High modulus basaltic glasses containing titanium oxide

Modified basalt compositions with additives like TiO₂ and P₂O₅ enhance meltability and mechanical properties, addressing meltability and drawability challenges, resulting in high modulus, low-density glass fibers suitable for industrial applications.

WO2026240922A1PCT designated stage Publication Date: 2026-11-19CORNING INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/US2026/024135
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-14
Filing Date
2026-04-17
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Basalt, despite its abundance, presents challenges in meltability and drawability into fibers due to high melting temperatures and viscosities, leading to high energy inputs and limited large-scale production of high modulus, high strength glass fibers.

Method used

Modified basalt-based compositions incorporating additives such as TiO₂, P₂O₅, and ZrO₂ to enhance meltability and mechanical properties, allowing for the production of high modulus glass fibers with reduced energy input.

Benefits of technology

The modified compositions result in higher Young's modulus fibers with competitive specific modulus values, maintaining low density and improving drawability, making them more accessible and cost-effective for industrial use.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure US2026024135_19112026_PF_FP_ABST
    Figure US2026024135_19112026_PF_FP_ABST
Patent Text Reader

Abstract

A glass, comprising: 3-9.3 mol.% Al2O3; 6.9-14 mol.% CaO; 3-5 mol.% Fe; 0-4 mol.% K2O; 11.3-35 mol.% MgO; 0-0.15 mol.% Mn; 0-3 mol.% Na2O; 35-65 mol.% SiO2; and 1-15 mol.% Ti; wherein the Fe is iron in any oxidation state that is assumed to be present as Fe2O3, the Ti is titanium in any oxidation state that is assumed to be present as TiO2, and the Mn is manganese in any oxidation state that is assumed to be present as MnO2. A method for making glass fibers, the method comprising: providing a mixture comprising (1) natural basalt rock, and (2) a source of Ti; heating the mixture to produce a melt; and drawing the glass fibers from the melt; wherein the glass fibers comprise: 3-9.3 mol.% Al2O3; 6.9-14 mol.% CaO; 3-5 mol.% Fe; 0-4 mol.% K2O; 11.3-35 mol.% MgO; 0-0.15 mol.% Mn; 0-3 mol.% Na2O; 35-65 mol.% SiO2; and 0.1-15 mol.% Ti.
Need to check novelty before this filing date? Find Prior Art

Description

Attorney Docket No. SP25-087 PCTHIGH MODULUS BASALTIC GLASSES CONTAINING TITANIUM OXIDECROSS-REFERENCE TO RELATED APPLICATION

[0001] This application claims the benefit of priority under 35 U. S. C. § 119 of U. S. Provisional Application No. 63 / 805,435 filed on May 14, 2025, the content of which is relied upon and incorporated herein by reference in its entirety.FIELD

[0002] The disclosure relates generally to basaltic glasses having modified compositions, and more particularly to glass fibers made from such compositions.BACKGROUND

[0003] Basalt is a widely available natural resource, making up over 90% of all volcanic rock on Earth. It is found in numerous deposits worldwide, each with a unique chemical composition. Despite its abundance and potential for use in high modulus, high strength fibers, basalt can present challenges in terms of meltability and drawability into fibers, as well as relatively lower strength of any glass fibers that are produced directly from melting natural basalt. The high melting temperatures and viscosities of acidic basalt compositions in particular complicate large-scale production, requiring significant energy inputs. Therefore, it would be highly desirable find ways to take advantage of this abundant natural resource, such as by modifying its composition, and to form glass fibers from such modified compositions having desired strength. This disclosure is directed toward these, as well as other, important goals.SUMMARY

[0004] The disclosure relates, in various aspects, to a glass, comprising: 3-9.3 mol.% AI2O3; 6.9-14 mol.% CaO; 3-5 mol.% Fe; 0-4 mol.% K2O; 11.3-35 mol.% MgO; 0-0.15 mol.% Mn; 0-3 mol.% Na2O; 35-65 mol.% SiO2; and 1-15 mol.% Ti; wherein the Fe is iron in any oxidation state that is assumed to be present as Fe2O3, the Ti is titanium in any oxidation state that is assumed to be present as TiO2, and the Mn is manganese in any oxidation state that is assumed to be present as MnO2.

[0005] The disclosure also relates, in various aspects, to A method for making glass fibers, the method comprising: providing a mixture comprising (1) natural basalt rock, and (2) a source of Ti; heating the mixture to produce a melt; and drawing the glass fibers from the melt; wherein the glass fibers comprise: 3-9.3 mol.% Al2O3; 6.9-14 mol.% CaO; 3-5 mol.% Fe; 0-4 mol.% K2O; 11.3-35 mol.% MgO; 0-0.15 mol.% Mn; 0-3 mol.% Na2O; 35-65 mol.% SiO2; and 0.1-15 mol.% Ti; wherein the Fe is iron in any oxidation state that is assumed to be present as Fe2O3, the Ti is titanium in anyAttorney Docket No. SP25-087 PCToxidation state that is assumed to be present as TiO2, and the Mn is manganese in any oxidation state that is assumed to be present as MnO2.

[0006] Additional features and advantages of the disclosure will be set forth in the detailed description which follows, and in part will be readily apparent to those skilled in the art from that description or recognized by practicing the aspects as described herein, including the detailed description which follows, the claims, as well as the appended drawings.

[0007] It is to be understood that both the foregoing general description and the following detailed description are merely exemplary and are intended to provide an overview or framework for understanding the nature and character of the disclosure and claims. The accompanying drawings are included to provide a further understanding of the disclosure and are incorporated into and constitute a part of this specification. The drawings illustrate various aspects of the disclosure and together with the description serve to explain the principles and operations of the various aspects.BRIEF DESCRIPTION OF THE DRAWINGS

[0008] The following detailed description can be further understood when read in conjunction with the following drawings. Whenever possible, the same reference numerals will be used throughout the drawings to refer to the same or like parts. It is to be understood that the figures are not drawn to scale and the size of each depicted component or the relative size of one component to another is not intended to be limiting.

[0009] FIG. 1 is a line graph depicting Young’s modulus vs. specific modulus for various glasses.DETAILED DESCRIPTION

[0010] The terms “glass” and “glass composition” are generally used interchangeably herein. As used herein, a “glass” exhibits an amorphous microstructure that is free or substantially free of crystals or crystallites (i.e., are not glass-ceramics). As used herein, a “glass-ceramic” exhibits both an amorphous microstructure and one or more crystal phases or crystallites. Any glass herein may be subjected to a suitable ceramming cycle that produces a glass-ceramic.

[0011] Herein, glasses are expressed in terms of the mol.% of particular components included therein on an oxide basis as batched unless otherwise indicated (e.g., the amounts may instead be expressed in wt.%). Any component having more than one oxidation state may be present in a composition in any oxidation state. However, concentrations of such component are expressed in terms of the oxide in which such component is at its lowest oxidation state unless otherwise indicated.

[0012] As used herein, “Fe” is iron in any oxidation state that is assumed to be present as Fe2O3, “Ti” is titanium in any oxidation state that is assumed to be present as TiC “Mn” is manganese in any oxidation state that is assumed to be present as MnCL, “Cu” is copper in any oxidation state that is assumed to be present as CuO, and “Cr” is chromium in any oxidation state that is assumed to beAttorney Docket No. SP25-087 PCTpresent as Cr2O3. In other words, when calculating the components of a composition, each of iron, titanium, manganese, copper, and chromium is assumed to be present as the aforementioned indicated oxides, even if such metals or metal ions are actually present in a different oxidation state. These assumptions simplify calculations and allow the straightforward expression of compositional components without determining the actual oxidation state of each metal or metal ion.

[0013] As used herein, the terms “mass” and “weight” are used interchangeably herein.

[0014] As used herein, the term “>0” means “greater than zero” and in an amount greater than what may be present from tramp impurities. Similarly, terms such as “>0-10” means “greater than zero and less than or equal to 10.” Similar meanings can be ascribed to similar terms that merely have different numbers. As used herein, “tramp” means compositional components that are not actively added to a glass composition, but instead are present (a) due to equipment (e.g., furnace components) that has touched the molten glass or precursors thereof, (b) due to entering with the raw materials, and / or (c) because of changeover in the furnace from a prior glass composition to a new glass composition. Such tramp components can include, for example, iron (e.g., as Fe2O3), titanium (e.g., as TiO2), zirconium (e.g., as ZrO2), or precious metals such as platinum and / or rhodium. Each tramp component, if present at all, will typically be present in an amount of less than 0.05 mol.% (e.g., less than 0.04 mol.%, less than 0.03 mol.%, less than 0.02 mol.%, or less than 0.01 mol.%).

[0015] As used herein, a “natural basalt rock” is a crystalline or partially crystalline solid composed of a mixture of minerals, formed through geological processes. Its composition remains unaltered from what is found in nature, reflecting the original mineralogical and chemical characteristics imparted by its geological formation. While its physical form may be modified through size-reducing processes such as crushing or grinding, these actions do not alter the inherent chemical composition of the rock.

[0016] High modulus, high strength glass fibers have a strong longitudinal stiffness but remain flexible due to their small diameter. These glass fibers are used to make stiff composite materials in a flexible form factor across a range of industries including aerospace, defense, architectural, automotive, and energy generation. Specific applications include wind turbine blades and pressurized tanks for hydrogen storage. Silicate glass fiber is a commonly used high modulus, high strength material, and E-glass represents a commodity variant. Silicate glass fiber has lower manufacturing costs than other synthetic fibers, such as carbon fiber. However, specialty glass fibers designed to have industry-leading modulus or strength, such as R-glass, S-glass, and their derivatives, are more expensive to produce due to the expensive rare earth elements raw materials, and high melting and forming temperatures.

[0017] Continuous basalt fibers (CBF) are another high modulus, high strength fiber material, with mechanical properties comparable to specialty glass fibers. Basalt is a naturally formed, extrusive igneous (volcanic) rock composed of Si-Al-Ca-Mg-Na-K-Ti-and Fe. Over 90% of all volcanic rock on Earth is basalt. There are many basalt deposits throughout the world, see Figure 1.Attorney Docket No. SP25-087 PCTEach basalt source has a unique chemistry with weight percentages of oxides ranging from 42-58% SiO2; 1-2% TiO2; 11-20% A12O3; 8-16% FeO+Fe2O3; 4-12% MgO; 7-13% CaO; and 2-4% Na2O+K2O. Basalts are classified by SiO2content as alkaline (about 42 wt% SiO2), mildly acidic (43-46 wt% SiO2), or acidic (>46 wt% SiO2). Basalt fibers have improved chemical corrosion resistance over other glass fibers, are easier to recycle, and the abundant natural source material does not require energy-intensive processing resulting in low raw materials cost. Despite these benefits, industry has been slow to adopt the use of CBF because current production volumes are too low, raising the final price point too high for widespread use.

[0018] CBF is manufactured at low volumes throughout the world, most is generated in Eastern Europe and China using acidic basalt compositions. The high SiO2compositions allow for the high mechanical properties of the fiber. However, processing these acidic basalt compositions is very challenging. Acidic basalt compositions are more viscous, have higher melting temperatures (Tmof about 1400-1650 °C), and similarly higher forming temperatures (Tf of about 1300-1550 °C), than traditional E-glass fibers (Tmof about 1345-1460 °C, and Tf of about 1180-1280 °C). High forming temperatures are required because basalts have a high crystallization temperature and crystallization rate. In addition, the high iron contents of basalts means that the melt absorbs more energy than a more conventional glass fiber composition. This poor heat permeability means it takes more time and energy to uniformly heat a basalt melt. Therefore, large scale, high efficiency production of CBF is currently not possible largely because the manufacturing of basalt fibers requires too high energy inputs.

[0019] As fiber glass melter designs are trending toward all electric to meet sustainability goals, CBF manufacturing will be more viable. The use of submerged electrodes in the glass melt will allow for a more uniformly heated basalt melt. Improve meltability of the basalt and therefore reduced energy input required to form a homogeneous melt is desired to make CBF accessible to the markets in a cost-effective manner.

[0020] Disclosed herein are modified basalt-based compositions that achieve desired properties, such as improved mechanical properties and / or being easier to draw into fibers. Modification of chemical composition by introducing additives is an effective way to impact meltability and physical properties of CFBs. In particular, the mechanical properties (most notably the Young’s modulus) of the modified compositions are increased relative to the starting basalts, all while maintaining a low density allowing for higher Young’s modulus fibers at competitive specific modulus values. This is achieved through the addition of various additives, including oxides of transition metals (e.g., TiO2), high-field strength elements, and / or rare earth elements, which results in an increase in the Young’s modulus without a marked increase in density. Oxides of transition metals in particular are by far the least expensive additives and provide a sizeable boost in modulus. This has allowed the ability to make fibers with higher modulus than industry standard glasses (E, S, and R glasses), all while maintaining similar specific modulus. Moreover, P2O3can additionally be added to improve viscosityAttomey Docket No. SP25-087 PCTof the basalt melt to render it drawable for making glass fibers, generally by increasing the viscosity of the basalt melt without negatively affecting mechanical properties. In this regard, the addition of P2O5 in these basalt compositions allowed control of the viscosity of the melt at drawing temperatures, since, in some cases, the composition could not be drawn as a fiber due to its low viscosity, but the addition of P2O5 allowed high quality fibers to be drawn. ZrCF can play a dual role, where it can help modulate viscosity and provide an increase to the Young’s modulus. Ultimately, the modifications to natural basalts allow for taking an abundant and inexpensive raw material (basalt) and tweaking its properties to render it stronger and easier to produce than current industry standards.

[0021] Disclosed herein are glasses and glass-ceramics. In some aspects, the glasses or glassceramics comprise:3-9.3 mol.% AI2O3;6.9-14 mol.% CaO;3-5 mol.% Fe;0-4 mol.% K2O;11.3-35 mol.% MgO;0-0.15 mol.% Mn;0-3 mol.% Na2O;35-65 mol.% SiO2; and0.1-15 mol.% Ti or 1-15 mol.% Ti;wherein the Fe is iron in any oxidation state that is assumed to be present as Fe2O3, the Ti is titanium in any oxidation state that is assumed to be present as TiO2, and the Mn is manganese in any oxidation state that is assumed to be present as MnO2.

[0022] In some aspects, the glasses or glass-ceramics can comprise AI2O3 in an amount (mol.%) of at least 2, at least 2.5, at least 3, at least 3.5, at least 4, at least 4.5, at least 5, at least 5.5, at least 6, at least 6.5, at least 7, at least 7.5, at least 8, at least 8.5, at least 9, at least 9.3, at least 9.5, at least 10, 10 or less, 9.5 or less, 9.3 or less, 9 or less, 8.5 or less, 8 or less, 7.5 or less, 7 or less, 6.5 or less, 6 or less, 5.5 or less, 5 or less, 4.5 or less, 4 or less, 3.5 or less, 3 or less, 2.5 or less, 2 or less, or any range formed from any two of the foregoing endpoints. For example, in some aspects, the glasses or glassceramics can comprise AI2O3 in an amount (mol.%) of 2-2.5, 2-3, 2-3.5, 2-4, 2-4.5, 2-5, 2-5.5, 2-6, 2- 6.5, 2-7, 2-7.5, 2-8, 2-8.5, 2-9, 2-9.3, 2-9.5, 2-10, 2.5-3, 2.5-3.5, 2.5-4, 2.5-4.5, 2.5-5, 2.5-5.5, 2.5-6,2.5-6.5, 2.5-7, 2.5-7.5, 2.5-8, 2.5-8.5, 2.5-9, 2.5-9.3, 2.5-9.5, 2.5-10, 3-3.5, 3-4, 3-4.5, 3-5, 3-5.5, 3-6, 3-6.5, 3-7, 3-7.5, 3-8, 3-8.5, 3-9, 3-9.3, 3-9.5, 3-10, 3.5-4, 3.5-4.5, 3.5-5, 3.5-5.5, 3.5-6, 3.5-6.5, 3.5-7,3.5-7.5, 3.5-8, 3.5-8.5, 3.5-9, 3.5-9.3, 3.5-9.5, 3.5-10, 4-4.5, 4-5, 4-5.5, 4-6, 4-6.5, 4-7, 4-7.5, 4-8, 4- 8.5, 4-9, 4-9.3, 4-9.5, 4-10, 4.5-5, 4.5-5.5, 4.5-6, 4.5-6.5, 4.5-7, 4.5-7.5, 4.5-8, 4.5-8.5, 4.5-9, 4.5-9.3,4.5-9.5, 4.5-10, 5-5.5, 5-6, 5-6.5, 5-7, 5-7.5, 5-8, 5-8.5, 5-9, 5-9.3, 5-9.5, 5-10, 5.5-6, 5.5-6.5, 5.5-7,5.5-7.5, 5.5-8, 5.5-8.5, 5.5-9, 5.5-9.3, 5.5-9.5, 5.5-10, 6-6.5, 6-7, 6-7.5, 6-8, 6-8.5, 6-9, 6-9.3, 6-9.5, 6-10, 6.5-7, 6.5-7.5, 6.5-8, 6.5-8.5, 6.5-9, 6.5-9.3, 6.5-9.5, 6.5-10, 7-7.5, 7-8, 7-8.5, 7-9, 7-9.3, 7-9.5, 7-Attorney Docket No. SP25-087 PCT10, 7.5-8, 7.5-8.5, 7.5-9, 7.5-9.3, 7.5-9.5, 7.5-10, 8-8.5, 8-9, 8-9.3, 8-9.5, 8-10, 8.5-9, 8.5-9.3, 8.5-9.5,8.5-10, 9-9.3, 9-9.5, 9-10, 9.3-9.5, 9.3-10, or 9.5-10. In particular, in some aspects, the glasses or glass-ceramics can comprise AI2O3 in an amount (mol.%) of 2-9, 3-9.3, 3-9, 4-9, or 4.5-9. In some aspects, the glasses or glass-ceramics are free, or substantially free, of AI2O3.

[0023] In some aspects, the glasses or glass-ceramics can comprise CaO in an amount (mol.%) of at least 6, at least 6.5, at least 6.9, at least 7, at least 7.2, at least 7.5, at least 8, at least 9, at least 10, at least 11, at least 12, at least 13, at least 14, at least 15, 15 or less, 14 or less, 13 or less, 12 or less, 11 or less, 10 or less, 9 or less, 8 or less, 7.5 or less, 7.2 or less, 7 or less, 6.9 or less, 6.5 or less, 6 or less, or any range formed from any two of the foregoing endpoints. For example, in some aspects, the glasses or glass-ceramics can comprise CaO in an amount (mol.%) of 6-6.5, 6-6.9, 6-7, 6-7.2, 6-7.5, 6-8, 6-9, 6-10, 6-11, 6-12, 6-13, 6-14, 6-15, 6.5-6.9, 6.5-7, 6.5-72, 6.5-7.5, 6.5-8, 6.5-9, 6.5-10, 6.5- 11, 6.5-12, 6.5-13, 6.5-14, 6.5-15, 6.9-7, 6.9-72, 6.9-7.5, 6.9-8, 6.9-9, 6.9-10, 6.9-11, 6.9-12, 6.9-13, 6.9-14, 6.9-15, 7-7.2, 7-7.5, 7-8, 7-9, 7-10, 7-11, 7-12, 7-13, 7-14, 7-15, 72-7.5, 7.2-8, 7.2-9, 7.2-10, 7.2-11, 7.2-12, 7.2-13, 7.2-14, 7.2-15, 7.5-8, 7.5-9, 7.5-10, 7.5-11, 7.5-12, 7.5-13, 7.5-14, 7.5-15, 8-9, 8-10, 8-11, 8-12, 8-13, 8-14, 8-15, 9-10, 9-11, 9-12, 9-13, 9-14, 9-15, 10-11, 10-12, 10-13, 10-14, 10-15, 11-12, 11-13, 11-14, 11-15, 12-13, 12-14, 12-15, 13-14, 13-15, or 14-15. In particular, in some aspects, the glasses or glass-ceramics can comprise CaO in an amount (mol.%) of 6-15, 6.9-14, 7-13, or 6.9-12. In some aspects, the glasses or glass-ceramics are free, or substantially free, of CaO.

[0024] In some aspects, the glasses or glass-ceramics can comprise Fe in an amount (mol.%) of at least 2.8, at least 3, at least 3.2, at least 3.4, at least 3.5, at least 3.6, at least 3.8, at least 4, at least 4.2, at least 4.4, at least 4.5, at least 4.6, at least 4.8, at least 5, at least 5.2, 5.2 or less, 5 or less, 4.8 or less, 4.6 or less, 4.5 or less, 4.4 or less, 4.2 or less, 4 or less, 3.8 or less, 3.6 or less, 3.5 or less, 3.4 or less, 3.2 or less, 3 or less, 2.8 or less, or any range formed from any two of the foregoing endpoints. For example, in some aspects, the glasses or glass-ceramics can comprise Fe in an amount (mol.%) of2.8-3, 2.8-3.2, 2.8-3.4, 2.8-3.5, 2.8-3.6, 2.8-3.8, 2.8-4, 2.8-4.2, 2.8-4.4, 2.8-4.5, 2.8-4.6, 2.8-4.8, 2.8-5,2.8-5.2, 3-3.2, 3-3.4, 3-3.5, 3-3.6, 3-3.8, 3-4, 3-4.2, 3-4.4, 3-4.5, 3-4.6, 3-4.8, 3-5, 3-5.2, 3.2-3.4, 3.2-3.5, 3.2-3.6, 3.2-3.8, 3.2-4, 3.2-4.2, 3.2-4.4, 3.2-4.5, 3.2-4.6, 3.2-4.8, 3.2-5, 3.2-5.2, 3.4-3.5, 3.4-3.6,3.4-3.8, 3.4-4, 3.4-4.2, 3.4-4.4, 3.4-4.5, 3.4-4.6, 3.4-4.8, 3.4-5, 3.4-5.2, 3.5-3.6, 3.5-3.8, 3.5-4, 3.5-4.2,3.5-4.4, 3.5-4.5, 3.5-4.6, 3.5-4.8, 3.5-5, 3.5-5.2, 3.6-3.8, 3.6-4, 3.6-4.2, 3.6-4.4, 3.6-4.5, 3.6-4.6, 3.6-4.8, 3.6-5, 3.6-5.2, 3.8-4, 3.8-4.2, 3.8-4.4, 3.8-4.5, 3.8-4.6, 3.8-4.8, 3.8-5, 3.8-5.2, 4-4.2, 4-4.4, 4-4.5, 4-4.6, 4-4.8, 4-5, 4-5.2, 4.2-4.4, 4.2-4.5, 4.2-4.6, 4.2-4.8, 4.2-5, 4.2-5.2, 4.4-4.5, 4.4-4.6, 4.4-4.8, 4.4-5, 4.4-5.2, 4.5-4.6, 4.5-4.8, 4.5-5, 4.5-5.2, 4.6-4.8, 4.6-5, 4.6-5.2, 4.8-5, 4.8-5.2, or 5-5.2. In particular, in some aspects, the glasses or glass-ceramics can comprise Fe in an amount (mol.%) of 2.8-5.2, 3-5,3.5-4.5, or 3.2-4.6. In some aspects, the glasses or glass-ceramics are free, or substantially free, of Fe. Fe is iron in any oxidation state that is assumed to be present as Fe2O3.

[0025] In some aspects, the glasses or glass-ceramics can comprise K2O in an amount (mol.%) of 0, >0, at least 0.5, at least 1, at least 1.5, at least 2, at least 2.5, at least 3, at least 3.5, at least 4, at leastAttorney Docket No. SP25-087 PCT4.5, at least 5, 5 or less, 4.5 or less, 4 or less, 3.5 or less, 3 or less, 2.5 or less, 2 or less, 1.5 or less, 1 or less, 0.5 or less, or any range formed from any two of the foregoing endpoints. For example, in some aspects, the glasses or glass-ceramics can comprise K2O in an amount (mol.%) of 0-0.5, 0-1, 0- 1.5, 0-2, 0-2.5, 0-3, 0-3.5, 0-4, 0-4.5, 0-5, >0-0.5, >0-1, >0-1.5, >0-2, >0-2.5, >0-3, >0-3.5, >0-4, >0- 4.5, >0-5, 0.5-1, 0.5-1.5, 0.5-2, 0.5-2.5, 0.5-3, 0.5-3.5, 0.5-4, 0.5-4.5, 0.5-5, 1-1.5, 1-2, 1-2.5, 1-3, 1- 3.5, 1-4, 1-4.5, 1-5, 1.5-2, 1.5-2.5, 1.5-3, 1.5-3.5, 1.5-4, 1.5-4.5, 1.5-5, 2-2.5, 2-3, 2-3.5, 2-4, 2-4.5, 2-5, 2.5-3, 2.5-3.5, 2.5-4, 2.5-4.5, 2.5-5, 3-3.5, 3-4, 3-4.5, 3-5, 3.5-4, 3.5-4.5, 3.5-5, 4-4.5, 4-5, or 4.5-5. In particular, in some aspects, the glasses or glass-ceramics can comprise K2O in an amount (mol.%) of 0-5, 0-4, 0-1, >0-2, or >0-1.5. In some aspects, the glasses or glass-ceramics are free, or substantially free, of K2O.

[0026] In some aspects, the glasses or glass-ceramics can comprise Na20 in an amount (mol.%) of 0, >0, at least 0.5, at least 1, at least 1.5, at least 2, at least 2.5, at least 3, at least 3.5, at least 4, 4 or less, 3.5 or less, 3 or less, 2.5 or less, 2 or less, 1.5 or less, 1 or less, 0.5 or less, or any range formed from any two of the foregoing endpoints. For example, in some aspects, the glasses or glass-ceramics can comprise Na20 in an amount (mol.%) of 0-0.5, 0-1, 0-1.5, 0-2, 0-2.5, 0-3, 0-3.5, 0-4, >0-0.5, >0-1, >0-1.5, >0-2, >0-2.5, >0-3, >0-3.5, >0-4, 0.5-1, 0.5-1.5, 0.5-2, 0.5-2.5, 0.5-3, 0.5-3.5, 0.5-4, 1-1.5, 1-2, 1-2.5, 1-3, 1-3.5, 1-4, 1.5-2, 1.5-2.5, 1.5-3, 1.5-3.5, 1.5-4, 2-2.5, 2-3, 2-3.5, 2-4, 2.5-3, 2.5-3.5, 2.5-4, 3-3.5, 3-4, or 3.5-4. In particular, in some aspects, the glasses or glass-ceramics can comprise Na20 in an amount (mol.%) of 0-4, 0-3, >0-2, or 0.5-3. In some aspects, the glasses or glass-ceramics are free, or substantially free, of Na20.

[0027] In some aspects, the glasses or glass-ceramics can comprise Na2O+K2O in an amount (mol.%) of 0, >0, at least 0.5, at least 1, at least 1.5, at least 2, at least 2.5, at least 3, at least 3.5, at least 4, at least 4.5, at least 5, 5 or less, 4.5 or less, 4 or less, 3.5 or less, 3 or less, 2.5 or less, 2 or less, 1.5 or less, 1 or less, 0.5 or less, or any range formed from any two of the foregoing endpoints. For example, in some aspects, the glasses or glass-ceramics can comprise Na2O+K2O in an amount (mol.%) of 0-0.5, 0-1, 0-1.5, 0-2, 0-2.5, 0-3, 0-3.5, 0-4, 0-4.5, 0-5, >0-0.5, >0-1, >0-1.5, >0-2, >0-2.5, >0-3, >0-3.5, >0-4, >0-4.5, >0-5, 0.5-1, 0.5-1.5, 0.5-2, 0.5-2.5, 0.5-3, 0.5-3.5, 0.5-4, 0.5-4.5, 0.5-5, 1- 1.5, 1-2, 1-2.5, 1-3, 1-3.5, 1-4, 1-4.5, 1-5, 1.5-2, 1.5-2.5, 1.5-3, 1.5-3.5, 1.5-4, 1.5-4.5, 1.5-5, 2-2.5, 2-3, 2-3.5, 2-4, 2-4.5, 2-5, 2.5-3, 2.5-3.5, 2.5-4, 2.5-4.5, 2.5-5, 3-3.5, 3-4, 3-4.5, 3-5, 3.5-4, 3.5-4.5, 3.5-5, 4-4.5, 4-5, or 4.5-5. In particular, in some aspects, the glasses or glass-ceramics can comprise Na2O+K2O in an amount (mol.%) of 0-5, 0-3, >0-5, or 0.5-4. In some aspects, the glasses or glassceramics are free, or substantially free, of Na2O+K2O.

[0028] In some aspects, the glasses or glass-ceramics can comprise MgO in an amount (mol.%) of at least 10, at least 11.3, at least 11.5, at least 15, at least 20, at least 25, at least 30, at least 32, at least 35, 35 or less, 32 or less, 30 or less, 25 or less, 20 or less, 15 or less, 11.5 or less, 11.3 or less, 10 or less, or any range formed from any two of the foregoing endpoints. For example, in some aspects, the glasses or glass-ceramics can comprise MgO in an amount (mol.%) of 10- 11.3, 10- 11.5, 10-15,Attomey Docket No. SP25-087 PCT10-20, 10-25, 10-30, 10-32, 10-35, 11.3-11.5, 11.3-15, 11.3-20, 11.3-25, 11.3-30, 11.3-32, 11.3-35, 11.5-15, 11.5-20, 11.5-25, 11.5-30, 11.5-32, 11.5-35, 15-20, 15-25, 15-30, 15-32, 15-35, 20-25, 20-30, 20-32, 20-35, 25-30, 25-32, 25-35, 30-32, 30-35, or 32-35. In particular, in some aspects, the glasses or glass-ceramics can comprise MgO in an amount (mol.%) of 11.3-35, 11.5-32, 11.5-15, or 25-32. In some aspects, the glasses or glass-ceramics are free, or substantially free, of MgO.

[0029] In some aspects, the glasses or glass-ceramics can comprise Mn in an amount (mol.%) of 0, >0, at least 0.02, at least 0.04, at least 0.06, at least 0.08, at least 0.1, at least 0.12, at least 0.14, at least 0.15, at least 0.16, at least 0.18, at least 0.2, 0.2 or less, 0.18 or less, 0.16 or less, 0.15 or less, 0.14 or less, 0.12 or less, 0.1 or less, 0.08 or less, 0.06 or less, 0.04 or less, 0.02 or less, or any range formed from any two of the foregoing endpoints. For example, in some aspects, the glasses or glassceramics can comprise Mn in an amount (mol.%) of 0-0.02, 0-0.04, 0-0.06, 0-0.08, 0-0.1, 0-0.12, 0-0.14, 0-0.15, 0-0.16, 0-0.18, 0-0.2, >0-0.02, >0-0.04, >0-0.06, >0-0.08, >0-0.1, >0-0.12, >0-0.14, >0-0.15, >0-0.16, >0-0.18, >0-0.2, 0.02-0.04, 0.02-0.06, 0.02-0.08, 0.02-0.1, 0.02-0.12, 0.02-0.14, 0.02-0.15, 0.02-0.16, 0.02-0.18, 0.02-0.2, 0.04-0.06, 0.04-0.08, 0.04-0.1, 0.04-0.12, 0.04-0.14, 0.04-0.15, 0.04-0.16, 0.04-0.18, 0.04-0.2, 0.06-0.08, 0.06-0.1, 0.06-0.12, 0.06-0.14, 0.06-0.15, 0.06-0.16, 0.06-0.18, 0.06-0.2, 0.08-0.1, 0.08-0.12, 0.08-0.14, 0.08-0.15, 0.08-0.16, 0.08-0.18, 0.08-0.2, 0.1-0.12, 0.1-0.14, 0.1-0.15, 0.1-0.16, 0.1-0.18, 0.1-0.2, 0.12-0.14, 0.12-0.15, 0.12-0.16, 0.12-0.18, 0.12-0.2, 0.14-0.15, 0.14-0.16, 0.14-0.18, 0.14-0.2, 0.15-0.16, 0.15-0.18, 0.15-0.2, 0.16-0.18, 0.16-0.2, or 0.18-0.2. In particular, in some aspects, the glasses or glass-ceramics can comprise Mn in an amount (mol.%) of 0-0.2, 0-0.15, >0-0.12, or 0-0.14. In some aspects, the glasses or glass-ceramics are free, or substantially free, of Mn. Mn is manganese in any oxidation state that is assumed to be present as MnO2.

[0030] In some aspects, the glasses or glass-ceramics can comprise SiCh in an amount (mol.%) of at least 35, at least 40, at least 42, at least 45, at least 50, at least 55, at least 60, at least 65, 65 or less, 60 or less, 55 or less, 50 or less, 45 or less, 42 or less, 40 or less, 35 or less, or any range formed from any two of the foregoing endpoints. For example, in some aspects, the glasses or glass-ceramics can comprise SiO2in an amount (mol.%) of 35-40, 35-42, 35-45, 35-50, 35-55, 35-60, 35-65, 40-42, 40-45, 40-50, 40-55, 40-60, 40-65, 42-45, 42-50, 42-55, 42-60, 42-65, 45-50, 45-55, 45-60, 45-65, 50-55, 50-60, 50-65, 55-60, 55-65, or 60-65. In particular, in some aspects, the glasses or glass-ceramics can comprise SiO2in an amount (mol.%) of 35-65, 42-60, 42-50, or 50-60. In some aspects, the glasses or glass-ceramics are free, or substantially free, of SiO2.

[0031] In some aspects, the glasses or glass-ceramics can comprise Ti in an amount (mol.%) of 0, >0, at least 0.1, at least 1, at least 2, at least 3, at least 4, at least 5, at least 6, at least 7, at least 8, at least 9, at least 10, at least 11, at least 12, at least 13, at least 14, at least 15, 15 or less, 14 or less, 13 or less, 12 or less, 11 or less, 10 or less, 9 or less, 8 or less, 7 or less, 6 or less, 5 or less, 4 or less, 3 or less, 2 or less, 1 or less, 0.1 or less, or any range formed from any two of the foregoing endpoints. For example, in some aspects, the glasses or glass-ceramics can comprise Ti in an amount (mol.%) of 0-Attorney Docket No. SP25-087 PCT0.1, 0-1, 0-2, 0-3, 0-4, 0-5, 0-6, 0-7, 0-8, 0-9, 0-10, 0-11, 0-12, 0-13, 0-14, 0-15, >0-0.1, >0-1, >0-2, >0-3, >0-4, >0-5, >0-6, >0-7, >0-8, >0-9, >0-10, >0-11, >0-12, >0-13, >0-14, >0-15, 0.1-1, 0.1-2, 0.1-3, 0.1-4, 0.1-5, 0.1-6, 0.1-7, 0.1-8, 0.1-9, 0.1-10, 0.1-11, 0.1-12, 0.1-13, 0.1-14, 0.1-15, 1-2, 1-3, 1-4,1-5, 1-6, 1-7, 1-8, 1-9, 1-10, 1-11, 1-12, 1-13, 1-14, 1-15, 2-3, 2-4, 2-5, 2-6, 2-7, 2-8, 2-9, 2-10, 2-11,2-12, 2-13, 2-14, 2-15, 3-4, 3-5, 3-6, 3-7, 3-8, 3-9, 3-10, 3-11, 3-12, 3-13, 3-14, 3-15, 4-5, 4-6, 4-7, 4-8, 4-9, 4-10, 4-11, 4-12, 4-13, 4-14, 4-15, 5-6, 5-7, 5-8, 5-9, 5-10, 5-11, 5-12, 5-13, 5-14, 5-15, 6-7, 6- 8, 6-9, 6-10, 6-11, 6-12, 6-13, 6-14, 6-15, 7-8, 7-9, 7-10, 7-11, 7-12, 7-13, 7-14, 7-15, 8-9, 8-10, 8-11, 8-12, 8-13, 8-14, 8-15, 9-10, 9-11, 9-12, 9-13, 9-14, 9-15, 10-11, 10-12, 10-13, 10-14, 10-15, 11-12, 11-13, 11-14, 11-15, 12-13, 12-14, 12-15, 13-14, 13-15, or 14-15. In particular, in some aspects, the glasses or glass-ceramics can comprise Ti in an amount (mol.%) of 0.1-15, 1-15, 2-10, or 1-10. In some aspects, the glasses or glass-ceramics are free, or substantially free, of Ti. Ti is titanium in any oxidation state that is assumed to be present as TiO2.

[0032] In some aspects, the glasses or glass-ceramics can comprise the ratio Fe / Ti in an amount (mol.% / mol.%) of 0, >0, at least 0.1, at least 0.5, at least 1, at least 1.5, at least 2, at least 2.5, at least 3, at least 3.5, at least 4, at least 4.5, at least 5, 5 or less, 4.5 or less, 4 or less, 3.5 or less, 3 or less, 2.5 or less, 2 or less, 1.5 or less, 1 or less, 0.5 or less, 0.1 or less, or any range formed from any two of the foregoing endpoints. For example, in some aspects, the glasses or glass-ceramics can comprise the ratio Fe / Ti in an amount (mol.% / mol.%) of 0-0.1, 0-0.5, 0-1, 0-1.5, 0-2, 0-2.5, 0-3, 0-3.5, 0-4, 0-4.5, 0-5, >0-0.1, >0-0.5, >0-1, >0-1.5, >0-2, >0-2.5, >0-3, >0-3.5, >0-4, >0-4.5, >0-5, 0.1-0.5, 0.1-1, 0.1-1.5, 0.1-2, 0.1-2.5, 0.1-3, 0.1-3.5, 0.1-4, 0.1-4.5, 0.1-5, 0.5-1, 0.5-1.5, 0.5-2, 0.5-2.5, 0.5-3, 0.5-3.5, 0.5-4, 0.5-4.5, 0.5-5, 1-1.5, 1-2, 1-2.5, 1-3, 1-3.5, 1-4, 1-4.5, 1-5, 1.5-2, 1.5-2.5, 1.5-3, 1.5-3.5, 1.5-4, 1.5-4.5, 1.5-5, 2-2.5, 2-3, 2-3.5, 2-4, 2-4.5, 2-5, 2.5-3, 2.5-3.5, 2.5-4, 2.5-4.5, 2.5-5, 3-3.5, 3-4, 3-4.5,3-5, 3.5-4, 3.5-4.5, 3.5-5, 4-4.5, 4-5, or 4.5-5. In particular, in some aspects, the glasses or glassceramics can comprise the ratio Fe / Ti in an amount (mol.% / mol.%) of 0.1-3, 0.1-2, or >0-2.

[0033] In some aspects, the glasses or glass-ceramics can comprise P2O5 in an amount (mol.%) of 0, >0, at least 0.5, at least 1, at least 1.5, at least 2, at least 2.5, at least 3, at least 4, at least 5, at least 6, at least 7, at least 8, at least 9, at least 10, 10 or less, 9 or less, 8 or less, 7 or less, 6 or less, 5 or less, 4 or less, 3 or less, 2.5 or less, 2 or less, 1.5 or less, 1 or less, 0.5 or less, or any range formed from any two of the foregoing endpoints. For example, in some aspects, the glasses or glass-ceramics can comprise P2O5 in an amount (mol.%) of 0-0.5, 0-1, 0-1.5, 0-2, 0-2.5, 0-3, 0-4, 0-5, 0-6, 0-7, 0-8, 0-9, 0-10, >0-0.5, >0-1, >0-1.5, >0-2, >0-2.5, >0-3, >0-4, >0-5, >0-6, >0-7, >0-8, >0-9, >0-10, 0.5-1, 0.5-1.5, 0.5-2, 0.5-2.5, 0.5-3, 0.5-4, 0.5-5, 0.5-6, 0.5-7, 0.5-8, 0.5-9, 0.5-10, 1-1.5, 1-2, 1-2.5, 1-3, 1-4,1-5, 1-6, 1-7, 1-8, 1-9, 1-10, 1.5-2, 1.5-2.5, 1.5-3, 1.5-4, 1.5-5, 1.5-6, 1.5-7, 1.5-8, 1.5-9, 1.5-10, 2-2.5,2-3, 2-4, 2-5, 2-6, 2-7, 2-8, 2-9, 2-10, 2.5-3, 2.5-4, 2.5-5, 2.5-6, 2.5-7, 2.5-8, 2.5-9, 2.5-10, 3-4, 3-5, 3-6, 3-7, 3-8, 3-9, 3-10, 4-5, 4-6, 4-7, 4-8, 4-9, 4-10, 5-6, 5-7, 5-8, 5-9, 5-10, 6-7, 6-8, 6-9, 6-10, 7-8, 7- 9, 7-10, 8-9, 8-10, or 9-10. In particular, in some aspects, the glasses or glass-ceramics can compriseAttomey Docket No. SP25-087 PCTP2O5 in an amount (mol.%) of >0-5, 1-5, or 1.5-4. In some aspects, the glasses or glass-ceramics are free, or substantially free, of P2O5.

[0034] In some aspects, the glasses or glass-ceramics can comprise additional components, such as Li2O, oxides of transition metals, oxides of high field strength elements, oxides of rare earth elements, or any combination thereof. In some aspects, the additional components can include SrO, ZrO2, Cu, ZnO, V2O5, Cr, CoO, Nb2O5, La2O3, Y2O3, Li2O, or any combination thereof, in which Cu is copper in any oxidation state that is assumed to be present as CuO, and Cr is chromium in any oxidation state that is assumed to be present as Cr2O3. In some aspects, the glasses or glass-ceramics comprise ZrO2. In some aspects, the glasses or glass-ceramics can comprise at least one of SrO, ZrO2, Cu, ZnO, V2O5, Cr, CoO, Nb2O5, La2O3, Y2O3, and Li2O. In some aspects, the glasses or glassceramics can comprise a sum of SrO + ZrO2+ Cu + ZnO + V2O5+ Cr + CoO + Nb2O5+ La2O3+ Y2O3+ Li2O in an amount of at least 0.1 mol.%. In some aspects, a sum of SrO + ZrO2+ Cu + ZnO + V2O5+ Cr + CoO + Nb2O5+ La2O3+ Y2O3+ Li2O is at least 0.1 mol.%. In some aspects, any of the aforementioned sums, or any of the amounts of any individual component, (mol.%) can be 0, >0, at least 1, at least 2, at least 3, at least 4, at least 5, at least 6, at least 7, at least 8, at least 9, at least 10, 10 or less, 9 or less, 8 or less, 7 or less, 6 or less, 5 or less, 4 or less, 3 or less, 2 or less, 1 or less, or any range formed from any two of the foregoing endpoints. For example, in some aspects, any of the aforementioned sums, or any of the amounts of any individual component, (mol.%) can be 0-1, 0-2, 0-3, 0-4, 0-5, 0-6, 0-7, 0-8, 0-9, 0-10, >0-1, >0-2, >0-3, >0-4, >0-5, >0-6, >0-7, >0-8, >0-9, >0-10, 1-2, 1-3, 1-4, 1-5, 1-6, 1-7, 1-8, 1-9, 1-10, 2-3, 2-4, 2-5, 2-6, 2-7, 2-8, 2-9, 2-10, 3-4, 3-5, 3-6, 3-7, 3-8, 3- 9, 3-10, 4-5, 4-6, 4-7, 4-8, 4-9, 4-10, 5-6, 5-7, 5-8, 5-9, 5-10, 6-7, 6-8, 6-9, 6-10, 7-8, 7-9, 7-10, 8-9, 8- 10, or 9-10. In particular, in some aspects, any of the aforementioned sums, or any of the amounts of any individual component, (mol.%) can be 0.1-10, >0-5, 1-6, or 2-4. In some aspects, the glasses or glass-ceramics are free, or substantially free, of any one or more of SrO, ZrO2, Cu, ZnO, V2O5, Cr, CoO, Nb2O5, La2O3, Y2O3, and Li2O.

[0035] In some aspects, the glasses or glass-ceramics can have a Young's modulus (GPa) that can be at least 90, at least 92, at least 94, at least 96, at least 98, at least 100, at least 102, at least 104, at least 106, at least 108, at least 110, at least 112, at least 114, at least 116, at least 118, at least 120, 120 or less, 118 or less, 116 or less, 114 or less, 112 or less, 110 or less, 108 or less, 106 or less, 104 or less, 102 or less, 100 or less, 98 or less, 96 or less, 94 or less, 92 or less, 90 or less, or any range formed from any two of the foregoing endpoints. For example, in some aspects, the Young's modulus (GPa) can be 90-92, 90-94, 90-96, 90-98, 90-100, 90-102, 90-104, 90-106, 90-108, 90-110, 90-112, 90-114, 90-116, 90-118, 90-120, 92-94, 92-96, 92-98, 92-100, 92-102, 92-104, 92-106, 92-108, 92-110, 92-112, 92-114, 92-116, 92-118, 92-120, 94-96, 94-98, 94-100, 94-102, 94-104, 94-106, 94-108, 94-110, 94-112, 94-114, 94-116, 94-118, 94-120, 96-98, 96-100, 96-102, 96-104, 96-106, 96-108, 96-110, 96-112, 96-114, 96-116, 96-118, 96-120, 98-100, 98-102, 98-104, 98-106, 98-108, 98-110, 98-112, 98-114, 98-116, 98-118, 98-120, 100-102, 100-104, 100-106, 100-108, 100-110, 100-112, 100-Attomey Docket No. SP25-087 PCT114, 100-116, 100-118, 100-120, 102-104, 102-106, 102-108, 102-110, 102-112, 102-114, 102-116, 102-118, 102-120, 104-106, 104-108, 104-110, 104-112, 104-114, 104-116, 104-118, 104-120, 106-108, 106-110, 106-112, 106-114, 106-116, 106-118, 106-120, 108-110, 108-112, 108-114, 108-116, 108-118, 108-120, 110-112, 110-114, 110-116, 110-118, 110-120, 112-114, 112-116, 112-118, 112-120, 114-116, 114-118, 114-120, 116-118, 116-120, or 118-120. In particular, in some aspects, the Young's modulus (GPa) is 90-120, 92-116, 100-120, 92 or more, or 98-120.

[0036] In some aspects, the glasses or glass-ceramics can have a specific modulus (GPa•cm3•g-1) that can be at least 32, at least 32.5, at least 33, at least 33.5, at least 34, at least 34.5, at least 35, at least 35.5, at least 36, at least 36.5, at least 37, at least 37.5, at least 38, at least 38.5, at least 39, at least 39.5, at least 40, 40 or less, 39.5 or less, 39 or less, 38.5 or less, 38 or less, 37.5 or less, 37 or less, 36.5 or less, 36 or less, 35.5 or less, 35 or less, 34.5 or less, 34 or less, 33.5 or less, 33 or less, 32.5 or less, 32 or less, or any range formed from any two of the foregoing endpoints. For example, in some aspects, the specific modulus (GPa•cm3•g-1) can be 32-32.5, 32-33, 32-33.5, 32-34, 32-34.5, 32- 35, 32-35.5, 32-36, 32-36.5, 32-37, 32-37.5, 32-38, 32-38.5, 32-39, 32-39.5, 32-40, 32.5-33, 32.5- 33.5, 32.5-34, 32.5-34.5, 32.5-35, 32.5-35.5, 32.5-36, 32.5-36.5, 32.5-37, 32.5-37.5, 32.5-38, 32.5- 38.5, 32.5-39, 32.5-39.5, 32.5-40, 33-33.5, 33-34, 33-34.5, 33-35, 33-35.5, 33-36, 33-36.5, 33-37, 33- 37.5, 33-38, 33-38.5, 33-39, 33-39.5, 33-40, 33.5-34, 33.5-34.5, 33.5-35, 33.5-35.5, 33.5-36, 33.5- 36.5, 33.5-37, 33.5-37.5, 33.5-38, 33.5-38.5, 33.5-39, 33.5-39.5, 33.5-40, 34-34.5, 34-35, 34-35.5, 34- 36, 34-36.5, 34-37, 34-37.5, 34-38, 34-38.5, 34-39, 34-39.5, 34-40, 34.5-35, 34.5-35.5, 34.5-36, 34.5- 36.5, 34.5-37, 34.5-37.5, 34.5-38, 34.5-38.5, 34.5-39, 34.5-39.5, 34.5-40, 35-35.5, 35-36, 35-36.5, 35- 37, 35-37.5, 35-38, 35-38.5, 35-39, 35-39.5, 35-40, 35.5-36, 35.5-36.5, 35.5-37, 35.5-37.5, 35.5-38,35.5-38.5, 35.5-39, 35.5-39.5, 35.5-40, 36-36.5, 36-37, 36-37.5, 36-38, 36-38.5, 36-39, 36-39.5, 36-40, 36.5-37, 36.5-37.5, 36.5-38, 36.5-38.5, 36.5-39, 36.5-39.5, 36.5-40, 37-37.5, 37-38, 37-38.5, 37-39, 37-39.5, 37-40, 37.5-38, 37.5-38.5, 37.5-39, 37.5-39.5, 37.5-40, 38-38.5, 38-39, 38-39.5, 38-40,38.5-39, 38.5-39.5, 38.5-40, 39-39.5, 39-40, or 39.5-40. In particular, in some aspects, the specific modulus (GPa•cm3•g-1) is 32-40, 33-38, or 31.5-39.

[0037] In some aspects, the glasses or glass-ceramics can have a strain point (°C) that can be at least 590, at least 595, at least 600, at least 605, at least 610, at least 615, at least 620, at least 625, at least 630, at least 635, at least 640, at least 645, at least 650, at least 655, at least 660, 660 or less, 655 or less, 650 or less, 645 or less, 640 or less, 635 or less, 630 or less, 625 or less, 620 or less, 615 or less, 610 or less, 605 or less, 600 or less, 595 or less, 590 or less, or any range formed from any two of the foregoing endpoints. For example, in some aspects, the strain point (°C) can be 590-595, 590-600, 590-605, 590-610, 590-615, 590-620, 590-625, 590-630, 590-635, 590-640, 590-645, 590-650, 590-655, 590-660, 595-600, 595-605, 595-610, 595-615, 595-620, 595-625, 595-630, 595-635, 595-640, 595-645, 595-650, 595-655, 595-660, 600-605, 600-610, 600-615, 600-620, 600-625, 600-630, 600-635, 600-640, 600-645, 600-650, 600-655, 600-660, 605-610, 605-615, 605-620, 605-625, 605-630, 605-635, 605-640, 605-645, 605-650, 605-655, 605-660, 610-615, 610-620, 610-625, 610-630, 610-Attorney Docket No. SP25-087 PCT635, 610-640, 610-645, 610-650, 610-655, 610-660, 615-620, 615-625, 615-630, 615-635, 615-640, 615-645, 615-650, 615-655, 615-660, 620-625, 620-630, 620-635, 620-640, 620-645, 620-650, 620-655, 620-660, 625-630, 625-635, 625-640, 625-645, 625-650, 625-655, 625-660, 630-635, 630-640, 630-645, 630-650, 630-655, 630-660, 635-640, 635-645, 635-650, 635-655, 635-660, 640-645, 640-650, 640-655, 640-660, 645-650, 645-655, 645-660, 650-655, 650-660, or 655-660. In particular, in some aspects, the strain point (°C) is 590-660, 605-660, or 610-645. The strain point is measured according to bending beam viscosity (BBV).

[0038] In some aspects, the glasses or glass-ceramics can have a anneal point (°C) that can be at least 630, at least 635, at least 640, at least 645, at least 650, at least 655, at least 660, at least 665, at least 670, at least 675, at least 680, at least 685, at least 690, at least 695, at least 700, 700 or less, 695 or less, 690 or less, 685 or less, 680 or less, 675 or less, 670 or less, 665 or less, 660 or less, 655 or less, 650 or less, 645 or less, 640 or less, 635 or less, 630 or less, or any range formed from any two of the foregoing endpoints. For example, in some aspects, the anneal point (°C) can be 630-635, 630-640, 630-645, 630-650, 630-655, 630-660, 630-665, 630-670, 630-675, 630-680, 630-685, 630-690, 630-695, 630-700, 635-640, 635-645, 635-650, 635-655, 635-660, 635-665, 635-670, 635-675, 635-680, 635-685, 635-690, 635-695, 635-700, 640-645, 640-650, 640-655, 640-660, 640-665, 640-670, 640-675, 640-680, 640-685, 640-690, 640-695, 640-700, 645-650, 645-655, 645-660, 645-665, 645-670, 645-675, 645-680, 645-685, 645-690, 645-695, 645-700, 650-655, 650-660, 650-665, 650-670, 650-675, 650-680, 650-685, 650-690, 650-695, 650-700, 655-660, 655-665, 655-670, 655-675, 655-680, 655-685, 655-690, 655-695, 655-700, 660-665, 660-670, 660-675, 660-680, 660-685, 660-690, 660-695, 660-700, 665-670, 665-675, 665-680, 665-685, 665-690, 665-695, 665-700, 670-675, 670-680, 670-685, 670-690, 670-695, 670-700, 675-680, 675-685, 675-690, 675-695, 675-700, 680-685, 680-690, 680-695, 680-700, 685-690, 685-695, 685-700, 690-695, 690-700, or 695-700. In particular, in some aspects, the anneal point (°C) is 630-700, 650-680, or 640-690. The anneal point is measured according to bending beam viscosity (BBV).

[0039] In some aspects, the glasses or glass-ceramics can have a platinum interface liquidus temperature (°C) that can be at least 1100, at least 1150, at least 1200, at least 1250, at least 1300, at least 1350, at least 1400, at least 1450, at least 1500, 1500 or less, 1450 or less, 1400 or less, 1350 or less, 1300 or less, 1250 or less, 1200 or less, 1150 or less, 1100 or less, or any range formed from any two of the foregoing endpoints. For example, in some aspects, the platinum interface liquidus temperature (°C) can be 1100-1150, 1100-1200, 1100-1250, 1100-1300, 1100-1350, 1100-1400, 1100-1450, 1100-1500, 1150-1200, 1150-1250, 1150-1300, 1150-1350, 1150-1400, 1150-1450, 1150-1500, 1200-1250, 1200-1300, 1200-1350, 1200-1400, 1200-1450, 1200-1500, 1250-1300, 1250-1350, 1250-1400, 1250-1450, 1250-1500, 1300-1350, 1300-1400, 1300-1450, 1300-1500, 1350-1400, 1350-1450, 1350-1500, 1400-1450, 1400-1500, or 1450-1500. In particular, in some aspects, the platinum interface liquidus temperature (°C) is 1100-1500, 1150-1400, or 1100-1400. The platinum interfaceAttomey Docket No. SP25-087 PCTliquidus temperature is measured according to the gradient boat liquidus method of ASTM C829-81 (2015).

[0040] In some aspects, any of the glasses disclosed herein are in the form of a glass fiber. Glass fibers are widely employed to reinforce composite materials, providing enhanced strength and durability while maintaining a flexible form factor. These fibers are utilized across various industries to create stiff composites that withstand demanding conditions. In aerospace and defense, glass fibers are integral to constructing components that require durability and lightweight properties. In the automotive sector, they are used to reinforce parts for improved safety and performance. The energy generation industry benefits from glass fiber-reinforced composites in applications such as wind turbine blades and pressurized tanks for hydrogen storage, where strength and reliability are crucial. Additionally, glass fibers find applications in architectural structures, sporting goods, and electronics packaging, where they contribute to superior mechanical properties and resilience. In some aspects, the glass fibers are used to strengthen a material, such as a polymer matrix. In some aspects, the glass fibers can be embedded in a polymer matrix. All of the disclosures herein with respect to the compositions and properties for the glasses are equally applicable to the compositions and properties of the glass fibers.

[0041] In some aspects, the glass fibers have an average diameter of 100 microns or less. In some aspects, the glass fibers can have an average diameter (microns) that can be at least 5, at least 9, at least 10, at least 15, at least 20, at least 25, at least 30, at least 35, at least 40, at least 45, at least 50, at least 55, at least 60, at least 65, at least 70, at least 75, at least 80, at least 85, at least 90, at least 95, at least 100, 100 or less, 95 or less, 90 or less, 85 or less, 80 or less, 75 or less, 70 or less, 65 or less, 60 or less, 55 or less, 50 or less, 45 or less, 40 or less, 35 or less, 30 or less, 25 or less, 20 or less, 15 or less, 10 or less, 9 or less, 5 or less, or any range formed from any two of the foregoing endpoints. For example, in some aspects, the average diameter (microns) can be 5-9, 5-10, 5-15, 5-20, 5-25, 5-30, 5-35, 5-40, 5-45, 5-50, 5-55, 5-60, 5-65, 5-70, 5-75, 5-80, 5-85, 5-90, 5-95, 5-100, 9-10, 9-15, 9-20, 9-25, 9-30, 9-35, 9-40, 9-45, 9-50, 9-55, 9-60, 9-65, 9-70, 9-75, 9-80, 9-85, 9-90, 9-95, 9-100, 10-15, 10-20, 10-25, 10-30, 10-35, 10-40, 10-45, 10-50, 10-55, 10-60, 10-65, 10-70, 10-75, 10-80, 10-85, 10-90, 10-95, 10-100, 15-20, 15-25, 15-30, 15-35, 15-40, 15-45, 15-50, 15-55, 15-60, 15-65, 15-70, 15-75, 15-80, 15-85, 15-90, 15-95, 15-100, 20-25, 20-30, 20-35, 20-40, 20-45, 20-50, 20-55, 20-60, 20-65, 20-70, 20-75, 20-80, 20-85, 20-90, 20-95, 20-100, 25-30, 25-35, 25-40, 25-45, 25-50, 25-55, 25- 60, 25-65, 25-70, 25-75, 25-80, 25-85, 25-90, 25-95, 25-100, 30-35, 30-40, 30-45, 30-50, 30-55, 30- 60, 30-65, 30-70, 30-75, 30-80, 30-85, 30-90, 30-95, 30-100, 35-40, 35-45, 35-50, 35-55, 35-60, 35- 65, 35-70, 35-75, 35-80, 35-85, 35-90, 35-95, 35-100, 40-45, 40-50, 40-55, 40-60, 40-65, 40-70, 40- 75, 40-80, 40-85, 40-90, 40-95, 40-100, 45-50, 45-55, 45-60, 45-65, 45-70, 45-75, 45-80, 45-85, 45-90, 45-95, 45-100, 50-55, 50-60, 50-65, 50-70, 50-75, 50-80, 50-85, 50-90, 50-95, 50-100, 55-60, 55-65, 55-70, 55-75, 55-80, 55-85, 55-90, 55-95, 55-100, 60-65, 60-70, 60-75, 60-80, 60-85, 60-90, 60-95, 60-100, 65-70, 65-75, 65-80, 65-85, 65-90, 65-95, 65-100, 70-75, 70-80, 70-85, 70-90, 70-95, 70-Attomey Docket No. SP25-087 PCT100, 75-80, 75-85, 75-90, 75-95, 75-100, 80-85, 80-90, 80-95, 80-100, 85-90, 85-95, 85-100, 90-95, 90-100, or 95-100. In particular, in some aspects, the average diameter (microns) is 100 or less, 9-25, 5-100, or 5-50.

[0042] In some aspects, disclosed is a method for making glass fibers. In some aspects, the method comprises: providing a mixture comprising (1) natural basalt rock, and (2) a source of Ti and optionally additional components (e.g., a source of SrO, ZrO2, Cu, ZnO, V2O5, Cr, CoO, Nb2O5, La2O3. Y2O3, Li2O. Mn, or any combination thereof); heating the mixture to produce a melt; and drawing the glass fibers from the melt. In some aspects, the glass fibers comprise any of the glass compositions disclosed herein. In particular, in some aspects, the glass fibers comprise 3-9.3 mol.% AI2O3; 6.9-14 mol.% CaO; 3-5 mol.% Fe; 0-4 mol.% K2O; 11.3-35 mol.% MgO; 0-0.15 mol.% Mn; 0-3 mol.% Na2O; 35-65 mol.% SiO2; and 0.1-15 mol.% Ti; wherein Fe is iron in any oxidation state that is assumed to be present as Fe2O3. Ti is titanium in any oxidation state that is assumed to be present as TiO2, Mn is manganese in any oxidation state that is assumed to be present as MnO2, Cu is copper in any oxidation state that is assumed to be present as CuO, and Cr is chromium in any oxidation state that is assumed to be present as Cr2O3.

[0043] In some aspects, the natural basalt rock has any suitable average largest dimension. In some aspects, the average largest dimension is any value that facilitates combining the rock with one or more additives, such as a source of Ti, and melting to form a melt. For example, in some aspects, the average largest dimension is from 1 micron, to a few millimeters, or to a few centimeters. In particular, in some aspects, the average largest dimension is 1-500 microns, 0.5-5 mm, or 0.5-5 cm. The size is not particularly limited.

[0044] In some aspects, the heating step for making glass fibers is generally any temperature that is sufficient to melt the mixture. Such temperatures can range from 950-1300 °C. Higher temperatures can be employed if desired, though typically there is no need as a higher temperature than needed to produce a melt merely increases costs without any benefit.

[0045] In some aspects, any suitable drawing temperature can be employed when drawing glass fibers. Once a melt is formed, the temperature can be adjusted so as to provide a molten glass with a suitable viscosity for drawing, provided that the molten glass is not cooled below the liquidus temperature. In some aspects, the drawing temperature (°C) can be at least 78, at least 850, at least 900, at least 950, at least 1000, at least 1050, at least 1100, at least 1150, at least 1200, at least 1250, at least 1300, at least 1350, at least 1400, 1400 or less, 1350 or less, 1300 or less, 1250 or less, 1200 or less, 1150 or less, 1100 or less, 1050 or less, 1000 or less, 950 or less, 900 or less, 850 or less, 78 or less, or any range formed from any two of the foregoing endpoints. For example, in some aspects, the drawing temperature (°C) can be 78-850, 78-900, 78-950, 78-1000, 78-1050, 78-1100, 78-1150, 78-1200, 78-1250, 78-1300, 78-1350, 78-1400, 850-900, 850-950, 850-1000, 850-1050, 850-1100, 850-1150, 850-1200, 850-1250, 850-1300, 850-1350, 850-1400, 900-950, 900-1000, 900-1050, 900-1100, 900-1150, 900-1200, 900-1250, 900-1300, 900-1350, 900-1400, 950-1000, 950-1050, 950-1100, 950-Attorney Docket No. SP25-087 PCT1150, 950-1200, 950-1250, 950-1300, 950-1350, 950-1400, 1000-1050, 1000-1100, 1000-1150, 1000-1200, 1000-1250, 1000-1300, 1000-1350, 1000-1400, 1050-1100, 1050-1150, 1050-1200, 1050-1250, 1050-1300, 1050-1350, 1050-1400, 1100-1150, 1100-1200, 1100-1250, 1100-1300, 1100-1350, 1100-1400, 1150-1200, 1150-1250, 1150-1300, 1150-1350, 1150-1400, 1200-1250, 1200-1300, 1200-1350, 1200-1400, 1250-1300, 1250-1350, 1250-1400, 1300-1350, 1300-1400, or 1350-1400. In particular, in some aspects, the drawing temperature (°C) is 850-1400, 850-1300, or 900-1250.

[0046] Various aspects are contemplated herein, several of which are set forth in the paragraphs below. It is explicitly contemplated that any aspect or portion thereof can be combined to form a combination. The phrase “any other aspect herein” means any numbered aspect herein, or any aspect or aspects disclosed elsewhere herein.

[0047] Aspect 1. A glass, comprising:3-9.3 mol.% Al2O3;6.9-14 mol.% CaO;3-5 mol.% Fe;0-4 mol.% K2O;11.3-35 mol.% MgO;0-0.15 mol.% Mn;0-3 mol.% Na2O;35-65 mol.% SiO2; and1-15 mol.% Ti;wherein the Fe is iron in any oxidation state that is assumed to be present as Fe2O3, the Ti is titanium in any oxidation state that is assumed to be present as TiO2, and the Mn is manganese in any oxidation state that is assumed to be present as MnO2.

[0048] Aspect 2. The glass of aspect 1, or any other aspect herein, comprising a Young’s modulus of 90-120 GPa.

[0049] Aspect 3. The glass of any one of aspects 1-2, or any other aspect herein, comprising a specific modulus of 32-40 GPa•cm3•g-1.

[0050] Aspect 4. The glass of any one of aspects 1-3, or any other aspect herein, further comprising P2O5.

[0051] Aspect 5. The glass of any preceding claim, wherein the AI2O3, CaO, Fe, K2O, MgO, SiO2, or any combination thereof are present in at least one of the following amounts:4-9 mol.% AI2O3;7-13 mol.% CaO;3.5-4.5 mol.% Fe;0-2 mol.% K2O;11.5-32 mol.% MgO;42-60 mol.% SiO2;Attorney Docket No. SP25-087 PCTany combination thereof.

[0052] Aspect 6. The glass of any one of aspects 1-5, or any other aspect herein, wherein the Ti is present in an amount of 2-10 mol.%.

[0053] Aspect 7. The glass of any one of aspects 1-6, or any other aspect herein, wherein Fe / Ti is 0.1-3.

[0054] Aspect 8. The glass of any one of aspects 1-7, or any other aspect herein, further comprising at least one of SrO, ZrO2, Cu, ZnO, V2O5, Cr, CoO, Nb2O5, La2O3, Y2O3, and Li2O, wherein the Cu is copper in any oxidation state that is assumed to be present as CuO, and the Cr is chromium in any oxidation state that is assumed to be present as C’ Ch.

[0055] Aspect 9. The glass of any one of aspects 1-8, or any other aspect herein, comprising a strain point of 590-660 °C, as measured according to bending beam viscosity (BBV).

[0056] Aspect 10. The glass of any one of aspects 1-9, or any other aspect herein, comprising an anneal point of 630-700 °C, as measured according to bending beam viscosity (BBV).

[0057] Aspect 11. The glass of any one of aspects 1-10, or any other aspect herein, comprising a platinum interface liquidus temperature of 1100-1500 °C, as measured according to the gradient boat liquidus method of ASTM C829-81 (2015).

[0058] Aspect 12. A glass fiber comprising the glass of any one of aspects 1-11, or any other aspect herein.

[0059] Aspect 13. The glass fiber of aspect 12, any preceding aspects, or any other aspect herein, comprising an average diameter of 100 pm or less.

[0060] Aspect 14. A composite comprising the glass fiber of aspect 12 or 13, any preceding aspect, or any other aspect herein, embedded in a polymer matrix.

[0061] Aspect 15. A method for making glass fibers, the method comprising:providing a mixture comprising (1) natural basalt rock, and (2) a source of Ti; heating the mixture to produce a melt; anddrawing the glass fibers from the melt;wherein the glass fibers comprise:3-9.3 mol.% AI2O3;6.9-14 mol.% CaO;3-5 mol.% Fe;0-4 mol.% K2O;11.3-35 mol.% MgO;0-0.15 mol.% Mn;0-3 mol.% Na2O;35-65 mol.% SiO2; and0.1-15 mol.% Ti;Attorney Docket No. SP25-087 PCTwherein the Fe is iron in any oxidation state that is assumed to be present as Fe2O3. the Ti is titanium in any oxidation state that is assumed to be present as TiC and the Mn is manganese in any oxidation state that is assumed to be present as MnCh.

[0062] Aspect 16. The method of aspect 15, any preceding aspect, or any other aspect herein, wherein the drawing is conducted at a temperature of 850-1400 °C.

[0063] Aspect 17. The method of aspect 15 or 16, any preceding aspect, or any other aspect herein, wherein the glass fibers comprise a Young’s modulus of 90-120 GPa.

[0064] Aspect 18. The method of any one of aspects 15-17, any preceding aspect, or any other aspect herein, wherein the glass fibers comprise a specific modulus of 32-40 GPa•cm3•g-1.

[0065] Aspect 19. The method of any one of aspects 15-18, any preceding aspect, or any other aspect herein, wherein the glass fibers further comprise P2O5.

[0066] Aspect 20. The method of any one of aspects 15-19, any preceding aspect, or any other aspect herein, wherein the glass fibers comprise the AI2O3, CaO, Fe, K2O, MgO, SiC>2, or any combination thereof in at least one of the following amounts:4-9 mol.% AI2O3;7-13 mol.% CaO;3.5-4.5 mol.% Fe;0-1 mol.% K2O;11.5-32 mol.% MgO;42-60 mol.% SiO2;any combination thereof.

[0067] Aspect 21. The method of any one of aspects 15-20, any preceding aspect, or any other aspect herein, wherein the glass fibers comprise the Ti in an amount of 1-10 mol.%.

[0068] Aspect 22. The method of any one of aspects 15-21, any preceding aspect, or any other aspect herein, wherein the glass fibers comprise a ratio Fe / Ti of 0.1-3.

[0069] Aspect 23. The method of any one of aspects 15-22, any preceding aspect, or any other aspect herein, wherein the glass fibers further comprise at least one of SrO, ZrO2, Cu, ZnO, V2O5, Cr, CoO, Nb2O5, La2C>3, Y2O3, and Li2O, wherein the Cu is copper in any oxidation state that is assumed to be present as CuO, and the Cr is chromium in any oxidation state that is assumed to be present as Cr2O3.

[0070] Aspect 24. The method of any one of aspects 15-23, any preceding aspect, or any other aspect herein, wherein the glass fibers comprise at least one of:a strain point of 590-660 °C, as measured according to bending beam viscosity (BBV);an anneal point of 630-700 °C, as measured according to bending beam viscosity (BBV);Attorney Docket No. SP25-087 PCTa platinum interface liquidus temperature 1100-1500 °C, as measured according to the gradient boat liquidus method of ASTM C829-81 (2015).

[0071] Aspect 25: A combination of any two or more preceding aspects or any portion(s) thereof.EXAMPLES

[0072] The following examples illustrate non-limiting aspects of the disclosure and are not intended to be limiting on the scope of the disclosure or claims.

[0073] The Poisson’s ratio (v), the Young’s modulus (E), and the shear modulus (G) of the glass compositions were measured by a resonant ultrasonic spectroscopy technique of the general type set forth in ASTM E2001-13, titled “Standard Guide for Resonant Ultrasound Spectroscopy for Defect Detection in Both Metallic and Non-metallic Parts.” The specific modulus (GPa•cm3•g-1)) is calculated by dividing the Young’s modulus (GPa) by the density (g / cm3). The density of the glass compositions was determined using the buoyancy method of ASTM C693-93(2013).

[0074] The term “annealing point,” as used herein, refers to the temperature at which the viscosity of the glass composition is 1×1013.18poise. The term “strain point,” as used herein, refers to the temperature at which the viscosity of the glass composition is 1×1014.68poise. The strain point and annealing point of the glass compositions was determined using the fiber elongation (FE) method of ASTM C336-71(2015) or the beam bending viscosity (BBV) method of ASTM C598-93(2013).

[0075] The term “liquidus viscosity” refers to the viscosity of a molten glass at the liquidus temperature, wherein the “liquidus temperature” refers to the temperature at which crystals first appear as a molten glass cools down from the melting temperature, or the temperature at which the very last crystals melt away as temperature is increased from room temperature. The platinum interface liquidus temperature of the glasses herein were measured using the standard gradient boat liquidus method of ASTM C829-81 (2015). This involves placing crushed glass particles in a platinum boat, placing the boat in a furnace having a region of gradient temperatures, heating the boat in an appropriate temperature region for 24 hours, and determining by means of microscopic examination the highest temperature at which crystals appear at the platinum interface. More particularly, the glass sample is removed from the Pt boat in one piece, and examined using polarized light microscopy to identify the location and nature of crystals which have formed against the Pt interface and the temperature of the Pt interface when crystals form. Because the gradient of the furnace is very well known, temperature vs. location can be well estimated, within 5-10 °C. If desired, testing may be carried out at longer times (e.g., 72 hours) to observe slower growing phases. The liquidus viscosity (poise) was determined from the liquidus temperature.Example 1

[0076] This example demonstrates the preparation of basalt-type glasses and drawing fibers.Attorney Docket No. SP25-087 PCT

[0077] All of the glasses in Table 2 were prepared by standard crucible melting methods and are reported in Table 2 as batched. These glasses were prepared by crushing the relevant natural basalt rock shown in Table 1, adding raw materials (e.g., source of titanium oxide for all glasses) to the natural basalt rock to form a mixture that when melted and cooled achieves a desired target composition, heating the mixture in a crucible at 1550 °C for a time period sufficient to form a molten mixture, and then pouring the molten mixture onto a surface to cool. While 1550 °C was used for melting, this temperature was higher than needed and was employed only for demonstration purposes (i.e., a lower temperature may be employed if desired). The natural basalt rocks in Table 1 were also melted into glasses by standard crucible melting methods, though basalt B3 did not form a glass. The resulting glasses were analyzed for various properties and are reported in Table 1 and Table 2. Certain glasses in Table 1 and Table 2 were also drawn into fibers using standard drawing techniques at temperatures between about 900-1250 °C. While fiber drawing conditions were not necessarily optimized for these experiments, it is contemplated that various optimizations can be performed to obtain drawable fibers.Table 1Attorney Docket No. SP25-087 PCTfFe is iron in any oxidation state that is assumed to be present as Fe2O3. Ti is titanium in any oxidation state that is assumed to be present as TiO2, and Mn is manganese in any oxidation state that is assumed to be present as MnO2Table 2Attorney Docket No. SP25-087 PCTfFe is iron in any oxidation state that is assumed to be present as Fe2O3. Ti is titanium in any oxidation state that is assumed to be present as TiO2and Mn is manganese in any oxidation state that is assumed to be present as MnO2

[0078] The Young’s modulus was plotted against the specific modulus in FIG. 1 for the glasses of Table 2 compared to the industry standard E, S, and R shown in Table 3, as well as basalts Bl, B2, and B4 shown in Table 1. As can be seen in FIG. 1, the glasses of Table 2 have higher modulus than the industry standard glasses (E, S, and R glasses), all while maintaining similar specific modulus. InAttorney Docket No. SP25-087 PCTaddition, the glasses of Table 2 generally have a higher Young’s modulus than the glasses made from basalts Bl, B2, and B4, while generally being easier to melt and draw into fibers.Table 3

[0079] Whenever a group is described as comprising at least one of a group of elements and combinations thereof, it is understood that the group may comprise, consist essentially of, or consist of any number of those elements recited, either individually or in combination with each other. Similarly, whenever a group is described as consisting of at least one of a group of elements or combinations thereof, it is understood that the group may consist of any number of those elements recited, either individually or in combination with each other. Further, while various features, elements, or steps of particular aspects or embodiments may be disclosed using the transitional phrase “comprising,” it is intended that alternative aspects or embodiments, including those that may be described using the transitional phrases “consisting of’ or “consisting essentially of,” are implied. Thus, for example, implied alternative aspects or embodiments to a device that comprises A+B+C include aspects or embodiments where a device consists of A+B+C and aspects or embodiments where a device consists essentially of A+B+C.

[0080] As used herein, the term “and / or,” when used in a list of two or more items, means that any one of the listed items can be employed by itself, or any combination of two or more of the listed items can be employed. For example, if a composition is described as containing components A, B, and / or C, the composition can contain A alone; B alone; C alone; A and B in combination; A and C in combination; B and C in combination; or A, B, and C in combination.

[0081] Where a range of numerical values is recited herein, comprising upper and lower values, unless otherwise stated in specific circumstances, the range is intended to include the endpointsAttorney Docket No. SP25-087 PCTthereof, and all integers, fractions, and decimals within the range. Further, when an amount, concentration, or other value or parameter is given as a range, one or more ranges, or a list of upper values and lower values, this is to be understood as specifically disclosing all ranges formed from any pair of any upper range limit or value and any lower range limit or value, regardless of whether such pairs are separately disclosed.

[0082] It will be appreciated that the various disclosed aspects or embodiments may involve particular features, elements or steps that are described in connection with that particular aspect or embodiment. It will also be appreciated that a particular feature, element, or step, although described in relation to one particular aspect or embodiment, may be interchanged or combined with alternate aspects or embodiments in various non-illustrated combinations or permutations.

[0083] References herein to the positions of elements (e.g., “top,” “bottom,” “above,” “below,” “first,” “second,” etc.) are merely used to describe the orientation of various elements in the FIGURES. It should be noted that the orientation of various elements may differ according to other exemplary embodiments, and that such variations are intended to be encompassed by the present disclosure. Moreover, these relational terms are used solely to distinguish one entity or action from another entity or action, without necessarily requiring or implying any actual such relationship or order between such entities or actions.

[0084] As utilized herein, “optional,” “optionally,” or the like are intended to mean that the subsequently described component, event, or circumstance can or cannot occur or be present, and that the description includes instances where the component, event, or circumstance occurs / is present and instances where it does not occur / is not present. As used herein, the indefinite articles “a,” “an,” and the corresponding definite article “the” mean “at least one” or “one or more,” unless otherwise specified. It also is understood that the various features disclosed in the specification and the drawings can be used in any and all combinations.

[0085] With respect to the use of substantially any plural and / or singular terms herein, those having skill in the art can translate from the plural to the singular and / or from the singular to the plural as is appropriate to the context and / or application. The various singular / plural permutations may be expressly set forth herein for the sake of clarity.

[0086] The term “substantially” may be utilized herein to represent the inherent degree of uncertainty that may be attributed to any quantitative or qualitative comparison, value, measurement, or other representation. This term is also utilized herein to represent the degree by which a quantitative or qualitative representation may vary from a stated reference without resulting in a change in the basic character or function of the subject matter at issue. Thus, for example, a composition that is “substantially free” of any specific component (e.g., AI2O3, MgO, or any other component) is one in which the component is not actively added or batched into the composition, but may be present in small amounts as a contaminant (e.g., less than 1000, 500, 400, 300, 200, or 100 ppm), or, if actively added or batched, is present in an amount less than 1 wt.% (e.g., or can beAttorney Docket No. SP25-087 PCTspecified to be less than 0.5 wt.%, 0.1 wt.%, or 0.05 wt.%.), based on total amount of the composition (moles or mass for ppm, and mass for wt.%). Similarly, for example, a surface of a glass-based substrate or article that is “substantially planar” is one in which there may be slight deviations from planarity, but the overall character and function of the surface is unaffected by such deviations for the purposes of the surface being planar.

[0087] It will be apparent to those ordinarily skilled in the art that various modifications and variations can be made to the present disclosure without departing from the spirit and scope of the disclosure. Since modifications combinations, sub-combinations, and variations of the disclosed embodiments incorporating the spirit and substance of the disclosure may occur to persons ordinarily skilled in the art, the disclosure should be construed to include everything within the scope of the appended claims and their equivalents.

Claims

Attorney Docket No. SP25-087 PCTWHAT IS CLAIMED IS:

1. A glass, comprising:3-9.3 mol.% AI2O3;6.9-14 mol.% CaO;3-5 mol.% Fe;0-4 mol.% K2O;11.3-35 mol.% MgO;0-0.15 mol.% Mn;0-3 mol.% Na2O;35-65 mol.% SiO2; and1-15 mol.% Ti;wherein the Fe is iron in any oxidation state that is assumed to be present as Fe2O3, the Ti is titanium in any oxidation state that is assumed to be present as TiO2, and the Mn is manganese in any oxidation state that is assumed to be present as MnO2.

2. The glass of any preceding claim, comprising a Young’s modulus of 90-120 GPa.

3. The glass of any preceding claim, comprising a specific modulus of 32-40 GPa*cm3«g-1.

4. The glass of any preceding claim, further comprising P2O5.

5. The glass of any preceding claim, wherein the AI2O3, CaO, Fe, K2O, MgO, SiO2, or any combination thereof are present in at least one of the following amounts:4-9 mol.% AI2O3;7-13 mol.% CaO;3.5-4.5 mol.% Fe;0-2 mol.% K2O;11.5-32 mol.% MgO;42-60 mol.% SiO2;any combination thereof.

6. The glass of any preceding claim, wherein the Ti is present in an amount of 2-10 mol.%.

7. The glass of any preceding claim, wherein Fe / Ti is 0.1-3.

8. The glass of any preceding claim, further comprising at least one of SrO, ZrO2, Cu, ZnO,V2O5, Cr, CoO, Nb2O5, La2O3, Y2O3, and Li2O, wherein the Cu is copper in any oxidation state that is assumed to be present as CuO, and the Cr is chromium in any oxidation state that is assumed to be present as Cr2O3.Attorney Docket No. SP25-087 PCT9. The glass of any preceding claim, comprising a strain point of 590-660 °C, as measured according to bending beam viscosity (BBV).

10. The glass of any preceding claim, comprising an anneal point of 630-700 °C, as measured according to bending beam viscosity (BBV).

11. The glass of any preceding claim, comprising a platinum interface liquidus temperature of1100-1500 °C, as measured according to the gradient boat liquidus method of ASTM C829-81 (2015).

12. A glass fiber comprising the glass of any preceding claim.

13. The glass fiber of claim 12, comprising an average diameter of 100 pm or less.

14. A composite comprising the glass fiber of claim 12 or 13 embedded in a polymer matrix.

15. A method for making glass fibers, the method comprising:providing a mixture comprising (1) natural basalt rock, and (2) a source of Ti; heating the mixture to produce a melt; anddrawing the glass fibers from the melt;wherein the glass fibers comprise:3-9.3 mol.% Al2O3;6.9-14 mol.% CaO;3-5 mol.% Fe;0-4 mol.% K2O;11.3-35 mol.% MgO;0-0.15 mol.% Mn;0-3 mol.% Na2O;35-65 mol.% SiO2; and0.1-15 mol.% Ti;wherein the Fe is iron in any oxidation state that is assumed to be present as Fe2O3. the Ti is titanium in any oxidation state that is assumed to be present as TiCK and the Mn is manganese in any oxidation state that is assumed to be present as MnC>2.

16. The method of claim 15, wherein the drawing is conducted at a temperature of 850-1400 °C.

17. The method of claim 15 or 16, wherein the glass fibers comprise a Young’s modulus of 90-120 GPa.

18. The method of any one of claims 15-17, wherein the glass fibers comprise a specific modulus of 32-40 GPa*cm3*g1.Attorney Docket No. SP25-087 PCT19. The method of any one of claims 15-18, wherein the glass fibers further comprise P2O5.

20. The method of any one of claims 15-19, wherein the glass fibers comprise the AI2O3, CaO, Fe, K2O, MgO, SiC>2, or any combination thereof in at least one of the following amounts:4-9 mol.% AI2O3;7-13 mol.% CaO;3.5-4.5 mol.% Fe;0-1 mol.% K2O;11.5-32 mol.% MgO;42-60 mol.% SiO2;any combination thereof.

21. The method of any one of claims 15-20, wherein the glass fibers comprise the Ti in an amount of 1-10 mol.%.

22. The method of any one of claims 15-21, wherein the glass fibers comprise a ratio Fe / Ti of 0.1-3.

23. The method of any one of claims 15-22, wherein the glass fibers further comprise at least one of SrO, ZrC>2, Cu, ZnO, V2O5, Cr, CoO, Nb2O5, La2O3, Y2O3, and Li2O, wherein the Cu is copper in any oxidation state that is assumed to be present as CuO, and the Cr is chromium in any oxidation state that is assumed to be present as C^Ch.

24. The method of any one of claims 15-23, wherein the glass fibers comprise at least one of:a strain point of 590-660 °C, as measured according to bending beam viscosity (BBV);an anneal point of 630-700 °C, as measured according to bending beam viscosity (BBV);a platinum interface liquidus temperature 1100-1500 °C, as measured according to the gradient boat liquidus method of ASTM C829-81 (2015).