applied to power modules have a structure in which multiple cooling fins are integrally formed on a square-shaped base plate. Since an intermediate layer, such as the base plate, is interposed between the heatsink and the ceramic substrate constituting the power module, the heat conduction path becomes longer and thermal resistance increases. Consequently, insufficient heat dissipation is not achieved during high-output operation, which can lead to performance degradation and deterioration of power semiconductor devices.

[0005] Second, the square-shaped base plate acts as a factor that increases the overall thickness and weight of the power module, which poses a problem in that it fails to meet the trend of automotive power conversion systems requiring miniaturization and lightweighting. Additionally, the application of the base plate increases the complexity of the manufacturing process, leading to higher manufacturing costs and reduced mass producibility.

[0006] Third, reliability issues such as substrate bowing, thermal stress, and interfacial delamination are likely to occur due to the difference in the coefficient of thermal expansion (CTE) between the heat sink, which includes a square plate-shaped base plate, and the ceramic substrate. In particular, this can lead to a decrease in lifespan in a repetitive temperature cycle environment, and the heat dissipation efficiency may decrease as the distance between the heat source (power semiconductor device) and the coolant increases by the thickness of the base plate.

[0007] The matters described in the background technology above are intended to aid in understanding the background of the invention and may include matters that are not disclosed prior art.

[0008] The technical problem that the present invention aims to solve is to provide a ceramic substrate unit and a method for manufacturing the same, which simultaneously achieves miniaturization, weight reduction, process simplification, and cost reduction through a structure in which cooling fins are directly bonded to the lower part of a ceramic substrate, exhibits improved cooling performance, and ensures bonding reliability.

[0009] According to one aspect of the present invention as a means of solving the problem, a ceramic substrate unit for a power module comprises: a ceramic substrate; an upper metal layer formed on the upper surface of the ceramic substrate and configured to mount a component for mounting on the substrate; a flat lower metal layer formed on the lower surface of the ceramic substrate; and a plurality of cooling fins directly bonded to the lower surface of the lower metal layer, wherein the plurality of cooling fins are independently configured without being connected to one another and are bonded to the lower metal layer by a brazing or sintering bonding method.

[0010] In a ceramic substrate unit according to one aspect, a first brazing filler may be interposed between the upper metal layer and the ceramic substrate and between the lower metal layer and the ceramic substrate, and a second brazing filler may be interposed between the cooling fin and the lower metal layer.

[0011] In a ceramic substrate unit according to one aspect, the first brazing filler and the second brazing filler may be formed of an Ag-Cu alloy.

[0012] In a ceramic substrate unit according to one aspect, the second brazing filler may be composed of an Ag-Cu alloy having an Ag content higher than the Ag content of the first brazing filler.

[0013] In a ceramic substrate unit according to one aspect, a pretreatment plating layer may be further formed on the lower surface of the lower metal layer or on the surface of the bonding portion of the cooling fin. In this case, the pretreatment plating layer may be made of an Ag-Cu alloy.

[0014] In a ceramic substrate unit according to one aspect, the thickness of the pretreatment plating layer may be 0.3㎛ or more and 5.0㎛ or less.

[0015] In a ceramic substrate unit according to one aspect, a brazing filler for brazing joint between the pretreatment plating layer and the lower metal layer or between the pretreatment plating layer and the cooling fin may be disposed.

[0016] In a ceramic substrate unit according to one aspect, an Ag-based sintered bonding layer is formed between the cooling fin and the lower metal layer, and the sintered bonding layer may be configured to mediate direct sintered bonding between the lower metal layer and the cooling fin.

[0017] In a ceramic substrate unit according to one aspect, the sintered bonding layer may be formed from an Ag-Cu alloy paste containing Ag and Cu.

[0018] According to one aspect, the ceramic substrate unit is formed such that the plurality of cooling fins are not connected to each other but are independently bonded directly to the lower metal layer, thereby allowing a portion of the lower surface of the lower metal layer to be directly exposed to the cooling channel partitioned between adjacent cooling fins. As a result, the portion of the lower surface of the lower metal layer exposed to the cooling channel comes into direct contact with the refrigerant, thereby increasing the heat dissipation area and shortening the heat transfer path, which can improve overall heat dissipation efficiency.

[0019] In a ceramic substrate unit according to one aspect, the plurality of cooling fins may have the same shape and size.

[0020] According to another aspect of the present invention as a means of solving the problem, a method for manufacturing a ceramic substrate unit for a power module is provided, comprising the steps of forming an upper metal layer on the upper surface of a ceramic substrate, forming a lower metal layer on the lower surface of the ceramic substrate, and directly bonding a plurality of cooling fins to the lower surface of the lower metal layer, wherein the plurality of cooling fins are configured independently without being connected to one another.

[0021] A method for manufacturing a ceramic substrate unit according to another aspect may further include the step of seating the plurality of cooling fins on an alignment jig as a step prior to bonding the cooling fins to the lower surface of the lower metal layer.

[0022] In this case, in the step of directly bonding the plurality of cooling fins to the lower surface of the lower metal layer, the plurality of aligned cooling fins can be directly bonded to the lower surface of the lower metal layer at once using the alignment jig.

[0023] In the step of directly bonding the plurality of cooling pins to the lower surface of the lower metal layer in the method for manufacturing a ceramic substrate unit according to another aspect, the cooling pins may be directly bonded to the lower surface of the lower metal layer by brazing or sintering bonding.

[0024] In a method for manufacturing a ceramic substrate unit according to another aspect, in the step of forming the upper metal layer and the step of forming the lower metal layer, the upper metal layer and the lower metal layer are brazed and joined to the upper and lower surfaces of the ceramic substrate using a first brazing filler, and in the step of directly joining the plurality of cooling fins to the lower surface of the lower metal layer, the plurality of cooling fins can be directly brazed and joined to the lower surface of the lower metal layer using a second brazing filler.

[0025] In a method for manufacturing a ceramic substrate unit according to another aspect, the first brazing filler and the second brazing filler can be formed of an Ag-Cu alloy.

[0026] In this case, the second brazing filler may use an Ag-Cu alloy having an Ag content higher than the Ag content of the first brazing filler.

[0027] In a method for manufacturing a ceramic substrate unit according to another aspect, as a step prior to bonding a plurality of cooling fins to the lower surface of the lower metal layer, the method may further include the step of forming an Ag-Cu alloy plating layer comprising Ag and Cu on the lower surface of the lower metal layer or on the bonding surface of the cooling fins.

[0028] According to the present invention, a conventional base plate-based heat sink structure can be replaced by directly bonding cooling fins to the lower surface of a ceramic substrate. In this structure, since the intermediate layer constituting the base plate is removed, the heat conduction path is shortened and the thermal resistance is lowered, allowing heat from the power semiconductor device to be dissipated more effectively, thereby preventing device degradation and performance deterioration in high-power operating environments.

[0029] Furthermore, since the base plate is eliminated from the heatsink, the overall thickness and weight of the substrate are reduced, enabling the miniaturization and lightweighting of the power module to meet market demands. This is particularly advantageous for applications where lightweight design and space efficiency are critical, such as automotive power conversion systems. In addition, the simplification of components streamlines the manufacturing process and reduces overall manufacturing costs.

[0030] Furthermore, since the base plate is omitted, the present invention can minimize problems such as substrate warping, delamination, and thermal stress caused by the difference in the coefficient of thermal expansion (CTE) between the ceramic substrate and the cooling fins. In addition, since interfacial reliability is maintained even in environments with repeated temperature changes, the degradation of the module's lifespan can be prevented even under long-term operating conditions. Therefore, stable operation is possible in high-power systems requiring high heat resistance and high reliability.

[0031] Furthermore, a structure that directly dissipates heat to the outside through cooling fins on the ceramic substrate minimizes the distance between the heat source and the cooling path, thereby improving the cooling response speed and shortening the time required to achieve thermal equilibrium in the module, which in turn enhances the energy efficiency of the entire system. Consequently, it is possible to provide high-performance ceramic substrate technology that is improved in structural, thermal, and process aspects.

[0032] FIG. 1 is a perspective view of a ceramic substrate unit according to an embodiment of the present invention.

[0033] FIG. 2 is an exploded perspective view showing the heat dissipation fins separated from a ceramic substrate unit according to an embodiment of the present invention.

[0034] FIG. 3 is a cross-sectional view of a ceramic substrate according to an embodiment of the present invention, viewed from the direction of line A-A' in FIG. 1.

[0035] FIG. 4 is an enlarged cross-sectional view of the main part of the present invention illustrating a modified example of a structure in which cooling fins are brazed to a lower metal layer.

[0036] FIG. 5 is an enlarged cross-sectional view of a key portion showing another preferred embodiment of a ceramic substrate according to an embodiment of the present invention.

[0037] FIG. 6 is a process flowchart for explaining a method for manufacturing a ceramic substrate according to an embodiment of the present invention.

[0038] Hereinafter, preferred embodiments of the present invention will be described in detail.

[0039] In describing the embodiments of the present invention, identical or similar components are assigned the same reference numerals, and redundant descriptions thereof are omitted. Furthermore, detailed descriptions of related prior art are omitted if it is determined that such detailed descriptions could obscure the essence of the embodiments disclosed in this specification.

[0040] In addition, the attached drawings are intended only to facilitate understanding of the embodiments disclosed in this specification, and the technical concept disclosed in this specification is not limited by the attached drawings, and it should be noted that they include all modifications, equivalents, and substitutions that fall within the concept and technical scope of the present invention.

[0041] The embodiments are provided to more fully explain the invention to those skilled in the art, and the following embodiments may be modified in various different forms, and the scope of the invention is not limited to the following embodiments. Rather, these embodiments are provided to make the disclosure more faithful and complete and to fully convey the spirit of the invention.

[0042] The terms used herein are for describing specific embodiments and are not intended to limit the invention. Additionally, the singular form in this specification may include the plural form unless the context clearly indicates otherwise.

[0043] In the description of the embodiments, where each layer (film), region, pattern, or structure is described as being formed "on" or "under" the substrate, each layer (film), region, pad, or pattern, "on" and "under" include both being formed "directly" and "indirectly" through another layer. In addition, the reference for the top or bottom of each layer is, in principle, based on the drawings.

[0044] The drawings are intended solely to facilitate an understanding of the concept of the present invention and should not be interpreted as limiting the scope of the invention. Additionally, relative thicknesses, lengths, or sizes in the drawings may be exaggerated for convenience and clarity of explanation.

[0045] FIG. 1 is a perspective view of a ceramic substrate unit according to an embodiment of the present invention, and FIG. 2 is an exploded perspective view showing a heat dissipation fin separated from a ceramic substrate unit according to an embodiment of the present invention. FIG. 3 is a cross-sectional view of a ceramic substrate according to an embodiment of the present invention viewed along the line A-A' of FIG. 1.

[0046] Referring to FIGS. 1 to 3, a ceramic substrate unit (10) according to an embodiment of the present invention comprises a ceramic substrate (100) and a plurality of cooling fins (150) directly bonded to the ceramic substrate (100). The ceramic substrate (100) may be configured such that an upper metal layer (120) and a lower metal layer (130) are formed respectively on the upper and lower surfaces of a ceramic substrate (110), and the plurality of cooling fins (150) may be directly bonded to the lower surface of the lower metal layer (130) by brazing or sintering.

[0047] In the embodiment, the ceramic substrate (110) may be composed of an oxide-based or nitride-based ceramic material having high thermal conductivity and excellent flexural strength. For example, the ceramic substrate (110) may be formed from any one of Al2O3, AlN, Si3N4, and ZTA (Zirconia Toughened Alumina). An upper metal layer (120) and a lower metal layer (130) may be formed by brazing metal foils on both sides of the ceramic substrate (110).

[0048] The upper metal layer (120) can be formed into a circuit pattern capable of electrical circuit connection of mounting components, such as power semiconductor devices or conductive spacers, through chemical or physical etching or mechanical processing. The lower metal layer (130) can be configured in a flat plate shape without a special pattern. These upper metal layer (120) and lower metal layer (130) can be made of one of Cu, Cu alloy (CuMo, etc.), or Al, which have excellent electrical and thermal conductivity (about 350 W / m·K).

[0049] For brazing, a brazing joint layer made of a metal material comprising at least one of Ag, AgCu, or AgCuTi may be used. The heat treatment temperature for brazing may be 780 degrees or higher and 900 degrees or lower. This is a temperature condition that can prevent deformation of the ceramic substrate and the metal layer or oxidation of the metal layer while ensuring stable bonding between the ceramic substrate and the metal layer.

[0050] The ceramic substrate (100) may be an Active Metal Brazing (AMB) substrate having a structure in which metal layers (120, 130) are bonded to the upper and lower surfaces of a ceramic substrate (110). The AMB substrate has the advantage of having excellent durability and heat dissipation performance, and can maintain stable electrical and mechanical properties even in high-temperature environments. In the following embodiments, the AMB substrate is described as a preferred example, but it is not limited thereto, and the ceramic substrate may be a Direct Bonding Copper (DBC) substrate, so it should be noted that this may also be included within the scope of the present invention.

[0051] Considering that the ceramic substrate (110) constituting the ceramic substrate (100) is applied to a power module operating in a high-temperature environment, the thickness of the ceramic substrate (100) is preferably at least 0.25 mm. In addition, the thickness of the upper metal layer (120) and the lower metal layer (130) bonded to the upper and lower surfaces of the ceramic substrate (110) is preferably at least 0.127 mm to efficiently dissipate heat from the power semiconductor device and to ensure a solid bond with the substrate.

[0052] The cooling fin (150) can be formed as an integral structure with the ceramic substrate by being directly bonded to one side of the lower metal layer (130) (the lower surface of the lower metal layer in the drawing) without a separate intermediate structure such as a base plate. The cooling fin (150) is intended to prevent overheating of the ceramic substrate through heat dissipation and can be formed from a material with high thermal conductivity. For example, one of Cu, Al, AlSiC, CuMo, CuW, Cu / CuMo / Cu, Cu / Mo / Cu, or a composite material thereof may be used.

[0053] The cooling fins (150) are composed of multiple fins and may be formed in a rectangular column shape as exemplified in the drawing (Fig. 2), as well as in a column shape with a circular or elliptical cross-sectional shape. Additionally, they may be formed in a column shape with a cross-sectional shape of a polygon greater than a triangle. The cooling fins (150) may be applied to an air-cooled or water-cooled environment. In the case of air cooling, it is an environment where air is supplied as a refrigerant, and in the case of water cooling, it is an environment where cooling water is circulated and supplied by a pump.

[0054] A plurality of cooling fins (150) can preferably be arranged such that they have the same shape and size and the spacing between adjacent cooling fins is constant. Accordingly, the flow uniformity of the refrigerant flowing along the cooling channel (not shown) partitioned between the cooling fins (150) is ensured, so that heat dissipation is not concentrated in a specific area but is evenly distributed over the entire area, thereby improving the overall heat dissipation performance.

[0055] In the embodiment, a plurality of cooling fins (150) are configured independently without being connected to each other and can be directly bonded to one surface of the lower metal layer (130). Accordingly, a portion of the lower surface of the lower metal layer (130) is directly exposed to the cooling channel partitioned between the cooling fins (150) and comes into direct contact with the refrigerant flowing along the cooling channel. As a result, the heat dissipation area is increased, and the heat transfer path is shortened, thereby improving the overall heat dissipation efficiency.

[0056] Here, it is clearly stated that the concept that a portion of the lower surface of the lower metal layer (130) is directly exposed to the cooling channel should be interpreted as including not only cases where a portion of the lower surface of the lower metal layer is directly exposed to the cooling channel without any intermediate structure (e.g., base plate) in the context, but also cases where a corrosion-preventing plating layer or coating layer is formed on the lower surface of the lower metal layer to prevent corrosion, or where a bonding layer is partially formed for bonding with cooling fins, and such plating layer, coating layer, or bonding layer is exposed to the cooling channel.

[0057] As previously mentioned, the cooling fin (150) can be directly joined to one side (the lower side in the drawing) of the lower metal layer (130) by brazing or sintering. Below, we will examine the configuration of the present invention in more detail by classifying it according to the joining method. Figure 3 above is a cross-sectional view illustrating a structure in which the cooling fin (150) is brazed to the lower metal layer (130). Referring to this, we will first examine an embodiment in which the cooling fin is brazed to the lower metal layer.

[0058] Referring to FIG. 3, a brazing filler (hereinafter referred to as the "first brazing filler") may be interposed between the upper metal layer (120) and the ceramic substrate (110) and between the lower metal layer (130) and the ceramic substrate (110) for brazing bonding between the ceramic substrate (110) and the metal layers. Additionally, a brazing filler (hereinafter referred to as the "second brazing filler") may be formed between the cooling fin (150) and the lower metal layer (130) for solid brazing bonding between them.

[0059] The first brazing filler (f1) and the second brazing filler (f2) can be formed by various known methods, such as the foil method, the plating method, and the paste application method (P-Filler method). The first brazing filler (f1) is placed between the ceramic substrate (110) and the upper and lower metal layers (120, 130), respectively, to mediate a strong thermal and mechanical bond between them. The second brazing filler (f2) mediates a strong thermal and mechanical bond between the lower metal layer (130) and the cooling fin (150).

[0060] In this embodiment, the first brazing filler (f1) and the second brazing filler (f2) may be composed of an Ag-based alloy containing silver (Ag). As a preferred example, the first brazing filler (f1) and the second brazing filler (f2) may be formed of an Ag-Cu alloy containing silver (Ag) and copper (Cu). Since the Ag-Cu alloy has a high level of thermal conductivity, it is suitable for high-temperature power modules. In addition, the Ag-Cu alloy has the advantage of securing bonding strength while preserving the structural properties of the ceramic substrate (110).

[0061] In particular, Ag has strong oxidation resistance, maintaining a stable state at high temperatures, and can contribute to maintaining stable bonding quality by suppressing oxide formation during the bonding process. Ag also has excellent wettability with metals or ceramics at specific brazing temperatures (generally 600 to 900 degrees), allowing it to spread uniformly across the bonding surface to form a solid bonding layer.

[0062] When the first brazing filler (f1) and the second brazing filler (f2) are formed of an Ag-Cu alloy, each filler (f1 and f2) may contain Ag in different amounts. Preferably, the second brazing filler (f2) may be composed of an Ag-Cu alloy with a higher Ag content than the first brazing filler (f1). In this case, the brazing bonding process between the cooling fin (150) and the lower metal layer (130) can be stably performed at a lower temperature than the brazing bonding process between the ceramic substrate (110) and the metal layer.

[0063] Generally, Ag alloys have the characteristic that the higher the Ag content, the lower the effective melting point. Therefore, considering this characteristic of the Ag alloy, if the Ag content of the second brazing filler (f2) is set high, the subsequent brazing process between the lower metal layer (130) and the cooling fin (150) through the second brazing filler (f2) can be performed at a relatively lower temperature than the brazing process between the ceramic substrate (110) and the metal layer through the first brazing filler (f1).

[0064] When the temperature of the subsequent brazing bonding process (brazing bonding process between the lower metal layer and the cooling fin) is lowered, the deformation caused by thermal expansion of the ceramic substrate (100) is reduced, thereby reducing thermal stress. In particular, remelting of the joint formed by the first brazing filler (f1) between the ceramic substrate (110) and the metal layers is prevented, thereby maintaining the structural stability of the bonding layer and reliably preventing the phenomenon of layer separation between the ceramic substrate (110) and the metal layers.

[0065] As a preferred example, the first brazing filler (f1) may be formed from an Ag-Cu alloy with an Ag-Cu composition ratio of 5:5, and the second brazing filler (f2) may be formed from an Ag-Cu alloy with an Ag-Cu composition ratio of 7:3. As another preferred example, the first brazing filler (f1) may be formed from an Ag-Cu alloy with an Ag-Cu composition ratio of 6:4, and the second brazing filler (f2) may be formed from an Ag-Cu alloy with an Ag-Cu composition ratio of 7:3.

[0066] When an Ag-Cu alloy with an Ag-Cu composition ratio of 5:5 is used as a brazing filler for primary brazing (bonding between a ceramic substrate (110) and a metal layer), brazing can be performed at approximately 890°C on the binary eutectic phase diagram of the Ag-Cu alloy. Additionally, in the case of an Ag-Cu alloy with an Ag-Cu composition ratio of 6:4, brazing can be performed at approximately 850°C.

[0067] On the other hand, an Ag-Cu alloy with an Ag-to-Cu ratio of 7:3 can be brazed at approximately 780°C. Therefore, if an Ag-Cu alloy with an Ag-to-Cu composition ratio of 7:3 is used as a brazing material for brazing between a lower metal layer (130) and a cooling fin (150), brazing can be performed at a temperature approximately 70°C to 110°C lower than the primary brazing process (bonding process between the ceramic substrate and the metal layers), thereby resolving the problems of remelting and layer separation in the primary brazing joint.

[0068] FIG. 4 is an enlarged cross-sectional view of the main part of the present invention illustrating a modified example of a structure in which cooling fins are brazed to a lower metal layer.

[0069] As illustrated in FIG. 4, a pretreatment plating layer (140) may be further formed on the lower surface of the lower metal layer (130). Although not illustrated, the pretreatment plating layer (140) may be formed on the joint surface of the cooling fin (150) (the upper surface of the cooling fin in the drawing). The pretreatment plating layer (140) may be composed of an Ag-Cu alloy containing Ag and Cu, as a pretreatment for inducing surface activation, improved wettability, and prevention of oxidation.

[0070] In this case, a brazing filler (second brazing filler) for brazing joint between the lower metal layer (130) and the cooling fin (150) may be placed between the pretreatment plating layer (140) and the cooling fin (150) (when the pretreatment plating layer is formed on the lower metal layer) or between the pretreatment plating layer (140) and the lower metal layer (130) (when the pretreatment plating layer is formed on the joint surface of the cooling fin), depending on the formation location of the pretreatment plating layer (140).

[0071] When a pretreatment plating layer (140) composed of an Ag-Cu alloy is additionally formed in this manner, the fusion and diffusion characteristics of the brazing filler formed of the Ag-Cu alloy are further improved, thereby enhancing the adhesion and durability of the brazing joint. In addition, the overall reliability of the joint can be further improved due to the oxidation prevention effect of the pretreatment plating layer (140) during the joining process.

[0072] FIG. 5 is an enlarged cross-sectional view of a key portion showing another preferred embodiment of a ceramic substrate according to an embodiment of the present invention, showing a structure in which cooling fins are bonded to a lower metal layer by a sintering method.

[0073] Referring to FIG. 5, the cooling fin (150) can be sintered and bonded to the lower surface of the lower metal layer (130) through an Ag-based sintered bonding layer (b1). In this case, unlike a brazing bonding structure, the cooling fin (150) and the lower metal layer (130) can form a bonding layer through solid-state diffusion via a sintering mechanism. Accordingly, the bonding layer can have low porosity and improved adhesion. Here, the sintered bonding layer (b1) may be formed from an Ag-based paste.

[0074] Since sintering bonding can typically be performed at a relatively low temperature of 200 to 300°C, thermal stress applied to the entire ceramic substrate (100) can be minimized. In addition, since the bonding layer is not remelted, structural stability is maintained even under thermal cycle conditions, and a stable heat transfer path can be secured without layer delamination or degradation of bonding reliability even in a repetitive operation environment.

[0075] In a preferred embodiment, the cooling fin (150) can be bonded to the lower metal layer (130) by sintering via an Ag-Cu alloy sintered bonding layer (b1). The Ag-Cu alloy paste used at this time is composed of metal particles containing Ag and Cu as main components and an organic binder, and can form a high-density metal bonding layer by sintering at a certain temperature. In particular, the sintering temperature can be controlled by adjusting the Ag content in the paste.

[0076] When using an Ag-Cu alloy paste, the sintering temperature can be lowered further compared to high-purity Ag, and as the Cu content increases, a reduction in material costs can also be expected. In addition, since the Ag-Cu sintered bonding layer (b1) simultaneously provides excellent thermal conductivity (Ag > Cu) and strong mechanical bonding strength, a stable heat transfer structure can be maintained without detachment of the cooling fins (150) or interface damage even under thermal shock or repeated power cycles.

[0077] As a result, the sintered bonding structure between the lower metal layer (130) and the cooling fin (150) using Ag-Cu alloy paste can provide very advantageous technical effects in terms of heat dissipation performance, process stability, and cost reduction required in high-power power modules.

[0078] Although not shown in the drawing, the sintered bonding structure through the Ag-based sintered bonding layer (b1) may also include the aforementioned pretreatment plating layer (140, see FIG. 4). In this case, the pretreatment plating layer (140) may be formed on the lower surface of the lower metal layer (130) or on the bonding surface of the cooling fin (150), similar to the modified example of the brazing bonding structure described above, and may be composed of an Ag-Cu alloy containing Ag and Cu.

[0079] FIG. 6 is a process flowchart for explaining a method for manufacturing a ceramic substrate according to an embodiment of the present invention. For convenience of explanation, the configurations shown in the preceding attached drawings will be described by referring to the corresponding reference numerals.

[0080] Referring to FIG. 6 and the preceding drawings together, a method for manufacturing a ceramic substrate according to an embodiment includes the step of forming an upper metal layer (120) on the upper surface of a ceramic substrate (110) (S100), the step of forming a lower metal layer (130) on the lower surface of the ceramic substrate (110) located opposite the surface on which the upper metal layer (120) is formed (S200), and the step of directly bonding a plurality of cooling fins (150) to one surface of the lower metal layer (130) (the lower surface of the lower metal layer in the drawing) (S300).

[0081] In steps S100 and S200, an upper metal layer (120) and a lower metal layer (130) can be bonded to a ceramic substrate (110) through a brazing process, respectively. Specifically, an Ag-based brazing filler can be interposed between the ceramic substrate (110) and the metal layers (120, 130), and the metal layers can be bonded to the upper and lower surfaces of the ceramic substrate (110) by performing brazing at a temperature between approximately 800°C and 900°C.

[0082] After step S100, if necessary, a process may be added to process the upper metal layer (120) into a circuit pattern shape capable of electrical circuit connection for mounting components such as power semiconductor devices or conductive spacers. This process may include chemical or physical etching or mechanical processing. In the embodiment, the upper metal layer (120) and the lower metal layer (130) may be composed of Cu, Cu alloy, Al, etc., having excellent electrical and thermal conductivity (about 350 W / m·K).

[0083] In step S300, direct joining of cooling fins (150) through brazing can be considered. That is, in step S300, a plurality of cooling fins (150) can be directly joined to the lower surface of the lower metal layer (130) formed on the lower part of the ceramic substrate (110) via step S200 using a brazing method. At this time, an Ag-based brazing filler can be used for the brazing joining between the lower metal layer (130) and the plurality of cooling fins (150), just as in steps S100 and S200.

[0084] The brazing filler used in steps S100 and S200 and S300 may be an Ag-Cu alloy containing silver (Ag) and copper (Cu). Since the Ag-Cu alloy has a high level of thermal conductivity, it is suitable for high heat power modules and has the advantage of securing bonding strength while preserving the structural properties of the ceramic substrate (110). In particular, Ag has strong oxidation resistance and can maintain a stable state at high temperatures.

[0085] As a preferred example, the brazing filler in steps S100 and S200 (first brazing filler) and the brazing filler in step S300 (second brazing filler) may be composed of Ag-Cu alloys with different Ag contents. More preferably, if the second brazing filler (f2) is composed of an Ag-Cu alloy with a higher Ag content than that of the first brazing filler (f1), the brazing temperature in step S300 can be significantly lowered compared to the brazing temperatures in steps S100 and S200.

[0086] In step S300, in addition to the aforementioned brazing method, a configuration in which the cooling fin (150) is directly bonded to the lower surface of the lower metal layer (130) through a sintering method may also be considered. In this case, an Ag-based sintering paste is interposed between the cooling fin (150) and the lower metal layer (130), and by performing a sintering treatment at a predetermined temperature, a high-density metal bonding layer based on solid-state diffusion can be formed.

[0087] Since sintering bonding can typically be performed at a relatively low temperature of 200 to 300°C, thermal stress applied to the entire ceramic substrate can be minimized. In addition, because the bonding layer is not remelted, structural stability is maintained even under thermal cycling conditions, and a stable heat transfer path can be secured without layer delamination or degradation of bonding reliability even in repetitive operation environments.

[0088] As a preferred example, the Ag-based sintering paste may be an Ag-Cu alloy paste. The Ag-Cu alloy paste consists of metal particles containing Ag and Cu as main components and an organic binder, and can form a high-density metal bonding layer by sintering at a certain temperature. In particular, since the sintering temperature can be controlled by adjusting the Ag content in the paste, the thermal effect on the ceramic substrate (110) and the metal layer can be effectively mitigated.

[0089] Furthermore, the Ag-Cu alloy paste allows for a lower sintering temperature compared to high-purity Ag, which is advantageous for reducing thermal damage to the substrate and preventing structural deformation due to thermal expansion, and as the Cu content increases, a reduction in material costs can also be expected. In addition, since the Ag-Cu sintered bonding layer (b1) provides excellent thermal conductivity and strong mechanical bonding strength simultaneously, a stable heat transfer structure can be maintained without detachment of the cooling fins (150) or interface damage caused by thermal shock.

[0090] Meanwhile, in directly bonding a plurality of cooling fins (150) to the lower surface of the lower metal layer (130), a plurality of cooling fins (150) can be directly bonded to the lower surface of the lower metal layer (130) at once using an alignment jig (not shown) configured to align and fix the cooling fins (150) at a predetermined position. To this end, in the manufacturing method according to the embodiment, a step (S250) of placing a plurality of cooling fins (150) on the alignment jig may be added between step S200 and step S300.

[0091] The manufacturing method according to the embodiment may further include the step (not shown) of forming a pretreatment plating layer (140) on the lower surface of the lower metal layer (130) or on the surface of the bonding portion of the cooling fins (150) before bonding a plurality of cooling fins (150) to the lower surface of the lower metal layer (130) by brazing or sintering. Here, the pretreatment plating layer (140) may be composed of an Ag-Cu alloy containing Ag and Cu to activate the bonding interface, improve wettability, and prevent oxidation.

[0092] In the step of forming the pretreatment plating layer (140), the pretreatment plating layer (140) can be formed through various known metal coating processes such as electroless plating and deposition, and the step can be added between the aforementioned steps S200 and S250 or between steps S250 and S300.

[0093] According to the present invention described above, a conventional base plate-based heat sink structure can be replaced by directly bonding cooling pins to the lower surface of a ceramic substrate. In this structure, since the intermediate layer constituting the base plate is removed, the heat conduction path is shortened and the thermal resistance is lowered, allowing heat from the power semiconductor device to be dissipated more effectively, thereby preventing device degradation and performance deterioration in high-power operating environments.

[0094] Furthermore, since the base plate is eliminated from the heatsink, the overall thickness and weight of the substrate are reduced, enabling the miniaturization and lightweighting of the power module to meet market demands. This is particularly advantageous for applications where lightweight design and space efficiency are critical, such as automotive power conversion systems. In addition, the simplification of components streamlines the manufacturing process and reduces overall manufacturing costs.

[0095] Furthermore, since the base plate is omitted, the present invention can minimize problems such as substrate warping, delamination, and thermal stress caused by the difference in the coefficient of thermal expansion (CTE) between the ceramic substrate and the cooling fins. In addition, since interfacial reliability is maintained even in environments with repeated temperature changes, the degradation of the module's lifespan can be prevented even under long-term operating conditions. Therefore, stable operation is possible in high-power systems requiring high heat resistance and high reliability.

[0096] Furthermore, a structure that directly dissipates heat to the outside through cooling fins on the ceramic substrate minimizes the distance between the heat source and the cooling path, thereby improving the cooling response speed and shortening the time required to achieve thermal equilibrium in the module, which in turn enhances the energy efficiency of the entire system. Consequently, it is possible to provide high-performance ceramic substrate technology that is improved in structural, thermal, and process aspects.

[0097] The above description is merely an illustrative explanation of the technical concept of the present invention, and those skilled in the art to which the present invention pertains will be able to make various modifications and variations within the scope of the essential characteristics of the present invention.

[0098] Accordingly, the embodiments disclosed in this invention are intended to illustrate, not limit, the technical concept of the invention, and the scope of the technical concept of the invention is not limited by these embodiments. The scope of protection of this invention shall be interpreted by the claims below, and all technical concepts within an equivalent scope shall be interpreted as being included within the scope of rights of this invention.

Claims

1. In a ceramic substrate unit for a power module, Ceramic substrate; An upper metal layer formed on the upper surface of the ceramic substrate and configured to mount a component for substrate mounting; A flat lower metal layer formed on the lower surface of the ceramic substrate; and It includes a plurality of cooling fins directly bonded to the lower surface of the lower metal layer; A ceramic substrate unit characterized in that the plurality of cooling fins are configured independently without being connected to each other and are joined to the lower metal layer by brazing or sintering.

2. In Paragraph 1, A first brazing filler is interposed between the upper metal layer and the ceramic substrate and between the lower metal layer and the ceramic substrate, and A ceramic substrate unit characterized by having a second brazing filler interposed between the cooling fin and the lower metal layer.

3. In Paragraph 2, A ceramic substrate unit characterized in that the first brazing filler and the second brazing filler are formed of an Ag-Cu alloy.

4. In Paragraph 3, A ceramic substrate unit characterized in that the second brazing filler has an Ag content higher than the Ag content of the first brazing filler.

5. In Paragraph 1, It further includes a pretreatment plating layer formed on the lower surface of the lower metal layer or on the joint surface of the cooling fin, and A ceramic substrate unit characterized in that the above-mentioned pretreatment plating layer is made of an Ag-Cu alloy.

6. In Paragraph 5, A ceramic substrate unit characterized by the thickness of the pretreatment plating layer being 0.3㎛ or more and 5.0㎛ or less.

7. In Paragraph 5, A ceramic substrate unit characterized by having a brazing filler disposed between the pretreatment plating layer and the lower metal layer or between the pretreatment plating layer and the cooling fin.

8. In Paragraph 1, An Ag-based sintered bonding layer is formed between the cooling fin and the lower metal layer, and A ceramic substrate unit characterized by the above-described sintering bonding layer being configured to mediate direct sintering bonding between the lower metal layer and the cooling fin.

9. In Paragraph 8, The above sintered bonding layer is, A ceramic substrate unit characterized by being formed from an Ag-Cu alloy paste containing Ag and Cu.

10. In Paragraph 1, A ceramic substrate unit characterized by a portion of the lower surface of the lower metal layer being directly exposed to a cooling channel partitioned between adjacent cooling fins.

11. In Paragraph 1, A ceramic substrate unit characterized in that the plurality of cooling fins above have the same shape and size.

12. A method for manufacturing a ceramic substrate unit for a power module, A step of forming an upper metal layer on the upper surface of a ceramic substrate; A step of forming a lower metal layer on the lower surface of the ceramic substrate; and The method includes the step of directly bonding a plurality of cooling fins to the lower surface of the lower metal layer; A method for manufacturing a ceramic substrate unit characterized in that the plurality of cooling fins are not connected to each other and are configured independently.

13. In Paragraph 12, The method further includes the step of seating the plurality of cooling fins on an alignment jig as a step prior to bonding the cooling fins to the lower surface of the lower metal layer. A method for manufacturing a ceramic substrate unit, characterized in that, in the step of directly bonding the plurality of cooling fins to the lower surface of the lower metal layer, the plurality of cooling fins aligned using the alignment jig are directly bonded to the lower surface of the lower metal layer at once.

14. In Paragraph 12, In the step of directly bonding the plurality of cooling fins above to the lower surface of the lower metal layer, A method for manufacturing a ceramic substrate unit characterized by directly bonding the above cooling fins to the lower surface of the lower metal layer by brazing or sintering.

15. In Paragraph 12, In the step of forming the upper metal layer and the step of forming the lower metal layer, Using a first brazing filler, the upper metal layer and the lower metal layer are brazed and joined to the upper and lower surfaces of the ceramic substrate, and In the step of directly bonding the plurality of cooling fins above to the lower surface of the lower metal layer, A method for manufacturing a ceramic substrate unit characterized by directly brazing bonding the plurality of cooling fins to the lower surface of the lower metal layer using a second brazing filler.

16. In Paragraph 15, A method for manufacturing a ceramic substrate unit characterized by forming the first brazing filler and the second brazing filler from an Ag-Cu alloy.

17. In Paragraph 16, A method for manufacturing a ceramic substrate unit, characterized in that the second brazing filler has an Ag content higher than the Ag content of the first brazing filler.

18. In Paragraph 12, A method for manufacturing a ceramic substrate unit further comprising the step of forming a pretreatment plating layer containing Ag and Cu on the lower surface of the lower metal layer or on the surface of the bonding portion of the cooling fins before bonding a plurality of cooling fins to the lower surface of the lower metal layer.