Photocurable INKS for automotive interior applications
A UV curable ink composition with defined components forms an opaque layer on automotive display glass with high adhesion and optical density, addressing throughput and adhesion issues in existing inks, ensuring durability and performance.
Patent Information
- Application Number
- PCT/US2026/025754
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-16
- Filing Date
- 2026-04-29
- Publication Date
- 2026-11-19
AI Technical Summary
Existing inks for decorating automotive display cover glass suffer from low throughput, inadequate adhesion, and undesirable optical density, making them unsuitable for automotive interior applications.
A UV curable ink composition comprising specific weight percentages of pigment, dispersant, photoinitiators, reactive diluent, and monomers, which forms an opaque layer with high adhesion and optical density on glass substrates after curing, using a process compatible with commercial inkjet printheads.
The ink composition achieves high optical density and adhesion to glass, maintaining a thickness of less than 15 pm with pencil hardness greater than 3H and adhesion greater than 4B, even under varying environmental conditions.
Smart Images

Figure US2026025754_19112026_PF_FP_ABST
Abstract
Description
Attorney Docket No. : SP25-093PCTPHOTOCURABLE INKS FOR AUTOMOTIVE INTERIOR APPLICATIONSCross-Reference To Related Applications
[0001] This application claims the benefit of priority under 35 U.S.C. § 119 of U.S.Provisional Application No. 63 / 807078 filed May 16, 2025, the content of which is incorporated herein by reference in its entirety.Field
[0002] The present specification generally relates to automotive interior glass articles and, in particular, photocurable inks used to form opaque layers on display cover glass having relatively high adhesion to the glass and high optical density.Technical Background
[0003] Automotive interiors may include displays that include a display cover glass. A display module (e.g., a liquid crystal display (“LCD”) module, an organic light emitting diode (“OLED”) display module, or other suitable type of display module) may be laminated to or otherwise integrated with the cover glass such that the cover glass protects the display module and / or provides one or more performance enhancing attributes (e.g., anti-glare or anti -reflective properties) to the display module. A decorative ink may be applied to areas of the cover glass to conceal various components (e.g., electrical and mechanical connections) of the display and / or provide the display with a uniform appearance when the display is powered down. Certain existing inks used for decorating display cover glass may suffer from various deficiencies, such as low throughput, undesirable optical density, and inadequate adhesion, rendering these inks unsuitable for automotive interior applications.
[0004] Accordingly, an alternative ink that meets requirements associated with automotive interior display applications is needed.SUMMARY
[0005] A first aspect (1) of the present disclosure pertains to an ultraviolet curable ink composition comprising, based on a total weight of the ultraviolet curable ink composition: a pigment in an amount greater than or equal to 11 wt% and less than or equal to 20 wt%; aAttorney Docket No. : SP25-093PCTdispersant in an emount greater than or equal to 3 wt% and less than or equal to 10 wt% dispersant; a type I photoinitiator in an amount in a range from 1 wt% to 6 wt%; a type II photoinitiator in an amount in a range from 1 wt% to 6 wt%; an amine synergist in an amount in a range from 1 wt% to 4 wt%; a reactive diluent an an amount greater than or equal to 10 wt% and less than or equal to 42 wt%; a multifunctional monomer in an amount greater than or equal to 2 wt% and less than or equal to 20 wt%; and a total difunctional monomer content that is greater than or equal to 10 wt% and less than or equal to 75 wt%.
[0006] An aspect (2) of the present disclosure pertains to an ultraviolet curable ink composition according to the aspect (1), wherein the total difunctional monomer content is greater than or equal to 50 wt%.
[0007] An aspect (3) of the present disclosure pertains to an ultraviolet curable ink composition according to any of the aspects ( 1 )-(2), wherein the multifunctional monomer is present in an amount less than 5 wt%.
[0008] An aspect (4) of the present disclosure pertains to an ultraviolet curable ink composition according to any of the aspects (l)-(3), wherein the pigment is present in an amount that is less than or equal to 13 wt%.
[0009] An aspect (5) of the present disclosure pertains to an ultraviolet curable ink composition according to any of the aspects ( 1 )-(4), wherein a total monomer content of the ink composition excluding the reactive diluent, calculated by combining amounts of monofunctional monomer, difunctional monomer, and multifunctional monomer in the ink composition, is greater than or equal to 50 wt% and less than or equal to 80 wt%.
[0010] An aspect (6) of the present disclosure pertains to an ultraviolet curable ink composition according to the aspect (5), wherein the reactive diluent consists of one or more A-vinyl monomers, so that the total monomer content excludes the N-vinyl monomers.
[0011] An aspect (7) of the present disclosure pertains to an ultraviolet curable ink composition according to any of the aspects ( 1 )-(6), wherein the multifunctional monomer is present in an amount that is greater than or equal to 4 wt% and less than or equal to 10 wt%.Attorney Docket No. : SP25-093PCT
[0012] An aspect (8) of the present disclosure pertains to an ultraviolet curable ink composition according to any of the aspects (l)-(7), wherein the ultraviolet curable ink composition is free of resin and free of TPO.
[0013] An aspect (9) of the present disclosure pertains to an ultraviolet curable ink composition according to any of the aspects (l)-(8), wherein the ultraviolet curable ink composition exhibits a viscosity greater than or equal to 8 cPs and less than or equal to 15 cPs at a temperature of 45°C.
[0014] An aspect (10) of the present disclosure pertains to a glass article comprising: a glass substrate having a first major surface and a second major surface, the second major surface being opposite the first major surface; and an opaque layer disposed on the second major surface, the opaque layer being a cured layer formed completely of monomeric subunits, wherein: the opaque layer comprises a thickness less than or equal to 15 pm and an optical density greater than or equal to 5.0, and after curing solely via exposure to ultraviolet (“UV”) radiation, the opaque layer exhibits: a pencil hardness greater than or equal to 3H, when measured according to ASTM 3363, and an adhesion to the glass substrate greater than or equal to 4B, after being subjected to a temperature of 85°C at 95% relative humidity for a period of at least 500 hours, when tested according to ASTM 3359.
[0015] An aspect (11) of the present disclosure pertains to a glass article according to the aspect (10), wherein the glass article exhibits: a CIELAB SCI L* value less than or equal to 30, when illuminated at a 10° angle by a D65 illuminant, a CIELAB SCI a* value greater than or equal to -0.05 and less than or equal to 0.15, and a CIELAB SCI b* value greater than or equal to -0.3 and less than or equal to -0.1, when illuminated at a 10° angle by a D65 illuminant.
[0016] An aspect (12) of the present disclosure pertains to a glass article according to any of the aspects (10)-(l 1), wherein after 500 1 hour cycles of being held at a temperature of -40°C for 0.5 hours and a temperature of 95°C for 0.5 hours, the opaque layer exhibits an adhesion to the glass substrate greater than or equal to 4B, when tested according to ASTM 3359, wherein the glass article exhibits a maximum AE value (both SCI and SCE), measured both prior to and after the 500 1 hour cycles, less than 2.0.
[0017] An aspect (13) of the present disclosure pertains to a method of preparing an ink composition comprising: mixing a pigment dispersion with additional components of the ink composition so that the pigment dispersion is contained in the ink composition in an amountAttorney Docket No. : SP25-093PCTin a range from 25 wt% to 50 wt%, wherein the pigment dispersion, prior to the mixing, comprises: a pigment having a particle size of less than 200 nm, the pigment being contained in the pigment dispersion in an amount that is greater than or equal to 25 wt% and less than or equal to 35 wt %; a dispersant in an amount in a range from 10 wt% to 30 wt%; and one or more monomers in an amount in a range from 30 wt% to 70 wt%, wherein the additional components comprise: greater than 0 wt% and less than or equal to 10 wt% of a photoinitiator package, the photoinitiator package comprising a type I photoinitiator, a type II photoinitiator, and an amine synergist; greater than or equal to 10 wt% and less than or equal to 42 wt% of a reactive diluent, the reactive diluent comprising a viscosity less than 5 cPs at 25°C; greater than or equal to 2 wt% and less than or equal to 20 wt% of a multifunctional monomer; and greater than or equal to 0 wt% and less than or equal to 40 wt% of a difunctional monomer, wherein at least one of the one or more monomers in the pigment dispersion is a pigment difunctional monomer such that, after the mixing, the ink composition comprises a total difunctional monomer content that is greater than or equal to 10 wt% and less than or equal to 75 wt%.
[0018] An aspect (14) of the present disclosure pertains to a method according to the aspect (13), wherein, after the mixing, the pigment is present in the ink composition in an amount that is greater than or equal to 11 wt% and less than or equal to 20 wt%.
[0019] An aspect (15) of the present disclosure pertains to a method according to any of the aspects (13)-(14), wherein, the pigment is a carbon black pigment and has a d50 particle size that is greater than or equal to 100 nm and less than or equal to 200 nm.
[0020] An aspect (16) of the present disclosure pertains to a method according to the aspect (15), the d50 particle size is greater than or equal to 160 nm and less than or equal to 180 nm.
[0021] An aspect (17) of the present disclosure pertains to a method according to any of the aspects (13)-(16), wherein the ultraviolet curable ink composition is free of resin and free of TPO.
[0022] An aspect (18) of the present disclosure pertains to a method according to any of the aspects ( 13)-(l 7), wherein, after the mixing, the ultraviolet curable ink composition exhibits a viscosity greater than or equal to 8 cPs and less than or equal to 15 cPs at a temperature ofAttorney Docket No. : SP25-093PCT
[0023] An aspect (19) of the present disclosure pertains to a method according to any of the aspects (13)-(18), wherein: the pigment dispersion comprises from 40 wt% to 70 wt% of the pigment difunctional monomer, and after the mixing, the total difunctional monomer content is greater than or equal to 50 wt%.
[0024] An aspect (20) of the present disclosure pertains to a method according to any of the aspects (13)-(19), wherein, after the mixing, the multifunctional monomer is present in an amount less than 5 wt%.
[0025] An aspect (21) of the present disclosure pertains to a method according to any of the aspects (13)-(20), wherein, after the mixing the pigment is present in an amount that is less than or equal to 13 wt%.
[0026] An aspect (22) of the present disclosure pertains to a method according to any of the aspects (13)-(21), wherein a total monomer content of the ink composition excluding the reactive diluent, calculated by combining amounts of monofunctional monomer, difunctional monomer, and multifunctional monomer in the ink composition, is greater than or equal to 50 wt% and less than or equal to 80 wt%.
[0027] An aspect (23) of the present disclosure pertains to a method according to the aspect (22), wherein the reactive diluent consists of one or more A- vinyl monomers, so that the total monomer content excludes the N-vinyl monomers.
[0028] An aspect (24) of the present disclosure pertains to a method according to any of the aspects (13)-(23), wherein, after the mixing, the multifunctional monomer is present in an amount that is greater than or equal to 4 wt% and less than or equal to 10 wt%.
[0029] An aspect (25) of the present disclosure pertains to a method according to any of the aspects (13)-(24), wherein, prior to the mixing, the pigment dispersion exhibits a viscosity that greater than or equal to 100 cPs is less than or equal to 350 cPs over a temperature range from 30°C to 50°C.
[0030] Additional features and advantages of the photocurable inks and primers and glass articles comprising same described herein will be set forth in the detailed description which follows, and in part will be readily apparent to those skilled in the art from that description orAttorney Docket No. : SP25-093PCTrecognized by practicing the embodiments described herein, including the detailed description which follows, the claims, as well as the appended drawings.
[0031] It is to be understood that both the foregoing general description and the following detailed description describe various embodiments and are intended to provide an overview or framework for understanding the nature and character of the claimed subject matter. The accompanying drawings are included to provide a further understanding of the various embodiments, and are incorporated into and constitute a part of this specification. The drawings illustrate the various embodiments described herein, and together with the description serve to explain the principles and operations of the claimed subject matter.BRIEF DESCRIPTION OF THE DRAWINGS
[0032] FIG. l is a perspective view of a vehicle interior with vehicle interior systems having displays, according to one or more embodiments of the present disclosure;
[0033] FIG. 2 schematically depicts a cross-sectional view of a display of a vehicle interior system through the line 2-2 depicted in FIG. 1, according to one or more embodiments of the present disclosure;
[0034] FIG. 3 depicts a flow diagram of a method of forming a glass article with an opaque layer, according to one or more embodiments of the present disclosure;
[0035] FIG. 4 depicts a plot of viscosity versus temperature for an example pigment dispersion, according to one or more embodiments of the present disclosure;
[0036] FIG. 5 depicts a plot of viscosity versus temperature for an example photocurable ink using the example pigment dispersion represented in FIG. 4, according to one or more embodiments of the present disclosure; and
[0037] FIG. 6 depicts a photograph of a sample formed from the example photocurable ink represented in FIG. 5 after being subjected to a cross-hatch adhesion test, according to one or more embodiments of the present disclosure.DETAILED DESCRIPTION
[0038] Reference will now be made in detail to various embodiments of photocurable inks and ink primers used to form opaque layers on display cover glass having relatively highAttorney Docket No. : SP25-093PCTadhesion to the glass and high optical density. In some embodiments, an ultraviolet ink composition includes, based on a total weight of the ultraviolet curable ink composition, greater than or equal to 25 wt% and less than or equal to 50 wt% of a pigment dispersion, with additional components (above what is included in the pigment dispersion) comprising: greater than 0 wt% and less than or equal to 10 wt% of a photoinitiator package, greater than or equal to 10 wt% and less than or equal to 42 wt% of a reactive diluent, greater than or equal to 2 wt% and less than or equal to 20 wt% of a multifunctional monomer (as used herein, the term “multifunctional” is used to describe a molecule having more than two functional groups), and greater than or equal to 0 wt% and less than or equal to 40 wt% of a difunctional monomer that is added separately from the pigment dispersion. The photoinitiator package includes a type I photoinitiator, a type II photoinitiator, and an amine synergist. The reactive diluent includes a viscosity less than 5 cPs at 25°C.
[0039] In other embodiments, a glass article includes a glass substrate having a first major surface and a second major surface, the second major surface being opposite the first major surface, and an opaque layer disposed on the second major surface. The opaque layer is disposed on the second major surface and includes a photocurable ink including at least 11 wt% of a pigment. The opaque layer is resin free and TPO free. By “resin free,” it is meant that the opaque layer is not formed from an ink composition that contains a polymeric backbone resin therein (pre-cure). As a result, the opaque layer is comprises completely of reactive monomeric subunits. The opaque layer comprises a thickness less than or equal to 15 pm and an optical density greater than or equal to 5.0. After curing solely via exposure to ultraviolet (“UV”) radiation, the opaque layer exhibits a pencil hardness greater than or equal to 3H, when measured according to ASTM 3363, and an adhesion to the glass substrate greater than or equal to 4B, after being subjected to a temperature of 85°C at 95% relative humidity for a period of at least 500 hours, when tested according to ASTM 3359.
[0040] In some embodiments, a method of fabricating a glass article includes, forming an ink composition by mixing a pigment dispersion with additional components of the ink composition, depositing at least one layer of a ultraviolet curable ink composition onto a first major surface of a glass substrate at a deposition temperature less than or equal to 65°C using an inkjet printhead and, using UV light from a UV light source to cure the ultraviolet curable ink composition. During the depositing, the photocurable ink has a viscosity less than 13 cPs. The ultraviolet curable ink composition includes, based on a total weight of the ultraviolet inkAttorney Docket No. : SP25-093PCTcomposition, greater than or equal to 25 wt% and less than or equal to 50 wt% of a pigment dispersion, and additional components (over what is included in the pigment dispersion) greater than 0 wt% and less than or equal to 10 wt% of a photoinitiator package, greater than or equal to 10 wt% and less than or equal to 42 wt% of a reactive diluent, greater than or equal to 2 wt% and less than or equal to 20 wt% of a multifunctional monomer, and greater than or equal to 0 wt% and less than or equal to 40 wt% of a difunctional monomer.
[0041] The photocurable ink compositions described herein may formed by adding the photoinitiator package, reactive diluent, monomers, and any other components to a pigment dispersions that has been produced in a suitable dispermat. The pigment dispersion has a suitably high amount of a pigment to meet the optical density requirements provided herein. The pigment dispersion includes, based on a total weight of the pigment dispersion, at least 25 wt% of a pigment, with the remainder being made up by a dispersant, one or more monomers, and optional additives. For example, the pigment dispersion can contain greater than or equal to 25 wt% and less than or equal to 35% of a suitable pigment (e.g., carbon black) having a particule size less than 200 nm (unless otherwise noted herein, the term “particle size” refers to a d50 particle size). The amount of pigment in the pigment dispersion, for example, can be 25 wt%, 26 wt%, 27 wt%, 28 wt%, 29 wt%, 30 wt%, 31 wt%, 32 wt%, 33 wt%, 34 wt%, 35 wt%, or any concentration lying in any range bounded by any two of such values as inclusive enpoints (e.g., from 25 wt% to 35 wt%, from 25 wt% to 33 wt%, from 30 wt% to 35 wt%, from 33 wt% to 35 wt%, etc.). Including such an amount of pigment enables the optical density requirement to be met while still providing a suitable viscosity for compatibility with commercial inkjet printheads.
[0042] The pigment disersion can also include from 10 wt% to 30% of a suitable dispersant to ensure that the pigment has an adequate particle size distribution to provide the color and mechanical performance described herein. The dispersant, when added in suitable amounts, ensures the pigment dispersion is stable and can lower grinding times needed to botain the desired particle size. The dispersant used may depend on the pigment contained in the pigment dispersion (e.g., polymers of a co-polymer dispersant may be selected to be adsorbed onto the surface of the pigment particles and have chains that extend to overcome van der Waals ofrces between the particles). In aspects, the dispersant can be a commericially available dispersant suitable for use in UV-curable inks with carbon black pigments. Some examples of suitable dispersants are available from BYK® such as BYKJET-9152 and Borchi® Gen 0451. TheAttorney Docket No. : SP25-093PCTamount of dispsersant in the pigment dispersion may be 10 wt%, 12 wt%, 14 wt%, 16 wt%, 18 wt%, 20 wt%, 22 wt%, 24 wt%, 26 wt%, 28 wt%, 30 wt%, or any concentration bounded by any two of such values as inclusive enpoints (e.g., from 10 wt% to 30 wt%, from 10 wt% to 20 wt%, from 13 wt% to 18 wt%, from 20 wt% to 30 wt%, etc.).
[0043] In aspects, the amount of pigment contained in the pigment dispersion can depend on the pigment particles used. For example, when oxidized pigment particles (such as Mogul® E, available from Cabot Coorporation) are used, lesser amounts of dispersant is needed than if a non-oxidized pigment is used. In aspects, when oxidized pigment particles are used, the amount of dispersant in the pigment dispersion can be greater than or equal to 10 wt% and less than or equal to 20% (e.g., greater than or equal to 12 wt% and less than or equal to 20 wt%, greater than or equal to 13 wt% and less than or equal to 19 wt%, greater than or equal to 15 wt% and less than or equal to 18 wt%). The dispersant selected can also determine the amount of dispersant needed to provide the pigment dispersion with a suitable particle size distribution. For example, the anchor groups in the dispersant, and their affinity to surface groups exposed on the pigment particles can determine an amount of dispersant needed to provide a suitable dispersion effect. Dispersants with a plurality of affinic groups configured to form bonds with surface groups on the pigment may require smaller amounts of dispersants than those with only a single affinic group.
[0044] In addition to the pigment and the dispersant, a remainder of the pigment dispersion can include one or more monomers. For example, in aspects, the dispersion can include from 30 wt% to 70 wt% of a difunctional monomer. The difunctional monomer may be chosen to to facilitate polymermerization with remaining components in the ink composition during the curing process. The difunctional monomer may be chosen, for example, to have a high polymerization reactivity with the reactive diluent in the ink composition to provide a suitable post-cure hardness. In aspects, the amount of reactive monomer in the pigment dispersion can be 30 wt%, 35 wt%, 40 wt%, 45 wt%, 50 wt%, 55 wt%, 60 wt%, 65 wt%, 70 wt%, or any concentration lying in any range bounded by any two of the preceding values as inclusive enpoints (e.g., from 30 wt% to 70 wt%, from 35 wt% to 70 wt%, from 40 wt% to 70 wt%, from 40 wt% to 60 wt%, from 45 wt% to 70 wt%, from 30 wt% to 60 wt%, from 40 wt% to 60 wt%, from 45 wt% to 55 wt %).
[0045] In aspects, the amounts of dispersant and reactive monomer in the pigment dispersant may be selected to maximize the amount of pigment loading in the dispersion whileAttorney Docket No. : SP25-093PCTmaintaining a relatively low viscosity. For example, the combination of dispersant and reactive monomer can be selected so that, at a pigment loading of more than 30 wt% (e.g., 30 wt%, 31 wt%, 32 wt%, 33 wt%, 34 wt%, 35 wt%, or any value lying in any range bounded by any two of such values as inclusive enpoints), while the pigment dispersion further exhibits a viscosity that is less than or equal to 350 cPs over a temperature range from 30°C to 50°C. This viscosity has been found to be exhibited when the pigment dispersion contains from 13 wt% to 18 wt% of the dispersant and from 40 wt% to 60 wt% of a difunctional monomer when an oxidized carbon black pigment is used. Such viscosity of the pigment dispersion can facilitate a final viscosity of the ink composition that is suitable for use with commercial inkjet printheads. In embodiments, the ink composition may exhibit a viscosity greater than or equal to 8 cPs and less than or equal to 13 cPs at a temperature of 45°C, rendering it suitable for use with production printheads.
[0046] Various embodiments of photocurable inks and glass articles comprising same will be described herein with specific reference to the appended drawings.
[0047] Ranges may be expressed herein as from “about” one particular value, and / or to “about” another particular value. When such a range is expressed, another embodiment includes from the one particular value and / or to the other particular value. Similarly, when values are expressed as approximations, by use of the antecedent “about,” it will be understood that the particular value forms another embodiment. It will be further understood that the endpoints of each of the ranges are significant both in relation to the other endpoint, and independently of the other endpoint.
[0048] Directional terms as used herein - for example up, down, right, left, front, back, top, bottom - are made only with reference to the figures as drawn and are not intended to imply absolute orientation.
[0049] Unless otherwise expressly stated, it is in no way intended that any method set forth herein be construed as requiring that its steps be performed in a specific order, nor that with any apparatus specific orientations be required. Accordingly, where a method claim does not actually recite an order to be followed by its steps, or that any apparatus claim does not actually recite an order or orientation to individual components, or it is not otherwise specifically stated in the claims or description that the steps are to be limited to a specific order, or that a specific order or orientation to components of an apparatus is not recited, it is in no way intended thatAttorney Docket No. : SP25-093PCTan order or orientation be inferred, in any respect. This holds for any possible non-express basis for interpretation, including: matters of logic with respect to arrangement of steps, operational flow, order of components, or orientation of components; plain meaning derived from grammatical organization or punctuation, and; the number or type of embodiments described in the specification.
[0050] As used herein, the singular forms “a,” “an” and “the” include plural referents unless the context clearly dictates otherwise. Thus, for example, reference to “a” component includes aspects having two or more such components, unless the context clearly indicates otherwise.
[0051] As used herein, the “deposition temperature” refers to the temperature of an ink at ejection from a printhead.
[0052] As used herein, the “optical density” refers to how well a material reduces the power of light that passes through the material, per unit thickness, as measured with a densitometer.
[0053] As used herein, the “adhesion” refers to adhesion of a material after being subjected to the given conditions, when tested according to ASTM 3359.
[0054] As used herein, the “pencil hardness” is measured according to ASTM 3363.
[0055] As used herein, the “viscosity” is measured at the given temperature according to ASTMD445.
[0056] As used herein, the term “free” when used to describe the amount, concentration, or absence of a particular component in a composition or article, means that the component is not present in the composition or article.
[0057] Automotive interiors may include displays that include a display cover glass. A display module (e.g., a liquid crystal display (“LCD”) module, an organic light emitting diode (“OLED”) display module, or other suitable type of display module) may be laminated to or otherwise integrated with the cover glass such that the cover glass protects the display module and / or provides one or more performance enhancing attributes (e.g., anti-glare or anti -reflective properties) to the display module. A decorative ink may be applied to areas of the cover glass to conceal various components (e.g., electrical and mechanical connections) of the display and / or provide the display with a uniform appearance when the display is powered down.Attorney Docket No. : SP25-093PCT
[0058] Certain existing inks used for decorating display cover glass may suffer from various deficiencies rendering these inks unsuitable for automotive interior applications. For example, some existing inks may be applied through a screen-printing process, which may require multiple layers to provide a desired optical density. Such inks may have relatively low throughputs in production. Other existing inks (e.g., UV-curable inks) may fail to provide a desired optical density and / or provide adequate adhesion to the cover glass either initially or after being subjected to environmental testing associated with variable environmental conditions (e.g., in terms of temperature or humidity) that automotive interior components are exposed to. Adequate adhesion may be more difficult to achieve as the amount of pigment in the ink is increased.
[0059] Disclosed herein are ink compositions and ink primers which mitigate the aforementioned problems. Specifically, the UV photocurable inks described herein may be used to form opaque layers on display cover glass with high-throughput curing processes. Once the photocurable ink is cured, the opaque layer may have a relatively high adhesion to glass and high optical density. Regarding adhesion, the ink primers described herein including an adhesion promoter may be used to adequately adhere ink compositions including at least 11 wt% of a pigment to a glass substrate without compromising the desired post-cure thickness (e.g., less than 15 pm) and optical density (e.g., greater than 5) of the resulting opaque layer.
[0060] Ink Compositions
[0061] The ink compositions described herein may be used to form opaque layers on display cover glass having a desirable post-cure thickness (e.g., less than 15 pm) with high-throughput curing processes. Once the photocurable ink is cured, the opaque layer may have a relatively high adhesion to glass (e.g., greater than or equal to 4B) and high optical density (e.g., greater than 5). The terms “photocurable ink,” “ink composition,” and “photocurable ink composition” are used interchangeable throughout.
[0062] The ink compositions described herein may be ultraviolet curable ink compositions. The ink compositions may generally be described as comprising a pigment dispersion, a photoinitiator package, a reactive diluent, a multifunctional monomer, and, optionally, a difunctional monomer.Attorney Docket No. : SP25-093PCT
[0063] Pigment Dispersion
[0064] The pigment dispersion imparts the desired optical density to the resulting opaque layer. The ink composition may comprise a minimum amount of the pigment dispersion (e.g., greater than or equal to 25 wt%) to ensure that that the desired optical density (e.g., greater than 5) is achieved at the desired post-cure thickness (e.g., less than 15 pm). The amount of the pigment dispersion in the ink composition may be limited (e.g., less than or equal to 50 wt%) to ensure that the ink composition is curable. Accordingly, in embodiments, the ink composition may comprise, based on a total weight of the ink composition, greater than or equal to 25 wt% and less than or equal to 50 wt% of the pigment dispersion. In embodiments, the amount of the pigment dispersion in the ink composition may be, based on a total weight of the ink composition, greater than or equal to 25 wt%, greater than or equal to 30 wt%, or even greater than or equal to 35 wt%. In embodiments, the amount of the pigment dispersion in the ink composition may be, based on a total weight of the ink composition, less than or equal to 50 wt%, less than or equal to 45 wt%, or even less than or equal to 40 wt%. In embodiments, the amount of the pigment dispersion in the ink composition may be, based on a total weight of the ink composition, greater than or equal to 25 wt% and less than or equal to 50 wt%, greater than or equal to 25 wt% and less than or equal to 45 wt%, greater than or equal to 25 wt% and less than or equal to 40 wt%, greater than or equal to 30 wt% and less than or equal to 50 wt%, greater than or equal to 30 wt% and less than or equal to 45 wt%, greater than or equal to 30 wt% and less than or equal to 40 wt%, greater than or equal to 35 wt% and less than or equal to 50 wt%, greater than or equal to 35 wt% and less than or equal to 45 wt%, or even greater than or equal to 35 wt% and less than or equal to 40 wt%, or any and all subranges formed from any of these endpoints.
[0065] As described herein, the pigment dispersion comprises a pigment, a dispersant, and one or more monomers (“reactive monomer”, which can include “pigment difunctional monomers”). In embodiments, the pigment may comprise carbon black, iron oxide, carbon nanotubes, graphene, carbon fibers, titanium oxide (black), or combinations thereof. In embodiments, the pigment may comprise C.I. Pigment Black 6, 7, 12, 20, 31, and 32; PO71; PO38; carbon black, titanium black; aniline black; anthraquinone black pigment; or combinations thereof. The pigment dispersion may comprise a minimum amount of pigment (e.g., at least 25 wt%) to ensure that that the desired optical density (e.g., greater than 5) is achieved at the desired post-cure thickness (e.g., less than 15 pm). The amount of the pigmentAttorney Docket No. : SP25-093PCTin the pigment dispersion may be limited (e.g., less than or equal to 35 wt%) to preserve UV curability and flexibility in the composition space. Accordingly, in embodiments, the amount of pigment in the pigment dispersion may be, based on a total weight of the pigment dispersion, greater than or equal 25 wt%, greater than or equal to 30 wt%, or even greater than or equal to 33 wt%. In embodiments, the amount of the pigment in the pigment dispersion may be, based on a total weight of the pigment dispersion, less than or equal to 35 wt%„ or even less than or equal to 30 wt%. In embodiments, the amount of the pigment in the pigment dispersion may be, based on a total weight of the pigment dispersion, greater than or equal to 25 wt% and less than or equal to 35 wt%, greater than or equal to 25 wt% and less than or equal to 33 wt%, greater than or equal to 30 wt% and less than or equal to 35 wt%, greater than or equal to 35 wt% and less than 30 wt%, or any and all sub-ranges formed from any of these endpoints.
[0066] In embodiments, a remainder of the pigment dispersion comprises the dispsersant and reactive monomer. Suitable disperants and amounts thereof are provided elsewhere herein. The amount of reactive monomer in the pigment dispersion can be 30 wt%, 35 wt%, 40 wt%, 45 wt%, 50 wt%, 55 wt%, 60 wt%, 65 wt%, 70 wt%, or any concentration lying in any range bounded by any two of the preceding values as inclusive enpoints (e.g., from 30 wt% to 70 wt%, from 35 wt% to 70 wt%, from 40 wt% to 70 wt%, from 40 wt% to 60 wt%, from 45 wt% to 70 wt%, from 30 wt% to 60 wt%, from 40 wt% to 60 wt%, from 45 wt% to 55 wt %).
[0067] In embodiments, the reactive monomer of the pigment dispersion may comprise isobornyl acrylate, 1,6-hexanediol diacrylate, dipropylene glycol diacrylate, tri ethyleneglycol divinyl ether, ethylene glycol phenyl ether acrylate, propoxylated neopentyl glycol diacrylate, or combinations thereof. The reactive monomer of the pigment dispersion can also include any of the difunctional monomers mentioned with respect to the remainder of the ink composition described herein.
[0068] In embodiments, the amount of pigment dispersion and the amount of pigment in the pigment dispersion is configured such that the ink composition may comprise, based on a total weight of the ink composition (e.g., after the pigment dispersion and the remainder of the componnets are combined), at least 11 wt% of the pigment to facilitate the opaque layer formed therefrom having a relatively high optical density (e.g., greater than or equal to 5) at relatively low thicknesses (e.g., less than or equal to 15 pm, post curing). In embodiments, the amount of pigment in the ink composition may be, based on a total weight of the ink composition, greater than or equal to 11 wt%, greater than or equal to 13 wt%, greater than or equal to 15Attorney Docket No. : SP25-093PCTwt%, greater than or equal to 17 wt%. In embodiments the amount of pigment in the ink composition can be less than or equal to 20 wt%, less than or equal to 17 wt%, less than or equal to 15 wt%, or even less than or equal to 13 wt%.
[0069] Additional Copmponents of Ink Composition Other than Those of Pigment Dispersion
[0070] The ranges for monomers in this section exclude any amount of the same type of component (e.g., difunctional monomer) that is also included in the pigment dispersion. For example, if the pigment dispersion contains a difunctional monomer in a first amount, and the additional components contain a difunctional monomer in a second amount, then the total amount of difunctional monomer in the ink composition is a summation the first amount (scaled by the amount of pigment dispersion included in the ink composition) and the second amount. To illustrate, if an ink composition is formed by mixing 33.33 wt% of pigment dispersion and the remaining additional components, and the pigment dispersion contains 60 wt% difunctional monomer, while the additional components specify 10 wt% difunctional monomer, the total difunctional monomer content according to this example is 20 wt% (wt% of difunctional monomer attributed to that included in pigment dispersion) + 10 wt% (added in additional components) = 40 wt%. If the pigment dispersion does not contain a difunctional monomer, then the total amount of multifunctional monomer present in the ink composition is that specified in this section. If the pigment dispersion contains a difunctional monomer and not a multifunctional monomer, then the total multifunctional content in the ink composition lies within the ranges specified in the following paragraphs of this section.
[0071] The photoinitiator package of the ink composition facilitates curing of the ink composition, such as by using a UV LED. The ink composition may include a minimum amount of the photoinitiator package (e.g., greater than 0 wt%) to ensure curability of the ink composition. The amount of the photoinitiator package may be limited (e.g., less than or equal to 10 wt%) to preserve flexibility in the composition space for the remaining components while still providing favorable UV curing performance. Accordingly, in embodiments, the ink composition may comprise, based on a total weight of the ink composition, greater than 0 wt% and less than or equal to 10 wt% of the photoinitiator package. In embodiments, the amount of the photoinitiator package in the ink composition may be, based on a total weight of the ink composition, greater than 0 wt%, greater than or equal to 1 wt%, greater than or equal to 2 wt%, greater than or equal to 3 wt%, or even greater than or equal to 4 wt%. In embodiments,Attorney Docket No. : SP25-093PCTthe amount of the photoinitiator package in the ink composition may be, based on a total weight of the ink composition, less than or equal to 10 wt%, or even less than or equal to 8 wt%. In embodiments, the amount of the photoinitiator package in the ink composition may be, based on a total weight of the ink composition, greater than 0 wt% and less than or equal to 10 wt%, greater than 0 wt% and less than or equal to 8 wt%, greater than or equal to 1 wt% and less than or equal to 10 wt%, greater than or equal to 1 wt% and less than or equal to 8 wt%, greater than or equal to 2 wt% and less than or equal to 10 wt%, greater than or equal to 2 wt% and less than or equal to 8 wt%, greater than or equal to 3 wt% and less than or equal to 10 wt%, greater than or equal to 3 wt% and less than or equal to 8 wt%, greater than or equal to 4 wt% and less than or equal to 10 wt%, or even greater than or equal to 4 wt% and less than or equal to 8 wt%, or any and all sub-ranges formed from any of these endpoints.
[0072] The photoinitiator package of the ink composition may comprise a type I photoinitiator, a type II photoinitiator, and an amine synergist.
[0073] In embodiments, the type I photoinitiator may comprise phenylbis(2,4,6-trimethyl benzoyl)phosphine oxide (e.g. Irgacure 819, available from BASF); 1 -hydroxy cyclohexylphenyl ketone (e.g. Irgacure 184 available from BASF); (2,6-dimethoxybenzoyl)-2,4,4-trimethylpentyl phosphine oxide (e.g. commercial blends Irgacure 1800, 1850, and 1700 available from BASF); 2,2-dimethoxyl-2-phenyl acetophenone (e.g. Irgacure 651, available from BASF); (2,4,6-trimethylbenzoyl)diphenyl phosphine oxide (e.g. Lucirin TPO available from BASF, Munich, Germany); ethoxy(2,4,6-trimethylbenzoyl)phenyl phosphine oxide (e.g. Lucirin TPO-L from BASF); or combinations thereof.
[0074] In embodiments, an amount of the type I photoinitiator in the ink composition may be, based on a total weight of the ink composition, greater than or equal to 2 wt% and less than or equal to 8 wt%, greater than or equal to 2 wt% and less than or equal to 6 wt%, greater than or equal to 4 wt% and less than or equal to 8 wt%, or even greater than or equal to 4 wt% and less than or equal to 6 wt%, or any and all sub-ranges formed from any of these endpoints.
[0075] In embodiments, the type II photoinitiator may comprise isopropylthioxanthone, benzophenone, 4-phenylbenzophenone, methyl-2-benzoylbenzoate, ketosulphone, or combinations thereof.
[0076] In embodiments, an amount of the type II photoinitiator in the ink composition may be, based on a total weight of the ink composition, greater than or equal to 1 wt% and less thanAttorney Docket No. : SP25-093PCTor equal to 4 wt%, greater than or equal to 1 wt% and less than or equal to 3 wt%, greater than or equal to 2 wt% and less than or equal to 4 wt%, or even greater than or equal to 2 wt% and less than or equal to 3 wt%, or any and all sub-ranges formed from any of these endpoints. In embodiments, the amount of the type I photoinitiator in the ink composition may be greater than the amount of the type II photoinitiator to facilitate photopolymerization.
[0077] In embodiments, the amine synergist may comprise ethyl 4-(dimethylamino) benzoate; N, N-[2-(4-dimethylaminobenzoyl)oxyethylen-l-yl] methylamine; N-methyl diethanolamine; ethyl-4-dimethyl aminobenzoate; 2-ethylhexyl-4-dimethylaminobenzoate; or combinations thereof.
[0078] In embodiments, an amount of the amine synergist in the ink composition may be, based on a total weight of the ink composition, greater than or equal to 1 wt% and less than or equal to 4 wt%, greater than or equal to 1 wt% and less than or equal to 3 wt%, greater than or equal to 2 wt% and less than or equal to 4 wt%, or even greater than or equal to 2 wt% and less than or equal to 3 wt%, or any and all sub-ranges formed from any of these endpoints.
[0079] The reactive diluent of the ink composition imparts a relatively low viscosity (e.g., less than 5 cPs at 25°C) to improve curing performance while also aiding in providing a low overall viscosity. In embodiments, the reactive diluent may comprise vinyl methyl oxazolidinone; 5-methyl-3-vinyloxazolidin-2-one; other A-vinyl monomers, such as N-vinylcarbazole, A-vinylindole derivatives, A-vinylpyrrolidone, A-vinyl caprolactam, N-vinylformamide, A-vinyl acetoamide derivatives, A-vinyl(na)phthalimides, N-vinylimidazolium salts, and A-vinyltriazoles; or combinations thereof.
[0080] The ink composition may include a minimum amount of reactive diluent (e.g., greater than or equal to 10 wt%) to ensure that the ink composition will cure. Accordingly, in embodiments, the ink composition may comprise, based on a total weight of the ink composition, greater than or equal to 10 wt% and less than or equal to 42 wt% of a reactive diluent. In embodiments, the amount of the reactive diluent in the ink composition may be, based on a total weight of the ink composition, greater than or equal to 10 wt%, greater than or equal to 15 wt%, greater than or equal to 20 wt%, or even greater than or equal to 25 wt%. In embodiments, the amount of the reactive diluent in the ink composition may be, based on a total weight of the ink composition, less than or equal to 42 wt%, less than or equal to 40 wt%, less than or equal to 35 wt%, less than or equal to 30 wt%, less than or equal to 25 wt%, orAttorney Docket No. : SP25-093PCTeven less than or equal to 20 wt%. In embodiments, the amount of the reactive diluent in the ink composition may be, based on a total weight of the ink composition, greater than or equal to 10 wt% and less than or equal to 42 wt%, greater than or equal to 10 wt% and less than or equal to 40 wt%, greater than or equal to 10 wt% and less than or equal to 35 wt%, greater than or equal to 10 wt% and less than or equal to 30 wt%, greater than or equal to 10 wt% and less than or equal to 25 wt%, greater than or equal to 10 wt% and less than or equal to 20 wt%, greater than or equal to 15 wt% and less than or equal to 42 wt%, greater than or equal to 15 wt% and less than or equal to 40 wt%, greater than or equal to 15 wt% and less than or equal to 35 wt%, greater than or equal to 15 wt% and less than or equal to 30 wt%, greater than or equal to 15 wt% and less than or equal to 25 wt%, greater than or equal to 15 wt% and less than or equal to 20 wt%, greater than or equal to 20 wt% and less than or equal to 42 wt%, greater than or equal to 20 wt% and less than or equal to 40 wt%, greater than or equal to 20 wt% and less than or equal to 35 wt%, greater than or equal to 20 wt% and less than or equal to 30 wt%, greater than or equal to 20 wt% and less than or equal to 25 wt%, greater than or equal to 25 wt% and less than or equal to 42 wt%, greater than or equal to 25 wt% and less than or equal to 40 wt%, greater than or equal to 25 wt% and less than or equal to 35 wt%, or even greater than or equal to 25 wt% and less than or equal to 30 wt%, or any and all subranges formed from these endpoints.
[0081] The multifunctional monomer of the ink composition facilitates cure via high crosslinking, thereby increasing the mechanical properties of the resulting in the opaque layer. In embodiments, the multifunctional monomer may comprise dipentaerythritol hexaacrylate (e.g., M600 DPHA). Other suitable amide and acrylate compositions for use as the reactive diluent and the multifunctional monomer may be found in U.S. Patent No. 7,423,105 B2, entitled “Fast Curing Primary Optical Fiber Coatings,” hereby incorporated by reference in its entirety.
[0082] Examples of the multifunctional acrylate monomers that may be included in the ink composition include hexanediol diacrylate, trimethylolpropane triacrylate, pentaerythritol triacrylate, polyethylene glycol diacrylate (for example tetraethylene glycol diacrylate), dipropylene glycol diacrylate, tri(propylene glycol) triacrylate, neopentyl glycol diacrylate, bis(pentaerythritol) hexaacrylate, 3-methyl pentanediol diacrylate, and the acrylate esters of ethoxylated or propoxylated glycols and polyols, for example, propoxylated neopentyl glycol diacrylate, ethoxylated trimethylolpropane triacrylate, and mixtures thereof.Attorney Docket No. : SP25-093PCT
[0083] In addition, suitable multifunctional methacrylate monomers may also include esters of methacrylic acid (i.e. methacrylates), such as hexanediol dimethacrylate, trimethylolpropane trimethacrylate, triethyleneglycol dimethacrylate, diethyleneglycol dimethacrylate, ethyleneglycol dimethacrylate, 1,4-butanediol dimethacrylate, and mixtures thereof.
[0084] In embodiments, the multifunctional (meth)acrylate monomers may be selected from propoxylated neopentyl glycol diacrylate, ethoxylated trimethylolpropane triacrylate, dipropylene glycol diacrylate, tripropylene glycol diacrylate, and mixtures thereof.
[0085] The ink composition may comprise a minimum amount of multifunctional monomer (e.g., greater than or equal to 2 wt%) to ensure that the ink composition will cure. The amount of the multifunctional monomer may be limited (e.g., less than or equal to 20 wt%) to impart a relatively low viscosity and thereby preserve jettability. Accordingly, in embodiments, the ink composition may comprise, based on a total weight of the ink composition, greater than or equal to 2 wt% and less than or equal to 20 wt% of the multifunctional monomer. In embodiments, the amount of multifunctional monomer in the ink composition may be, based on a total weight of the ink composition, greater than or equal to 2 wt%, greater than or equal to 4 wt%, greater than or equal to 7 wt%, or even greater than or equal to 10 wt%. In embodiments, the amount of multifunctional monomer in the ink composition may be, based on a total weight of the ink composition, may be less than or equal to 20 wt%, less than or equal to 16 wt%, or even less than or equal to 12 wt%. In embodiments, the amount of the multifunctional monomer in the ink composition may be, based on a total weight of the ink composition, greater than or equal to 2 wt% and less than or equal to 20 wt%, greater than or equal to 2 wt% and less than or equal to 16 wt%, greater than or equal to 2 wt% and less than or equal to 12 wt%, greater than or equal to 4 wt% and less than or equal to 20 wt%, greater than or equal to 4 wt% and less than or equal to 16 wt%, greater than or equal to 4 wt% and less than or equal to 12 wt%, greater than or equal to 4 wt% and less than or equal to 10 wt%, greater than or equal to 10 wt% and less than or equal to 16 wt%, or even greater than or equal to 10 wt% and less than or equal to 12 wt%, or any and all sub-ranges formed from any of these endpoints. In aspects, the amount of multifunctional monomer can be limited to releavtively low amounts in the preceding ranges (to less than or equal to 10wt%, less than or equal to 7 wt%, or even less than or equal to 5 wt%) should the pigment dispersion contain a monomer that is particularly reactive with the other components of the ink composition. In aspects, for example, the monomer in the pigment dispersion can match the difunctional monomerAttorney Docket No. : SP25-093PCTcontained in the remainder of the ink composition and, in such cases, proper selection of the reactive diluent can eliminate the need for the multifunctional monomer to a certain extent, which aids in maintaining the viscosity of the ink composition relatively low.
[0086] The ink composition may further comprise a difunctional monomer to build mechanical properties while maintaining low viscosity. In embodiments, the difunctional monomer may comprise difunctional acrylates and methacrylates, such as 3-methyl-l,5-pentanediyl diacrylate, dipropylene glycol diacrylate, or combinations thereof. In embodiments, the ink composition may comprise, based on a total weight of the ink composition, greater than or equal to greater than or equal to 0 wt% and less than or equal to 40 wt% of the difunctional monomer (excluding any difunctional monomer present in the pigment dispersion). In embodiments, the ink composition may comprise, based on a total weight of the ink composition, greater than or equal to greater than or equal to 10 wt% and less than or equal to 40 wt% of the difunctional monomer. In embodiments, the amount of the difunctional monomer in the ink composition may be, based on a total weight of the ink composition, greater than or equal to 0 wt%, greater than or equal to 5 wt%, greater than or equal to 10 wt%, or even greater than or equal to 15 wt%. In embodiments, the amount of the difunctional monomer in the ink composition may be, based on a total weight of the ink composition, less than or equal to 40 wt%, less than or equal to 35 wt%, less than or equal to 25 wt%, or even less than or equal to 15 wt%. In embodiments, the amount of the difunctional monomer in the ink composition may be, based on a total weight of the ink composition, greater than or equal to 0 wt% and less than or equal to 40 wt%, greater than or equal to 0 wt% and less than or equal to 36 wt%, greater than or equal to 0 wt% and less than or equal to 30 wt % greater than or equal to 0 wt% and less than or equal to 15 wt%, greater than or equal to 5 wt% and less than or equal to 35 wt%, greater than or equal to 5 wt% and less than or equal to 25 wt%, greater than or equal to 5 wt% and less than or equal to 15 wt%, greater than or equal to 10 wt% and less than or equal to 35 wt%, greater than or equal to 10 wt% and less than or equal to 25 wt%, greater than or equal to 10 wt% and less than or equal to 15 wt%, greater than or equal to 15 wt% and less than or equal to 36 wt%, or even greater than or equal to 15 wt% and less than or equal to 25 wt%, or any and all sub-ranges formed from any of these endpoints.Attorney Docket No. : SP25-093PCT
[0087] Aspects of Total Ink Composition (after pigment dispersion and remaining components are mixed)
[0088] The relative amounts of the reactive diluent, the multifunctional monomer, and the difunctional monomer may be tailored based on the characteristics of the reactive monomer in the pigment dispersions. That is, the amount of the difunctional monomer relative to the reactive diluent and the particular difunctional monomer used may be based on the viscosity and reactivity of the reactive monomer in the pigment dispersion.
[0089] In embodiments, a combined amount of the reactive diluent, the multifunctional monomer, and the difunctional monomer may be less than or equal to 80 wt% to achieve a relatively low viscosity (e.g., less than 20 cPs at 25°C) while providing enough composition space for other components to facilitate UV curability and to achieve the desired optical density (e.g., greater than 5). Relatively high combined amount of the reactive diluent, the multifunctional monomer, and the difunctional monomer (e.g., greater than or equal to 65 wt%, greater than or equal to 70 wt%, and greater than or equal to 75 wt%) may be used if the amount of multifunctional monomer is relatively low (e.g., less than or equal to 10 wt%, less than or equal to 7 wt%, or even less than or equal to 5 wt%) to facilitate maintaining a viscosity in this range. In embodiments, a combined amount of the reactive diluent, the multifunctional monomer, and the difunctional monomer may be less than or equal to 60 wt%, less than or equal to 50 wt%, less than or equal to 40 wt%, or even less than or equal to 30 wt%.
[0090] In embodiments, based on the ranges in the preceding two sections, after mixing of the pigment dispersion with the additional components, the ink composition may comprise a pigment in an amount greater than or equal to 11 wt% and less than or equal to 20 wt%; a dispersant in an emount greater than or equal to 3 wt% and less than or equal to 10 wt% dispersant; a type I photoinitiator in an amount in a range from 1 wt% to 6 wt%; a type II photoinitiator in an amount in a range from 1 wt% to 6 wt%; an amine synergist in an amount in a range from 1 wt% to 4 wt%; greater than or equal to 10 wt% and less than or equal to 42 wt% of a reactive diluent; greater than or equal to 2 wt% and less than or equal to 20 wt% of a multifunctional monomer; and a total difunctional monomer content that is greater than or equal to 10 wt% and less than or equal to 75 wt%. In aspects, for example, when the multifunctional monomer content is relatively low (e.g., less than or equal to 10 wt% or less than or equal to 5 wt%), the total difunctional monomer content of the ink composition may be relatively high (e.g., greater than or equal to 50 wt%, or even greater than or equal to 55 wt%)Attorney Docket No. : SP25-093PCTto provide an ink composition with suitable post cure mechanical properties. Such high amounts can be obtained, for example, when both the pigment dispersion and additional components include difunctional monomers.
[0091] In aspects, after the mixing, a total monomer content of the ink composition excluding the reactive diluent, calculated by combining amounts of monofunctional monomer (if any are present), difunctional monomer, and multifunctional monomer in the ink composition, is greater than or equal to 50 wt% and less than or equal to 80 wt%. Such high monomer content facilitates providing a suitably low viscosity for jetting, while an opaque layer with suitable mechanical properties can be provided with appropriate selection of the monomers, reactive diluent, and photoinitiators.
[0092] The ink composition may further comprise an adhesion promoter to facilitate the inks binding to the glass without the use of a primer. Suitable adhesion promoters can include 3-(methacryloyloxy)propyltrimethoxy silane, 3 -(acryloyloxy)propyltrimethoxy silane, (3-mercaptopropyl)trimethoxysilane, and allyltrimethylsilane and any other acrylated silane. Other suitable adhesion promoters can be found in U.S. Patent Application Ser. No.15 / 337,459, filed on October 28, 2016, hereby incorporated by reference in its entirety. In embodiments, ink composition further comprises greater than 0 wt% and less than or equal to 10 wt% of the adhesion promoter.
[0093] In embodiments, the ink compositions described herein are free of resin, which aids in maintaining a low viscosity suitable for inkjet printing, and free of TPO, which is a requirement for REACH compliance.
[0094] The ink compositions described herein may also satisfy various environmental compliance standards. For example, in embodiments, the ink compositions described herein may contain less than 10 wt% volatile organic compounds, thus satisfying GB 35807-2020, entitled “Limits of Volatile Organic Compounds (VOCs) in Printing Ink,” hereby incorporated by reference in its entirety. Moreover, the ink compositions described herein may be free of halogenated hydrocarbon and free of the solvents identified by CAS Registry Number in Table 1.Attorney Docket No. : SP25-093PCT
[0095] Table 1Component CAS1 Ethylbenzene 100-41-42 Propylene oxide (Oxirane, methyl-) 75-56-93 Styrene (Benzene, ethenyl-) 100-42-54 benzene 71-43-25 Isopropyl nitrite 541-42-46 Butyl nitrite 544-16-17 Ethylene glycol monoethyl ether (2 -Ethoxy ethanol) 110-80-58 Ethylene glycol ether acetate 111-15-99 Ethylene glycol monomethyl ether (2 -Methoxyethanol) 109-86-410 Ethylene glycol formaldehyde acetate (2 -Methoxy ethyl Acetate) 110-49-611 2-nitropropane 79-46-912 N-methyl-2-pyrrolidone 872-50-413 Triethylene glycol dimethyl ether 112-49-214 Ethylene glycol dimethyl ether 110-71-415 Ethylene glycol diethyl ether 629-14-116 Toluene 108-88-317 Xylene 1330-20-7
[0096] Such solvents are known to have potentially harmful effects on the environment and / or human health. Certain existing ink compositions incorporate the solvents listed in Table 1 in order to provide UV-curable inks with relatively high optical densities that are compatible with inkjet printing. The ink compositions described herein provide such favorable attributes without such harmful solvents. The ink compositions of the present disclosure provide uncured viscosities suitable for inkjet printing without the addition of harmful solvents, and thus facilitate relatively high throughput (e.g., greater than 20 m2 / hour, greater than 30 m2 / hour, greater than 40 m2 / hour, greater than 50 m2 / hour) printing process with commercially available printheads. Inkjet printing processes are beneficially compatible with chemically strengthened cover glass, unlike certain other inks based on ceramic frits that require relatively high curing temperatures.
[0097] In embodiments, the ink compositions may have a viscosity greater than or equal to 1 cPs and less than or equal to 100 cPs over a temperature range from 30°C to 50°C. InAttorney Docket No. : SP25-093PCTembodiments, the ink compositions described herein may be compatible with commercially available inkjet printing processes (e.g., have an un-cured viscosity of less than 13 cPs at at 45°C) to facilitate relatively low-cost, high throughout production processes.
[0098] In aspects, an ink primer may be used to help adhere the ink compositions described herein to the substrate. Any of the ink primers described in U.S. Patent Publication No.2025 / 0019556A1, entitled “Photocurable Inks and Primers for Automotive Interior Applications and Glass Articles Comprising the Same,” herein incorporated by reference in its entirety, can be used.
[0099] In aspects, the ink compositions described herein can be used in a layer as a multicomponent ink stack. For example, the ink compositions described herein can be used as a second pigmented layer in an ink stack with any of the first pigmented layers described in U.S. Provisional Patent Application No. 63 / 695,125, entitled “Ultraviolet Curable Ink Stacks for Automotive Interior Applications and Substrates Comprising the Same,” herein incorporated by reference in its entirety.
[0100] Referring now to FIG. 1, a vehicle interior 2000 including three different vehicle interior systems 100, 200, 300 is shown. Vehicle interior system 100 includes a center console base 110 with a curved surface 120 including a display 230. Vehicle interior system 200 includes a dashboard base 210 with a curved surface 220 including a display 230. The dashboard base 210 typically includes an instrument panel 215 which may also include a curved display. Vehicle interior system 300 includes a dashboard steering wheelbase 310 with a curved surface 320 and a display 330. In embodiments, the vehicle interior system may include a base that is an arm rest, a pillar, a seat back, a floorboard, a headrest, a door panel, or any portion of the interior of a vehicle that includes a curved surface. In embodiments, the displays 130, 230, 330 are flat and comprise cover glass with planar major surfaces. In embodiments, one or more of the displays 130, 230, 330 are curved, and the curved display may include curved cover glass that may be hot-formed or cold-formed to possess such curvature. For example, such embodiments may incorporate opaque layers formed of the photocurable ink compositions described herein disposed on cold-formed glass substrates. Such cold-forming may involve any of the techniques described in U.S. Pre-Grant Publication No. 2019 / 0329531 Al, entitled “Laminating thin strengthened glass to curved molded plastic surface for decorative and display cover application,” U.S. Pre-Grant Publication No.2019 / 0315648 Al, entitled “Cold-formed glass article and assembly process thereof,” U.S. PreAttorney Docket No. : SP25-093PCTGrant Publication No. 2019 / 0012033 Al, entitled “Vehicle interior systems having a curved cover glass and a display or touch panel and methods for forming the same,” and U.S. Patent Application No. 17 / 214,124, entitled “Curved glass constructions and methods for forming same,” which are hereby incorporated by reference in their entireties.
[0100] The embodiments of the glass articles described herein may be used in any or all of vehicle interior systems 100, 200 and 300. While FIG. 1 shows an automobile interior, the various embodiments of the vehicle interior system may be incorporated into any type of vehicle such as trains, automobiles (e.g., cars, trucks, buses and the like), seacraft (boats, ships, submarines, and the like), and aircraft (e.g., drones, airplanes, jets, helicopters and the like), including both human-piloted vehicles, semi-autonomous vehicles and fully autonomous vehicles. Further, while the description herein relates primarily to the use of the glass articles in vehicle displays, it should be understood that various embodiments discussed herein may be used in any type of display application.
[0101] FIG. 2 schematically depicts a cross-sectional view of the display 230 through the line 2-2 of FIG. 1, according to an example embodiment where the display 230 is flat. While FIG. 2 depicts an example of the display 230, it should be understood that the displays 130, 330 described herein with respect to FIG. 1 may have similar cross-sectional structures and incorporate the photocurable inks described herein in a similar manner. While the display 230 is flat in the embodiment depicted in FIG. 2, embodiments are also envisioned where the display 230 is curved and the glass article 400 comprises one or more curved surfaces (e.g., as a result of being cold-formed or hot-formed to have a suitable curved shape).
[0102] As shown in FIG. 2, the glass article 400 comprises at least a substrate 450 and an opaque layer 500, and optionally includes a light management layer 460. The substrate 450 has a first major surface 470 facing a viewer and a second major surface 480 upon which the opaque layer 500 is, at least in part, disposed. As used herein, the term "dispose" includes coating, depositing and / or forming a material onto a surface using any known method in the art. The disposed material may constitute a layer, as defined herein. As used herein, the phrase "disposed on" includes the instance of forming a material onto a surface such that the material is in direct contact with the surface and also includes the instance where the material is formed on a surface, with one or more intervening material(s) is between the disposed material and the surface. The intervening material(s) may constitute a layer, as defined herein. The term "layer" may include a single layer or may include one or more sub-layers. Such sub-layers may be inAttorney Docket No. : SP25-093PCTdirect contact with one another. The sub-layers may be formed from the same material or two or more different materials. In one or more alternative embodiments, such sub-layers may have intervening layers of different materials disposed therebetween. In one or more embodiments, a layer may include one or more contiguous and uninterrupted layers and / or one or more discontinuous and interrupted layers (i.e., a layer having different materials formed adjacent to one another). A layer or sub-layers may be formed by any known method in the art, including discrete deposition or continuous deposition processes. In one or more embodiments, the layer may be formed using only continuous deposition processes, or, alternatively, only discrete deposition processes.
[0103] In embodiments, the substrate 450 is a glass substrate that is optionally chemically strengthened and comprises a thickness of from 0.05 to 2.0 mm. In one or more embodiments, the substrate 450 may be a transparent plastic, such as PMMA, polycarbonate and the like, or may be a glass material (which may be optionally strengthened).
[0104] The various glass substrate(s) of the glass articles discussed herein, such as the substrate 450, may be formed from any suitable glass composition comprising soda lime glass, aluminosilicate glass, borosilicate glass, boroaluminosilicate glass, alkali-containing aluminosilicate glass, alkali-containing borosilicate glass, and alkali-containing boroaluminosilicate glass.
[0105] In embodiments, the glass article 400 comprises a functional surface layer 490. The functional surface layer 490 can be configured to provide one or more of a variety of functions. For example, the functional surface layer 490 may be optical coating configured to provide easy-to-clean performance, anti-glare properties, antireflection properties, and / or half-mirror coating. Such optical coatings can be created using single layers or multiple layers. In the case of anti-reflection functional surface layers, such layers may be formed using multiple layers having alternating high refractive index and low refractive index. Non-limiting examples of low refractive index films include SiCh, MgF2, and AI2O3, and non-limiting examples of high refractive index films include Nb2Os, TiCh, ZrCh, HfCh, and Y2O3. In embodiments, the total thickness of such an optical coating (which may be disposed over an anti-glare surface or a smooth substrate surface) is from 5 nm to 750 nm. Additionally, in embodiments, the functional surface layer 490 that provides easy-to-clean performance also provides enhanced feel for touch screens and / or coating / treatments to reduce fingerprints. In some embodiments, functional surface layer 490 is integral to the first surface of the substrate. For example, suchAttorney Docket No. : SP25-093PCTfunctional surface layers can include an etched surface in the first surface of the substrate 450 providing an anti-glare surface (or haze of from, e.g., 2% to 20%).
[0106] The opaque layer 500 is printed onto the light management layer 460, when included. Certain existing UV-curable inks have been shown to be incompatible (e.g., lack the requisite adhesion) with the light management layer 460. For example, existing photocurable inks, when used for the opaque layer, may chemically react with the ink of the light management layer 460 (either upon deposition or after environmental testing) to change the characteristics (e.g., color, size) of the ink layers. Existing photocurable inks may also diffuse into the light management layer 460 and degrade performance thereof. The photocurable ink compositions described herein, when used to form the opaque layer 500 and printed on the light management layer 460, do not suffer from such deficiencies and still provide adequate adhesion to the substrate 450 even when the light management layer 460 is present.
[0107] The light management layer 460, when included, may be printed on the substrate 450. In embodiments, the light management layer 460 is formed from a suitable thermal or UV cured ink. The light management layer 460 may generally reduce the optical transmission of the glass article 400 such that the glass article 400 exhibits a similar appearance to users irrespective of whether the display 540 is powered on or off. For example, the light management layer 460 may obscure edges of the display region 520, rendering the boundaries of the display region 520 inconspicuous to viewers when the display is powered off. The light management layer 460 may generally be constructed as described in any of International Patent Application Publication Nos. WO 2019 / 055458 Al, entitled “Black Deadfront for Display Device and Methods,” WO 2020 / 205519 Al, entitled “Decorated Glass Having a Printed Ink Layer,” or WO 2021 / 118835 Al, entitled, “Display Devices and Articles with Color-Matched Display and Non-Display Areas,” each of which are hereby incorporated by reference in their entirety.
[0108] Referring still to FIG. 2, in embodiments, the opaque layer 500 may be constructed of at least one of the photocurable ink compositions and the ink primers described herein. For example, in some embodiments, the opaque layer 500 may be comprise a photocurable ink comprising at least 11 wt% of a pigment. In other embodiments, the opaque layer may comprise an ink composition comprising at least 11 wt% of a pigment and an adhesion promoter. In such embodiments, the adhesion promoter is bonded to the glass substrate and the ink composition is polymerized with the adhesion promoter. Accordingly, the opaque layerAttorney Docket No. : SP25-093PCT500 may comprise a relatively high optical density (e.g., greater than or equal to 5) in order to block light transmittance. In embodiments, the opaque layer 500 is used to block light from transmitting trough certain regions of the glass article 400. In embodiments, the opaque layer 500 obscures functional or non-decorative elements provided for the operation of the glass article 400. In embodiments, the opaque layer 500 is provided to outline backlit icons and / or other graphics (not depicted) so as to increase the contrast at the edges of such icons and / or graphics.
[0109] In embodiments, as shown in FIG. 2, the glass article 400 is placed over or in front of a display 540. In one or more embodiments, the display 540 may include a touch-enabled displays which include a display and touch panel. Exemplary displays include LED display, a DLP MEMS chip, LCDs, OLEDs, transmissive displays, and the like. The glass article 400 may generally have an average transmittance from 380 nm to 750 nm that is greater than or equal to 10% (e.g., greater than or equal to 20%, greater than or equal to 30%, greater than or equal to 40%, greater than or equal to 50%, greater than or equal to 60%, greater than or equal to 70%). The high optical density of the opaque layer 500, however, causes the areas of the glass article 400 incorporating the opaque layer 500 to have relatively low optical transmission (e.g., an average transmittance of less than or equal to 0.1% in the visible spectrum). Accordingly, the boundaries of the opaque layer 500 may define a display region 520 where the glass article 400 exhibits a relatively high optical transmission to facilitate visibility of images generated by the display 540.
[0110] In the depicted embodiment, the opaque layer 500 covers the edges 550 of the display 540 to hide the edges 550 from view through the first surface 470. The opaque layer 500 may also be used to obscure various other components from view (e.g., electrical connections, mechanical housings, and the like). The opaque layer 500 generally facilitates a desired portion of the display 540 being viewable by users viewing the first surface 470.[OHl] In embodiments, the opaque layer 500 is applied via inkjet printing over the light management layer 460 and / or over the second surface 480 of the substrate 450. In embodiments, the opaque layer 500 may be directly deposited onto the second surface 480 of the substrate 450 using a suitable inkjet process. In embodiments, prior to deposition of the opaque layer 500, in embodiments not utilizing the ink primers described herein, the second surface 480 may be primed using a suitable primer (e.g., an acryloxy silane primer) to facilitateAttorney Docket No. : SP25-093PCTadhesion of the opaque layer 500 to the substrate 450. Any suitable treatment to the second surface 480 may be used to facilitate adhesion of the opaque layer 500 to the substrate 450.
[0112] As described herein, the opaque layer 500 has a relatively high adhesion to glass. In embodiments, the opaque layer 500 exhibits an adhesion to the glass substrate greater than or equal to 4B, after being subjected to a temperature of 85°C at 95% relative humidity for a period of at least 500 hours, when tested according to ASTM 3359. In embodiments, the opaque layer 500 exhibits an adhesion to the glass substrate greater than or equal to 4B, after 500 1 hour cycles of being held at a temperature of -40°C for 0.5 hours and a temperature of 95°C for 0.5 hours, when tested according to ASTM 3359.
[0113] The opaque layer 500 may have a desired thickness of less than or equal to 15 pm. In embodiments, the opaque layer 500 may have a thickness less than or equal to 15 pm or even less than or equal to 10 pm. In embodiments, the opaque layer 500 may have a thickness greater than or equal to 1 pm or even greater than or equal to 5 pm. In embodiments, the opaque layer 500 may have a thickness greater than or equal to 1 pm and less than or equal to 15 pm, greater than or equal to 1 pm and less than or equal to 10 pm, greater than or equal to 5 pm and less than or equal to 15 pm, or even greater than or equal to 5 pm and less than or equal to 10 pm, or any and all sub-ranges formed from any of these endpoints.
[0114] In embodiments, the photocurable ink compositions and / or ink primers described herein may be tailored to meet particular appearance requirements associated with design needs. The opaque layer 500 can be any color; in particular embodiments, though, the opaque layer 500 is black or gray. For example, a cover glass comprising an opaque layer constructed of the photocurable ink compositions and / or ink primers described herein may meet any of the black mask color targets in Table 2.Attorney Docket No. : SP25-093PCT
[0115] Table 2CM700D (CIE D65, 10°) Measurement through bare glassInk Type SCI SCEL* a* b* L* a* b* Black Mask 25.0Black Mask 25.3Black Mask 25.7Black Mask 25.9Black Mask 26.0Black Mask 26.8 0.05 -0.2 <1 0 0 Black Mask 27.4Black Mask 27.7Black Mask 28.3Black Mask 28.5Black Mask 30.1
[0116] In embodiments, opaque layers constructed using the photocurable ink compositions and / or ink primers described herein may meet any of the combinations of values contained in the Table 2 within the tolerances outlined in the Table 3 below.
[0117] Table3OD AE within the part L* Tol a* Tol b* Tol> 4 0.6 ± 0.10 ± 0.10 ± 0.10
[0118] As demonstrated by Tables 2 and 3, glass articles incorporating the photocurable ink compositions and / or ink primers described herein, when viewed from an uncoated surface of the cover glass (e.g., from a side of the glass opposite to that on which a display disposed) may generally have CIELAB L* values that are less than or equal to 30 (less than or equal to 29, less than or equal to 28, less than or equal to 27, less than or equal to 25, less than or equal to 25), CIELAB a* values (specular component included) that are greater than or equal to -0.05 and less than or equal to 0.15, and CIELAB b* values (specular component included) that are less than or equal to -0.1 and greater than or equal to -0.3, when illuminated with a CIE D65 illuminant at a 10° angle of incidence. When the specular component is excluded, the glass article may exhibit CIE L* values that are less than or equal to 1, and CIELAB a* and b* values with magnitudes that are less than or equal to 0.1. Areas of the cover glass coated with the photocurable ink compositions and / or ink primers described herein may exhibit dark, neutral appearances to facilitate concealing various components from view.Attorney Docket No. : SP25-093PCT
[0119] The photocurable ink compositions and / or ink primers of the present disclosure may also be used to construct opaque layers on a glass article that exhibit favorable reliability testing results when compared to certain existing photocurable inks and / or ink primers. Automotive interior components are subjected to environmental conditions that are highly variable (e.g., in terms of temperature and relative humidity). In embodiments, opaque layers may meet one or more of the following criteria when subjected to the reliability testing outlined in Table 4.
[0120] Table 4Acceptance Sample Test Test Method / Conditions / ToolCriteria Size 1. Test Condition(1) Preconditioning: 55 °C ± 2 °C with a relative humiditynot exceeding 20 % for a period of 24 h prior to the firstcycle of the damp heat test.@ Cycles 1-5: include cold phasea) 0-1.5 hr: raise to 25 °C ± 2 °C, 93 ± 3%b) 1.5-2.5 hr: raise to 65 °C ± 2 °C , 93 ± 3%c) 2.5-5.5 hr: keep at 65 °C ± 2°C , 93 ± 3%d) 5.5-7 / 8 hr: decrease to 25 °C ± 2°C , 80-96%A - Damp e) 8 -9.5 / 10.5 hr: raise to 65 °C ± 2°C , 93 ± 3% 1. Delta E (before / after test) Heat, Cyclic f) -9.5 / 10.5 -13.5 hr: keep at 65 °C ± 2°C , 93 ± 3% <2 2 (with Frost)g) 13.5 -15 / 16 hr: decrease to 25°C ± 2°C , 80-96% 2. Ink adhesion > 4Bh) -15 / 16 -17.5 hr: keep at 25 °C ± 2°C , 93 ± 3%i) 17.5-18 hr: decrease to -10 °C ± 2°C , uncontrolled%j) 18-21 hr: keep at -10 °C ± 2°C , uncontrolled%k) 21-22.5 hr: raise to 25 °C ± 2°C , uncontrolled%€) 22.5-24 hr: keep at 25 °C ± 2°C , 93 ± 3%(5) Cycles 6-10: without a cold phasea) @ a)- g)b) 15 / 16 -24 hr: keep at 25 °C ± 2°C , 93 ± 3%2) Total cycles: 10 (5+5)B.l - High 1. Delta E (before / after test) Temp / High 2 Humidity 65°C / 95 %RH, 500 hrs <22. Ink adhesion > 4BB.2 - High 3. Delta E (before / after test) Temp / High 85°C / 95 %RH, 500 hrs 2 Humidity <21. Ink adhesion > 4BC - High 2. Delta E (before / after test) Temp. 95 °C, 500 hrs 2<23. Ink adhesion > 4BD - Low 1. Delta E (before / after test) Temp. -40 °C, 500 hrs 2<22. Ink adhesion > 4BTest temp.: TRT (23 °C);Test duration: 2 Hr; 1. No crack / bleach / color E - Chemical change allowedMethod: Wet a cotton cloth (30*30 mm) with 50 ml respectiveResistance 2chemical agent (e.g., ammonia base cleaner, antifreeze, soda, citricacid, electric grease connector, nail polish remover, hand cleaner, 2. Delta E (before / after test) hand lotion, battery liquid); Wet the DUT with this cotton cloth until <2it is completely wet, let redundant agent drip off the DUTD - Salty Salty Water Chamber: 5% NaCl, 35 °C for 72 hrs -> water cleaning - 1. Delta E (before / after test) Water > drying 2<22. Ink adhesion > 4BF - Cross 1. Ink deterioration such asHatch Tape ASTM 3359 flaking, peeling, cracking 2 Test or blistering: not allowed2. Ink adhesion > 4BAttorney Docket No. : SP25-093PCT1. Test condition1) Z-IN1 profile of DIN 75220(1) dry air (15 days)- chamber temp: +80 ±3 °C- relative humidity: < 30G - Solar - Irradiance: 830 ± 80 [W / m2] 1. Delta E (before / after test) Radiation @ humid climate (10 days) <2 2 Test - chamber temp: +80 ±3 °C 2. Ink adhesion > 4B- relative humidity: > 40 3. No cracking allowed - Irradiance: 830 ± 80 [W / m2]2) Test duration: 25 days (15 days dry test, 10 days humid climatetest)H - Thermal Thermal Shock Test Machine -40 °C (0.5 hr) -95 °C (0.5 hr), 500 1. Delta E (before / after test)Shock Test cycles 2<22. Ink adhesion > 4B
[0121] Certain existing UV-curable inkjet compatible inks crack or otherwise fail when subjected to such testing conditions, rendering these inks unsuitable for certain automotive interior applications. For example, certain existing inks have been found to shrink and / or crack when subjected to Test B contained in the Table 4 above, while opaque layers formed from the photocurable ink compositions and / or ink primers described herein meet the testing criteria contained in the Table 4.
[0122] In embodiments, the glass article exhibits a maximum AE value (both SCI and SCE), measured both prior to and after 500 1 hour cycles of being held at a temperature of -40°C for 0.5 hours and a temperature of 95°C for 0.5 hours, less than 2.0
[0123] In addition to meeting the aforementioned reliability testing requirements, the photocurable ink compositions and / or ink primers described herein may meet additional requirements to render them suitable for use with certain commercially available inkj et printers. For example, the pigment may comprise an average particle size less than or equal to 200 nm (e.g., from 150 nm to 180 nm) to achieve a desirable L*. In embodiments, the photocurable ink and / or in the ink primer may comprise a liquid surface tension greater than or equal to 25 dynes / cm and less than or equal to 35 dynes / cm. In embodiments, the opaque layer may exhibit a cured surface tension greater than 36 dynes / cm. In embodiments, the opaque layer may exhibit an electrical resistivity greater than or equal to IxlO9Q / sq, when measured according to ASTM D-257 at 100V DC.
[0124] The opaque layers described herein may also exhibit a pencil hardness of greater than or equal to 3H when measured according to ASTM 3363, entitled “Standard Test Method for Film Hardness by Pencil Test,” hereby incorporated by reference in its entirety, with a 750 g weight and the pencil at a 45° angle, after curing with a narrowband UV LED light sourceAttorney Docket No. : SP25-093PCTemitting narrowband (e.g., less than or equal to 20 nm bandwidth, less than or equal to 30 nm bandwidth) curing light. Use of such UV LEDs saves space, cost, and is less environmentally harmful when compared with certain existing UV curing lamps. Certain existing UV-curing inks may not sufficiently cure to have such a pencil hardness due when meeting the optical density requirements described herein due to opacity of the ink inhibiting curing. The photoinitiators of the inks and / or ink primers described herein may be selected to facilitate curing using UV LEDs, while still meeting the pencil hardness and optical density requirements described herein.
[0125] As such, the photocurable inks and / or ink primers described herein are able to provide relatively high optical density to facilitate efficacy as a black matrix layer in a display, while being compatible with high throughput inkjet printing process and also meeting stringent reliability testing requirements associated with automotive interior displays. The photocurable inks and / or ink primers described herein save fabrication costs for display glass articles while still providing highly reliable opaque layers demonstrated to provide consistent color performance over the lifetime of the component.
[0126] Methods of Fabricating Glass Article
[0127] Referring now to FIG. 3, a method of fabricating a glass article is shown at 300. The method 600 may be performed to fabricate the glass article 400 described herein with respect to FIG. 2. Accordingly, reference will be made to various components described with respect to FIG. 2 to aid in the description of the method. It should be understood that other glass articles may be formed via performance of the method 600 and that the method 600 is not limited to a particular number or order of process steps.
[0128] At block 602, the substrate 450 is fabricated. Any suitable glass production process, such as a fusion down draw process, a float process, or the like may be used. Additional details regarding glass forming methods are provided herein. At block 604, the substrate 450 is treated. For example, in embodiments, the substrate 450 is subjected to a strengthening treatment (e.g., ion exchange strengthening, thermal strengthening).
[0129] In embodiments, the treatments applied to the substrate 450 during the block 604 may be used to form the functional surface layer 490. For example, in embodiments, substrate 450 is chemically etched such that at least the first surface 470 exhibits anti-glare properties. A suitable anti -reflective coating and / or ETC coating may also be deposited onto the first surfaceAttorney Docket No. : SP25-093PCT470 via a suitable deposition process. In embodiments, the second surface 480 may be primed (e.g., using a suitable chemical primer or ink) to facilitate adhesion of the opaque layer 500 thereto. In embodiments, the light management layer 460 may be deposited and cured onto the second surface 480 (e.g., a suitable ink may be cured thermally or via exposure to electromagnetic radiation).
[0130] At block 606, a photocurable ink is prepared and deposited onto the second surface 480 to initiate forming the opaque layer 500. In aspects, to prepare the photocurable ink a pigment dispersion can be mixed with the remaining components of the ink composition. Preparing the photocurable ink can include forming the pigment dispersion, which can include adding the desired amount of monomer an dispersant into a commercially available dispermat. The desired amount of pigment can then be added with an appropriate amount of griding media (e.g., 1.5 mm zirconia grinding media). Grinding can then occur for a suitable time period to achieve a particle size less than 200 nm for the pigment. After the dispersion is formed, it can be mixed with the remainder of the components of the ink composition diescribed herein in desired amounts.
[0131] A suitable inkjet printing device may be used to deposit droplets of a suitable size onto the second surface 480 such that the photocurable ink forms a suitable pattern. Various parameters used to operate the inkjet printing device (e.g., control waveform, translation rate, deposition temperature) may vary depending on the composition of the photocurable ink and desired deposition pattern. As noted with respect to block 604, the second surface 480 may have an ink primer applied thereto prior to deposition of the photocurable ink.
[0132] At block 608, the photocurable ink is cured on the second surface 480 via exposure to electromagnetic radiation generated by a UV LED. In embodiments, the UV LED emits radiation having a relatively narrow bandwidth (e.g., less than or equal to 50 nm, less than or equal to 40 nm, less than or equal to 30 nm, less than or equal to 20 nm) surrounding a center UV wavelength (e.g., 375 nm, 380 nm, 385 nm, 390 nm, 395 nm, 400 nm). Operational parameters of the UV LED (e.g., output intensity, exposure period) may vary depending on various aspects of the opaque layer 500 (e.g., thickness, composition).
[0133] In embodiments, the blocks 606 and 608 may be performed while the substrate 450 comprises a planar shape. In embodiments, the blocks 606 and 608 are performed while the substrate is in a curved shape. For example, after application of at least some of the treatmentsAttorney Docket No. : SP25-093PCTdescribed with respect to the block 604, the substrate 450 may be cold-formed via the methods described herein, and the opaque layer 500 may be formed on a cold-formed glass substrate. In embodiments, a suitable display panel is laminated to the glass article such that the opaque layer 500 at least partially covers the display panel.
[0134] Given the relatively high pigment concentration in each of the ink compositions, it may be beneficial to use a multi-print and cure architecture to cure the photocurable described herein. Such an architecture is described in U.S. Patent Publication No. 2025 / 0019556A1.Examples
[0135] In order that various embodiments be more readily understood, reference is made to the following examples, which are intended to illustrate various embodiments of ink compositions and ink primers described herein.
[0136] Pigment Dispersion
[0137] Example pigment dispersions were formed using the following process. First, a desired amount of monomer (ranged from 30 wt% to 70 wt% in various examples) and dispersant (ranged from 10 wt% to 30 wt% in various examples) were added into a BYK® Dispermat APS vessel. An amount of 1.5mm zirconia griding media was also added to the vessel. The vessel was then placed under the BYK Dispermat with the spindle already attached. The spindle was then lowered into vessel and spun at 350 rpms to mix the dispersant and monomer for 15mins. Then, the desired amount of carbon black was added. The spindle was then spun at 350rpms for 19-20 hours to do the appropriate amount of dispersing / grinding. The vessel was kept at a constant 25C using a chiller during all operation. The final pigment concentration in the monomer ranged from 25-35%. The particle size of the carbon black in the dispersion was <200 nm. Indeed, the particle of the carbon black pigment in the ink was 150nm-180 nm, which is suitable for jetting from the inkjet printheads. An example pigment dispersion, which allowed the greatest amount of pigment dispersion while obtaining the lowest viscosity, is provided in the Table 5.Attorney Docket No. : SP25-093PCT
[0138] Table 5Component Amount (wt %)33%Cabot Mogul E17%BYK 9152 Dispersant50%MPDDA 3-Methyl-l,5-pentanediyl diacrylate
[0139] A viscosity curve for the above example pigment dispersion is provided in FIG. 4. As shown, the pigment dispersion exhibits a viscosity that is greater than or equal to 100 cPs is less than or equal to 350 cPs over a temperature range from 30°C to 50°C. At a common jetting temperature of 45°C, the viscosity of the pigment dispersion is less than or equal to 200 cPs. Such a viscosity facilitates forming an ink composition that is suitable for use with production inkjet printheads.
[0140] Ink Composition
[0141] An example ink composition was formulated using the pigment dispersion described in table 5. The composition details are provided in the Table 6
[0142] Table 6ComponentHigh Pigment Dispersion 32819 BIS(2,4,6- TRIMETHYLBENZOYL)PHENYLPHOSPHINE 4OXIDE (IGM Resins)ITX 2-isopropylthioxanthone (IGM Resins) 2EDB Ethyl 4-(dimethylamino) benzoate (IGM Resins) 2Vmox Vinyl methyl oxazolidinone (BASF) 20M600 DPHA dipentaerythritol hexaacrylated (Miwon) 4Attorney Docket No. : SP25-093PCTM222 DPGDA dipropylene glycoldiacrylate (Miwon)or MPDDA 3-Methyl-l,5- 36pentanediyl diacrylate (Allnex)Total 100
[0143] A viscosity curve for the above ink composition is provided in FIG. 5. As shown, the pigment dispersion exhibits a viscosity that is less than or equal to 15 cPs over a temperature range from 30°C to 50°C. At a common jetting temperature of 45°C, the viscosity of the pigment dispersion is less than or equal to 13 cPs. Such a is suitable for use with production inkjet printheads.
[0144] Samples generated according to the Example described in Table 6 were cured on a glass substrate via expsosure to UV radiation and then measured for optical density of the resultant opaque layers using a densitometer. When the thickness was 8.8 pm, the optical density was mreasued to be approximately 3.97. When the thickness was 11.6, the optical density was mreasured to be 5. The Example thus meets the stringent optical density requirements described herein when having a low thickness of less than 15 pm. A sample formed from the Example described in Table 6 was also deposited on a glass substrate that was wipe coated to have methacryloxy silane-based primer. This same was tested for adhesion. The results are provided in FIG. 6. As shown, the sample passed the adhesion test (adhesion of 5B when measured according to ASTM 3359).
[0145] It will be apparent to those skilled in the art that various modifications and variations may be made to the embodiments described herein without departing from the spirit and scope of the claimed subj ect matter. Thus, it is intended that the specification cover the modifications and variations of the various embodiments described herein provided such modification and variations come within the scope of the appended claims and their equivalents.
Claims
Attorney Docket No. : SP25-093PCTCLAIMS1. An ultraviolet curable ink composition comprising, based on a total weight of the ultraviolet curable ink composition:a pigment in an amount greater than or equal to 11 wt% and less than or equal to 20 wt%;a dispersant in an emount greater than or equal to 3 wt% and less than or equal to 10 wt% dispersant;a type I photoinitiator in an amount in a range from 1 wt% to 6 wt%;a type II photoinitiator in an amount in a range from 1 wt% to 6 wt%;an amine synergist in an amount in a range from 1 wt% to 4 wt%;a reactive diluent in an amount greater than or equal to 10 wt% and less than or equal to 42 wt%;a multifunctional monomer in an amount greater than or equal to 2 wt% and less than or equal to 20 wt%; anda total difunctional monomer content that is greater than or equal to 10 wt% and less than or equal to 75 wt%.
2. The ultraviolet curable ink composition of claim 1, wherein the total difunctional monomer content is greater than or equal to 50 wt%.
3. The ultraviolet curable ink composition of any one of claims 1-2, wherein the multifunctional monomer is present in an amount less than 5 wt%.
4. The ultraviolet curable ink composition of any one of claims 1-3, wherein the pigment is present in an amount that is less than or equal to 13 wt%.
5. The ultraviolet curable ink composition of any one of claims 1-4, wherein a total monomer content of the ink composition excluding the reactive diluent, calculated by combining amounts of monofunctional monomer, difunctional monomer, and multifunctional monomer in the ink composition, is greater than or equal to 50 wt% and less than or equal to 80 wt%.Attorney Docket No. : SP25-093PCT6. The ultraviolet curable ink composition of claim 5, wherein the reactive diluent consists of one or more A-vinyl monomers, so that the total monomer content excludes the N-vinyl monomers.
7. The ultraviolet curable ink composition of any one of claims 1-6, wherein the multifunctional monomer is present in an amount that is greater than or equal to 4 wt% and less than or equal to 10 wt%.
8. The ultraviolet curable ink composition of any one of claims 1-7, wherein the ultraviolet curable ink composition is free of resin and free of TPO.
9. The ultraviolet curable ink composition of any one of claims 1 -8, wherein the ultraviolet curable ink composition exhibits a viscosity greater than or equal to 8 cPs and less than or equal to 15 cPs at a temperature of 45°C.
10. A glass article comprising:a glass substrate having a first major surface and a second major surface, the second major surface being opposite the first major surface; andan opaque layer disposed on the second major surface, the opaque layer being a cured layer of the ink composition according to any of claims 1-9, such that the opaque layer is formed completely of monomeric subunits, wherein:the opaque layer comprises a thickness less than or equal to 15 pm and an optical density greater than or equal to 5.0, andafter curing solely via exposure to ultraviolet (“UV”) radiation, the opaque layer exhibits:a pencil hardness greater than or equal to 3H, when measured according to ASTM 3363, andan adhesion to the glass substrate greater than or equal to 4B, after being subjected to a temperature of 85°C at 95% relative humidity for a period of at least 500 hours, when tested according to ASTM 3359.
11. The glass article of claim 10, wherein the glass article exhibits:a CIELAB SCI L* value less than or equal to 30, when illuminated at a 10° angle by a D65 illuminant,Attorney Docket No. : SP25-093PCTa CIELAB SCI a* value greater than or equal to -0.05 and less than or equal to 0.15, anda CIELAB SCI b* value greater than or equal to -0.3 and less than or equal to -0.1, when illuminated at a 10° angle by a D65 illuminant.
12. The glass article of any of claims 10-11, wherein after 500 1 hour cycles of being held at a temperature of -40°C for 0.5 hours and a temperature of 95°C for 0.5 hours, the opaque layer exhibits an adhesion to the glass substrate greater than or equal to 4B, when tested according to ASTM 3359, wherein the glass article exhibits a maximum AE value (both SCI and SCE), measured both prior to and after the 500 1 hour cycles, less than 2.0.
13. A method of preparing an ink composition comprising:mixing a pigment dispersion with additional components of the ink composition so that the pigment dispersion is contained in the ink composition in an amount in a range from 25 wt% to 50 wt%, wherein the pigment dispersion, prior to the mixing, comprises:a pigment having a particle size of less than 200 nm, the pigment being contained in the pigment dispersion in an amount that is greater than or equal to 25 wt% and less than or equal to 35 wt %;a dispersant in an amount in a range from 10 wt% to 30 wt%; and one or more monomers in an amount in a range from 30 wt% to 70 wt%, wherein the additional components comprise:greater than 0 wt% and less than or equal to 10 wt% of a photoinitiator package, the photoinitiator package comprising a type I photoinitiator, a type II photoinitiator, and an amine synergist;greater than or equal to 10 wt% and less than or equal to 42 wt% of a reactive diluent, the reactive diluent comprising a viscosity less than 5 cPs at 25°C;greater than or equal to 2 wt% and less than or equal to 20 wt% of a multifunctional monomer; andgreater than or equal to 0 wt% and less than or equal to 40 wt% of a difunctional monomer, wherein at least one of the one or more monomers in the pigment dispersion is a pigment difunctional monomer such that, after the mixing, the ink composition comprises a total difunctional monomer content that is greater than or equal to 10 wt% and less than or equal to 75 wt%.Attorney Docket No. : SP25-093PCT14. The method of claim 13, wherein, after the mixing, the pigment is present in the ink composition in an amount that is greater than or equal to 11 wt% and less than or equal to 20 wt%.
15. The method of any of claims 13-14, wherein, the pigment is a carbon black pigment and has a d50 particle size that is greater than or equal to 100 nm and less than or equal to 200 nm.
16. The method of claim 15, wherein the d50 particle size is greater than or equal to 160 nm and less than or equal to 180 nm.
17. The method of any one of claims 13-16, wherein the ultraviolet curable ink composition is free of resin and free of TPO.
18. The method of any one of claims 13-17, wherein, after the mixing, the ultraviolet curable ink composition exhibits a viscosity greater than or equal to 8 cPs and less than or equal to 15 cPs at a temperature of 45°C.
19. The method of any one of claims 13-18, wherein:the pigment dispersion comprises from 40 wt% to 70 wt% of the pigment difunctional monomer, andafter the mixing, the total difunctional monomer content is greater than or equal to 50 wt%.
20. The method of any one of claims 13-19, wherein, after the mixing, the multifunctional monomer is present in an amount less than 5 wt%.
21. The method of any one of claims 13-20, wherein, after the mixing the pigment is present in an amount that is less than or equal to 13 wt%.Attorney Docket No. : SP25-093PCT22. The method of any one of claims 13-21, wherein a total monomer content of the ink composition excluding the reactive diluent, calculated by combining amounts of monofunctional monomer, difunctional monomer, and multifunctional monomer in the ink composition, is greater than or equal to 50 wt% and less than or equal to 80 wt%.
23. The method of claim 22, wherein the reactive diluent consists of one or more TV- vinyl monomers, so that the total monomer content excludes the N-vinyl monomers.
24. The method of any of claims 13-23, wherein, after the mixing, the multifunctional monomer is present in an amount that is greater than or equal to 4 wt% and less than or equal to 10 wt%.
25. The method of any of claims 13-24, wherein, prior to the mixing, the pigment dispersion exhibits a viscosity that greater than or equal to 100 cPs is less than or equal to 350 cPs over a temperature range from 30°C to 50°C.