Depolymerized polyol composition and method for preparing same

The depolymerization of waste polyurethane into a high-quality polyol composition with controlled molecular weights and alkylene oxide additions addresses the issues of low-quality recycled polyols and toxic emissions, enhancing recycling efficiency and reducing costs.

WO2026240607A1PCT designated stage Publication Date: 2026-11-19MITSUI CHEM & SKC POLYURETHANES INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2026/096934
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-07-11
Filing Date
2026-05-13
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Existing methods for recycling waste polyurethane produce low-quality polyol due to the presence of hydroxyl and amine groups, requiring additional processing, and generate carcinogenic byproducts, while incineration results in toxic hydrogen cyanide emissions.

Method used

A depolymerization process using specific molecular weight ranges of polyols and alkylene oxide additions to produce a high-quality polyol composition, including a mixture of polyols with varying molecular weights and controlled hydroxyl group density to enhance reactivity and physical properties.

Benefits of technology

The process yields a high-quality polyol with controlled properties, enabling efficient recycling of waste polyurethane and reducing environmental and economic costs by improving the quality and reactivity of the recycled material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2026096934_19112026_PF_FP_ABST
    Figure KR2026096934_19112026_PF_FP_ABST
Patent Text Reader

Abstract

A recycled polyol according to the present invention includes 25% to 50% of a first polyol, having a number average molecular weight (Mn) of more than 1,130 g / mol, and 5% to 18% of a second polyol, having a number average molecular weight (Mn) of 660 g / mol to 1,130 g / mol, on the basis of the total amount of a composition, with the remainder comprising a polyol having a number average molecular weight (Mn) of less than 660 g / mol.
Need to check novelty before this filing date? Find Prior Art

Description

Depolymerization polyol composition and method for preparing the same The examples relate to a depolymerization polyol composition and a method for preparing the same. Polyurethane is widely used not only in the manufacture of soft foam used as cushioning material for automobiles and sofas, and rigid foam used as insulation for refrigerators and buildings, but also in paints, adhesives, and coatings. These polyurethanes have the advantage of being able to control their physical properties in various ways depending on the selection of polyols and isocyanates and processing conditions, but the amount of polyurethane waste (hereinafter referred to as waste polyurethane) that is scrapped and discarded is not small, and effective recycling measures are required due to the toxicity and corrosiveness caused by hydrogen cyanide (HCN) generated during the incineration of waste polyurethane. Methods for recycling waste polyurethane include physical methods that utilize crushed waste polyurethane, and chemical methods that utilize hydrolysis and depolymerization reactions. Since the hydrolysis method using water has a low conversion rate compared to process conditions and is not economically viable, and the depolymerization reaction using amines generates carcinogens as byproducts, research is continuing on glycol depolymerization reactions, which are easy to process and highly economical. For example, Korean registered patent No. 10-1012185 discloses a method for converting waste polyurethane into polyol by glycol depolymerization, but compounds having hydroxyl groups and compounds having amine groups are also produced. Therefore, the polyol produced in this way has the disadvantage that it has low quality and requires an additional process to reduce compounds having hydroxyl groups and compounds having amine groups in order to improve quality. The example aims to provide a high-quality polyol composition and a method for manufacturing the same by depolymerizing waste polyurethane. The depolymerization polyol composition according to the present invention comprises a first polyol having a number average molecular weight (Mn) greater than 1,800 g / mol in an amount of 20% to 45% based on the total area of ​​the composition, a second polyol having a number average molecular weight of 430 g / mol to 1,800 g / mol in an amount of 2% to 18% based on the total area of ​​the composition, and the remaining component comprises a polyol having a number average molecular weight (Mn) less than 430 g / mol. In a depolymerization polyol composition according to one embodiment, a third polyol having a number average molecular weight (Mn) of 320 g / mol to 430 g / mol may be further included in an amount of 3% to 15% based on the total area of ​​the composition. In a depolymerization polyol composition according to one embodiment, a fourth polyol having a number average molecular weight (Mn) of 210 g / mol to 320 g / mol may be further included in an amount of 0.1% to 10% based on the total area of ​​the composition. In a depolymerization polyol composition according to one embodiment, a fifth polyol having a number average molecular weight (Mn) of 100 g / mol to 210 g / mol may be further included in an amount of 10% to 30% based on the total area of ​​the composition. In a depolymerization polyol composition according to one embodiment, a sixth polyol having a number average molecular weight (Mn) of less than 100 g / mol may be further included in an amount of 5% to 30% based on the total area of ​​the composition. Meanwhile, the alkylene oxide addition depolymerization polyol composition according to the present invention comprises a seventh polyol with an alkylene oxide addition having a number average molecular weight (Mn) of 3,000 g / mol to 10,000 g / mol in an amount of 1% to 20% based on the total area of ​​the composition, a eighth polyol with an alkylene oxide addition having a number average molecular weight (Mn) of 100 g / mol to 3,000 g / mol in an amount of 60% to 95% based on the total area of ​​the composition, and the remaining component comprises a polyol having a number average molecular weight (Mn) of less than 100 g / mol. Meanwhile, a method for preparing a depolymerized polyol composition according to the present invention comprises the steps of: preparing a crushed material containing waste polyurethane; and mixing the crushed material and a polyhydric alcohol and heat-treating to form a regenerated polyol, wherein the regenerated polyol comprises a first polyol having a number average molecular weight (Mn) greater than 1,800 g / mol in an amount of 20% to 45% based on the total area of ​​the composition, and a second polyol having a number average molecular weight (Mn) of 430 g / mol to 1,800 g / mol in an amount of 2% to 18% based on the total area of ​​the composition, and the remaining component comprises a polyol having a number average molecular weight (Mn) less than 430 g / mol. In a method for preparing a depolymerized polyol composition according to one embodiment, the heat treatment may be performed at 100°C to 400°C. In a method for preparing a depolymerized polyol composition according to one embodiment, the polyhydric alcohol may be one or more selected from the group consisting of ethylene glycol, tripropylene glycol, diethylene glycol, thiodiethylene glycol, neopentyl glycol, triethylene glycol, tetraethylene glycol, dipropylene glycol, tripropylene glycol, and pentaerythritol. In a method for preparing a depolymerized polyol composition according to one embodiment, a first catalyst is used in the step of forming the regenerated polyol, and the first catalyst may be one or more selected from the group consisting of potassium hydroxide, sodium hydroxide, potassium acetate, zinc acetate, a mixture of sodium acetate and strontium acetate, and a mixture of potassium acetate and strontium acetate. Meanwhile, a method for preparing an alkylene oxide addition depolymerization polyol composition according to the present invention comprises the steps of: preparing a crushed material containing waste polyurethane; mixing the crushed material and a polyhydric alcohol and heat-treating to form a regenerated polyol; and reacting an alkylene oxide with the regenerated polyol to form an addition polymerization polyol, wherein the addition polymerization polyol has a number average molecular weight (Mn) of 3,000 g / mol to 10,000 g / mol and contains a seventh polyol with added alkylene oxide in an amount of 1% to 20% based on the total area of ​​the composition, and contains an eighth polyol with added alkylene oxide having a number average molecular weight (Mn) of 100 g / mol to 3,000 g / mol in an amount of 60% to 95% based on the total area of ​​the composition, and the remaining component comprises a polyol having a number average molecular weight (Mn) of less than 100 g / mol. In a method for preparing an alkylene oxide addition depolymerization polyol composition according to one embodiment, the alkylene oxide may be one or more selected from the group consisting of ethylene oxide, propylene oxide, butylene oxide, pentene oxide, hexene oxide, cyclopentene oxide, and cyclohexane oxide. In a method for preparing an alkylene oxide addition depolymerization polyol composition according to one embodiment, the step of forming the addition polymerization polyol may be performed at 100°C to 400°C. In a method for preparing an alkylene oxide addition depolymerization polyol composition according to one embodiment, a second catalyst is used in the step of forming the addition polymerization polyol, and the second catalyst may be one or more selected from the group consisting of phosphazene, potassium hydroxide, sodium hydroxide, cesium hydroxide, imidazole-based catalysts, and dicyanide metal catalysts. The regenerated polyol according to the present invention comprises a ninth polyol having a number average molecular weight (Mn) greater than 1,130 g / mol in an amount of 25% to 50% based on the total area of ​​the composition, a tenth polyol having a number average molecular weight (Mn) of 660 g / mol to 1,130 g / mol in an amount of 5% to 18% based on the total area of ​​the composition, and the remaining component comprises a polyol having a number average molecular weight (Mn) less than 660 g / mol. The regenerated polyol according to one embodiment may further include a first polyol having a number average molecular weight (Mn) of 280 g / mol to 660 g / mol in an amount of 10% to 25% based on the total area of ​​the composition. The regenerated polyol according to one embodiment may further include a 12th polyol having a number average molecular weight (Mn) of less than 280 g / mol in an amount of 25% to 50% based on the total area of ​​the composition. The regenerated polyol according to one embodiment may have a hydroxyl group value of 250 mgKOH / g to 450 mgKOH / g. The recycled polyol according to one embodiment may have a viscosity of 100 mPa·s to 10,000 mPa·s at 25°C. Meanwhile, a method for manufacturing a regenerated polyol according to the present invention comprises the steps of: introducing a polyhydric alcohol and a solvent into a reactor and heating the temperature of the reactor to 170°C to 250°C; crushing waste polyurethane to prepare a crushed material, introducing the crushed material and a catalyst into the reactor to produce a depolymerizing agent mixture; and cooling the reactor to 90°C to 190°C. The method comprises the step of obtaining a regenerated polyol by filtering the above depolymerization mixture through a filter with a diameter of 200 μm to 300 μm; wherein the regenerated polyol comprises a ninth polyol having a number average molecular weight (Mn) greater than 1,130 g / mol in an amount of 25% to 50% based on the total area of ​​the composition, and a tenth polyol having a number average molecular weight (Mn) of 660 g / mol to 1,130 g / mol in an amount of 5% to 18% based on the total area of ​​the composition, and the remaining component comprises a polyol having a number average molecular weight (Mn) less than 660 g / mol. In a method for manufacturing a regenerated polyol according to one embodiment, the polyhydric alcohol and the solvent may be mixed in a weight ratio of 1:1 to 10:1. In a method for manufacturing a regenerated polyol according to one embodiment, the solvent may have a weight-average molecular weight (Mw) of 1,000 g / mol to 4,000 g / mol. In a method for producing a regenerated polyol according to one embodiment, the solvent may have a hydroxyl group value of 30 mgKOH / g to 150 mgKOH / g. In a method for producing a regenerated polyol according to one embodiment, the polyhydric alcohol may have a weight-average molecular weight (Mw) of 100 g / mol to 400 g / mol. In a method for producing a regenerated polyol according to one embodiment, the polyhydric alcohol may have a hydroxyl group value of 300 mgKOH / g to 700 mgKOH / g. In a method for producing a regenerated polyol according to one embodiment, the polyhydric alcohol may be one or more selected from the group consisting of ethylene glycol, tripropylene glycol, diethylene glycol, thiodiethylene glycol, neopentyl glycol, triethylene glycol, tetraethylene glycol, dipropylene glycol, tripropylene glycol, and pentaerythritol. In a method for producing a regenerated polyol according to one embodiment, the catalyst may be one or more selected from the group consisting of potassium hydroxide, sodium hydroxide, potassium acetate, zinc acetate, a mixture of sodium acetate and strontium acetate, and a mixture of potassium acetate and strontium acetate. The depolymerizable polyol composition according to the present invention comprises a 14th polyol having a number average molecular weight (Mn) of 700 g / mol to 2,500 g / mol in an amount of 7% to 20% based on the total area of ​​the composition, a 15th polyol having a number average molecular weight (Mn) of less than 100 g / mol in an amount of less than 5% based on the total area of ​​the composition, and the remaining components comprise a polyol having a number average molecular weight (Mn) of 100 g / mol or more and less than 700 g / mol and a polyol having a number average molecular weight (Mn) of more than 2,500 g / mol. According to one embodiment, the depolymerized polyol composition may further include a 16th polyol having a number average molecular weight (Mn) of more than 2,500 g / mol in an amount of 10% to 40% based on the total area of ​​the composition. According to one embodiment, the depolymerized polyol composition may further include a polyol of the 17th having a number average molecular weight (Mn) of 100 g / mol to 250 g / mol in an amount of 30% to 50% based on the total area of ​​the composition. According to one embodiment, the depolymerized polyol composition may further include a polyol of the 18th having a number average molecular weight (Mn) of 250 g / mol to 700 g / mol in an amount of 10% to 30% based on the total area of ​​the composition. Meanwhile, the alkylene oxide addition depolymerization polyol composition according to the present invention comprises a sixth polyol with an alkylene oxide addition having a number average molecular weight (Mn) of less than 260 g / mol in an amount of 0.01% to 10% based on the total area of ​​the composition, a ninth polyol with an alkylene oxide addition having a number average molecular weight (Mn) of more than 3,000 g / mol in an amount of 1% to 20% based on the total area of ​​the composition, and the remaining component comprises a polyol having a number average molecular weight (Mn) of 260 g / mol to 3,000 g / mol. According to one embodiment, the alkylene oxide addition depolymerization polyol composition may further include a 20th polyol having a number average molecular weight (Mn) of 260 g / mol to 3,000 g / mol in an amount of 70% to 90% based on the total area of ​​the composition. Meanwhile, a method for preparing a depolymerized polyol composition according to the present invention comprises the steps of: preparing a crushed material containing waste polyurethane; and mixing the crushed material and a polyhydric alcohol and heat-treating to form a regenerated polyol, wherein the regenerated polyol comprises a 14th polyol having a number average molecular weight (Mn) of 700 g / mol to 2,500 g / mol in an amount of 7% to 20% based on the total area of ​​the composition, and the regenerated polyol comprises a 15th polyol having a number average molecular weight (Mn) of less than 100 g / mol in an amount of less than 5% based on the total area of ​​the composition, and the remaining components comprise a polyol having a number average molecular weight (Mn) of 100 g / mol or more and less than 700 g / mol and a polyol having a number average molecular weight (Mn) greater than 2,500 g / mol. According to one embodiment, the heat treatment can be performed at 100°C to 400°C. According to one embodiment, the polyhydric alcohol may be one or more selected from the group consisting of ethylene glycol, tripropylene glycol, diethylene glycol, thiodiethylene glycol, neopentyl glycol, triethylene glycol, tetraethylene glycol, dipropylene glycol, tripropylene glycol, and pentaerythritol. According to one embodiment, a first catalyst is used in the step of forming the regenerated polyol, and the first catalyst may be one or more selected from the group consisting of potassium hydroxide, sodium hydroxide, potassium acetate, zinc acetate, a mixture of sodium acetate and strontium acetate, and a mixture of potassium acetate and strontium acetate. Meanwhile, a method for preparing an alkylene oxide addition depolymerization polyol composition according to the present invention comprises the steps of: preparing a crushed material containing waste polyurethane; mixing the crushed material and a polyhydric alcohol and heat-treating to form a regenerated polyol; and reacting an alkylene oxide with the regenerated polyol to form an addition polymerization polyol, wherein the addition polymerization polyol has a number average molecular weight (Mn) of less than 260 g / mol and includes a polyol of the 18th with added alkylene oxide in an amount of 0.01% to 10% based on the total area of ​​the composition, wherein the addition polymerization polyol has a number average molecular weight (Mn) greater than 3,000 g / mol and includes a polyol of the 19th with added alkylene oxide in an amount of 1% to 20% based on the total area of ​​the composition, and the remaining component includes a polyol having a number average molecular weight (Mn) of 260 g / mol to 3,000 g / mol. According to one embodiment, the alkylene oxide may be one or more selected from the group consisting of ethylene oxide, propylene oxide, butylene oxide, pentene oxide, hexene oxide, cyclopentene oxide, and cyclohexane oxide. According to one embodiment, the step of forming the addition polymerization polyol can be performed at 100°C to 400°C. According to one embodiment, a second catalyst is used in the step of forming the addition polymerization polyol, and the second catalyst may be one or more selected from the group consisting of phosphazene, potassium hydroxide, sodium hydroxide, cesium hydroxide, imidazole-based catalysts, and dicyanide metal catalysts. A method for preparing a depolymerized polyol composition according to one embodiment enables the resolution of environmental problems and cost reduction by recycling waste polyurethane, as the high reactivity between waste polyurethane and polyhydric alcohols results in a high yield of the finally prepared depolymerized polyol composition. When an alkylene oxide is added to a depolymerization polyol composition according to one embodiment, the density of hydroxyl groups is controlled to improve reactivity with isocyanate, thereby allowing for the control of physical properties such as viscosity of the depolymerization polyol composition. When an alkylene oxide is added to a depolymerized polyol composition according to one embodiment, the chain of the polyol may be lengthened and the molecular weight may be increased, and the tensile strength and flexibility of the polyurethane foam manufactured using this can be controlled. Figure 1 is a graph showing the results of gel permeation chromatography of the depolymerized polyol composition according to Preparation Example 1. Figure 2 is a graph showing the results of gel permeation chromatography of the depolymerized polyol composition according to Preparation Example 4. Figure 3 is a graph showing the results of gel permeation chromatography of the depolymerized polyol composition according to Preparation Example 8. Figure 4 is a graph showing the results of gel permeation chromatography of the depolymerized polyol composition according to Preparation Example 12. Figure 5 is a graph showing the results of gel permeation chromatography of the depolymerized polyol composition according to Preparation Example 14. Figure 6 is a graph showing the results of gel permeation chromatography of the depolymerized polyol composition according to Preparation Example 16. The invention is described in detail below through embodiments. The embodiments are not limited to those disclosed below and may be modified in various forms as long as the essence of the invention is not altered. In this specification, when a part is described as "comprising" a certain component, this means that, unless specifically stated otherwise, it does not exclude other components but may include additional components. In addition, all numerical ranges representing physical property values, dimensions, etc. of the components described in this specification should be understood to be modified by the term "approximately" in all cases unless otherwise specified. In this specification, terms such as first, second, primary, secondary, etc. are used to describe various components, and said components are not limited by said terms. These terms are used solely for the purpose of distinguishing one component from another. In addition, ppm, which is stated as the content in each composition, may be a unit expressed on a weight basis. The depolymerized polyol composition according to the example may be a regenerated polyol. That is, the depolymerized polyol composition according to the example may be a composition comprising regenerated polyols. In addition, in the depolymerization polyol composition according to the example, the content of each polyol can be determined by gel permeation chromatography (GPC). That is, in the depolymerization polyol composition according to the example, the content of each polyol can be determined as a percentage of the area determined by gel permeation chromatography. That is, the content of each polyol can be determined as a percentage of the area corresponding to each number-average molecular weight out of the total area determined by GPC. The depolymerizable polyol composition according to one embodiment may be selected from at least two of the group consisting of a first polyol, a second polyol, a third polyol, a fourth polyol, a fifth polyol, or a sixth polyol. A depolymerized polyol according to one embodiment may include a first polyol and a second polyol. A depolymerized polyol composition according to one embodiment may include a first polyol having a number average molecular weight (Mn) greater than about 1,800 g / mol in an amount of about 20% to about 45% based on the total area of ​​the composition, a second polyol having a number average molecular weight (Mn) of about 430 g / mol to about 1,800 g / mol in an amount of about 2% to about 18% based on the total area of ​​the composition, and the remaining component may include a polyol having a number average molecular weight (Mn) less than about 430 g / mol. The number average molecular weight of the first polyol may be greater than about 1,800 g / mol, greater than about 2,000 g / mol, greater than about 2,200 g / mol, greater than about 2,400 g / mol, or greater than about 2,500 g / mol. At the same time, the number average molecular weight of the first polyol may be less than about 20,000 g / mol, less than about 10,000 g / mol, less than about 10,000 g / mol, less than about 8,000 g / mol, or less than about 6,000 g / mol. The number average molecular weight of the first polyol may be about 1,800 g / mol to about 20,000 g / mol, about 2,800 g / mol to about 20,000 g / mol, about 2,200 g / mol to about 20,000 g / mol, about 2,400 g / mol to about 20,000 g / mol, about 2,500 g / mol to about 20,000 g / mol, or about 1,800 g / mol to about 10,000 g / mol. A depolymerizable polyol composition according to one embodiment may include the first polyol in an amount greater than about 20%, greater than about 22%, greater than about 24%, greater than about 25%, or about 27% based on the total area of ​​the depolymerizable polyol composition. At the same time, a depolymerizable polyol composition according to one embodiment may include the first polyol in an amount less than about 45%, less than about 43%, less than about 41%, less than about 39%, or less than about 37% based on the total area of ​​the depolymerizable polyol composition. A depolymerized polyol composition according to one embodiment may contain the first polyol in an amount of about 20% to about 45%, about 22% to about 45%, about 24% to about 43%, about 25% to about 41%, or about 27% to 39% based on the total area of ​​the depolymerized polyol composition. In a depolymerization polyol composition according to one embodiment, the first polyol may be represented by the following chemical formula 1. [Chemical Formula 1] In the above chemical formula 1, m can be 1 to 2 and n can be 1 to 2. In the above chemical formula 1, n can be 2 and m can be 1. In the above chemical formula 1, n and m can be 1. In the above chemical formula 1, X includes a structure derived from diisocyanate, and Y and Z may include a structure derived from glycol. In the above chemical formula 1, X may have a structure derived from a polyol having a number average molecular weight of 1,100 g / mol to 24,500 g / mol. In the above chemical formula 1, X may include propylene oxide (PO) or ethylene oxide (EO) as a repeating structure, or may include a structure in which propylene oxide and ethylene oxide are repeated in a block, random, or alternating form. For example, in the above chemical formula 1, X can be a structure such as -[CH₂CH(CH₃)O]n CH2-, which is a PO single repeating structure; -[CH₂CH₂O]n CH2-, which is an EO single repeating structure; -[CH₂CH₂O]m-[CH₂CH(CH₃)O]n CH2-, which is an EO-PO block copolymer structure; and -[CH₂CH₂O / CH₂CH(CH₃)O]m CH2-, which is an EO / PO random copolymer structure. In the above chemical formula 1, in X, m and n can each be integers from 1 to 500. In the above chemical formula 1, Y may include a unit derived from methylene diphenyl diisocyanate (MDI) or toluene diisocyanate (TDI). In the above chemical formula 1, Y can be represented by the following chemical formula 1-1 or chemical formula 1-2. [Chemical Formula 1-1] [Chemical Formula 1-2] In the above chemical formula 1, Z may include a unit derived from ethylene glycol, propylene glycol, 1,4-butanediol, 1,3-propanediol, diethylene glycol, and triethylene glycol. In the above chemical formula 1, Z may include - C2H4-, - C3H6-, - C4H8-, - C2H4- O - C2H4- or - C2H4- O - C2H4- O - C2H4-. In the above chemical formula 1, Z can be represented by the following chemical formula 1-3. [Chemical Formula 1-3] Since the depolymerization polyol composition according to the example contains the first polyol in the above amount, it has appropriate viscosity and / or appropriate reactivity and can extend the chain during the polymerization process. That is, in the depolymerization polyol composition according to the example, the first polyol can be used as a viscosity modifier, a reactive curing agent, or a polymer chain extender. The number average molecular weight of the second polyol may be greater than about 430 g / mol, greater than about 435 g / mol, greater than about 440 g / mol, or greater than about 450 g / mol. At the same time, the number average molecular weight of the second polyol may be less than about 1,800 g / mol, less than about 1,500 g / mol, less than about 1,000 g / mol, or less than about 800 g / mol. The number average molecular weight of the second polyol may be about 430 g / mol to about 1,800 g / mol, about 435 g / mol to about 1,800 g / mol, about 450 g / mol to about 1,800 g / mol, about 430 g / mol to about 1,500 g / mol, about 450 g / mol to about 1,500 g / mol, or about 450 g / mol to about 1,000 g / mol. In a depolymerization polyol composition according to one embodiment, the second polyol may be included in an amount greater than about 2%, greater than about 3%, greater than about 4%, or greater than about 5% based on the total area of ​​the composition. At the same time, in a depolymerization polyol composition according to one embodiment, the second polyol may be included in an amount less than about 18%, less than about 17%, or less than about 16% based on the total area of ​​the composition. In a depolymerized polyol composition according to one embodiment, the second polyol may be included in an amount of about 2% to about 18%, about 3% to about 17%, about 4% to about 16%, or about 5% to about 15% based on the total area of ​​the composition. The second polyol may be a triol. The second polyol may include three to five hydroxyl groups. In a depolymerization polyol composition according to one embodiment, the second polyol may be represented by the following chemical formula 2. [Chemical Formula 2] In the above chemical formula 2, X may have a structure derived from a trifunctional polyol having a number average molecular weight of about 400 g / mol to about 1,000 g / mol. X may have a structure in which trimethylolpropane (TMP) or glycerol is the core and propylene oxide (PO) or ethylene oxide (EO) is included as a repeating structure, or PO and EO are included as a repeating structure in a block, random, or alternating form. For example, in the above chemical formula 2, X can be a structure such as TMP-[PO]n (n=1~30), which is a PO single repeating structure; TMP-[EO]n (n=1~30), which is an EO single repeating structure; TMP-[EO]m-[PO]n, which is an EO-PO block copolymer structure; and TMP-[EO / PO]p, which is an EO / PO random copolymer structure. Here, m, n, and p can each be integers from 1 to 30. The above second polyol can be represented by the following chemical formula 2-1. [Chemical Formula 2-1] In the above chemical formula 2-1, R can be a structure such as -[CH₂CH(CH₃)O]n CH2-, a PO single repeating structure; -[CH₂CH₂O]n CH2-, an EO single repeating structure; -[CH₂CH₂O]m-[CH₂CH(CH₃)O]n CH2-, an EO-PO block copolymer structure; and -[CH₂CH₂O / CH₂CH(CH₃)O]m CH2-, an EO / PO random copolymer structure. In R, m and n can each be integers from 1 to 200. Since the depolymerization polyol composition according to the example contains the second polyol in the above amount, it has appropriate viscosity and / or appropriate reactivity and can extend the chain during the polymerization process. That is, in the depolymerization polyol composition according to the example, the second polyol can be used as a viscosity modifier, a reactive curing agent, or a polymer chain extender. The number average molecular weight of the third polyol may be greater than about 320 g / mol, greater than about 330 g / mol, or greater than about 350 g / mol. At the same time, the number average molecular weight of the third polyol may be less than about 400 g / mol, less than about 390 g / mol, or less than about 380 g / mol. The depolymerization polyol composition according to the example may include the third polyol in an amount greater than about 4 wt%, greater than about 5%, or greater than about 6% based on the total area of ​​the composition. At the same time, the depolymerization polyol composition according to the example may include the third polyol in an amount less than about 15%, less than about 13%, or less than about 11% based on the total area of ​​the composition. The number average molecular weight of the third polyol may be about 320 g / mol to about 430 g / mol, about 330 g / mol to about 420 g / mol, or about 340 g / mol to about 410 g / mol. In addition, the depolymerized polyol composition according to the example may include the third polyol in an amount of about 3% to about 15%, about 4% to about 13%, or about 6% to about 11% based on the total area of ​​the composition. The above third polyol may include a linear diol. In a depolymerization polyol composition according to one embodiment, the third polyol may be represented by the following chemical formula 3. [Chemical Formula 3] In the above chemical formula 3, X may be derived from a linear polyol having a number average molecular weight of 280 g / mol to 400 g / mol. X may include propylene oxide (PO) or ethylene oxide (EO) as a repeating structure, or may include PO and EO as a repeating structure in a block, random, or alternating form. For example, the above X can be a structure such as -[CH₂CH(CH₃)O]n CH2- (n=1~10), which is a PO single repeating structure; -[CH₂CH₂O]n CH2- (n=1~10), which is an EO single repeating structure; -[CH₂CH₂O]m-[CH₂CH(CH₃)O]n CH2-, which is an EO-PO block copolymer structure; and -[CH₂CH₂O / CH₂CH(CH₃)O]p CH2-, which is an EO / PO random copolymer structure. Here, m, n, and p can each be integers from 1 to 10. Since the depolymerizable polyol composition according to the example contains the third polyol in the above amount, it has appropriate viscosity and / or appropriate reactivity and can provide hydroxyl groups during the polymerization process. That is, in the depolymerizable polyol composition according to the example, the third polyol can be used as a molecular weight regulator, a viscosity regulator, or a terminal hydroxyl group provider. The fourth polyol may include an amine group and a hydroxyl group. The fourth polyol may include a prepolymer including an amine group and a hydroxyl group. The fourth polyol may include one amine group and two hydroxyl groups. In a depolymerized polyol composition according to one embodiment, the number average molecular weight of the fourth polyol may be greater than about 210 g / mol, greater than about 230 g / mol, or greater than about 250 g / mol. At the same time, the number average molecular weight of the fourth polyol may be less than about 320 g / mol, less than about 300 g / mol, or less than about 280 g / mol. The depolymerization polyol composition according to the example may include the fourth polyol in an amount greater than about 0.5%, greater than about 1%, or greater than about 2% based on the total area of ​​the composition. At the same time, the depolymerization polyol composition according to the example may include the fourth polyol in an amount less than about 8%, less than about 7%, or less than about 6% based on the total area of ​​the composition. The number average molecular weight of the above-mentioned fourth polyol may be about 210 g / mol to about 320 g / mol, about 220 g / mol to about 310 g / mol, about 230 g / mol to about 300 g / mol, or about 230 g / mol to about 320 g / mol. The depolymerized polyol composition according to the example may include the fourth polyol in an amount of about 0.1% to about 10%, about 1% to about 8%, about 2% to about 6%, or about 0.1% to about 4% based on the total area of ​​the composition. In a depolymerization polyol composition according to one embodiment, the fourth polyol may be represented by the following chemical formula 4. [Chemical Formula 4] In the above chemical formula 4, X may include a unit derived from methylene diphenyl diisocyanate (MDI) or toluene diisocyanate (TDI). In the above chemical formula 4, Y and Z may each independently include units derived from ethylene glycol, propylene glycol, 1,4-butanediol, 1,3-propanediol, diethylene glycol, and triethylene glycol. In the above chemical formula 4, Y and Z may each independently include - C2H4-, - CH2(CH3)CH2-, - C3H6-, - C4H8-, - C2H4- O - C2H4- or - C2H4- O - C2H4- O - C2H4-. Since the depolymerization polyol composition according to the example contains the fourth polyol in the above amount, it has appropriate viscosity and / or appropriate reactivity, and can provide appropriate molecular weight and appropriate curability during the polymerization process. That is, in the depolymerization polyol composition according to the example, the fourth polyol can be used as a viscosity modifier, a molecular weight modifier, or a curability imparting agent. The fifth polyol may include an amine group and a hydroxyl group. The fifth polyol may include a prepolymer including an amine group and a hydroxyl group. The fifth polyol may include one amine group and one hydroxyl group. The number average molecular weight of the fifth polyol may be greater than about 100 g / mol, greater than about 120 g / mol, greater than about 130 g / mol, or greater than about 150 g / mol. At the same time, the number average molecular weight of the fifth polyol may be less than about 210 g / mol, less than about 200 g / mol, or less than about 190 g / mol. The number average molecular weight (Mn) of the above fifth polyol may be about 100 g / mol to about 210 g / mol, about 120 g / mol to about 200 g / mol, or about 130 g / mol to about 200 g / mol. In addition, the depolymerization polyol composition according to the example may include the fifth polyol in an amount greater than about 12%, greater than about 13%, or greater than about 14% based on the total area of ​​the composition. At the same time, the depolymerization polyol composition according to the example may include the fifth polyol in an amount less than about 23%, less than 21%, or less than 18% based on the total area of ​​the composition. The depolymerized polyol composition according to the example may further include the fifth polyol in an amount of about 10% to about 30%, about 12% to about 23%, or about 14% to about 18% based on the total area of ​​the composition. In a depolymerization polyol composition according to one embodiment, the fifth polyol may be represented by the following chemical formula 5. [Chemical Formula 5] In the above chemical formula 5, Y may include a unit derived from methylene diphenyl diisocyanate (MDI) or toluene diisocyanate (TDI). In the above chemical formula 5, Y can be represented by the above chemical formula 1-1 or the above chemical formula 1-2. In the above chemical formula 5, Z may include a unit derived from ethylene glycol, propylene glycol, 1,4-butanediol, 1,3-propanediol, diethylene glycol, and triethylene glycol. In the above chemical formula 5, Z may include at least one of - C2H4-, - CH2(CH3)CH2-, - C3H6-, - C4H8-, - C2H4- O - C2H4-, or - C2H4- O - C2H4- O - C2H4-. Since the depolymerization polyol composition according to the example contains the fifth polyol in the above amount, it has appropriate viscosity and / or appropriate reactivity, and can provide appropriate molecular weight and appropriate curability during the polymerization process. That is, in the depolymerization polyol composition according to the example, the fifth polyol can be used as a viscosity modifier, a molecular weight modifier, or a curability imparting agent. The above sixth polyol may include glycol. The sixth polyol may be selected from at least one of the group consisting of ethylene glycol, propylene glycol, 1,4-butanediol, 1,3-propanediol, diethylene glycol, or triethylene glycol. The number average molecular weight of the above-mentioned sixth polyol may be about 10 g / mol to less than about 100 g / mol. The depolymerized polyol composition according to the example may include the sixth polyol in an amount of about 5% to 30%, about 1% to about 20%, or about 3% to about 15% based on the total area of ​​the composition. The number average molecular weight of the sixth polyol may be about 10 g / mol to about 95 g / mol or about 10 g / mol to about 90 g / mol. The depolymerization polyol composition according to the example may include the sixth polyol in an amount greater than about 4%, greater than about 6%, or greater than about 7% based on the total area of ​​the composition. At the same time, the depolymerization polyol composition according to the example may include the sixth polyol in an amount less than about 13 wt, less than about 11%, or less than about 10% based on the total area of ​​the composition. In a depolymerization polyol composition according to one embodiment, the sixth polyol may be represented by the following chemical formula 6. [Chemical Formula 6] In the above chemical formula 6, Z may include at least one unit derived from ethylene glycol, propylene glycol, 1,4-butanediol, 1,3-propanediol, diethylene glycol, or triethylene glycol. In the above chemical formula 6, Z may include at least one of - C2H4-, - CH2(CH3)CH2-, - C3H6-, - C4H8-, - C2H4- O - C2H4-, or - C2H4- O - C2H4- O - C2H4-. Since the depolymerizable polyol composition according to the example contains the sixth polyol in the above amount, it has appropriate viscosity and / or appropriate reactivity and can provide hydroxyl groups during the polymerization process. That is, in the depolymerizable polyol composition according to the example, the sixth polyol can be used as a molecular weight regulator, a viscosity regulator, or a terminal hydroxyl group provider. An addition polymerization polyol composition according to one embodiment comprises the depolymerization polyol composition and may further comprise at least one of the seventh polyol or the eighth polyol. An addition polymerization polyol composition according to one embodiment comprises at least two of the first polyol, the second polyol, the third polyol, the fourth polyol, the fifth polyol, and the sixth polyol, and may comprise at least one of the seventh polyol or the eighth polyol. An addition polymerization polyol composition according to one embodiment can be formed by an addition reaction between the depolymerization polyol composition and an alkylene oxide. An addition polymerization polyol composition according to one embodiment may be formed by adding propylene oxide and / or ethylene oxide to the depolymerization polyol composition. The seventh polyol may be formed by an alkylene oxide addition reaction. The seventh polyol may be formed by the addition polymerization of propylene oxide and / or ethylene oxide to at least one of the first polyol, the second polyol, the third polyol, the fourth polyol, the fifth polyol, or the sixth polyol. The number average molecular weight of the seventh polyol may be about 3,000 g / mol to about 10,000 g / mol. The addition polymerization polyol composition according to the example may contain the seventh polyol in an amount of about 1% to about 20% based on the total area of ​​the composition. Additionally, the eighth polyol may be formed by an alkylene oxide addition reaction. The eighth polyol may be formed by the addition polymerization of propylene oxide and / or ethylene oxide to at least one of the first polyol, the second polyol, the third polyol, the fourth polyol, the fifth polyol, or the sixth polyol. The number average molecular weight of the eighth polyol may be about 100 g / mol to about 3,000 g / mol. The addition polymerization polyol composition according to the example may contain the eighth polyol in an amount of about 60% to about 95% based on the total area of ​​the composition. The above seventh polyol may include a triol. The number average molecular weight of the seventh polyol may be greater than about 3,000 g / mol, greater than about 3,500 g / mol, or greater than about 4,000 g / mol. At the same time, the number average molecular weight of the seventh polyol may be less than about 13,000 g / mol, less than about 10,000 g / mol, less than about 8,000 g / mol, or less than about 7,000 g / mol. An addition polymerization polyol composition according to one embodiment may include the seventh polyol in an amount greater than about 1%, greater than about 3%, greater than about 5%, greater than about 6%, or greater than about 10% based on the total weight of the composition. At the same time, an addition polymerization polyol composition according to one embodiment may include the seventh polyol in an amount less than about 20%, less than about 19%, or less than about 17% based on the total weight of the composition. The above seventh polyol can be represented by the following chemical formula 7. [Chemical Formula 7] In the above chemical formula 7, X may include a unit derived from a trifunctional polyol (triol) having a number average molecular weight of 2,600 g / mol to 19,500 g / mol. In the above chemical formula 7, X may include a structure in which propylene oxide (PO) or ethylene oxide (EO) is repeatedly bonded to trimethylolpropane (TMP) or glycerol. Additionally, in the above chemical formula 7, X may include a structure in which PO and EO are repeatedly bonded to trimethylolpropane (TMP) or glycerol in a block, random, or alternating form. For example, in the above chemical formula 7, X may be TMP-[PO]n (n=20~200), which is a PO single repeating structure, or TMP-[EO]m-[PO]n, which is an EO / PO block copolymer structure. Here, m and n are the number of repetitions, and the number average molecular weight of X can be appropriately adjusted within the range of 2,600~19,500 g / mol. In the above chemical formula 7, A includes a repeating propylene oxide structure and may be in the form of 2 to 10 repeated branched chains. The above seventh polyol can be represented by the following chemical formula 7-1. [Chemical Formula 7-1] In the above chemical formula 7-1, R may include at least one of - [PO]n - CH2-, - [EO]n - CH2-, or - [EO]m - [PO]n - CH2-. In addition, the above m and the above n may be 1 to 1000. The above m and the above n may have appropriate values ​​so that the seventh polyol has a number average molecular weight as described above. Since the addition polymerization polyol composition according to the example contains the seventh polyol in the above amount, it has appropriate viscosity and / or appropriate curability and can provide an appropriate molecular weight during the polymerization process. That is, in the addition polymerization polyol composition according to the example, the seventh polyol can be usefully used as a viscosity modifier, a curability imparting agent, and a molecular weight modifier. The eighth polyol may include three or more hydroxyl groups. The eighth polyol may include three to six hydroxyl groups. The eighth polyol may include three to five hydroxyl groups. The eighth polyol may include a prepolymer containing urethane bonds. The eighth polyol may include one to four urethane bonds. The number average molecular weight of the eighth polyol may be greater than about 100 g / mol, greater than about 600 g / mol, greater than about 800 g / mol, or greater than about 1,000 g / mol. At the same time, the number average molecular weight of the eighth polyol may be less than about 3,000 g / mol, less than about 2,700 g / mol, or less than about 2,500 g / mol. The number average molecular weight of the eighth polyol may be about 100 g / mol to about 3000 g / mol, about 600 g / mol to about 2700 g / mol, about 800 g / mol to about 2500 g / mol, or about 1000 g / mol to about 3000 g / mol. The addition polymerization polyol composition according to the example may include the eighth polyol in an amount greater than about 60%, greater than about 65%, greater than about 70%, or greater than about 80% based on the total area of ​​the composition. At the same time, the addition polymerization polyol composition according to the example may include the eighth polyol in an amount less than about 95%, less than about 93%, or less than about 91% based on the total area of ​​the composition. The addition polymerization polyol composition according to the example may include the eighth polyol in an amount of about 60% to about 95%, about 65% to about 90%, about 70% to about 90%, or about 80% to about 95% based on the total area of ​​the composition. The above eighth polyol may be represented by any one of the following chemical formula 8-1, the following chemical formula 8-2, or the following chemical formula 8-3. [Chemical Formula 8-1] In the above chemical formula 8-1, Y may include a structure derived from methylene diphenyl diisocyanate (MDI) or toluene diisocyanate (TDI). In the above chemical formula 8-1, R1 and R2 may each independently include at least one unit derived from ethylene glycol, propylene glycol, 1,4-butanediol, 1,3-propanediol, diethylene glycol, or triethylene glycol. In the above chemical formula 8-1, R1 and R2 may each independently include at least one of - C2H4-, - CH2(CH3)CH2-, - C3H6-, - C4H8-, - C2H4- O - C2H4-, or - C2H4- O - C2H4- O - C2H4-. In the above chemical formula 8-1, A1 and A2 are each branched chain structures containing propylene oxide (PO) as a repeating structure, and may include a structure that repeats the -CH2CH(CH3)O- repeating unit 2 to 10 times. The compound of Chemical Formula 8-1 above can be usefully used as a curability imparting agent, viscosity modifier, or polymer chain extender for depolymerized polyol compositions. [Chemical Formula 8-2] In the above chemical formula 8-2, Y may be a structure derived from methylene diphenyl diisocyanate (MDI) or toluene diisocyanate (TDI). In the above chemical formula 8-2, Y may include the above chemical formula 1-1 or the above 1-2. In the above chemical formula 8-2, Z may include at least one of units derived from ethylene glycol, propylene glycol, 1,4-butanediol, 1,3-propanediol, diethylene glycol, or triethylene glycol. In the above chemical formula 8-2, A1 and A2 are each branched chain structures containing propylene oxide as a repeating structure, and may be structures repeated 2 to 10 times. In the above chemical formula 8-2, A1 and A2 may each independently include at least one of - C2H4-, - CH2(CH3)CH2-, - C3H6-, - C4H8-, - C2H4- O - C2H4-, or - C2H4- O - C2H4- O - C2H4-. The compound of Chemical Formula 8-2 above can be usefully used as a curability imparting agent, viscosity modifier, or polymer chain extender for depolymerized polyol compositions. [Chemical Formula 8-3] In the above chemical formula 8-3, Z may include at least one of units derived from ethylene glycol, propylene glycol, 1,4-butanediol, 1,3-propanediol, diethylene glycol, or triethylene glycol. In the above chemical formula 8-3, Z may each independently include at least one of - C2H4-, - CH2(CH3)CH2-, - C3H6-, - C4H8-, - C2H4- O - C2H4-, or - C2H4- O - C2H4- O - C2H4-. In the above chemical formula 8-3, A1 and A2 are each branched chains containing a repeating structure of propylene oxide (-CH₂CH(CH₃)O-) and may be structures repeated 2 to 10 times. The compound of Chemical Formula 8-3 above can be usefully used as a viscosity modifier, molecular weight modifier, or terminal hydroxyl group provider for depolymerization polyol compositions. A method for preparing a depolymerized polyol composition according to an example comprises the steps of: preparing a crushed material containing waste polyurethane; and mixing the crushed material and a polyhydric alcohol and heat-treating to form a regenerated polyol, wherein the regenerated polyol may contain a first polyol having a number average molecular weight (Mn) of more than 1,800 g / mol in an amount of 20% to 45% based on the total area of ​​the composition, and the regenerated polyol may contain a second polyol having a number average molecular weight (Mn) of 430 g / mol to 1,800 g / mol in an amount of 2% to 18% based on the total area of ​​the composition. The depolymerization polyol composition according to the example may include the following steps. (1) Step of preparing a crushed material containing waste polyurethane The above step involves collecting the waste polyurethane and physically crushing it. The waste polyurethane may exist in various forms, such as foam or coatings. By forming the waste polyurethane into small particles or powder, the reaction surface area can be increased during the depolymerization process, thereby enhancing the reaction rate and efficiency. The above-mentioned crushed material can be produced by crushing hard waste polyurethane foam or soft waste polyurethane foam. When polyols are manufactured using such waste polyurethane, there are effects of cost reduction and environmental protection. For example, the above-mentioned crushed material may be manufactured by crushing polyurethane used in furniture and mattresses, polyurethane from scrapped car seats, or polyurethane used in electronic and electrical products. Specifically, the above-mentioned crushed material used in the present invention may be manufactured by crushing Slabstock Foam (SLAB), which is a polyurethane foam continuously produced in the form of large blocks. (2) A step of mixing the above-mentioned pulverized material and polyhydric alcohol and heat-treating to form a regenerated polyol. The above step is a step in which pulverized waste polyurethane is mixed with polyhydric alcohol and heated, thereby breaking down the cross-links of the polyurethane and forming a regenerated polyol through a depolymerization reaction. The polyols formed by the decomposition of the above polyurethane may have a number average molecular weight of 1,000 g / mol to 5,000 g / mol. For example, the decomposition product may have a number average molecular weight of 1,500 g / mol to 4,500 g / mol, or 2,000 g / mol to 4,000 g / mol. The above polyhydric alcohol may be used in a ratio of about 60% to 400% by weight, about 80% to 350% by weight, or about 100% to 300% by weight, based on the weight of the ground material. The polyalcohol may be one or more selected from the group consisting of ethylene glycol, tripropylene glycol, diethylene glycol, thiodiethylene glycol, neopentyl glycol, triethylene glycol, tetraethylene glycol, dipropylene glycol, tripropylene glycol, and pentaerythritol. Preferably, the polyalcohol may be one or more selected from ethylene glycol, tripropylene glycol, and diethylene glycol. Preferably, the polyalcohol may be tripropylene glycol. The step of forming the regenerated polyol above may involve performing a depolymerization reaction at 100°C to 400°C for 1 to 10 hours. Specifically, after mixing the ground material and the polyhydric alcohol, the regenerated polyol may be obtained by performing a depolymerization reaction at 100°C to 400°C, 120°C to 380°C, 130°C to 380°C, 150°C to 370°C, or 180°C to 370°C for 2 to 9 hours, 3 to 8 hours, or 4 to 7 hours. If the depolymerization temperature and time satisfy the above ranges, the reaction rate can be appropriately controlled to produce a regenerated polyol with a uniform molecular weight. A first catalyst may be used in the step of forming the regenerated polyol. The first catalyst may include one or more selected from the group consisting of potassium hydroxide, sodium hydroxide, potassium acetate, zinc acetate, a mixture of sodium acetate and strontium acetate, and a mixture of potassium acetate and strontium acetate. Preferably, the first catalyst may be one or more selected from potassium hydroxide and sodium hydroxide. By using the catalyst, a polyol composition of uniform molecular weight can be produced by appropriately controlling the reaction rate. The first catalyst may be added in an amount of 0.0001% to 5% by weight based on the total weight of the ground material. For example, the first catalyst may be added in an amount of 0.0002% to 3% by weight or 0.0003% to 2% by weight based on the total weight of the ground material. The above-mentioned regenerated polyol comprises a first polyol having a number average molecular weight (Mn) of more than 1,800 g / mol in an amount of 20% to 45% based on the total area of ​​the composition, and the above-mentioned regenerated polyol comprises a second polyol having a number average molecular weight (Mn) of 430 g / mol to 1,800 g / mol in an amount of 2% to 18% based on the total area of ​​the composition. The above-mentioned pulverized material and the above-mentioned polyhydric alcohol may be mixed in a weight ratio of 1:1 to 10:1. For example, the above-mentioned pulverized material and the above-mentioned polyhydric alcohol may be mixed in a weight ratio of 1:1 to 9:1, 2:1 to 8:1, or 3:1 to 7:1. When mixed in the above weight ratios, the reactivity between the waste polyurethane and the polyhydric alcohol is increased, which may result in a high yield of the finally produced depolymerized polyol composition. Accordingly, a depolymerization polyol composition according to the example can be prepared. In order for the depolymerization polyol composition according to the example to include the first polyol, the second polyol, the third polyol, the fourth polyol, the fifth polyol, and the sixth polyol in the amounts as described above, the process conditions for manufacturing the regenerated polyol can be appropriately controlled. In order for the depolymerization polyol composition according to the example to include the first polyol, the second polyol, the third polyol, the fourth polyol, the fifth polyol, and the sixth polyol in the above amounts, the weight ratio of the ground material and the polyhydric alcohol, the content of the catalyst, the depolymerization reaction time, and the depolymerization process temperature can be appropriately controlled. In order for the depolymerization polyol composition according to the example to include the first polyol, the second polyol, the third polyol, the fourth polyol, the fifth polyol, and the sixth polyol in the same amount as above, the weight ratio of the waste polyurethane foam crushed material and the polyhydric alcohol may be about 2:1 to about 1:2, about 1.5:1 to 1:1.5, about 1.3:1 to about 1:1.3, or about 1.2:1 to about 1:1.2. In addition, for the depolymerization polyol composition according to the example to include the first polyol, the second polyol, the third polyol, the fourth polyol, the fifth polyol, and the sixth polyol in the above amounts, the catalyst may be included in the reactants in an amount of about 1000 ppm to about 5000 ppm, about 1200 ppm to about 4500 ppm, or about 1500 ppm to about 4000 ppm based on the weight of the total reactants. In addition, in order for the depolymerization polyol composition according to the example to include the first polyol, the second polyol, the third polyol, the fourth polyol, the fifth polyol, and the sixth polyol in the amounts as described above, the reactants may be depolymerized at a temperature of about 180°C to about 240°C, about 190°C to about 230°C, or about 200°C to about 220°C for about 5 hours to about 8 hours, about 5 hours to about 7 hours, or about 4 hours or about 7 hours. (3) A step of reacting the above regenerated polyol with alkylene oxide to form an addition polymerized polyol. That is, an alkylene oxide is reacted with the depolymerization polyol composition according to the example, and an addition polymerization polyol composition according to the example can be formed. The above step is a step of increasing the molecular weight of a polyol composition by reacting an alkylene oxide with a regenerated polyol obtained through depolymerization to perform an addition polymerization reaction. Specifically, the above step can perform an addition polymerization reaction with the alkylene oxide through a reactive hydroxyl group located at the end of the main chain of the regenerated polyol. The above addition polymerization polyol composition comprises a seventh polyol with an alkylene oxide added having a number average molecular weight (Mn) of 3,000 g / mol to 10,000 g / mol in an amount of 1% to 20% based on the total area of ​​the composition, and the addition polymerization polyol comprises an eighth polyol with an alkylene oxide added having a number average molecular weight (Mn) of 100 g / mol to 3,000 g / mol in an amount of 60% to 95% based on the total area of ​​the composition, and the remaining component comprises a polyol having a number average molecular weight (Mn) of less than 100 g / mol. The above alkylene oxide may be one or more selected from the group consisting of ethylene oxide, propylene oxide, butylene oxide, pentene oxide, hexene oxide, cyclopentene oxide, and cyclohexane oxide. Preferably, the above alkylene oxide may be one or more selected from ethylene oxide and propylene oxide. In one embodiment, the alkylene oxide may be used in combination with ethylene oxide (EO) and propylene oxide (PO). The content of the ethylene oxide and propylene oxide can be adjusted to a ratio of 1:1 to 10:1. Increasing the ratio of the ethylene oxide may result in a more uniform increase in molecular weight. The above-mentioned recycled polyol may contain 2 to 10 hydroxyl groups per molecule. For example, the above-mentioned recycled polyol may contain 2 to 8, 3 to 8, or 4 to 7 hydroxyl groups per molecule. When the number of hydroxyl groups per molecule of the above-mentioned recycled polyol satisfies the above range, reactivity with alkylene oxide is increased, thereby forming a polyol composition having a high molecular weight. When a polyurethane foam is formed using such a polyol composition, it can have excellent mechanical properties. The step of forming the addition polymerization polyol above may involve performing a depolymerization reaction at 100°C to 400°C for 1 to 10 hours. Specifically, after mixing alkylene oxide with the regenerated polyol, an additional polymerization reaction may be performed at 100°C to 400°C, 120°C to 380°C, 130°C to 380°C, 150°C to 370°C, or 180°C to 370°C for 2 to 9 hours, 3 to 8 hours, or 4 to 7 hours to obtain a polyol composition. If the addition polymerization temperature and time satisfy the above ranges, a polyol composition of uniform molecular weight can be produced by appropriately controlling the reaction rate. A second catalyst may be used in the step of forming the addition polymerization polyol. The second catalyst may be one or more selected from the group consisting of phosphazene, potassium hydroxide, sodium hydroxide, cesium hydroxide, imidazole-based catalysts, and dicyanide metal catalysts. Preferably, the second catalyst may be one or more selected from phosphazene, potassium hydroxide, and sodium hydroxide. By using the catalyst, a polyol composition of uniform molecular weight can be produced by appropriately controlling the reaction rate. In order for the addition polymerization polyol composition to contain the seventh polyol and the eighth polyol within the ranges described above, the alkylene oxide can be reacted in the depolymerization polyol composition under appropriate process conditions. For example, in order for the addition polymerization polyol composition to contain the seventh polyol and the eighth polyol in the ranges described above, the depolymerization polyol composition and propylene oxide may be reacted at a temperature of about 90°C to about 150°C for about 5 hours to about 8 hours in a weight ratio of about 20:80 to about 40:60. A depolymerizable polyol composition according to another embodiment may include a ninth polyol and a tenth polyol. A depolymerizable polyol composition according to another embodiment may include the ninth polyol, the tenth polyol, the eleventh polyol, and the twelfth polyol. The ninth polyol may have a number average molecular weight (Mn) greater than about 1,130 g / mol. A depolymerized polyol composition according to another embodiment may contain the ninth polyol in an amount of about 25% to about 50% based on the total area of ​​the composition. Additionally, the 10th polyol may have a number average molecular weight (Mn) of about 660 g / mol to about 1,130 g / mol. In this case, the depolymerization polyol composition according to another embodiment may contain the 10th polyol in an amount of about 5% to about 18% based on the total area of ​​the composition. The depolymerization polyol composition according to another embodiment may include the 10th polyol and the 11th polyol as residual components. The 10th polyol and the 11th polyol may have a number average molecular weight (Mn) of less than 660 g / mol. The number average molecular weight of the ninth polyol may be greater than about 1,130 g / mol, greater than about 2,000 g / mol, greater than about 2,500 g / mol, or greater than about 3,000 g / mol. At the same time, the number average molecular weight of the ninth polyol may be less than about 20,000 g / mol, less than about 15,000 g / mol, less than about 10,000 g / mol, less than about 8,000 g / mol, or less than about 6,000 g / mol. The number average molecular weight of the ninth polyol may be about 1,130 g / mol to about 20,000 g / mol, about 2,000 g / mol to about 20,000 g / mol, about 2,500 g / mol to about 20,000 g / mol, about 3,000 g / mol to about 20,000 g / mol, or about 3,000 g / mol to about 10,000 g / mol. A depolymerizable polyol composition according to another embodiment may include the ninth polyol in an amount greater than about 25%, greater than about 27%, greater than about 29%, greater than about 30%, or greater than about 35% based on the total area of ​​the composition. At the same time, a depolymerizable polyol composition according to another embodiment may include the ninth polyol in an amount less than about 50%, less than about 47%, or less than about 45% based on the total area of ​​the composition. The ninth polyol may include a polyester structure. Additionally, the ninth polyol may include an amine group and a hydroxyl group. In a regenerated polyol according to one embodiment, the ninth polyol may be represented by the following chemical formula 9. [Chemical Formula 9] In the above chemical formula 9, Z may represent a polyester structure formed by the condensation reaction of glycol and a dibasic carboxylic acid. For example, in the above chemical formula 9, Z may include -[OCH₂CH₂OOC(CH₂)₄CO]n- formed by the condensation of ethylene glycol and adipic acid, or -[O(CH₂)₄OOC-C6H₄-CO]n- formed by the condensation of 1,4-butanediol and phthalic anhydride. In the above chemical formula 9, in Z, n may be 1 to 100. In the above chemical formula 9, X may include a unit derived from a polyol having a number average molecular weight of 800 g / mol to 8,500 g / mol. In the above chemical formula 9, X may include a repeating structure of propylene oxide, such as polypropylene glycol (PPG-2000, PPG-4000), for example. In the above chemical formula 9, Y may include a structure derived from methylene diphenyl diisocyanate (MDI) or toluene diisocyanate (TDI). In the above chemical formula 9, Y may be the above chemical formula 1-1 or the above chemical formula 1-2. The above 10th polyol may include 3 to 7 hydroxyl groups. The above 10th polyol may include a polyhydric alcohol including 4 to 7 hydroxyl groups. The number average molecular weight of the 10th polyol may be greater than about 660 g / mol, greater than about 680 g / mol, greater than about 700 g / mol, greater than about 750 g / mol, or greater than about 800 g / mol. At the same time, the number average molecular weight of the 10th polyol may be less than about 1,130 g / mol, less than about 1,000 g / mol, or less than about 900 g / mol. The number average molecular weight of the above 10th polyol may be about 660 g / mol to about 1,130 g / mol, about 680 g / mol to about 1,130 g / mol, about 700 g / mol to about 1,130 g / mol, about 750 g / mol to about 1,000 g / mol, or about 800 g / mol to about 900 g / mol. A depolymerizable polyol composition according to another embodiment may include the second polyol in an amount greater than about 5%, greater than about 7%, or greater than about 10% based on the total area of ​​the composition. At the same time, a depolymerizable polyol composition according to another embodiment may include the second polyol in an amount less than about 18%, less than about 17%, or less than about 16.5% based on the total area of ​​the composition. A depolymerized polyol composition according to another embodiment may contain the second polyol in an amount of about 5% to about 18%, about 7% to about 17%, or about 10% to about 16.5% based on the total area of ​​the composition. In a depolymerization polyol composition according to one embodiment, the 10th polyol may be represented by the following chemical formula 10. [Chemical Formula 10] In the above chemical formula 10, X may include a structure derived from a polyhydric alcohol such as pentaerythritol or trimethylolpropane (TMP). In the above chemical formula 10, X may be derived from a polyol having a number average molecular weight of about 600 g / mol to about 700 g / mol, preferably about 620 g / mol to about 680 g / mol. X may include a repeating structure of propylene oxide (PO). For example, the 10th polyol may include a pentaerythritol-PO polyol in which PO is bonded to a pentaerythritol core. The above eleventh polyol may include an ester group. The above eleventh polyol may be an ester polyol including two hydroxyl groups. The above eleventh polyol may include two hydroxyl groups and one amine group. The above eleventh polyol may include one hydroxyl group and one amine group. The number average molecular weight of the above 11th polyol may be about 280 g / mol to about 660 g / mol. A depolymerized polyol composition according to another embodiment may include the eleventh polyol in an amount of about 10% to about 25% based on the total area of ​​the composition. The number average molecular weight of the 11th polyol may be greater than about 280 g / mol, greater than about 300 g / mol, greater than about 350 g / mol, or greater than about 400 g / mol. At the same time, the number average molecular weight of the 11th polyol may be less than about 660 g / mol, less than about 640 g / mol, or less than about 630 g / mol. A depolymerizable polyol composition according to another embodiment may contain the eleventh polyol in an amount greater than about 10%, greater than about 11%, or greater than about 13% based on the total area of ​​the composition. At the same time, a depolymerizable polyol composition according to another embodiment may contain the eleventh polyol in an amount less than about 25%, less than about 23%, less than about 21%, or less than about 20%. The above eleventh polyol may be represented by the following chemical formula 11-1, the following chemical formula 11-2, or the following chemical formula 11-3. [Chemical Formula 11-1] In the above chemical formula 11-1, Z may comprise a polyester structure formed by the condensation reaction of glycol and a dibasic carboxylic acid. Z may comprise, for example, -[OCH₂CH₂OOC(CH₂)₄CO]n- formed by the condensation of ethylene glycol and adipic acid, or -[O(CH₂)₄OOC-C6H₄-CO]n- formed by the condensation of 1,4-butanediol and phthalic anhydride, and n may be an integer from 1 to 100. In the above chemical formula 11, the glycol may be at least one of the group consisting of ethylene glycol, propylene glycol, 1,4-butanediol, 1,3-propanediol, diethylene glycol, and triethylene glycol. The above dibasic carboxylic acid may be phthalic anhydride or adipic acid. [Chemical Formula 11-2] In the above chemical formula 11-2, Y may include a unit derived from methylene diphenyl diisocyanate (MDI) or toluene diisocyanate (TDI). In the above chemical formula 11-2, Y may include the above chemical formula 1-1 or the above 1-2. In the above chemical formula 11-2, Z1 and Z2 may each independently comprise at least one of units derived from ethylene glycol, propylene glycol, 1,4-butanediol, 1,3-propanediol, diethylene glycol, or triethylene glycol. In the above chemical formula 11-2, Z1 and Z2 may each independently include at least one of - C2H4-, - CH2(CH3)CH2-, - C3H6-, - C4H8-, - C2H4- O - C2H4-, or - C2H4- O - C2H4- O - C2H4-. [Chemical Formula 11-3] In the above chemical formula 11-3, Y may include a unit derived from methylene diphenyl diisocyanate (MDI) or toluene diisocyanate (TDI). In the above chemical formula 11-3, Y may include the above chemical formula 1-1 or the above chemical formula 1-2. In the above chemical formula 11-3, Z may include at least one of units derived from ethylene glycol, propylene glycol, 1,4-butanediol, 1,3-propanediol, diethylene glycol, or triethylene glycol. In the above chemical formula 11-3, Z may include at least one of - C2H4-, - CH2(CH3)CH2-, - C3H6-, - C4H8-, - C2H4- O - C2H4-, or - C2H4- O - C2H4- O - C2H4-. The compounds of the above chemical formulas 11-1 to 11-3 can be used as viscosity modifiers or curability imparters for depolymerized polyol compositions. The above 12th polyol may include glycol. The above 12th polyol may be selected from at least one of the group consisting of ethylene glycol, propylene glycol, 1,4-butanediol, 1,3-propanediol, diethylene glycol, or triethylene glycol. The number average molecular weight of the 12th polyol may be less than about 280 g / mol. The number average molecular weight (Mn) of the 12th polyol may be less than about 280 g / mol, less than about 260 g / mol, less than about 230 g / mol, or less than about 200 g / mol. At the same time, the number average molecular weight of the 12th polyol may be greater than about 10 g / mol, greater than about 20 g / mol, or greater than about 30 g / mol. A depolymerized polyol composition according to another embodiment may contain the 12th polyol in an amount of about 25% to about 50% based on the total area of ​​the composition. In a depolymerization polyol composition according to another embodiment, the 12th polyol may be included in an amount greater than about 25%, greater than about 26%, or greater than about 27% based on the total area of ​​the composition. At the same time, in a depolymerization polyol composition according to another embodiment, the 12th polyol may be included in an amount less than about 50%, less than about 48%, or less than 45% based on the total area of ​​the composition. The number average molecular weight of the above 12th polyol may be about 10 g / mol to about 280 g / mol. The depolymerized polyol composition according to the example may include the 12th polyol in an amount of about 25% to 50%, about 26% to about 48%, or about 27% to about 45% based on the total area of ​​the composition. In a depolymerization polyol composition according to one embodiment, the 12th polyol may be represented by the following chemical formula 12. [Chemical Formula 12] In the above chemical formula 12, Z may include at least one unit derived from ethylene glycol, propylene glycol, 1,4-butanediol, 1,3-propanediol, diethylene glycol, or triethylene glycol. In the above chemical formula 12, Z may include at least one of - C2H4-, - CH2(CH3)CH2-, - C3H6-, - C4H8-, - C2H4- O - C2H4- or - C2H4- O - C2H4- O - C2H4-. Since the depolymerizable polyol composition according to another embodiment contains the 12th polyol in the same amount as above, it has appropriate viscosity and / or appropriate reactivity and can provide hydroxyl groups during the polymerization process. That is, in the depolymerizable polyol composition according to another embodiment, the 12th polyol can be used as a molecular weight regulator, a viscosity regulator, or a terminal hydroxyl group provider. A method for preparing a depolymerized polyol composition according to another embodiment comprises the steps of: introducing a polyhydric alcohol and a solvent into a reactor and heating the temperature of the reactor to 170°C to 250°C; crushing waste polyurethane to prepare a crushed material, introducing the crushed material and a catalyst into the reactor to prepare a depolymerizing agent mixture; and cooling the reactor to 90°C to 190°C. The method comprises the step of obtaining a regenerated polyol by filtering the above depolymerization mixture through a filter with a diameter of 200 μm to 300 μm; wherein the regenerated polyol comprises a ninth polyol having a number average molecular weight (Mn) greater than 1,130 g / mol in an amount of 25% to 50% based on the total area of ​​the composition, and a tenth polyol having a number average molecular weight (Mn) of 660 g / mol to 1,130 g / mol in an amount of 5% to 18% based on the total area of ​​the composition, and the remaining component comprises a polyol having a number average molecular weight (Mn) less than 660 g / mol. (1) Step of heating after introducing polyalcohol and solvent into the reactor According to another embodiment, a polyalcohol and a solvent can be introduced into the reactor simultaneously. The above solvent may have a weight-average molecular weight (Mw) of 1,000 g / mol to 4,000 g / mol, 1,200 g / mol to 3,800 g / mol, or 1,500 g / mol to 3,500 g / mol. The above solvent may have a hydroxyl group value of 30 mgKOH / g to 150 mgKOH / g, 40 mgKOH / g to 130 mgKOH / g, or 50 mgKOH / g to 110 mgKOH / g. The above solvent may be used in a ratio of about 30% to 150% by weight, about 40% to 140% by weight, or about 50% to 120% by weight, based on the weight of the ground material. The above polyhydric alcohol may have a weight-average molecular weight (Mw) of 100 g / mol to 400 g / mol, 130 g / mol to 350 g / mol, or 150 g / mol to 270 g / mol. The above polyhydric alcohol may have a hydroxyl group value of 300 mgKOH / g to 700 mgKOH / g, 350 mgKOH / g to 650 mgKOH / g, or 400 mgKOH / g to 600 mgKOH / g. The above polyhydric alcohol may be used in a ratio of about 100% to 500% by weight, about 120% to 450% by weight, or about 140% to 400% by weight, based on the weight of the ground material. The polyalcohol may be one or more selected from the group consisting of ethylene glycol, tripropylene glycol, diethylene glycol, thiodiethylene glycol, neopentyl glycol, triethylene glycol, tetraethylene glycol, dipropylene glycol, tripropylene glycol, and pentaerythritol. Preferably, the polyalcohol may be one or more selected from ethylene glycol, tripropylene glycol, and diethylene glycol. Preferably, the polyalcohol may be tripropylene glycol. (2) Step of preparing a crushed material containing waste polyurethane The above step involves collecting the waste polyurethane and physically crushing it. The waste polyurethane may exist in various forms, such as foam or coatings. By forming the waste polyurethane into small particles or powder, the reaction surface area can be increased during the depolymerization process, thereby enhancing the reaction rate and efficiency. The above-mentioned crushed material can be produced by crushing hard waste polyurethane foam or soft waste polyurethane foam. When polyols are manufactured using such waste polyurethane, there are effects of cost reduction and environmental protection. (3) Step of preparing a depolymerization mixture The above step involves mixing crushed waste polyurethane with a polyhydric alcohol, a solvent, and a catalyst, wherein the cross-linking of the polyurethane is decomposed to form a regenerated polyol through a depolymerization reaction. The pulverized material containing the above polyurethane may have a number average molecular weight of 1,000 g / mol to 5,000 g / mol. For example, the pulverized material may have a number average molecular weight of 1,500 g / mol to 4,500 g / mol, or 2,000 g / mol to 4,000 g / mol. The step of preparing the above depolymerization agent mixture may involve performing a depolymerization reaction at 170°C to 250°C for 1 to 10 hours. Specifically, after mixing the ground material, polyhydric alcohol, and solvent, a regenerated polyol may be obtained by performing a depolymerization reaction at 180°C to 240°C, 190°C to 230°C, or 200°C to 220°C for 2 to 9 hours, 3 to 8 hours, or 4 to 7 hours. If the depolymerization temperature and time satisfy the above ranges, a regenerated polyol with a uniform molecular weight can be produced by appropriately controlling the reaction rate. The catalyst may include one or more selected from the group consisting of potassium hydroxide, sodium hydroxide, potassium acetate, zinc acetate, a mixture of sodium acetate and strontium acetate, and a mixture of potassium acetate and strontium acetate. Preferably, the catalyst may be one or more selected from potassium hydroxide and sodium hydroxide. By using the catalyst, a regenerated polyol of uniform molecular weight can be produced by appropriately controlling the reaction rate. The catalyst may be added in an amount of 0.0001% to 5% by weight based on the total weight of the ground material. For example, the catalyst may be added in an amount of 0.0002% to 3% by weight or 0.0003% to 2% by weight based on the total weight of the ground material. The above-mentioned regenerated polyol contains a first polyol having a number average molecular weight (Mn) greater than 1,130 g / mol in an amount of 25% to 50% based on the total area of ​​the composition, and a second polyol having a number average molecular weight (Mn) of 660 g / mol to 1,130 g / mol in an amount of 5% to 18% based on the total area of ​​the composition. The polyalcohol and solvent may be mixed in a weight ratio of 1:1 to 10:1. For example, the polyalcohol and solvent may be mixed in a weight ratio of 1:1 to 9:1, 2:1 to 8:1, or 3:1 to 7:1. When mixed in the above weight ratios, the reactivity between the waste polyurethane and the polyalcohol is increased under the solvent, which may result in a high yield of the finally produced recycled polyol. Subsequently, the method may include the step of cooling the reactor to 90°C to 190°C; and the step of filtering the depolymerization mixture through a filter with a diameter of 200 µm to 300 µm to obtain a regenerated polyol. In order for the depolymerization polyol composition according to another embodiment to include the ninth polyol, the tenth polyol, the eleventh polyol, and the twelveth polyol in appropriate amounts, the process conditions for producing the regenerated polyol can be appropriately controlled. In order for the depolymerization polyol composition according to the example to include the ninth polyol, the tenth polyol, the eleventh polyol, and the twelfth polyol in the above amounts, the type of waste polyurethane foam, the weight ratio of the polyhydric alcohol, the content of the catalyst, the depolymerization reaction time, and the depolymerization process temperature can be appropriately controlled. In order for the depolymerization polyol composition according to the example to include the ninth polyol, the tenth polyol, the eleventh polyol, and the twelfth polyol in the above amounts, the weight ratio of the waste polyurethane foam crushed material and the polyhydric alcohol may be about 1:1 to about 1:3, about 1:1.5 to 1:3, about 1:2 to about 1:3, or about 1:2 to about 1:4. In addition, for the depolymerization polyol composition according to the example to include the ninth polyol, the tenth polyol, the eleventh polyol, and the twelfth polyol in the above amounts, the catalyst may be included in the reactants in an amount of about 0.1 to about 0.5 parts by weight, about 0.2 to about 0.4 parts by weight, or about 0.15 to about 0.45 parts by weight, based on 100 parts by weight of the total reactants. In addition, for the depolymerization polyol composition according to the example to include the ninth polyol, the tenth polyol, the eleventh polyol, and the twelfth polyol in the amounts as described above, the reactants may be depolymerized at a temperature of about 180°C to about 240°C, about 190°C to about 230°C, or about 200°C to about 220°C for about 5 hours to about 8 hours, about 5 hours to about 7 hours, or about 4 hours or about 7 hours. A depolymerized polyol composition according to another embodiment may include a 13th polyol having a number average molecular weight (Mn) of about 700 g / mol to about 2,500 g / mol in an amount of about 7% to about 20% based on the total area of ​​the composition, and a 14th polyol having a number average molecular weight (Mn) of less than about 100 g / mol in an amount of less than about 5% based on the total area of ​​the composition. A depolymerized polyol composition according to another embodiment may include the 13th polyol, the 14th polyol, the 15th polyol, the 16th polyol, and the 17th polyol. The above 13th polyol may include 1 to 3 amine groups and 1 to 3 hydroxyl groups. The number average molecular weight of the 13th polyol may be greater than about 700 g / mol, greater than about 900 g / mol, greater than about 1,000 g / mol, or greater than about 1,200 g / mol. At the same time, the number average molecular weight of the 13th polyol may be less than about 2,500 g / mol, less than about 2,300 g / mol, less than about 2,100 g / mol, or less than about 2,000 g / mol. The first polyol may be included in an amount of 7% to 20%, 8% to 18%, 9% to 16%, or 10% to 15% based on the total area of ​​the composition. In a depolymerization polyol composition according to one embodiment, the 13th polyol may be represented by the following chemical formula 13. [Chemical Formula 13] HO-R 1 -OC(=O)-NH-R 2 -NH-C(=O)-OR 3 -OH In the above chemical formula 13, The above R 1 It includes a linear or branched structure having a repeating unit comprising at least one of an ether group or an ester group, and an alkylene group having 2 to 30 carbon atoms. The above R 2 It contains residues derived from aromatic or aliphatic isocyanate groups. The above R 3 is of carbon atoms with 2 to 4 carbon atoms It includes glycol derivatives containing alkylene groups. For example, the above R 1 Examples include polyethylene glycol units [-CH₂CH₂O-]n, polypropylene glycol units [-CH₂CH(CH₃)O-]n, polytetramethylene glycol units [-(CH₂)₄O-]n, polycaprolactone units [-(CH₂)5COO-]n, etc., and n can be an integer from 1 to 50. In the above chemical formula 13, the R 2 can mean a residue derived from an aromatic or aliphatic isocyanate group. The above R 2 It may be a residue derived from an aromatic isocyanate group. Examples include toluene diisocyanate (TDI) derivatives, methylene diphenyl diisocyanate (MDI) derivatives, hexamethylene diisocyanate (HDI) derivatives, etc. In the above chemical formula 13, the R 3 is of carbon atoms with 2 to 4 carbon atoms It refers to glycol derivatives containing an alkylene group. Examples include ethylene glycol, propylene glycol, and 1,3-butylene glycol. In the above chemical formula 13, the R 1 The number average molecular weight may be 400 g / mol to 2,000 g / mol, 500 g / mol to 1,800 g / mol, or 600 g / mol to 1,600 g / mol. In the above chemical formula 13, the R 2 The number average molecular weight may be 200 g / mol to 300 g / mol, 205 g / mol to 280 g / mol, or 210 g / mol to 270 g / mol. In the above chemical formula 13, the R 3 The number average molecular weight may be 50 g / mol to 120 g / mol, 55 g / mol to 110 g / mol, or 60 g / mol to 100 g / mol. The number average molecular weight of the 14th polyol may be less than about 100 g / mol, less than about 95 g / mol, or less than about 90 g / mol. At the same time, the number average molecular weight of the 14th polyol may be greater than about 10 g / mol. A depolymerizable polyol composition according to another embodiment may include the 14th polyol in an amount of less than about 5%, less than about 4%, less than about 3%, less than about 2.5%, less than about 2%, or less than about 1% based on the total area of ​​the composition. At the same time, a depolymerizable polyol composition according to another embodiment may include the 14th polyol in an amount greater than about 0.1 wt based on the total weight. A depolymerization polyol composition according to another embodiment can be prepared by depolymerizing soft waste polyurethane foam. Since the number average molecular weight of the 14th polyol in the prepared depolymerization polyol composition is less than 100 g / mol, the polyurethane foam prepared by the depolymerization polyol composition according to another embodiment can have improved flexibility. In a depolymerization polyol composition according to another embodiment, the 14th polyol may be represented by the following chemical formula 14. [Chemical Formula 14] HO-(CH2) n -OH In the above chemical formula 14, n may be an integer from 2 to 4, which represents an alkylene glycol compound having 2 to 4 carbon atoms. For example, the above 14th polyol may be selected from at least one of the group consisting of ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,3-butylene glycol and 1,4-butylene glycol, etc. The number average molecular weight of the 15th polyol may be greater than about 2,500 g / mol, greater than 2,600 g / mol, or greater than 2,700 g / mol. At the same time, the number average molecular weight of the 15th polyol may be less than about 5,000 g / mol. In addition, a depolymerized polyol composition according to another embodiment may include the 15th polyol in an amount of about 10% to about 40 wt, about 15% to about 35%, about 17% to about 33%, or about 20% to about 30% based on the total area of ​​the composition. In a depolymerization polyol composition according to another embodiment, a polyol having a number average molecular weight (Mn) greater than about 5,000 g / mol may be included in an amount of less than about 5% based on the total area of ​​the composition. Since polyol compounds having such high molecular weight are hardly detected, it can be confirmed that reaction conditions are optimized and uniform decomposition of the polyurethane polymer can be achieved. In other words, the efficiency of the depolymerization reaction and the quality stability of the recycled raw material can be confirmed. In a depolymerization polyol composition according to one embodiment, the 15th polyol may be represented by the following chemical formula 15. [Chemical Formula 15] HO-[R 4 -O] m -H In the above chemical formula 15, R 4 The structure comprises a linear or branched structure having a repeating unit comprising at least one of an ether group or an ester group, and the alkylene group having 2 to 100 carbon atoms, wherein m may be an integer from 1 to 100. Examples include polyethylene glycol units (-CH₂CH₂-), polypropylene glycol units (-CH₂CH(CH₃)-), polytetramethylene glycol units (-(CH₂)₄-), polycaprolactone units (-(CH₂)5COO-), etc. In the above chemical formula 15, the R 4 The number average molecular weight may be 400 g / mol to 2,000 g / mol, 500 g / mol to 1,800 g / mol, or 600 g / mol to 1,600 g / mol. In the above chemical formula 15, m may be 20 to 100, 25 to 95, or 30 to 90. The above 16th polyol may include a triol. The number average molecular weight of the above 16th polyol is about 100 g / mol to about 250 g / mol, and a depolymerized polyol composition according to another embodiment may include the above 16th polyol in an amount of about 30% to about 50% based on the total area of ​​the composition. The number average molecular weight of the 16th polyol may be greater than about 120 g / mol, greater than about 130 g / mol, greater than about 150 g / mol, or greater than about 170 g / mol. At the same time, the number average molecular weight of the 16th polyol may be less than about 230 g / mol, less than about 220 g / mol, or less than about 200 g / mol. A depolymerizable polyol composition according to another embodiment may include the 16th polyol in an amount greater than about 32%, greater than about 35%, greater than about 37%, or greater than about 40% based on the total area of ​​the composition. A depolymerizable polyol composition according to another embodiment may include the 16th polyol in an amount less than about 49%, less than about 48%, or less than about 46% based on the total area of ​​the composition. The above 16th polyol can be represented by the following chemical formula 16. [Chemical Formula 16] R 5 -(OH)3 In the above chemical formula 16, R 5 It may be an alkyl group or an alkylene group having 2 to 10 carbon atoms. Examples include an ethylene group, a propylene group, a butylene group, a pentylene group, a hexylene group, an octylene group, a decylene group, etc. In the above chemical formula 16, the R 5 The number average molecular weight may be 50 g / mol to 100 g / mol, 60 g / mol to 90 g / mol, or 65 g / mol to 85 g / mol. The compound of Chemical Formula 16 above is a low molecular weight polyol having a triol structure, for example, it may include glycerol, and can be used as a crosslinker in the polyurethane depolymerization process. The above 17th polyol has a number average molecular weight (Mn) of about 250 g / mol to about 700 g / mol, and the above 17th polyol may be included in a depolymerization polyol composition according to another embodiment in an amount of about 10% to about 30% based on the total area of ​​the composition. The above 17th polyol may have a number average molecular weight greater than about 300 g / mol, greater than about 350 g / mol, or greater than about 400 g / mol. At the same time, the above 17th polyol may have a number average molecular weight (Mn) less than about 650 g / mol, less than about 630 g / mol, or less than about 600 g / mol. A depolymerizable polyol composition according to another embodiment may contain the 17th polyol in an amount greater than about 12%, greater than about 14%, or greater than about 16% based on the total area of ​​the composition. At the same time, a depolymerizable polyol composition according to another embodiment may contain the 17th polyol in an amount less than or equal to about 28%, less than or equal to 26%, or less than or equal to 24%. In a depolymerization polyol composition according to another embodiment, the 17th polyol may be represented by the following chemical formula 17-1. [Chemical Formula 17-1] HO-R 6 -OC(=O)-NH-R 7 -NH-C(=O)-OR 8 -OH In the above chemical formula 17-1, the R 6 and R 8Each may independently include units derived from ethylene glycol, propylene glycol, and butylene glycol, for example, ethylene glycol units, propylene glycol units, butylene glycol units, etc. The above R 7 It refers to a residue derived from an aromatic or aliphatic isocyanate group, and may include, for example, toluene diisocyanate (TDI) derivatives, methylene diphenyl diisocyanate (MDI) derivatives, hexamethylene diisocyanate (HDI) derivatives, etc. In the above chemical formula 17-1, the R 6 and R 8 Each may independently have a number average molecular weight of 50 g / mol to 120 g / mol, 55 g / mol to 110 g / mol, or 60 g / mol to 100 g / mol. In the above chemical formula 17-1, the R 7 The number average molecular weight may be 200 g / mol to 300 g / mol, 205 g / mol to 280 g / mol, or 210 g / mol to 270 g / mol. The compound of the above chemical formula 17-1 can be synthesized as a structural unit of a polyurethane prepolymer or a depolymerized polyol. In a depolymerization polyol composition according to another embodiment, the 17th polyol may be represented by the following chemical formula 17-2. [Chemical Formula 17-2] H2N-R 9 -NH-C(=O)-OR 10 -OH In the above chemical formula 17-2, R 9 means a residue derived from an aromatic or aliphatic isocyanate group, and may include, for example, methylene diphenyl diisocyanate (MDI) derivatives, toluene diisocyanate (TDI) derivatives, hexamethylene diisocyanate (HDI) derivatives, etc. R 10It may include units derived from ethylene glycol, propylene glycol, and butylene glycol, for example, ethylene glycol units, propylene glycol units, butylene glycol units, etc. In the above chemical formula 17-2, the R 9 The number average molecular weight may be 200 g / mol to 300 g / mol, 205 g / mol to 280 g / mol, or 210 g / mol to 270 g / mol. In the above chemical formula 17-2, the R 10 The number average molecular weight may be 50 g / mol to 120 g / mol, 55 g / mol to 110 g / mol, or 60 g / mol to 100 g / mol. The compound of the above chemical formula 17-2 can be prepared by the reaction of an isocyanate compound with a glycol and can exist as a structural unit of a polyurethane depolymerization product. A depolymerized polyol composition according to another embodiment may include a copolymer oligomer of styrene and acrylonitrile. The copolymer oligomer may have a number average molecular weight (Mn) of less than 250 g / mol, 200 g / mol or less, 100 g / mol or less, or less than 100 g / mol. An addition polymerization polyol composition according to another embodiment may be formed by adding an alkylene oxide to a depolymerization polyol composition according to another embodiment. According to another embodiment, the addition polymerization polyol composition may be formed by adding polymerizing the alkylene oxide to at least one of the 13th polyol, the 14th polyol, the 15th polyol, the 16th polyol, and the 17th polyol. An addition polymerization polyol composition according to another embodiment comprises a polyol of the 18th with an alkylene oxide added having a number average molecular weight (Mn) of less than about 260 g / mol in an amount of about 0.01% to about 10% based on the total area of ​​the composition, and a polyol of the 19th with an alkylene oxide added having a number average molecular weight (Mn) of more than about 3,000 g / mol in an amount of 1% to 20% based on the total area of ​​the composition. The above 18th polyol may have a number average molecular weight (Mn) of less than about 230 g / mol, less than about 200 g / mol, or less than about 180 g / mol. An addition polymerization polyol composition according to another embodiment may include the 18th polyol in an amount greater than 0.1%, greater than 0.5%, or greater than 1% based on the total area of ​​the composition. At the same time, an addition polymerization polyol composition according to another embodiment may include the 18th polyol in an amount less than about 8%, less than about 7%, or less than about 6% based on the total area of ​​the composition. In an addition polymerization polyol composition according to another embodiment, the 18th polyol may be represented by the following chemical formula 18. [Chemical Formula 18] HO-(CH2) p -OH In the above chemical formula 18, p may be an integer from 2 to 4, representing an alkylene glycol compound having 2 to 4 carbon atoms. For example, ethylene glycol when p=2, 1,2-propylene glycol or 1,3-propylene glycol when p=3, and 1,3-butylene glycol or 1,4-butylene glycol when p=4 may be used. The compound of Chemical Formula 18 above is a low molecular weight glycol and can be used as a molecular weight regulator or viscosity regulator in the polyurethane depolymerization process. The above 19th polyol may have a number average molecular weight greater than 3,500 g / mol, greater than 4,000 g / mol, or greater than 5,000 g / mol. At the same time, the above 19th polyol may have a number average molecular weight (Mn) less than about 10,000 g / mol, less than about 9,000 g / mol, or less than about 8,000 g / mol. An addition polymerization polyol composition according to another embodiment may include the 19th polyol in an amount greater than about 5%, greater than about 7%, or greater than about 9% based on the total area of ​​the composition. At the same time, an addition polymerization polyol composition according to another embodiment may include the 19th polyol in an amount less than about 18%, less than about 16%, or less than about 15% based on the total area of ​​the composition. In an addition polymerization polyol composition according to another embodiment, the 19th polyol may be represented by the following chemical formula 19. [Chemical Formula 19] HO-[PO] q -OR 11 -O-[PO] r -OH In the above chemical formula 19, "PO" may be a repeating unit of propylene oxide. In the above chemical formula 19, the R 11 It may include at least one of ethylene glycol, propylene glycol, and butylene glycol. In the above chemical formula 19, the R 11 The number average molecular weight may be 50 g / mol to 120 g / mol, 55 g / mol to 110 g / mol, or 60 g / mol to 100 g / mol. In the above chemical formula 19, q and r can each independently be integers from 30 to 60. An addition polymerization polyol composition according to another embodiment may include a 20th polyol. The number average molecular weight of the 20th polyol may be about 260 g / mol to about 3,000 g / mol. An addition polymerization polyol composition according to another embodiment may include the 20th polyol in an amount of about 70% to about 90% based on the total area of ​​the composition. The above 20th polyol may have a number average molecular weight greater than about 300 g / mol, greater than about 350 g / mol, or greater than about 400 g / mol. At the same time, the above 20th polyol may have a number average molecular weight (Mn) of 2,000 g / mol or less, 1,500 g / mol or less, 1,000 g / mol or less, or 800 g / mol or less. In another embodiment, another addition polymerization polyol composition may contain the 20th polyol in an amount greater than about 72%, greater than about 75%, or greater than about 80% based on the total area of ​​the composition. At the same time, the addition polymerization polyol composition according to another embodiment may contain the 20th polyol in an amount less than about 88%, less than about 86%, or less than about 85% based on the total area of ​​the composition. In an alkylene oxide addition depolymerization polyol composition according to one embodiment, the 20th polyol may be represented by the following chemical formula 20-1. [Chemical Formula 20-1] HO-[PO] s -NH-C(=O)-NH-[PO] t -OC(=O)-OR 12 -OH In the above chemical formula 20-1, "PO" represents a repeating unit of propylene oxide having a -CH₂CH(CH₃)O- structure, and s and t can each independently be integers from 1 to 30. R 12It may include units derived from ethylene glycol, propylene glycol, and butylene glycol, for example, ethylene glycol units, propylene glycol units, butylene glycol units, etc. In the above chemical formula 20-1, the R 12 The number average molecular weight may be 50 g / mol to 120 g / mol, 55 g / mol to 110 g / mol, or 60 g / mol to 100 g / mol. The compound of the above chemical formula 20-1 can be prepared by the reaction of polypropylene oxide diamine with an isocyanate compound and a glycol, and can exist as a structural unit of a polyurethane depolymerization product. In an addition polymerization polyol composition according to another embodiment, the 20th polyol may be represented by the following chemical formula 20-2. [Chemical Formula 20-2] HO-[PO] u -NH-C(=O)-OR 13 -NH-C(=O)-OR 14 -OH In the above chemical formula 20-2, "PO" means a repeating unit of propylene oxide having a -CH₂CH(CH₃)O- structure, and u can be an integer from 1 to 50. R 13 and R 14 Each may independently include units derived from ethylene glycol, propylene glycol, and butylene glycol, for example, ethylene glycol units, propylene glycol units, butylene glycol units, etc. Also, R 13 and R 14 The number average molecular weight (Mn) of each can independently be 50 g / mol to 120 g / mol, preferably 55 g / mol to 110 g / mol, more preferably 60 g / mol to 100 g / mol. The compound of the above chemical formula 20-2 can be prepared through the reaction of polypropylene oxide diol / diamine with isocyanate compounds and glycols, and can exist as a structural unit of the polyurethane depolymerization product. In an addition polymerization polyol composition according to another embodiment, the 20th polyol may be represented by the following chemical formula 20-3. [Chemical Formula 20-3] HO-R 15 -OC(=O)-NH-R 16 -NH-C(=O)-OR 17 -OH In the above chemical formula 20-3, R 15 It may include a linear or branched structure having a repeating unit comprising at least one of an alkylene group having 2 to 30 carbon atoms and an ether group or an ester group, and as a trifunctional polyol, each branch chain may include -CH₂CH(CH₃)O-(PO repeating unit) and -CH₂CH₂O-(EO repeating unit). The above R 15 The number average molecular weight (Mn) of may be 100 g / mol to 2,000 g / mol, preferably 200 g / mol to 1,800 g / mol, and more preferably 300 g / mol to 1,600 g / mol. The above R 16 means a residue derived from an aromatic or aliphatic isocyanate group, and may include, for example, MDI derivatives, TDI derivatives, etc., and R 16 The number average molecular weight (Mn) of may be 200 g / mol to 300 g / mol, preferably 205 g / mol to 280 g / mol, more preferably 210 g / mol to 270 g / mol. The above R 17It may include units derived from ethylene glycol, propylene glycol, and butylene glycol, for example, including -CH₂CH₂-, -CH₂CH(CH₃)-, -(CH₂)₄- structures, and R 17 The number average molecular weight (Mn) of may be 50 g / mol to 120 g / mol, preferably 55 g / mol to 110 g / mol, more preferably 60 g / mol to 100 g / mol. The compound of the above chemical formula 20-3 can be prepared by polymerizing PO / EO in a trifunctional polyol, reacting it with a diisocyanate to form a urethane bond, and then terminating it with a glycol. In an addition polymerization polyol composition according to another embodiment, the 20th polyol may be represented by the following chemical formula 20-4. [Chemical Formula 20-4] R 18 -[(PO) v -OH] w In the above chemical formula 20-4, "PO" represents a repeating unit of propylene oxide having a -CH₂CH(CH₃)O- structure, v is an integer from 1 to 30, and w may be an integer from 1 to 30. The above R 18 It may include a linear or branched structure having a repeating unit comprising at least one of an ether group or an ester group, and may include, for example, structures such as -(CH₂CH₂O)n-(PEG), -(CH₂CH(CH₃)O)n-(PPG), -(CH₂)₄O-(PTMG), -(CH₂)5COO-(PCL), where n may be an integer from 1 to 50. The compound of the above chemical formula 20-4 has a structure in which branched terminal hydroxyl groups are introduced by polymerizing PO into a multifunctional polyol, and can be used as a viscosity modifier, dispersion stabilizer, etc. in polyurethane depolymerization compositions. A method for preparing a depolymerized polyol composition according to another embodiment comprises the steps of: preparing a crushed material containing waste polyurethane; and mixing the crushed material with a polyhydric alcohol and heat-treating it to form a regenerated polyol, wherein the regenerated polyol comprises a 13th polyol having a number average molecular weight (Mn) of 700 g / mol to 2,500 g / mol in an amount of 7% to 20% based on the total area of ​​the composition, and the regenerated polyol comprises a 14th polyol having a number average molecular weight (Mn) of less than 100 g / mol in an amount of less than 5% based on the total area of ​​the composition, and the remaining components comprise a polyol having a number average molecular weight (Mn) of 100 g / mol or more and less than 700 g / mol and a polyol having a number average molecular weight (Mn) of more than 2,500 g / mol. In a method for preparing a depolymerization polyol composition according to another embodiment, when the content ratio of crushed waste polyurethane foam and polyhydric alcohol, the depolymerization temperature and time, and / or the catalyst content are within a specific range, depolymerization efficiency and the quality of the regenerated polyol can be simultaneously secured. (1) Step of preparing a crushed material containing waste polyurethane The above step involves collecting the waste polyurethane and physically crushing it. The waste polyurethane may exist in various forms, such as foam or coatings. By forming the waste polyurethane into small particles or powder, the reaction surface area can be increased during the depolymerization process, thereby enhancing the reaction rate and efficiency. The above-mentioned crushed material can be produced by crushing hard waste polyurethane foam or soft waste polyurethane foam. When polyols are manufactured using such waste polyurethane, there are effects of cost reduction and environmental protection. For example, the above-mentioned crushed material can be manufactured by crushing polyurethane used in furniture and mattresses, polyurethane from waste car seats, or polyurethane used in electronic and electrical products. (2) A step of mixing the above-mentioned pulverized material and polyhydric alcohol and heat-treating to form a regenerated polyol. The above step is a step in which pulverized waste polyurethane is mixed with polyhydric alcohol and heated, thereby breaking down the cross-links of the polyurethane and forming a regenerated polyol through a depolymerization reaction. The regenerated polyol formed by the decomposition of the above-mentioned polyurethane powder may have a number average molecular weight of 1,000 g / mol to 5,000 g / mol. For example, the above-mentioned powder may have a number average molecular weight of 1,500 g / mol to 4,500 g / mol, or 2,000 g / mol to 4,000 g / mol. The above polyhydric alcohol may be used in a ratio of about 60% to 400% by weight, about 80% to 350% by weight, or about 100% to 300% by weight, based on the weight of the ground material. The polyalcohol may be one or more selected from the group consisting of ethylene glycol, tripropylene glycol, diethylene glycol, thiodiethylene glycol, neopentyl glycol, triethylene glycol, tetraethylene glycol, dipropylene glycol, tripropylene glycol, and pentaerythritol. Preferably, the polyalcohol may be one or more selected from ethylene glycol, tripropylene glycol, and diethylene glycol. Preferably, the polyalcohol may be tripropylene glycol. The step of forming the regenerated polyol above may involve performing a depolymerization reaction at 100°C to 400°C for 1 to 10 hours. Specifically, after mixing the ground material and the polyhydric alcohol, the regenerated polyol may be obtained by performing a depolymerization reaction at 100°C to 400°C, 120°C to 380°C, 130°C to 380°C, 150°C to 370°C, or 180°C to 370°C for 2 to 9 hours, 3 to 8 hours, or 4 to 7 hours. If the depolymerization temperature and time satisfy the above ranges, the reaction rate can be appropriately controlled to produce a regenerated polyol with a uniform molecular weight. A first catalyst may be used in the step of forming the regenerated polyol. The first catalyst may include one or more selected from the group consisting of potassium hydroxide, sodium hydroxide, potassium acetate, zinc acetate, a mixture of sodium acetate and strontium acetate, and a mixture of potassium acetate and strontium acetate. Preferably, the first catalyst may be one or more selected from potassium hydroxide and sodium hydroxide. By using the catalyst, a polyol composition of uniform molecular weight can be produced by appropriately controlling the reaction rate. The first catalyst may be added in an amount of 0.0001% to 5% by weight based on the total weight of the ground material. For example, the first catalyst may be added in an amount of 0.0002% to 3% by weight or 0.0003% to 2% by weight based on the total weight of the ground material. If the content of the first catalyst is excessively increased, the reaction rate increases, but problems such as increased viscosity, color change, and excessive heat generation may occur. The above-mentioned regenerated polyol contains a 13th polyol having a number average molecular weight (Mn) of 700 g / mol to 2,500 g / mol in an amount of 7% to 20% based on the total area of ​​the composition, and the above-mentioned regenerated polyol contains a 14th polyol having a number average molecular weight (Mn) of less than 100 g / mol in an amount of less than 5% based on the total area of ​​the composition. The above-mentioned pulverized material and the above-mentioned polyhydric alcohol may be mixed in a weight ratio of 1:1 to 10:1. For example, the above-mentioned pulverized material and the above-mentioned polyhydric alcohol may be mixed in a weight ratio of 1:1 to 8:1 or 1:1 to 3:2. When mixed within the above weight ratio range, the depolymerization reactivity is excellent, and the viscosity and OH value of the polyol after depolymerization appear uniformly, resulting in good quality of the recycled polyol. If the weight ratio falls outside the above range, problems may occur such as incomplete depolymerization due to a relative lack of polyhydric alcohol content, or increased viscosity leading to reduced processability or moldability. (3) A step of reacting the above regenerated polyol with alkylene oxide to form an addition polymerized polyol. The above step is a step of increasing the molecular weight of a polyol composition by reacting an alkylene oxide with a regenerated polyol obtained through depolymerization to perform an addition polymerization reaction. Specifically, the above step can perform an addition polymerization reaction with the alkylene oxide through a reactive hydroxyl group located at the end of the main chain of the regenerated polyol. The above addition polymerization polyol has a number average molecular weight (Mn) of less than 260 g / mol and includes the 18th polyol with added alkylene oxide in an amount of 0.01% to 10% based on the total area of ​​the composition, and the above addition polymerization polyol has a number average molecular weight (Mn) of more than 3,000 g / mol and includes the 19th polyol with added alkylene oxide in an amount of 1% to 20% based on the total area of ​​the composition. The above alkylene oxide may be one or more selected from the group consisting of ethylene oxide, propylene oxide, butylene oxide, pentene oxide, hexene oxide, cyclopentene oxide, and cyclohexane oxide. Preferably, the above alkylene oxide may be one or more selected from ethylene oxide and propylene oxide. In one embodiment, the alkylene oxide may be used in combination with ethylene oxide (EO) and propylene oxide (PO). The content of the ethylene oxide and propylene oxide can be adjusted to a ratio of 1:1 to 10:1. Increasing the ratio of the ethylene oxide may result in a more uniform increase in molecular weight. The above-mentioned recycled polyol may contain 2 to 10 hydroxyl groups per molecule. For example, the above-mentioned recycled polyol may contain 2 to 8, 3 to 8, or 4 to 7 hydroxyl groups per molecule. When the number of hydroxyl groups per molecule of the above-mentioned recycled polyol satisfies the above range, reactivity with alkylene oxide is increased, thereby forming a polyol composition having a high molecular weight. When a polyurethane foam is formed using such a polyol composition, it can have excellent mechanical properties. The step of forming the addition polymerization polyol above may involve performing a depolymerization reaction at 100°C to 400°C for 1 to 10 hours. Specifically, after mixing alkylene oxide with the regenerated polyol, an additional polymerization reaction may be performed at 100°C to 400°C, 120°C to 380°C, 130°C to 380°C, 150°C to 370°C, or 180°C to 370°C for 2 to 9 hours, 3 to 8 hours, or 4 to 7 hours to obtain a polyol composition. If the addition polymerization temperature and time satisfy the above ranges, a polyol composition of uniform molecular weight can be produced by appropriately controlling the reaction rate. A second catalyst may be used in the step of forming the addition polymerization polyol. The second catalyst may be one or more selected from the group consisting of phosphazene, potassium hydroxide, sodium hydroxide, cesium hydroxide, imidazole-based catalysts, and dicyanide metal catalysts. Preferably, the second catalyst may be one or more selected from phosphazene, potassium hydroxide, and sodium hydroxide. By using the catalyst, a polyol composition of uniform molecular weight can be produced by appropriately controlling the reaction rate. In order for the depolymerization polyol composition according to another embodiment to include the 13th polyol, the 14th polyol, the 15th polyol, the 16th polyol, and the 17th polyol in appropriate amounts, the process conditions for producing the regenerated polyol can be appropriately controlled. In order for the depolymerization polyol composition according to the example to include the 13th polyol, the 14th polyol, the 15th polyol, the 16th polyol, and the 17th polyol in the above amounts, the type of waste polyurethane foam (e.g., foam for automobile seats), the type of polyhydric alcohol (tripropylene glycol), the weight ratio of the waste polyurethane foam crushed material and the polyhydric alcohol, the content of the catalyst, the depolymerization reaction time, and the depolymerization process temperature can be appropriately controlled. In order for the depolymerization polyol composition according to the example to include the 13th polyol, the 14th polyol, the 15th polyol, the 16th polyol, and the 17th polyol in the above amounts, the weight ratio of the waste polyurethane foam crushed material and the polyhydric alcohol may be about 1:0.8 to about 1:1.2, about 1:0.7 to 1:1.3, about 1:0.8 to about 1:2, or about 10.7 to about 1:1.1. In addition, in order for the depolymerization polyol composition according to the example to include the 13th polyol, the 14th polyol, the 15th polyol, the 16th polyol, and the 17th polyol in the above amounts, the catalyst may be included in the reactants in an amount of about 0.1 to about 0.5 parts by weight, about 0.2 to about 0.4 parts by weight, or about 0.15 to about 0.45 parts by weight, based on 100 parts by weight of the total reactants. In addition, in order for the depolymerization polyol composition according to the example to include the 13th polyol, the 14th polyol, the 15th polyol, the 16th polyol, and the 17th polyol in the amounts as described above, the reactants may be depolymerized at a temperature of about 180°C to about 240°C, about 190°C to about 230°C, or about 200°C to about 220°C for about 5 hours to about 8 hours, about 5 hours to about 7 hours, or about 4 hours or about 7 hours. According to another embodiment, the present invention provides a method for producing a recycled polyol using waste polyurethane foam as a raw material, comprising the following steps. (a) A step of preparing crushed waste polyurethane by crushing waste polyurethane foam; (b) Based on the total amount of the mixture of the above-mentioned pulverized material and polyhydric alcohol, A step of preparing a depolymer by mixing 30% to 50% by weight of the above-mentioned ground material and 50% to 70% by weight of a polyhydric alcohol; and (c) Based on the total amount of the mixture of the above depolymer and high molecular weight polyol, A step of preparing a regenerated polyol by mixing 70% to 90% by weight of the above depolymer and 10% to 30% by weight of a high molecular weight polyol having a weight-average molecular weight (Mw) of 3,000 g / mol or more. (a) Step of preparing crushed waste polyurethane The above step involves collecting the waste polyurethane and physically crushing it. The waste polyurethane may exist in various forms, such as foam or coatings. By forming the waste polyurethane into small particles or powder, the reaction surface area can be increased during the depolymerization process, thereby enhancing the reaction rate and efficiency. The above-mentioned crushed material can be produced by crushing hard waste polyurethane foam or soft waste polyurethane foam. When polyols are manufactured using such waste polyurethane, there are effects of cost reduction and environmental protection. For example, the above-mentioned crushed material may be manufactured by crushing polyurethane used in furniture and mattresses, polyurethane of amine compounds remaining from the process of decomposition of polyurethane materials or parts used in the automotive industry, or polyurethane used in electronic and electrical products. (b) Step of preparing a depolymer According to the example, step (b) may be a step of preparing a depolymerization by mixing 30% to 50% by weight of the ground material and 50% to 70% by weight of the polyhydric alcohol, based on the total amount of the mixture of the ground material and the polyhydric alcohol. The above step is a step in which crushed waste polyurethane is mixed with polyhydric alcohol and heated, thereby breaking down the cross-links of the polyurethane and forming a depolymerized product through a depolymerization reaction. The pulverized material containing the above polyurethane may have a weight-average molecular weight (Mw) of 1,000 g / mol to 5,000 g / mol, 1,500 g / mol to 4,500 g / mol, or 2,000 g / mol to 4,000 g / mol. The above-mentioned pulverized material may be included in an amount of 30% to 50% by weight, 32% to 48% by weight, 34% to 46% by weight, or 35% to 45% by weight, based on the total amount of the mixture of the above-mentioned pulverized material and the polyhydric alcohol. The above polyhydric alcohol may have a weight-average molecular weight (Mw) of 50 g / mol to 500 g / mol, 100 g / mol to 400 g / mol, or 150 g / mol to 300 g / mol. The polyalcohol may be one or more selected from the group consisting of ethylene glycol, tripropylene glycol, diethylene glycol, thiodiethylene glycol, neopentyl glycol, triethylene glycol, tetraethylene glycol, dipropylene glycol, tripropylene glycol, and pentaerythritol. Preferably, the polyalcohol may be one or more selected from ethylene glycol, tripropylene glycol, and diethylene glycol. Preferably, the polyalcohol may be tripropylene glycol. The polyalcohol may be included in an amount of 50% to 70% by weight, 52% to 68% by weight, 54% to 66% by weight, or 55% to 65% by weight, based on the total amount of the mixture of the ground material and the polyalcohol. The step of forming the depolymer can be performed by carrying out a depolymerization reaction at 100°C to 400°C for 1 to 10 hours. Specifically, after mixing the ground material and the polyhydric alcohol, the depolymerization reaction can be carried out at 100°C to 400°C, 120°C to 380°C, 130°C to 380°C, 150°C to 370°C, or 180°C to 370°C for 2 to 9 hours, 3 to 8 hours, or 4 to 7 hours to obtain the depolymer. If the depolymerization temperature and time satisfy the above ranges, the reaction rate can be appropriately controlled to produce a regenerated polyol with a uniform molecular weight. A first catalyst may be used in the step of forming the above depolymer. The first catalyst may include one or more selected from the group consisting of potassium hydroxide, sodium hydroxide, potassium acetate, zinc acetate, a mixture of sodium acetate and strontium acetate, and a mixture of potassium acetate and strontium acetate. Preferably, the first catalyst may be one or more selected from potassium hydroxide and sodium hydroxide. By using the catalyst, a polyol composition of uniform molecular weight can be produced by appropriately controlling the reaction rate. The first catalyst may be added in an amount of 0.0001% to 5% by weight based on the total weight of the ground material. For example, the first catalyst may be added in an amount of 0.0002% to 3% by weight or 0.0003% to 2% by weight based on the total weight of the ground material. (c) Step of manufacturing recycled polyol According to the example, step (c) may be a step of preparing a regenerated polyol by mixing 70% to 90% by weight of the depolymer and 10% to 30% by weight of a high molecular weight polyol having a weight-average molecular weight (Mw) of 3,000 g / mol or more, based on the total amount of the mixture of the depolymer and the high molecular weight polyol. The above depolymer may be included in an amount of 72% to 88% by weight, 74% to 86% by weight, or 75% to 85% by weight, based on the total amount of the mixture of the above depolymer and the high molecular weight polyol. The high molecular weight polyol may have a weight-average molecular weight (Mw) of 4,000 g / mol or more, 5,000 g / mol or more, 6,000 g / mol or more, 7,000 g / mol or more, 7,500 g / mol or more, or 8,000 g / mol or more. As one example, the high molecular weight polyol may have a weight-average molecular weight (Mw) of 8,000 g / mol to 10,000 g / mol. The above high molecular weight polyol may be included in an amount of 12% to 28% by weight, 14% to 26% by weight, or 15% to 25% by weight, based on the total amount of the mixture of the depolymer and the high molecular weight polyol. The above high molecular weight polyol may be, for example, UL3318 or Y5613. In one embodiment, the high molecular weight polyol may have an OH Value of 15.0 mgKOH / g to 20.0 mgKOH / g. In one embodiment, the high molecular weight polyol may have an OH Value of 50.0 mgKOH / g to 60.0 mgKOH / g. In one embodiment, the high molecular weight polyol may have an OH Value of 160.0 mgKOH / g to 210.0 mgKOH / g. In one embodiment, the high molecular weight polyol may have an OH Value of 270.0 mgKOH / g to 330.0 mgKOH / g. The OH Value may be measured by the ASTM D 4274 method. In one embodiment, the high molecular weight polyol may have a viscosity of 1,800 cps to 3,000 cps at 25°C. In one embodiment, the high molecular weight polyol may have a viscosity of 150 cps to 400 cps at 25°C. The viscosity may be measured by the ASTM D 4878 method. In one embodiment, the high molecular weight polyol may have a moisture content of 300 ppm to 900 ppm. In one embodiment, the high molecular weight polyol may have a moisture content of 300 ppm to 600 ppm. In one embodiment, the high molecular weight polyol may have a moisture content of 5,000 ppm to 7,000 ppm. The moisture content may be measured by the ASTM E 203 method. In one embodiment, the high molecular weight polyol may have an acid value of 0.001 mg / KOH to 0.1 mg / KOH. In one embodiment, the high molecular weight polyol may have an acid value of 0.01 mg / KOH to 0.04 mg / KOH. In one embodiment, the high molecular weight polyol may have an acid value of 0.02 mg / KOH to 0.06 mg / KOH. In one embodiment, the high molecular weight polyol may have an acid value of 0.02 mg / KOH to 0.2 mg / KOH. The acid value may be measured by the ASTM D 4662 method. In one embodiment, the high molecular weight polyol may have a pH of 5.0 to 8.0. The pH may be measured by the SKC-M-704 method. In one embodiment, the high molecular weight polyol may have an APHA of 10 to 60. In one embodiment, the high molecular weight polyol may have an APHA of 20 to 60. In one embodiment, the high molecular weight polyol may have an APHA of 30 to 60. In one embodiment, the high molecular weight polyol may have an APHA of 30 to 40. The APHA may be measured by the ASTM D 1209 method. In one embodiment, the high molecular weight polyol may have a transparency (CPR) of 1.0 or less. The transparency may be measured by the ASTM D 6437 method. In one embodiment, the high molecular weight polyol may have a double bond amount (unsaturation) of 0.1 meq / g or less. In one embodiment, the high molecular weight polyol may have a double bond amount (unsaturation) of 0.05 meq / g or less. The double bond amount may be measured by the ASTM D 4671 method. In one embodiment, the high molecular weight polyol may have an antioxidant content of 800 ppm to 1,200 ppm. In one embodiment, the high molecular weight polyol may have an antioxidant content of 5,000 ppm to 7,000 ppm. In one embodiment, the high molecular weight polyol may have an antioxidant content of 1,000 ppm to 2,000 ppm. In one embodiment, the high molecular weight polyol may have an antioxidant content of 6,000 ppm to 8,000 ppm. In one embodiment, the high molecular weight polyol may have an antioxidant content of 7,000 ppm to 11,000 ppm. The antioxidant content may be measured by the UV-Vis method. In one embodiment, the high molecular weight polyol may have an ethylene oxide (EO) content of 20.0 wt% to 30.0 wt%. In one embodiment, the high molecular weight polyol may have an ethylene oxide (EO) content of 5.0 wt% to 12.0 wt%. The ethylene oxide content may be measured by the ASTM D 4875 method. In one embodiment, the high molecular weight polyol may have a potassium ion content of 10 ppm or less. In one embodiment, the high molecular weight polyol may have a potassium ion content of 6 ppm or less. The potassium ion content may be measured by the ASTM D 4668 method. In one embodiment, the high molecular weight polyol may have an active oxygen content of 2.0 ppm or less. In one embodiment, the high molecular weight polyol may have an active oxygen content of 1.7 ppm or less. The active oxygen content may be measured by the SKC-M-706 method. As one example, the high molecular weight polyol may be UL3318. The above UL3318 may be polypropylene glycol randomly mixed with ethylene oxide. The above UL3318 can improve the strength, durability, and hydrolytic properties of polyurethane and is a material that can be used to produce urethane for coatings, adhesives, sealants, and elastomers. As one example, the high molecular weight polyol may be Y5613. The above Y5613 may be polypropylene glycol randomly mixed with ethylene oxide. The above Y5613 is used in the production of conventional soft polyurethane slabstock foam and can be mixed with other polyols to obtain desired polyurethane foam properties. As one example, the high molecular weight polyol may be Y5603. The above Y5603 is a polypropylene glycol and can be used in the production of conventional soft polyurethane slabstock foam. The above Y5603 can be mixed with other polyols to obtain desired polyurethane foam properties. As one example, the high molecular weight polyol may be DF600. The above DF600 may be a polyether diol that can be used to widely produce urethanes for coatings, adhesives, sealants, and elastomers as prepolymers as well as in one-shot formulations. As one example, the high molecular weight polyol may be Y1030. The above Y1030 is a polypropylene glycol and can be used particularly in the production of low-elasticity slabstock foam for furniture. The above Y1030 can be mixed with other polyols to obtain desired polyurethane foam properties. The present invention will be described in more detail below based on examples and comparative examples. However, the following examples and comparative examples are merely illustrative for further explaining the present invention, and the present invention is not limited by the following examples and comparative examples. Preparation Example Preparation Example 1 - Preparation of Regenerated Polyol #1 A four-necked flask equipped with a heating mantle, a condenser, a stirring device, and a temperature controller was prepared. Subsequently, waste polyurethane foam (Sewon Co., SLAB) was crushed using a grinder to prepare crushed waste polyurethane foam. The crushed waste polyurethane foam, tripropylene glycol (TPG, SK picglobal), and the first catalyst (KOH, 3,500 ppm based on the total weight of the reactants) were introduced into the flask. The crushed waste polyurethane foam and the tripropylene glycol were introduced in a ratio of 55:45. Subsequently, the temperature of the reactants introduced into the flask was increased to 210°C at a heating rate of 3.5°C / minute. Afterward, the reactants were depolymerized for 6 hours. Once the reaction was terminated, the temperature of the reaction product was slowly lowered over 2 hours. Subsequently, the cooled reactant was filtered through a filter having a diameter of 254 μm, and regenerated polyol (depolymerized polyol composition) #1 was prepared. Preparation Examples 2 to 5 - Preparation of Regenerated Polyols #2 to #5 Regenerated polyols #2 to #5 were each prepared in the same manner as in Preparation Example 1, except that the content ratio of waste polyurethane foam crushed material and tripropylene glycol, the depolymerization temperature and time, and the content of the first catalyst used were changed as shown in Table 1 below. Classification Weight Ratio (Crushed Waste Polyurethane: TPG) Depolymerization Temperature (°C) Depolymerization Time (Hour) Content of First Catalyst (ppm, based on total reactant weight) Preparation Example 155 : 452 106 3,500 Preparation Example 260 : 402 106 3,500 Preparation Example 355 : 452 101 22,000 Preparation Example 440 : 602 106 3,500 Preparation Example 550 : 502 106 3,500 Preparation Example 6 - Preparation of Addition Polyol #1 600 g of the regenerated polyol #1 prepared in Preparation Example 1 above and the second catalyst (KOH, approximately 3000 ppm based on the total weight of the reactants) were introduced into a pressurized reactor. The reactants inside the reactor were stirred by a stirring device, and the temperature of the reactants was raised to approximately 110°C, and the pressure inside the reactor was reduced by a vacuum pump. After being continuously reduced for 1 hour, the inside of the reactor was maintained in a vacuum state. After the temperature of the reactor was maintained at approximately 110°C, 1400 g of propylene oxide was introduced into the reactor for approximately 340 minutes. The regenerated polyol #1 and the propylene oxide were reacted in a content ratio of 30:70. After the introduction of the propylene oxide was completed, the reaction proceeded until the internal pressure of the reactor became constant. Once the internal pressure of the reactor became constant, the vacuum pump was used again to remove any remaining propylene oxide inside the reactor. Subsequently, the remaining catalyst was removed, and addition polymerization polyol #1 was obtained. Preparation Example 7 - Preparation of Addition Polyol #2 It was prepared in the same manner as Preparation Example 6, except that recycled polyol #3 was used instead of recycled polyol #1, and the weight ratio of recycled polyol #3 to propylene oxide was 26:74. Preparation Example 8 - Preparation of Recycled Polyol #8 A four-necked flask equipped with a heating mantle, a condenser, a stirring device, and a temperature controller was prepared, and 50g of hydroxypropyl glycol (HPG, SK picglobal) and 20g of solvent (TF3000) were added to the flask. The temperature of the flask was increased to 210℃ at a heating rate of 3.5℃ / min. Subsequently, 30g of crushed waste polyurethane foam (LNG board) prepared by crushing waste polyurethane foam with a crusher and 0.35g of catalyst (KOH) were placed in a flask, and a depolymerization reaction was carried out for 6 hours while maintaining a temperature of 210℃. When the reaction was completed, the temperature was lowered to 120℃ by natural cooling for 1 hour, and then filtered through a filter with a diameter of 254 μm to produce recycled polyol #8. For reference, the above hydroxypropyl glycol (HPG) refers to a substance in which tripropylene glycol, tetrapropylene glycol, and pentapropylene glycol are mixed in a ratio of 8.5 : 82.9 : 5.8. The above HPG has Mw = 237 g / mol, hydroxyl group value = 472 mgKOH / g, and functional group value = 2. For reference, the above TF3000 refers to a solvent with Mw = 3,000 g / mol, hydroxyl group value = 56 mgKOH / g, and functional group value = 3. Preparation Examples 9 to 11 - Preparation of Regenerated Polyols #9 to #11 Recycled polyols #9 to #11 were prepared in the same manner as in Preparation Example 8, except that the content of crushed waste polyurethane foam, the type and content of polyhydric alcohol, and the type and content of solvent were changed as shown in Table 2. For reference, TPG has Mw = 192 g / mol, hydroxyl group value = 584 mgKOH / g, and functional group value = 2. For reference, TF1800 refers to a solvent with Mw = 1,800 g / mol, hydroxyl value = 93.5 mgKOH / g, and functional value = 3. Preparation Examples 12 and 13 - Preparation of Regenerated Polyols #12 and #13 Regenerated polyols #12 and #13 were prepared in the same manner as in Preparation Example 1, except for the type and content of the polyalcohol and the fact that no solvent was added. Classification Waste Polyurethane Crushed Material Content (g) Type of Polyhydric Alcohol Content of Polyhydric Alcohol (g) Type of Solvent Content of Solvent (g) Preparation Example 8 30 HPG 50 TF 300 0 20 Preparation Example 9 30 TPG 50 TF 300 0 20 Preparation Example 10 30 TPG 50 TF 180 0 20 Preparation Example 11 20 TPG 60 TF 180 0 20 Preparation Example 12 50 HPG 50 -- Preparation Example 13 40 TPG 60 -- Preparation Example Preparation Example 14 - Preparation of Regenerated Polyol #14 A 4-neck flask equipped with a heating mantle, a condenser, a stirring device, and a temperature controller was prepared, and 1500g of tripropylene glycol (TPG, SK picglobal) was added to the flask, along with 10.5g of the first catalyst (KOH). After increasing the temperature of the flask to 210℃ at a heating rate of 3.5℃ / min, 1500g of crushed waste polyurethane foam (extracted from waste car seats) was added and the depolymerization reaction was carried out for 6 hours. Once the reaction was complete, the temperature was slowly lowered over 2 hours, and the mixture was filtered through a filter with a diameter of 254 μm to produce recycled polyol #14. Preparation Examples 15 to 17 - Preparation of Regenerated Polyols #15 to #17 Regenerated polyols #15 to #17 were each prepared in the same manner as in Preparation Example 14, except that the content of waste polyurethane foam crushed material, the content of tripropylene glycol (TPG), the depolymerization temperature and time, and the content of the first catalyst used were changed as shown in Table 3 below. Content of crushed waste polyurethane foam (g) TPG content (g) Polymerization temperature (°C) Polymerization time (hours) Content of first catalyst (g) Preparation Example 14 1500 1500 210 6 10.5 Preparation Example 15 1800 1200 210 12 10.5 Preparation Example 16 1800 1200 210 6 15.0 Preparation Example 17 1800 1200 210 6 30.0 Preparation Example 18 - Preparation of Addition Polyol #3 650 g of regenerated polyol #1 prepared in Preparation Example 1 and 3,000 ppm of the second catalyst (KOH) were introduced into a pressurized reactor. While stirring the inside of the reactor using a stirring device, the temperature of the reactor was raised to 110°C, and then the pressure was reduced using a vacuum pump. After continuously reducing the pressure for 1 hour, the vacuum pump was turned off, and the inside of the reactor was maintained under vacuum. The temperature of the reactor was raised again to 110°C, and 2,050 g of propylene oxide was introduced over 340 minutes. After the introduction of propylene oxide was completed, the reaction was carried out until the internal pressure of the reactor became constant. Once the internal pressure became constant, the remaining propylene oxide was removed by reducing the pressure again using a vacuum pump, and the remaining catalyst was removed using Magnesol to obtain addition polymerization polyol #3. Preparation Examples 19 and 20 - Preparation of Addition Polyols #4 and #5 Addition polymerization polyol #4 and addition polymerization polyol #5 were prepared in the same manner as Preparation Example 5, except that the type and content of the regenerated polyol, the content of propylene oxide, the reaction temperature, and the content of the second catalyst were changed as shown in Table 4 below. Content of polymerized polyol, content of regenerated polyol (g), content of propylene oxide (g), reaction temperature (°C), content of second catalyst (ppm) Preparation Example 18#365020501103000 Preparation Example 19#4135013501103000 Preparation Example 20#5108016201103000 Experimental Example 1: Gel Permeation Chromatography (GPC) The content of polyols according to number average molecular weight in the polyol compositions according to the above preparation examples was measured using gel permeation chromatography (GPC). The content of each polyol was derived from the area of ​​each peak based on the total area of ​​the GPC peaks. Tetrahydrofuran (THF) was used as the organic solvent. The measurement results are shown in the tables below. Classification Less than 100g / mol (%) 100g / mol ~210g / mol (%) 210g / mol ~320g / mol (%) 320g / mol ~430g / mol (%) 430g / mol ~1,800g / mol (%) More than 1,800g / mol (%) Preparation Example 1 23.66 25.94 7.8 26.81 5.88 29.89 Preparation Example 2 12.83 21.27 4.67 10.78 15.37 35.08 Preparation Example 3 20.11 25.9 18.24 7.07 10.57 28.10 Preparation Example 4 17.47 36.15 7.17 9.54 14.93 14.74 Preparation Example 514.9027.687.9111.5521.6416.32 Classification 100g / mol ~3,000g / mol(%) Over 3,000g / mol(%) Preparation Example 686.6113.39 Preparation Example 786.4313.57 Classification Less than 280g / mol (%) 280g / mol ~660g / mol (%) 660g / mol ~1,130g / mol (%) More than 1,130g / mol (%) Preparation Example 8 28.69 14.33 16.57 40.41 Preparation Example 9 27.21 18.63 15.87 38.29 Preparation Example 10 27.51 18.24 15.30 38.95 Preparation Example 11 39.75 16.38 12.54 31.33 Preparation Example 12 19.11 18.30 20.15 42.44 Preparation Example 13 28.39 21.79 20.34 29.48 Classification Less than 100g / mol (%) 100g / mol ~250g / mol (%) 250g / mol ~700g / mol (%) 700g / mol ~2,500g / mol (%) More than 2,500g / mol (%) Preparation Example 14 - 45.36 20.41 11.10 23.13 Preparation Example 15 - 44.50 19.12 10.37 26.01 Preparation Example 16 - 6.42 39.30 18.47 8.09 27.72 Preparation Example 17 - 7.10 43.01 16.13 6.98 26.78 Classification Less than 260g / mol (%) 260g / mol ~3,000g / mol (%) More than 3,000g / mol (%) Preparation Example 185.2984.4310.29 Preparation Example 193.0381.9914.97 Preparation Example 201.5384.4014.07 Experimental Example 2: Measurement of OH Value of Polyol Composition The above OH Value refers to the number of mg of NaOH required to neutralize acetic acid combined with hydroxyl groups when acetylating 1 g of the sample, and was measured according to ASTM E222-10. The measurement results are shown in the tables below. Experimental Example 3: Measurement of Viscosity of Polyol Composition The viscosity of the polyol compositions prepared according to the above preparation examples was measured using Brookfield's DV-2 at 25°C. The measurement results are shown in the tables below. Experimental Example 4: Measurement of impurities in the polyol composition during the depolymerization process After the depolymerization reaction according to the above manufacturing examples was completed, filtration was performed using a nonwoven fabric filter (air permeability 8±2 cc / cm2 / sec), and the weight of impurities caught in the filter was measured and the results are shown in the tables below. Experimental Example 5: Measurement of Recycle Content (R / C) of Polyol Composition The R / C of the polyol composition prepared through the depolymerization process according to the above manufacturing examples is the content of the foam used in the polyol synthesis, and the calculated value is the content of the foam added based on 100% of the final composite, and the calculated value is shown in the tables below. Experimental Example 6: Measurement of yield of polyol composition The yield of the polyol composition prepared through the depolymerization process according to the above manufacturing examples was measured. Specifically, the amount of the polyol composition produced after depolymerization was expressed as a percentage relative to the amount of waste polyurethane input. The measurement results are shown in the tables below. Classification OH Value Viscosity Impurities R / C Yield Unit mgKOH / gmPa·s %%% Preparation Example 137 21,000 0.47 559 6.96 Preparation Example 234 41,550 0.24 609 7.52 Preparation Example 34 30550 0.585 59 5.56 Preparation Example 44 67 4500 0.13 409 8.34 Preparation Example 54 197 000 0.29 509 7.61 Preparation Example 61 203 20-16.59 5.00 Preparation Example 71 26300-14.39 5.60 Classification OH Value Viscosity Impurities Yield Unit mgKOH / gmPa·s %% Preparation Example 83 15.8 180 0 2.7 49 4.25 Preparation Example 93 89.01 370 2.16 95.38 Preparation Example 10 38 7.41 180 3.24 9 4.25 Preparation Example 11 43 2.7 380 3.4 7 9 4.60 Preparation Example 12 33 9.32 2300 3.4 4 9 2.17 Preparation Example 13 46 0.21 80 0 2.66 9 4.28 Classification OH Value Viscosity Impurities R / C Yield Unit mgKOH / gmPa·s %%% Preparation Example 1449 7.5 270 4.2 509 1.8 Preparation Example 1539 9.6 1 200 7.9 608 8.1 Preparation Example 1639 7.1 1 460 8.6 608 6.4 Preparation Example 1741 6.4 1 320 20.0 607 5.0 Preparation Example 1812 6.3 250 -9.6 91.0 Preparation Example 1922 0.0 320 -259 0.0 Preparation Example 2018 0.9 340 -209 0.0 Through Tables 10 and 12 above, it can be seen that the polyol composition prepared through the depolymerization process according to the above manufacturing examples can produce a polyurethane with high flexibility and low crosslinking density by optimizing the balance of OH Value, viscosity, and impurity content. Through Table 12 above, it can be confirmed that the polyol composition prepared through the depolymerization process according to the above manufacturing examples has a high yield while having viscosity and Recycle Content within an appropriate range. Examples and Comparative Examples Example 1 - Preparation of Polyurethane Foam Twenty parts by weight of the recycled polyol #1 prepared in Preparation Example 1 above were added to a plastic beaker. Subsequently, 60 parts by weight of base polyol 1 (OH value = 56 mgKOH / g), 20 parts by weight of base polyol 2 (OH value = 35 mgKOH / g), 10 parts by weight of polymer polyol (OH value = 30 mgKOH / g), 3.3 parts by weight of distilled water, 0.1 parts by weight of amine catalyst, 1.0 parts by weight of silicone foam stabilizer, and 0.2 parts by weight of curing catalyst were added to the beaker. Subsequently, the mixture was mixed using a high-speed stirrer at 4,000 rpm for 3 minutes to obtain a mixture. The average OH value of the mixture is 77.06 mgKOH / g. The mixture consists of a total of 104.6 parts by weight, and the mixing ratio of each component is as described above. Subsequently, toluene diisocyanate (TDI) was added to the mixture in an amount of 48.9 parts by weight, where the total amount of the mixture was 100 parts by weight, and then foamed to produce a polyurethane foam. The content of each component is as shown in Table 5 below. Examples 2 to 5 - Preparation of Polyurethane Foam Polyurethane foam was prepared in the same manner as in Example 1, except that recycled polyols #2 and #3 and addition polymerization polyols #1 and #2 were applied instead of recycled polyol #1 during the preparation of the polyurethane foam, and the content of toluene diisocyanate was applied as shown in Table 5 below. The average OH value of the polyol mixture in Example 2 above is 74.67 mgKOH / g. The average OH value of the polyol mixture in Example 3 above is 82.79 mgKOH / g. The average OH value of the polyol mixture in Example 4 above is 53.63 mgKOH / g. The average OH value of the polyol mixture in Example 5 above is 53.63 mgKOH / g. Comparative Examples 1 and 2 - Preparation of Polyurethane Foam Polyurethane foam was manufactured in the same manner as in Example 1, except that recycled polyols #4 and #5 were applied instead of recycled polyol #1, respectively, during the manufacture of the polyurethane foam, and the content of toluene diisocyanate was applied as shown in Table 13 below. The average OH value of the polyol mixture in Comparative Example 1 above is 86.62 mgKOH / g. The average OH value of the polyol mixture in Comparative Example 2 above is 81.84 mgKOH / g. Classification Type of Polyol Content of Toluene Isocyanate [parts by weight] Example 1 Regenerated Polyol #1 48.90 Example 2 Regenerated Polyol #2 48.47 Example 3 Regenerated Polyol #3 49.92 Example 4 Additive Polymerization Polyol #1 44.71 Example 5 Additive Polymerization Polyol #2 44.71 Comparative Example 1 Regenerated Polyol #4 50.60 Comparative Example 2 Regenerated Polyol #5 49.75 Examples and Comparative Examples Example 6 - Preparation of Polyurethane Foam Two parts by weight of recycled polyol #8 prepared in Preparation Example 8 were added to a plastic beaker. Subsequently, 48 parts by weight of base polyol 1 (OH value = 450 mgKOH / g), 20 parts by weight of base polyol 2 (OH value = 235 mgKOH / g), 5 parts by weight of base polyol 3 (OH value = 410 mgKOH / g), 20 parts by weight of base polyol 4 (OH value = 240 mgKOH / g), 7 parts by weight of base polyol 5 (OH value = 93.5 mgKOH / g), 1.65 parts by weight of distilled water, 0.5 parts by weight of amine catalyst, 2.0 parts by weight of silicone foam stabilizer, 20.0 parts by weight of flame retardant, 2.8 parts by weight of trimer catalyst, and 15.0 parts by weight of foaming agent were added to the beaker. Subsequently, the mixture was mixed at 4,000 rpm for 3 minutes using a high-speed stirrer to obtain a mixture. The above mixture consists of a total of 141.95 parts by weight, and the mixing ratio of each component is as above. Subsequently, 150 parts by weight of methylene diphenyl diisocyanate (MDI) were added to the mixture, with the total amount of the mixture being 100 parts by weight, and then foamed to produce a rigid polyurethane foam. Examples 7 to 9 and Comparative Examples 3 and 4 - Preparation of Polyurethane Foam A rigid polyurethane foam was prepared in the same manner as in Example 6, except that recycled polyols #9 to #13 were applied instead of recycled polyol #8 during the preparation of the polyurethane foam (see Table 14). Classification Type of Recycled Polyol Example 6 Recycled Polyol #8 Example 7 Recycled Polyol #9 Example 8 Recycled Polyol #10 Example 9 Recycled Polyol #11 Comparative Example 3 Recycled Polyol #12 Comparative Example 4 Recycled Polyol #13 Example 10 - Preparation of Polyurethane Foam The recycled polyol #14 prepared in Preparation Example 14 above, base polyol 1 (OH Value = 22 mgKOH / g), base polyol 2 (OH Value = 35 mgKOH / g) 30 wt%, base polyol 3 (OH Value = 56 mgKOH / g) 2 wt%, base polyol 4 (OH Value = 31 mgKOH / g) 1.1 wt%, polymer polyol (OH Value = 20 mgKOH / g) 18 wt%, foaming agent (water) 0.15 wt%, crosslinking agent (OH Value = 1601 mgKOH / g) 0.15 wt%, amine-based catalyst 0.48 wt%, and foam stabilizer 0.8 wt% were mixed. The above mixture consists of a total of 107.46 parts by weight, and the mixing ratio of each component is as described above. Subsequently, an isocyanate (Kumho Mitsui MC82W product) in which methylene diisocyanate (MDI) and toluene diisocyanate (TDI) are mixed in a certain ratio was added to the above mixture, with 44.3 parts by weight of the isocyanate being added to the total mixture as 100 parts by weight. Then, the mixture was poured into an open box with dimensions of 350 cm X 350 cm X 200 cm to produce polyurethane foam. The content of each component is as shown in Table 15 below. Example 11 - Preparation of Polyurethane Foam When manufacturing the polyurethane foam, recycled polyol #15 is applied instead of recycled polyol #14, and the content of each component is as shown in Table 15 below. Otherwise, it is the same as Example 10. Examples 12 to 14 - Preparation of Polyurethane Foam When manufacturing the polyurethane foam, addition polymerization polyols #3 to #5 are applied instead of the recycled polyol #14, and the content of each component is as shown in Table 15 below. Otherwise, it is the same as Example 10. Comparative Examples 5 and 6 - Preparation of Polyurethane Foam When manufacturing the polyurethane foam, recycled polyols #15 and #16 were applied instead of recycled polyol #14, respectively, and the content of each component is as shown in Table 15 below. Otherwise, it is the same as Example 10. Classification Type of Polyol Content of Recycled Polyol (weight%) Content of Base Polyol 1 (weight%) Content of Isocyanate (parts by weight) Example 10 Recycled Polyol #1 45.4 46.6 44.3 Example 11 Recycled Polyol #1 54.5 47.5 42.7 Example 12 Additive Polymerization Polyol #3 28 24.0 44.9 Example 13 Additive Polymerization Polyol #4 10.8 41.2 43.5 Example 14 Additive Polymerization Polyol #5 13.5 38.5 43.5 Comparative Example 5 Recycled Polyol #1 64.5 47.5 42.7 Comparative Example 6 Recycled Polyol #1 74.5 47.5 42.8 Experimental Example 7: Evaluation of Moldability of Polyurethane Foam In the above examples and comparative examples, the moldability of the polyurethane foam was evaluated by marking X for cases where the reaction rate was too fast to properly pour into the beaker or where shrinkage occurred in the foam after manufacturing, and O for cases where such problems did not occur. The results are shown in Table 16 below. Classification Molding Example 10 Example 20 Example 30 Example 40 Example 50 Comparative Example 1X Comparative Example 2X Classification Molding Example 100 Example 110 Example 120 Example 130 Example 140 Comparative Example 5X Comparative Example 6X Experimental Example 8: Evaluation of Reactivity of Polyurethane Foam When manufacturing polyurethane foam according to the above examples and comparative examples, the time (Cream Time, C / T) from immediately after mixing the isocyanate and polyol until the point where the mixture begins to become cloudy was measured. In addition, the rise time (R / T) taken for the foam to reach its maximum expansion height was measured. The measurement results are shown in Table 18 below. In addition, the settling rate, which is the ratio of the foam shrinkage after maximum expansion following foaming, was calculated according to Formula 1 below. The measurement results are shown in Table 19 below. [Formula 1] Settling = ((Maximum Height - Final Height) / Maximum Height) X 100 Classification Cream Time Expansion Time Unit Second (sec) Second (sec) Example 1 19132 Example 2 19134 Example 3 19139 Example 4 19126 Example 5 19130 Comparative Example 118144 Comparative Example 2 17149 Classification Cream Time Expansion Time Sedimentation Rate Unit sec (sec) sec (sec) % Example 10 12 12 0 11 Example 11 12 11 6 8.4 Example 12 12 10 5 15 Example 13 13 12 9 7.6 Example 14 12 12 8 14 Comparative Example 5 12 Unmeasurable Uncalculable Comparative Example 6 12 Unmeasurable Uncalculable Experimental Example 9: Density Measurement The density of the polyurethane foams prepared in the above examples and comparative examples was measured using a universal testing machine (UTM) analyzer in accordance with ASTM D-3574-86. The measurement results are shown in the tables below. Experimental Example 10: Measurement of Hardness (25% ILD, 65% ILD) The ILD of the polyurethane foams prepared in the above examples and comparative examples was measured using a UTM analyzer in accordance with ASTM D-3574-86. The measurement results are shown in the tables below. Experimental Example 11: Measurement of Deflection Coefficient The deflection modulus of the polyurethane foams prepared in the above examples and comparative examples was measured using a UTM analyzer in accordance with ASTM D-3574-86. The measurement results are shown in the tables below. Experimental Example 12: Measurement of Tear Strength The tear strength of the polyurethane foams prepared in the above examples and comparative examples was measured using a UTM analyzer in accordance with ASTM D-3574-86. The measurement results are shown in the tables below. Experimental Example 13: Tensile strength (

[0112] tensile strength measurement The tensile strength of the polyurethane foams prepared in the above examples and comparative examples was measured using a UTM analyzer in accordance with ASTM D-3574-86. The measurement results are shown in Table 20 below. Experimental Example 14: Measurement of Elongation The polyurethane foams prepared in the above examples and comparative examples were subjected to elongation measurements using a UTM analyzer in accordance with ASTM D-3574-86. The measurement results are shown in Table 20 below. Experimental Example 15: Measurement of Rebound Elasticity The rebound elasticity of the polyurethane foams prepared in the above examples and comparative examples was measured using a UTM analyzer in accordance with ASTM D-3574. The measurement results are shown in Table 20 below. Experimental Example 16: Measurement of Permanent Compression Set The permanent compression reduction of the polyurethane foams prepared in the above examples and comparative examples was measured using a UTM analyzer in accordance with ASTM D-3574-86. The permanent compression reduction refers to the recovery rate when the foam is restored after compression. The measurement results are shown in Table 22 below. - Dry: Measured under normal atmospheric conditions - Wet: Measured after high temperature and high humidity conditions (70℃, 95% RH) Experimental Example 17: Measurement of Resilience The resilience of the polyurethane foams prepared in the above examples and comparative examples was measured using a UTM analyzer in accordance with ASTM D-3574. Rebound elasticity was measured. The measurement results are shown in Table 20 below. Specifically, polyurethane foam was compressed to 50%, maintained at 23°C and 50% RH for 22 hours, and the degree of thickness recovery was measured 30 minutes after pressure was released. This was expressed as a percentage of the original thickness indicating how much of the compressed state remained. A lower measured value indicates superior resilience. Experimental Example 18: Measurement of Dynamic Fatigue The dynamic fatigue of the polyurethane foams prepared in the above examples and comparative examples was measured using a UTM analyzer in accordance with ASTM D-3574-86. Dynamic fatigue refers to how well performance is maintained after the application of repetitive loading. The measurement results are shown in Table 22 below. - Thickness Loss: Thickness loss rate after repeated compression - Hardness Loss: Rate of hardness reduction after repeated compression Experimental Example 19: Measurement of Hysteresis Loss The hysteresis loss of the polyurethane foams prepared in the above examples and comparative examples was measured using a UTM analyzer in accordance with ASTM D-3574-5. The measurement results are shown in Table 22 below. Experimental Example 20: Measurement of Stress Relaxation The polyurethane foams prepared in the above examples and comparative examples were measured using the test method below, and the results are shown in Table 22 below. Using a specimen cut to a size of 50 mm in width and length and 25 mm in thickness, the specimen was pre-compressed twice to a load of 19.6 N (or 2 kgf) at a speed of 100 mm / min using a UTM analyzer, and then the load was removed at the same speed to return it to its initial thickness. Immediately after the second load removal, compression was applied to the specimen at the same speed and force, and the displacement was maintained for 2 hours. The rate of change of load was then calculated, and the stress relaxation was calculated according to Equation 2 below. [Formula 2] Stress Relaxation (%) = (Fo - F1) / Fo X 100 In Equation 2 above, Fo = initial load (19.6N), F1 = load after 2 hours (N) Experimental Example 21: Breathability Measurement The air permeability of the polyurethane foams prepared in the above examples and comparative examples was measured using air flow meters in accordance with the ASTM D-3574 method. The measurement results are shown in Table 20 below. Three specimens are prepared with dimensions of 51.0±0.3 X 51.0±0.3 X 25.0±0.5. Measurements are taken in the Foam Rise direction, perpendicular to it, and in the horizontal direction, respectively, and the average value is taken for each direction. Classification Density Hardness Tear Strength Tensile Strength Elongation Rebound Elasticity Restoration Breathability 25% ILD 65% ILD Unit kg / m² 3kg / 314cm 2 kPakPa%%%Ft 3 / min Example 1 30.2 20.6 38.70.70 1.2 21 58 322.1 34.06 Example 2 30.8 21.3 39.90.7 31.1 51 45 37 1.7 42.40 Example 3 30.8 22.1 41.70.6 21.1 31 53 26 2.0 28.94 Example 4 30.6 21.2 39.70.60 1.1 1 64 40 1.9 50.33 Example 5 30.6 21.0 39.5 0.5 9 1.0 91 60 38 1.9 45.21 Comparative Example 1---------Comparative Example 2--------- Through Table 20 above, it can be confirmed that the polyurethane foams of the examples are excellent in terms of durability, resilience, and elasticity. On the other hand, the polyurethane foams of the comparative examples had poor moldability, such as shrinkage, making it impossible to measure mechanical properties. Experimental Example 22: Strength Measurement The strength of the polyurethane foams prepared in the above examples and comparative examples was measured in the horizontal or vertical direction using a UTM analyzer in accordance with ASTM D-3574-86. The measurement results are shown in Table 21 below. Experimental Example 23: Measurement of Thermal Conductivity The thermal conductivity of the polyurethane foams prepared in the above examples and comparative examples was measured using a FOX 200 instrument according to the KSL 9016 method. The measurement results are shown in Table 21 below. Classification Density Hardness Thermal Conductivity Vertical Horizontal Vertical Horizontal Unit kg / m 3 N / cm 2 kcal / m·hr·℃ Example 6 36.4 36.5 2.6 80.99 195.2 Example 7 36.0 36.5 2.7 41.0 8 195.6 Example 8 35.1 35.0 2.6 51.2 7193.6 Example 9 36.1 36.4 2.7 01.0 3194.5 Comparative Example 3 35.4 35.6 2.6 81.0 8 212.8 Comparative Example 4 35.8 36.0 2.6 90.99 209.7 Through Table 21 above, it can be confirmed that the polyurethane foam of the examples has a thermal conductivity of 200 kcal / m·hr·℃ or less, so it has superior thermal insulation performance compared to the comparative example. Classification Density Hardness Deflection Modulus Tear Strength Tensile Strength Elongation Permanent Compression Reduction Rate Dynamic Fatigue Hysteresis Stress Loss Relaxation 25% ILD 65% ILD Wet Thickness Loss Hardness Loss Unit kg / m² 3 kg / 314cm 2 -kPakPa%%%%% Example 1067.117.451.12.7759.8119.611212.38.91.913.22130.7 Example 1166.523.967.32.7563.7129.41078.66.41.512.72026 Example 1267.112.640.23.2254.9125.41152712.62.715.722.927 Example 1366.427.575.32.7067.6135.21016.75.21.612.417.322.2 Example 1465.512.939.92.9456.8117.61122512.82.716.120.224 Comparative Example 5-------------Comparative Example 6------------- Through Table 22 above, it can be confirmed that the polyurethane foams of the examples are excellent in terms of durability, resilience, and elasticity. On the other hand, the polyurethane foams of the comparative examples had poor moldability, such as shrinkage, making it impossible to measure mechanical properties. Preparation Example 21 - Waste polyurethane foam: Polyurethane foam from scrapped car seats - Polyhydric alcohol: Tripropylene glycol (TPG, SK picglobal) - First Catalyst: KOH - High molecular weight polyols: Use UL3318 (refer to Table 23 below), Y5613 (refer to Table 24 below), Y5603L (refer to Table 25 below), DF600 (refer to Table 26 below), or Y1030 (refer to Table 27 below). Classification Unit Production Spec.maxPrdctnSpec Sales Spec.maxSaleSpecTest Method OH Value mg KOH / g 17.60 18.40 17.50 18.50 ASTM D 4274 Viscosity cps @ 25℃ 2100.00 2700.00--ASTM D 4878 Moisture content ppm-500.00-800.00 ASTM E 203 Acid Value mg / KOH-0.02-0.02 ASTM D 4662 pH-5.50 7.50 5.50 7.50 SKC-M-704 Color APHA-30.00-50.00 ASTM D 1209 Transparency--1.00-1.00 ASTM D 6437 Double bond amount meq / g-0.010--ASTM D 4671 Antioxidant Content ppm 900.00 1100.00--UV-Vis Ethylene Oxide Content wt% 24.00 26.00--ASTM D 4875 Classification Unit Production Spec.maxPrdctnSpec Sales Spec.maxSaleSpecTest Method OH Value mg KOH / g 54.50 57.50 54.00 58.00 ASTM D 4274 Moisture Content ppm-400.00-800.00 ASTM E 203 Acid Value mg / KOH-0.02-0.03 ASTM D 4662 pH-5.50 7.50 5.50 7.50 SKC-M-704 Color APHA-35.00-35.00 ASTM D 1209 Potassium Ion Content ppm-5.00-- ASTM D 4668 Double Bond Amount meq / g-0.05-0.05 ASTM D 4671 Antioxidant Content ppm-8000.00 10000.00-- UV-Vis Ethylene Oxide Content wt% 7.50 9.50 -- ASTM D 4875 Active oxygen content ppm 1.50 -- SKC-M-706 Classification Unit Production Spec.maxPrdctnSpec Sales Spec.maxSaleSpecTest Method Acid Value mg / KOH-0.02-0.03 ASTM D 4662 Antioxidant Content ppm 5600.006400.00--UV-Vis Color APHA-35.00-35.00 ASTM D 1209 Potassium Ion Content ppm-5.00--ASTM D 4668 OH Value mg KOH / g 54.5057.5054.0058.00 ASTM D 4274 pH-5.507.505.507.50 SKC-M-704 Double Binding Amount meq / g-0.045-0.050 ASTM D 4671 Moisture Content ppm-400.00-800.00 ASTM E 203 Classification Unit Production Spec.maxPrdctnSpec Sales Spec.maxSaleSpecTest Method Acid Value mg / KOH-0.04-0.04 ASTM D 4662 Antioxidant Content ppm 1200 1800--UV-Vis Appearance-No-dip-SKC-M-123 Color APHA-20-50 ASTM D 1209 Transparency--1.0-1.0 ASTM D 6437 OH Value mgKOH / g 180.00 194.00 177.00 197.00 ASTM D 4274 pH-5.50 7.50 5.50 7.50 SKC-M-704 Double Binding Amount meq / g-0.03--ASTM D 4671 Moisture Content ppm-300-500 ASTM E 203 Classification Unit Production Spec.maxPrdctnSpec Sales Spec.maxSaleSpecTest Method Acid Value mg / KOH - 0.04 - 0.1 ASTM D 4662 Active Oxygen Content ppm - 1.50 --SKC-M-706 Antioxidant Content ppm 6700.00 7300.00 --UV-Vis Color APHA - 40-50 ASTM D 1209 Potassium Ion Content ppm - 5 --ASTM D 4668 OH Value mg KOH / g 2953 15290 320 ASTM D 4274 pH - 5.57.55.57.5 SKC-M-704 Double Bond Amount meq / g - 0.04 --ASTM D 4671 Viscosity cps @ 25℃ 230330 --ASTM D 4878 Moisture Content ppm - 500-800 ASTM E 203 A four-necked flask equipped with a heating mantle, a condenser, a stirring device, and a temperature controller was prepared. Tripropylene glycol (TPG) was added to the flask, followed by the addition of the first catalyst. The temperature of the flask was raised to 210°C at a heating rate of 3.5°C / min, then raised to 200°C. Subsequently, crushed waste polyurethane foam, prepared by crushing waste polyurethane foam with a grinder, was added, and the depolymerization reaction was carried out for 6 hours. Upon completion of the reaction, the temperature was slowly lowered over 2 hours, and the mixture was filtered through a filter with a diameter of 254 μm to produce a depolymer. Then, the depolymer was mixed with the prepared high molecular weight polyol to produce a regenerated polyol. The respective contents are as listed in Table 6 below. Additional Manufacturing Examples 22 to 28 The final recycled polyol was prepared in the same manner as the additional preparation example, except that the content of each input material was different as shown in Table 28 below. Content of crushed waste polyurethane [parts by weight] Content of polyhydric alcohol [parts by weight] Content of high molecular weight polyol [parts by weight] Catalyst [ppm] UL3318Y5613 Preparation Example 21244-3500 Preparation Example 2224-43500 Preparation Example 23243640-3500 Preparation Example 24334-3500 Preparation Example 25424-3500 Preparation Example 26514-3500 Preparation Example 2742-43500 Preparation Example 2842-41000

Claims

A first polyol having a number average molecular weight (Mn) greater than 1.1,800 g / mol is included in an amount of 20% to 45% based on the total area of ​​the composition, A second polyol having a number average molecular weight (Mn) of 430 g / mol to 1,800 g / mol is included in an amount of 2% to 18% based on the total area of ​​the composition, A depolymerized polyol composition comprising a polyol having a number average molecular weight (Mn) of less than 430 g / mol as the residual component.

2. In Paragraph 1, The above depolymerization polyol composition further comprises a third polyol having a number average molecular weight (Mn) of 320 g / mol to 430 g / mol in an amount of 3% to 15% based on the total area of ​​the composition.

3. In Paragraph 1, The above depolymerization polyol composition further comprises a fourth polyol having a number average molecular weight (Mn) of 210 g / mol to 320 g / mol in an amount of 0.1% to 10% based on the total area of ​​the composition.

4. In Paragraph 1, The above depolymerization polyol composition further comprises a fifth polyol having a number average molecular weight (Mn) of 100 g / mol to 210 g / mol in an amount of 10% to 30% based on the total area of ​​the composition.

5. In Paragraph 1, The above depolymerization polyol composition further comprises a sixth polyol having a number average molecular weight (Mn) of less than 100 g / mol in an amount of 5% to 30% based on the total area of ​​the composition. A seventh polyol with an alkylene oxide added having a number average molecular weight (Mn) of 6.3,000 g / mol to 10,000 g / mol is included in an amount of 1% to 20% based on the total area of ​​the composition, The composition comprises an alkylene oxide-added eighth polyol having a number average molecular weight (Mn) of 100 g / mol to 3,000 g / mol, in an amount of 60% to 95% based on the total area of ​​the composition, An alkylene oxide addition polymerization polyol composition comprising a polyol having a number average molecular weight (Mn) of less than 100 g / mol as the remaining component.

7. A step of preparing a crushed material containing waste polyurethane; and The method includes the step of mixing the above-mentioned pulverized material and polyhydric alcohol and heat-treating to form a regenerated polyol, A method for preparing a depolymerized polyol composition, wherein the above-mentioned regenerated polyol comprises a first polyol having a number average molecular weight (Mn) greater than 1,800 g / mol in an amount of 20% to 45% based on the total area of ​​the composition, a second polyol having a number average molecular weight of 430 g / mol to 1,800 g / mol in an amount of 2% to 18% based on the total area of ​​the composition, and the remaining component comprises a polyol having a number average molecular weight (Mn) less than 430 g / mol.

8. In Paragraph 7, A method for preparing a depolymerized polyol composition, wherein the above heat treatment is performed at 100°C to 400°C.

9. In Paragraph 7, A method for preparing a depolymerized polyol composition in which the above polyhydric alcohol is one or more selected from the group consisting of ethylene glycol, tripropylene glycol, diethylene glycol, thiodiethylene glycol, neopentyl glycol, triethylene glycol, tetraethylene glycol, dipropylene glycol, tripropylene glycol, and pentaerythritol.

10. In Paragraph 7, In the step of forming the above-mentioned regenerated polyol, a first catalyst is used, and A method for preparing a depolymerized polyol composition in which the first catalyst is one or more selected from the group consisting of potassium hydroxide, sodium hydroxide, potassium acetate, zinc acetate, a mixture of sodium acetate and strontium acetate, and a mixture of potassium acetate and strontium acetate.

11. A step of preparing a crushed material containing waste polyurethane; A step of mixing the above-mentioned pulverized material and polyhydric alcohol and heat-treating to form a regenerated polyol; and The method includes the step of reacting an alkylene oxide with the above-mentioned regenerated polyol to form an addition polymerized polyol, and A method for preparing an alkylene oxide addition polymerization polyol composition comprising: the addition polymerization polyol having a number average molecular weight of 3,000 g / mol to 10,000 g / mol; a seventh polyol with an alkylene oxide added having a number average molecular weight (Mn) of 100 g / mol to 3,000 g / mol, comprising a seventh polyol with an alkylene oxide added having a number average molecular weight (Mn) of 60% to 95% based on the total area of ​​the composition; and the remaining component comprising a polyol having a number average molecular weight (Mn) of less than 100 g / mol.

12. In Paragraph 11, A method for preparing an alkylene oxide addition polymerization polyol composition in which the above alkylene oxide is one or more selected from the group consisting of ethylene oxide, propylene oxide, butylene oxide, pentene oxide, hexene oxide, cyclopentene oxide, and cyclohexane oxide.

13. In Paragraph 11, A method for preparing an alkylene oxide addition polymerization polyol composition, wherein the step of forming the above addition polymerization polyol is performed at 100°C to 400°C.

14. In Paragraph 11, In the step of forming the above addition polymerization polyol, a second catalyst is used, and A method for preparing an alkylene oxide addition polymerization polyol composition in which the second catalyst is one or more selected from the group consisting of phosphazene, potassium hydroxide, sodium hydroxide, cesium hydroxide, imidazole-based catalysts, and dicyanide metal catalysts. The composition comprises a polyol of the fourth type having a number average molecular weight (Mn) of 15.700 g / mol to 2,500 g / mol in an amount of 7% to 20% based on the total composition, The composition comprises a 15th polyol having a number average molecular weight (Mn) of less than 100 g / mol in an amount of less than 5% based on the total composition, A depolymerized polyol composition comprising a polyol having a number average molecular weight (Mn) of 100 g / mol or more and less than 700 g / mol and a polyol having a number average molecular weight (Mn) of more than 2,500 g / mol.

16. In Paragraph 15, The above depolymerization polyol composition further comprises a 16th polyol having a number average molecular weight (Mn) of greater than 2,500 g / mol in an amount of 10% to 40% based on the total composition.

17. In Paragraph 15, The above depolymerization polyol composition further comprises a polyol of the 17th having a number average molecular weight (Mn) of 100 g / mol to 250 g / mol in an amount of 30% to 50% based on the total composition.

18. In Paragraph 15, The above depolymerization polyol composition further comprises a polyol of the 18th having a number average molecular weight (Mn) of 250 g / mol to 700 g / mol in an amount of 10% to 30% based on the total composition.