Method for manufacturing electrode for secondary battery, electrode for secondary battery, and secondary battery

By laminating a dry electrode film onto a current collector with electroplated protrusions and rolling with a vibrating roll, the method addresses issues of adhesion and voids, enhancing battery performance and reliability.

WO2026240556A1PCT designated stage Publication Date: 2026-11-19SAMSUNG SDI CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2026/096744
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-14
Filing Date
2026-05-08
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Existing methods for manufacturing electrodes for secondary batteries, such as pattern-coating or laminating dry electrode films on current collectors, result in low processability and economic efficiency, and can damage the current collector or electrode film, leading to poor adhesion and increased voids at the interface, which degrade battery performance.

Method used

A method involving laminating a dry electrode film onto a current collector with protrusions formed by electroplating, rolling with a vibrating roll under controlled conditions to enhance adhesion without an adhesion-promoting layer, reducing voids and improving interface contact.

Benefits of technology

This method enhances adhesion between the current collector and dry electrode film, reducing voids and interfacial resistance, thereby improving battery lifespan and reliability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2026096744_19112026_PF_FP_ABST
    Figure KR2026096744_19112026_PF_FP_ABST
Patent Text Reader

Abstract

The present disclosure provides a method for manufacturing an electrode for a secondary battery, an electrode for a secondary battery, and a secondary battery, the electrode having high adhesion between a current collector and a dry electrode film even without an adhesion promoting layer, and suppressing a side reaction of an electrolyte by reducing occurrence of voids at an interface between the current collector and the dry electrode film. The method for manufacturing an electrode for a secondary battery comprises a step of laminating a dry electrode film on at least one surface of a current collector on which a plurality of protrusions are formed, and rolling same, wherein the average height of the plurality of protrusions of the current collector is 1.7 μm to 5.0 μm; and the rolling is performed using a vibration roll.
Need to check novelty before this filing date? Find Prior Art

Description

Method for manufacturing an electrode for a secondary battery, electrode for a secondary battery and a secondary battery

[0001] The present disclosure relates to a method for manufacturing an electrode for a secondary battery, an electrode for a secondary battery, and a secondary battery.

[0002]

[0003] With the rapid proliferation of battery-powered electronic devices such as mobile phones, laptop computers, and electric vehicles, the demand for high-energy-density, high-capacity rechargeable batteries is rapidly increasing. Accordingly, research and development to improve the performance of lithium-ion batteries is actively underway.

[0004] A lithium secondary battery is a battery comprising a positive electrode and a negative electrode containing an active material capable of lithium ion intercalation and deintercalation, and an electrolyte, which produces electrical energy through oxidation and reduction reactions when lithium ions are intercalated or deintercalated from the positive and negative electrodes.

[0005] Research is actively being conducted on the fabrication of electrodes containing solvent-free dry electrode films. Dry electrode films include electrode active materials, binders, and conductive materials, and are manufactured in the form of films or sheets.

[0006] In order to form a non-bonded area in an electrode including a dry electrode film, there is a method of pattern-coating an adhesion-promoting layer on a current collector. However, this method has low processability and economic efficiency because the pattern coating must be performed according to the specifications of the battery. Another method is to laminate the dry electrode film onto the front surface of the current collector and then remove only a portion of the dry electrode film. However, this method may damage the current collector and / or the dry electrode film.

[0007] The information described above disclosed in the background technology of this invention is intended only to enhance understanding of the background of the present invention and may therefore include information that does not constitute prior art.

[0008]

[0009] The present invention provides a method for manufacturing an electrode for a secondary battery, an electrode for a secondary battery, and a secondary battery, wherein the adhesion between a current collector and a dry electrode film is high even without an adhesion promoting layer, and the occurrence of voids at the interface between the current collector and the dry electrode film is reduced to suppress side reactions of the electrolyte.

[0010] However, the technical problems that the present invention aims to solve are not limited to those described above, and other unmentioned problems can be clearly understood by those skilled in the art from the description of the invention below.

[0011]

[0012] A method for manufacturing an electrode for a secondary battery according to an embodiment of the present invention is provided to solve the above technical problem.

[0013] 1. A method for manufacturing an electrode for a secondary battery includes the step of laminating a dry electrode film onto at least one surface of a current collector having a plurality of protrusions formed thereon and rolling, wherein the current collector has an average height of the plurality of protrusions of 1.7 μm to 5.0 μm, and the rolling is performed using a vibrating roll.

[0014] 2.1 A method for manufacturing an electrode for a secondary battery, wherein the average spacing of the plurality of protrusions in the current collector is 5.0 μm or less.

[0015] 3.1 to 2, a method for manufacturing an electrode for a secondary battery, wherein the plurality of protrusions are formed by electroplating.

[0016] 4.1 to 3. A method for manufacturing an electrode for a secondary battery, wherein the current collector does not include an adhesion promoting layer.

[0017] A method for manufacturing an electrode for a secondary battery, wherein, in accordance with 5.1 to 4, the vibrating roller vibrates at a vibration speed of 10 to 10,000 times per second.

[0018] A method for manufacturing an electrode for a secondary battery, wherein, in accordance with 6.1 to 5, the rolling is performed under a load of 1,000 to 3,000 kg.

[0019] An electrode for a secondary battery according to one embodiment of the present invention is provided to solve the above technical problem.

[0020] 7. An electrode for a secondary battery comprises a current collector having a plurality of protrusions formed thereon; and a dry electrode film positioned on the current collector, wherein the average height of the plurality of protrusions is 1.5 μm to 5.0 μm, and the area ratio of a void at the interface between the current collector and the dry electrode film is 1 to 20%.

[0021] 8.7, an electrode for a secondary battery in which the average spacing of the plurality of protrusions in the current collector is 5.0 μm or less.

[0022] 9.7 to 8, wherein the current collector does not include an adhesion promoting layer, an electrode for a secondary battery.

[0023] An electrode for a secondary battery according to 10.7 to 9, wherein the current collector is a copper foil, the dry electrode film comprises a negative electrode active material and a binder, the negative electrode active material comprises one or more of a carbon-based negative electrode active material and a silicon-based negative electrode active material, the average particle size D50 is 10 μm to 20 μm, and the binder comprises polytetrafluoroethylene (PTFE), polyolefin, or a mixture thereof.

[0024] A secondary battery according to one embodiment of the present invention for solving the above technical problem includes an electrode for a secondary battery or an electrode for a secondary battery manufactured by the method for manufacturing an electrode for a secondary battery.

[0025]

[0026] According to the present invention, the adhesion between the current collector and the dry electrode film is high, so there is no need to form an adhesion-enhancing layer on the current collector, resulting in excellent manufacturing processability.

[0027] According to the present invention, the lifespan and reliability of the battery can be improved by reducing the occurrence of voids at the interface between the current collector and the dry electrode film and suppressing side reactions of the electrolyte.

[0028] However, the effects obtainable through the present invention are not limited to those described above, and other unmentioned technical effects will be clearly understood by those skilled in the art from the description of the invention below.

[0029]

[0030] The following drawings attached to this specification illustrate preferred embodiments of the present invention and serve to further enhance understanding of the technical concept of the present invention together with the detailed description of the invention provided below; therefore, the present invention should not be interpreted as being limited only to the matters described in such drawings.

[0031] Figure 1 is a photograph of the protrusions formed on the entire current collector before rolling.

[0032] FIG. 2 illustrates a method for manufacturing an electrode for a secondary battery according to one embodiment.

[0033] FIG. 3 illustrates an electrode according to one embodiment of the present invention.

[0034] FIGS. 4 to 7 illustrate a secondary battery according to one embodiment.

[0035] Figure 8 is a photograph of the interface between the current collector and the dry electrode film in the electrode of Example 1.

[0036] Figure 9 is a photograph of the interface between the current collector and the dry electrode film in the electrode of Comparative Example 1.

[0037]

[0038] Preferred embodiments of the present invention will be described in detail below with reference to the attached drawings. Prior to this, terms and words used in this specification and claims should not be interpreted as being limited to their ordinary or dictionary meanings. Instead, based on the principle that the inventor can appropriately define the concepts of terms to best describe their invention, they should be interpreted in a meaning and concept consistent with the technical spirit of the present invention. Therefore, the embodiments described in this specification and the configurations illustrated in the drawings are merely some of the most preferred embodiments of the present invention and do not represent all of the technical spirit of the present invention. It should be understood that various equivalents and modifications capable of replacing them may exist at the time of filing this application.

[0039] Additionally, as used herein, “comprise, include” and / or “comprising, including” specify the presence of the mentioned features, numbers, steps, actions, parts, elements, and / or groups thereof, and do not exclude the presence or addition of one or more other features, numbers, actions, parts, elements, and / or groups.

[0040] Additionally, to aid in understanding the invention, the attached drawings are not drawn to actual scale, and the dimensions of some components may be exaggerated. Furthermore, the same reference numerals may be assigned to identical components in different embodiments.

[0041] The statement that two subjects of comparison are 'identical' means that they are 'substantially identical.' Therefore, substantial identity may include deviations considered low in the industry, for example, deviations within 5%. Additionally, the statement that a parameter is uniform in a given area may mean that it is uniform from an average perspective.

[0042] Although terms such as "first," "second," etc., are used to describe various components, it goes without saying that these components are not limited by these terms. These terms are used merely to distinguish one component from another, and unless specifically stated otherwise, the first component may also be the second component.

[0043] Throughout the specification, unless specifically stated otherwise, each component may be singular or plural.

[0044] The fact that any configuration is placed on the "upper (or lower)" of a component or on the "upper (or lower)" of a component may mean not only that any configuration is placed in contact with the upper (or lower) surface of said component, but also that another configuration may be interposed between said component and any configuration placed on (or below) said component.

[0045] Furthermore, where it is stated that one component is "connected," "coupled," or "connected" to another component, it should be understood that while said components may be directly connected or connected to each other, another component may be "interposed" between each component, or that each component may be "connected," "coupled," or "connected" through another component. Additionally, when it is stated that a part is electrically coupled with another part, this includes not only cases where they are directly connected but also cases where they are connected with another component in between.

[0046] Throughout the specification, "A and / or B" means A, B, or A and B unless specifically stated otherwise. That is, "and / or" includes any combination or any combination of the enumerated items. "C to D" means C or more and D or less, unless specifically stated otherwise.

[0047] The terms used in this specification are intended to describe embodiments of the present disclosure and are not intended to limit the present disclosure.

[0048] Hereinafter, a method for manufacturing an electrode for a secondary battery, an electrode for a secondary battery, and a secondary battery including the same according to the present invention will be described in detail.

[0049] The following description applies only to lithium secondary batteries. However, the present invention can be applied to secondary batteries of different metal ions other than lithium, in addition to lithium secondary batteries.

[0050] Method for manufacturing an electrode for a secondary battery

[0051] A method for manufacturing an electrode for a secondary battery according to one embodiment is a method for manufacturing an electrode comprising a dry electrode film.

[0052] The above manufacturing method includes the step of laminating a dry electrode film onto at least one surface of a current collector having a plurality of protrusions and rolling, wherein the average height of the plurality of protrusions of the current collector is 1.7 μm to 5.0 μm, and the rolling is performed using a vibrating roll.

[0053] First, the current collector among the above manufacturing methods will be explained in detail.

[0054] The above-mentioned current collector has a plurality of protrusions formed thereon. Specifically, the plurality of protrusions are formed by extending from the above-mentioned current collector.

[0055] Figure 1 is a photograph of a protrusion formed on a current collector before rolling. Referring to Figure 1, the protrusion formed on the current collector before rolling is needle-shaped and has a sharply protruding outermost surface. Therefore, the protrusion may be advantageous for increasing the adhesion between the current collector and the dry electrode film.

[0056] The average height of the plurality of protrusions in the above current collector is 1.7㎛ to 5.0㎛. If the average height of the plurality of protrusions is 1.7㎛ or more, it may be easier to increase the degree of penetration of the protrusions into the dry electrode film during rolling, thereby increasing the adhesion between the dry electrode film and the current collector. If the average height of the plurality of protrusions is 5.0㎛ or less, there may be an advantageous effect in increasing the adhesion. For example, the average height of a plurality of protrusions in the above-mentioned current collector may be 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3.0, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, 4.0, 4.1, 4.2, 4.3, 4.4, 4.5, 4.6, 4.7, 4.8, 4.9, 5.0㎛, 2.0㎛ to 5.0㎛.

[0057] Here, 'average height' is the average value of the heights of the protrusions, and may be the average value obtained by measuring the height of each protrusion included per unit area of ​​the entire current collector. For example, the average height of the protrusions may be measured as the average value of the heights of 20 protrusions by taking a cross-sectional image of a sample processed for 20 minutes or more using a JEOL CP (IB-19520CCP) ion voltage of 5.0 kV or higher and an air gas of 4.5 or higher with a JEOL Mini SEM (JCM-7000).

[0058] Here, 'height of the protrusion' may refer to the vertical distance from the top of the protrusion to the entire house when the protrusion extends vertically from the entire house.

[0059] According to one embodiment, the average spacing of the plurality of protrusions in the current collector is 5.0 μm or less, for example, 0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3.0, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, 4.0, 4.1, 4.2, 4.3, 4.4, It may be 4.5, 4.6, 4.7, 4.8, 4.9, 5.0㎛, greater than 0㎛ and less than or equal to 5.0㎛, 0.5㎛ to 5.0㎛, or 2.0㎛ to 5.0㎛. Within the above range, it may be easier to increase the adhesion between the dry electrode film and the current collector by increasing the degree of penetration of the protrusions into the dry electrode film. Here, 'average spacing' is the average value of the spacing between protrusions among the current collectors, and may be the average value obtained after measuring the spacing between protrusions included per unit area, and the spacing between protrusions may be measured in the same way as height.

[0060] According to one embodiment, the plurality of protrusions may be needle-shaped. The needle-shaped protrusions are easy to penetrate into the dry electrode film, which can facilitate increasing the adhesion between the current collector and the dry electrode film.

[0061] If the plurality of protrusions can be formed on the current collector with the shape, average height, and average spacing described above, the method of formation may not be restricted. However, in order to form the plurality of protrusions integrally with the current collector, the plurality of protrusions may be formed by plating.

[0062] According to one embodiment, the plurality of protrusions may be formed by plating the current collector. The plating may include electrolytic plating or electroless plating, and preferably may include electrolytic plating.

[0063] The above electrolytic plating may be carried out by the following method, but is not limited thereto. Hereinafter, the description is limited to the case where the current collector is a copper foil, but the present invention is not limited thereto.

[0064] The above electrolytic plating involves preparing an electrolyte by adjusting an aqueous solution containing nickel salts and copper salts to a pH of 1 to 5 (e.g., 2 to 4), introducing a current collector and an insoluble anode into the electrolyte, and then maintaining an electrolyte temperature of 25°C to 45°C and 1 A / dm² 2 Up to 5A / dm 2 The process can be carried out by electrolysis for 1 to 5 seconds at a current density. Examples of the nickel salts include nickel sulfate, nickel nitrate, nickel chloride, nickel acetate, etc., and these may be used alone or in a mixture of two or more types, but are not limited thereto. Examples of the copper salts include copper sulfate, copper nitrate, copper chloride, copper acetate, etc., and these may be used alone or in a mixture of two or more types, but are not limited thereto.

[0065] The concentrations of the nickel salt and the copper salt, respectively, in the above electrolyte can be adjusted considering the average height of the target protrusion.

[0066] The above electrolytic plating may be performed in an electrolyte containing the aforementioned nickel salt and copper salt, but electrolytic plating using an aqueous solution containing copper salt and sulfuric acid may also be additionally performed. Examples of the copper salt include copper sulfate, copper nitrate, copper chloride, copper acetate, etc., and these may be used individually or in a mixture of two or more types, but are not limited thereto. The above electrolytic plating is performed by immersing the electrolytically plated current collector and the insoluble electrode as anodes into the electrolyte at a liquid temperature of 25°C to 45°C and 10 A / dm² 2 Up to 20 A / dm 2It can be performed by electrolysis for 1 to 5 seconds at a current density, but is not limited thereto.

[0067] According to one embodiment, the current collector may not include an adhesion promoting layer.

[0068] Here, the 'adhesion-promoting layer' is a layer formed on the surface of a current collector to increase the adhesion between the current collector and the dry electrode film, and may include a primer layer. For example, the primer layer may be formed from a composition including a conductive material and a binder. The adhesion-promoting layer may also collectively refer to a layer that increases the adhesion between the current collector and the dry electrode film in the dry electrode film.

[0069] A dry electrode film is laminated to at least one surface of the above-mentioned current collector. The lamination can be performed by transporting the above-mentioned current collector and the dry electrode film from different transport units and then laminating them.

[0070] The above dry electrode film may include an active material and a binder. The active material and the binder are each described below.

[0071] In the present invention, the rolling of the current collector and the dry electrode film includes rolling using a vibrating roll.

[0072] As described above, the current collector has a plurality of protrusions formed thereon, so when the current collector and the dry electrode film are simply rolled without a vibrating roll, the degree of penetration of the protrusions into the dry electrode film is low, which may result in a large number of voids at the interface between the current collector and the dry electrode film.

[0073] The aforementioned voids can reduce the adhesion between the current collector and the dry electrode film and increase the interfacial resistance between the current collector and the dry electrode film, thereby degrading the efficiency and lifespan of the battery. The vibrating roller can minimize the occurrence of voids by increasing the degree of penetration of the protrusions into the dry electrode film. Through this, the adhesion between the current collector and the dry electrode film is enhanced, thereby reducing the occurrence of detachment of the dry electrode film from the current collector and lowering the interfacial resistance, which can improve rapid charging and cell lifespan.

[0074] In one embodiment, the vibrating roll is composed of a first vibrating roll positioned above and a second vibrating roll positioned below the laminate of the current collector and the dry electrode film. The first roll and the second roll rotate and vibrate simultaneously with respect to the driving direction of the laminate, thereby allowing the protrusion to penetrate deeper into the dry electrode film. For example, the vibrating roll may vibrate at a vibration speed of 10 to 10,000 times per second. The rotation and vibration of the vibrating roll may be controlled by a control unit connected to the vibrating roll.

[0075] In one embodiment, the rolling can be performed under a load of 1,000 to 3,000 kg.

[0076] FIG. 2 illustrates a method for manufacturing an electrode for a secondary battery according to one embodiment.

[0077] Referring to FIG. 2, the manufacturing method comprises: a current collector conveying unit that conveys a current collector (200) unwound from a winding roll (1); a dry electrode film laminating unit that laminates a dry electrode film (230) to the current collector conveyed from the current collector conveying unit; and a system that rolls the laminate of the current collector and the dry electrode film conveyed from the dry electrode film laminating unit through a vibrating rolling roll (310) having a first vibrating roll (310A) and a second vibrating roll (310B). The dry electrode film (230) can be unwound from the winding rolls (5, 6) and conveyed.

[0078] Although not shown in FIG. 2, the vibration rolling roll (310) can have its vibration speed, rotation speed, etc. controlled by a control unit. Additionally, although not shown in FIG. 2, it may further include a vibration motor that vibrates the vibration rolling roll.

[0079] The above dry electrode film may be a cathode or an anode.

[0080] According to one embodiment, the electrode may be a negative electrode. According to another embodiment, the electrode may be a positive electrode.

[0081] cathode

[0082] The above cathode comprises a current collector; and a dry electrode film located on at least one surface of the current collector, and the dry electrode film may comprise a cathode active material and a binder.

[0083] The above current collector is not particularly limited as long as it provides high conductivity without causing chemical changes in the battery. For example, the above current collector may be stainless steel, aluminum, nickel, titanium, calcined carbon, copper, or aluminum or stainless steel, copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, or a polymer substrate coated with a conductive metal that has been surface-treated with carbon, nickel, titanium, silver, etc.

[0084] The above current collector may have a thickness of 5㎛ to 50㎛, but is not specifically limited thereto. For example, the above current collector may have a thickness of 5㎛ to 20㎛. For example, the above current collector may be a copper foil.

[0085] The above dry electrode film may include a negative electrode active material and a binder, and optionally include an electrode powder including a conductive material. The above dry electrode film may be in the form of a strip or a sheet having a predetermined thickness.

[0086] The above-mentioned negative electrode active material includes a material capable of reversibly intercalating / deintercalating lithium ions, lithium metal, an alloy of lithium metal, a material capable of doping and dedoping lithium, or a transition metal oxide.

[0087] A material capable of reversibly intercalating / deintercalating the above lithium ions may be a carbon-based negative electrode active material, such as crystalline carbon, amorphous carbon, or a combination thereof. Examples of the crystalline carbon include graphite, such as natural graphite or artificial graphite, and examples of the amorphous carbon include soft carbon or hard carbon, mesophase pitch carbide, calcined coke, etc.

[0088] As a material capable of doping and undoping the above lithium, a Si-based negative electrode active material or a Sn-based negative electrode active material may be used. The above Si-based negative electrode active material may be silicon, a silicon-carbon composite, SiOx (0 < x < 2), a Si-based alloy, or a combination thereof.

[0089] The silicon-carbon composite may be a composite of silicon and amorphous carbon. According to one embodiment, the silicon-carbon composite may be in the form of silicon particles and amorphous carbon coated on the surface of the silicon particles.

[0090] The silicon-carbon composite may further include crystalline carbon. For example, the silicon-carbon composite may include a core comprising crystalline carbon and silicon particles and an amorphous carbon coating layer located on the surface of the core.

[0091] In one embodiment, the negative electrode active material may have an average particle size D50 of 10 μm to 20 μm, for example, 13 μm to 18 μm. Within this range, it may be used in the current collector described above.

[0092] The binder described above may be included without particular limitation as long as it is capable of fiberization during the manufacturing step of the dry electrode film described below. Fiberization may refer to a process of micronizing and dividing the polymer. For example, fiberization may be performed using mechanical shear force, etc. The surface of the fiberized polymer fiber is loosened to generate a large number of microfibers, and the dry electrode film may be manufactured by causing the generated microfibers to aggregate the electrode active material and / or the conductive material described below.

[0093] In one embodiment, the binder may comprise polytetrafluoroethylene (PTFE), polyolefin, or a mixture thereof. Specifically, the binder may comprise polytetrafluoroethylene, and more specifically, may be polytetrafluoroethylene. Specifically, the polytetrafluoroethylene may be included in an amount of 60% by weight or more, for example, 90 to 100% by weight, based on the total weight of the binder.

[0094] In another embodiment, the binder may further include a non-fibrous binder. For example, the non-fibrous binder may include one or more of polyethylene oxide, polyvinylidene fluoride, and polyvinylidene fluoride-co-hexafluoropropylene.

[0095] In one embodiment, the binder may be included in the dry electrode film in a fibrous state.

[0096] The above conductive material may include carbon black-based compounds, graphite such as natural graphite or artificial graphite; conductive fibers such as carbon fibers or metal fibers; metal powders such as fluorinated carbon, aluminum, or nickel powder; conductive whiskey such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives.

[0097] In one embodiment, the dry electrode film may comprise 80 to 99 weight% of a negative electrode active material, for example, 90 to 99.5 weight%, 0.5 to 20 weight% of a binder, for example, 0.5 to 10 weight%, and 0.5 to 20 weight% of a conductive material, for example, 0.5 to 10 weight%. Within the above range, the manufacture of the dry electrode film may be easy, and there may be an effect of improving mechanical strength by promoting PTFE fiberization within the electrode.

[0098] anode

[0099] The above positive electrode comprises a current collector; and a dry electrode film located on at least one surface of the current collector, and the dry electrode film may comprise a positive electrode active material and a binder.

[0100] The current collector described above may be the current collector described in the above cathode. For example, the current collector may be an aluminum foil.

[0101] The above dry electrode film may include an electrode powder comprising a positive active material and a binder, and optionally a conductive material. The above dry electrode film may be in the form of a strip or a sheet having a predetermined thickness.

[0102] As the above-mentioned positive electrode active material, a compound capable of reversible intercalation and deintercalation of lithium (a lithated intercalation compound) may be used. Specifically, one or more composite oxides of lithium and a metal selected from cobalt, manganese, nickel, and combinations thereof may be used.

[0103] The above composite oxide may be a lithium transition metal composite oxide, and specific examples include a lithium nickel-based oxide, a lithium cobalt-based oxide, a lithium manganese-based oxide, a lithium iron phosphate-based compound, a cobalt-free nickel-manganese-based oxide, or a combination thereof.

[0104] As an example, a compound represented by any one of the following chemical formulas may be used. Li a A 1-b X b O 2-c D c (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05); Li a Mn 2-b X b O 4-c D c (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05); Li a Ni 1-b-c Co b X c O 2-α D α (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.5, 0<α<2); Li a Ni 1-b-c Mn b X c O 2-α D α (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.5, 0<α<2); Li a Ni b Co c L 1 d G e O2(0.90≤a≤1.8, 0≤b≤0.9, 0≤c≤0.5, 0≤d≤0.5, 0≤e≤0.1); Li a NiG bO2(0.90≤a≤1.8, 0.001≤b≤0.1); Li a CoG b O2(0.90≤a≤1.8, 0.001≤b≤0.1); Li a Mn 1-b G b O2(0.90≤a≤1.8, 0.001≤b≤0.1); Li a Mn2G b O4(0.90≤a≤1.8, 0.001≤b≤0.1); Li a Mn 1-g G g PO4(0.90≤a≤1.8, 0≤g≤0.5); Li (3-f) Fe2(PO4)3(0≤f≤2); Li a FePO4(0.90≤a≤1.8).

[0105] In the above chemical formula, A is Ni, Co, Mn, or a combination thereof; X is Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, a rare earth element, or a combination thereof; D is O, F, S, P, or a combination thereof; G is Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V, or a combination thereof; L 1 is Mn, Al, or a combination thereof.

[0106] In one embodiment, the positive active material may have an average particle size D50 of 10 μm to 50 μm, for example, 20 μm to 40 μm. Within this range, it may be used in the current collector described above.

[0107] The binder and the conductive material may be substantially the same as those described in the cathode.

[0108] In one embodiment, the dry electrode film may comprise 80 to 99 weight% of a positive active material, for example, 90 to 99.5 weight%, 0.5 to 20 weight% of a binder, for example, 0.5 to 10 weight%, and 0.5 to 20 weight% of a conductive material, for example, 0.5 to 10 weight%. Within the above range, the manufacture of the dry electrode film may be easy, and there may be an effect of improving mechanical strength by promoting PTFE fiberization within the electrode.

[0109] The above dry electrode film can be manufactured by the following steps. The method described below can be applied to the cathode and the anode, respectively.

[0110] (a) A process of preparing a powdered mixture comprising an electrode active material, a binder, and a conductive material;

[0111] (b) A process of kneading the above powdered mixture to produce a mass of the mixture;

[0112] (c) a process of crushing the above mixture lumps to obtain electrode powder; and

[0113] (d) A process of calendering the above electrode powder to obtain a self-supporting dry electrode film.

[0114] First, the electrode active material, binder, and conductive material are mixed to prepare a powder mixture. The mixing is performed so that the electrode active material and the binder are uniformly distributed within the mixture, and since the mixture is in powder form, it is not limited to any method that enables simple mixing. However, since the mixture is intended to manufacture a dry electrode film, it does not contain a solvent. The mixing can be performed by dry mixing, for example, by introducing the materials into a device such as a blender.

[0115] In one embodiment, the mixing time is not particularly limited but can be performed for 1 second to 10 minutes. Meanwhile, the mixing speed is not particularly limited but can be appropriately controlled within a range of about 3,000 rpm to 30,000 rpm. As a specific example, the mixing can be prepared by mixing in a mixer at 5,000 rpm to 20,000 rpm for 30 seconds to 2 minutes, specifically at 10,000 rpm to 15,000 rpm for 30 seconds to 5 minutes, in terms of controlling high uniformity and the degree of crystallinity of the binder resin.

[0116] Next, a kneading process is performed on the mixture obtained above to fiberize the binder. The kneading is a step of forming a mixture mass with a solid content of 100% by weight by binding or connecting the electrode active materials and / or the conductive material as the binder fiberizes.

[0117] Specifically, the mixing of step (b) can be controlled at a speed of 10 rpm to 100 rpm. For example, the mixing can be controlled at a speed of 40 rpm or higher or 70 rpm or lower within the above range. The mixing can be performed for 1 minute to 30 minutes. For example, it can be performed for 3 minutes to 7 minutes at a speed of 40 rpm to 70 rpm within the above range. Meanwhile, the mixing can be controlled at a shear rate in the range of 10 / s to 500 / s. In a specific embodiment of the present invention, the mixing can be performed for 1 minute to 30 minutes, and the shear rate can be controlled at a range of 30 / s to 100 / s.

[0118] In addition, this mixing step can be performed under high temperature and pressure conditions above atmospheric pressure, and more specifically, under pressure conditions higher than atmospheric pressure. More specifically, the mixing can be performed on the mixture in a range of 70°C to 200°C, specifically 90°C to 150°C.

[0119] In addition, it can be performed at a pressure above atmospheric pressure, specifically at a pressure of 1 atm to 3 atm, and more specifically at 1.1 atm to 3 atm. If performed outside the above range at a pressure too high, it is undesirable because excessive shear force and pressure may be applied, which may cause the formed fibers to be cut or the density of the mixture lumps to become too high. That is, according to the present invention, the intended effect of the present invention can be achieved when a low-shear mixing process is performed under high temperature and pressure above atmospheric pressure conditions instead of high-shear mixing.

[0120] Next, a step is performed to obtain a powder for electrodes by grinding the mixture mass produced through the above mixing step again.

[0121] Specifically, although the mixture mass produced through the above kneading may be calendered immediately, in this case, the mixture mass may need to be pressed under high pressure and high temperature to produce a thin film, and consequently, problems may arise such as the film density becoming too high or a uniform film not being obtained. According to the present invention, the produced mixture mass undergoes the grinding step.

[0122] The grinding described above is not limited but can be performed using known grinding devices such as blenders or grinders. In a specific embodiment of the present invention, the grinding speed may be controlled within a range of 3,000 rpm to 30,000 rpm. Meanwhile, the grinding time may be appropriately controlled within a range of 1 second to 10 minutes. However, the grinding speed and time are not specifically limited to the above ranges. As a specific example, the grinding may be performed for 30 seconds to 10 minutes at a speed of 5,000 rpm to 20,000 rpm, or for 30 seconds to 5 minutes at a speed of 10,000 rpm to 18,000 rpm. By performing sufficient grinding within the above ranges, it is easy to form into a film and the degree of fine powder generation can be reduced.

[0123] A dry electrode film is manufactured by heating and pressing the above electrode powder. Specifically, the electrode powder obtained by completing the grinding step as described above is fed into a calendering process.

[0124] The electrode powder is heat-pressed by a calendering process and processed into a sheet-shaped dry electrode film. The calendering process may be performed by a pair of opposing calendering rollers. In one embodiment of the present invention, the calendering process may be performed in such a manner that the electrode powder passes through a plurality of calendering rollers.

[0125] The above electrode powder may be pretreated before performing the calendering process.

[0126] The above pretreatment process can be performed by applying heat to the electrode powder so that the temperature of the powder is maintained at 80°C or higher, preferably 100°C or higher, for a predetermined period of time. The time of the pretreatment process can be performed for 1 minute or more and can be appropriately adjusted depending on the amount of powder. For example, the temperature of the powder can be maintained at a temperature of 80°C or higher for 1 minute or more, or at a temperature of 100°C or higher for 1 minute or more. Alternatively, the heating temperature of the electrode powder is preferably controlled to be below the melting point of the binder resin to prevent deterioration of the electrode components contained in the electrode powder, for example, the binder resin used. For example, it can be controlled to 320°C or lower. The above pretreatment process can be performed using a commonly used heating device, such as a convection oven or an infrared heating device. At this time, it is preferable that the electrode powder be stirred so that it does not remain stagnant while being heated.

[0127] electrodes for secondary batteries

[0128] An electrode for a secondary battery according to one embodiment comprises a current collector having a plurality of protrusions formed thereon; and a dry electrode film positioned on the current collector, wherein the average height of the plurality of protrusions is 1.5 μm to 5.0 μm, and the area ratio of a void at the interface between the current collector and the dry electrode film is 1% to 20%.

[0129] The "average height of multiple protrusions" among the above electrodes can be measured by the method described above.

[0130] The above "void" refers to an empty space generated by the low degree of penetration of protrusions into the dry electrode film, and may mean an empty space existing at the interface between the current collector and the dry electrode film. The void may reduce the adhesion between the current collector and the dry electrode film and increase the interfacial resistance between the current collector and the dry electrode film, thereby degrading the efficiency and lifespan of the battery.

[0131] The "void area ratio" mentioned above can be measured by processing the SEM cross-sectional image taken to measure the average height of the protrusions above using the Threshold function of the ImageJ program. Since the voids are photographed darker than the current collector or the active material, the brightness of the Threshold is adjusted to include the voids, and then the ratio of the area occupied by the voids to the total area of ​​the interface in the thickness direction of the active material and the current collector is calculated. Specifically, the brightness of the current collector and the active material is 130 to 200, and the brightness of the voids is 0 to 100.

[0132] The plurality of protrusions protrude to a predetermined height and penetrate into the dry electrode film. The plurality of protrusions can provide an anchoring effect that physically bonds the current collector and the dry electrode film. Therefore, by the dry electrode film and the plurality of protrusions coming into contact and adhering to each other, the adhesion between the first region of the current collector and the dry electrode film can be increased without an adhesion-enhancing layer, thereby allowing for excellent manufacturing processability of the electrode.

[0133] The average height of the plurality of protrusions is 1.5㎛ to 5.0㎛. If the average height of the plurality of protrusions is 1.5㎛ or more, the adhesion between the current collector and the dry electrode film can be increased without an adhesion promoting layer. If the average height of the plurality of protrusions is 5.0㎛ or less, there may be an effect of physical bonding with the dry electrode film. For example, the average height of the above-mentioned protrusions may be 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3.0, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, 4.0, 4.1, 4.2, 4.3, 4.4, 4.5, 4.6, 4.7, 4.8, 4.9, 5.0㎛, 1.5㎛ or more and less than 5.0㎛. The above-mentioned average height may be achieved by the method for manufacturing the electrode of the secondary battery described above.

[0134] The above electrode has a void area ratio of 1% to 20%. If the void area ratio exceeds 20%, there are many empty spaces at the interface between the current collector and the dry electrode film, which lowers the adhesion between the current collector and the dry electrode film and increases the interfacial resistance, thereby deteriorating cell life or efficiency characteristics and increasing the likelihood of the film detaching from the current collector when immersed in the electrolyte. If the void area ratio is less than 1%, the surface area of ​​the active material in contact with the current collector increases, which may cause adverse reactions at the interface. For example, the void area ratio may be 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20%, 5% to 15%.

[0135] The above average height and the above area ratio can be realized by the method for manufacturing the electrode of the secondary battery described above.

[0136] FIG. 3 is a cross-sectional view of an electrode for a secondary battery according to one embodiment.

[0137] Referring to FIG. 3, the electrode for a secondary battery comprises a current collector (200); a dry electrode film (300) located on one side of the current collector (200) and comprising an active material (301) and a binder (302), and the current collector (200) comprises a plurality of protrusions (210) formed extending from the current collector (200). The electrode for a secondary battery may include a void (220) at the interface between the current collector (200) and the dry electrode film (300), and the area ratio of the void (220) at the interface between the current collector (200) and the dry electrode film (300) is 1% to 20%.

[0138] secondary battery

[0139] Another embodiment is a secondary battery, wherein the secondary battery includes an electrode for a secondary battery according to the first embodiment.

[0140] In one embodiment, the battery may include a positive electrode according to one embodiment and a negative electrode according to one embodiment. In another embodiment, the battery may include a positive electrode and a negative electrode according to one embodiment. In yet another embodiment, the battery may include a positive electrode and a negative electrode according to one embodiment.

[0141] The above-mentioned cathode may be manufactured using a composition comprising the cathode active material described above. The cathode active material is the same as described above. The composition may further include a binder and / or a conductive material. The cathode may be manufactured through a wet process. The binder and conductive material may be selected from ordinary types known to those skilled in the art.

[0142] The above-mentioned anode may be manufactured using a composition comprising the anode active material described above. The above-mentioned anode active material is the same as described above. The composition may further include a binder and / or a conductive material. The above-mentioned anode may be manufactured through a wet process. The binder and the conductive material may be selected from ordinary types known to those skilled in the art.

[0143] A lithium secondary battery may further include an electrolyte. The electrolyte for a lithium secondary battery includes a non-aqueous organic solvent and a lithium salt.

[0144] The above-mentioned non-aqueous organic solvent serves as a medium through which ions involved in the electrochemical reaction of the battery can move.

[0145] The above-mentioned non-aqueous organic solvent may be a carbonate-based, ester-based, ether-based, ketone-based, or alcohol-based solvent, a non-protic solvent, or a combination thereof, and may be used alone or in a mixture of two or more types.

[0146] In addition, when using carbonate-based solvents, cyclic carbonates and chain carbonates can be mixed and used.

[0147] Depending on the type of lithium secondary battery, a separator may be present between the positive and negative electrodes. As such a separator, polyethylene, polypropylene, polyvinylidene fluoride, or a multilayer film of two or more layers thereof may be used.

[0148] The above separator may include a porous substrate and a coating layer comprising an organic material, an inorganic material, or a combination thereof located on one or both sides of the porous substrate.

[0149] The above organic material may include a polyvinylidene fluoride-based antibody or a (meth)acrylic-based polymer.

[0150] The above inorganic materials are Al2O3, SiO2, TiO2, SnO2, CeO2, MgO, NiO, CaO, GaO, ZnO, ZrO2, Y2O3, It may include, but is not limited to, inorganic particles selected from SrTiO3, BaTiO3, Mg(OH)2, boehmite, and combinations thereof.

[0151] The above organic and inorganic materials may exist mixed in a single coating layer, or may exist in a stacked form with a coating layer containing organic materials and a coating layer containing inorganic materials.

[0152] The above lithium secondary battery can be classified into cylindrical, prismatic, pouch, coin, etc., depending on its shape. FIGS. 4 to 7 are schematic diagrams illustrating a lithium secondary battery according to one embodiment, where FIG. 4 is a cylindrical battery, FIG. 5 is a prismatic battery, and FIGS. 6 and 7 are pouch-type batteries. Referring to FIGS. 4 to 7, the lithium secondary battery (100) may include an electrode assembly (40) having a separator (30) interposed between a positive electrode (10) and a negative electrode (20), and a case (50) in which the electrode assembly (40) is housed. The positive electrode (10), the negative electrode (20), and the separator (30) may be impregnated with an electrolyte (not shown). The lithium secondary battery (100) may include a sealing member (60) that seals the case (50) as in FIG. 4. In addition, in FIG. 5, the lithium secondary battery (100) may include a positive lead tab (11) and a positive terminal (12), a negative lead tab (21) and a negative terminal (22). As shown in FIG. 6 and FIG. 7, the lithium secondary battery (100) may include electrode tabs (70), namely a positive tab (71) and a negative tab (72), which serve as electrical passages for inducing current formed in the electrode assembly (40) to the outside.

[0153] A lithium secondary battery according to one embodiment of the present invention may be applied to automobiles, mobile phones, and / or various types of electric devices, etc., but the present invention is not limited thereto.

[0154] The aforementioned lithium secondary battery can be used to manufacture a battery pack. A battery pack according to an embodiment of the present invention includes an assembly in which individual batteries are electrically connected and a pack housing that accommodates the same. Components such as a busbar for electrical connection of the batteries, a cooling unit, and external terminals may be further included.

[0155] A battery pack may be mounted in a vehicle. The vehicle may be, for example, an electric vehicle, a hybrid vehicle, or a plug-in hybrid vehicle. The vehicle includes a four-wheeled vehicle or a two-wheeled vehicle. A vehicle according to one embodiment of the present invention includes a battery pack according to one embodiment of the present invention. The vehicle operates by receiving power from the battery pack according to one embodiment of the present invention.

[0156]

[0157] Examples and comparative examples of the present invention are described below. However, the following examples are merely one example of the present invention, and the present invention is not limited to the following examples.

[0158]

[0159] Example 1

[0160] Manufacturing of dry electrode films

[0161] 96.7 wt% of artificial graphite as a cathode active material, 1.8 wt% of polytetrafluoroethylene as a binder, and 1.5 wt% of carbon black were introduced into a blender and mixed at 10,000 rpm for 1 minute to obtain a mixture. Next, the obtained mixture was introduced into a kneader and kneaded at 110°C at a speed of 60 rpm for 5 minutes to obtain a mass of the mixture, after which the mass of the mixture was introduced into a blender and ground at 14,000 rpm for 60 seconds to obtain an electrode powder. Subsequently, the electrode powder was repeatedly compressed using a calender roll (roll diameter: 200 mm, roll temperature: 70°C) to obtain a dry electrode film (thickness 117 μm).

[0162] The entire house is gilded

[0163] A copper current collector (copper foil) was plated using an electroplating method to produce a current collector having a plurality of protrusions formed extending from the current collector, and the average height of the plurality of protrusions is 2.5 μm.

[0164] Manufacturing of electrodes

[0165] A laminate was manufactured by placing the dry electrode film manufactured above on the manufactured current collector.

[0166] An electrode for a secondary battery was manufactured by rolling the above laminated body under a load of 1600 kg while passing it between opposing vibrating rolling rolls.

[0167] Example 2

[0168] A dry electrode film (thickness 117 μm) and a current collector (average height of multiple protrusions 2.5 μm) were prepared in the same manner as in Example 1.

[0169] A dry electrode was manufactured in the same manner as in Example 1, except that the vibration speed when driving the vibrating rolling roll in Example 1 was increased by 10%.

[0170] Comparative Example 1

[0171] A dry electrode film (thickness 117 μm) and a current collector (average height of multiple protrusions 2.5 μm) were manufactured in the same manner as in Example 1.

[0172] A laminate was manufactured by placing the dry electrode film manufactured above on the manufactured current collector.

[0173] An electrode for a secondary battery was manufactured by rolling the above laminated body under a load of 1600 kg while passing it between opposing rolling rolls (without vibration).

[0174]

[0175] The electrodes in the examples and comparative examples were evaluated as follows.

[0176] (1) Average height of the protrusions on the entire sample: The average height of 20 protrusions is calculated by taking cross-sectional images of a sample processed for more than 20 minutes with an ion voltage of 5.0 kV or higher and an air gas of 4.5 or higher using a JEOL CP (IB-19520CCP) and a JEOL Mini SEM (JCM-7000).

[0177] (2) Void area ratio: SEM cross-sectional image taken to measure the average height of the protrusion

[0178] It is processed and measured using the Threshold function of the ImageJ program. Since voids are captured darker than the current collector or active material, the brightness of the Threshold is adjusted to include the voids, and then the percentage of the area of ​​the interface between the active material and the current collector that the voids occupy is measured.

[0179] (3) Adhesion strength between current collector and electrode film: Measured by the Peel Test of the Tinius Olsen UTM (universal testing machine). An electrode with a stacked current collector and a dry electrode film was cut to a specimen size of 5 cm x 2.5 cm. One jig of the UTM (universal testing machine) was connected to the current collector, and the other jig was connected to the dry electrode film. The peel strength was measured when the dry electrode film was peeled at a peeling speed of 100 min / mm and a peeling angle of 180° at 25 degrees.

[0180] (4) Interface between current collector and electrode film: The results of the interface between the current collector and the dry electrode film were obtained using SEM and are shown in Figures 8 and 9.

[0181] Example 1 Example 2 Comparative Example 1 Average height of protrusions on the current collector before rolling 2.5㎛ 2.5㎛ 2.5㎛ Average height of protrusions on the current collector in the electrode after rolling 2.3㎛ 2.1㎛ 2.5㎛ Void area ratio 10% 5% 35% Adhesion strength between current collector and dry electrode film 1.7gf / mm 2.3gf / mm 0.5gf / mm

[0182] As shown in Table 1 above, according to the method of manufacturing the electrode of the example, the adhesion between the current collector and the dry electrode film is high, so it is possible to eliminate the need to form an adhesion-enhancing layer on the current collector. In addition, the method of manufacturing the electrode of the example reduces the occurrence of voids at the interface between the current collector and the dry electrode film, thereby suppressing side reactions of the electrolyte and increasing the lifespan and reliability of the battery. Furthermore, referring to FIG. 8, it can be seen that there are very few voids at the interface between the current collector and the dry electrode film.

[0183] However, as shown in Table 1 above, the adhesion between the current collector and the dry electrode film was low according to the manufacturing method of the electrode of the comparative example. In addition, it can be seen that voids occurred at the interface between the current collector and the dry electrode film and the adhesion between the current collector and the dry electrode film was low according to the manufacturing method of the electrode of the comparative example. Furthermore, referring to FIG. 9, it can be seen that there are many voids at the interface between the current collector and the dry electrode film.

[0184]

[0185] Although the present invention has been described above by limited embodiments and drawings, the present invention is not limited thereto, and it is obvious that various modifications and variations are possible within the scope of the technical spirit of the present invention and the equivalent scope of the claims described below by those skilled in the art to which the present invention belongs.

Claims

1. A step of laminating a dry electrode film onto at least one surface of a current collector having a plurality of protrusions formed thereon and rolling, and The above current collector has an average height of the plurality of protrusions of 1.7㎛ to 5.0㎛. A method for manufacturing an electrode for a secondary battery, wherein the above rolling is performed using a vibrating roll.

2. A method for manufacturing an electrode for a secondary battery according to claim 1, wherein the average spacing of the plurality of protrusions in the current collector is 5.0 μm or less.

3. A method for manufacturing an electrode for a secondary battery according to claim 1, wherein the plurality of protrusions are formed by electrolytic plating.

4. A method for manufacturing an electrode for a secondary battery according to claim 1, wherein the current collector does not include an adhesion promoting layer.

5. A method for manufacturing an electrode for a secondary battery according to claim 1, wherein the vibrating roller vibrates at a vibration speed of 10 to 10,000 times per second.

6. A method for manufacturing an electrode for a secondary battery according to claim 1, wherein the rolling is performed under a load of 1,000 to 3,000 kg.

7. A current collector having multiple protrusions formed thereon; and It includes a dry electrode film located on the above current collector, and The average height of the plurality of protrusions is 1.5㎛ to 5.0㎛, and An electrode for a secondary battery, wherein the area ratio of a void at the interface between the current collector and the dry electrode film is 1 to 20%.

8. An electrode for a secondary battery according to claim 7, wherein the average spacing of the plurality of protrusions in the current collector is 5.0 μm or less.

9. An electrode for a secondary battery according to claim 7, wherein the current collector does not include an adhesion promoting layer.

10. In paragraph 7, the current collector is a copper foil, and The above dry electrode film comprises a negative electrode active material and a binder, and The above negative electrode active material comprises one or more of a carbon-based negative electrode active material and a silicon-based negative electrode active material, and has an average particle size D50 of 10㎛ to 20㎛, and The above binder comprises polytetrafluoroethylene (PTFE), polyolefin, or a mixture thereof, for an electrode for a secondary battery.