Ceramic substrate, power module including same, and method for manufacturing ceramic substrate
The ceramic substrate with nickel plating and silver sintered bonding layers addresses high manufacturing costs and reliability issues in high-voltage power modules by providing cost-effective and reliable bonding for semiconductor devices and heat dissipation blocks.
Patent Information
- Application Number
- PCT/KR2026/096070
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-15
- Filing Date
- 2026-04-20
- Publication Date
- 2026-11-19
AI Technical Summary
Existing ceramic substrates for high-voltage power modules face issues with high manufacturing costs due to excessive use of silver plating, which is sensitive to sulfidation and leads to bonding failures, interfacial defects, and reduced reliability, and silver migration causes electrical short circuits.
A ceramic substrate with nickel plating layers on both surfaces and partial silver sintered bonding layers for secure bonding with power semiconductor devices and heat dissipation blocks, using nickel plating to reduce costs and improve bonding reliability.
The solution reduces manufacturing costs, enhances bonding reliability, and prevents electrical short circuits by using nickel plating with controlled surface roughness and silver sintered bonding layers, ensuring stable operation in high-temperature environments.
Smart Images

Figure KR2026096070_19112026_PF_FP_ABST
Abstract
Description
Ceramic substrate and power module including the same, and method for manufacturing a ceramic substrate
[0001] The present invention relates to a ceramic substrate, and more particularly to a ceramic substrate suitable for a high-voltage power module requiring high mechanical strength, thermal conductivity, and heat dissipation performance, a power module including the same, and a method for manufacturing the ceramic substrate.
[0002] Power semiconductor devices are core components of electronic systems that perform functions such as rectification, switching, and power amplification, and are configured in various device forms including diodes, transistors, and thyristors. These power semiconductor devices are designed to handle high voltage and high current, playing an essential role in achieving improved energy efficiency and miniaturization. In particular, power modules equipped with power semiconductor devices function as critical components in high-power applications such as hybrid and electric vehicles.
[0003] Power modules consist of power semiconductor devices and circuit boards for mounting them, and factors such as heat dissipation efficiency, mechanical reliability, and durability play a critical role in high-power operating environments. Accordingly, ceramic-based AMB substrates are widely used as circuit boards for power modules by providing excellent insulation properties, high thermal conductivity, and high-temperature stability. In particular, the AMB structure, in which copper electrodes are bonded to both sides of a ceramic substrate, is suitable for high-performance power modules as it can provide stable electrical connections and excellent heat dissipation performance even at high temperatures.
[0004] Meanwhile, as the application of high-efficiency power semiconductor devices such as SiC expands, reliable bonding technology at high temperatures above 250 degrees is becoming increasingly important. To this end, Ag sintering bonding technology is attracting attention, and Ag plating on the copper electrode of the ceramic substrate is required for Ag sintering. This is because problems such as bonding failures, interfacial defects, and reduced reliability can easily occur if sintering is performed directly without Ag plating.
[0005] However, silver (Ag) is sensitive to sulfidation reactions, and reliability issues regarding quality may arise, such as interfacial oxidation and migration failures with copper in high-temperature environments. In particular, when silver is plated on the front surface of a copper electrode, the use of expensive silver is excessive, which increases manufacturing costs and reduces the economic efficiency of the entire process.
[0006] The matters described in the background technology above are intended to aid in understanding the background of the invention and may include matters that are not disclosed prior art.
[0007] The technical problem that the present invention aims to solve is to provide a ceramic substrate, a power module including the same, and a method for manufacturing the ceramic substrate, which can secure the rigidity of the manufacturing process and improve bonding reliability by plating Ni on a copper electrode instead of the costly Ag plating, and bonding a power semiconductor device onto the said Ni plating layer using an Ag sintering method.
[0008] Another technical problem that the present invention aims to solve is to provide a ceramic substrate that can resolve electrical defects, such as electrical short circuits, that may occur due to the migration phenomenon of silver (Ag), a power module including the same, and a method for manufacturing the ceramic substrate.
[0009] According to one aspect of the present invention as a means of solving the problem, a ceramic substrate for a power module on which a power semiconductor device is mounted comprises: a ceramic substrate; an upper metal layer and a lower metal layer formed respectively on the upper and lower surfaces of the ceramic substrate; a first front plating layer and a second front plating layer plated to cover the entire surface of the upper metal layer and the lower metal layer; and a first partial bonding layer partially formed on the first front plating layer to mediate bonding between the first front plating layer and the power semiconductor device, wherein the first front plating layer and the second front plating layer are nickel (Ni) plating layers, and the first partial bonding layer is an Ag sintered bonding layer containing silver (Ag).
[0010] In a ceramic substrate according to one aspect, the surface roughness of the region where the first partial bonding layer is formed among the first front plating layer may be Ra 0.3㎛ or more and 2.0㎛ or less, Rz 3㎛ or more and 8㎛ or less, and Rmax 5㎛ or more and 15㎛ or less.
[0011] In a ceramic substrate according to one aspect, the thickness of the first partial bonding layer may be 0.1 μm or more and 1.0 μm or less.
[0012] A ceramic substrate according to one aspect further comprises a second partial bonding layer mediating bonding between the second front plating layer and a heat dissipation block, wherein the second partial bonding layer may be partially formed on the second front plating layer corresponding to the heat dissipation block.
[0013] In a ceramic substrate according to one aspect, the surface roughness of the region where the second partial bonding layer is formed among the second front plating layer may be Ra 0.3㎛ or more and 2.0㎛ or less, Rz 3㎛ or more and 8㎛ or less, and Rmax 5㎛ or more and 15㎛ or less.
[0014] In a ceramic substrate according to one aspect, the thickness of the second partial bonding layer may be 0.1 μm or more and 1.0 μm or less.
[0015] In a ceramic substrate according to one aspect, the second partial bonding layer may be an Ag sintered bonding layer containing silver (Ag).
[0016] According to another aspect of the present invention as a means of solving the problem, a power module is provided comprising a ceramic substrate having an upper metal layer formed on the upper surface and a lower metal layer formed on the lower surface of the ceramic substrate, a power semiconductor device mounted on the upper metal layer of the ceramic substrate, and a heat dissipation block bonded to the lower metal layer of the ceramic substrate, wherein a first front plating layer is formed to cover the entire surface of the upper metal layer on the ceramic substrate, a second front plating layer is formed to cover the entire surface of the lower metal layer, a first partial bonding layer is partially formed on the first front plating layer corresponding to the power semiconductor device, the first front plating layer and the second front plating layer are nickel (Ni) plating layers, and the first partial bonding layer is an Ag sintered bonding layer containing silver (Ag).
[0017] In a power module according to another aspect, the surface roughness of the area where the first partial bonding layer is formed among the first front plating layer may be Ra 0.3㎛ or more and 2.0㎛ or less, Rz 3㎛ or more and 8㎛ or less, and Rmax 5㎛ or more and 15㎛ or less.
[0018] In a power module according to another aspect, the thickness of the first partial bonding layer may be 0.1㎛ or more and 1.0㎛ or less.
[0019] A power module according to another aspect further comprises a second partial bonding layer formed on the second front plating layer, wherein the second partial bonding layer may be formed in a portion of the second front plating layer where the heat dissipation block is bonded.
[0020] In a power module according to another aspect, the surface roughness of the region where the second partial bonding layer is formed among the second partial bonding layers may be Ra 0.3㎛ or more and 2.0㎛ or less, Rz 3㎛ or more and 8㎛ or less, and Rmax 5㎛ or more and 15㎛ or less.
[0021] In a power module according to another aspect, the thickness of the second partial bonding layer may be 0.1㎛ or more and 1.0㎛ or less.
[0022] In a power module according to another aspect, the second partial bonding layer may be an Ag sintered bonding layer containing silver (Ag).
[0023] According to another aspect of the present invention as a means of solving the problem, a method for manufacturing a ceramic substrate for a power module comprises the steps of: forming an upper metal layer on the upper surface of a ceramic substrate and forming a lower metal layer on the lower surface; forming a first front plating layer to cover the entire surface of the upper metal layer and forming a second front plating layer to cover the entire surface of the lower metal layer; and partially forming a first partial bonding layer on the first front plating layer to correspond to a power semiconductor device, wherein the first front plating layer and the second front plating layer are formed of nickel (Ni), and the first partial bonding layer is formed of an Ag sintered paste containing silver (Ag).
[0024] In a method for manufacturing a ceramic substrate according to another aspect, the step of forming the first front plating layer and the second front plating layer may form the first front plating layer and the second front plating layer as nickel plating layers through electrolytic plating or electroless plating.
[0025] In a method for manufacturing a ceramic substrate according to another aspect, the step of partially forming the first partial bonding layer may be formed in a portion of the upper metal layer where the power semiconductor device is mounted, with an area corresponding to the lower surface of the power semiconductor device.
[0026] A method for manufacturing a ceramic substrate according to another aspect further comprises the step of forming a second partial bonding layer on the second front plating layer, wherein in the step of forming the second partial bonding layer, the second partial bonding layer may be formed in a portion of the second front plating layer where a heat dissipation block is bonded.
[0027] In a method for manufacturing a ceramic substrate according to another aspect, the second partial bonding layer can be formed with an Ag sintered paste containing silver (Ag).
[0028] According to the present invention, instead of plating high-cost silver (Ag) on a copper electrode, nickel (Ni) is plated on the entire surface, and then a power semiconductor device is bonded to the Ni plating layer using an Ag sintering method, thereby reducing manufacturing costs and improving the economic efficiency of the process. In the case of the nickel plating layer, the interfacial stability and oxidation resistance are excellent, so bonding strength and reliability with the Ag sintered material can be secured.
[0029] In addition, defects such as electrical short circuits caused by silver migration, which can occur in full Ag plating methods, can be effectively prevented. Accordingly, this provides a useful technical means to simultaneously improve the structural stability and lifespan characteristics of power modules that require operational reliability in high-temperature environments.
[0030] In addition, by imparting a specific degree of roughness to the surface of the area where the partial bonding layer is formed in the front plating layer made of Ni, the adhesion with the partial bonding layer (Ag sintered bonding layer) disposed on the front drawing layer of the area where the surface roughness is formed can be increased, which has the advantage of further improving bonding reliability.
[0031] FIG. 1 is a plan view of a ceramic substrate according to an embodiment of the present invention.
[0032] FIG. 2 is a bottom view of a ceramic substrate according to an embodiment of the present invention.
[0033] 3 is a cross-sectional view of a ceramic substrate according to an embodiment of the present invention, viewed along the line A-A' of FIG. 1.
[0034] FIG. 4 is a cross-sectional view illustrating a power module in which a power semiconductor device and a heat dissipation block are bonded to the ceramic substrate of FIG. 2.
[0035] FIG. 5 is a process flowchart for explaining a method for manufacturing a ceramic substrate according to an embodiment of the present invention.
[0036] Hereinafter, preferred embodiments of the present invention will be described in detail.
[0037] In describing the embodiments of the present invention, identical or similar components are assigned the same reference numerals, and redundant descriptions thereof are omitted. Furthermore, detailed descriptions of related prior art are omitted if it is determined that such detailed descriptions could obscure the essence of the embodiments disclosed in this specification.
[0038] In addition, the attached drawings are intended only to facilitate understanding of the embodiments disclosed in this specification, and the technical concept disclosed in this specification is not limited by the attached drawings, and it should be noted that they include all modifications, equivalents, and substitutions that fall within the concept and technical scope of the present invention.
[0039] The embodiments are provided to more fully explain the invention to those skilled in the art, and the following embodiments may be modified in various different forms, and the scope of the invention is not limited to the following embodiments. Rather, these embodiments are provided to make the disclosure more faithful and complete and to fully convey the spirit of the invention.
[0040] The terms used herein are for describing specific embodiments and are not intended to limit the invention. Additionally, the singular form in this specification may include the plural form unless the context clearly indicates otherwise.
[0041] In the description of the embodiments, where each layer (film), region, pattern, or structure is described as being formed "on" or "under" the substrate, each layer (film), region, pad, or pattern, "on" and "under" include both being formed "directly" and "indirectly" through another layer. In addition, the reference for the top or bottom of each layer is, in principle, based on the drawings.
[0042] The drawings are intended solely to facilitate an understanding of the concept of the present invention and should not be interpreted as limiting the scope of the invention. Additionally, relative thicknesses, lengths, or sizes in the drawings may be exaggerated for convenience and clarity of explanation.
[0043] FIG. 1 is a plan view of a ceramic substrate according to an embodiment of the present invention, and FIG. 2 is a bottom view of a ceramic substrate according to an embodiment of the present invention. FIG. 3 is a cross-sectional view of a ceramic substrate according to an embodiment of the present invention viewed along the line A-A' of FIG. 1.
[0044] Referring to FIGS. 1 to 3, a ceramic substrate (100) according to an embodiment of the present invention comprises a ceramic substrate (110), an upper metal layer (120) and a lower metal layer (130) formed respectively on the upper and lower surfaces of the ceramic substrate (110). A first front plating layer (140) and a second front plating layer (150) are formed respectively on the upper metal layer (120) and the lower metal layer (130), and a first partial bonding layer (160) and a second partial bonding layer (170) may be partially formed on the first front plating layer (140) and the second front plating layer (150).
[0045] The ceramic substrate (110) may be composed of an oxide-based or nitride-based ceramic material having high thermal conductivity and excellent flexural strength. For example, the ceramic substrate (110) may be formed from any one of Al2O3, AlN, Si3N4, and ZTA (Zirconia Toughened Alumina). An upper metal layer (120) and a lower metal layer (130) may be formed by brazing metal foils on both sides of the ceramic substrate (110).
[0046] The upper metal layer (120) can be formed into a circuit pattern capable of electrical circuit connection of a mounting component, such as a power semiconductor device (200) or a conductive spacer, by etching or machining. The upper metal layer (120) and the lower metal layer (130) can be made of any one of Cu, a Cu alloy (CuMo, etc.), or Al.
[0047] Brazing bonding may utilize a brazing bonding layer made of a metal material comprising at least one of Ag, AgCu, or AgCuTi. The heat treatment temperature for brazing bonding may be 780 degrees or higher and 900 degrees or lower. This is intended to ensure stable bonding between the ceramic substrate (110) and the metal layer, taking into account temperature conditions that can prevent deformation or oxidation of the metal layer.
[0048] The ceramic substrate (100) may be an Active Metal Brazing (AMB) substrate in which metal layers (120, 130) are bonded to the upper and lower surfaces of a ceramic substrate (110). The AMB substrate has excellent durability and heat dissipation performance, and has the advantage of maintaining stable electrical and mechanical properties even in high-temperature environments. In the embodiment, the AMB substrate is described as a preferred example, but is not limited thereto, and the ceramic substrate (100) may be a Direct Bonding Copper (DBC) substrate.
[0049] Considering that the ceramic substrate (110) constituting the ceramic substrate (100) is applied to a power module operating in a high-temperature environment, the thickness of the ceramic substrate (100) is preferably at least 0.25 mm. In addition, the thickness of the upper metal layer (120) and the lower metal layer (130) bonded to the upper and lower surfaces of the ceramic substrate (110) is preferably at least 0.127 mm to efficiently dissipate heat from the power semiconductor device (200) and to ensure a solid bond with the substrate.
[0050] In the embodiment, a first front plating layer (140) and a second front plating layer (150) may be formed respectively on the upper metal layer (120) and the lower metal layer (130) of the ceramic substrate (100). The first front plating layer (140) may be plated to cover the entire surface of the upper metal layer (120), preferably the entire upper surface of the upper metal layer (120), and the second front plating layer (150) may be plated to cover the entire surface of the lower metal layer (130), preferably the entire lower surface of the lower metal layer (130).
[0051] The first front plating layer (140) and the second front plating layer (150) may be nickel plating layers (hereinafter referred to as 'Ni plating layers'). The Ni plating layer may be formed through an electrolytic plating or electroless plating process using a plating solution containing nickel (Ni). The Ni plating layer not only provides excellent electrical and thermal conductivity but also enables reliable bonding with a partial bonding layer in a subsequent process.
[0052] In particular, nickel (Ni) is a common metal that can ensure economic viability as its plating cost is lower than that of silver (Ag). It can also form a relatively stable oxide film in air, and since the oxide film is thin and stable, it can provide the advantage of not interfering with sintering bonding. In addition, it has higher chemical stability than silver (Ag), making it resistant to sulfidation reactions. When sintered with Ag, Ag particles can form a stable bonding layer by diffusion bonding or mechanical interlocking with the nickel (Ni) surface.
[0053] The first partial bonding layer (160) may be partially formed on the first front plating layer (140) corresponding to the power semiconductor device. Preferably, it may be formed in a portion of the first front plating layer (140) on which the power semiconductor device is mounted, with an area corresponding to the lower surface (bonding surface) of the power semiconductor device. This first partial bonding layer (160) mediates a solid bond between the first front plating layer (140) and the power semiconductor device.
[0054] In the embodiment, the first partial bonding layer (160) may be an Ag sintered bonding layer formed by applying an Ag paste containing silver (Ag) and then firing it. In partially forming an Ag sintered bonding layer on the first front plating layer (140) to correspond to a power semiconductor device, the Ag paste can be precisely formed through a screen printing method in which the Ag paste is applied in a pattern corresponding to the shape or area of the power semiconductor device (200).
[0055] In some cases, an Ag particle-based film may be used as an Ag sintered bonding layer. In this case, an Ag particle-based film having an area corresponding to the area of a power semiconductor device is placed on a first front plating layer (140) at a location where the power semiconductor device is to be mounted, and an Ag sintered bonding layer can be formed by bonding using a sintering bonding method that applies pressure and heat. This film method has an advantage over the paste method in terms of thickness uniformity.
[0056] The first partial bonding layer (160), which is an Ag-based sintered bonding layer, provides high electrical and thermal conductivity, so it can effectively transfer current and heat generated during the operation of a power semiconductor device. In addition, it enables reliable bonding with the power semiconductor device in a subsequent sintering bonding process. In particular, since diffusion between Ag particles is easy, the sintering density is high, and accordingly, a sintered bonding layer with low porosity and excellent bonding strength can be formed.
[0057] A second partial bonding layer (170) may be partially formed on the second front plating layer (150) corresponding to the heat dissipation block. Preferably, it may be formed in a portion of the second front plating layer (150) to which the heat dissipation block is bonded, with an area corresponding to the upper surface (bonding surface) of the heat dissipation block. This second partial bonding layer (170) mediates a strong bond between the second front plating layer (150) and the heat dissipation block.
[0058] In the embodiment, the second partial bonding layer (170) may be an Ag sintered bonding layer formed by applying an Ag paste containing silver (Ag) and then firing it. In partially forming the Ag sintered bonding layer on the second front plating layer (150) to correspond to the heat dissipation block, the Ag paste may be precisely partially formed through a screen printing method in which the Ag paste is applied in a pattern corresponding to the shape or area of the heat dissipation block.
[0059] In some cases, an Ag particle-based film may be used as an Ag sintered bonding layer. In this case, an Ag particle-based film having an area corresponding to the area of the heat dissipation block is placed on the second front plating layer (150) at the location where the heat dissipation block is to be mounted, and an Ag sintered bonding layer can be formed by bonding it using a sintering bonding method that applies pressure and heat. This film method has an advantage over the paste method in terms of thickness uniformity.
[0060] The second partial bonding layer (170) is an Ag-based sintered bonding layer, so it can provide high thermal conductivity. Therefore, it can effectively transfer high-temperature heat generated during the operation of the power semiconductor device to the heat dissipation block. In addition, it enables reliable bonding with the heat dissipation block in the subsequent sintering bonding process. In particular, since diffusion between Ag particles is easy, the sintering density is high, and accordingly, a sintered bonding layer with low porosity and excellent bonding strength can be formed.
[0061] FIG. 4 is a cross-sectional view illustrating a power module in which a power semiconductor device and a heat dissipation block are bonded to the ceramic substrate of FIG. 2.
[0062] Referring to FIG. 4, the power module (1) includes a power semiconductor device (200) mounted on an upper metal layer (120) of a ceramic substrate (100) and a heat dissipation block (300) bonded to a lower metal layer (130) of a ceramic substrate (100). As an example, the power semiconductor device (200) may be SiC, GaN, IGBT, etc., and the heat dissipation block (300) may be a spacer or a heat sink that is relatively larger in volume than such a spacer.
[0063] A first front plating layer (140) is formed to cover the entire surface of the upper metal layer (120) (the upper surface of the upper metal layer in the drawing), and a first partial bonding layer (160) may be partially formed on the upper surface of the first front plating layer (140). The first partial bonding layer (160) mediates a stable and robust bond between the first front plating layer (140) and the power semiconductor device (200).
[0064] The first partial bonding layer (160) may be an Ag sintered bonding layer containing silver (Ag). Ag sintered paste has the characteristic of providing high electrical and thermal conductivity and bonding strength even at high temperatures.
[0065] Power modules operate in high-temperature environments due to their characteristics. Therefore, it is difficult to maintain bonding characteristics and secure sufficient bonding strength using conventional low-melting-point solder. On the other hand, the Ag sintered bonding layer has high high-temperature safety and excellent bonding strength because the melting point of the sintered material rises to 700 degrees or higher after bonding. Therefore, it is preferable to use a paste containing Ag particles or an Ag particle-based film as the Ag sintered bonding layer for the first partial bonding layer (160).
[0066] The first front plating layer (140) is preferably formed as a Ni plating layer when considering the bonding strength with the Ag-based first partial bonding layer (160) and the manufacturing cost. The Ni plating layer can be formed through an electrolytic plating or electroless plating process using a plating solution containing nickel (Ni). The Ni plating layer not only provides excellent electrical and thermal conductivity but also ensures interfacial bonding reliability with the Ag-based partial bonding layer during a subsequent sintering process.
[0067] In some cases, the first full-surface plating layer (140) may be formed with a nickel (Ni)-based alloy capable of stable bonding with silver (Ag) when considering inter-material interaction characteristics such as interfacial reaction, diffusion characteristics, mutual solubility, and chemical stability. For example, the first full-surface plating layer (140) may be formed by applying a metal alloy such as Ni-Ag.
[0068] The area where the first partial bonding layer (160) is formed in the first front plating layer (140) may be given roughness with a specific surface roughness. Here, surface roughness refers to the degree of fine irregularities formed on the surface of the first front plating layer (140) where the first partial bonding layer (160) is formed, and can be expressed by parameters such as arithmetic mean roughness (Ra), maximum roughness height (Rmax), and maximum height roughness (Rz).
[0069] In the embodiment, the surface roughness of the first front plating layer (140) may be Ra 0.3㎛ or more and 2.0㎛ or less, Rz 3㎛ or more and 8㎛ or less, and Rmax 5㎛ or more and 15㎛ or less. If Ra is less than 0.3㎛, the surface of the first front plating layer (140) may be excessively smooth, which may reduce adhesion with the Ag sintered bonding layer. Conversely, if Ra exceeds 2.0㎛, the surface may become excessively rough, which may cause a problem where the Ag sintered bonding layer does not adhere locally.
[0070] Accordingly, considering the stable and robust bonding with the first partial bonding layer (160), which is an Ag sintered bonding layer, the surface roughness of the area where the first partial bonding layer (160) is formed in the first full-surface plating layer (140) is preferably 0.3㎛ or more and 2.0㎛ or less based on Ra, which represents the arithmetic mean roughness. At this time, when the Ra value is 0.3㎛ or more and 2.0㎛ or less, the corresponding Rz value may be 3㎛ or more and 8㎛ or less, and the Rmax value may be 5㎛ or more and 15㎛.
[0071] In the embodiment, the thickness of the first front plating layer (140) is preferably 0.1 μm or more and 1.0 μm or less. If the thickness of the first front plating layer (140) is too thin, less than 0.1 μm, it is difficult to impart surface roughness to a part of the first front plating layer (140) (a part where the first partial bonding layer is formed), and if the thickness of the first front plating layer (140) exceeds 1.0 μm, the process time for forming the first front plating layer (140) becomes longer, which may reduce mass production efficiency.
[0072] If the first front plating layer (140) is formed only on a portion of the upper metal layer (120) rather than on the front surface, the remaining surface of the upper metal layer (120) where the plating layer is not formed is exposed to the air. In particular, if the upper metal layer (120) is copper (Cu), the surface is prone to oxidation due to the copper's characteristic of reacting with oxygen in the air, and the copper oxide film is not as dense or hard as the nickel (Ni) oxide film, but is loose and uneven, so it cannot effectively prevent further oxidation.
[0073] On the other hand, if a first front plating layer (140) based on Ni is formed to cover the entire surface of the upper metal layer (120), oxidation can be effectively suppressed because the surface of the upper metal layer (120) is not directly exposed to air. In particular, nickel (Ni) has the advantage of being cheaper than silver (Ag) because the oxide film formed on the surface is denser and more stable compared to copper (Cu), which is advantageous for blocking further oxidation, and the oxide film formed on the surface is denser and more stable.
[0074] The power semiconductor device (200) can maintain a robust and highly reliable bonding state by being sintered and bonded to the first front plating layer (140) through the first partial bonding layer (Ag sintered bonding layer, 160). This bonding structure enables excellent interfacial stability and electrical characteristics to be secured even in high temperature and high current environments. Here, the sintering temperature for sintering bonding is preferably about 250°C or higher and 350°C or lower, considering the sintering characteristics of the Ag paste or Ag particle-based film.
[0075] A second front plating layer (150) is formed on the lower metal layer (130) to cover the entire surface (the lower surface of the lower metal layer in the drawing), and a second partial bonding layer (170) may be partially formed on the lower surface of the second front plating layer (150). The second front plating layer (150) may be formed with a thickness of 0.1 μm or more and 1.0 μm or less through electrolytic plating or electroless plating, and the second partial bonding layer (170) may be formed in a portion of the lower metal layer (130) where the heat dissipation block (300) is bonded.
[0076] The second partial bonding layer (170) may be an Ag sintered bonding layer, similar to the first partial bonding layer (160) described above which contains silver (Ag), and the second full plating layer (150) is preferably formed as a Ni plating layer when considering the bonding strength and manufacturing cost with the Ag-based second partial bonding layer (170). The Ni plating layer not only provides excellent electrical and thermal conductivity, but also ensures interfacial bonding reliability with the Ag-based partial bonding layer during the subsequent sintering process.
[0077] In some cases, a second full-surface plating layer (150) may be formed with a nickel (Ni)-based alloy capable of stable bonding with silver (Ag), considering inter-material interaction characteristics such as interfacial reaction, diffusion characteristics, mutual solubility, and chemical stability. For example, a metal alloy such as Ni-Ag may be applied to form the second full-surface plating layer (150).
[0078] The area where the second partial bonding layer (170) is formed in the second full-face plating layer (150) may be given roughness with a specific surface roughness. Here, surface roughness refers to the degree of fine irregularities formed on the surface of the second full-face plating layer (150) where the second partial bonding layer (170) is formed, and can be expressed by parameters such as arithmetic mean roughness (Ra), maximum roughness height (Rmax), and maximum height roughness (Rz).
[0079] In the embodiment, the surface roughness of the second front plating layer (150) may be Ra 0.3㎛ or more and 2.0㎛ or less, Rz 3㎛ or more and 8㎛ or less, and Rmax 5㎛ or more and 15㎛ or less. If Ra is less than 0.3㎛, the surface of the second front plating layer (150) may be excessively smooth, which may reduce adhesion with the Ag sintered bonding layer. Conversely, if Ra exceeds 2.0㎛, the surface may become excessively rough, which may cause a problem where the Ag sintered bonding layer does not adhere locally.
[0080] Accordingly, considering the stable and robust bonding with the second partial bonding layer (170), which is an Ag sintered bonding layer, the surface roughness of the area where the second partial bonding layer (170) is formed in the second full-surface plating layer (150) is preferably 0.3㎛ or more and 2.0㎛ or less based on Ra, which represents the arithmetic mean roughness. At this time, when the Ra value is 0.3㎛ or more and 2.0㎛ or less, the corresponding Rz value may be 3㎛ or more and 8㎛ or less, and the Rmax value may be 5㎛ or more and 15㎛.
[0081] When a second front plating layer (150) based on Ni is formed to cover the entire surface of the lower metal layer (130), the surface of the lower metal layer (130) is prevented from being directly exposed to air, so oxidation can be effectively suppressed. In particular, nickel (Ni) has the advantage of being cheaper than silver (Ag) because the oxide film formed on the surface is denser and more stable compared to copper (Cu), which is advantageous for blocking further oxidation, and the oxide film formed on the surface is more dense and stable.
[0082] The heat dissipation block (300) can maintain a robust and highly reliable bonded state by being sintered and bonded to the second front plating layer (150) through the second partial bonding layer (Ag sintered bonding layer, 170). This bonding structure ensures excellent interfacial stability and electrical characteristics even in high temperature and high current environments. Here, considering the sintering characteristics of the Ag paste or Ag particle-based film, the sintering temperature for the sintered bonding is preferably about 250 degrees or higher and 350 degrees or lower.
[0083] Meanwhile, a brazing filler (not shown) is used for brazing bonding between the ceramic substrate (110) and the upper and lower metal layers (120, 130). The brazing filler is placed between the ceramic substrate (110) and the upper metal layer (120) and between the ceramic substrate (110) and the lower metal layer (130), respectively, to facilitate strong thermal and mechanical bonding between them. The brazing filler can be formed on the surface of the ceramic substrate (110) by various methods such as paste application, foil attachment, or electroless plating.
[0084] For example, the brazing filler may be composed of an Ag alloy containing Ag. Preferably, it may be made of an Ag-Cu alloy. Since the Ag-Cu alloy has a high level of thermal conductivity, it can maximize heat dissipation performance in the power module when high heat is present. The Ag-Cu alloy can also maximize bonding strength while preserving the structural properties of the ceramic substrate (110) due to its characteristics.
[0085] In particular, Ag has strong oxidation resistance, maintaining a stable state at high temperatures, and can contribute to maintaining stable bonding quality by suppressing oxide formation during the bonding process. Ag also has excellent wettability with metals or ceramics at specific brazing temperatures (generally 600 to 900 degrees), allowing it to spread uniformly across the bonding surface to form a solid bonding layer.
[0086] An Ag-based first partial bonding layer (160) is formed between the first front plating layer (140) of the ceramic substrate (100) and the power semiconductor device (200), and an Ag-based second partial bonding layer (170) is also disposed between the second front plating layer (150) and the heat dissipation block (300). According to an embodiment, the first partial bonding layer (160) and the second partial bonding layer (170) may be composed of an Ag alloy sintered material. Preferably, they may be composed of an Ag-Cu alloy sintered material, similar to a brazing filler.
[0087] Ag alloys have the characteristic that the higher the Ag content, the lower the effective melting point. A lower effective melting point allows joining to be performed at a lower temperature. Therefore, if an Ag alloy with a higher Ag content than the brazing filler (a joining layer that joins the ceramic substrate and the upper and lower metal layers) which is the primary brazing agent in the process is used as the secondary joining layer (first partial joining layer and second partial joining layer), the temperature of the secondary joining process can be lowered compared to the primary joining.
[0088] If the temperature of the secondary bonding process is lowered, the deformation caused by thermal expansion of the ceramic substrate (100) is reduced, thereby reducing thermal stress. Additionally, if the temperature of the secondary bonding process is set lower than the liquidus temperature of the brazing filler alloy composition, the brazing filler is not remelted, so the bonding state can be maintained stably, and the problem of layer separation (separation between the ceramic substrate and the metal layer) due to remelting can also be reliably prevented.
[0089] As a preferred example, the brazing filler may be formed of an Ag-Cu alloy with a composition ratio of Ag to Cu of 5:5, and the first partial bonding layer (160) and the second partial bonding layer (170) may be sintered Ag-Cu alloy bonding layers with a composition ratio of Ag to Cu of 7:3. As another preferred example, the brazing filler may be an Ag-Cu alloy with a composition ratio of Ag to Cu of 6:4, and the first partial bonding layer (160) and the second partial bonding layer (170) may be sintered Ag-Cu alloy bonding layers with a composition ratio of Ag to Cu of 7:3.
[0090] When an Ag-Cu alloy with an Ag-Cu composition ratio of 5:5 is used as a brazing filler for primary brazing (bonding between a ceramic substrate and a metal layer), brazing is possible at approximately 890 degrees on the binary eutectic phase diagram of the Ag-Cu alloy. In the case of an Ag-Cu alloy with an Ag-Cu composition ratio of 6:4, brazing is possible at approximately 850 degrees.
[0091] On the other hand, in the case of an Ag-Cu alloy with an Ag-to-Cu composition ratio of 7:3, sintering bonding is possible at approximately 780 degrees. Therefore, if an Ag-Cu alloy with an Ag-to-Cu composition ratio of 7:3 is used as a bonding layer for secondary sintering bonding (bonding between the first partial bonding layer and the power semiconductor device, and bonding between the second partial bonding layer and the heat dissipation block), bonding can be performed at a temperature approximately 70 to 110 degrees lower than the primary brazing bonding temperature of a 5:5 or 6:4 composition.
[0092] Since the brazing filler is used for bonding between the ceramic substrate (110) and the upper and lower metal layers (120, 130), mechanical strength and heat resistance are important, and since the first partial bonding layer (160) and the second partial bonding layer (170) are used for bonding the power semiconductor device (200) and the heat dissipation block (300) to the front plating layer (140, 150), relatively high thermal conductivity and low bonding temperature are more important.
[0093] Therefore, adjusting the bonding characteristics by increasing the Ag content of the first partial bonding layer (160) and the second partial bonding layer (170) corresponding to the second bonding layer can be considered an effective design strategy to lower the bonding temperature and improve thermal conductivity to optimize overall heat dissipation performance.
[0094] FIG. 5 is a process flowchart for explaining a method for manufacturing a ceramic substrate according to an embodiment of the present invention. For convenience of explanation, the configurations shown in the preceding attached drawings will be described by referring to the corresponding reference numerals.
[0095] Referring to FIG. 5 and the preceding drawings together, a method for manufacturing a ceramic substrate according to an embodiment comprises the steps of: forming an upper metal layer (120) on the upper surface of a ceramic substrate (110) and forming a lower metal layer (130) on the lower surface (S100); forming a first front plating layer (140) to cover the entire surface of the upper metal layer (120) and forming a second front plating layer (150) to cover the entire surface of the lower metal layer (130) (S200); and partially forming a first partial bonding layer (160) on the first front plating layer (140) (S300).
[0096] In step S100, the upper metal layer (120) and the lower metal layer (130) can be bonded to the ceramic substrate (110) through a brazing process. More specifically, a brazing filler can be placed between the metal layers (120, 130) and the ceramic substrate (110), respectively, and brazing can be performed at a temperature between 800 and 900 degrees to form the upper metal layer (120) and the lower metal layer (130), respectively, on the upper and lower surfaces of the ceramic substrate (110). Here, the metal layers (120, 130) may be made of Cu, Cu alloy, Al, etc.
[0097] In step S200, the first front plating layer (140) and the second front plating layer (150) may be Ni plating layers. The Ni plating layer can be formed through an electrolytic plating or electroless plating process using a plating solution containing nickel (Ni). Additionally, it can be formed through physical vapor deposition (PVD), which involves vaporizing a metal under vacuum conditions and depositing it onto the surface of a metal layer. However, electrolytic plating or electroless plating has the advantage of allowing for precise control of the plating thickness.
[0098] In step S300, the first partial bonding layer (160) can be formed in a portion of the first front plating layer (140) where the power semiconductor device (200) is mounted, with an area corresponding to the lower surface (bonding surface) of the power semiconductor device (200). In the embodiment, the first partial bonding layer (160) may be an Ag sintered bonding layer formed by partially applying Ag paste to the area where the power semiconductor device (200) is to be mounted using a screen printing method or the like, and then sintering the result.
[0099] In some cases, an Ag particle-based film may be used as the first partial bonding layer (160). In this case, an Ag particle-based film having an area corresponding to the area of the power semiconductor device (200) may be placed on the first front plating layer (140) at the location where the power semiconductor device (200) is to be mounted, and an Ag sintered bonding layer may be formed by bonding using a sintering bonding method that applies pressure and heat.
[0100] According to an embodiment, a step (S250) of applying roughness to a specific surface roughness in the area where the first partial bonding layer (160) is formed in the first full-face plating layer (140) may be added. This step of applying roughness (S250) may be performed between step S200 and step S300. Here, surface roughness refers to the degree of fine irregularities formed on the surface of the first full-face plating layer (140) where the first partial bonding layer (160) is formed.
[0101] In step S250, the surface roughness of the first front plating layer (140) can be formed as Ra 0.3㎛ or more and 2.0㎛ or less, Rz 3㎛ or more and 8㎛ or less, and Rmax 5㎛ or more and 15㎛ or less. If Ra is less than 0.3㎛, the surface of the first front plating layer (140) may be excessively smooth, which may reduce adhesion with the Ag sintered bonding layer. Conversely, if Ra exceeds 2.0㎛, the surface may become excessively rough, which may cause a problem where the Ag sintered bonding layer does not adhere locally.
[0102] In step S250, surface roughness can be imparted to the surface of the first front plating layer (140) (the part where the first partial bonding layer is formed) through, for example, chemical etching, sputtering, laser processing, etc.
[0103] In the preceding S200 step, the thickness of the first front plating layer (140) is preferably 0.1 μm or more and 1.0 μm or less. This is because if the thickness of the first front plating layer (140) is too thin (less than 0.1 μm), it is difficult to impart surface roughness to the surface of the first front plating layer (140) where the first partial bonding layer (160) is formed in the S250 step, and if the thickness exceeds 1.0 μm, the process time for forming the first front plating layer (140) becomes longer, which may reduce mass production efficiency.
[0104] The method for manufacturing a ceramic substrate according to the embodiment may further include the step (S400) of forming a second partial bonding layer (170) on the second front plating layer (150). The second partial bonding layer (170) may be formed through the same process as in step S300. That is, the second partial bonding layer (170) may be formed by applying Ag paste to a portion of the second front plating layer (150) where the heat dissipation block (300) is bonded, with an area corresponding to the upper surface (bonding surface) of the heat dissipation block (300), and then drying and firing the result.
[0105] Although the process flowchart of FIG. 5 illustrates the S400 step being performed after the S300 step, the S300 and S400 steps do not necessarily have to be performed sequentially, and the order of execution may be changed. That is, it is acceptable to perform the S400 step first and the S300 step second; therefore, it should be noted that such a change in the chronological order is also included within the scope of the technical concept of the present invention.
[0106] According to an embodiment, a step (S350) of applying roughness to a specific surface roughness in the area where the second partial bonding layer (170) is formed in the second full-face plating layer (150) may be added. This step of applying roughness (S350) may be performed between step S200 and step S400. Here, surface roughness refers to the degree of fine irregularities formed on the surface of the second full-face plating layer (150) where the second partial bonding layer (170) is formed.
[0107] In step S350, the surface roughness of the second front plating layer (150) can be formed as Ra 0.3㎛ or more and 2.0㎛ or less, Rz 3㎛ or more and 8㎛ or less, and Rmax 5㎛ or more and 15㎛ or less. If Ra is less than 0.3㎛, the surface of the second front plating layer may be excessively smooth, which may reduce adhesion with the Ag sintered bonding layer. Conversely, if Ra exceeds 2.0㎛, the surface may become excessively rough, which may cause a problem where the Ag sintered bonding layer does not adhere locally.
[0108] In step S350, surface roughness can be imparted to the surface of the second front plating layer (150) (the part where the second partial bonding layer is formed) through, for example, chemical etching, sputtering, laser processing, etc.
[0109] In the preceding S200 step, the thickness of the second front plating layer (150) is preferably 0.1㎛ or more and 1.0㎛ or less. This is because if the thickness of the second front plating layer (150) is too thin (less than 0.1㎛), it is difficult to impart surface roughness to the surface of the second front plating layer (150) where the second partial bonding layer (170) is formed in the S350 step, and if the thickness exceeds 1.0㎛, the process time for forming the second front plating layer (150) becomes longer, which may reduce mass production efficiency.
[0110] According to the present invention described above, instead of plating high-cost silver (Ag) on a copper electrode, nickel (Ni) is plated on the entire surface, and then a power semiconductor device is bonded to the said Ni plating layer using an Ag sintering method, thereby reducing manufacturing costs and improving the economic efficiency of the process. In the case of the nickel plating layer, the interfacial stability and oxidation resistance are excellent, so bonding strength and reliability with the Ag sintered material can be secured.
[0111] In addition, defects such as electrical short circuits caused by silver migration, which can occur in full Ag plating methods, can be effectively prevented. Accordingly, this provides a useful technical means to simultaneously improve the structural stability and lifespan characteristics of power modules that require operational reliability in high-temperature environments.
[0112] In addition, by imparting a specific degree of roughness to the surface of the area where the partial bonding layer is formed in the front plating layer made of Ni, the adhesion with the partial bonding layer (Ag sintered bonding layer) disposed on the front drawing layer of the area where the surface roughness is formed can be increased, which has the advantage of further improving bonding reliability.
[0113] The above description is merely an illustrative explanation of the technical concept of the present invention, and those skilled in the art to which the present invention pertains will be able to make various modifications and variations within the scope of the essential characteristics of the present invention.
[0114] Accordingly, the embodiments disclosed in this invention are intended to illustrate, not limit, the technical concept of the invention, and the scope of the technical concept of the invention is not limited by these embodiments. The scope of protection of this invention shall be interpreted by the claims below, and all technical concepts within an equivalent scope shall be interpreted as being included within the scope of rights of this invention.
Claims
1. A ceramic substrate for a power module on which a power semiconductor device is mounted, Ceramic substrate; An upper metal layer and a lower metal layer formed respectively on the upper and lower surfaces of the ceramic substrate; A first front plating layer and a second front plating layer plated to cover the entire surface of the upper metal layer and the lower metal layer; and A first partial junction layer partially formed on the first front plating layer and mediating junction between the first front plating layer and a power semiconductor device; comprising The first front plating layer and the second front plating layer are nickel (Ni) plating layers, and A ceramic substrate characterized in that the first partial bonding layer is an Ag sintered bonding layer containing silver (Ag).
2. In Paragraph 1, A ceramic substrate characterized in that the surface roughness of the region where the first partial bonding layer is formed in the first front plating layer is Ra 0.3㎛ or more and 2.0㎛ or less, Rz 3㎛ or more and 8㎛ or less, and Rmax 5㎛ or more and 15㎛ or less.
3. In Paragraph 1, A ceramic substrate characterized in that the thickness of the first partial bonding layer is 0.1㎛ or more and 1.0㎛ or less.
4. In Paragraph 1, It further includes a second partial bonding layer that mediates bonding between the second front plating layer and the heat dissipation block; A ceramic substrate characterized in that the second partial bonding layer is partially formed on the second front plating layer corresponding to the heat dissipation block.
5. In Paragraph 4, A ceramic substrate characterized in that the surface roughness of the region where the second partial bonding layer is formed in the second front plating layer is Ra 0.3㎛ or more and 2.0㎛ or less, Rz 3㎛ or more and 8㎛ or less, and Rmax 5㎛ or more and 15㎛ or less.
6. In Paragraph 4, A ceramic substrate characterized in that the thickness of the second partial bonding layer is 0.1㎛ or more and 1.0㎛ or less.
7. In Paragraph 4, A ceramic substrate characterized in that the second partial bonding layer is an Ag sintered bonding layer containing silver (Ag).
8. A ceramic substrate having an upper metal layer formed on the upper surface and a lower metal layer formed on the lower surface; A power semiconductor device mounted on an upper metal layer of the ceramic substrate; and A heat dissipation block bonded to the lower metal layer of the ceramic substrate; comprising A first front plating layer is formed to cover the entire surface of the upper metal layer on the ceramic substrate, and a second front plating layer is formed to cover the entire surface of the lower metal layer. A first partial bonding layer is partially formed on the first front plating layer in correspondence with the above power semiconductor device, and The above first front plating layer and second front plating layer are nickel (Ni) plating layers, and A power module characterized in that the first partial bonding layer is an Ag sintered bonding layer containing silver (Ag).
9. In Paragraph 8, A power module characterized by the surface roughness of the region where the first partial bonding layer is formed in the first front plating layer being Ra 0.3㎛ or more and 2.0㎛ or less, Rz 3㎛ or more and 8㎛ or less, and Rmax 5㎛ or more and 15㎛ or less.
10. In Paragraph 8, A power module characterized in that the thickness of the first partial bonding layer is 0.1㎛ or more and 1.0㎛ or less.
11. In Paragraph 8, It further includes a second partial bonding layer formed on the second front plating layer; A power module characterized in that the second partial bonding layer is formed in a portion of the second front plating layer where the heat dissipation block is bonded.
12. In Paragraph 11, A power module characterized by the surface roughness of the region where the second partial bonding layer is formed in the second front plating layer being Ra 0.3㎛ or more and 2.0㎛ or less, Rz 3㎛ or more and 8㎛ or less, and Rmax 5㎛ or more and 15㎛ or less.
13. In Paragraph 11, A power module characterized in that the thickness of the second partial bonding layer is 0.1㎛ or more and 1.0㎛ or less.
14. In Paragraph 11, A power module characterized in that the second partial bonding layer is an Ag sintered bonding layer containing silver (Ag).
15. A method for manufacturing a ceramic substrate for a power module, A step of forming an upper metal layer on the upper surface of a ceramic substrate and forming a lower metal layer on the lower surface; A step of forming a first front plating layer to cover the entire surface of the upper metal layer and forming a second front plating layer to cover the entire surface of the lower metal layer; and The method includes the step of partially forming a first partial junction layer on the first front plating layer to correspond to a power semiconductor device; The first front plating layer and the second front plating layer are formed of nickel (Ni), and A method for manufacturing a ceramic substrate characterized by forming the first partial bonding layer with Ag sintering paste.
16. In Paragraph 15, The step of forming the first front plating layer and the second front plating layer is A method for manufacturing a ceramic substrate characterized by forming a nickel plating layer through electroplating or electroless plating.
17. In Paragraph 15, The step of partially forming the first partial bonding layer is, A method for manufacturing a ceramic substrate characterized by forming the first partial bonding layer in the upper metal layer with an area corresponding to the lower surface of the power semiconductor device in a portion of the region where the power semiconductor device is mounted.
18. In Paragraph 15, The method further includes the step of forming a second partial bonding layer on the second front plating layer; In the step of forming the second partial bonding layer, A method for manufacturing a ceramic substrate characterized by forming the second partial bonding layer in a portion of the area where a heat dissipation block is bonded to the second front plating layer.
19. In Paragraph 18, A method for manufacturing a ceramic substrate characterized by forming the second partial bonding layer with Ag sintered paste.