Powder metallurgical method for preparing tungsten-chromium-based composite
A tungsten-chromium composite with a dual-phase structure is manufactured through a powder metallurgical process, addressing the limitations of pure tungsten by enhancing oxidation resistance and ductility, thus maintaining structural integrity in high-temperature environments.
Patent Information
- Application Number
- PCT/KR2026/096249
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2026-02-25
- Filing Date
- 2026-04-23
- Publication Date
- 2026-11-19
AI Technical Summary
Existing tungsten materials used in high-temperature environments, such as fusion reactors, suffer from poor oxidation resistance, ductility, and a high ductile-brittle transition temperature (DBTT), making them brittle and prone to cracking.
A powder metallurgical method involving mixing tungsten and chromium powders to form a core-shell composite, followed by hydrogen reduction and spark plasma sintering, creating a tungsten-chromium composite with a dual-phase structure that includes a chromium matrix and dispersed tungsten particles.
The composite exhibits improved oxidation resistance, high strength, and ductility, maintaining structural integrity in extreme conditions, reducing the DBTT and preventing crack propagation.
Smart Images

Figure KR2026096249_19112026_PF_FP_ABST
Abstract
Description
Powder metallurgical manufacturing method of tungsten-chromium-based composites
[0001] The present invention relates to composite materials, a method for manufacturing the same, and applications thereof, and more specifically, to a method for manufacturing intermetallic composites and applications thereof.
[0002] The Korean national research and development projects that supported this invention are as follows:
[0003] Project Unique Number 2710017863
[0004] Assignment No. 00445448
[0005] Ministry of Science and ICT
[0006] Project Management (Specialized) Agency Name: National Research Foundation of Korea
[0007] Research Project Name: Original Technology Development Project
[0008] Research Project Title: Development of High-Toughness Tungsten-Based Face-to-Face Materials with Excellent Plasma Resistance for Fusion Reactors
[0009] Name of Project Executing Organization: Seoul National University Industry-Academic Cooperation Foundation
[0010] Research Period: July 1, 2024 – December 31, 2028
[0011] Project unique number not assigned
[0012] Project No. 2026-RISE-01-016-01
[0013] Ministry of Education
[0014] Project Management (Specialized) Agency Name: Seoul RISE Center
[0015] Research Project Name: Seoul Metropolitan Government Regional Innovation-Centered University Support System (RISE)
[0016] Research Project Title: Seoul National University Regional Innovation-Centered University Support System (RISE)_Leading Global Industry-Academic Cooperation
[0017] Project Implementing Organization Name: Seoul National University (RISE Project Group)
[0018] Research Period: June 1, 2025 – August 31, 2026
[0019] Plasma-facing component (PFC) technology is a core technology for designing, manufacturing, and operating materials and structures with excellent heat resistance, corrosion resistance, and wear resistance to protect equipment (such as fusion reactors and semiconductor equipment) and maximize performance in high-temperature (ultra-high-temperature) plasma environments. PFCs are critical materials and components directly exposed to high-temperature plasmas exceeding thousands of degrees Celsius within fusion devices or semiconductor etching / deposition equipment. High-melting-point metals such as tungsten (W) are primarily used to withstand extreme thermal loads and particle collisions, and active research and development, including thermal and particle load testing and internal cooling structures, is currently underway. In particular, with the construction of the International Thermonuclear Experimental Reactor (ITER) and the technological advancements of private fusion companies, the advancement of tungsten-based materials capable of withstanding high-temperature and high-heat loads and the introduction of liquid metal technology are becoming key issues.
[0020] Most next-generation tokamaks, including the International Thermonuclear Experimental Reactor (ITER), adopt tungsten as a core material due to its high melting point and low sputtering yield. Tungsten possesses advantages such as a high melting point (3422°C), high hardness, high thermal conductivity, a low erosion rate, and low deuterium adsorption capacity. However, major challenges include a relatively high ductile-brittle transition temperature (DBTT), increased brittleness caused by deuterium / neutron exposure / irradiation, fuzzy phenomena resulting from interaction with plasma, and surface melting at high temperatures. Additionally, materials composed of pure tungsten have the disadvantage of relatively poor ductility and difficulty in securing oxidation resistance under harsh conditions.
[0021] Therefore, there is a need to develop materials (composites) that have superior oxidation resistance and improved ductile-brittle transition temperature (DBTT) characteristics compared to existing tungsten materials. In addition, there is a need to secure manufacturing technology for materials (composites) that can have excellent oxidation resistance while possessing high strength and high ductility characteristics.
[0022] The technical problem that the present invention aims to solve is to provide a powder metallurgical method for manufacturing an intermetallic composite material that has superior oxidation resistance and improved ductile-brittle transition temperature (DBTT) characteristics compared to existing tungsten materials.
[0023] Furthermore, the technical problem that the present invention aims to solve is to provide a powder metallurgical manufacturing method for an intermetallic composite material having high strength and high ductility characteristics while also possessing excellent oxidation resistance.
[0024] In addition, the technical problem that the present invention aims to solve is to provide an intermetallic composite material manufactured by the above-described method.
[0025] The problems that the present invention aims to solve are not limited to those mentioned above, and other unmentioned problems will be understood by those skilled in the art from the description below.
[0026] According to one embodiment of the present invention, a method for manufacturing a tungsten-chromium-based composite is provided, comprising: a step of mixing a tungsten powder composed of a plurality of tungsten (W) particles and a chromium powder composed of a plurality of chromium (Cr) particles by a milling method to form a core-shell based composite powder comprising a plurality of core-shell particles having a core particle portion composed of tungsten and a shell portion composed of chromium covering the surface of the core particle portion; a step of heat-treating the core-shell based composite powder in an atmosphere containing hydrogen (H2) to perform a hydrogen (H2) reduction treatment to form a core-shell based composite powder that has been reduced; and a step of sintering the core-shell based composite powder that has been reduced to form a tungsten-chromium-based composite comprising a matrix composed of chromium or containing chromium as a main material and a plurality of embedded particles composed of tungsten or containing tungsten as a main material, which are embedded and distributed within the matrix at least partially spaced apart from each other.
[0027] The ratio (A / B) between the -3σ particle size (A) of the tungsten powder and the +3σ particle size (B) of the chromium powder may be greater than 3, where σ represents the standard deviation.
[0028] The average particle size of the above tungsten powder may be about 150 μm or less.
[0029] In the total amount of the tungsten powder and the chromium powder, the content of the tungsten powder may be about 60 to 90 wt%, and the content of the chromium powder may be about 10 to 40 wt%.
[0030] The above milling can be performed for about 30 minutes or more under conditions of about 200 to 8000 rpm without using milling balls.
[0031] The heat treatment for the above hydrogen (H2) reduction treatment can be performed at a temperature in the range of about 700 to 1500°C.
[0032] Before the step of forming the core-shell based composite powder, a step of pre-treating at least one of the tungsten powder and the chromium powder may be further performed, and the pre-treatment step may include a step of heat-treating at least one of the tungsten powder and the chromium powder so that hydrogen (H2) reduction treatment is performed in an atmosphere containing hydrogen (H2).
[0033] The above sintering can be performed using the spark plasma sintering (SPS) method.
[0034] The above discharge plasma sintering (SPS) method sintering can be performed in an atmosphere containing hydrogen (H2) at a temperature of about 800 to 1800°C and a pressure of about 200 MPa or less.
[0035] The above tungsten-chromium based composite can have a relative density of about 90% or more.
[0036] In the above tungsten-chromium-based composite, the content of the matrix may be about 10 to 40 wt%, and the content of the plurality of embedded particles may be about 60 to 90 wt%.
[0037] According to another embodiment of the present invention, a tungsten-chromium based composite material manufactured using the method described above is provided.
[0038] According to embodiments of the present invention, a powder metallurgical method for manufacturing an intermetallic composite material can be realized that has excellent oxidation resistance and improved ductile-brittle transition temperature (DBTT) characteristics compared to conventional tungsten materials. Furthermore, according to embodiments of the present invention, a powder metallurgical method for manufacturing an intermetallic composite material that has excellent oxidation resistance while possessing high strength and high ductility characteristics can be realized.
[0039] According to one embodiment of the present invention, a composite powder having a core-shell particle structure is prepared using a high-energy milling method, and a dual-phase composite material having tungsten (W) particles distributed within a chromium (Cr) matrix can be easily prepared therefrom by spark plasma sintering (SPS). The composite material can have excellent strength and ductility characteristics while having a relatively low ductile-brittle transition temperature (DBTT), and can also have high relative density and excellent oxidation resistance.
[0040] Therefore, the composite material manufactured according to the embodiment can maintain ductility in high-temperature, high-heat, and high-particle-flux environments such as a fusion reactor, and effectively prevent the occurrence and propagation of cracks. In addition, the composite material manufactured according to the embodiment is expected to maintain material stability even in ultra-high temperature and oxygen exposure environments of fusion reactor accident scenarios.
[0041] However, the effects of the present invention are not limited to the above effects and can be extended in various ways without departing from the technical concept and scope of the present invention.
[0042] FIG. 1 is a flowchart illustrating a powder metallurgical manufacturing method of a tungsten (W)-chromium (Cr)-based composite according to one embodiment of the present invention.
[0043] FIG. 2 is a schematic diagram of a process for explaining a powder metallurgical manufacturing method of a tungsten-chromium-based composite according to one embodiment of the present invention.
[0044] FIG. 3 is a scanning electron microscope (SEM) image exemplarily showing tungsten powder and chromium powder that can be applied to a method for manufacturing a tungsten-chromium-based composite according to one embodiment of the present invention.
[0045] FIG. 4 is an SEM image exemplarily showing a core-shell powder that can be formed in a method for manufacturing a tungsten-chromium-based composite according to one embodiment of the present invention.
[0046] FIG. 5 is a graph exemplarily showing the particle size distribution of tungsten powder that can be applied to a method for manufacturing a tungsten-chromium-based composite according to one embodiment of the present invention.
[0047] FIG. 6 is a graph exemplarily showing the particle size distribution of chromium powder that can be applied to a method for manufacturing a tungsten-chromium-based composite according to one embodiment of the present invention.
[0048] FIG. 7 is a graph showing a binary phase diagram between tungsten (W) and chromium (Cr) that can be applied to the manufacture of a composite material according to one embodiment of the present invention.
[0049] FIG. 8 is an SEM image showing a core-shell based composite powder formed through mechanical milling and a tungsten-chromium based composite material manufactured from the core-shell based composite powder by discharge plasma sintering (SPS) according to one embodiment of the present invention.
[0050] Figure 9 is an SEM image according to a comparative example, showing a composite powder formed through mechanical milling and a composite material manufactured from the composite powder by discharge plasma sintering (SPS).
[0051] FIG. 10 is an SEM image showing a tungsten-chromium based composite material manufactured according to one embodiment of the present invention.
[0052] FIG. 11 is an SEM cross-sectional image showing a tungsten-chromium-based composite material manufactured according to one embodiment of the present invention.
[0053] Figure 12 is an SEM image showing a tungsten-chromium-based composite prepared according to a comparative example.
[0054] FIG. 13 is an SEM image showing a tungsten-chromium-based composite material manufactured according to one embodiment of the present invention.
[0055] FIG. 14 is a graph showing the results of a three-point bending test to evaluate the toughness of a material according to an embodiment and a comparative example of the present invention.
[0056] FIG. 15 is a graph showing the results of a three-point bending test for a tungsten-chromium based composite (W / Cr) and a pure tungsten material (pure W) according to an embodiment of the present invention.
[0057] FIG. 16 is a graph showing the results of a uniaxial tensile test for a tungsten-chromium based composite (W / Cr) and a pure tungsten material (pure W) according to an embodiment of the present invention.
[0058] FIG. 17 is a photographic image showing the results of evaluating the oxidation resistance of a tungsten-chromium based composite (W / Cr composite) and a pure tungsten material (pure W) according to an embodiment of the present invention.
[0059] FIG. 18 is a diagram showing the results of analyzing the elemental distribution of a cross-section of a composite material using energy-dispersive X-ray spectroscopy (EDS) after performing an exposure test in which a tungsten-chromium-based composite material (W / Cr composite material) according to an embodiment of the present invention was exposed to a high-temperature oxidizing environment.
[0060] FIG. 19 is a schematic diagram showing a nuclear fusion reactor (tokamak nuclear fusion reactor) to which a tungsten-chromium-based composite according to one embodiment of the present invention can be applied.
[0061] FIG. 20 is a cross-sectional view showing a diverter constituent unit to which a tungsten-chromium-based composite according to one embodiment of the present invention can be applied.
[0062] Embodiments of the present invention will be described in detail below with reference to the attached drawings. The sizes or thicknesses of the areas or parts depicted in the attached drawings may be slightly exaggerated for the clarity of the specification and convenience of explanation. Throughout the detailed description, the same reference numerals indicate the same components.
[0063] FIG. 1 is a flowchart illustrating a powder metallurgical manufacturing method of a tungsten (W)-chromium (Cr)-based composite according to one embodiment of the present invention.
[0064] FIG. 2 is a schematic diagram of a process for explaining a powder metallurgical manufacturing method of a tungsten-chromium-based composite according to one embodiment of the present invention.
[0065] Referring to FIGS. 1 and 2, a method for manufacturing a tungsten-chromium-based composite according to an embodiment of the present invention may include a step (S10) of mixing a tungsten powder composed of a plurality of tungsten (W) particles and a chromium powder composed of a plurality of chromium (Cr) particles by a milling method to form a core-shell based composite powder comprising a core particle portion composed of tungsten and a shell portion composed of a plurality of core-shell particles covering the surface of the core particle portion and chromium. The method for manufacturing the tungsten-chromium-based composite may include a step (S20) of heat-treating the core-shell based composite powder in an atmosphere containing hydrogen (H2) so that a hydrogen (H2) reduction treatment is performed to form a reduced core-shell based composite powder. Additionally, the method for manufacturing the tungsten-chromium-based composite may include the step (S30) of sintering the reduction-treated core-shell-based composite powder to form a tungsten-chromium-based composite comprising a matrix composed of chromium or containing chromium as the main material, and a plurality of embedded particles composed of tungsten or containing tungsten as the main material, which are embedded and distributed within the matrix at least partially spaced apart from each other.
[0066] In step S10, the average particle size of the tungsten powder may be larger than the average particle size of the chromium powder. The ratio (A / B) between the -3σ particle size (A) of the tungsten powder and the +3σ particle size (B) of the chromium powder may be greater than approximately 3, where σ represents the standard deviation. The ratio (A / B) between the particle size (A) corresponding to -3σ in the particle size distribution of the tungsten powder and the particle size (B) corresponding to +3σ in the particle size distribution of the chromium powder may be greater than approximately 3. In this case, the formation of the core-shell particles can be easily achieved. As relatively large tungsten particles collide with relatively small chromium particles, the chromium particles adhere to the surface of the tungsten particles through friction, forming a shell. When the chromium particles have a significantly small size, the formation of the shell portion may be facilitated by aggregation on the surface of the tungsten particles.
[0067] The -3σ particle size (A) of the above tungsten powder corresponds to a relatively small size within the tungsten particle size distribution, and the +3σ particle size (B) of the above chromium powder corresponds to a relatively large size within the chromium particle size distribution. Therefore, the fact that the ratio (A / B) is greater than about 3 may mean that the 'small size' in the above tungsten powder is about 3 times larger than the 'large size' in the above chromium powder. When these conditions are satisfied, the formation of the core-shell particles can be easily achieved. The upper limit of the above ratio (A / B) may not be specifically limited, but as a non-limiting example, the above ratio (A / B) may be about 1000 or less, about 500 or less, or about 100 or less.
[0068] According to one embodiment, the average particle size of the tungsten powder may be about 150 μm or less. For example, the average particle size of the tungsten powder may be in the range of about 3 to 150 μm or about 30 to 150 μm. When using tungsten powder having a relatively large average particle size, chromium particles having a small size may adhere well to the surface of the tungsten particles without clumping together well, and as a result, the formation of core-shell particles can be achieved more easily. In addition, the average particle size of the tungsten powder may affect the physical properties of the tungsten-chromium-based composite material finally manufactured. Meanwhile, the average particle size of the chromium powder may be about 10 μm or less or about 5 μm or less. The purity of the above tungsten powder may be greater than, for example, about 99.9%, and the purity of the above chromium powder may be greater than, for example, about 99.2%.
[0069] In step S10, the volume ratio (W:Cr) between the tungsten powder and the chromium powder may be, for example, in the range of 5:5 to 8:2. As a non-limiting example, the volume ratio (W:Cr) between the tungsten powder and the chromium powder may be in the range of 5:5 to 7:3 (e.g., 6:4), but is not limited thereto. Meanwhile, in the total amount of the tungsten powder and the chromium powder, the content of the tungsten powder may be about 60 to 90 wt%, and the content of the chromium powder may be about 10 to 40 wt%. When the volume ratio (W:Cr) between the tungsten powder and the chromium powder or the weight ratio between the tungsten powder and the chromium powder is within an appropriate range, the formation of core-shell particles may be easy, and it may be advantageous for improving the physical properties of the manufactured tungsten-chromium-based composite.
[0070] In step S10, the milling can be performed without using milling balls, for example, under conditions of about 200 to 8000 rpm for about 30 minutes or more. The milling may be high-energy milling using high-speed rotation conditions (rpm). If milling balls are used, an action closer to grinding occurs rather than adsorption / attachment between particles through friction, and consequently, it may act disadvantageously for core-shell particle formation. Therefore, by rotating the mixer body (i.e., milling vial) at high speed without using milling balls, particle adsorption / attachment characteristics due to friction and collision between tungsten particles and chromium particles can be induced. The rotation rpm may be in the range of about 200 to 8000 rpm or about 500 to 8000 rpm, and the milling process time may be about 30 minutes or more, about 2 hours or more, about 5 hours or more, or about 10 hours or more. The milling process time may be about 100 hours or less. By the above milling, chromium particles may be attached to the surface of tungsten particles to form a shell shape, and the tungsten particles may maintain their original shape or nearly intact, or, in some cases, be crushed to some extent. Additionally, in some cases, some chromium particles may not be attached to the surface of tungsten particles and may exist separately, and the separately existing chromium particles may exist at least partially clustered together.
[0071] According to a specific example, in step S10, the milling can be performed for 20 hours under conditions of a volume ratio (W:Cr) of 6:4 and a rotational speed of 1060 rpm, but this is merely an example and specific conditions can be varied.
[0072] Based on the tungsten particles in step S10, about 90% or more, about 95% or more, about 99% or more, or the entirety of the tungsten particles may constitute the core-shell particles. The shell portion composed of chromium in all or most of the core-shell particles may completely (or nearly completely) surround the surface of the core particle portion composed of tungsten. The proportion (volume ratio) of the core-shell powder in the core-shell-based composite powder produced through step S10 may be about 80% or more, about 90% or more, or about 95% or more. The entirety of the core-shell-based composite powder may also consist of the core-shell powder.
[0073] In step S20, the heat treatment for the hydrogen (H2) reduction treatment can be performed, for example, at a temperature in the range of about 700 to 1500°C for about 2 to 25 hours. The heating rate in the heat treatment for the hydrogen (H2) reduction treatment can be, for example, about 3 to 20°C / min. The heat treatment can be performed using a tubular furnace or oven, and can be performed by flowing hydrogen (H2) gas or a gas containing hydrogen (H2) through the tubular furnace or oven. The flow rate of the hydrogen (H2) gas or the gas containing hydrogen (H2) can be, for example, about 0.5 to 5 L / min, but is not limited thereto.
[0074] Oxides may be present in the core-shell based composite powder, and by performing the hydrogen (H2) reduction treatment in step S20, the oxides can be reduced to convert them into a metallic material or the oxidation state of the metal can be controlled. Therefore, if step S20 is performed appropriately, it is possible to prevent oxides from forming in the tungsten-chromium based composite material produced at the end and to improve the physical properties of the composite material.
[0075] According to a specific example, in step S20, the hydrogen (H2) reduction treatment can be performed for 15 hours at a temperature of 1200°C and a heating rate of 10°C / min while flowing hydrogen (H2) gas at a flow rate of 1 L / min, but this is merely an example and specific conditions can be varied.
[0076] If necessary, a step of pre-treating at least one of the tungsten powder and the chromium powder may be further performed prior to step S10 (i.e., the step of forming the core-shell based composite powder). The pre-treatment step may include a step of heat-treating at least one of the tungsten powder and the chromium powder so that a hydrogen (H2) reduction treatment is performed in an atmosphere containing hydrogen (H2). By treating the tungsten powder and the chromium powder with hydrogen (H2) reduction before the milling process, the possibility of oxide formation can be reduced and the characteristics of the core-shell powder manufacturing can be improved. The specific conditions of the hydrogen (H2) reduction treatment performed prior to the milling process may be the same or similar to the hydrogen (H2) reduction treatment performed in step S20.
[0077] In step S30, the reduction-treated core-shell based composite powder may be sintered to form a tungsten-chromium based composite material comprising a matrix composed of chromium or containing chromium as the main material, and a plurality of embedded particles composed of tungsten or containing tungsten as the main material, which are embedded and distributed within the matrix at least partially spaced apart from each other. The reduction-treated core-shell based composite powder may be sintered using a device capable of applying at least two of heat, electric current, and pressure simultaneously or separately. The reduction-treated core-shell based composite powder may be sintered using Joule heating through the application of electric current along with the application of heat and / or pressure from an external source. For example, the reduction-treated core-shell based composite powder may be sintered by a spark plasma sintering (SPS) method. Composite powders having a core-shell structure can be easily sintered using the discharge plasma sintering (SPS) method and can be advantageously applied to realize composite materials having a desired microstructure in the embodiments of the present invention. The tungsten-chromium-based composite material may have a dual-phase structure having a continuous matrix phase and a discontinuous particle phase, or may include a dual-phase structure. Discharge plasma sintering (SPS) is a technique that produces a high-density sintered body within a short period of time by simultaneously applying pressure and a pulsed current to a powder sample. High-temperature heating within minutes may be possible through the generation of inter-particle discharge plasma and Joule heating. By using discharge plasma sintering (SPS), rapid sintering within minutes to tens of minutes is possible compared to conventional sintering methods; dense sintered bodies can be obtained even at relatively low temperatures due to high pressure and instantaneous plasma generation; and productivity can be improved through high energy efficiency and short process time.
[0078] The above discharge plasma sintering (SPS) can be performed by loading the reduction-treated core-shell based composite powder into a mold, creating a given gas atmosphere inside a chamber, applying pressure to the powder while applying a pulsed current (DC current) to sinter it, and then cooling it.
[0079] According to one embodiment, the discharge plasma sintering (SPS) method sintering can be performed for about 5 to 60 minutes at a temperature of about 800 to 1800°C and a pressure of about 200 MPa or less in an atmosphere containing hydrogen (H2). The temperature condition may be in the range of about 800 to 1800°C, or about 1100 to 1700°C, or about 1200 to 1600°C, or about 1300 to 1600°C, and the pressure condition may be in the range of about 20 to 200 MPa or about 65 to 200 MPa. When the process is performed under appropriate temperature and pressure conditions, it may be advantageous to obtain a dense sintered body (composite material) with high physical properties. After reaching the maximum temperature, the holding time may be about 5 to 60 minutes, and then cooling may be performed without applying a pulse current (DC current). The heating rate can be, for example, about 30 to 300 °C / min. If the above conditions are satisfied, it may be advantageous to manufacture a high-density composite material having excellent physical properties.
[0080] As the sintering temperature increases within a given temperature range, it may be advantageous for forming a dense sintered body. However, if the sintering temperature becomes excessively high, there is a possibility that the two-phase structure will not be maintained and will be destroyed. When using the discharge plasma sintering (SPS) method, it may be advantageous for manufacturing composites in which the two-phase structure is not destroyed due to the rapid heating rate and rapid sintering. According to an embodiment of the present invention, a composite having high density can be formed without destroying the two-phase structure.
[0081] The sintering of the above discharge plasma sintering (SPS) method can be performed in a gas atmosphere containing hydrogen (H2). For example, the sintering can be performed in a hydrogen (H2) atmosphere or in a mixed gas atmosphere containing hydrogen (H2) and argon (Ar). The hydrogen (H2) content (by volume) in the mixed gas may be about 2% or more. By performing sintering in a gas atmosphere containing hydrogen (H2), the possibility of oxidation of chromium (Cr), etc., can be effectively blocked.
[0082] According to a specific example, in step S30, the discharge plasma sintering (SPS) can be performed for 10 minutes at a temperature of 1300°C and a pressure of 120 MPa in a mixed gas atmosphere of argon (Ar) and 3% hydrogen (H2) by volume, with a heating rate of 200°C / min, but this is merely an example and specific conditions can be varied.
[0083] The tungsten-chromium-based composite manufactured through step S30 may include a matrix composed of chromium or containing chromium as a main material and forming a continuous phase, and a plurality of embedded particles embedded and distributed within the matrix so as to be at least partially spaced apart from each other, composed of tungsten or containing tungsten as a main material and forming a discontinuous phase. In terms of including a continuous matrix phase and a discontinuous particle phase, the tungsten-chromium-based composite may be said to have a dual-phase structure. Although the tungsten-chromium-based composite may be said to have a roughly dual-phase structure, it may also include at least one additional separate phase in addition to the two phases mentioned above.
[0084] Approximately 90% or more, approximately 95% or more, or the entirety of the above matrix may be composed of chromium. In this respect, the matrix may be referred to as a 'Cr matrix' or a 'Cr-based matrix'. Approximately 90% or more, approximately 95% or more, or the entirety of the plurality of embedded particles may be composed of tungsten. In this respect, the plurality of embedded particles may be referred to as 'W embedded particles' or 'W-based embedded particles'. Within the tungsten-chromium-based composite, a substantial portion or most of the plurality of embedded particles may exist spaced apart from one another. For example, approximately 70% or more, approximately 80% or more, or approximately 90% or more of the plurality of embedded particles may be distributed spaced apart from one another.
[0085] The tungsten-chromium-based composite manufactured through step S30 may have a relative density of about 90% or more, about 93% or more, or about 95% or more. The tungsten-chromium-based composite may be a significantly dense sintered body. The porosity of the tungsten-chromium-based composite may be about 10% or less, about 7% or less, or about 5% or less. According to an embodiment of the present invention, a dense composite having high density and excellent physical properties can be manufactured from the core-shell based composite powder by the discharge plasma sintering (SPS) method. However, in some cases, the tungsten-chromium-based composite may have a relative density less than about 90%, and the relative density of the tungsten-chromium-based composite may be improved through post-processing steps such as rolling or forging.
[0086] In the above tungsten-chromium-based composite, the content of the matrix may be about 10 to 40 wt%, and the content of the plurality of embedded particles may be about 60 to 90 wt%. When these conditions are satisfied, the tungsten-chromium-based composite may be advantageous for realizing excellent physical properties suitable for the intended purpose in the embodiments of the present invention.
[0087] In the tungsten-chromium-based composite, the average particle size of the plurality of embedded particles may be, for example, about 150 μm or less. For example, the average particle size of the plurality of embedded particles may be in the range of about 3 to 150 μm or about 30 to 150 μm. The plurality of embedded particles may have the same or nearly the same dimensions / characteristics as the plurality of tungsten particles (initial particles) used in step S10. In the milling step of S10, the tungsten particles may maintain their original shape or nearly the same shape, or, in some cases, may be partially ground.
[0088] The tungsten-chromium-based composite manufactured according to an embodiment of the present invention may have a non-lamellar structure. In the case of a composite (alloy) having a lamellar structure formed by spinodal decomposition, etc., it may generally have brittleness and poor ductility. A composite having a lamellar structure formed by spinodal decomposition, etc., may have a small interlayer spacing of less than about 1 μm. However, the composite manufactured according to an embodiment of the present invention may not have a lamellar structure and may have a structure in which a plurality of W embedded particles are relatively uniformly distributed within a Cr matrix (i.e., a particle dispersion structure within the matrix), thereby having high strength and high ductility while having improved ductile-brittle transition temperature (DBTT) characteristics. In some cases, the tungsten-chromium-based composite according to an embodiment of the present invention may have a lamellar structure or a similar structure depending on the shape of the embedded particles, and in this case, the interlayer spacing of the lamellar structure may be about 1 μm or more. Therefore, such a structure may differ from a typical lamellar structure formed by spinodal decomposition.
[0089] The plurality of embedded particles may have relatively high strength compared to the matrix, and the matrix may have relatively high ductility compared to the plurality of embedded particles. The tungsten-chromium-based composite may have high strength and high ductility characteristics in relation to having a structure in which the plurality of high-strength embedded particles are uniformly distributed within the high-ductility matrix. In addition, the tungsten-chromium-based composite may have high oxidation resistance compared to pure tungsten material and may have a low ductile-brittle transition temperature (DBTT) compared to pure tungsten material. Chromium, which forms the main material of the matrix, can provide high oxidation resistance to the internal material of the composite even under relatively harsh conditions. The ductile-brittle transition temperature (DBTT) of a pure tungsten material may be approximately 400°C or higher, whereas the ductile-brittle transition temperature (DBTT) of a tungsten-chromium-based composite manufactured according to an embodiment of the present invention may be approximately 300°C or higher and approximately 400°C or lower. Therefore, the composite can maintain high ductility characteristics without transitioning to brittleness even in a temperature range of approximately 300 to 400°C. Due to its superior oxidation resistance and improved ductile-brittle transition temperature (DBTT) characteristics compared to pure tungsten, this composite (W-Cr two-phase composite) can have useful applications in fields such as nuclear fusion reactors.
[0090] Meanwhile, conventional heavy alloy composites containing nickel (Ni) may not be applicable to nuclear fusion reactors, unlike nuclear fission reactors. Since Ni produces elements with long half-lives that emit strong radiation when neutrons are irradiated in a nuclear fusion reactor, heavy alloy composites containing Ni may not be suitable for use in nuclear fusion reactors. However, the tungsten-chromium based composite manufactured according to the embodiment of the present invention may have properties suitable for application in the field of nuclear fusion reactors.
[0091] Additionally, in the tungsten-chromium-based composite, a solid solution region (first solid solution region) in which Cr atoms diffuse into W, which is the main material, may exist at the edge portion of the embedded particle (the portion in contact with the matrix). Furthermore, a solid solution region (second solid solution region) in which W atoms diffuse into Cr, which is the main material, may exist at the boundary portion of the matrix (the portion in contact with the embedded particle). The first and second solid solution regions can be considered boundary regions and may have a considerably thin thickness. Compounds between W and Cr may not occur.
[0092] FIG. 3 is a scanning electron microscope (SEM) image exemplarily showing tungsten powder and chromium powder that can be applied to a method for manufacturing a tungsten-chromium-based composite according to one embodiment of the present invention.
[0093] Referring to FIG. 3, the average particle size of the tungsten powder may be larger than the average particle size of the chromium powder. During the high-energy milling process, relatively large tungsten particles collide with relatively small chromium particles, and through friction, the chromium particles adhere to the surface of the tungsten particles to form a shell. When the chromium particles have a significantly small size, the formation of the shell portion may be facilitated by aggregation on the surface of the tungsten particles.
[0094] FIG. 4 is an SEM image exemplarily showing a core-shell powder that can be formed in a method for manufacturing a tungsten-chromium-based composite according to one embodiment of the present invention.
[0095] Referring to FIG. 4, the left image shows the external shape of a core-shell particle, and the right image shows a cross-section of a core-shell particle. The shell portion, composed of chromium in whole or in most of the core-shell particle, can completely (or nearly completely) surround the surface of the core particle portion, which is composed of tungsten. The composite powder having a core-shell structure can be easily sintered by the discharge plasma sintering (SPS) method and can be advantageously applied to realize a composite material having a desired microstructure in the embodiments of the present invention.
[0096] FIG. 5 is a graph exemplarily showing the particle size distribution of tungsten powder that can be applied to a method for manufacturing a tungsten-chromium-based composite according to one embodiment of the present invention.
[0097] FIG. 6 is a graph exemplarily showing the particle size distribution of chromium powder that can be applied to a method for manufacturing a tungsten-chromium-based composite according to one embodiment of the present invention.
[0098] Referring to FIGS. 5 and 6, the ratio (A / B) between the -3σ particle size (A) of the tungsten powder and the +3σ particle size (B) of the chromium powder may be greater than about 3. In other words, the ratio (A / B) between the particle size (A) corresponding to -3σ in the particle size distribution of the tungsten powder and the particle size (B) corresponding to +3σ in the particle size distribution of the chromium powder may be greater than about 3. In this embodiment, A may be 28.42653 μm and B may be 6.70125 μm, and the ratio (A / B) may be 4.242. If the condition that the ratio (A / B) is greater than 3 is satisfied, the formation of core-shell particles can be easily achieved.
[0099] The -3σ particle size (A) of the above tungsten powder corresponds to a relatively small size within the tungsten particle size distribution, and the +3σ particle size (B) of the above chromium powder corresponds to a relatively large size within the chromium particle size distribution. Therefore, the fact that the ratio (A / B) is greater than about 3 may mean that the 'small size' in the above tungsten powder is about 3 times larger than the 'large size' in the above chromium powder. When these conditions are satisfied, the formation of the core-shell particles can be easily achieved. The upper limit of the above ratio (A / B) may not be specifically limited, but as a non-limiting example, the above ratio (A / B) may be about 1000 or less, about 500 or less, or about 100 or less.
[0100] FIG. 7 is a graph showing a binary phase diagram between tungsten (W) and chromium (Cr) that can be applied to the manufacture of a composite material according to one embodiment of the present invention.
[0101] Referring to FIG. 7, sintering must be performed below the high-temperature stable phase formation temperature of the two powder materials (W, Cr) to obtain a two-phase structure, and at a higher temperature, the two-phase structure may be destroyed. The area marked in yellow in FIG. 7 (i.e., the shaded area) indicates the sinterable temperature range and composition area in the phase diagram.
[0102] FIG. 8 is an SEM image showing a core-shell based composite powder formed through mechanical milling and a tungsten-chromium based composite material manufactured from the core-shell based composite powder by discharge plasma sintering (SPS) according to one embodiment of the present invention.
[0103] Referring to FIG. 8, a core-shell powder can be formed through a milling process according to an embodiment, comprising a core particle portion composed of tungsten and a shell portion composed of chromium covering the surface of the core particle portion. Additionally, a tungsten-chromium-based composite having a given microstructure can be formed from the core-shell powder by a discharge plasma sintering (SPS) method. The tungsten-chromium-based composite may include a matrix (10) composed of chromium or containing chromium as a main material and a plurality of embedded particles (20) composed of tungsten or containing tungsten as a main material, which are embedded and distributed within the matrix (10) at least partially spaced apart from each other. The tungsten-chromium-based composite may be said to have a two-phase structure in which a plurality of embedded particles (20) are substantially uniformly distributed within the matrix (10).
[0104] Figure 9 is an SEM image according to a comparative example, showing a composite powder formed through mechanical milling and a composite material manufactured from the composite powder by discharge plasma sintering (SPS).
[0105] Referring to FIG. 9, the composite powder according to the comparative example does not have a core-shell structure, and the composite material formed therefrom may have a microstructure in which the internal particles are unevenly distributed. Therefore, the mechanical and thermal properties of the composite material according to the comparative example may be degraded.
[0106] FIG. 10 is an SEM image showing a tungsten-chromium based composite material manufactured according to one embodiment of the present invention.
[0107] Referring to FIG. 10, as previously described, a tungsten-chromium-based composite according to an embodiment of the present invention may include a matrix (10) composed of chromium or containing chromium as a main material, and a plurality of embedded particles (20) that are embedded and distributed within the matrix (10) at least partially spaced apart from each other and composed of tungsten or containing tungsten as a main material. In other words, the tungsten-chromium-based composite may include a matrix (10) that is composed of chromium or contains chromium as a main material and forms a continuous phase, and a plurality of embedded particles (20) that are embedded and distributed within the matrix (10) at least partially spaced apart from each other and are composed of tungsten or containing tungsten as a main material and form a discontinuous phase. In terms of including a continuous matrix phase and a discontinuous particle phase, the tungsten-chromium-based composite may be said to have a dual-phase structure. The above tungsten-chromium based composite can be said to have a roughly two-phase structure, but in some cases, it may include at least one additional separate phase in addition to the two phases mentioned above.
[0108] About 90% or more, about 95% or more, or the whole of the matrix (10) may be composed of chromium. In this respect, the matrix (10) may be referred to as a 'Cr matrix' or a 'Cr-based matrix'. About 90% or more, about 95% or more, or the whole of the plurality of embedded particles (20) may be composed of tungsten. In this respect, the plurality of embedded particles (20) may be referred to as 'W embedded particles' or 'W-based embedded particles'.
[0109] In the above tungsten-chromium-based composite, at the edge portion (the portion in contact with the matrix) of the embedded particle (20), a solid solution region (first solid solution region) in which Cr atoms have diffused in while W forms the main material may exist. Additionally, at the boundary portion (the portion in contact with the embedded particle) of the matrix (10), a solid solution region (second solid solution region) in which W atoms have diffused in while Cr forms the main material may exist. The first and second solid solution regions can be referred to as boundary regions and may have a considerably thin thickness.
[0110] FIG. 11 is an SEM cross-sectional image showing a tungsten-chromium-based composite material manufactured according to one embodiment of the present invention.
[0111] Referring to FIG. 11, a tungsten-chromium based composite according to an embodiment of the present invention may be manufactured through a high-energy milling step, a hydrogen (H2) reduction treatment step, and a discharge plasma sintering (SPS) step. Here, the high-energy milling step may be performed for 20 hours without using milling balls, under conditions of a volume ratio (W:Cr) of 6:4 and a rotation speed of 1060 rpm. The hydrogen (H2) reduction treatment step may be performed for 15 hours at a temperature of 1200°C using 99.999% hydrogen (H2) gas. The discharge plasma sintering (SPS) step may be performed for 10 minutes at a temperature of 1300°C and a pressure of 100 MPa in a mixed gas atmosphere of argon (Ar) and 3% hydrogen (H2) by volume. Depending on the temperature, pressure, and time conditions of the above-mentioned discharge plasma sintering (SPS), the porosity and pore distribution characteristics of the tungsten-chromium-based composite material produced may vary.
[0112] The tungsten-chromium-based composite material manufactured in this embodiment may include a first portion (P1) in contact with or adjacent to a surface and a second portion (P2) positioned relatively inward from the first portion (P1), and the second portion (P2) may be a portion positioned spaced apart from the surface (exposed surface). The porosity of the first portion (P1) may be relatively higher than the porosity of the second portion (P2). For example, a small number of pores (isolated pores) may be found only in the first portion (P1), and there may be no pores or substantially few pores found in the second portion (P2). However, depending on the process conditions, the distribution of pores throughout the composite material may be made uniform, or pores may be made almost non-existent.
[0113] Figure 12 is an SEM image showing a tungsten-chromium-based composite prepared according to a comparative example. The comparative example in Figure 12 is a case where the composite was prepared by discharge plasma sintering (SPS) without applying a hydrogen (H2) reduction process after the milling step.
[0114] FIG. 13 is an SEM image showing a tungsten-chromium-based composite material manufactured according to one embodiment of the present invention. The embodiment of FIG. 13 is a case in which a hydrogen (H2) reduction process is applied after a milling step, and then the composite material is manufactured by discharge plasma sintering (SPS).
[0115] In FIGS. 12 and 13, discharge plasma sintering (SPS) was performed for 10 minutes at a temperature of 1300°C and a pressure of 120 MPa in a mixed gas atmosphere of argon (Ar) and 3% hydrogen (H2) by volume. In the example of FIG. 13, the hydrogen (H2) reduction process was performed for 15 hours at a temperature of 1200°C.
[0116] Referring to FIGS. 12 and 13, in the comparative example where the hydrogen (H2) reduction process was not applied, it can be seen that oxides were formed within the matrix. In this case, the mechanical properties of the composite material may be degraded due to the oxides. On the other hand, in the example where the hydrogen (H2) reduction process was applied, it can be seen that no oxides were formed within the matrix. Therefore, the composite material manufactured according to the example can have excellent mechanical properties.
[0117] FIG. 14 is a graph showing the results of a three-point bending test to evaluate the toughness of a material according to an embodiment and a comparative example of the present invention.
[0118] In FIG. 14, samples Cr_m70W and Cr_m60W are composite materials according to the embodiment and have a structure in which a plurality of W particles are embedded within a Cr matrix. Cr_m70W refers to a sample in which W powder is applied at a volume fraction of 70%, and Cr_m60W refers to a sample in which W powder is applied at a volume fraction of 60%. In FIG. 14, samples W_m20W and W_m10W are composite materials according to the comparative example and have a structure in which a plurality of Cr particles are embedded within a W matrix. W_m20W refers to a sample in which W powder is applied at a volume fraction of 20%, and W_m10W refers to a sample in which W powder is applied at a volume fraction of 10%. Meanwhile, the Cr sample refers to a pure Cr material, and the W sample refers to a pure W material. The test temperature was 300℃, and the strain rate was ~10 -5 s -1 It was.
[0119] Referring to FIG. 14, it can be seen that the composite material (Cr_m70W and Cr_m60W) according to an embodiment of the present invention exhibits improved toughness compared to a pure W material and improved strength characteristics compared to a pure Cr material. In addition, it can be seen that the composite material (Cr_m70W and Cr_m60W) according to the embodiment exhibits significantly improved fracture toughness characteristics compared to the composite material (W_m20W and W_m10W) according to the comparative example.
[0120] FIG. 15 is a graph showing the results of a three-point bending test for a tungsten-chromium-based composite (W / Cr) and a pure tungsten material (pure W) according to an embodiment of the present invention. The tungsten-chromium-based composite (W / Cr) according to the embodiment is a two-phase composite having a microstructure in which the W particle phase is distributed within the Cr matrix connecting phase. The test temperature was 300°C.
[0121] Referring to FIG. 15, it can be seen that while the pure tungsten material (pure W) exhibits brittleness at a relatively low temperature of about 300°C, the tungsten-chromium based composite (W / Cr) according to an embodiment of the present invention has ductility even at a relatively low temperature.
[0122] FIG. 16 is a graph showing the results of a uniaxial tensile test for a tungsten-chromium-based composite (W / Cr) and a pure tungsten material (pure W) according to an embodiment of the present invention. The tungsten-chromium-based composite (W / Cr) according to the embodiment is a two-phase composite, having a microstructure in which the W particle phase is distributed within the Cr matrix connecting phase.
[0123] Referring to FIG. 16, commercial pure tungsten material (pure W) has a ductile-brittle transition temperature (DBTT) of about 400 to 500°C, whereas the tungsten-chromium-based composite (W / Cr) according to an embodiment of the present invention exhibits ductility at 400°C or lower and can have a ductile-brittle transition temperature (DBTT) of about 300 to 400°C. Therefore, the tungsten-chromium-based composite (W / Cr) according to the embodiment can overcome the low-temperature brittleness of the pure tungsten material (pure W).
[0124] FIG. 17 is a photographic image showing the results of evaluating the oxidation resistance of a tungsten-chromium based composite (W / Cr composite) and a pure tungsten material (pure W) according to an embodiment of the present invention. After exposing the two specimens to a high-temperature oxidizing environment, changes in shape / mode were observed visually. An exposure test was conducted at a temperature of 1000°C for 20 hours in an atmospheric environment.
[0125] Referring to Fig. 17, the external appearance of the two specimens before the test was almost identical, but after the exposure test, the pure tungsten material (pure W) was completely oxidized and could not function as a structural material. On the other hand, the W / Cr composite according to the example did not show significant changes in appearance or color, and a metallic luster was observed when checking the cross-section.
[0126] FIG. 18 is a diagram showing the results of analyzing the elemental distribution of a cross-section of a tungsten-chromium-based composite (W / Cr composite) according to an embodiment of the present invention using energy-dispersive X-ray spectroscopy (EDS) after performing an exposure test in which the composite was exposed to a high-temperature oxidizing environment. The conditions of the exposure test were the same as those described in FIG. 17. In FIG. 18, (1) SE diagram represents a secondary electron image, and (2) W, (3) Cr, and (4) O diagrams represent the distribution of the corresponding elements, respectively.
[0127] Referring to FIG. 18, it was confirmed that in the W / Cr composite according to the embodiment in which W particle phases are isolated and distributed within a Cr matrix linkage structure, an oxide layer of approximately 50 μm or less is formed only on the surface, and the interior is not oxidized. This is a characteristic similar to stainless steel, which may be because the Cr oxide film formed on the surface protects the interior of the composite from external oxygen. Since the isolated W particle phases are not oxidized due to the highly oxidation-resistant Cr matrix linkage structure, the composite can have excellent oxidation resistance overall.
[0128] A tungsten-chromium-based composite manufactured according to an embodiment of the present invention can be applied to various parts and equipment. The tungsten-chromium-based composite can be applied to a plasma-facing component (PFC), and equipment including said plasma-facing component (PFC) can be provided. The equipment may include, for example, a fusion reactor.
[0129] Pure W materials for fusion reactors have high strength but suffer from the disadvantages of a high ductile-brittle transition temperature (DBTT) and low elongation. Additionally, commercial pure W materials may be vulnerable to oxidation and sublimation in the event of a fusion reactor accident. The composite material according to the embodiment of the present invention has a structure in which Cr, which has a low ductile-brittle transition temperature (DBTT), forms the matrix and W particles are uniformly dispersed; this allows crack propagation to be effectively delayed even at relatively low temperatures, enabling it to function as a high-strength and high-ductility material. Furthermore, the composite material according to the embodiment (two-phase composite) can possess excellent oxidation resistance because W, which is relatively susceptible to oxidation, is isolated (surrounded) by Cr, which has high oxidation resistance, and is not exposed to oxygen.
[0130] Under normal circumstances, the interior of a fusion reactor maintains a high vacuum; however, if the airtight seal is breached due to an accident, it is expected to reach atmospheric pressure (oxygen exposure) within seconds to hours, depending on the scale of the accident. Sudden pressure changes within the fusion reactor can damage components, and in particular, if cooling pipes are destroyed, it can lead to a cooling water leak. Furthermore, if cooling pipes rupture due to an accident, even if the fusion reaction is immediately halted, the plasma-facing components inside the reactor are expected to maintain ultra-high temperatures of 1,200 to 1,450 K for several weeks due to nuclear reactions of radioactive elements. Steam generated by the leakage of cooling water can cause the pressure inside the fusion reactor to rise rapidly, potentially leading to the destruction of the vessel.
[0131] Therefore, plasma-facing materials for fusion reactors need to maintain stability even in ultra-high temperature / oxygen exposure environments in preparation for accidents such as LOCA (loss of coolant accident) and LOVA (loss of vacuum accident). The tungsten-chromium-based composite according to the embodiment of the present invention is expected to satisfy the requirements of such plasma-facing materials for fusion reactors.
[0132] FIG. 19 is a schematic diagram showing a nuclear fusion reactor (tokamak nuclear fusion reactor) to which a tungsten-chromium-based composite according to one embodiment of the present invention can be applied.
[0133] Referring to FIG. 19, a fusion reactor may include plasma-facing components such as a first wall and a divertor. Due to radiant heat and particle flux, the inner wall of the fusion reactor must be made of a material that has a high melting point and can withstand high-energy particle irradiation. In particular, the divertor is a component where high heat flux / high particle flux is concentrated, and its surface can reach a temperature of up to 2000°C or higher. The tungsten-chromium-based composite according to an embodiment of the present invention can be applied, for example, to a part corresponding to a relatively low temperature portion of the divertor.
[0134] FIG. 20 is a cross-sectional view showing a diverter constituent unit to which a tungsten-chromium-based composite according to one embodiment of the present invention can be applied.
[0135] Referring to FIG. 20, a diverter unit applied to a fusion reactor may have a block structure through which a cooling fluid (C1) passes. The diverter unit may include a block body (50), a cooling pipe (60) penetrating the block body (50), and an intermediate layer (70) disposed between the block body (50) and the cooling pipe (60). The intermediate layer (70) may have a tube or ring shape as a type of insertion layer. The cooling fluid (C1) may flow into the interior of the cooling pipe (60). A tungsten-chromium-based composite according to an embodiment of the present invention may be applied to a block body (50) corresponding to a relatively low-temperature part among the components of the diverter. The tungsten-chromium-based composite may be applied to at least a part of the block body (50).
[0136] There is a possibility that cracks may occur in the block body (50) due to thermal stress. If cracks generated on the surface propagate to the cooling pipe (60), there is a possibility that it may lead to a major accident, such as a leak of cooling water. Since the temperature near the cooling pipe (60) is below the ductile-brittle transition temperature (DBTT) range of tungsten, general tungsten materials may be brittle, making it difficult to effectively prevent crack propagation. However, the tungsten-chromium based composite according to the embodiment of the present invention has high ductility and a relatively low ductile-brittle transition temperature (DBTT), so it is expected that the occurrence and propagation of cracks can be effectively prevented. The application field of the composite according to the embodiment of the present invention is not limited to nuclear fusion reactors and can be varied as needed.
[0137] According to the embodiments of the present invention described above, a powder metallurgical manufacturing method for an intermetallic composite material can be realized that has excellent oxidation resistance and improved ductile-brittle transition temperature (DBTT) characteristics compared to conventional tungsten materials. Furthermore, according to the embodiments of the present invention, a powder metallurgical manufacturing method for an intermetallic composite material that possesses excellent oxidation resistance while having high strength and high ductility characteristics can be realized. According to one embodiment of the present invention, a composite powder having a core-shell particle structure is manufactured using a high-energy milling method, and from this, a dual-phase composite material in which tungsten (W) particles are distributed within a chromium (Cr) matrix can be easily manufactured using a spark plasma sintering (SPS) method. The composite material can have excellent strength and ductility characteristics while having a relatively low ductile-brittle transition temperature (DBTT), and additionally, can have high relative density and excellent oxidation resistance. Therefore, the composite material manufactured according to the embodiment can maintain ductility in high-temperature, high-heat, and high-particle-flux environments such as a fusion reactor, and effectively prevent the occurrence and propagation of cracks. In addition, the composite material manufactured according to the embodiment is expected to maintain material stability even in ultra-high temperature and oxygen exposure environments of fusion reactor accident scenarios.
[0138] This specification discloses preferred embodiments of the present invention. Although specific terms have been used, they are used merely in a general sense to facilitate the explanation of the technical content of the present invention and to aid in understanding the invention, and are not intended to limit the scope of the present invention. It is obvious to those skilled in the art that, in addition to the embodiments disclosed herein, other variations based on the technical concept of the present invention are possible. Those skilled in the art will understand that the powder metallurgical method for manufacturing a tungsten-chromium-based composite and the tungsten-chromium-based composite manufactured by this method, according to the embodiments described with reference to FIGS. 1 to 8, FIGS. 10, FIGS. 11, and FIGS. 13 to 20, can be variously substituted, changed, and modified within the scope of the technical concept of the present invention. As a specific example, the powder metallurgical manufacturing method according to the embodiment of the present invention is not limited to the manufacture of tungsten and chromium composites, but can also be applied to the manufacture of other intermetallic composites, such as Fe-Cu-based composites and Al-Zn-based composites. Therefore, the scope of the invention should not be determined by the described embodiment, but by the technical concept described in the patent claims.
Claims
1. A step of mixing tungsten powder composed of a plurality of tungsten (W) particles and chromium powder composed of a plurality of chromium (Cr) particles by a milling method to form a core-shell based composite powder comprising a plurality of core-shell particles having a core particle portion composed of tungsten and a shell portion composed of chromium covering the surface of the core particle portion; A step of forming a reduced core-shell based composite powder by heat treating the above core-shell based composite powder in an atmosphere containing hydrogen (H2) so that a hydrogen (H2) reduction treatment is performed; and A method for manufacturing a tungsten-chromium-based composite, comprising the step of sintering the above-described reduction-treated core-shell-based composite powder to form a tungsten-chromium-based composite comprising a matrix composed of chromium or containing chromium as the main material and a plurality of embedded particles composed of tungsten or containing tungsten as the main material, which are embedded and distributed within the matrix at least partially spaced apart from each other.
2. In Paragraph 1, A method for manufacturing a tungsten-chromium based composite material in which the ratio (A / B) between the -3σ particle size (A) of the tungsten powder and the +3σ particle size (B) of the chromium powder is greater than 3, where σ represents the standard deviation.
3. In Paragraph 1, A method for manufacturing a tungsten-chromium based composite material in which the average particle size of the tungsten powder is 150 μm or less.
4. In Paragraph 1, A method for manufacturing a tungsten-chromium based composite, wherein the content of the tungsten powder is 60 to 90 wt% and the content of the chromium powder is 10 to 40 wt% in the total amount of the tungsten powder and the chromium powder.
5. In Paragraph 1, A method for manufacturing a tungsten-chromium-based composite material, wherein the above milling is performed for 30 minutes or more under conditions of 200 to 8000 rpm without using milling balls.
6. In Paragraph 1, A method for manufacturing a tungsten-chromium-based composite material in which the heat treatment for the above hydrogen (H2) reduction treatment is performed at a temperature in the range of 700 to 1500°C.
7. In Paragraph 1, The method further includes a step of pre-treating at least one of the tungsten powder and the chromium powder prior to the step of forming the core-shell based composite powder, A method for manufacturing a tungsten-chromium based composite material, comprising the step of heat treating at least one of the tungsten powder and the chromium powder in an atmosphere containing hydrogen (H2) so that hydrogen (H2) reduction treatment is performed.
8. In Paragraph 1, A method for manufacturing a tungsten-chromium based composite material in which the above sintering is performed by a spark plasma sintering (SPS) method.
9. In Paragraph 8, A method for manufacturing a tungsten-chromium-based composite material, wherein the above-mentioned discharge plasma sintering (SPS) method is performed in an atmosphere containing hydrogen (H2) at a temperature of 800 to 1800°C and a pressure of 200 MPa or less.
10. In Paragraph 1, The above tungsten-chromium-based composite is a method for manufacturing a tungsten-chromium-based composite having a relative density of 90% or more.
11. In Paragraph 1, A method for manufacturing a tungsten-chromium-based composite, wherein the content of the matrix in the tungsten-chromium-based composite is 10 to 40 wt% and the content of the plurality of embedded particles is 60 to 90 wt%.
12. A tungsten-chromium based composite manufactured using the method described in any one of claims 1 to 11.