Conductive particles, conductive material, and connection structure
By employing a core with a Ni, P, and B conductive layer and a 15 nm or less gold layer, the conductive particles address the stability and reliability issues in ACFs, enhancing electrical connections in COG and COP applications.
Patent Information
- Application Number
- PCT/KR2026/097005
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-15
- Filing Date
- 2026-05-14
- Publication Date
- 2026-11-19
AI Technical Summary
Conventional conductive particles used in anisotropic conductive films (ACFs) face challenges in maintaining stable electrical connections with high reliability at fine-pitch spacings due to high contact resistance and low compressive strength, particularly in applications like Chip On Glass (COG) and Chip On Plastic (COP), where gold-coated particles with large grain sizes exacerbate these issues.
The conductive particles are designed with a core composed of a divinylbenzene-based monomer, a styrene-based monomer, and a silicon-based monomer, featuring a conductive layer of Ni, P, and B, with a gold conductive layer limited to a grain size of 15 nm or less, optimized to enhance compressive strength and reduce contact resistance.
This design significantly improves the reliability and durability of electrical connections in fine-pitch environments by minimizing contact resistance and increasing compressive strength, ensuring long-term stability and performance in display packaging technologies.
Smart Images

Figure KR2026097005_19112026_PF_FP_ABST
Abstract
Description
Conductive particles, conductive materials, and connection structures
[0001] The present invention relates to a conductive particle comprising a core and a conductive layer, an anisotropic conductive material using the same, and a connection structure.
[0002] Anisotropic Conductive Film (ACF) is a key technology that enables fine-pitch connections for electronic components and is a widely used material, particularly in display packaging such as Chip on Glass (COG) and Chip on Plastic (COP). ACF consists of an epoxy-based adhesive and metal-coated conductive particles, which serve to form electrical connections between the gold bumps of the IC and the ITO pads of the substrate. Due to the properties of the adhesive, this connection provides stable electrical connectivity while preventing short circuits between the conductive particles.
[0003] The conductive particles used in ACFs generally consist of metal-coated polymer particles or metal particles. Among these, polymer particles coated with Ni and Au provide high conductivity and low contact resistance, and their high compressive strength allows them to maintain stability even in fine-pitch connections. In particular, gold (Au) coatings offer moisture resistance and high-temperature stability, and electrical properties are maximized when the coating thickness and grain size are optimized. The size and distribution density of the conductive particles directly affect contact resistance and compressive strength; consequently, smaller grain sizes allow for lower contact resistance and higher reliability.
[0004] Modern ACF technology demands stable connections at increasingly smaller pitch spacings, and to meet this need, arrangement and fixation technologies for conductive particles are continuously being developed. Designing the system to prevent particle movement to reduce the risk of short circuits and improve connection performance is considered a critical challenge. Furthermore, active research is being conducted to lower contact resistance through the deformation of conductive particles and the optimization of contact areas.
[0005] To meet these technical requirements, the present invention proposes a conductive particle comprising a core, a conductive layer containing Ni, P, and B disposed on the core, and a gold conductive layer containing Au on the conductive layer, wherein the grain size of the gold conductive layer is designed to be within a specific range. Such a structure can significantly improve the compressive strength of the conductive particle and minimize contact resistance, thereby maximizing reliability in fine-pitch connections.
[0006] The present invention aims to improve the connection reliability of conductive particles in display packaging technologies, such as Chip On Glass (COG) and Chip On Plastic (COP), which require fine-pitch connections. Conventional conductive particles have problems such as reduced electrical connection stability due to high contact resistance or low compressive strength. In particular, in the case of gold (Au) coated conductive particles, a large grain size reduces the contact area, which consequently increases contact resistance and can negatively affect long-term reliability. Therefore, the present invention aims to provide stable and highly reliable electrical connections even in fine-pitch environments by limiting the grain size of the gold conductive layer to a certain level or lower, thereby reducing contact resistance and improving compressive strength.
[0007] The conductive particle of the present invention comprises a core; a conductive layer comprising Ni, P, and B disposed on the core; and a gold conductive layer comprising Au on the conductive layer; and preferably, the surface grain size of the gold conductive layer is 15 nm or less.
[0008] It is preferable that the above conductive layer further includes Pd.
[0009] The conductive layer preferably comprises a first conductive layer comprising Ni and P; and a second conductive layer comprising Ni and B formed on the first conductive layer.
[0010] It is preferable that the above core comprises a monomer composed of a divinylbenzene-based monomer; a styrene-based monomer; an acrylate-based monomer; a silicon-based monomer; and a combination thereof.
[0011] It is more preferable that the above styrene-based monomer comprises a monomer consisting of styrene; alpha-methylstyrene (α-Methylstyrene); beta-methylstyrene (β-Methylstyrene); para-methylstyrene (p-Methylstyrene); ethylstyrene; hydroxystyrene; vinylxylene; monochlorostyrene; dichlorostyrene; dibromostyrene; vinylnaphthalene; or a combination thereof.
[0012] The above acrylate-based monomers are methyl methacrylate (MMA); ethyl methacrylate; propyl methacrylate; butyl methacrylate; benzyl methacrylate; methyl acrylate (MA); ethyl acrylate (EA); propyl acrylate; butyl acrylate; 2-ethylhexyl acrylate; 1,6-hexanediol diacrylate; tetramethylol methane tetraacrylate; ethylene glycol diacrylate; It is more preferable to include monomers composed of ethylene glycol dimethacrylate; propylene glycol diacrylate; trimethylolpropane triacrylate; ethylene glycol dimethacrylate; pentaerythritol tetramethacrylate; or a combination thereof.
[0013] The above silicon-based monomers are vinyltrimethoxysilane; methylchlorosilane; mercaptopropyltrimethoxysilane; vinyltriethoxysilane; phenylchlorosilane; aminopropyltriethoxysilane; epoxycyclohexylethyltrimethoxysilane; [3-(methacryloyloxy)propyl]trimethoxysilane; tetramethoxysilane (TMOS); tetraethoxysilane (TEOS); and triethoxyvinylsilane. It is more preferable to include monomers composed of trimethylchlorosilane (TMCS); hexamethyldisilazane (HMDS); octamethylcyclotetrasiloxane (D4); decamethylcyclopentasiloxane (D5); polymethylphenylsiloxane; polydiphenylsiloxane; tris(trimethylsiloxy)silane; or a combination thereof.
[0014] In another aspect of the present invention, the conductive particles are preferably composed of an anisotropic conductive material.
[0015] In another aspect of the present invention, the anisotropic conductive material is preferably composed of a connection structure.
[0016] The above connection structure is preferably a COG (Chip On Glass) or COP (Chip On Plastic).
[0017] The present invention provides the effect of significantly improving reliability in fine-pitch connections by optimizing the structure and characteristics of conductive particles. In particular, by limiting the crystal grain size of the gold conductive layer to 15 nm or less, contact resistance is minimized, and the compressive strength of the conductive particles is increased, thereby maximizing the stability of the electrical connection. This design maintains high conductivity and low contact resistance even in fine-pitch environments, while simultaneously ensuring long-term reliability and durability. Consequently, the present invention contributes to realizing high-performance and high-reliability electrical connections required in display packaging technologies such as COG and COP.
[0018] Figure 1 shows reference materials (Ni (No. 98-067-1092) and Au (No. 98-061-1625) for using X-ray wavelengths as a light source in Panalytical BV’s X-ray diffraction equipment.
[0019] Figure 2 schematically illustrates the XRD measurement results of Example 5 measured based on the above reference materials.
[0020] FIG. 3 is a TEM (transmission electron microscope) image showing the thickness of the gold conductive layer after processing the cross-section of the conductive particle according to Example 11 of the present invention.
[0021] The conductive particle of the present invention comprises a core; a conductive layer comprising Ni, P, and B disposed on the core; and a gold conductive layer comprising Au on the conductive layer; and preferably, the surface grain size of the gold conductive layer is 15 nm or less.
[0022] Hereinafter, some embodiments of the present invention will be described in detail with reference to the exemplary drawings. In assigning reference numerals to the components of each drawing, the same components may have the same reference numeral as much as possible, even if they are shown in different drawings.
[0023] In describing the present invention, if it is determined that a detailed description of related known configurations or functions may obscure the essence of the invention, such detailed description may be omitted. Where terms such as "comprising," "having," or "consisting of" are used in this specification, other parts may be added unless "only" is used. Where a component is expressed in the singular, it may include a plural unless otherwise explicitly stated.
[0024] Additionally, terms such as first, second, A, B, (a), (b), etc., may be used when describing the components of the present invention. These terms are used merely to distinguish the components from other components, and the essence, order, sequence, or number of the components are not limited by such terms.
[0025] In describing the positional relationship of components, where it is stated that two or more components are "connected," "combined," or "joined," it should be understood that while the two or more components may be directly "connected," "combined," or "joined," they may also be "connected," "combined," or "joined" with other components "intervened." Here, the other components may be included in one or more of the two or more components that are "connected," "combined," or "joined" with one another.
[0026] Furthermore, when it is stated that a component, such as a layer, membrane, region, or plate, is "on" or "on" another component, it should be understood that this includes not only the case where it is "directly on" another component, but also the case where there is another component in between. Conversely, when it is stated that a component is "directly on" another part, it should be understood that this means there is no other part in between.
[0027] In describing the temporal flow relationship regarding components, methods of operation, or methods of production, for example, when the temporal or sequential relationship is described using "after," "following," "next," or "before," it may include cases where the relationship is not continuous unless "immediately" or "directly" is used.
[0028] Meanwhile, where numerical values or corresponding information regarding a component are mentioned, even without separate explicit notation, the numerical values or corresponding information may be interpreted as including a margin of error that may occur due to various factors (e.g., process factors, internal or external shock, noise, etc.).
[0029] The terms used in this specification and the appended claims are as follows, to the extent that they do not deviate from the spirit of the invention, unless otherwise stated.
[0030] Hereinafter, embodiments of the present invention will be described in detail. However, these are presented as examples and are not intended to limit the present invention, and the present invention is defined only by the scope of the claims set forth below.
[0031] Each component is explained in detail below.
[0032] 1. Conductive particles
[0033] The conductive particles according to the embodiments of the present invention are utilized as anisotropic conductive materials and are applied to COG (Chip On Glass) and COP (Chip On Plastic) substrates to simultaneously provide electrical connection and insulation.
[0034] The conductive particles may be composed of metals or metal alloys such as silver, copper, nickel, and gold, and may also include forms in which metal plating is applied to polymer particles. The particle sizes vary from hundreds of nanometers to tens of micrometers and may have a uniform or non-uniform size distribution. The conductive particles of the present invention provide electrical conductivity in the vertical direction and maintain insulation in the horizontal direction, thereby preventing short circuits between fine-pitch electrodes. This is suitable for high-resolution displays and miniaturized electronic devices.
[0035] In particular, the COG method enables the fabrication of miniaturized electronic devices by directly connecting the glass substrate of the display panel and the driving IC, and forms a stable electrical connection between the upper and lower electrodes through a thermal compression process. The COP method is applied in a similar manner to plastic substrates and plays an important role, especially in applications such as flexible displays.
[0036] Consequently, the conductive particles according to the embodiments of the present invention enable high-density and high-reliability electrical connections on COG and COP substrates, which is considered a significant innovative element in display technology and the manufacture of other electronic devices.
[0037] A conductive particle according to an embodiment of the present invention comprises: a core; a conductive layer comprising Ni, P, and B disposed on the core; and a gold conductive layer comprising Au on the conductive layer; wherein the crystal grain size of the gold conductive layer is 15 nm or less.
[0038] 1-1. Core
[0039] The core is an insulating particle with very low electrical conductivity and can be manufactured from resin microparticles; it is applied to anisotropic conductive materials and is produced as a material that does not easily break when the conductive particles are electrically connected.
[0040] It is preferable that the particle size of the above core be 1.0 μm to 6.0 μm.
[0041] The core according to an embodiment of the present invention is preferably a copolymer composed of a divinylbenzene-based monomer; a styrene-based monomer; an acrylate-based monomer; a silicon-based monomer; or a combination thereof.
[0042] The above-mentioned divinylbenzene copolymer is mainly prepared by a copolymerization reaction using divinylbenzene monomers and styrene monomers, and in this process, divinylbenzene acts as a crosslinking agent to control the physical and chemical properties of the polymer.
[0043] The above styrene-based monomer may be one or more selected from the group consisting of styrene; alpha-methylstyrene (α-Methylstyrene); beta-methylstyrene (β-Methylstyrene); para-methylstyrene (p-Methylstyrene); ethylstyrene; hydroxystyrene; vinylxylene; monochlorostyrene; dichlorostyrene; dibromostyrene; and vinylnaphthalene.
[0044] The above acrylate-based monomers are methyl methacrylate (MMA); ethyl methacrylate; propyl methacrylate; butyl methacrylate; benzyl methacrylate; methyl acrylate (MA); ethyl acrylate (EA); propyl acrylate; butyl acrylate; 2-ethylhexyl acrylate; 1,6-hexanediol diacrylate; tetramethylol methane tetraacrylate; ethylene glycol diacrylate; One or more selected from the group consisting of ethylene glycol dimethacrylate; propylene glycol diacrylate; trimethylolpropane triacrylate; ethylene glycol dimethacrylate; and pentaerythritol tetramethacrylate may be used.
[0045] The above silicon-based monomers are vinyltrimethoxysilane; methylchlorosilane; mercaptopropyltrimethoxysilane; vinyltriethoxysilane; phenylchlorosilane; aminopropyltriethoxysilane; epoxycyclohexylethyltrimethoxysilane; [3-(methacryloyloxy)propyl]trimethoxysilane; tetramethoxysilane (TMOS); tetraethoxysilane (TEOS); and triethoxyvinylsilane. One or more selected from the group consisting of trimethylchlorosilane (TMCS); hexamethyldisilazane (HMDS); octamethylcyclotetrasiloxane (D4); decamethylcyclopentasiloxane (D5); polymethylphenylsiloxane; polydiphenylsiloxane; and tris(trimethylsiloxy)silane may be used.
[0046] 1-2. Challenge Layer
[0047] The conductive layer of the present invention comprises a Ni conductive layer comprising Ni, P, and B; and a gold conductive layer comprising Au on the conductive layer; and preferably, the surface grain size of the gold conductive layer is 15 nm or less.
[0048] In addition, the conductive layer of the present invention preferably includes Ni, P, and B, and more preferably includes Pd.
[0049] Specifically, the above Ni conductive layer may be composed of three elements including Ni, Ni-PB, or four elements including Ni-PB-Pd, but is not limited thereto.
[0050] It is preferable that the above Ni conductive layer comprises a first conductive layer comprising Ni and P and a second conductive layer comprising Ni and B formed on the first conductive layer.
[0051] The thickness of the above Ni conductive layer is preferably 80 nm to 400 nm, more preferably 90 nm to 300 nm, and most preferably 100 nm to 250 nm.
[0052] If the thickness of the conductive layer is less than the above range, the electrical resistance of the conductive particles increases, and if it exceeds the above range, delamination between the conductive layer and the insulating bead may occur even if the conductive particles are minimally deformed under the heating / pressure bonding conditions of the anisotropic conductive material, which may reduce the reliability of the product.
[0053] The grain size of the gold conductive layer is preferably 15 nm or less, preferably 1 nm to 15 nm, preferably 3 nm to 15 nm, and more preferably 5 nm to 15 nm.
[0054] As in the present invention, the critical significance of the grain size of the gold layer is very important in that it can simultaneously improve the electrical, mechanical, and thermal properties of the metal layer. When the grain size is reduced, the density of the grain boundaries increases, leading to improved strength and the formation of a uniform strength distribution. In particular, the refined grain structure of the gold conductive layer within the above range maintains a uniform contact area between particles, thereby reducing powder resistance, which plays a key role in providing stable electrical connections in fine-pitch bonding technology for highly integrated electronic devices.
[0055] In addition, refining the grain size alleviates stress concentration within the metal layer, thereby suppressing cracking or delamination even in environments of thermal and mechanical stress. This structural stability ensures the reliability of the metal layer even during long-term use and enables superior durability and performance compared to existing technologies. Therefore, setting the grain size to 15 nm or less serves as an optimal condition for simultaneously securing low powder resistance and high reliability, and can make a significant technological contribution to the manufacturing process of next-generation high-performance electronic devices.
[0056] The thickness of the gold conductive layer is preferably 1 nm to 30 nm, preferably 5 nm to 30 nm, and more preferably 10 nm to 30 nm.
[0057] In this invention, limiting the thickness of the gold conductive layer to within the aforementioned range is an optimized design for reducing contact resistance and ensuring resistance stability. This range contributes to maximizing electrical performance by maintaining a fine crystal grain structure and a uniform surface of the conductive particles. In particular, a thickness exceeding this range provides a sufficient conduction path to facilitate current flow and enhances resistance to metal oxidation and thermal stress. Conversely, if the thickness exceeds this range, the crystal grain size increases, leading to increased surface roughness and a reduced contact area, which may result in increased contact resistance. Furthermore, excessive thickness can reduce the flexibility of the metal, thereby compromising long-term reliability and thermal stability.
[0058] It is preferable that the conductive layer of the present invention includes a protrusion layer on the conductive layer.
[0059] The shape of the above-mentioned protrusion may be spherical; elongated; or a cluster of multiple particles, but is not limited thereto. The most preferred shape is one that narrows toward the ends.
[0060] The size of the above protrusion layer is preferably 50 nm to 500 nm, preferably 100 nm to 350 nm.
[0061] The above-mentioned protrusion layer includes a first protrusion portion having a protrusion on the protrusion; and a second protrusion portion not having a protrusion on the protrusion.
[0062] It is preferable that the ratio of the number of the first protrusions is 1% to 30% of the sum of the number of the first protrusions and the number of the second protrusions.
[0063] The above range has the advantage of providing reliability and efficiency in ultra-fine pitch connections. When the first protrusion is 1% or more, a sufficient contact area with the electrode is secured, which lowers contact resistance and enables a stable electrical connection. In addition, by ensuring that the ratio of the first protrusion does not exceed 30%, excessive clumping of conductive particles or short circuits is prevented, thereby maintaining insulation characteristics. Setting this range is effective in simultaneously ensuring connection reliability and electrical stability.
[0064] If it is less than 1%, the first protrusion is insufficient, which reduces the contact area with the electrode, and consequently, there is a possibility that contact resistance will increase or connection reliability will decrease. Conversely, if it exceeds 30%, the protrusion becomes excessive, which may cause interference between conductive particles, increasing the risk of short circuits and making it difficult to achieve uniform dispersion during the manufacturing process.
[0065] It is preferable that the above protrusion layer does not contain P.
[0066] It is desirable to apply an anti-corrosion treatment to the outer surface of the aforementioned conductive layer. Applying this treatment increases the contact angle between the surface of the conductive layer and moisture, thereby enhancing reliability in high-humidity environments. Additionally, it has the effect of minimizing performance degradation of the connecting components by preventing impurities from dissolving in water. Therefore, hydrophobic anti-corrosion agents are generally used. Methods for applying the anti-corrosion coating to the surface of the conductive layer include dissolving the anti-corrosion agent in a solvent and then immersing or spraying it onto the surface of the conductive particles. Furthermore, a hydrophilic treatment is also possible to ensure compatibility with the characteristics of the ACF resin.
[0067] 1-3. Insulating microparticle layer
[0068] Insulating microparticles are particles formed in a first region on a conductive layer to prevent short circuits with adjacent electrodes when conductive particles are used as an anisotropic conductive material, and may also be provided on the protrusions if protrusions are provided.
[0069] Insulating resin particles or inorganic particles may be used as the material for insulating microparticles. The resin particles include at least one or more resins selected from the group consisting of styrene or styrene-based materials containing alkyl groups having 1 or more carbon atoms, acrylates or methacrylates containing alkyl groups having 1 or more carbon atoms, and acrylate-based materials having diacrylate or dimethacrylate at both ends of glycols having 1 or more carbon atoms, and the inorganic particles include one or two or more materials selected from the group consisting of trimethoxysilane-based materials containing acrylic groups, phenyl groups, and vinyl groups.
[0070] The particle size can be 90 nm or larger to provide an insulating effect, but 100 nm to 300 nm is preferred to ensure contact resistance and insulation resistance, and more preferably 100 nm to 250 nm.
[0071] In addition, to improve insulation and conductivity effects, insulating microparticles of different particle sizes may be mixed and used, or organic and inorganic particles may be mixed and used.
[0072] A wet method is used to attach insulating microparticles to the surface of conductive particles by mixing the solvent, conductive particles, and insulating microparticles together. The insulating microparticles are polymers having first substituents on their surface that have a bonding force with the metal of the conductive layer of the conductive particles, and are attached to the conductive layer or protrusions of the insulating microparticles by means of the first substituents.
[0073] The first substituent is any heteroelement or substituent that has a bonding force such as a covalent bond or a polar bond with respect to the metal, or has a high affinity for the metal and can be attached and fixed to the metal surface, specifically selected from the group consisting of a hetero group, an ether group, a carbonate group, and a hydroxyl group, and preferably at least one selected from the group consisting of sulfur, phosphorus, nitrogen, and oxygen can be used as the heterogroup.
[0074] At this time, it is preferable that the insulating microparticles be attached to 5% to 40% of the total surface area of the outer surface of the conductive layer (including protrusions if any). If less than 5%, the proportion of insulating particles is low, making it difficult to achieve an insulating effect, and if more than 40%, a problem arises in which the contact resistance increases as the number of insulating microparticles increases. Therefore, even if insulating microparticles are attached, a portion of the surface of the conductive layer of the conductive particles remains open.
[0075] It is preferable that the average diameter of the above conductive particles is 1.5 μm to 5.0 μm.
[0076] The average diameter of the above conductive particles is determined using the mode value measured with a Particle Size Analyzer (BECKMAN MULTISIZER TM3). The number of conductive particles measured is 75,000.
[0077] 2. Method for manufacturing conductive particles
[0078] A method for manufacturing conductive particles according to an embodiment of the present invention includes a step of providing an insulating bead (core) (S1), a step of forming a conductive layer (S2), a surface treatment step (S3), and a drying step (S4).
[0079] At this time, the insulating bead providing step (S1) includes an insulating bead particle synthesis step (S1a) and a plating catalyst activation step (S1b).
[0080] First, in the insulating bead particle synthesis step (S1a), insulating beads are manufactured by using monomers such as divinylbenzene, styrene-based, acrylate-based, and silicon-based monomers, or monomers mixed with the above monomers, to produce a copolymer by polymerizing via seed polymerization, dispersion polymerization, suspension polymerization, emulsion polymerization, etc.
[0081] The above styrene-based monomer may be one or more selected from the group consisting of styrene; alpha-methylstyrene (α-Methylstyrene); beta-methylstyrene (β-Methylstyrene); para-methylstyrene (p-Methylstyrene); ethylstyrene; hydroxystyrene; vinylxylene; monochlorostyrene; dichlorostyrene; dibromostyrene; and vinylnaphthalene.
[0082] The above acrylate-based monomers are methyl methacrylate (MMA); ethyl methacrylate; propyl methacrylate; butyl methacrylate; benzyl methacrylate; methyl acrylate (MA); ethyl acrylate (EA); propyl acrylate; butyl acrylate; 2-ethylhexyl acrylate; 1,6-hexanediol diacrylate; tetramethylol methane tetraacrylate; ethylene glycol diacrylate; One or more selected from the group consisting of ethylene glycol dimethacrylate; propylene glycol diacrylate; trimethylolpropane triacrylate; ethylene glycol dimethacrylate; and pentaerythritol tetramethacrylate may be used.
[0083] The above silicon-based monomers are vinyltrimethoxysilane; methylchlorosilane; mercaptopropyltrimethoxysilane; vinyltriethoxysilane; phenylchlorosilane; aminopropyltriethoxysilane; epoxycyclohexylethyltrimethoxysilane; [3-(methacryloyloxy)propyl]trimethoxysilane; tetramethoxysilane (TMOS); tetraethoxysilane (TEOS); triethoxyvinylsilane; One or more selected from the group consisting of trimethylchlorosilane (TMCS); hexamethyldisilazane (HMDS); octamethylcyclotetrasiloxane (D4); decamethylcyclopentasiloxane (D5); polymethylphenylsiloxane; polydiphenylsiloxane; and tris(trimethylsiloxy)silane may be used.
[0084] After the above-mentioned core formation, the core particles are finally obtained through filtration, washing, classification, and drying processes.
[0085] The core particles generated in the above process may have various average diameter distributions, and can be separated into core particles having a specific average diameter through the classification process.
[0086] It is preferable that the particle size of the core particle is 1.0 μm to 6.0 μm.
[0087] Next, in the plating catalyst activation step (S1b), the core particles prepared in the previous step S1a are activated as an electroless plating catalyst. At this time, the plating catalyst used in the plating catalyst activation step (S1b) may be replaced by attaching small metal or inorganic particles to insulating microparticles, provided that the same effect can be provided.
[0088] Specifically, the plating catalyst activation step (S1b) involves pre-treating the core particles using various known methods for sensitizing the electroless plating catalyst after surfactant treatment, then introducing the sensitized insulating bead particles into a solution containing a precursor of the electroless metal plating catalyst, and performing an activation treatment.
[0089] The particles activated in this manner are placed in a solution containing a strong acid and stirred at room temperature to perform accelerated treatment, thereby obtaining catalyst-treated insulating bead particles for electroless plating.
[0090] Next, the conductive layer formation step (S2) includes an insulating bead dispersion step (S2a) and a conductive layer formation step (S2b).
[0091] In the insulating bead dispersion step (S2a), insulating beads are introduced into and dispersed in the alloy plating solution to form the conductive layer. The alloy plating solution is prepared by sequentially dissolving a precursor of an alloy element, a complexing agent, a stabilizer, and a surfactant.
[0092] The catalyst-treated insulating bead particles obtained in step (S1b) above are introduced into the prepared plating solution, and dispersion treatment is performed using an ultrasonic homogenizer.
[0093] It is desirable to adjust the pH of the dispersion treatment solution to 5.5 to 6.5 using ammonia water, etc., so that the adhesion and dispersibility between the insulating bead and the conductive layer can be improved during the initial Ni reduction reaction in the conductive layer formation step (S2b) described later. If the pH is less than 5.5, for example, pH 4 or lower, the adhesion and dispersibility are good, but the reactivity is too low, so there is a possibility that some particles will not be plated, and if the pH is higher than 6.5, the surface of the conductive layer may be formed loosely due to abnormal precipitation of Ni, and the adhesion and dispersibility may be poor.
[0094] Next, a process (S2b) is performed to form a conductive layer on an insulating bead immersed in a dispersed plating solution. The number of layers, material, method of formation of the conductive layer, or method of formation of the protrusions are not limited. It is preferable that the thickness of the conductive layer be formed to be 80 nm to 400 nm, and the protrusions may be formed integrally or separately. For example, the protrusions may be formed by growing integrally with the conductive layer, by forming a conductive layer after attaching nano-sized particles to the insulating bead, or by forming a first conductive layer on the insulating bead, attaching nano-sized particles, and forming a second conductive layer of the same or different material as the first conductive layer.
[0095] For example, the protrusions can be formed integrally with the conductive layer by introducing a boron precursor into the nickel-based alloy plating solution in the insulating bead dispersion step (S2a), and by introducing an alloy element containing a precursor of one or more elements selected from Cu, Au, Ag, W, Mo, Pd, Co, and Pt into the dispersion-treated plating solution in the step of forming the protruding conductive layer (S2b) to form a protruding conductive layer with a concentration gradient.
[0096] At this time, the alloying elements to be divided and added can be added in 2 to 5 portions at intervals of 10 to 30 minutes, or in 2 to 4 portions at intervals of 15 to 25 minutes. At this time, the amount added can be divided and added with increased content, or added continuously if necessary, but it is desirable to increase the amount added according to the adding speed at regular intervals so that the concentration can be increased towards the direction of the protrusion.
[0097] Before and after the aforementioned split addition, it is desirable to maintain the pH of the plating solution within a controlled range depending on the type of alloying element added to form a protruding conductive layer. For example, when adding precursor B, it is desirable to maintain the pH within the range of 8.5 to 9.0. In this case, if the pH of the plating solution is low, reactivity is low, causing problems with protrusion formation; conversely, if the pH is too high, abnormal precipitation occurs excessively, disrupting the balance of the plating solution and resulting in defective plating.
[0098] In addition, applying temperature-raising conditions is more desirable because it prevents excessive abnormal precipitation during the protrusion formation mechanism, thereby enabling the formation of desired protrusions.
[0099] It is preferable that the above protrusion layer does not contain P.
[0100] The shape of the above-mentioned protrusion may be spherical; elongated; or a cluster of multiple particles, but is not limited thereto. The most preferred shape is one that narrows toward the ends.
[0101] The size of the above protrusion layer is preferably 50 nm to 500 nm, preferably 100 nm to 350 nm.
[0102] The above-mentioned protrusion layer includes a first protrusion portion having a protrusion on the protrusion; and a second protrusion portion not having a protrusion on the protrusion.
[0103] It is preferable that the ratio of the number of the first protrusions is 1% to 30% of the sum of the number of the first protrusions and the number of the second protrusions.
[0104] The above range has the advantage of providing reliability and efficiency in ultra-fine pitch connections. When the first protrusion is 1% or more, a sufficient contact area with the electrode is secured, which lowers contact resistance and enables a stable electrical connection. In addition, by ensuring that the ratio of the first protrusion does not exceed 30%, excessive clumping of conductive particles or short circuits is prevented, thereby maintaining insulation characteristics. Setting this range is effective in simultaneously ensuring connection reliability and electrical stability.
[0105] The surface treatment step (S3) is a step of introducing a surface treatment layer to the surface of the conductive particles.
[0106] The above surface treatment step (S3) is preferably performed by a wet method.
[0107] The above surface treatment step (S3) may use a method of dissolving a surface treatment material in a solvent and then immersing or spraying it onto the surface of the conductive particle.
[0108] The wet method allows for the attachment of uniform particles, but subsequent drying of the conductive particles is required.
[0109] Performing the above surface treatment increases the contact angle when the conductive layer surface comes into contact with moisture, thereby enhancing reliability in high-humidity environments and reducing performance degradation of the connection member by allowing impurities to dissolve in water. Therefore, it is generally desirable to use a surface treatment material that is hydrophobic.
[0110] As a material for forming a surface treatment layer, a compound may be used that includes at least one substituent selected from the group consisting of thiol groups, phosphate groups, and phosphate ester groups, which are substituents capable of bonding with metals and having hydrophobic properties, and includes a hydrophobic hydrocarbon chain having three or more carbon atoms.
[0111] The above hydrophobic hydrocarbons having 3 or more carbon atoms may specifically use substances from the fatty acid series, alkyl groups, or phenol groups, and in this case, the substances are more specifically C6~C 60 alkyl group of, C6~C 60 cycloalkyl group of, C6~C 60 aryl group of, C7~C 60 arylalkyl group of, C3~C 60 It may be an alkyl ether group, or a substance containing two or more of the above substances in a chain.
[0112] The drying step (S4) is a step for drying the wet-manufactured conductive particles, and the drying process is carried out between 100°C and 200°C, although the drying temperature varies depending on the type of solvent.
[0113] The anisotropic conductive material of the present invention, composed of a mixture of conductive particles and insulating particles, is manufactured by mixing the conductive particles produced in steps (S1) to (S4) and the insulating particles that have been washed, classified, and dried in the insulating bead providing step (S1).
[0114] It is preferable that the above mixing process be carried out by a physical method. Specifically, it is preferable to perform the process using equipment such as a roll mill or an agitator.
[0115] It is preferable that the average diameter of the conductive particles is larger than that of the insulating particles.
[0116] It is preferable that the average diameter of the above conductive particles is 1.5 μm to 5.0 μm.
[0117] The average diameter of the above conductive particles is determined using the mode value measured with a Particle Size Analyzer (BECKMAN MULTISIZER TM3). At this time, it is preferable that the number of particles measured be 75,000.
[0118] 4. Anisotropic conductive materials
[0119] The conductive particles of the present invention can be composed of an anisotropic conductive material.
[0120] An anisotropic conductive material can be manufactured by dispersing the conductive particles of the present invention in a resin binder. Examples of anisotropic conductive materials include anisotropic conductive materials, anisotropic conductive materials (ACF), and anisotropic conductive sheets. After uniformly dispersing the conductive particles in a resin binder, the material can be used as an anisotropic conductive material or spread thinly on the surface of a release liner to be used as an anisotropic film.
[0121] The above anisotropic conductive film is preferably 2 to 10 times the size of the conductive particles used. The above anisotropic conductive film may be composed solely of a layer containing conductive particles, or it may be divided into a layer containing conductive particles (conductive layer) and a layer without them (insulating layer). The insulating layer may exist above and below the conductive layer, or only above and below. The presence of the insulating layer may vary depending on the application of the ACF used, or it may be used to prevent breakage during use when the thickness of the conductive layer is too thin.
[0122] At this time, the resin binder is not particularly limited. Examples include vinyl resins such as styrene-based, acrylic-based, and vinyl acetate-based resins, thermoplastic resins such as polyolefin-based and polyamide-based resins, and curable resins such as urethane-based and epoxy-based resins. The resin may be used alone or in combination of two or more types. In particular, it is preferable for the resin binder to include monomers of the same series as the aforementioned insulating beads, as this allows for similar behavior in varying temperature environments.
[0123] For the purpose of polymerization or curing of binder resins, radical initiators such as BPO (Benzoyl Peroxide) or photoinitiators such as TPO (Trimethylbenzoyl Phenylphosphinate), and epoxy-based latent curing agents such as HX3941HP can be used alone or in combination.
[0124] In addition, other substances may be added to the resin binder to the extent that they do not hinder the achievement of the objectives of the present invention. Examples include colorants, softeners, heat stabilizers, light stabilizers, antioxidants, inorganic particles, etc.
[0125] 5. Connection structure
[0126] In the present invention, when the aforementioned conductive particles are used, the use, structure, and material of the connection structure are not particularly limited. That is, the connection structure connects circuit boards using the conductive particles of the present invention or the anisotropic conductive material of the present invention.
[0127] The technology of configuring conductive particles as anisotropic conductive materials and applying them to connection structures is a key method for simultaneously addressing electrical connection and mechanical fixation in display panels. Here, the connection structure can be implemented, for example, via COG (Chip On Glass) and COP (Chip On Plastic) methods, enabling signal transmission between electrodes by attaching driver ICs to glass and plastic substrates, respectively. The anisotropic conductive material consists of conductive particles dispersed in a curable resin and possesses the characteristic of providing electrical conductivity in the compression direction while maintaining insulation in the vertical direction. This characteristic enables stable connections even between minute electrodes, thereby enhancing the reliability of the connection structure.
[0128] Conductive particles enhance electrical reliability and durability through surface treatment and deform under pressure and heat within the connection structure to form an electrical connection between the upper and lower electrodes. Simultaneously, as the resin cures, it provides mechanical stability, thereby improving the structural integrity of the connection structure. These conductive particles are compatible with various substrate materials and are designed to ensure high reliability in COG and COP type connection structures.
[0129] The COG connection structure directly connects driver ICs to a glass substrate and is designed to enable stable connections even at fine pitches. This is utilized as an essential technology in applications such as high-resolution displays. The COP connection structure attaches driver ICs to a flexible substrate for applications such as flexible displays and is designed to maintain reliability even in environments involving repeated bending.
[0130] The proper configuration of conductive particles significantly impacts the performance of the connection structure. Properly designed conductive particles reduce the risk of short circuits and ensure stable connections, while arrangement techniques enable the achievement of maximum efficiency with a minimum number of particles. Consequently, connection structures implemented using COG and COP methods provide high precision and reliability, playing a crucial role in next-generation display technology.
[0131] Hereinafter, specific synthetic examples and embodiments according to the present invention are described, but the synthetic examples and embodiments of the present invention are not limited thereto.
[0132] <Example>
[0133] I. Preparation of Core Particles
[0134] (Preparation Example 1)
[0135] 750 g of monomer TMPTA (Trimethylolpropane triacrylate), 750 g of DVB (Divinyl benzene), and 750 g of Styrene were placed in a 3 L glass beaker, and 50 g of initiator BPO was added and treated in a 40 kHz ultrasonic bath for 10 minutes to prepare the first solution.
[0136] A second solution was prepared by adding 500g of dispersion stabilizer PVP (Polyvinylpyrrolidone)-30K and 20g of surfactant Solusol (Dioctyl sulfosuccinate sodium salt) to 4,000g of deionized water in a 5L PP beaker and dissolving them.
[0137] The above first solution and second solution were placed in a 50L reactor, 40,000g of deionized water was added, and the solution was treated with an ultrasonic homogenizer (20kHz, 600W) for 90 minutes. The solution was then rotated at 120rpm, the temperature was raised to 35℃ and maintained for 3 hours, and then the temperature was raised again to 85℃. After the solution reached 85℃, the temperature was maintained for 16 hours to perform the polymerization process.
[0138] Core resin microparticles were obtained by subjecting polymerized microparticles to filtration, washing, classification, and drying processes. The average diameter of the core resin microparticles prepared above was determined using the mode value measured with a Particle Size Analyzer (BECKMAN MULTISIZER M4). The number of core microparticles measured at this time was 75,000. The average diameter was 2.8 μm.
[0139] (Preparation Example 2)
[0140] A dilute aqueous base solution (a) was prepared by adding 1.2g of 3% ammonia solution to 200g of deionized water, and a monomer mixed solution (b) was prepared by mixing 10g of VTMS (vinyltrimethoxysilane) and 10g of MPTMS (3-methacryloxypropyltrimethoxysilane). The monomer mixed solution (b) was added to the aqueous base solution (a) while stirring at low speed, and the core intermediate was synthesized by an overnight reaction at room temperature.
[0141] Afterward, 1.0 g of the organic monomer HDDA (hexandiol diacrylate) was added, the temperature was raised to 75°C, and an aqueous solution of 0.2 g of KPS dissolved in 5 g of deionized water was added, and the reaction was carried out for 10 hours.
[0142] After naturally settling the above reaction solution to remove the supernatant, 95% ethanol was added and small particles were removed by centrifugation at least 10 times.
[0143] The average diameter of the cores manufactured above was determined using the particle mode value with a Particle Size Analyzer (BECKMAN MULTISIZER M4), and the number of cores measured was 75,000. The average diameter of the cores was 2.8 μm.
[0144] II. Preparation of conductive particles including a conductive layer
[0145] (Preparation Example 3)
[0146] ① Catalytic Treatment Process
[0147] A cleaning and degreasing process was performed to remove excess unreacted monomers and oil components present in the core by placing 30g of the core of Preparation Example 1, prepared in Process I above, into a solution of 800g of deionized water and 1g of the surfactant Triton X100 and treating it in an ultrasonic bath for 1 hour. The final step of the cleaning and degreasing process was to perform a washing process three times using deionized water at 40℃. Pd catalyst treatment was applied to the core after the etching process was completed. After dissolving 150g of stannous chloride and 300g of 35-37% hydrochloric acid in 600g of deionized water, the core that had undergone the cleaning and degreasing treatment was placed in the solution and sensitized by immersion and stirring for 30 minutes at 30℃, followed by washing three times.
[0148] A sensitized core was immersed in 1 g of palladium chloride and 200 g of 35–37% hydrochloric acid in 600 g of deionized water and activated at 40°C for 1 hour. After activation, a washing process was performed three times.
[0149] The activated core was placed in a solution of 100g of 35–37% hydrochloric acid and 600g of deionized water and stirred at room temperature for 10 minutes for accelerated treatment. After the accelerated treatment, the core was washed three times to obtain a catalyst-treated core for electroless plating.
[0150] ② First conductive layer process containing Ni and P
[0151] Plating solution (a) was prepared by sequentially dissolving 300g of nickel sulfate as a Ni salt, 5g of sodium acetate and 2g of lactic acid as complexing agents, 0.001g of Pb-acetate and 0.001g of sodium thiosulfate as stabilizers, and 1g of PEG-1200, 1.5g of PEG-400, and 0.02g of Triton X100 as surfactants in 3500g of deionized water in a 5L reactor. The catalyst-treated core was placed into the prepared solution (a), and dispersion treatment was performed for 10 minutes using an ultrasonic homogenizer. After dispersion treatment, the pH of the solution was adjusted to 5.7 using ammonia water - solution (b)
[0152] Solution (c) was prepared by dissolving 500g of deionized water, 380g of sodium hypophosphite (a reducing agent), and 0.0001g of sodium thiosulfate (a stabilizer) in a 1L beaker.
[0153] While maintaining the temperature of the above 5L reactor (solution (b)) at 65℃, the solution (c) was added at a rate of 10g per minute using a metering pump, and the reactor temperature was heated and maintained to reach 75℃ in 30 minutes.
[0154] After the above solution (c) was added and maintained for 30 minutes, Ni-plated conductive particles were obtained.
[0155] ③ Second conductive layer process including Ni and B
[0156] Solution (a) was prepared by dissolving 300g of deionized water, 33g of DMAB (Dimethylamineborane) as a reducing agent, and 0.002g of sodium thiosulfate as a stabilizer in a 1L beaker.
[0157] Solution (b) was prepared by dissolving 500g of deionized water, 155g of nickel sulfate, 0.6g of PdCl2, and 10g of hydrochloric acid in a 1L beaker.
[0158] The temperature of the solution (c) in which the first conductive layer containing Ni and P was completed was cooled and maintained to reach 35°C.
[0159] Ammonia water was additionally added to the above 5L reactor solution (c) to adjust the pH to 8.0 until the solution temperature reached 35℃.
[0160] The above solutions (a) and (b) were introduced into the above 5L reactor at a rate of 20g per minute using a metering pump.
[0161] After the above solutions (a) and (b) were added, they were maintained for 30 minutes to obtain Ni-plated conductive particles.
[0162] (Preparation Example 4)
[0163] Conductive particles were prepared in the same manner as in Preparation Example 3, except that the core of Preparation Example 2 prepared in the above Process I was introduced.
[0164] III. Preparation of conductive particles containing a gold conductive layer
[0165] (Example 1)
[0166] To the conductive particles of Preparation Example 3 prepared in the above Step II, 2000g of distilled water (DI water), 130g of PEG#600 (polyethylene glycol 600), 42g of potassium hydroxide (KOH), 74g of citric acid, and 10g of potassium gold cyanide were added and stirred at 30℃ for 15 minutes to prepare the conductive particles of Example 1.
[0167] (Example 2)
[0168] To the conductive particles of Preparation Example 4 prepared in the above Step II, 2000g of distilled water (DI water), 130g of PEG#600 (polyethylene glycol 600), 42g of potassium hydroxide (KOH), 74g of citric acid, and 4g of potassium gold cyanide were added and stirred at 30℃ for 15 minutes to prepare the conductive particles of Example 2.
[0169] (Example 3)
[0170] Conductive particles of Example 3 were prepared using the same method as Example 1, except that the conductive particles of Preparation Example 3 prepared in the above II process were reacted at a temperature of 45°C.
[0171] (Example 4)
[0172] Conductive particles of Example 4 were prepared using the same method as Example 1, except that the conductive particles of Preparation Example 4 prepared in the above II process were reacted at a temperature of 45°C.
[0173] (Example 5)
[0174] Conductive particles of Example 5 were prepared using the same method as Example 1, except that the conductive particles of Preparation Example 3 prepared in the above II process were reacted at a temperature of 60°C.
[0175] (Example 6)
[0176] Conductive particles of Example 6 were prepared using the same method as Example 1, except that the conductive particles of Preparation Example 4 prepared in the above II process were reacted at a temperature of 60°C.
[0177] (Example 7)
[0178] Conductive particles of Example 7 were prepared using the same method as in Example 1, except that the conductive particles of Preparation Example 3 prepared in Process II above were reacted at a temperature of 75℃.
[0179] (Example 8)
[0180] Conductive particles of Example 8 were prepared using the same method as Example 1, except that the conductive particles of Preparation Example 4 prepared in the above II process were reacted at a temperature of 75°C.
[0181] (Example 9)
[0182] Conductive particles of Example 9 were prepared using the same method as Example 1, except that the conductive particles of Preparation Example 3 prepared in the above II process were reacted at a temperature of 90°C.
[0183] (Example 10)
[0184] Conductive particles of Example 10 were prepared using the same method as Example 1, except that the conductive particles of Preparation Example 4 prepared in the above II process were reacted at a temperature of 90°C.
[0185] (Example 11)
[0186] To the conductive particles of Preparation Example 3 prepared in the above Step II, 2000g of distilled water (DI water), 130g of PEG#600 (polyethylene glycol 600), 42g of potassium hydroxide (KOH), 74g of citric acid, and 10g of potassium gold cyanide were added and stirred at 60℃ for 5 minutes to prepare the conductive particles of Example 1.
[0187] (Example 12)
[0188] The conductive particles of Example 2 were prepared in the same manner as Example 11, except that Au plating was reacted for 10 minutes on the conductive particles of Preparation Example 3 prepared in Process II above.
[0189] (Example 13)
[0190] The conductive particles of Example 3 were prepared in the same manner as in Example 11, except that Au plating was reacted for 15 minutes on the conductive particles of Preparation Example 3 prepared in the above Step II.
[0191] (Example 14)
[0192] The conductive particles of Example 4 were prepared in the same manner as in Example 11, except that Au plating was reacted for 20 minutes on the conductive particles of Preparation Example 3 prepared in Process II above.
[0193] (Example 15)
[0194] The conductive particles of Example 5 were prepared in the same manner as in Example 11, except that Au plating was reacted for 25 minutes on the conductive particles of Preparation Example 3 prepared in Process II above.
[0195] (Example 16)
[0196] The conductive particles of Example 6 were prepared in the same manner as in Example 11, except that Au plating was reacted for 30 minutes on the conductive particles of Preparation Example 3 prepared in Process II above.
[0197] (Example 17)
[0198] To the conductive particles of Preparation Example 4 prepared in Process II above, 2000g of distilled water (DI water), 130g of PEG#600 (polyethylene glycol 600), 42g of potassium hydroxide (KOH), 74g of citric acid, and 4g of potassium gold cyanide were added and stirred at 30℃ for 15 minutes to prepare the conductive particles of Example 17.
[0199] (Example 18)
[0200] Conductive particles of Example 18 were prepared using the same method as in Example 17, except that the reaction was performed at a temperature of 45℃ on the conductive particles of Preparation Example 4 prepared in Process II above.
[0201] (Example 19)
[0202] Conductive particles of Example 19 were prepared using the same method as in Example 17, except that the reaction was performed at a temperature of 60°C on the conductive particles of Preparation Example 3 prepared in Process II above.
[0203] (Example 20)
[0204] Conductive particles of Example 20 were prepared using the same method as in Example 17, except that the reaction was performed at a temperature of 75°C on the conductive particles of Preparation Example 3 prepared in Process II above.
[0205] (Example 21)
[0206] Conductive particles of Example 21 were prepared using the same method as in Example 17, except that the reaction was performed at a temperature of 90°C on the conductive particles of Preparation Example 4 prepared in Process II above.
[0207] (Comparative Example 1)
[0208] Conductive particles of Comparative Example 1 were prepared using the same method as in Example 1, except that the reaction was performed at a temperature of 110℃ on the conductive particles of Preparation Example 3 prepared in Process II above.
[0209] (Comparative Example 2)
[0210] Conductive particles of Comparative Example 2 were prepared using the same method as in Example 1, except that the conductive particles of Preparation Example 4 prepared in the above II process were reacted at a temperature of 110°C.
[0211] (Comparative Example 3)
[0212] The conductive particles of Comparative Example 3 were prepared in the same manner as in Example 11, except that Au plating was reacted for 120 minutes on the conductive particles of Preparation Example 3 prepared in Process II above.
[0213] (Comparative Example 4)
[0214] Conductive particles of Comparative Example 4 were prepared using the same method as in Example 1, except that the conductive particles of Preparation Example 4 prepared in the above II process were reacted at a temperature of 110°C.
[0215] (Comparative Example 5)
[0216] The conductive particles of Manufacturing Example 3 prepared in the above II process were used as the conductive particles of Comparative Example 5.
[0217] The average grain size of the Au layer in Examples 1 to 21 and Comparative Examples 1 to 5 was determined by sampling a conductive particle sample in the X-Ray diffraction instrument measuring holder of Panalytical BV, using a copper (Cu) X-ray wavelength as a light source, and calculating it using [Equation 1] according to the reference data (Ni (No. 98-067-1092) and Au (No. 98-061-1625)) in [Fig. 1] below, and was derived as shown in [Fig. 2] and summarized in [Table 1] and [Table 2].
[0218] [Equation 1] Grain size (nm) = 0.94 x λ / (β·cosθ)
[0219] Here, λ is the wavelength of the copper (Cu) X-ray used for measurement, β is the diffusion of diffraction lines due to grain size, and θ is the diffraction angle 2θ / θ.
[0220] In addition, the thickness of the gold conductive layer of Examples 11 to 21 and Comparative Examples 3 to 5 was verified as shown in [Fig. 3] using FE-TEM of JEOL and EDS of FEI after processing half the cross-section of the conductive particle size using TESCAN’s Dual Beam-FIB (Ga source).
[0221] IV. Evaluation of Conductive Particles (Compressive Strength)
[0222] Compressive strength refers to the compressive strength value according to the amount of deformation of the particles while compressing conductive particles. That is, the relationship between compressive force and amount of deformation when compressing conductive particles can be expressed by the following [Equation 2].
[0223] [Equation 2]
[0224]
[0225] Here, F is the load value (kg) at % compressive strain, S is the compressive displacement (mm) at % compressive strain, E is the compressive strength of the conductive particle (kgf / mm²), R is the radius of the bead (mm), and δ is the Poisson ratio of the particle.
[0226] If we define the K value, that is, the compressive strength according to the amount of deformation, in the above [Equation 2], it can be written as [Equation 3].
[0227] [Equation 3]
[0228]
[0229] Here, K is the compressive strength according to the deformation amount of the conductive particle.
[0230] Therefore, by substituting [Equation 3] into [Equation 2], the compressive strength value according to the amount of deformation of the conductive particles can be obtained as shown in [Equation 4].
[0231] [Equation 4]
[0232]
[0233] Therefore, using a flat indenter with a side length of 50 μm on a Micro Compress Tester (MCT; FISHERSCOPE HM2000), the compression speed of the indenter was set to 0.33 mN / sec, and the rise speed was measured under the condition that it reached 0.1 mN in 10 seconds.
[0234] In the present invention, the compressive strength of the conductive particles of Examples 1 to 10 and Comparative Examples 1 and 2 was evaluated, and the strain of the conductive particles was 20% (K 20 Measured based on the ) and summarized in Table 1.
[0235] V. Preparation of Anisotropic Conductive Film
[0236] 2g of naphthalene-based epoxy resin HP4032D (DIC), 20g of phenoxy resin YP-50 (Toto Kasei), 25g of acrylic epoxy resin VR-60 (Showa Denko), 22g of thermosetting agent HXA-3922HP (Asahi Chemical), and 5g of epoxysilane coupling agent A-187 (Momentive) were thoroughly stirred, and then a mixture with a solid content of 50% was prepared using toluene as a solvent.
[0237] Conductive particles prepared in Examples 1 to 21 and Comparative Examples 1 to 5 were added to the mixture at a weight ratio of 10%, and then an anisotropic conductive paste was prepared by mixing for 5 minutes using a rotational mixer under conditions of 400 rpm rotation and 150 rpm rotation. A film with a thickness of 20 µm was made on a release film using the above anisotropic conductive paste, and then dried in the atmosphere using a hot air dryer at 75°C for 5 minutes to produce a final anisotropic conductive film with a thickness of 12 µm.
[0238] VI. Manufacture of Connection Structure and Measurement of Connection Resistance
[0239] 1) Electrode for resistance measurement
[0240] For resistance measurement, an electrode was fabricated by depositing ITO (Indium Tin Oxide) on a glass substrate to form a transparent electrode, and an FPCB with an electrode width of 20 μm and an electrode spacing of 50 μm.
[0241] 2) Joining
[0242] The above anisotropic conductive film was cut to a width of 3 mm, and a bonding jig with a width of 1 mm and a length of 30 mm was used to press it onto a glass substrate with ITO at 0.2 MPa, 120°C, and 10 seconds, after which an FPCB was placed on top and bonded at 45 MPa, 200°C, and 20 seconds to fabricate a connection structure.
[0243] 3) Measurement of contact resistance
[0244] The resistance of the electrodes of the FPCB of the connection structure manufactured above was measured using an ADCMT 6871E Digital Multimeter 2-probe device and summarized in Tables 1 and 2.
[0245] 4) Stability Measurement (Resistance Rise Rate)
[0246] The reliability resistance was determined by measuring the resistance after leaving the sample for 250 hours under conditions of 85℃ / 85% humidity, and the stability of the conductive particles of Examples 11 to 21 and Comparative Examples 3 to 5 according to the resistance increase rate as shown in [Equation 5] below.
[0247] [Equation 5]
[0248]
[0249] Stability: Stability Resistance / Initial Contact Resistance
[0250] To measure the resistance, the connector that had been left for 250 hours was placed in a dry oven at 100°C for 24 hours to remove residual moisture, and then the resistance was measured using an ADCMT 6871E Digital Multimeter 2 probe and summarized in Table 2.
[0251] Average grain size of gold conductive layer (nm) K20 compressive strength of conductive particles (N / mm 2) Contact Resistance (Ω) Comparative Example 1 20.11 3500 1.11 Comparative Example 2 19.8 13800 1.05 Example 1 3.11 6900 0.60 Example 2 3.31 7300 0.58 Example 3 5.51 6700 0.63 Example 4 6.01 7000 0.60 Example 5 7.51 6500 0.67 Example 6 68.58 6800 0.65 Example 7 11.51 6200 0.72 Example 8 12.10 6400 0.70 Example 9 13.51 6000 0.75 Example 10 14.90 6200 0.73
[0252] In Table 1 above, for the example, as the grain size is refined, the density of grain boundaries increases, thereby enabling the realization of high strength. In addition, the fine grain structure relieves stress concentration within the metal layer, suppressing cracking or delamination even in thermal and mechanical stress environments, and maintaining stable electrical properties over a long period. These characteristics contribute to meeting the high reliability and stability required in highly integrated fine-pitch bonding technology.
[0253] On the other hand, in the comparative example, the grain size is relatively large at 20 nm, so the large grain size reduces the structural uniformity of the metal layer, making it prone to stress concentration and increasing the likelihood of cracking or delamination in a long-term usage environment. As a result, the comparative example has low reliability and has limitations in satisfying the performance required for fine-pitch bonding technology in high-performance electronic devices.
[0254] Gold Conductive Layer Thickness (nm) Gold Conductive Layer Grain Average Size (nm) Initial Contact Resistance (Ω) Stability (Resistance increase rate after 250 hr at 85 / 85 (%)) Comparative Example 3: 35.2 nm 12.11 nm 1.2031 Comparative Example 4: 15.2 nm 20.12 nm 1.1040 Comparative Example 5: 1.221,501 Example 1: 115.2 nm 9.13 nm 0.7350 Example 12: 10.2 nm 9.01 nm 0.7040 Example 13: 15.3 nm 8.95 nm 0.6736 Example 14: 19.2 nm 8.98 nm 0.6533 Example 15: 24.9 nm 9.11 nm 0.6232 Example 16: 29.9 nm 9.20 nm 0.5832 Example 17 15.1 nm 3.01 nm 0.5730 Example 18 14.8 nm 6.32 nm 0.6140 Example 19 15.2 nm 8.92 nm 0.6437 Example 20 14.9 nm 12.10 nm 0.7138 Example 21 15.3 nm 14.95 nm 0.7442
[0255] In Table 2 above, the initial contact resistance and stability according to the thickness and grain size of the gold conductive layer were compared, and the embodiment of the present invention exhibits superior performance compared to the comparative example. In Comparative Example 3, the gold conductive layer thickness is set to 35 nm and the grain size is 12 nm. If the gold conductive layer is excessively thick, the gold layer is excessively formed, which reduces the adhesion between conductive particles and increases the initial contact resistance. In addition, an excessive gold layer has the disadvantage of increasing manufacturing costs.
[0256] Comparative Example 4 is a case where the gold conductive layer thickness is set to 15 nm and the grain size is set to 20 nm. Although the thickness of the gold conductive layer is appropriate, the grain size is too large, which increases the grain boundary area and causes obstruction to the electron transport path. This leads to an increase in contact resistance and a decrease in the stability of the electrical connection.
[0257] In particular, in the case of Comparative Example 5, in which a gold (Au) conductive layer was not formed, it was confirmed that the resistance increased rapidly due to severe oxidation of the nickel layer caused by the absence of a protective layer in a high-humidity environment.
[0258] Examples 11 to 16 represent cases where the gold conductive layer thickness was gradually increased from 5 nm to 30 nm while maintaining the grain size at 9 nm. These examples exhibit low contact resistance and high stability by forming a sufficient gold conductive layer thickness to provide an electron transport path while preventing a decrease in adhesion due to excessive thickness. In particular, when the gold conductive layer thickness is 10 to 30 nm, the contact resistance is stably low and the contact reliability is excellent.
[0259] Examples 17 and 18 represent cases where the gold conductive layer thickness was fixed at 15 nm and the grain size was adjusted to 3 nm and 6 nm, respectively. As the grain size decreases, surface uniformity improves and the grain boundary area is reduced, thereby improving the electron transport path; this leads to a reduction in contact resistance and an improvement in stability. In particular, Example 17 demonstrates the lowest contact resistance and the highest stability.
[0260] Examples 20 and 21 represent cases where the grain size was increased to 12 nm and 15 nm, respectively, while maintaining the same gold conductive layer thickness. Despite the relatively large grain size, these examples still provide a stable electrical connection and exhibit good performance in terms of contact resistance and stability. This demonstrates that excellent performance can be maintained under various conditions within the range of gold conductive layer thickness and grain size set in the present invention.
[0261] The above description is merely illustrative of the present invention, and those skilled in the art to which the present invention pertains will be able to make various modifications within the scope of the essential characteristics of the present invention.
[0262] Accordingly, the embodiments disclosed in this specification are intended to illustrate, not limit, the invention, and the spirit and scope of the invention are not limited by these embodiments. The scope of protection of the invention shall be interpreted by the claims, and all technology within an equivalent scope shall be interpreted as being included within the scope of rights of the invention.
[0263] The present invention relates to a conductive particle comprising a core and a conductive layer, an anisotropic conductive material using the same, and a connection structure.
Claims
1. A conductive particle comprising: a core; a conductive layer comprising Ni, P, and B disposed on the core; a gold conductive layer comprising Au on the conductive layer, wherein the grain size of the gold conductive layer is 15 nm or less.
2. The conductive particle according to claim 1, wherein the thickness of the gold conductive layer is 1 nm to 30 nm.
3. In claim 1, the conductive layer comprises conductive particles further comprising Pd.
4. The conductive particle according to claim 1, wherein the conductive layer comprises: a first conductive layer comprising Ni and P; and a second conductive layer comprising Ni and B formed on the first conductive layer.
5. In claim 1, the core is a conductive particle comprising a monomer composed of a divinylbenzene-based monomer; a styrene-based monomer; an acrylate-based monomer; a silicon-based monomer; or a combination thereof.
6. In claim 5, the styrene-based monomer comprises a monomer comprising styrene; alpha-methylstyrene (α-Methylstyrene); beta-methylstyrene (β-Methylstyrene); para-methylstyrene (p-Methylstyrene); ethylstyrene; hydroxystyrene; vinylxylene; monochlorostyrene; dichlorostyrene; dibromostyrene; vinylnaphthalene; or a combination thereof.
7. In claim 5, the acrylate-based monomer comprises methyl methacrylate (MMA); ethyl methacrylate; propyl methacrylate; butyl methacrylate; benzyl methacrylate; methyl acrylate (MA); ethyl acrylate (EA); propyl acrylate; butyl acrylate; 2-ethylhexyl acrylate; 1,6-hexanediol diacrylate; tetramethylol methane tetraacrylate; ethylene glycol diacrylate; A conductive particle comprising a monomer consisting of ethylene glycol dimethacrylate; propylene glycol diacrylate; trimethylolpropane triacrylate; ethylene glycol dimethacrylate; pentaerythritol tetramethacrylate; or a combination thereof.
8. In claim 5, the silicon-based monomer is vinyltrimethoxysilane; methylchlorosilane; mercaptopropyltrimethoxysilane; vinyltriethoxysilane; phenylchlorosilane; aminopropyltriethoxysilane; epoxycyclohexylethyltrimethoxysilane; [3-(methacryloyloxy)propyl]trimethoxysilane; tetramethoxysilane (TMOS); tetraethoxysilane (TEOS); A conductive particle comprising a monomer composed of triethoxyvinylsilane; trimethylchlorosilane (TMCS); hexamethyldisilazane (HMDS); octamethylcyclotetrasiloxane (D4); decamethylcyclopentasiloxane (D5); polymethylphenylsiloxane; polydiphenylsiloxane; tris(trimethylsiloxy)silane; or a combination thereof.
9. An anisotropic conductive material comprising the conductive particles of claim 1.
10. A connection structure comprising the anisotropic conductive material according to claim 9.
11. In claim 10, the connection structure is a connection structure that is COG (Chip On Glass) or COP (Chip On Plastic).