Pellets of bast hemp fiber and methods of manufacturing same

The development of bast hemp pellets through milling and optional coupling agent use addresses the need for focused bast hemp fiber processing, resulting in superior natural fiber-reinforced plastics for automotive components.

WO2026241220A1PCT designated stage Publication Date: 2026-11-19ISIAH ENTERPRISES INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/US2026/027724
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-12
Filing Date
2026-05-12
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Existing technologies primarily utilize hurd fibers or a combination of bast and hurd fibers for reinforcing materials in thermoplastic polymers, lacking a focused process for bast hemp fibers alone, which are more suitable for specific applications like automotive components.

Method used

A process is developed to manufacture compressed bast hemp pellets using decorticated hemp bast fibers, milled to optimal length and diameter, optionally with a coupling agent, suitable for downstream combination with thermoplastic polymers.

Benefits of technology

The bast hemp pellets exhibit superior material properties, enhancing the performance of natural fiber-reinforced plastics with improved characteristics such as tensile strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure US2026027724_19112026_PF_FP_ABST
    Figure US2026027724_19112026_PF_FP_ABST
Patent Text Reader

Abstract

Hemp pellets are manufactured using only the bast portion of hemp stalks into a form suitable for downstream use with plastic compounding extrusion equipment and processes. Decorticated hemp bast fiber is milled to produce a milled material. A suitable coupling agent is combined with the milled material to produce compressed bast hemp pellets. The decorticated hemp bast fiber may be milled using a pressure wave mill apparatus. The coupling agent may be combined with the milled material using a pellet mill apparatus.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] PELLETS OF BAST HEMP FIBER AND METHODS OF MANUFACTURING SAME

[0002] CROSS-REFERENCE TO RELATED APPLICATIONS

[0003] This application claims the benefit of U. S. provisional patent application No. 63 / 804,131, filed May 12, 2025, now pending, the entirety of which is hereby incorporated by reference.

[0004] BACKGROUND OF THE INVENTION

[0005] 1. Field of the Invention

[0006] The present invention relates, in general, to hemp fibers and, in particular, to pellets made of bast hemp fibers, and their methods of manufacture.

[0007] 2. General Background of the Invention

[0008] In the United States, the Agricultural Improvement Act of 2018 removed hemp from the Drug Enforcement Administration’s schedule of controlled substances. Since then, the use of hemp in industrial and consumer products has become a matter of growing interest, particularly in the United States.

[0009] One potential application of hemp is as a reinforcing material when added to thermoplastic polymers, such as, for example, polypropylene. In such applications, hemp bast fibers are employed as a substitute for glass-filled polypropylene. Such hemp reinforced plastics may have application in, without limitation, the automotive industry.

[0010] Hemp stalks contain two main types of fiber. Bast, or long fibers, are found in the bark of the plant. Hurd, or short fibers, are found in the core of the stem. Most commonly, hurd fibers, or a combination of bast and hurd fibers, have been used as a plastic reinforcing material. The present invention, however, employs only the bast fibers of hemp plants in order to create a plastic reinforcing material, in the form of pellets that are suitable for further combination with a thermoplastic polymer. In particular, bast hemp pellets of the present invention may be combined with a thermoplastic polymer using a compounding extrusion apparatus, in order to produce downstream bioplastic pellets. These bioplastic pellets may be injection molded into, for example, automotive components, such as internal automotive mounting brackets.

[0011] BRIEF SUMMARY OF THE INVENTION

[0012] The present invention comprises compressed hemp pellets manufactured with only the bast portion of hemp stalks, as well as processes for manufacturing such pellets. The resultant pellets are in a form suitable for downstream use with plastic compounding extrusion equipment and processes.

[0013] Decorticated hemp bast fiber is first provided. The decorticated hemp bast fiber is milled to produce a milled material. Next, a suitable coupling agent may be provided. If provided, the coupling agent is combined with the milled material to produce compressed bast hemp pellets. Alternatively, no coupling agent may be used.

[0014] In a preferred embodiment, the decorticated hemp bast fiber is milled using a pressure wave mill apparatus. Moreover, in a preferred embodiment, the coupling agent, if one is used, is combined with the milled material using a pellet mill apparatus.

[0015] Accordingly, it is an object of the present invention to provide a process for processing bast hemp fiber into pellets.

[0016] It is another object of the present invention to provide bast hemp fiber pellets having properties that are suitable for subsequent combination with a thermoplastic material.

[0017] Other objects, features and advantages of the invention will be apparent from the following detailed disclosure, taken in conjunction with the accompanying sheets of drawings.

[0018] BRIEF DESCRIPTION OF THE SEVERAL VIEWS OF THE DRAWINGS

[0019] Fig. 1 is a process flow diagram of a method of manufacturing bast hemp fiber pellets in accordance with the present invention;

[0020] Fig. 2 is a photograph of decorticated bast hemp fiber, employed in the manufacturing of bast hemp fiber pellets in accordance with the present invention;

[0021] Fig. 3 is a photograph of bast hemp fibers following the milling step in the manufacturing of bast hemp fiber pellets in accordance with the present invention; and

[0022] Fig. 4 is a photograph of bast hemp fiber pellets, manufactured in accordance with the present invention.

[0023] DETAILED DESCRIPTION OF THE INVENTION

[0024] While this invention is susceptible of embodiment in many different forms, there is shown in the drawings and will herein be described in detail, one specific embodiment, with the understanding that the present disclosure is to be considered merely an exemplification of the principles of the invention and the application is limited only to the appended claims.

[0025] Referring to Fig. 1 and the photograph of Fig. 2, decorticated bast fiber 100 is first obtained and provided in bulk. Typically, a decortication apparatus is employed to mechanically separate the bast fibers from the remainder of the hemp plant. Such decorticated bast fiber 100 are generally many inches long in average length.

[0026] Next, in step 200, the decorticated bast fiber is processed into a milled material optimal length and diameter. The milled material has a fibrous form, and, in a preferred embodiment, may have a consistency similar to that of cotton candy. In a preferred embodiment of the invention, this processing is performed using a milling apparatus and, more particularly, a pressure interference wave mill, such as the apparatus discussed in U. S. Patent Publication No.

[0027] 2017 / 0252751, the entirety of which is hereby incorporated by reference. The pressure wave mill may be operated at a speed of, for example, 3,000 revolutions per minute. In one embodiment of the present invention, the decorticated bast fiber is processed by the pressure wave mill at least twice, resulting in shorter fibers. The resulting milled hemp bast fiber 300 is shown in the photograph of Fig. 3. Annexes A and B to this specification are laboratory test reports regarding the properties of the milled bast fiber 300.

[0028] Next, in step 500, milled bast fiber 300 is further processed using a pelletizing apparatus. The pelletizing apparatus may comprise, for example, a pellet mill manufactured by Buskirk Engineering of Ossian, Indiana. During step 500, milled bast fiber is combined with a suitable coupling agent 400 to create compressed bast hemp pellets 600, such as those shown in the photograph of Fig. 4. In a preferred embodiment, coupling agent 400 is water. Alternatively, coupling agent 400 may be selected to provide a chemical treatment to milled bast fiber 300 to improve bonding characteristics when bast hemp pellets are further combined with a thermoplastic polymer downstream, preferably through the use of a compounding extrusion apparatus. The specific formulation of coupling agent 400 may vary, depending upon the particular downstreamapplication. In another alternative embodiment, no coupling agent is provided or used, and milled bast fiber 300 is processed dry.

[0029] Compared to other natural fiber products used in the plastics industry, compressed bast hemp pellets 600 have superior material properties (including, without limitation, aspect ratio, tensile strength), resulting in natural fiber-reinforced plastics with improved material characteristics.

[0030] It will be understood that modifications and variations may be effected without departing from the spirit and scope of the present invention. It will be appreciated that the present disclosure is intended as an exemplification of the invention and is not intended to limit the invention to the specific embodiments illustrated and described. The disclosure is intended to cover, by the appended claims, all such modifications as fall within the scope of the claims.

[0031] ANNEX A

[0032] Test Results FTIR, Infrared Spectroscopy, ASTM E1252

[0033] Microinfrared analysis was performed on the sample using a Thermo Scientific Nicolet iN10 FTIR microscope in transmission.

[0034] Industrial Hemp Micronized Hurd Powder

[0035]

[0036] sample has similar functional groups to a cellulose (hemp)

[0037] Test Results

[0038] 1. FTIR, Infrared Spectroscopy, ASTM E1252

[0039] Microinfrared analysis was performed on the sample using a Thermo Scientific Nicolet iN10 FTIR microscope in transmission.

[0040]

[0041] 2. The sample has similar functional groups to a cellulose (hemp)

[0042] Note: Absorbance used to estimate percent Lignin’s found are 1506 and 1471cm-l The Industrial fiber Bast did not show and absorbances in these regions, The Industrial Hemp Micronized Hurd Powder show one absorbance

[0043] At 1506cm- 1.

[0044] Test Results

[0045] 2. Thermogravimetric Analysis (TGA)

[0046] Specimen weighing approximately 13 mg was heated from 25°C to 650°C at a rate of 15°C per minute in a nitrogen environment. At 6 ()’~'C, the environment was switched from nitrogen to air and heating continued to 900%'. The Delta Y values represent weight change over the entire run.

[0047] Industrial Hemp Bast Fiber

[0048]

[0049] Test Results

[0050] 2. Thermogravimetric Analysis ( TGA)

[0051] Specimen weighing approximately 3 g was heated from 25°C to 650°C at a rate of 15°C per minute in a nitrogen environment. 650°C, the environment was switched from nitrogen to air and heating continued to 900°C The Delta Y values represent weight change over the entire run.

[0052] Industrial Hemp Micronized Hurd Powder

[0053]

[0054] Test Results

[0055] <3. Differential Scanning Calorimetry (DSC)

[0056] The DSC analysis was performed using a TA Q100 DSC at 10° / min heat rate from -40°C to 220°C under nitrogen gas.

[0057] Industrial Hemp Bast Fiber 1 Heat

[0058] Same®', i&istfai? fcerrtp Bast Fibsr

[0059] Size: 7.1500 mg DSC

[0060] Method: Sample Run

[0061]

[0062] Instrument: DSC Q100 V9.9 Build 303

[0063]

[0064] Test Results

[0065] 3. Differential Scanning Calorimetry (DSC)

[0066] The DSC analysis was performed using a TA Q100 DSC at. lO^'min heat rate from -40%’ to 220°C raider nitrogen gas.

[0067] Industrial Hemp Bast Fiber cooling

[0068]

[0069] Test Results

[0070] 3. Differential Scanning Calorimetry (DSC)

[0071] The DSC analysis was performed using a TA Q100 DSC at lO° / mm heat fate from -40" C to 220“C under nitrogen gas.

[0072] Industrial Hemp Bast Fiber 2ndHeat

[0073]

[0074] Test Results

[0075] 3. Differential Scanning Calorimetry (DSC)

[0076] The DSC analysis was performed using a TA Q100 DSC at 10° / min heat rate from -40°C to 220°C under nitrogen gas.

[0077] Industrial Hemp Micronized Hurd Powder1StHeat

[0078]

[0079] Test Results

[0080] 3. Differential Scanning Calorimetry (DSC)

[0081] The DSC analysis was performed using a TA Q100 DSC at 10° / min heat rate from -40°C to 220°C under nitrogen gas.

[0082] Industrial Hemp Micronized Hurd Powder cooling

[0083]

[0084] Test Results

[0085] 3. Differential Scanning Calorimetry (DSC)

[0086] The DSC analysis was performed using a TA Q100 DSC at 10° / min heat rate from -40°C to 220°C under nitrogen gas.

[0087] Industrial Hemp Micronized Hurd Powder 2“aHeat

[0088]

[0089]

[0090] Test Results

[0091] Partide size microscope

[0092] Industrial Hemp Bast Fiber

[0093]

[0094] Auto measurements (Data + Statistics)

[0095]

[0096]

[0097]

[0098]

[0099]

[0100] Test Results

[0101] 4- Particle size microscope

[0102] Iiidustaal Hemp Micromzed Hurd Powder

[0103]

[0104] Anta eOTnrem nts (Date 5tatis£k&

[0105]

[0106]

[0107]

[0108] Test Results

[0109] 4, Particle size mterusc&pe

[0110] Hurd powder

[0111]

[0112] Au o measurements (Data - Statistics}

[0113]

[0114]

[0115]

[0116]

[0117] Test Results

[0118] 5. Strength test of longer Bast fiber

[0119] maximum

[0120] Sample Lb. force PSI

[0121] Single strand 1 0.22 73

[0122] Single strand 2 0.24 80

[0123] Single strand 3 0.34 113

[0124] Single strand 4 0.2 67

[0125] Single strand 5 0.25 83

[0126] Average 0.25 83

[0127] Sample test using force gate and looped single strand.

[0128] Test Equipment

[0129] 1. E-387, Thermo Scientific Nicolet iN 10 Infrared Microscope

[0130] 2. E-773, TGA

[0131] 3. E-443, DSC

[0132] 4. E-l 167 force Gauge

[0133] 5. E-058-02 Microscope Image system

[0134] ANNEX B

[0135] Materials

[0136] Three hemp fiber reinforcements were submitted to the lab for analysis in two

[0137] subsamples each, Thermalgravimetric analysis (TGA) was performed on the samples.

[0138] One subsample from each hemp fiber rinforcement was tested m a nitrogen environment and the other was tested in an oxygen environment, Sample 1 (in nitrogen) showed 5.26% of the sample burning off at 48.6°€‘ and 80,9% at 297, 7°C leaving behind a residue of

[0139] 0.99% (Figure ChmO-1). Sample I (in oxygen) showed 87.5% of the sanjple burning off at 296.4°€ leaving behind a residue of 12.1% (Figure ChmO-2). Sample 2 (in nitrogen) showed 77.1% of the sample burning off at 284.6°C leaving behind a residue of 2.43%

[0140] (Figure ChmO-3). Sample 2 (in oxygen) showed 79.0% of the sample burning off at

[0141] 285. i'-’C leaving behind a residue of 20.4% (Figure ChmO-4). Sample 3 (in nitrogen)

[0142] showed 69.9% of the sample burning off at 288.7®C leaving behind a residue of 19,4% (Figure Chm0~5). Sample 3 (in oxygen) showed 64.6% of the sample homing off at

[0143] 288.1FC and 12.4% at 379.5°C leaving behind a residue of 23.1% (Figure ChmO-6). The TGA curves were overlayed for comparison (Figure Chm. O-7).

[0144]

[0145] Figure Chm0-I. TGA curve of Sample I in nitrogen showing 5.26% of the sample

[0146] burning off at 48.6®C and 80.9% at 297.7°C leaving behind a residue of 0.99%.

[0147]

[0148]

[0149] Figure ChmO-2. TGA curve of Sample 1 m oxygen showing 87.5% of the sample burning off at 2.4°C leavin -behind a residue of 12.1%.

[0150]

[0151] Figure GhmQ-3. TGA curve of Sample 2 in nitrogen showing 77.1% of the sample burning off at 284.6°C leaving behind a residue of 2.43%.

[0152]

[0153]

[0154] Figure Ch O~i. TGA curve of Sample 2 in oxygen showing 79, 0% of the sample burning off at 285. C leaving behind a residue of 20.4%,

[0155]

[0156] Figure ChniO-5. TGA curve of Sample 3 in nitrogen showing 69.9% of the sample burning off at 288.7°C leaving behind a residue of 10.4%,

[0157]

[0158]

[0159] Figure ChmO-6. TGA curve of Sample 3 in oxygen showing 64.6 of the sample burning off at 288.0°C and 12.4 at 379.5°C leaving beliind a residue of 23.1%.

[0160]

[0161] Figure ChmO-7. Overlay of all six samples for comparison.

[0162]

[0163] 31

Claims

What is claimed is:

1. A process for manufacturing compressed bast hemp fiber pellets, comprising the steps of:- providing decorticated hemp bast fiber;milling the decorticated hemp bast fiber to produce a milled material;- providing a suitable coupling agent; andcombining the coupling agent and the milled material to produce compressed bast hemp pellets.

2. The process according to claim 1, wherein the milling step comprises using a pressure interference wave mill apparatus.

3. The process according to claim 1, wherein the combining step comprises using a pellet mill apparatus.