Membrane electrode assembly architecture for stabilizing precious metal-free materials in proton exchange membrane
The MEA architecture with AEI-stabilized transition metal catalysts addresses the high costs and instability of PEMWEs by creating a spatial pH gradient, enhancing catalyst stability and reducing overpotential losses, thus achieving efficient PGM-free hydrogen production.
Patent Information
- Application Number
- PCT/US2026/027535
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-12
- Filing Date
- 2026-05-11
- Publication Date
- 2026-11-19
AI Technical Summary
Current proton exchange membrane water electrolyzers (PEMWEs) rely on precious metals like iridium for oxygen evolution reaction (OER), leading to high hydrogen production costs and material instability in acidic environments, necessitating the development of cost-effective, stable, PGM-free catalysts and systems.
An anode catalyst layer comprising transition metal catalysts, such as Co₃O₄, dispersed in an anion exchange ionomer (AEI) with a local alkaline pH, creating a spatial pH gradient within the catalyst layer to stabilize the catalysts and facilitate OER, eliminating the need for additional water dissociation catalysts.
The proposed membrane electrode assembly (MEA) architecture with AEI-stabilized transition metal catalysts achieves stable operation at high current densities and reduces overpotential losses, extending the catalyst's durability and reducing the reliance on precious metals.
Smart Images

Figure US2026027535_19112026_PF_FP_ABST
Abstract
Description
Reference No.: 2025-793-2, UCI 25.08 PCTInventor’s last name: Zenyuk et alDocument Date: May 8, 2025MEMBRANE ELECTRODE ASSEMBLY ARCHITECTURE FOR STABILIZING PRECIOUS METAL-FREE MATERIALS WITHIN A CATALYST LAYER IN PROTON EXCHANGE MEMBRANE WATER ELECTROLYZERS CROSS-REFERENCE TO RELATED APPLICATIONS
[0001] This application claims benefit of U.S. Provisional Application No. 63 / 804,061 filed May 12, 2025, the specification(s) of which is / are incorporated herein in their entirety by reference.FIELD OF THE INVENTION
[0002] The present invention relates to water electrolysis, in particular, to a membrane electrode assembly (MEA) architecture to stabilize platinum group metal (PGM)-free materials for operation in a modified PEM water electrolyzer.BACKGROUND OF THE INVENTION
[0003] Rising global energy demands and climate change challenges have accelerated efforts to develop clean and sustainable energy carrier alternatives to fossil fuels. Hydrogen is a promising energy vector, as it has a high caloric energy value and high gravimetric energy density. It can be used as a fuel across various sectors. Currently, the majority of it is produced in a steam-methane reforming process, but a promising alternative is water electrolysis, which produces hydrogen (Hz) using water and low-carbon emissions electricity. Hydrogen then can be used in industries that are difficult to decarbonize, such as energy, transportation, chemical manufacturing, and agriculture. Among many electrolyzers present on the market, proton exchange membrane water electrolyzers (PEMWE) have the advantages of operating at high differential pressures, using smaller footprint stacks, and operating at higher current densities.
[0004] The oxygen evolution reaction (OER) is sluggish and uses large overpotentials in PEMWEs. Currently, precious materials like iridium are employed as OER catalysts in PEMWEs, resulting in high hydrogen production costs. The U.S. Department of Energy's hydrogen production cost target is set at $1 per kilogram by 2031. Achieving this goal requires either reducing the iridium loading in the catalysts or finding suitable, cost-effective alternatives to iridium. Therefore, it is essential to develop efficient andReference No.: 2025-793-2, UCI 25.08 PCTInventor’s last name: Zenyuk et alDocument Date: May 8, 2025durable anode catalyst layers that do not rely on iridium or other platinum group metals (PGMs) for PEMWEs.
[0005] A strong emphasis has been placed on using cost-effective materials, such as transition metals, due to their variable oxidation states and activities across a broad pH range. Perfluorosulfonic acid (PFSA) polymers like Nation™ and Aquivion® are commonly used as binders in catalyst layers. This means PEMWE functions in highly acidic environments (pH ~ 0-3). Such extreme conditions pose significant challenges in finding new materials, as most, apart from iridium and other PGM materials, have shown little durability under these harsh conditions. Transition metal catalysts are not stable in acidic environments, as thermodynamics indicates. Significant efforts focus on discovering or synthesizing new materials to reduce their dissolution. Key advancements have been made to integrate durable PGM-free materials. These include strengthening the metal-oxide (M-O) bonds within the y-MnO2structure (M94%), implementing water-hydroxide bridges to mitigate ion leaching from the crystal lattice (CWO-del-48), modifying the active sites of spinel Co3O4by doping with lanthanum and manganese (LMCF); and enhancing electron transport by introducing halogens in manganese oxides (Mn75O10Br3).
[0006] Some research studies have focused on developing bipolar membrane water electrolyzers that operate at two different pH levels at the anode and cathode. The goal is to effectively integrate cost-effective materials as anodes under alkaline operation since these materials remain stable in alkaline conditions. However, these systems often require a water dissociation (WD) catalyst to dissociate water into H+and OH-ions, where OH-ions transport to the anode to create a local alkaline pH for OER. This results in additional overpotential losses, especially when the system needs to operate at higher current densities. Efforts have been made to reduce these overpotential losses by decreasing the thickness of components, such as membranes, effectively achieving an interface of a few microns compared to using a relatively thicker 40 pm membrane. Alternatively, these losses can be further reduced by exploring various other WD catalysts and optimizing the thickness of WD catalysts. However, these systems either involve an additional layer of WD catalysts and / or rely on precious materials, such as lrOx, to conduct the reaction. Hence, there is a need for novel systems that canReference No.: 2025-793-2, UCI 25.08 PCTInventor’s last name: Zenyuk et alDocument Date: May 8, 2025decrease the loading of iridium used in the PEMWE system or to substitute it with non-precious alternatives, such as various transition materials.BRIEF SUMMARY OF THE INVENTION
[0007] It is an objective of the present invention to provide systems and devices that allow for PGM-free water electrolysis, as specified in the independent claims. Embodiments of the invention are given in the dependent claims. Embodiments of the present invention can be freely combined with each other if they are not mutually exclusive.
[0008] According to some embodiments, the present invention features an anode catalyst comprising at least one transition metal catalyst disposed in a substrate having a local alkaline pH. In some embodiments, the substrate comprises an anion exchange ionomer (AEI) or ionic liquid. In other embodiments, the at least one transition metal catalyst is dispersed in the AEI.
[0009] In some embodiments, the AEI may comprise a polymer backbone functionalized with alkaline groups. Without wishing to be bound to a particular theory or mechanism, the functionalized polymer backbone is effective for facilitating conduction of anions while remaining stable under alkaline conditions. In some embodiments, the polymer backbone may comprise poly(aryl piperidinium) (PAP), poly(ethylene) (PE), polystyrene (PS), polysulfones (PS), poly(phenyleneoxide)s (PPO), poly(phenylene)s (PP), poly(fluorene) (PF), poly(ethylene-co-tetrafluoroethylene) (EFTE), polybenzylimidazole (PBI), ora combination thereof.
[0010] In non-limiting embodiments, a weight ratio of the substrate to the transition metal compound ranges from about 0.05 to about 0.45.
[0011] In some embodiments, the transition metal catalyst may comprise Co3O4, cobalt oxides doped with nickel, manganese, or copper, or other platinum group metal (PGM)-free metal oxides, or mixed oxides of Co or Ni. In other embodiments, the anode catalyst is free of platinum group metal (PGM)-based materials.
[0012] According to other embodiments, the present invention features an anode comprising an anode catalyst in contact with a proton exchange membrane (PEM). The anode catalyst may comprise at least one transition metal catalyst disposed in a substrate such that the substrate is interfacing the PEM.Reference No.: 2025-793-2, UCI 25.08 PCTInventor’s last name: Zenyuk et alDocument Date: May 8, 2025
[0013] In some embodiments, the substrate is an anion exchange ionomer (AEI), wherein the AEI has a local alkaline pH, wherein the anode catalyst is an anode catalyst layer (ACL) comprising the at least one transition metal catalyst dispersed in the AEI, wherein the ACL is disposed on a porous transport layer (PTL) and interfacing the PEM.
[0014] According to other embodiments, the present invention features a water electrolyzer comprising an anode, a cathode operatively coupled to the anode, and a proton exchange membrane (PEM) interposed between said anode and said cathode. The anode may comprise an anode catalyst in contact with a porous transport layer (PTL), said anode catalyst comprising at least one transition metal catalyst disposed in a substrate having a local alkaline pH. In some embodiments, the substrate comprises an anion exchange ionomer (AEI). The anode catalyst may be an anode catalyst layer (ACL) comprising the at least one transition metal catalyst dispersed in the AEI. The ACL (105) is interfacing the PTL (110) and the PEM is facing the ACL. In some embodiments, the water electrolyzer is utilized in an oxygen evolution reaction.
[0015] In other embodiments, the water electrolyzer may further comprise an AEI interlayer coating the ACL (105) such that the AEI interlayer is disposed between the ACL (105) and the PEM (130). In some other embodiments, the water electrolyzer may further comprise a source of electrical energy configured to apply a voltage between the anode and cathode.
[0016] In some embodiments, the AEI may comprise a polymer backbone functionalized with alkaline groups. The functionalized polymer backbone may be effective for facilitating conduction of anions while remaining stable under alkaline conditions. In some embodiments, the polymer backbone comprises poly(aryl piperidinium) (PAP), poly(ethylene) (PE), polystyrene (PS), polysulfones (PS), poly(phenyleneoxide)s (PPO), poly(phenylene)s (PP), poly(fluorene) (PF), poly(ethylene-co-tetrafluoroethylene) (EFTE), polybenzylimidazole (PBI), ora combination thereof.
[0017] In non-limiting embodiments, the substrate may comprise an alkaline ionic liquid effective for facilitating conduction of anions while remaining stable under alkaline conditions. The transition metal catalyst may be dispersed in the alkaline ionic liquid. In some embodiments, the transition metal catalyst comprises Co304, cobalt oxides doped with nickel, manganese, or copper, or other platinum group metal (PGM)-free metal oxides, or mixed oxides of Co or Ni. In other embodiments, the PTL is Pt-coated.Reference No.: 2025-793-2, UCI 25.08 PCTInventor’s last name: Zenyuk et alDocument Date: May 8, 2025
[0018] In other embodiments, the cathode is a catalyst-coated membrane. In a non-limiting embodiment, the catalyst-coated membrane may comprise Pt / C disposed on a cation exchange membrane.
[0019] The present invention emphasizes the stabilization of electrode materials made from transition metals that are prone to rapid dissolution and focuses on enhancing their durability during PEM water electrolysis operations. The local microenvironment in the anode was tuned by incorporating an anion exchange ionomer (AEI) into the anode catalyst layer to stabilize transition metal catalysts without an additional WD layer. Therefore, rather than tailoring the catalysts themselves, the operational environment of the catalysts is being modified where they remain stable and integrating this architecture into a PEMWE that uses a standard Nation™ membrane, as summarized in FIG. 1. In some embodiments, the local microenvironment is modified by adjusting the local pH to levels that can achieve stability.
[0020] Due to the heterojunction created by the fixed charges, a potential gradient is established where one end of the interface is highly alkaline due to the AEI, and the other is highly acidic due to the Nation™ membrane. This leads to a spatial pH gradient within the catalyst layer, as depicted in part d of FIG. 1. Without wishing to limit the invention to any theory or mechanism, it is believed that this technical feature of the present invention provides two potential mechanisms for OER in such catalyst layer: i) acidic pathway for OER, as the local environment created by the addition of AEI might not be sufficiently alkaline; ii) alkaline pathway for OER, where water is dissociated at the PEM-AEI interface and OH- are transported to active sites of Co3O4. Both mechanisms are schematically shown in parts c and d of FIG. 1.
[0021] Any feature or combination of features described herein are included within the scope of the present invention provided that the features included in any such combination are not mutually inconsistent as will be apparent from the context, this specification, and the knowledge of one of ordinary skill in the art. Additional advantages and aspects of the present invention are apparent in the following detailed description and claims.BRIEF DESCRIPTION OF THE SEVERAL VIEWS OF THE DRAWING(S)
[0022] The features and advantages of the present invention will become apparent fromReference No.: 2025-793-2, UCI 25.08 PCTInventor’s last name: Zenyuk et alDocument Date: May 8, 2025a consideration of the following detailed description presented in connection with the accompanying drawings in which:
[0023] FIG. 1 shows a non-limiting embodiment of the present invention that is a membrane electrode assembly (MEA) incorporating PGM-free materials as anodes with anion exchange ionomers (AEI) in the catalyst layer, featuring a close-up of the anode section of the cell in (b), along with potential mechanisms for the oxygen evolution reaction (OER) illustrated in (c) for acidic OER and (d) for water dissociation and alkaline OER.
[0024] FIGs. 2A-2B is a comparison of the polarization curves and corresponding HFR values for the same catalyst, 1.5 mg / cm2Co3O4, utilizing two different ionomers, Nation™ and PiperlON®, while maintaining the same Ionomer to Catalyst (l / C) ratio. Nation™ inks (PEI) and Nation™ membranes (PEM) replicate conventional PEM water electrolysis operation, whereas PiperlON® inks (AEI) and membranes (AEM) replicate conventional AEM water electrolysis operation, along with 0.1 M KOH feed shown as comparison. The modified operation employs an AEl-based catalyst layer and integrates it into a PEM water electrolyzer assembly with a DI water feed.
[0025] FIG. 3A shows polarization curves comparing different l / C ratios for the same catalyst, 1.55 ± 0.05 mg / cm2C03O4.
[0026] FIG. 3B shows a corresponding zoomed-in HFR-free voltage in the activation region.
[0027] FIG. 3C shows the durability, measured in hours, under a constant current density hold of 200 mA / cm2that the cell lasted for each l / C ratio.
[0028] FIGs. 4A-4C show post-mortem MEA cross-sectional SEM images along with EDS mapping to examine the interfacial morphology and elemental distribution across various layers, as well as to identify compositional variations when comparing aged electrodes prepared with AEI (PiperlON®) l / C ratio 0.2 (FIG. 4A), l / C ratio 0.3 (FIG. 4B), and l / C ratio 0.4 (FIG. 4C).
[0029] FIG. 4D is a comparison of polarization curves at the beginning of life (BOL) and at the end of life (EOL) for Co3O4, with an l / C ratio of 0.2.
[0030] FIG. 4E is a comparison of the performance of the modified design with state-of-the-art catalysts under DI water operation at 80°C showing the required cell voltage to achieve a current density of 1 A. cm2at BOL. Nation™ ionomer is employed: LMCF using Nation™ 212 membrane, M94% using Nation™ 212 membrane, andReference No.: 2025-793-2, UCI 25.08 PCTInventor’s last name: Zenyuk et alDocument Date: May 8, 2025CWO-del-48 using Nation™ 117 membrane.
[0031] FIG. 5 is a comparison of cell voltage profile during the conditioning process of holding the cell at 200 mA / cm2for 90 minutes with the same catalyst, 1.55 ± 0.05 mg / cm2 Co3O4, but using Nation™ ionomer (PEI, red curve) and PiperlON® ionomer (AEI, blue curves with differing l / C ratios). PEI-based inks lead to rapid performance degradation during the conditioning process compared to AEl-based inks.
[0032] FIGs. 6A-6C show performance curves, which include: (FIG. 6A) the polarization curves along with their HFR-free values and corresponding HFR values, (FIG. 6B) cell voltage for 90-minute conditioning process by holding the cell at a constant 200 mA cm-2, and (FIG. 6C) the zoomed-in CV plots at the beginning of life (BOL) comparing PAA, Nation™, and PiperlON® ionomers within the anode of the PEMWE.
[0033] FIG. 7A illustrates a schematic and resulting architecture featuring a 10% by weight AEI Interlayer (IL) on the catalyst layer, prepared with an l / C ratio of 0.2.
[0034] FIG. 7B shows the polarization curves and the corresponding HFR values for the configurations with and without an interlayer. The HFR values are an order of magnitude higher for the system with the interlayer.
[0035] FIGs. 8A-8C show durability plots comparing the cell voltage profile for different l / C ratios at a current density hold of 200 mA.cnr2for (FIG. 8A) l / C: 0.2, (FIG. 8B) l / C: 0.3, and (FIG. 8C) l / C: 0.4. The voltage spikes represent the times of intermittent characterization approximately every 24 hours or potentiostat restart events. For all l / C ratios, the stabilized voltage is around 1.7 V.
[0036] FIGs. 9A-9C show performance curves, which include (FIG. 9A) the polarization curve along with its corresponding HFR values, (FIG. 9B) the Cyclic Voltammetry (CV) plot, and (FIG. 9C) the zoomed-in CV plot at the beginning of life (BOL) comparing the different l / C ratios.
[0037] FIGs. 10A-10C show performance curves, which include (FIG. 10A) the polarization curve along with its corresponding HFR values, (FIG. 10B) the Cyclic Voltammetry (CV) plot, and (FIG. 10C) the zoomed-in CV plot after about 24 hours of operation comparing the different l / C ratios.
[0038] FIGs. 11A-11C show performance curves, which include (FIG. 11A) the polarization curve along with its corresponding HFR values, (FIG. 11 B) the Cyclic Voltammetry (CV) plot, and (FIG. 11 C) the zoomed-in CV plot after about 48 hours of operation comparing the different l / C ratios.Reference No.: 2025-793-2, UCI 25.08 PCTInventor’s last name: Zenyuk et alDocument Date: May 8, 2025
[0039] FIGs. 12A-12C show performance curves, including (FIG. 12A) the polarization curves along with their HFR-free values and corresponding HFR values, (FIG. 12B) the 90-minute conditioning process by holding the cell at a constant 200 mA-cnr2, and (FIG.12C) the zoomed-in CV plots comparing the electrode prepared with AEI with an l / C ratio of 0.2 at BOL and after about 48 hours of operation with an electrode prepared without ionomer.
[0040] FIGs. 13A-13C show performance curves, which include (FIG. 13A) the polarization curve along with its corresponding HFR values, (FIG. 13B) the Cyclic Voltammetry (CV) plot, and (FIG. 13C) the zoomed-in CV plot after about 75 hours of operation comparing the different l / C ratios.
[0041] FIGs. 14A-14C show performance curves, which include (FIG. 14A) the polarization curve along with its corresponding HFR values, (FIG. 14B) the Cyclic Voltammetry (CV) plot, and (FIG. 14C) the zoomed-in CV plot after about 100 hours of operation comparing the different l / C ratios.
[0042] FIGs. 15A-15C show performance curves, which include (FIG. 15A) the polarization curve along with its corresponding HFR values, (FIG. 15B) the Cyclic Voltammetry (CV) plot, and (FIG. 15C) the zoomed-in CV plot after about 125 hours of operation comparing the two different l / C ratios.
[0043] FIGs. 16A-16C show performance curves for the l / C ratio of 0.4, which include (FIG. 16A) the polarization curve along with its corresponding HFR values, (FIG. 16B) the Cyclic Voltammetry (CV) plot, and (FIG. 16C) the zoomed-in CV plot after about 140 hours and 154 hours of operation respectively.
[0044] FIGs. 17A-17C show performance curves for the l / C ratio of 0.4, which include (FIG. 17A) the polarization curve along with its corresponding HFR values, (FIG. 17B) the Cyclic Voltammetry (CV) plot, and (FIG. 17C) the zoomed-in CV plot after about 178 hours and 205 hours of operation respectively.
[0045] FIGs. 18A-18C show performance curves for the l / C ratio of 0.2, which include (FIG. 18A) the polarization curve along with its corresponding HFR values, (FIG. 18B) the Cyclic Voltammetry (CV) plot, and (FIG. 18C) the zoomed-in CV plot comparing at the beginning of life (BOL) and end of life (EOL).
[0046] FIGs. 19A-19C show performance curves for the l / C ratio of 0.3, which include (FIG. 19A) the polarization curve along with its corresponding HFR values, (FIG. 19B)Reference No.: 2025-793-2, UCI 25.08 PCTInventor’s last name: Zenyuk et alDocument Date: May 8, 2025the Cyclic Voltammetry (CV) plot, and (FIG. 19C) the zoomed-in CV plot comparing at the beginning of life (BOL) and end of life (EOL).
[0047] FIGs. 20A-20C show performance curves for the l / C ratio of 0.4, which include (FIG. 20A) the polarization curve along with its corresponding HFR values, (FIG. 20B) the Cyclic Voltammetry (CV) plot, and (FIG. 20C) the zoomed-in CV plot comparing at the beginning of life (BOL) and end of life (EOL).
[0048] FIGs. 21A-2D show comparisons of HFR-free voltage and current densities at an applied cell voltage of 1.65 V (FIGs. 21A-21 B) and 1.85 V (FIGs. 21C-21D) with varying l / C ratios over time. The cell voltage of 1.65 V was selected to observe the activation region, while 1.85 V was chosen to examine the ‘S’ shape characteristics during the cell operation.
[0049] FIGs. 22A-22C show performance curves include (FIG. 22A) the polarization curve with its corresponding HFR values, (FIG. 22B) the Cyclic Voltammetry (CV) plot, and (FIG. 22C) the zoomed-in CV plot at the end of life (EOL), comparing the PiperlON® inks (AEI) with different l / C ratios (Open Circles) against the Beginning of Life (BOL) NafionTM ink (PEI). The PTL-only polarization curve performance is also included for comparison.
[0050] FIGs. 23A-23C show X-Ray Diffraction (XRD) patterns comparing the films of PEI (Nation) and AEI (PiperlON®) based electrodes when (FIG. 23A) spray deposition, (FIG.23B) anode section of the aged MEA, and (FIG. 23C) the cathode section of the aged MEA, along with the PDF® standard references to identify the pattern phases.
[0051] FIG. 24A show X-Ray Diffraction (XRD) patterns of AEI (PiperlON®) based electrodes focusing on the anode section of the aged MEA.
[0052] FIG. 24B show top-view SEM images along with EDS mapping for the aged anode prepared with AEI (PiperlON®).DETAILED DESCRIPTION OF THE INVENTION
[0053] Following list elements corresponding to a particular element referred to herein:
[0054] 10 water electrolyzer
[0055] 100 anode
[0056] 105 anode catalyst layer (ACL)
[0057] 110 porous transport layer (PTL)
[0058] 120 cathode
[0059] 130 proton exchange membrane (PEM)Reference No.: 2025-793-2, UCI 25.08 PCTInventor’s last name: Zenyuk et alDocument Date: May 8, 2025
[0060] As used herein, PiperlON® membranes and materials are manufactured from functionalized poly(aryl piperidinium) (PAP) polymer.
[0061] As used herein, Nation™ membranes and materials are manufactured from a copolymer of perfluoro-3,6-dioxa-4-methyl-7octene-sulfonic acid and tetrafluoroethylene (Teflon™) backbone, where the side chain terminates in a sulfonic acid (-SO3H).
[0062] As used herein, “alkaline” refers to a pH greater than 7, for example, 9-14.
[0063] Referring now to the figures, the present invention features an anode catalyst comprising at least one transition metal catalyst disposed in a substrate having a local alkaline pH. For example, the anode catalyst may comprise the transition metal catalyst dispersed in an anion exchange ionomer (AEI) or an ionic liquid.
[0064] In some embodiments, the substrate comprises an alkaline AEI. The AEls may comprise a functionalized polymer backbone. In some embodiments, the polymer backbone is functionalized with alkaline groups. Non-limiting examples of the polymer backbone include poly(aryl piperidinium) (PAP), poly(ethylene) (PE), polystyrene (PS), polysulfones (PS), poly(phenyleneoxide)s (PPO), poly(phenylene)s (PP), poly(fluorene) (PF), polybenzylimidazole (PBI), and poly(ethylene-co-tetrafluoroethylene) (EFTE).
[0065] In non-limiting embodiments, the functional groups of the polymer backbone may be a quaternary ammonium (-NR3+) such as trimethylammonium (TMA), N-methyl pyrrolidium (MPY), pyridinium such as N-aryl pyridinium or N-alkyl pyridinium, imidiazolium (IM), methylpiperidinium (MPRD), bi-guanidinium, or phosphonium such as quaternary phosphonium. In a non-limiting embodiment, the AEI may comprise a functionalized poly(aryl piperidinium) (PAP) polymer. For example, the AEI is a PiperlON® polymer.
[0066] In preferred embodiments, the anode catalyst is free of platinum group metal (PGM)-based materials. In a non-limiting embodiment, the transition metal catalyst comprises Co3O4, cobalt oxides doped with nickel, manganese, iron, copper, or other PGM-free metal oxides. For example, the transition metal catalyst may be doped Co3O4, such as those containing Mn. In other embodiments, the transition metal catalyst may comprise mixed oxides, such as those of Co and Ni. According to other embodiments, the present invention features an anode (100) comprising an anode catalyst in contactReference No.: 2025-793-2, UCI 25.08 PCTInventor’s last name: Zenyuk et alDocument Date: May 8, 2025with a porous transport layer (PTL, 110). The anode catalyst may comprise at least one transition metal catalyst disposed in a substrate having a local alkaline pH.
[0067] ln non-limiting embodiments, the substrate is an anion exchange ionomer (AEI). Referring to FIG. 1, the anode catalyst is an anode catalyst layer (ACL, 105) comprising the transition metal catalyst dispersed in the AEI. In some embodiments, the ACL (105) is disposed on a proton exchange membrane (PEM, 130) such that the ACL (105) is interfacing the PEM (130).
[0068] In some embodiments, the AEI comprises a polymer backbone functionalized with alkaline groups. Without wishing to limit the present invention, the AEI is effective for tuning a local microenvironment in the ACL (105) to stabilize the transition metal catalyst. The role of functionalizing polymers is to facilitate conduction of anions while remaining stable under alkaline conditions. Since these systems have primarily been used in alkaline environments, they are sometimes used interchangeably.
[0069] In some embodiments, the polymer backbone may comprise poly(aryl piperidinium) (PAP), poly(ethylene) (PE), polystyrene (PS), polysulfones (PS), poly(phenyleneoxide)s (PPO), poly(phenylene)s (PP), poly(fluorene) (PF), poly(ethylene-co-tetrafluoroethylene) (EFTE), polybenzylimidazole (PBI), or a combination thereof. In other embodiments, the functional groups may be trimethylammonium (TMA), imidiazolium (IM), and methylpiperidinium (MPRD). In a non-limiting embodiment, the AEI may comprise a functionalized poly(aryl piperidinium) (PAP) polymer.
[0070] In other embodiments, the substrate may comprise an alkaline ionic liquid. Without wishing to limit the present invention, the role of the ionic liquid is to facilitate conduction of anions while remaining stable under alkaline conditions. The transition metal catalyst may be dispersed in the alkaline ionic liquid, which is effective fortuning a local pH to stabilize the transition metal catalyst.
[0071] In some embodiments, the transition metal catalyst comprises Co3O4, cobalt oxides doped with nickel, manganese, iron, copper, or other PGM-free metal oxides. For example, the transition metal catalyst may be doped Co3O4, such as those containing Mn. In other embodiments, the transition metal catalyst may comprise mixed oxides,Reference No.: 2025-793-2, UCI 25.08 PCTInventor’s last name: Zenyuk et alDocument Date: May 8, 2025such as those of Co and Ni. In a non-limiting embodiment, the transition metal catalyst may comprise Co3O4.
[0072] In some embodiments, the PTL (110) is Pt-coated. In some embodiments, the ACL (105) is free of platinum group metal (PGM)-based materials.
[0073] In some embodiments, a weight ratio of the PAP polymer to transition metal compound ranges from about 0.05 to 0.45. In other embodiments, a weight ratio of the PAP polymer to transition metal compound ranges from about 0.05 to 0.25. For example, said ratio may be about 0.1 to about 0.2.
[0074] According to some other embodiments, the present invention features a water electrolyzer (10) comprising an anode (100), a cathode (120) operatively coupled to the anode (100), and a proton exchange membrane (PEM,130) interposed between said anode (100) and said cathode (120). The anode (100) may comprise an anode catalyst in contact with a porous transport layer (PTL, 110). In a non-limiting embodiment, the water electrolyzer is utilized for oxygen evolution reaction.
[0075] In some embodiments, the anode catalyst may comprise at least one transition metal catalyst disposed in a substrate having a local alkaline pH. The transition metal catalyst may comprise Co3O4, cobalt oxides doped with nickel, manganese, iron, copper, or other PGM-free metal oxides. For example, the transition metal catalyst may be doped Co3O4, such as those containing Mn. In other embodiments, the transition metal catalyst may comprise mixed oxides, such as those of Co and Ni.
[0076] In some embodiments, the substrate comprises an anion exchange ionomer (AEI). In a non-limiting embodiment, the anode catalyst is an anode catalyst layer (ACL, 105) comprising at least one transition metal catalyst dispersed in the AEI. The ACL (105) is disposed on and interfacing the PEM (130).
[0077] In some embodiments, the AEI may comprise the following backbones that are functionalized by alkaline groups: poly(aryl piperidinium) (PAP), poly(ethylene) (PE), polystyrene (PS), polysulfones (PS), poly(phenyleneoxide)s (PPG), poly(phenylene)s (PP), poly(fluorene) (PF), poly(ethylene-co-tetrafluoroethylene) (EFTE), polybenzylimidazole (PBI), or a combination thereof. In other embodiments, the functional groups may be trimethylammonium (TMA), imidiazolium (IM), andReference No.: 2025-793-2, UCI 25.08 PCTInventor’s last name: Zenyuk et alDocument Date: May 8, 2025methylpiperidinium (MPRD). The AEI is effective for tuning the local microenvironment in the ACL (105) to stabilize the transition metal catalyst.
[0078] In other embodiments, the substrate comprises an ionic liquid. The transition metal catalyst is dispersed in the ionic liquid. Without wishing to limit the present invention, the ionic liquid is effective fortuning a local pH to stabilize the transition metal catalyst.
[0079] In some embodiments, the PTL (110) is Pt-coated. In other embodiments, an AEI interlayer may be coating the ACL (105) such that the AEI interlayer is disposed between the ACL (105) and the PEM (130). In some other embodiments, the water electrolyzer (10) may further comprise a source of electrical energy configured to apply a voltage between the anode and cathode.
[0080] In some embodiments, the cathode (120) is a catalyst-coated membrane. For example, the catalyst-coated membrane may comprise Pt / C disposed on a cation exchange membrane, e.g. a Nation™ membrane.
[0081] EXAMPLES
[0082] The following are non-limiting examples of the present invention. It is to be understood that said examples are not intended to limit the present invention in any way. Equivalents or substitutes are within the scope of the present invention.
[0083] In a non-limiting embodiment, the present invention provides a membrane electrode assembly (MEA) architecture to stabilize PGM-free materials for operation in a modified PEM water electrolyzer. With this modified architecture, the cell voltage reached 1.884 V at 1 A / cm2and sustained over 200 hours of operation at 200 mA / cm2, which is the best result reported thus far for commercial Co3O4.r00841EXPERIMENTAL METHODS AND MATERIALS
[0085] Sintered Porous Transport Layers were purchased from Mott Corporation. Cobalt II III Oxide nanoparticles (Co3O4, >99.5%, 30-50 nm) were purchased from U.S. Research Nanomaterials, Inc. PiperlON® A ionomer dispersion (5 wt%) and 40pm PiperlON® anion exchange membrane were purchased from Versogen. Nation™ 212 membrane and D521 ionomer dispersion (5 wt%) were purchased from Ion Power, Inc. Polyacrylic acid (PAA), with approximately 0.1% cross-linking and an average molecularReference No.: 2025-793-2, UCI 25.08 PCTInventor’s last name: Zenyuk et alDocument Date: May 8, 2025weight of about 450,000 was purchased from Sigma-Aldrich. Platinum supported on carbon decal was purchased from 3M. Freudenberg H23C6 and H23C3 were purchased from the Fuel Cell Store. DI water, 18.2 MQ-cm resistivity, was produced on-site using a Milli-Q system from Millipore.
[0086] Modified PEM Operation
[0087] Preparation of Porous Transport Electrode (PTE) as Anode:
[0088] The Catalyst Coated Substrate (CCS) method is utilized to prepare the anode. For the catalyst ink, a 10 mg / mL ratio of Co304was added to a 1:9 v / v water / nPA solution. To this solution, a 5 wt% PiperlON® A ionomer dispersion was incorporated to achieve the desired l / C ratio. No pre-treatment of the PiperlON® A ionomer dispersion was done in this study. A similar method was employed for fabricating catalyst inks using the Nation™ D521 solution. The resulting ink was bath-sonicated for at least 60 minutes before being transferred into a hand-held airbrush linked to an air compressor. The platinum-sputtered bare PTLs were trimmed to a precise area of 6.25 cm2and weighed before spraying to determine the bare weight. The inks were sprayed onto the PTL substrate in multiple passes until a loading of 1.5 mg / cm2was reached by measuring the difference between the final and bare weights. For PAA-based electrodes, a 10 wt% PAA dispersion was prepared by adding 0.5 grams of PAA to 4.5 grams of a 7:3 waternPA solution, then stirring at room temperature until a clear dispersion was achieved. Catalyst inks were prepared using this PAA dispersion following a method similar to the one described above. The resulting inks were stirred overnight at room temperature before being sprayed onto the platinum-sputtered bare PTLs.
[0089] Preparation of Cathode:
[0090] The cathode electrode was prepared using a catalyst-coated membrane (CCM) approach. The standard and commercially available 0.12 mg / cm2Pt / C decal from 3M was utilized as the cathode. 6.25 cm2of this Pt / C decal was transferred onto a 25 cm2section of the as-received Nation™ 212 membrane, removing the protective film and backing layer of the Nation™ 212 membrane (thickness ~50pm), and then hot-pressed for 5 minutes at 130°C. The decal substrate was removed, and this half CCM membrane electrode was used as the cathode without any additional pre-treatment during cell assembly.Reference No.: 2025-793-2, UCI 25.08 PCTInventor’s last name: Zenyuk et alDocument Date: May 8, 2025
[0091] Electrolyzer-cell assembly and testing:
[0092] The commercially available anodized aluminum Scribner single-cell hardware is used as an end plate with a serpentine flow field made of titanium and graphite bipolar plates for the anode and cathode side, respectively, was used for all the experiments. The titanium bipolar plate also acted as the current collector on the anode end, whereas the gold-plated copper current collector was used at the cathode end. Freudenberg H23C6 and H23C3 were used as the gas diffusion layers (GDLs) on the cathode side, the fabricated PTE at the anode, along with 200pm Teflon gaskets on each side that provided the required compression for adequate testing. A sub-gasket of about 10 pm was also used to ensure an active area of 5cm2.
[0093] Electrolyzer cells were uniformly torqued in a star pattern with torque increments from 20 to 70 in-lbf. Pre-heated Milli-Q DI water was introduced into the anode section of the cell at a flow rate of 4.1 mL / min-cm2while the cathode inlet was capped, and the cathode outlet vented the produced hydrogen. The anode water was flown for about 30 minutes until the cell reached a temperature of 80°C, maintained by a rod heater, before conditioning and was recirculated for the duration of the experiment. A Kolibrik potentiostat (PTC-05100EW) and a Biologic HCP-803 potentiostat were used for electrochemical analysis in all the experiments. The conditioning protocol used here involved holding the cell at a current density of 200 mA / cm2for 90 minutes, after which beginning of life (BOL) performance was measured. The polarization curve was evaluated by holding the cell at a constant potential for about 50 to 60 seconds, with a step of 0.05 V from 1 ,3V to 2 / 2.2V. Cyclic voltammetry was measured at a scan rate of 50 mV / s, ranging from 0.1 V to 1.6 V. Potentiostatic electrochemical impedance spectroscopy (P-EIS) was performed, with the frequency ranging from 100 kHz to 500 / 100 mHz, and the high-frequency resistance (HFR) was obtained through fitting in the high-frequency region. The polarization curve and cyclic voltammetry scans were measured at 24-hour intervals until the end-of-life (EOL), while the cell was maintained at a constant current density of 200 mA / cm2.
[0094] AEM Operation:
[0095] Preparation of Porous Transport Electrode (PTE) as Anode:
[0096] CO304catalyst ink was prepared by adding Co3O4nanopowders into a 1:9 v / v water / nPA mixture at a 10 mg / mL ratio of catalyst to solvent. The ink was cold bathReference No.: 2025-793-2, UCI 25.08 PCTInventor’s last name: Zenyuk et alDocument Date: May 8, 2025sonicated for 30 minutes before adding 5wt% PiperlON® A ionomer dispersion (I :Cat = 0.2). The resulting final ink was bath sonicated in an ice bath for an additional 30 minutes and roll milled for 24 hours. After roll milling, the ink was sprayed using a handheld airbrush onto a 6.25 cm2PTL substrate, which had been weighed prior. The substrate was sprayed using multiple passes until the desired loading of 1.5 mg / cm2of Co3O4was achieved, measured by determining the difference between the initial and final weights of the PTE.
[0097] Preparation of Cathode:
[0098] The Pt / C catalyst ink was prepared in the same manner as the Co3O4catalyst using an l:C ratio of 0.5. The cathode GDE was prepared by airbrush spraying the Pt / C catalyst ink onto a 5 cm2GDL substrate to achieve the desired loading of 0.3 mgPt / cm2, measured using the initial and final weights.
[0099] Cell assembly, testing, and conditioning:
[0100] The cell was assembled using the Scribner hardware featuring a graphite flow field on the cathode, a gold-plated copper current collector, and a titanium flow field on the anode. Hard stop gaskets controlled the compression of the cathode GDE to 20%, ensuring good contact with the 40 pm Versogen AEM PiperlON® membrane. The Scribner cell hardware was tightened to a torque of 40 in-lbs in 10 in-lbs intervals to ensure proper contact within the cell. The cell was then mounted and heated to 80°C with a 0.1M KOH feed on the anode (cathode dry operation), allowing the system to equilibrate for an hour before starting conditioning / testing protocols. The conditioning of the MEA was performed using cyclic voltammetry between 1.2-1 ,9V to cycle the cobalt oxide catalysts between the 2+ and 3+ oxidation states in 0.1 M KOH for 700 cycles or until equilibrium was achieved. A current hold at 1 A / cm2was carried out afterward to further condition and stabilize the MEA prior to testing.
[0101] A Gamry 5000E potentiostat was used to conduct all measurements for this AEM study, employing galvanostatic holds between 5 mA / cm2and 1 A / cm2with galvanostatic EIS in between to determine high-frequency resistance (HFR) at every current density.
[0102] Physical Characterization:Reference No.: 2025-793-2, UCI 25.08 PCTInventor’s last name: Zenyuk et alDocument Date: May 8, 2025
[0103] X-ray Diffraction (XRD)
[0104] XRD analysis was used to examine the crystal structure of the film samples. The films were attached directly to the sample holder with double-sided adhesive tape and laid flat on the stage without any extra substrate or background material. Measurements were taken using a Rigaku Ultima III Powder X-ray diffractometer with a Cu Ka radiation source (A = 1.5405 A), operated at 40 kV and 30 mA. Data collection occurred in the 0-20 configuration over a 20 range of 10° to 90°. The resulting diffraction patterns were matched against standard references, ICDD PDF-5+, to identify the phases.
[0105] Scanning Electron Microscopy / Energy Dispersive X-ray Spectroscopy (SEM / EDS)
[0106] SEM and EDS were conducted using an FEI Magellan 400 XHR field emission SEM with an integrated EDS detector. All imaging and analysis were carried out at an accelerating voltage of 30 kV. For cross-sectional analysis, samples were embedded in epoxy resin, cured, and mechanically polished to create a smooth cross-sectional surface. These polished samples were mounted on SEM stubs with conductive carbon tape. SEM imaging and EDS mapping were then used to examine the internal morphology and elemental distribution across various layers, as well as to identify compositional variations at interfaces. For top-view analysis, samples prepared beforehand were directly mounted onto SEM stubs using conductive carbon tape. Surface morphology was characterized through secondary electron (SE) imaging, while EDS was employed to analyze surface composition.
[0107] Results
[0108] Commercial Co3O4catalyst was used for its high kinetic activity towards OER in pure water feed systems. The results are summarized in FIGs. 2A-2B. FIG. 2B compares polarization curves between the water electrolyzers operating with Co3O4catalyst in standard PEM configuration, standard AEM configuration, and modified configuration. In the conventional PEMWE configuration, the Co3O4catalyst is in contact with the Nation™ ionomer and Nation™ membrane. In the conventional AEM configuration, the Co304catalyst is in contact with the AEM and the AEI. The modified configuration from this study uses a PEM membrane and AEI ionomer that contacts the Co3O4catalyst, which combines the benefits of using a stable and durable Nation™Reference No.: 2025-793-2, UCI 25.08 PCTInventor’s last name: Zenyuk et alDocument Date: May 8, 2025membrane, fast HER kinetics in acidic media on Pt surfaces, along with the flexibility of using a DI water feed.
[0109] Due to the highly acidic conditions created by the Nation™ ionomer in the catalyst layer of the conventional PEMWE system, most of the cobalt species in the catalyst layer leached out, leading to a loss of current density, as shown in FIG. 2B. This loss of catalyst affected not only kinetic overpotential but also ohmic, as cobalt ions transported towards the cathode under the electric field, contaminating the membrane and thus reducing its ionic conductivity. This is evidenced in the high frequency resistance (HFR) measurements that are about 260 mQ.cm2at 100 mA.crrr2, more than twice compared to the uncontaminated cell.
[0110] FIGs. 22A-22C show the polarization curves for an electrolyzer with no anode catalyst layer but only a Pt-coated porous transport layer (PTL), showing similar polarization to the conventional PEI-PEM polarization curve demonstrated by FIG. 2B, indicating that most of the current generated is potentially from Pt being active for OER. The anode made with PEI (Nation™) yielded 0.12 A.cm-2, compared to 1.71 A.cm-2with AEI (PiperlON®) at a cell voltage of 2V for the same loading and l / C ratio. Although XRD patterns of catalyst inks (FIG. 23A) formulated with Nation™ and PiperlON® both showed characteristic peaks of Co3O4, the performance differences suggest that the local environment plays a key role in catalyst stability. FIGs. 6A-6C show the comparative performance of a relatively less acidic polymer binder, such as poly-acrylic acid (PAA), and compares it with the performance of PEI (Nation™) and AEI (PiperlON®). The anodes made with PAA, PEI, and AEI yielded 0.26 A.cm-2, 0.12 A.cm-2, and 1.71 A.cm2respectively, at a cell voltage of 2V for the same loading and l / C ratio, highlighting the influence of the local electrochemical environment in the catalyst layer on polarization behavior, proton exchange membrane (PEM)
[0111] To control the local environment using AEI, I / O ratios were varied in the anode catalyst layer, and the resulting polarization curves are summarized in FIG.3A-3B for l / C ratios of 0.2, 0.3, and 0.4 for the AEI-PEM electrolyzer and compared to the standard AEI-AEM electrolyzer. Higher kinetic losses were observed for AEI-PEM compared to the alkaline (AEI-AEM) processes using the same catalyst and ionomer. Furthermore, the AEI-AEM electrolyzer had 0.1 M KOH feed, whereas the AEI-PEMReference No.: 2025-793-2, UCI 25.08 PCTInventor’s last name: Zenyuk et alDocument Date: May 8, 2025electrolyzer had water feed. This offset in the kinetic region of polarization curves might be due to the Donnan or junction potential at the AEI-PEM interface.
[0112] As the AEI l / C ratio increases from 0.2 to 0.3 to 0.4, the cell voltages required to achieve a current density of 1 A / cm2were 1.88V, 1.92V, and 2.01V, respectively, as shown by FIG. 3A. FIG. 3B further illustrates the trend of increase in HFR-free voltage with an increase in l / C ratio with a zoomed-in plot of HFR-free voltage in the activation region, demonstrating that as the l / C ratio increases, the cell performance decreases. This l / C optimization study indicates that an l / C ratio of 0.2 is sufficient to maintain the local environment at the BOL. The addition of extra ionomer increases the electronic contact resistance, which has been attributed to the buildup of an ionomer film at the catalyst layer-porous transport layer interface in the anode and the partial electronic insulation of the catalyst by the ionomer, as also observed in IrOx-based FEM WE systems
[2324] . This effect is further supported by the observed increase in HFR values with higher l / C ratios (FIG. 3A), rising from about 90 mQ.cm2at l / C 0.2 to 105 mQ.cm2at l / C 0.3 and 120 mQ.cm2at l / C 0.4 at the current density of 700 mA. cm-2. These HFR increases due to increased ionomer content could also lead to an increase in kinetic overpotentials as observed in FIG. 3B, highlighting that even small increases in HFR can lead to noticeable performance differences observed in previous studies.
[0113] To ensure that the local environment of the electrode prepared with AEI is not impacted by the Nation™ membrane, an interlayer (IL) of AEI, comprising 10% of the mass of the electrode prepared with l / C 0.2, was spray-coated over the anode and assembled into a PEM water electrolyzer setup without any additional WD layer. The results are summarized in FIGs. 7A-7B. The outcome of this experiment resembles a reverse-biased condition of a Bipolar Membrane Water Electrolyzer (BPMWE) without a WD layer , indicating that a WD catalyst is necessary to facilitate the water dissociation at the junction, allowing the charge transfer. When an additional AEI interlayer (IL) was introduced, it separated the Co3O4anode from the PEM, thereby preventing charge transport (protons through PEM), emphasizing the need for an additional WD layer at the IL-PEM interface to facilitate the operation in IL-PEM systems.
[0114] The stability of the AEI-PEM water electrolyzer was further studied by using a constant current density hold of 200 mA.cm2and monitoring cell voltage. FIGs.Reference No.: 2025-793-2, UCI 25.08 PCTInventor’s last name: Zenyuk et alDocument Date: May 8, 20258A-8C show the cell voltage profiles as a function of time, where voltage spikes represent the times of intermittent characterization or potentiostat restart events. The end of life (EOL) criterion is met when the cell voltage exceeds 10% of the initial activity, here 1.9 V, at a current density of 200 mA / cm2. FIG. 3C summarizes the average time to failure for the three l / C ratios: 0.2, 0.3, and 0.4. The cell's stability improved from 100 hours to 205 hours as the l / C ratio increased from 0.2 to 0.4. This can be attributed to a greater ionomer coverage of the catalyst at higher l / C ratio, minimizing interfacial contact with the PEM membrane. The catalyst that contacts PEM will degrade faster due to low pH, thus creating a scenario where an increase in the l / C ratio improves the durability of the cell but at the cost of reduced performance.
[0115] The SEM of aged MEA cross-sections (FIG. 4A-4C) reveals that the catalyst layer (CL) thickness increases systematically with increasing l / C ratio, from 0.2 to 0.4. EDS mapping further reveals that cobalt is present not only throughout the anode catalyst layer but also in regions of the membrane and cathode, consistent with the leaching of cobalt ions and their migration towards the membrane and cathode. This supports our earlier assertion that catalyst particles closer to the PEM interface are more prone to dissolution. A thicker, more ionomer-rich catalyst layer can provide improved physical separation between the catalyst and the membrane, helping to mitigate degradation.
[0116] FIG. 4D illustrates the polarization curve comparison for l / C at 0.2 between the beginning of life (BOL) and the end of life (EOL). At the EOL, the performance is 0.29 A.crrr2, while at BOL, it is 1.71 A. cm2at a cell voltage of 2 V. Without wishing to limit the invention to a particular theory or mechanism, due to observations including an ‘S’ shape polarization curve during periodic electrochemical characterization, the inventors believe that the performance differences between beginning-of-life (BOL) and end-of-life (EOL) are primarily due to a combination of two interconnected factors: (i) cobalt ions leaching and (ii) increased membrane resistance resulting from cation contamination.
[0117] All performance curves from the periodic characterization, recorded at approximately 24-hour intervals, have been summarized in FIGs. 10A-17. These periodic characterizations have revealed that the cobalt species in the anode leached out and migrated towards the membrane and cathode. Consequently, the anode lacksReference No.: 2025-793-2, UCI 25.08 PCTInventor’s last name: Zenyuk et alDocument Date: May 8, 2025an adequate catalyst to support the anodic OER reaction, as observed in FIG. 4D. Hence, cation contamination and thereby the loss of catalyst at the anode are the primary causes of performance degradation overtime.
[0118] FIGs. 12A-12C show comparative plot of the performance of the l / C 0.2 electrode at BOL and after about 48 hours, compared to a case with an electrode prepared with no ionomer. The electrode without an ionomer represents a limiting case analogous to the case when all the ionomer has been degraded. The similarity in the signature 'S’ shape polarization curves between the no-ionomer case and after 48 hours potentially suggests that the ionomer is being degraded, leading to further exposure of cobalt species to the membrane and, consequently, cation contamination. This indicates that if the stability hold were performed at higher current densities, such as 1 A.cm-2, then this process of cation migration toward the membrane and cathode would become faster, and thus the degradation would be quicker. Similarly, AEM water electrolyzers without a supporting electrolyte (KOH) face durability issues due to ionomer oxidation.
[0119] FIGs. 22A-22C summarize the EOL polarization curves for the three l / C ratios used in this study. The early degradation of the ionomer, observed at 24 hours, shows that future stability is more closely linked to how well the catalyst particles are encapsulated within the ionomer matrix. Over time, cobalt species become exposed to the PEM, causing leaching and membrane contamination, which depend on the amount of cobalt species in the membrane and progress with time.
[0120] Additionally, the top view of SEM / EDS mapping of the aged anode (FIGs.24A-24B) surface revealed cobalt-rich aggregates in areas where oxygen was not co-located, indicating the possible redeposition of cobalt during cell operation. Supporting this, the XRD patterns of the EOL electrodes show a broad hump near the onset of the cobalt peaks, suggesting the presence of amorphous cobalt or cobalt-based species, which further points to cobalt dissolution and partial redeposition.
[0121] Furthermore, XRD analysis of the aged cathode region (FIG. 23C) revealed a broad peak near 25° 20, which may be due to CoCO3or overlap with amorphous carbon from the Pt / C support. However, no clear cobalt peaks appeared, illustrating XRD’s limitations in detecting low-concentration or amorphous species. Despite this, literature on Ir-based systems indicates that over 90% of dissolved speciesReference No.: 2025-793-2, UCI 25.08 PCTInventor’s last name: Zenyuk et alDocument Date: May 8, 2025are found in the membrane or cathode, supporting the likelihood of cobalt migration and redeposition at the cathode under similar electrochemical conditions.
[0122] When comparing the performance at the BOL with the current state-of-the-art materials in the literature, it was observed that to drive the cell at a constant 1 A.cm2, this system reached a cell voltage of 1.884 V, while other studies, y-MnOz (M94%), LMCF, and CWO-del-48, required 1.887 V, 2.25 V, and 1.77 V, respectively, as summarized in FIG. 4D. This observation not only highlights the system's modifications and stabilization but also indicates that it achieves the best-reported performance curves for commercial Co304in a PEM water electrolyzer setup, showcasing the significance of the findings in this paper, which can be applied to various materials previously discarded due to instability in highly acidic conventional PEM water electrolysis.
[0123] To the best of the inventors’ knowledge, Co3O4and Co2O3can facilitate water dissociation, but studies on BPMWE have only reported Co3O4as an anode in alkaline OER, not as a WD catalyst. Indeed, nearly all metal oxides dissociate water at rates significantly higher than bare membranes, and the bare AEM / CEM membrane-membrane interface is highly resistive.
[0124] This further raises the question of how the OER mechanism operates at the anode of the modified (AEI-PEM) system. Cobalt is prone to leaching. As previously discussed, the interfacial contact between the catalyst layer and the PEM and the necessity for protons to be transported through the PEM influence the OER mechanism in this modified system. The AEI in the catalyst layer envelops the cobalt species, thereby blocking them from being transported through the membrane to the cathode and delaying the loss of cell voltage. Increasing the I / O ratio reduced cell performance but increased cell durability, emphasizing that the exposure of the cobalt catalyst to the PEM determines the system's activity. Alternatively, cobalt in this system can also function as the WD catalyst and dissociate water into H+and OH' ions, with the H+ions transported to the cathode through the membrane while the OH- ions create a local alkaline environment, facilitating the OER through alkaline pathways similar to the BPMWE.
[0125] ConclusionsReference No.: 2025-793-2, UCI 25.08 PCTInventor’s last name: Zenyuk et alDocument Date: May 8, 2025
[0126] The MEA design presented here provides good activity and stability for PGM-free materials used in OER within PEMWE. This example highlights not only the system modifications and stabilization but also reports the best polarization curves for commercial Co3O4in a PEM water electrolyzer setup, where this system achieved a cell voltage of 1.884 V, while Y-MnO2(M94%), LMCF, and CWO-del-48 required 1.887 V, 2.25 V, and 1.77 V, respectively, to operate the cell at a constant 1 A.crrr2. The cells tested in different configurations demonstrated stability of 100 hours to 205 hours at an operating current density of 200 mA.cm-2. However, a performance decline was observed during periodic electrochemical characterization, which is likely due to ionomer degradation. The stability then depended on providing a better physical separation between the catalyst and the membrane, which helped enhance longevity.
[0127] Although there has been shown and described the preferred embodiment of the present invention, it will be readily apparent to those skilled in the art that modifications may be made thereto which do not exceed the scope of the appended claims. Therefore, the scope of the invention is only to be limited by the following claims. In some embodiments, the figures presented in this patent application are drawn to scale, including the angles, ratios of dimensions, etc. In some embodiments, the figures are representative only and the claims are not limited by the dimensions of the figures. In some embodiments, descriptions of the inventions described herein using the phrase “comprising” includes embodiments that could be described as “consisting essentially of” or “consisting of”, and as such the written description requirement for claiming one or more embodiments of the present invention using the phrase “consisting essentially of” or “consisting of” is met. As used herein, the term “about” refers to plus or minus 10% of the referenced number.
[0128] As used herein, the term “about” refers to plus or minus 10% of the referenced number.
[0129] Reference numbers recited herein, in the drawings, and in the claims are solely for ease of examination of this patent application and are exemplary. The reference numbers are not intended in any way to limit the scope of the claims to the particular features having the corresponding reference numbers in the drawings.
Claims
Reference No.: 2025-793-2, UCI 25.08 PCTInventor’s last name: Zenyuk et alDocument Date: May 8, 2025WHAT IS CLAIMED IS:
1. An anode catalyst comprising at least one transition metal catalyst disposed in a substrate having a local alkaline pH.
2. The anode catalyst of claim 1, wherein the substrate comprises an anion exchange ionomer (AEI) or ionic liquid.
3. The anode catalyst of claim 2, wherein the at least one transition metal catalyst is dispersed in the AEI.
4. The anode catalyst of claim 2, wherein the AEI comprises a polymer backbone functionalized with alkaline groups, wherein the functionalized polymer backbone is effective for facilitating conduction of anions while remaining stable under alkaline conditions.
5. The anode catalyst of claim 4, wherein the polymer backbone comprises poly(aryl piperidinium) (PAP), poly(ethylene) (PE), polystyrene (PS), polysulfones (PS), poly(phenyleneoxide)s (PPO), poly(phenylene)s (PP), poly(fluorene) (PF), poly(ethylene-co-tetrafluoroethylene) (EFTE), polybenzylimidazole (PBI), or a combination thereof.
6. The anode catalyst of claim 1, wherein a weight ratio of the substrate to the transition metal compound ranges from about 0.05 to about 0.45.
7. The anode catalyst of claim 1, wherein the transition metal catalyst comprises Co3O4, cobalt oxides doped with nickel, manganese, or copper, or other platinum group metal (PGM)-free metal oxides, or mixed oxides of Co or Ni.
8. The anode catalyst of claim 1, wherein the anode catalyst is free of platinum group metal (PGM)-based materials.
9. An anode (100) comprising an anode catalyst in contact with a proton exchange membrane (PEM, 130), said anode catalyst comprising at least one transition metal catalyst disposed in a substrate such that the substrate is interfacing the PEM (130).
10. The anode (100) of claim 9, wherein the substrate is an anion exchange ionomer (AEI), wherein the AEI has a local alkaline pH, wherein the anode catalyst is anReference No.: 2025-793-2, UCI 25.08 PCTInventor’s last name: Zenyuk et alDocument Date: May 8, 2025anode catalyst layer (ACL, 105) comprising the at least one transition metal catalyst dispersed in the AEI, wherein the ACL (105) is disposed on a porous transport layer (PTL, 110) and interfacing the PEM (130).
11. The anode (100) of claim 10, wherein the AEI comprises a polymer backbone functionalized with alkaline groups, wherein the functionalized polymer backbone is effective for facilitating conduction of anions while remaining stable under alkaline conditions.
12. The anode (100) of claim 11, wherein the polymer backbone comprises poly(aryl piperidinium) (PAP), poly(ethylene) (PE), polystyrene (PS), polysulfones (PS), poly(phenyleneoxide)s (PPO), poly(phenylene)s (PP), poly(fluorene) (PF), poly(ethylene-co-tetrafluoroethylene) (EFTE), polybenzylimidazole (PBI), or a combination thereof.
13. The anode (100) of claim 9, wherein the substrate comprises an alkaline ionic liquid, wherein the transition metal catalyst is dispersed in the alkaline ionic liquid, wherein the alkaline ionic liquid is effective for facilitating conduction of anions while remaining stable under alkaline conditions.
14. The anode of claim 9, wherein the transition metal catalyst comprises Co304, cobalt oxides doped with nickel, manganese, or copper, or other platinum group metal (PGM)-free metal oxides, or mixed oxides of Co or Ni.
15. The anode (100) of claim 9, wherein the PTL (110) is Pt-coated.
16. A water electrolyzer (10) comprising:a. an anode (100) comprising an anode catalyst in contact with a porous transport layer (PTL, 110), said anode catalyst comprising at least one transition metal catalyst disposed in a substrate having a local alkaline pH; b. a cathode (120) operatively coupled to the anode (100); andc. a proton exchange membrane (PEM, 130) interposed between said anode (100) and said cathode (120), said PEM (130) facing the anode (100).
17. The water electrolyzer (10) of claim 16, wherein the substrate comprises an anion exchange ionomer (AEI), wherein the anode catalyst is an anode catalyst layer (ACL, 105) comprising the at least one transition metal catalyst dispersed in the AEI, wherein the ACL (105) is interfacing the PTL (110).Reference No.: 2025-793-2, UCI 25.08 PCTInventor’s last name: Zenyuk et alDocument Date: May 8, 202518. The water electrolyzer (10) of claim 17, wherein the AEI comprises a polymer backbone functionalized with alkaline groups, wherein the functionalized polymer backbone is effective for facilitating conduction of anions while remaining stable under alkaline conditions.
19. The water electrolyzer (10) of claim 18, wherein the polymer backbone comprises poly(aryl piperidinium) (PAP), poly(ethylene) (PE), polystyrene (PS), polysulfones (PS), poly(phenyleneoxide)s (PPO), poly(phenylene)s (PP), poly(fluorene) (PF), poly(ethylene-co-tetrafluoroethylene) (EFTE), polybenzylimidazole (PBI), or a combination thereof.
20. The water electrolyzer (10) of claim 17, further comprising an AEI interlayer coating the ACL (105) such that the AEI interlayer is disposed between the ACL (105) and the PEM (130).
21. The water electrolyzer (10) of claim 16, wherein the substrate comprises an alkaline ionic liquid, wherein the transition metal catalyst is dispersed in the alkaline ionic liquid, wherein the alkaline ionic liquid is effective for facilitating conduction of anions while remaining stable under alkaline conditions.
22. The water electrolyzer (10) of claim 16, further comprising a source of electrical energy configured to apply a voltage between the anode and cathode.
23. The water electrolyzer (10) of claim 16, wherein the water electrolyzer is utilized in an oxygen evolution reaction.
24. The water electrolyzer (10) of claim 16, wherein the PTL (110) is Pt-coated.
25. The water electrolyzer (10) of claim 16, wherein the transition metal catalyst comprises Co304, cobalt oxides doped with nickel, manganese, or copper, or other platinum group metal (PGM)-free metal oxides, or mixed oxides of Co or Ni.
26. The water electrolyzer (10) of claim 16, wherein the cathode (120) is a catalyst-coated membrane.
27. The water electrolyzer (10) of claim 26, wherein the catalyst-coated membrane comprises Pt / C disposed on a cation exchange membrane.