Ceramic substrate unit and manufacturing method therefor
The ceramic substrate with a heatsink structure uses screen printing to apply Ag-based paste for partial electrodes, addressing unstable bonding issues in conventional plating, ensuring reliable high-temperature bonding and efficient manufacturing.
Patent Information
- Application Number
- PCT/KR2026/096069
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-15
- Filing Date
- 2026-04-20
- Publication Date
- 2026-11-19
AI Technical Summary
Conventional partial Ag plating on metal electrodes in ceramic substrates with integrated heatsinks is difficult and leads to unstable bonding due to diffusion or loss of the Ag plating layer during high-temperature brazing, affecting long-term reliability and uniformity.
A ceramic substrate with a heatsink structure that uses a screen printing method to apply Ag-based paste only on necessary parts, forming partial electrodes through a firing process, enabling high-temperature Ag sintered bonding and ensuring stable bonding reliability.
Stable semiconductor device bonding is achieved in high-temperature environments without plating diffusion or migration, reducing material waste and simplifying the process by precise application of Ag material, thus enhancing bonding reliability and manufacturing efficiency.
Smart Images

Figure KR2026096069_19112026_PF_FP_ABST
Abstract
Description
Ceramic substrate unit and method of manufacturing the same
[0001] The present invention relates to a ceramic substrate, and more specifically, to a ceramic substrate having a heat sink integrated structure, wherein an Ag-based partial electrode is formed by screen printing on a portion on which a power semiconductor device is to be mounted, and a method for manufacturing the same.
[0002] Power semiconductor devices are core components of electronic systems that perform functions such as rectification, switching, and power amplification, and are configured in various device forms including diodes, transistors, and thyristors. These power semiconductor devices are designed to handle high voltage and high current, playing an essential role in achieving improved energy efficiency and miniaturization. In particular, power modules equipped with power semiconductor devices function as critical components in high-power applications such as hybrid and electric vehicles.
[0003] Power modules consist of power semiconductor devices and circuit boards for mounting them, and factors such as heat dissipation efficiency, mechanical reliability, and durability play a critical role in high-power operating environments. Accordingly, ceramic-based AMB substrates are widely used as circuit boards for power modules by providing excellent insulation properties, high thermal conductivity, and high-temperature stability. In particular, the AMB structure, in which copper electrodes are bonded to both sides of a ceramic substrate, is suitable for high-performance power modules as it can provide stable electrical connections and excellent heat dissipation performance even at high temperatures.
[0004] Meanwhile, with the proliferation of next-generation high-efficiency power semiconductor devices such as SiC, stable bonding characteristics at high temperatures above 250 degrees are required, and silver (Ag) sintering technology is attracting attention for this purpose. Ag sintering is a bonding method based on the diffusion between silver particles, providing excellent thermal and mechanical reliability even in high-temperature environments. However, for Ag sintering to be performed stably, Ag must also be present on the surface to be bonded, so silver plating (Ag plating) is essential on a typical copper (Cu) electrode.
[0005] Conventionally, partial Ag plating was performed on the metal electrode (Cu) of the substrate beforehand, followed by Ag sintering bonding with the semiconductor device. However, in structures where the heatsink is integrated with the substrate (heatsink-AMB integrated type), the Ag plating layer diffuses or is lost during the high-temperature brazing bonding process, leading to problems such as the inability to subsequently sinter Ag or causing non-uniform bonding characteristics. In particular, due to physical constraints, partial Ag plating is difficult in substrates with a heatsink integrated structure, and migration of the Ag plating layer negatively affects long-term reliability.
[0006] The matters described in the background technology above are intended to aid in understanding the background of the invention and may include matters that are not disclosed prior art.
[0007] The technical problem that the present invention aims to solve is to provide a ceramic substrate and a method for manufacturing the same that overcome the limitations of existing partial plating processes, which make partial Ag plating impossible, by printing Ag-based paste only on necessary parts of a ceramic substrate integrated with a heatsink using a screen printing method and forming partial electrodes (partial Ag sintered layers) through a firing process, and to enable high-temperature Ag sintered bonding through Ag-based electrodes, thereby simultaneously securing high-temperature bonding reliability and manufacturing efficiency.
[0008] According to one aspect of the present invention as a means of solving the problem, a ceramic substrate for a power module having a heatsink is provided, comprising a ceramic substrate, an upper metal layer and a lower metal layer formed respectively on the upper and lower surfaces of the ceramic substrate, a heatsink bonded to the lower metal layer, and a partial electrode partially formed on the upper metal layer, wherein the partial electrode is formed by printing an Ag-based paste in a portion of the upper metal layer where a component for substrate mounting is mounted, and firing the printed Ag-based paste.
[0009] In a heat sink integrated ceramic substrate according to one aspect, a bonding surface having an uneven surface morphology may be formed in the region where the partial electrode is formed in the upper metal layer.
[0010] In a heat sink integrated ceramic substrate according to one aspect, the bonding surface may have a surface roughness of Ra 0.3㎛ or more and 2.0㎛ or less, Rz 3㎛ or more and 8㎛ or less, and Rmax 5㎛ or more and 15㎛ or less.
[0011] In a heat sink integrated ceramic substrate according to one aspect, the Ag-based paste forming the partial electrode may be a paste containing Ag or Ag-Cu.
[0012] In a heat sink integrated ceramic substrate according to one aspect, the Ag-based paste can be partially printed on an upper metal layer through screen printing.
[0013] In a ceramic substrate with an integrated heat sink according to one aspect, an upper metal layer and a lower metal layer are brazed to the ceramic substrate through a first brazing filler, and the heat sink can be brazed to the lower metal layer through a second brazing filler.
[0014] In a heat sink integrated ceramic substrate according to one aspect, the first brazing filler and the second brazing filler are formed of an Ag-Cu alloy, and the Ag-based paste forming the partial electrode may be an Ag-Cu alloy paste.
[0015] In a heat sink integrated ceramic substrate according to one aspect, the Ag content of the second brazing filler is higher than the Ag content of the first brazing filler, and the Ag-Cu alloy paste can be formed such that the Ag content is higher than the Ag content of the second brazing filler.
[0016] According to another aspect of the present invention as a means of solving the problem, a method for manufacturing a ceramic substrate for a power module comprises the steps of forming an upper metal layer on the upper surface of a ceramic substrate and forming a lower metal layer on the lower surface, bonding a heat sink to the lower metal layer, and forming a partial electrode on the upper metal layer. In the step of forming the partial electrode, an Ag-based paste may be printed on a portion of the upper metal layer where a component for substrate mounting is mounted, and the printed Ag-based paste may be formed by firing.
[0017] In a method for manufacturing a heat sink integrated ceramic substrate according to another aspect, the Ag-based paste used in the step of forming the partial electrode may be a paste containing Ag or Ag-Cu.
[0018] In a method for manufacturing a heat sink integrated ceramic substrate according to another aspect, in the step of forming the partial electrode, the partial electrode can be formed by screen printing the Ag-based paste.
[0019] In a method for manufacturing a heat sink integrated ceramic substrate according to another aspect, in the step of forming an upper metal layer on the upper surface of the ceramic substrate and forming a lower metal layer on the lower surface, a first brazing filler is interposed between the upper metal layer and the ceramic substrate and between the lower metal layer and the ceramic substrate, and then brazing is performed; and in the step of brazing a heat sink to the lower metal layer, a second brazing filler is interposed between the lower metal layer and the heat sink, and then brazing is performed to bond them.
[0020] In a method for manufacturing a heat sink integrated ceramic substrate according to another aspect, the first brazing filler and the second brazing filler are formed from an Ag-Cu alloy, and it is preferable to use an Ag-Cu alloy paste for the Ag-based paste forming the partial electrode.
[0021] In a method for manufacturing a heat sink integrated ceramic substrate according to another aspect, it is preferable to use a second brazing filler having an Ag content higher than that of the first brazing filler, and an Ag-Cu alloy paste having an Ag content higher than that of the second brazing filler.
[0022] According to the present invention, by forming partial electrodes by printing Ag paste via a screen printing method and firing it in a structure where conventional partial Ag plating is difficult (e.g., a ceramic substrate integrated with a heatsink), Ag-based sintered bonding is enabled even in a ceramic substrate integrated with a heatsink structure. Through this, stable semiconductor device bonding can be realized even in high-temperature environments, and highly reliable bonding can be achieved without plating diffusion or migration.
[0023] Furthermore, the screen printing method allows for the precise application of Ag material only to the required areas, thereby reducing material waste and simplifying the process. Moreover, applying the screen printing method eliminates the plating process, which is a pretreatment step for separate sintering bonding, thus simplifying the process and reducing costs. Consequently, process stability for electrode formation can be ensured in a heatsink-integrated ceramic substrate structure.
[0024] FIG. 1 is a plan view of a ceramic substrate according to an embodiment of the present invention.
[0025] FIG. 2 is a front view of a ceramic substrate according to an embodiment of the present invention.
[0026] FIG. 3 is a cross-sectional view of a ceramic substrate according to an embodiment of the present invention, viewed from the direction of line A-A' in FIG. 1.
[0027] FIG. 4 is an enlarged cross-sectional view of a key portion of a ceramic substrate according to another preferred embodiment of the present invention.
[0028] FIG. 5 is a process flowchart for explaining a method for manufacturing a ceramic substrate according to an embodiment of the present invention.
[0029] Hereinafter, preferred embodiments of the present invention will be described in detail.
[0030] In describing the embodiments of the present invention, identical or similar components are assigned the same reference numerals, and redundant descriptions thereof are omitted. Furthermore, detailed descriptions of related prior art are omitted if it is determined that such detailed descriptions could obscure the essence of the embodiments disclosed in this specification.
[0031] In addition, the attached drawings are intended only to facilitate understanding of the embodiments disclosed in this specification, and the technical concept disclosed in this specification is not limited by the attached drawings, and it should be noted that they include all modifications, equivalents, and substitutions that fall within the concept and technical scope of the present invention.
[0032] The embodiments are provided to more fully explain the invention to those skilled in the art, and the following embodiments may be modified in various different forms, and the scope of the invention is not limited to the following embodiments. Rather, these embodiments are provided to make the disclosure more faithful and complete and to fully convey the spirit of the invention.
[0033] The terms used herein are for describing specific embodiments and are not intended to limit the invention. Additionally, the singular form in this specification may include the plural form unless the context clearly indicates otherwise.
[0034] In the description of the embodiments, where each layer (film), region, pattern, or structure is described as being formed "on" or "under" the substrate, each layer (film), region, pad, or pattern, "on" and "under" include both being formed "directly" and "indirectly" through another layer. In addition, the reference for the top or bottom of each layer is, in principle, based on the drawings.
[0035] The drawings are intended solely to facilitate an understanding of the concept of the present invention and should not be interpreted as limiting the scope of the invention. Additionally, relative thicknesses, lengths, or sizes in the drawings may be exaggerated for convenience and clarity of explanation.
[0036] FIG. 1 is a plan view of a ceramic substrate according to an embodiment of the present invention, and FIG. 2 is a front view of a ceramic substrate according to an embodiment of the present invention. FIG. 3 is a cross-sectional view of a ceramic substrate according to an embodiment of the present invention viewed along the line A-A' of FIG. 1.
[0037] Referring to FIGS. 1 to 3, a ceramic substrate (100) according to an embodiment of the present invention comprises a ceramic substrate (110), an upper metal layer (120) and a lower metal layer (130) formed respectively on the upper and lower surfaces of the ceramic substrate (110), a heat sink (150) brazed to the lower metal layer (130), and a partial electrode (140) partially formed on the upper metal layer (120) opposite the heat sink (150).
[0038] The ceramic substrate (110) may be composed of an oxide-based or nitride-based ceramic material having high thermal conductivity and excellent flexural strength. For example, the ceramic substrate (110) may be formed from any one of Al2O3, AlN, Si3N4, and ZTA (Zirconia Toughened Alumina). An upper metal layer (120) and a lower metal layer (130) may be formed by brazing metal foils on both sides of the ceramic substrate (110).
[0039] The upper metal layer (120) can be formed into a circuit pattern capable of electrical circuit connection of mounting components, such as power semiconductor devices or conductive spacers, through chemical or physical etching or mechanical processing. The upper metal layer (120) and the lower metal layer (130) can be made of any one of Cu, Cu alloy (CuMo, etc.), or Al, which have excellent electrical and thermal conductivity.
[0040] For brazing, a brazing bonding layer made of a metal material comprising at least one of Ag, AgCu, or AgCuTi may be used. The heat treatment temperature for brazing may be 780 degrees or higher and 900 degrees or lower. This is intended to ensure stable bonding between the ceramic substrate and the metal layer, taking into account temperature conditions that can prevent deformation or oxidation of the metal layer.
[0041] The ceramic substrate (100) may be an Active Metal Brazing (AMB) substrate having a structure in which metal layers (120, 130) are bonded to the upper and lower surfaces of a ceramic substrate (110). The AMB substrate has excellent durability and heat dissipation performance, and has the advantage of maintaining stable electrical and mechanical properties even in high-temperature environments. In the embodiment, the AMB substrate is described as a preferred example, but is not limited thereto, and the ceramic substrate may be a Direct Bonding Copper (DBC) substrate.
[0042] Considering that the ceramic substrate (110) constituting the ceramic substrate (100) is applied to a power module operating in a high-temperature environment, the thickness of the ceramic substrate (100) is preferably at least 0.25 mm. In addition, the thickness of the upper metal layer (120) and the lower metal layer (130) bonded to the upper and lower surfaces of the ceramic substrate (110) is preferably at least 0.127 mm to efficiently dissipate heat from the power semiconductor device and to ensure a solid bond with the substrate.
[0043] The heat sink (150) can be formed as an integral structure with the ceramic substrate by brazing bonding to one side of the lower metal layer (130) (the lower surface of the lower metal layer in the drawing). The heat sink (150) is intended to prevent overheating of the ceramic substrate through heat dissipation and can be formed from a material with high thermal conductivity. For example, at least one of Cu, Al, AlSiC, CuMo, CuW, Cu / CuMo / Cu, Cu / Mo / Cu, and Cu / W / Cu, or a composite material thereof, may be used.
[0044] The heat sink (150) can operate in an air-cooled or water-cooled manner. In the case of air cooling, air is supplied as a refrigerant, and in the case of water cooling, cooling water can be circulated and supplied by a pump. As one embodiment, a slit-type heat sink (150) is shown in which a plurality of rod-shaped protrusions (154) are arranged on the lower surface of a flat-plate body (152), but it can be changed to various structures such as Micro Channel, Pin Fin, Micro Jet, and Slit type.
[0045] A partial electrode (140) may be formed on an upper metal layer (120) of a ceramic substrate (100). The partial electrode (140) may be partially formed on the upper surface of the upper metal layer (120) in correspondence with a component for substrate mounting (not shown). Preferably, it may be formed in a portion of the upper metal layer (120) on which the component for substrate mounting is mounted, with an area corresponding to the lower surface (bonding surface) of the component for substrate mounting.
[0046] In the following embodiments, a power semiconductor device is described as an example of a mounting component mounted on a partial plating layer (140). Here, the power semiconductor device may be SiC, GaN, IGBT, MOSFET, etc.
[0047] The partial electrode (140) mediates a rigid bond between the upper metal layer (120) and the power semiconductor device. In an embodiment, the partial electrode (140) may be an Ag-based sintered layer formed by partially printing an Ag-based paste containing silver (Ag) and then firing it at a specific temperature. Here, the specific temperature for firing the Ag-based paste may be in the range of about 350 to 900 degrees.
[0048] In forming a partial electrode (140) in a portion of the upper metal layer (120) with an area corresponding to a power semiconductor device, it can be formed precisely and selectively through a screen printing method in which an Ag-based paste is printed in a pattern corresponding to the shape or area of the power semiconductor device.
[0049] Since the partial electrode (140) is composed of an Ag-based sintered layer, it can provide high thermal conductivity. Therefore, high-temperature heat generated during the operation of the power semiconductor device can be effectively transferred to the upper metal layer (120). In addition, it enables reliable bonding with the power semiconductor device in a subsequent sintering bonding process. In particular, since diffusion between Ag particles is easy, a bonding layer having high sintering density, low porosity, and excellent bonding strength can be formed.
[0050] In addition, due to the characteristics of power modules operating in high-temperature environments, it may be difficult to ensure sufficient bonding strength and reliability using conventional low-melting-point solder bonding methods. However, since the melting point of the Ag-based sintered layer rises to over 700 degrees after bonding, the bonding characteristics can be stably maintained even at high temperatures. Accordingly, the lifespan and thermal and mechanical reliability of the power module can be improved.
[0051] As a preferred example, the Ag-based paste forming the partial electrode (140) may be an Ag paste containing Ag as a major component. As another preferred example, the Ag-based paste forming the partial electrode may be an Ag-Cu alloy paste containing Ag and Cu as major components.
[0052] Meanwhile, a brazing filler (hereinafter referred to as the "first brazing filler") is used for brazing joints between the ceramic substrate (110) and the metal layers (120, 130). A brazing filler (hereinafter referred to as the "second brazing filler") is also used for brazing joints between the lower metal layer (130) and the heat sink (150). The first brazing filler (f1) and the second brazing filler (f2) can be formed by various methods such as paste application, foil attachment, and electroless plating.
[0053] A first brazing filler (f1) is positioned between the ceramic substrate (110) and the upper metal layer (120) and between the ceramic substrate (110) and the lower metal layer (130), respectively, to mediate a strong thermal and mechanical bond between them. A second brazing filler (f2) mediates a strong thermal and mechanical bond between the lower metal layer (130) and the heat sink (150). These first brazing filler (f1) and second brazing filler (f2) may be composed of an Ag alloy containing Ag.
[0054] As a preferred example, the first brazing filler (f1) and the second brazing filler (f2) may be made of an Ag-Cu alloy composed of silver (Ag) and copper (Cu) in a certain ratio. Since the Ag-Cu alloy has a high level of thermal conductivity, it can maximize heat dissipation performance in the power module when high heat is present. In addition, the Ag-Cu alloy has the advantage of securing bonding strength while preserving the structural characteristics of the ceramic substrate (110).
[0055] In particular, Ag has strong oxidation resistance, maintaining a stable state at high temperatures, and can contribute to maintaining stable bonding quality by suppressing oxide formation during the bonding process. Ag also has excellent wettability with metals or ceramics at specific brazing temperatures (generally 600 to 900 degrees), allowing it to spread uniformly across the bonding surface to form a solid bonding layer.
[0056] As mentioned, an Ag-Cu alloy paste can be used as an Ag-based paste for forming partial electrodes. In this case, by adjusting the Ag content of the Ag-Cu alloy paste and the Ag content of the first and second brazing fillers (f1, f2) differently, the temperature of the final firing process (firing process for forming partial electrodes) can be stably controlled within a range lower than the temperature of the brazing joining process performed prior to it.
[0057] Generally, Ag alloys have the characteristic that the higher the Ag content, the lower the effective melting point. Considering this characteristic of Ag alloys, it is preferable to apply an Ag-Cu alloy with a higher Ag content than the first brazing filler (f1) as the second brazing filler (f2), and to form a partial electrode (140) on the upper metal layer (120) with an Ag-Cu alloy paste having an even higher Ag content than the second brazing filler (f2).
[0058] Through this compositional design, it is desirable to lower the temperature of the second bonding process (brazing between the lower metal layer and the heat sink through the second brazing filler) compared to the first bonding process (brazing between the ceramic substrate and the metal layer through the first brazing filler), and to stably perform the subsequent third firing process (a process of forming partial electrodes by firing the partially printed Ag-Cu alloy paste) at an even lower temperature.
[0059] When the temperature of the subsequent process (brazing bonding or firing process) is lowered, the deformation caused by thermal expansion of the ceramic substrate (100) is reduced, thereby reducing thermal stress, and by performing the process below the liquidus temperature of each brazing filler, remelting of the existing bond can be prevented. Accordingly, the structural stability of the bonding layer is maintained, and the phenomenon of layer separation between the ceramic substrate and the metal layer or between the lower metal layer and the heat sink can be reliably prevented.
[0060] As a preferred example, the first brazing filler (f1) may be formed from an Ag-Cu alloy with an Ag-Cu composition ratio of 5:5, and the second brazing filler (f2) may be formed from an Ag-Cu alloy with an Ag-Cu composition ratio of 6:4. Additionally, an Ag-Cu alloy paste with an Ag-Cu composition ratio of 7:3 may be used as the sintering material for forming the partial electrode (140).
[0061] When an Ag-Cu alloy with an Ag-Cu composition ratio of 5:5 is used as a brazing filler for primary brazing (bonding between a ceramic substrate and a metal layer), primary brazing can be performed at approximately 890°C on the binary eutectic phase diagram of the Ag-Cu alloy, and in the case of an Ag-Cu alloy with an Ag-Cu composition ratio of 6:4, brazing can be performed at approximately 850°C, so brazing can be performed at a lower temperature than primary brazing.
[0062] On the other hand, an Ag-Cu alloy with an Ag-to-Cu composition ratio of 7:3 can be sintered and joined at approximately 780 degrees. Therefore, if an Ag-Cu alloy paste with an Ag-to-Cu composition ratio of 7:3 is used as a material for forming partial electrodes (140), sintering treatment can be performed at a temperature approximately 70 to 110 degrees lower than the first and second brazing joining processes, thereby clearly resolving the problem of remelting of the brazing joint and the resulting layer separation.
[0063] FIG. 4 is an enlarged cross-sectional view of a key portion of a ceramic substrate according to another preferred embodiment of the present invention.
[0064] Referring to FIG. 4, in the region where a partial electrode (140) is formed in the upper metal layer (120), a bonding surface (122) having a surface morphology with a fine irregular shape having a size corresponding to the partial electrode (140) may be formed. In another embodiment, the surface roughness, which represents the degree of fine irregularity of the bonding surface (122), may be expressed by parameters such as arithmetic mean roughness (Ra), maximum roughness height (Rmax), and maximum height roughness (Rz).
[0065] In another embodiment, the surface roughness of the bonding surface (122) may be Ra 0.3 μm or more and 2.0 μm or less, Rz 3 μm or more and 8 μm or less, and Rmax 5 μm or more and 15 μm or less. If Ra is less than 0.3 μm, the surface of the bonding surface (122) is excessively smooth, which may reduce the adhesion of the Ag-based paste forming the partial electrode (140). Conversely, if Ra exceeds 2.0 μm, the surface becomes excessively rough, which may cause a problem where the Ag-based paste is not printed locally.
[0066] Therefore, considering stable and robust bonding with the Ag-based paste, the surface roughness of the bonding surface (122), which is the region where the partial electrode (140) is formed in the upper metal layer (120), is preferably 0.3 μm or more and 2.0 μm or less based on Ra, which represents the arithmetic mean roughness. At this time, when the Ra value is 0.3 μm or more and 2.0 μm or less, the corresponding Rz value is 3 μm or more and 8 μm or less, and the Rmax value may be 5 μm or more and 15 μm or less.
[0067] FIG. 5 is a process flowchart for explaining a method for manufacturing a ceramic substrate according to an embodiment of the present invention. For convenience of explanation, the configurations shown in the preceding attached drawings will be described by referring to the corresponding reference numerals.
[0068] Referring to FIG. 5 and the preceding drawings together, a method for manufacturing a ceramic substrate according to an embodiment includes the steps of forming an upper metal layer (120) on the upper surface of a ceramic substrate (110) and forming a lower metal layer (130) on the lower surface (S100), brazing a heat sink (150) to the lower metal layer (130) (S200), and forming a partial electrode (140) in a part area of the upper metal layer (120) (S300).
[0069] In step S100, the metal layers (120, 130) can be bonded to the ceramic substrate (110) through a brazing process. Specifically, a first brazing filler (f1) can be interposed between the metal layers (120, 130) and the ceramic substrate (110), and by performing brazing at a temperature between approximately 800 and 900 degrees, an upper metal layer (120) and a lower metal layer (130) can be formed on the upper and lower surfaces of the ceramic substrate (110), respectively.
[0070] In step S200, a second brazing filler (f2) is interposed between the lower metal layer (130) and the heat sink (150) among the metal layers formed on the ceramic substrate (110) through step S100, and then a brazing process is performed at a temperature of about 800 to 900 degrees, so that the lower metal layer (130) and the heat sink (150) can be brazed and joined. As a result, the heat sink (150) can be formed as an integrated structure on the ceramic substrate (100).
[0071] The heat sink (150) also serves to prevent deformation of the ceramic substrate in a high-temperature environment, but its primary role is to prevent overheating of the ceramic substrate through heat dissipation. Therefore, the material of the heat sink (150) is preferably a material with high thermal conductivity. For example, the heat sink (150) may be made of at least one of Cu, Al, AlSiC, CuMo, CuW, Cu / CuMo / Cu, Cu / Mo / Cu, and Cu / W / Cu, or a composite material thereof.
[0072] The heat sink (150) can operate in an air-cooled or water-cooled manner. In the case of air cooling, air is supplied as a refrigerant, and in the case of water cooling, cooling water can be circulated and supplied by a pump. As one embodiment, a slit-type heat sink (150) is shown in which a plurality of rod-shaped protrusions (154) are arranged on the lower surface of a flat-plate body (152), but it can be changed to various structures such as Micro Channel, Pin Fin, Micro Jet, and Slit type.
[0073] In step S100, a first brazing filler (f1) mediating bonding between the ceramic substrate (110) and the metal layers (120, 130) can be formed on the upper and lower surfaces of the ceramic substrate (110) through various methods such as paste application, foil attachment, and electroless plating, and in step S200, a second brazing filler (f2) can be formed on the lower surface of the lower metal layer (130) or on the upper surface of the heat sink (150) facing it through various methods such as paste application, foil attachment, and electroless plating.
[0074] In step S300, the partial electrode (140) can be formed by printing an Ag-based paste in a portion of the upper metal layer (120) where a power semiconductor device is mounted (S302), and firing the printed Ag-based paste (S304). In step S300, the Ag-based paste may be an Ag paste containing Ag as a major component. Additionally, an Ag-Cu alloy paste containing Ag and Cu as major components may be used.
[0075] In forming partial electrodes in a portion of the upper metal layer (120) where a power semiconductor device is mounted, the electrodes can be formed precisely and selectively through a screen printing method in which an Ag-based paste is printed at a location where the power semiconductor device is to be mounted in a pattern corresponding to the shape or area of the power semiconductor device, and the firing temperature may be in the range of about 350 degrees to 900 degrees.
[0076] According to an embodiment, a step (S250) of forming a bonding surface having an uneven surface morphology in the region where a partial electrode (140) is formed in the upper metal layer (120) may be added. Step S250 may be performed between the aforementioned steps S200 and S300. Here, the surface roughness of the bonding surface (122) may be formed such that Ra is 0.3 μm or more and 2.0 μm or less, Rz is 3 μm or more and 8 μm or less, and Rmax is 5 μm or more and 15 μm or less.
[0077] If Ra is less than 0.3 μm, the surface of the bonding surface (122) is excessively smooth, which may reduce the adhesion of the Ag-based sintered layer forming the partial electrode. Conversely, if Ra exceeds 2.0 μm, the surface becomes excessively rough, which may cause a problem where the Ag-based sintered layer does not adhere locally.
[0078] In step S250, for example, a bonding surface (122) having an uneven surface morphology can be partially formed on a portion of the upper metal layer (120) by masking only a portion of the upper metal layer (1200) to be formed so that only that portion of the bonding surface (122) is exposed to the outside, and then performing sputtering or laser processing.
[0079] In the method for manufacturing a ceramic substrate according to the embodiment, the first brazing filler (f1) and the second brazing filler (f2) can be formed from an Ag-Cu alloy. Additionally, in step S300, a partial electrode (140) can be formed using an Ag-Cu alloy paste. At this time, the second brazing filler can be configured such that the Ag content is higher than the Ag content of the first brazing filler, and the Ag-Cu alloy paste can be configured to have an Ag content higher than that of the second brazing filler.
[0080] By setting the Ag content of each material to progressively higher levels in this manner, the bonding and sintering processes can be performed at progressively lower temperatures according to the process sequence, which is advantageous for preventing thermal interference and ensuring the stability of each bonding interface. Consequently, the reliability and yield of the entire process can be improved.
[0081] According to the present invention, by forming partial electrodes by printing Ag paste via a screen printing method and firing it in a structure where conventional partial Ag plating is difficult (e.g., a ceramic substrate integrated with a heatsink), Ag-based sintered bonding is enabled even in a ceramic substrate integrated with a heatsink structure. Through this, stable semiconductor device bonding can be realized even in high-temperature environments, and highly reliable bonding can be achieved without plating diffusion or migration.
[0082] Furthermore, the screen printing method allows for the precise application of Ag material only to the required areas, thereby reducing material waste and simplifying the process. Moreover, applying the screen printing method eliminates the plating process, which is a pretreatment step for separate sintering bonding, thus simplifying the process and reducing costs. Consequently, process stability for electrode formation can be ensured in a heatsink-integrated ceramic substrate structure.
[0083] The above description is merely an illustrative explanation of the technical concept of the present invention, and those skilled in the art to which the present invention pertains will be able to make various modifications and variations within the scope of the essential characteristics of the present invention.
[0084] Accordingly, the embodiments disclosed in this invention are intended to illustrate, not limit, the technical concept of the invention, and the scope of the technical concept of the invention is not limited by these embodiments. The scope of protection of this invention shall be interpreted by the claims below, and all technical concepts within an equivalent scope shall be interpreted as being included within the scope of rights of this invention.
Claims
1. A ceramic substrate for a power module equipped with a heat sink, Ceramic substrate; An upper metal layer and a lower metal layer formed respectively on the upper and lower surfaces of the ceramic substrate; A heat sink bonded to the lower metal layer above; and A partial electrode partially formed on the upper metal layer; comprising The above partial electrode is, An Ag-based paste is printed on a portion of the upper metal layer above where a component for substrate mounting is mounted, and A heatsink integrated ceramic substrate characterized by being formed by firing the printed Ag-based paste.
2. In Paragraph 1, A heat sink integrated ceramic substrate characterized by having a bonding surface having an uneven surface morphology formed in the region where the partial electrode is formed in the upper metal layer.
3. In Paragraph 2, A heatsink integrated ceramic substrate characterized in that the bonding surface has a surface roughness of Ra 0.3㎛ or more and 2.0㎛ or less, Rz 3㎛ or more and 8㎛ or less, and Rmax 5㎛ or more and 15㎛ or less.
4. In Paragraph 1, The Ag-based paste forming the above partial electrode is, A heatsink integrated ceramic substrate characterized by being a paste containing Ag or Ag-Cu.
5. In Paragraph 1, A heatsink integrated ceramic substrate characterized by the above Ag-based paste being printed by a screen printing method.
6. In Paragraph 1, The upper metal layer and the lower metal layer are brazed to the ceramic substrate through a first brazing filler, and A heatsink integrated ceramic substrate characterized in that the heatsink is brazed to the lower metal layer through a second brazing filler.
7. In Paragraph 6, The first brazing filler and the second brazing filler are formed of an Ag-Cu alloy, and A heatsink integrated ceramic substrate characterized in that the Ag-based paste forming the above partial electrode is an Ag-Cu alloy paste.
8. In Paragraph 7, The Ag content of the second brazing filler is higher than the Ag content of the first brazing filler, and A heatsink integrated ceramic substrate characterized in that the Ag content of the above Ag-Cu alloy paste is higher than the Ag content of the above second brazing filler.
9. A method for manufacturing a ceramic substrate for a power module, A step of forming an upper metal layer on the upper surface of a ceramic substrate and forming a lower metal layer on the lower surface; A step of bonding a heat sink to the lower metal layer; and The method includes the step of partially forming a partial electrode on the upper metal layer; In the step of forming the above partial electrode, An Ag-based paste is printed on a portion of the upper metal layer above where a component for substrate mounting is mounted, and A method for manufacturing a heat sink integrated ceramic substrate characterized by forming the above-mentioned printed Ag-based paste by firing.
10. In Paragraph 9, In the step of forming the above partial electrode, A method for manufacturing a heat sink integrated ceramic substrate, characterized in that the above Ag-based paste is a paste containing Ag or Ag-Cu.
11. In Paragraph 9, In the step of forming the above partial electrode, A method for manufacturing a heat sink integrated ceramic substrate characterized by screen printing the above Ag-based paste.
12. In Paragraph 9, In the step of forming an upper metal layer on the upper surface of the ceramic substrate and forming a lower metal layer on the lower surface, After interposing a first brazing filler between the upper metal layer and the ceramic substrate and between the lower metal layer and the ceramic substrate, brazing bonding is performed, In the step of brazing a heat sink onto the lower metal layer, A method for manufacturing a heat sink integrated ceramic substrate characterized by interposing a second brazing filler between the lower metal layer and the heat sink and then performing brazing bonding.
13. In Paragraph 12, The first brazing filler and the second brazing filler are formed from an Ag-Cu alloy, and A method for manufacturing a heat sink integrated ceramic substrate characterized by using an Ag-Cu alloy paste as the Ag-based paste forming the above-mentioned partial electrode.
14. In Paragraph 13, The second brazing filler has an Ag content higher than the Ag content of the first brazing filler, and A method for manufacturing a heat sink integrated ceramic substrate, characterized in that the above Ag-Cu alloy paste has an Ag content higher than the Ag content of the above second brazing filler.