Aluminum-containing polyolefins and methods thereof

A continuous process for producing aluminum-containing polyolefin-based ionomers addresses the inefficiencies of cross-linked rubbers by forming terpolymers with enhanced melt strength and consistent properties, reducing costs and batch-to-batch variations.

WO2026241318A1PCT designated stage Publication Date: 2026-11-19EXXONMOBIL TECHNOLOGY & ENGINEERING CO
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/US2026/027881
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-16
Filing Date
2026-05-12
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Existing cross-linked rubbers face challenges in large-scale production due to high operational costs and batch-wise inefficiencies, leading to batch-to-batch variation in thermal and thermomechanical properties, and they cannot be reprocessed due to irreversible cross-linking.

Method used

A method for producing aluminum-containing polyolefin-based ionomers through a continuous process involving two reaction zones: one for polymerization and another for oxidation, using ethylene, additional alpha-olefin monomers, and an aluminum vinyl monomer, with specific catalyst systems and reagents to form terpolymers with enhanced melt strength and thermal/thermomechanical properties.

Benefits of technology

The method enables efficient, continuous production of terpolymers with improved melt strength and reduced operational costs, maintaining desired thermal and thermomechanical properties without sacrificing elasticity and toughness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure IMGF000013_0001
    Figure IMGF000013_0001
  • Figure IMGF000016_0001
    Figure IMGF000016_0001
  • Figure IMGF000016_0002
    Figure IMGF000016_0002
Patent Text Reader

Abstract

The present disclosure relates to polyolefin-based ionomers and production of polyolefin-based ionomers. More specifically, the present disclosure relates to aluminum-containing polyolefins, such as polyolefin-based ionomers, and methods of preparing such aluminum-containing polyolefins. In some embodiments, a method for preparing a terpolymer includes introducing two or more different α-olefin monomers and an aluminum vinyl monomer to a first reaction zone. The method further includes introducing a catalyst system to the first reaction zone to form a reaction mixture. The method further includes polymerizing the reaction mixture to form a polymer mixture. The method further includes transferring the polymer mixture from the first reaction zone to a second reaction zone. The method further includes introducing a reagent to the second reaction zone. The method further includes reacting the polymer mixture with the reagent to form a polymer composition comprising the terpolymer.
Need to check novelty before this filing date? Find Prior Art

Description

ALUMINUM-CONTAINING POLYOLEFINS AND METHODS THEREOFFIELD

[0001] The present disclosure relates to polyolefin-based ionomers and production of polyolefin-based ionomers. More specifically, the present disclosure relates to aluminum-containing polyolefins, such as polyolefin-based ionomers, and methods of preparing such aluminum-containing polyolefins.BACKGROUND

[0002] Cross-linked rubbers are used in numerous industrial and consumer applications, such as for coatings, seals, tires, tubing, and roofing, among many others. Cross-linked rubbers can be composed of vulcanized natural rubbers, polybutadiene, styrene-butadiene copolymers, acrylonitrile-butadiene copolymers, polyisoprene, isoprene-isobutylene copolymers, ethylene-propylene rubber, ethylene propylene diene monomer (EPDM) rubber, silicone elastomers, fluoroelastomers, polyurethane elastomers, and nitrile rubbers, among others. Cross-linked rubbers can be advantageous for combining toughness, elasticity, and resistance to heat, chemicals, and other environmental factors. However, cross-linked rubbers also have important disadvantages. For instance, cross-linked rubbers cannot flow, even at elevated temperature, due to their relatively high cross-linking density. Furthermore, cross-linked rubbers cannot be reprocessed because their cross-linking is irreversible.

[0003] Ionomers have recently garnered interest as polymer alternatives to cross-linked rubbers. Such materials have been shown to retain the mechanical properties of cross-linked rubbers, such as their ability to elastically deform, without the need to chemically cross-link the polymer. However, large scale and / or industrial size production of such materials is difficult due to high operational costs and inefficient batch-wise production. Furthermore, the batch-wise production of such materials can result in batch-to-batch variation in the thermal and thermomechanical properties of such materials.

[0004] Thus, there is a need to develop new, more efficient processes for large scale production of ionomeric materials.SUMMARY

[0005] The present disclosure relates to polyolefin-based ionomers and production of polyolefin-based ionomers. More specifically, the present disclosure relates to aluminum-containing polyolefins, such as polyolefin-based ionomers, and methods of preparing such aluminum-containing polyolefins.

[0006] In some embodiments, a method for preparing a terpolymer includes introducing two or more different a-olefin monomers and an aluminum vinyl monomer to a first reaction zone. The method further includes introducing a catalyst system to the first reaction zone to form a reaction mixture. The method further includes polymerizing the reaction mixture to form a polymer mixture. The method further includes transferring the polymer mixture from the first reaction zone to a second reaction zone. The method further includes introducing a reagent to the second reaction zone. The reagent includes an oxygen containing reagent, a sulfur containing reagent, or a combination thereof. The method further includes reacting the polymer mixture with the reagent to form a polymer composition comprising the terpolymer.

[0007] In some embodiments, a polymer composition includes a terpolymer. The terpolymer includes ethylene, propylene, and an aluminum vinyl monomer that has reacted with an oxygen containing reagent. The terpolymer includes an ethylene content of 25 wt% or less, a complex viscosity (r|*ooi) of about 100 kPa*s or more at 150°C, a shear elastic modulus (G’o.oi) of about 300 Pa or more at 150°C, and a strain hardening ratio greater than 1.1 at 150°C.BRIEF DESCRIPTION OF DRAWINGS

[0008] So that the manner in which the above recited features of embodiments of the present disclosure can be understood in detail, a more particular description of the disclosure, briefly summarized above, may be had by reference to embodiments, some of which are illustrated in the appended drawings. It is to be noted, however, that the appended drawings illustrate only typical embodiments of this disclosure and are therefore not to be considered limiting of its scope, for the disclosure may admit to other equally effective embodiments.

[0009] FIG. 1 is a flow diagram depicting a method of preparing a terpolymer, according to an embodiment described herein.

[0010] FIG. 2A is a graph illustrating a rheological roperty of terpolymers, according to an embodiment.

[0011] FIG. 2B is a graph illustrating a rheological property of terpolymers, according to an embodiment.

[0012] FIG. 2C is a graph illustrating a rheological property of terpolymers, according to an embodiment.

[0013] FIG. 3 is a graph illustrating a rheological property of terpolymers, according to an embodiment.DETAILED DESCRIPTION

[0014] The present disclosure provides a method for the continuous production of terpolymers composed of ethylene, one or more additional a-olefin monomers, and aluminum containing monomer units. The method disclosed herein utilizes a first reaction zone for the polymerization reaction and a second reaction zone for the oxidation reaction. The method disclosed herein has been shown to be a successfully continuous process, which can increase production efficiency and decrease cost. Reaction zone conditions and input ratios w ere additionally investigated to determine their effects on the resulting material’s thermal and thermomechanical properties. The terpolymers formed from the process disclosed herein allow for ion formation of the aluminum containing monomer units in the terpolymer composition. Without being bound by theory, such ion formation has shown to increase the melt strength of the terpolymer compositions without sacrificing other desired thermal and thermomechanical properties.

[0015] The term “and / or” refers to both the inclusive “and” case and the exclusive “or” case, and such terms are used herein for brevity. For example, a composition comprising “A and / or B” may comprise A alone, B alone, or both A and B; and a composition comprising “A and or B” may comprise A alone, or both A and B.

[0016] The percentage of a particular monomer in a polymer is expressed herein as weight percent (wt%) based on the total weight of the polymer present. Other percentages are expressed as weight percent (wt%), based on the total weight of the particular composition present, unless otherwise noted. Room temperature is 25°C ± 2°C and atmospheric pressure is 101.325 kPa unless otherwise noted.

[0017] For purposes herein a “polymer” refers to a compound having two or more “mer” units (see below for polyester mer units), that is, a degree of polymerization of two or more, where the mer units can be of the same or different species. A “homopolymer” is a polymer having mer units that are the same species. A “copolymer” is a polymer having two or more different species of mer units. A “terpolymer” is a polymer having three different species of mer units. “Different” in reference to mer units indicates that the mer units differ from each other by at least one atom or are different isomerically. Unless otherwise indicated, reference to a polymer herein includes a copolymer, a terpolymer, or any polymer comprising a plurality of the same or different species of repeating units.

[0018] The terms “aluminum vinyl compound,” “aluminum vinyl monomer,” and “aluminum containing monomer” may be used interchangeably.

[0019] The term “residue” or “unit”, as used herein, means the organic structure of the monomer in its as-polymerized form as incorporated into a polymer, e.g., throughpolymerization of the corresponding monomer. Throughout the specification and claims, reference to the monomer(s) in the polymer is understood to mean the corresponding as-polymerized form or residue of the respective monomer.

[0020] As used herein, an “olefin,” alternatively referred to as “alkene,” is a linear, branched, or cyclic compound of carbon and hydrogen having at least one double bond. For purposes of this specification and the claims appended thereto, when a polymer or copolymer is referred to as “comprising” an olefin, the olefin present in such polymer or copolymer is the polymerized form of the olefin. For example, when a copolymer is described as having an “ethylene” content of about 35 wt% to about 55 wt%, it is understood that the mer unit in the copolymer is derived from ethylene in the polymerization reaction and the derived units are present at about 35 wt% to about 55 wt%, based upon the weight of the copolymer.

[0021] As used herein, a “polymer” may refer to homopolymers, copolymers, interpolymers, terpolymers, etc. A “polymer” has two or more of the same or different monomer units. A “homopolymer” is a polymer having monomer units that are the same. A “copolymer” is a polymer having two or more monomer units that are different from each other. A “terpolymer” is a polymer having three monomer units that are different from each other. The term “different” as used to refer to monomer units indicates that the monomer units differ from each other by at least one atom or are different isomerically. Accordingly, the definition of copolymer, as used herein, includes terpolymers and the like. Likewise, the definition of polymer, as used herein, includes copolymers and the like.

[0022] As used herein, an ethylene polymer having a density of greater than 0.860 to less than 0.910 g / cm3may be referred to as an ethylene plastomer or plastomer; an ethylene polymer having a density of 0.910 to less than 0.925 g / cm3may be referred to as a “linear low density polyethylene” (LLDPE) when substantially linear (having minor or no long chain branching) as is typically the case for Ziegler-Nata or metallocene-catalyzed PE or branched low density polyethylene (LDPE) when significantly branched (having a high degree of long chain branching), as is often the case with free-radical polymerized PE; 0.925 to 0.940 g / cm3may be referred to as a “medium density polyethylene” (MDPE); and an ethylene polymer having a density of greater than 0.940 g / cm3may be referred to as a "high density polyethylene” (HDPE). Density is determined according to ASTM D792. Specimens are prepared according to ASTM D4703 - Annex 1 Procedure C followed by conditioning according to ASTM D618 - Procedure A prior to testing.

[0023] As used herein, and unless otherwise specified, the term “hydrocarbon” means a class of compounds containing hydrogen bound to carbon, and encompasses (i) saturatedhydrocarbon compounds, (ii) unsaturated hydrocarbon compounds, and (iii) mixtures of hydrocarbon compounds (saturated or unsaturated), including mixtures of hydrocarbon compounds having different values of n.

[0024] As used herein, a composition or film “free of’ a component refers to a composition / film substantially devoid of the component or comprising the component in an amount of less than 0.01 wt%, by weight of the total composition.

[0025] As used herein, the term “polymerization conditions” refers to conditions conducive to the reaction of one or more olefin monomers when contacted with an activated olefin polymerization catalyst to produce a polyolefin polymer, including a skilled artisan’s selection of temperature, pressure, reactant concentrations, optional solvent / diluents, reactant mixing / addition parameters, and other conditions within at least one polymerization reactor and / or reaction zone.

[0026] For the purposes of the present disclosure, the numbering scheme for the Periodic Table Groups is used as described in Chemical and Engineering News, v.63(5), pg. 27 (1985).

[0027] The following abbreviations may be used herein: Me is methyl, Et is ethyl, Ph is phenyl, PDI is polydispersity index, MAO is methylalumoxane, SMAO is supported methylalumoxane, NMR is nuclear magnetic resonance, ppm is part per million, THF is tetrahydrofuran.

[0028] As used herein, olefin polymerization catalyst(s) refer to any catalyst, such as an organometallic complex or compound that is capable of coordination polymerization addition where successive monomers are added in a monomer chain at the organometallic active center.

[0029] The terms “substituent.” “radical,” “group.” and “moiety ” may be used interchangeably.

[0030] The term “alpha-olefin” refers to an olefin having a terminal carbon-to-carbon double bond in the structure thereof ((R R )-C=CH2, where R and R can be independently hydrogen or any hydrocarbyl group; such as R is hydrogen and R is an alky l group). A “linear alpha-olefin” is an alpha-olefin defined in this paragraph wherein R is hydrogen, and R is hydrogen or a linear alkyl group.

[0031] For the purposes of the present disclosure, ethylene shall be considered an alphaolefin.

[0032] As used herein, and unless otherwise specified, the term “Cn” means hydrocarbon(s) having n carbon atom(s) per molecule, wherein n is a positive integer. Theterm “hydrocarbon” means a class of compounds containing hydrogen bound to carbon, and encompasses (i) saturated hydrocarbon compounds, (ii) unsaturated hydrocarbon compounds, and (iii) mixtures of hydrocarbon compounds (saturated and or unsaturated), including mixtures of hydrocarbon compounds having different values of n. Likewise, a “Cm-Cy” group or compound refers to a group or compound including carbon atoms at a total number thereof from m to y. Thus, aC1-C50 alkyl group refers to an alkyl group including carbon atoms at a total number thereof of about 1 to about 50.

[0033] Unless otherwise indicated, (e.g., the definition of "substituted hydrocarbyl", "substituted aromatic", etc.), the term “substituted” means that at least one hydrogen atom has been replaced with at least one non-hydrogen group, such as a hydrocarbyl group, a heteroatom, or a heteroatom containing group, such as halide (such as Br, Cl, F or I) or at least one functional group such as -NR*2, -OR*, -SeR*, -TeR*, -PR*2, -AsR*2, -SbR*2, -SR*, -BR*2,-SiR*3, -GeR*3, -SnR*3, -PbR*3, where each R* is independently a hydrocarbyl orhalocarbyl radical, and two or more R* may join together to form a substituted or unsubstituted completely saturated, partially unsaturated, or aromatic cyclic or polycyclic ring structure), or where at least one heteroatom has been inserted within a hydrocarbyl ring.

[0034] The term "substituted hydrocarbyl" means a hydrocarbyl radical in which at least one hydrogen atom of the hydrocarbyl radical has been substituted with at least one heteroatom (such as halide, e.g., Br, Cl, F or I) or heteroatom-containing group (such as a functional group, e.g., -NR*2, -OR*, -SeR*, -TeR*, -PR*2, -AsR*2, -SbR*2, -SR*, -BR*2, -SiR*3, -GeR*3,-SnR*3, -PbR*3, where each R* is independently a hydrocarbyl orhalocarbyl radical, and two or more R* may join together to form a substituted or unsubstituted completely saturated, partially unsaturated, or aromatic cyclic or polycyclic ring structure), or where at least one heteroatom has been inserted within a hydrocarbyl ring.

[0035] The term "substituted aromatic," means an aromatic group having 1 or more hydrogen groups replaced by a hydrocarbyl. substituted hydrocarbyl, heteroatom or heteroatom containing group.

[0036] The terms “hydrocarbyl radical,” “hydrocarbyl group,” or “hydrocarbyl” may be used interchangeably and are defined to mean a group including hydrogen and carbon atoms only. For example, a hydrocarbyl can be a C1-C100 radical that may be linear, branched, or cyclic, and when cyclic, aromatic or non-aromatic. Examples of such radicals may include,but are not limited to, alkyl groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, pentyl, iso-amyl, hexyl, octyl cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cyclooctyl, and aryl groups, such as phenyl, benzy l, naphthyl.

[0037] The terms “alkoxy” and “alkoxide” mean an alkyl or aryl group bound to an oxygen atom, such as an alkyd ether or ary l ether group / radical connected to an oxygen atom and can include those where the alkyl / aryl group is a Ci to Cio hydrocarbyl. The alkyl group may be straight chain, branched, or cyclic. The alkyl group may be saturated or unsaturated. Examples of suitable alkoxy radicals can include methoxy, ethoxy, n-propoxy, iso-propoxy, n-butoxy, iso-butoxy, sec-butoxy, tert-butoxy, phenoxyl.

[0038] The term "alkenyl" means a straight-chain, branched-chain, or cyclic hydrocarbon radical having one or more double bonds. These alkenyl radicals may be optionally substituted. Examples of suitable alkenyl radicals can include ethenyl, propenyl, allyl, 1,4-butadienyl, cyclopropenyl, cyclobutenyl, cyclopentenyl, cyclohexenyl, cycloctenyl, including their substituted analogues.

[0039] The terms “alkyl radical,” “alkyl group,” and “alky 1” are used interchangeably throughout this disclosure. For purposes of this disclosure, "alkyl radical" is defined to be Ci-Cioo alkyls that may be linear, branched, or cyclic. Examples of such radicals can include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobut l. sec-butyl, tert-buty l, pentyl, iso-amyl, hexyl, octyl, cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cyclooctyl, including their substituted analogues. Some examples of alkyl may include 1 -methylethyl, 1 -methylpropyl.1 -methylbutyl, 1 -ethylbutyl, 1,3 -dimethylbutyl, 1 -methyl- 1 -ethylbutyl, 1, 1 -diethylbutyl, 1 -propylpentyl, 1 -phenylethyl, i-propyl, 2-butyl, sec-pentyl, sec-hexyl, and the like.

[0040] The term "ary l" or "ary l group" means an aromatic ring and the substituted variants thereof, such as phenyl, 2-methyl-phenyl. xylyl, 4-bromo-xylyl. Likewise, “heteroaryl” means an aryl group where a ring carbon atom (or two or three ring carbon atoms) has been replaced with a heteroatom, such as N, O, or S. As used herein, the term "aromatic" also refers to pseudoaromatic heterocycles which are heterocyclic substituents that have similar properties and structures (nearly planar) to aromatic heterocyclic ligands, but are not by definition aromatic; likewise, the term aromatic also refers to substituted aromatics.

[0041] Where isomers of a named alkyl, alkenyl, alkoxide, or aryl group exist (e.g., n-butyl, iso-butyl, sec-butyl, and tert-butyl), reference to an alkyl, alkenyl, alkoxide, or aryl group without specifying a particular isomer (e.g., butyl) expressly discloses all isomers e.g., n-butyl, iso-butyl, sec-butyl, and tert-butyl).

[0042] The term "ring atom" means an atom that is part of a cyclic ring structure. By this definition, a benzyl group has six ring atoms and tetrahydrofuran has five ring atoms.

[0043] A heterocyclic ring is a ring having a heteroatom in the ring structure as opposed to a heteroatom substituted ring where a hydrogen on a ring atom is replaced with a heteroatom. For example, tetrahydrofuran is a heterocyclic ring and 4-N, N-dimethylamino-phenyl is a heteroatom-substituted ring. Other examples of heterocycles may include pyridine, imidazole, and thiazole.

[0044] As used herein, Mn is number average molecular weight, Mw is weight average molecular weight, and Mz is z average molecular weight, wt% is weight percent, and mol% is mole percent. Molecular weight distribution (MWD), also referred to as polydispersity index (PDI), is defined to be Mw divided by Mn. Unless otherwise noted, all molecular weight units (e.g., Mw, Mn, Mz) are g / mol.

[0045] The terms “catalyst compound”, “catalyst complex”, “transition metal complex”, “transition metal compound”, “precatalyst compound”, and “precatalyst complex” are used interchangeably.

[0046] A “catalyst system” is a combination of at least one catalyst compound, at least one activator, an optional coactivator, and an optional support material. When "catalyst system" is used to describe such a pair before activation, it means the unactivated catalyst complex (precatalyst) together with an activator and, optionally, a coactivator. When it is used to describe such a pair after activation, it means the activated complex and the activator or other charge-balancing moiety. The catalyst compound may be neutral as in a precatalyst, or a charged species with a counter ion as in an activated catalyst system. For the purposes of the present disclosure and the claims thereto, when catalyst systems are described as including neutral stable forms of the components, it is well understood by one of ordinary skill in the art, that the ionic form of the component is the form that reacts with the monomers to produce polymers. A polymerization catalyst system is a catalyst system that can polymerize monomers to polymer. Furthermore, catalyst compounds and activators represented by formulae herein are intended to embrace both neutral and ionic forms of the catalyst compounds and activators.

[0047] An “anionic ligand” is a negatively charged ligand which donates one or more pairs of electrons to a metal ion. A “Lewis base” or “neutral donor ligand” is a neutrally charged ligand which donates one or more pairs of electrons to a metal ion. Examples of Lewis bases include ethylether, trimethylamine, pyridine, tetrahydrofuran, dimethylsulfide, and triphenylphosphine. The term “heterocyclic Lewis base” refers to Lewis bases that arealso heterocycles. Examples of heterocyclic Lewis bases include pyridine, imidazole, thiazole, and furan.

[0048] A scavenger is a compound that can be added to facilitate polymerization by scavenging impurities. Some scavengers may also act as activators and may be referred to as coactivators. A coactivator, that is not a scavenger, may also be used in conjunction with an activator in order to form an active catalyst. In at least one embodiment, a coactivator can be pre-mixed with the transition metal compound to form an alkylated transition metal compound.

[0049] The term "continuous" means a system that operates without interruption or cessation for an extended period of time. For example, a continuous process to produce a polymer would be one where the reactants are continually introduced into one or more reactors and / or reaction zones and polymer product is continually withdrawn.

[0050] A solution polymerization means a polymerization process in which the polymer is dissolved in a liquid polymerization medium, such as an inert diluent or monomer(s) or their blends. A solution polymerization can be homogeneous. A homogeneous polymerization is one where the polymer product is dissolved in the polymerization medium. Suitable systems may be not turbid as described in J. Vladimir Oliveira, C. Dariva and J. C. Pinto, Ind. Eng. Chem. Res., 2000, Vol. 29, p. 4627.

[0051] A bulk poly merization means a polymerization process in which the monomers and or comonomers being polymerized are used as a solvent or diluent using little or no inert solvent as a solvent or diluent. A small fraction of inert sol vent / diluent might be used as a carrier for catalyst and scavenger. A bulk polymerization system contains less than 25 wt% of inert solvent or diluent, such as less than 10 wt%, such as less than 1 wt%, such as 0 wt%.

[0052] The term “single catalyst compound” refers to a catalyst compound corresponding to a single structural formula, although such a catalyst compound may comprise and be used as a mixture of isomers, e.g., stereoisomers.

[0053] A catalyst system that utilizes a single catalyst compound means a catalyst system that is prepared using only a single catalyst compound in the preparation of the catalyst system. Thus, such a catalyst system is distinguished from, for example, “dual” catalyst systems, which are prepared using two catalyst compounds having different stmctural formulas, e.g., the connectivity between the atoms, the number of atoms, and / or the type of atoms in the two cataly st compounds is different. Thus, one catalyst compound is considered different from another if it differs by at least one atom, by either number, type, or connection. For example, bisindenyl zirconium dichloride is different from (indenyl)(2-methylindenyl)zirconium di chloride which is different from (indenyl)(2-methylindenyl) hafnium dichloride. Unless otherwise noted, catalyst compounds that differ only in that they are stereoisomers of each other are not considered to be different catalyst compounds. For example, rac-dimethylsilylbis(2-methyl 4-phenyl)hafnium dimethyl and meso-dimethylsilylbis(2 -methyl 4-phenyl)hafnium dimethyl are considered to be not different.

[0054] The terms “cocatalyst’ ' and “activator’" are used herein interchangeably and are defined to be any compound which can activate any one of the catalyst compounds described above by converting the neutral catalyst compound to a catalytically active catalyst compound cation.

[0055] In an extrusion process, “viscosity"’ is a measure of resistance to shearing flow. Shearing is the motion of a fluid, layer-by-layer, like a deck of cards. When polymers flow through straight tubes or channels, the polymers are sheared, and resistance is expressed in terms of viscosity.

[0056] “Extensional"’ or “elongational viscosity” is the resistance to stretching. In fiber spinning, film blowing and other processes where molten polymers are stretched, the elongational viscosity plays a role. For example, for certain liquids, the resistance to stretching can be three times larger than in shearing. For some polymeric liquids, the elongational viscosity can increase (tension stiffening) with the rate, although the shear viscosity decreased.

[0057] The term “melt index” (“MI”) is the number of grams extruded in 10 minutes under the action of a standard load (2.16 kg) and is an inverse measure of viscosity. A high MI implies low viscosity, and a low MI implies high viscosity. In addition, polymers can have shear thinning behavior, which means that their resistance to flow decreases as the shear rate increases. This is due to, e.g., molecular alignments in the direction of flow and disentanglements. As provided herein, MI (h) is determined according to ASTM D1238-E (190°C / 2.16 kg), also sometimes referred to as I2 or I2.16.

[0058] The term “high load melt index” (“HLMI”), is the number of grams extruded in 10 minutes under the action of a standard load (21.6 kg) and is an inverse measure of viscosity. As provided herein. HLMI (I21) is determined according to ASTM D1238 (190°C / 21.6 kg) and is also sometimes referred to as I21 or I21.6.

[0059] The “melt index ratio” (“MIR”) provides an indication of the amount of shear thinning behavior of the polymer and is a parameter that can be correlated to the overall polymer mixture molecular weight distribution data obtained separately by using GelPermeation Chromatography (“GPC”) and possibly in combination with another polymer analysis including TREF. MIR is the ratio of I21 / I2 (also referred to as HLMI / MI).

[0060] The term '‘melt strength” is a measure of the extensional viscosity and is representative of the maximum tension that can be applied to the melt without breaking. Extensional viscosity is the polyethylene’s ability7to resist thinning at high draw rates and high draw ratios. In melt processing of polyolefins, the melt strength is defined by characteristics that can be quantified in process-related terms and in rheological terms. In extrusion blow molding and melt phase thermoforming, a branched polyolefin of the appropriate molecular weight can support the weight of the fully melted sheet or extruded portion prior to the forming stage. This behavior is sometimes referred to as sag resistance.

[0061] For the sake of brevity, only certain ranges are explicitly disclosed herein.However, ranges from any lower limit may be combined with any upper limit to recite a range not explicitly recited, as well as, ranges from any lower limit may be combined with any other lower limit to recite a range not explicitly recited, in the same way, ranges from any upper limit may be combined with any other upper limit to recite a range not explicitly recited. Additionally, “in a range” or “within a range” includes every point or individual value between its end points even though not explicitly recited and includes the end points themselves. Thus, every point or individual value may serve as its own lower or upper limit combined with any other point or individual value or any other lower or upper limit, to recite a range not explicitly recited.

[0062] FIG. 1 shows a process flow diagram of a method 100 for forming aluminum containing polyolefins. The method 100 can include introducing one or more monomers a catalyst system to a reaction zone to form reaction mixture that is subsequently polymerized to form a polymer mixture. The one or more monomers may be introduced to the reaction zone either simultaneously or sequentially. The polymer mixture flows to a second reaction zone where it reacts with an oxygen or sulfur containing reagent to form polyolefins with increased oxygen content, polarity, and melt strength. As discussed below, the polymerization and oxidation reactions are conducted in separate reaction zones. The method(s) disclosed herein separate these two reactions into two separate reaction zones to allow for the development of a continuous process. Such a continuous process(es) can enable continuous production of terpolymers at an increased production efficiency and reduced operational cost.

[0063] At operation 102 of the method, 100 includes introducing one or more monomer inputs to a first reaction zone. The monomer input may include one or more olefinmonomers and an aluminum containing monomer. The olefin monomer may include ethylene or a combination of ethylene and one or more olefin monomers. The olefin monomers may include substituted or unsubstituted C2to C40 alpha olefins, such as C2to C20alpha olefins, such as C2to C12alpha olefins, such as ethylene, propylene, butene, pentene, hexene, heptene, octene, nonene, decene, undecene, dodecene and isomers thereof. In at least one embodiment, the monomer includes ethylene and an optional comonomer including one or more C3to C40olefins, such as C4to C20olefins, such as C6to C12olefins. The ethylene monomer and the optional comonomer may be introduced to the first reaction zone simultaneously or sequentially. The C3to C40olefin monomers may be linear, branched, or cyclic. The C3to C40cyclic olefins may be strained or unstrained, monocyclic or polycyclic, and may optionally include heteroatoms and or one or more functional groups. In another embodiment, the monomer includes ethylene and an optional comonomer including one or more C3to C40olefins, such as C4to C20olefins, such as C6to C12olefins. The C4to C40olefin monomers may be linear, branched, or cyclic. The C4to C40cyclic olefins may be strained or unstrained, monocyclic or polycyclic, and may optionally include heteroatoms and or one or more functional groups.

[0064] A suitable aluminum containing monomer can include an aluminum vinyl compound (e g., an alkenylaluminum). In some embodiments, the aluminum vinyl compound is represented by Al(R’)3-v(R)v. where R is a hydrocarbenyl group containing 4 to 20 carbon atoms having an allyl chain end, R' is a hydrocarbyl group containing 1 to 30 carbon atoms, and v is 1 to 3 alternately v is 1.1 to 2.9, alternately 1.5 to 2.9, alternately 1.5 to 2.5, alternately 1.8 to 2.2. The compounds represented by Al(R’)3-v(R)v are typically a neutral species, but anionic formulations may be envisioned, such as those represented by [A1(R')4- (R)W]’, where w is 0.1 to 4, alternately 1.1 to 4, R is a hydrocarbenyl group containing 4 to 50 carbon atoms having an allyl chain end, and R' is a hydrocarbyl group containing 1 to 50 carbon atoms. In at least one embodiment, v is 1.

[0065] In at least one embodiment of a formula for an aluminum vinyl compound described herein, each R' is independently chosen from Ci to C50 hydrocarbyl groups (such as a Ci to C20 alkyl groups, preferably methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, undecyl, dodecyl, or an isomer thereof), and R is represented by -(CH2)nCH=CH2, where n is an integer from 2 to 18, preferably between 5 to 18, preferably 5 to 12, preferably 5 to 6. In at least one embodiment, an aluminum containing monomer can include isobutyl-di(oct-7-en-l-yl)-aluminum, isobutyl-di(dec-9-en-l-yl)-aluminum, isobutyl-di(non-8-en- 1 -yl)-aluminum, isobuty 1-di (hept-6-en- 1 -yl)-aluminum, dimethy l(oct-7 -en-1 -yl)aluminum, diethyl(oct-7-en-l-yl)aluminum, dibutyl(oct-7-en-l-yl)aluminum, diisobutyl(oct-7-en-l-yl)aluminum, diisobutyl(non-8-en-l-yl)aluminum, diisobutyl(dec-9-en-I -yl)aluminum, diisobutyl(dodec-10-en-l-yl)aluminum, diisobutyl(hept-6-en-l-yl)aluminum, diethyl(hept-6-en-l-yl)aluminum, dimethyl(hept-6-en-l-yl)aluminum and the like.

[0066] In at least one embodiment, the aluminum vinyl compound can be represented by the Formula (I):wherein each R is independently a Ci-Cio hydrocarbyl, and n is an integer from 3-10. In some embodiments, n is an integer from 6-8. In at least one embodiment, n is 6. In at least one embodiment, each R is isobutyl and n is an integer from 6-8, such as 6.

[0067] In at least one embodiment, an aluminum vinyl compound includes the organoaluminum reaction products of an aluminum reagent and an alkyl diene. An alkyl diene may include compounds having two “a-olefms” at two termini of the carbon chain. The alkyl diene can be a straight chain or branched alkyl chain and substituted or unsubstituted. Exemplary alkyl dienes may include 1,3-butadiene, 1,4-pentadiene, 1,5-hexadiene1,6-heptadiene, 1,7-octadiene, 1, 8-nonadiene, 1,9-decadiene, 1,10-undecadiene,1,11 -dodecadiene, 1,12-tridecadiene, 1,13 -tetradecadiene, 1,14-pentadecadiene,1,15-hexadecadiene, 1,16 -heptadecadiene, 1,17-octadecadiene, 1,18-nonadecadiene, 1,19-eicosadiene, 1,20-heneicosadiene, and the like. Exemplary aluminum reagents can include triisobutylaluminum, diisobutylaluminumhydride, isobutylaluminumdihydride. and aluminumhydride (AIH3).

[0068] In some embodiments, the monomer input(s) include a solvent and / or diluent. Suitable diluents / solvents include non-coordinating, inert liquids. In at least one embodiment, a solvent / diluent includes straight and branched-chain hydrocarbons, such as isobutane, butane, pentane, isopentane, hexanes, isohexane, heptane, octane, dodecane, and mixtures thereof; cyclic and alicyclic hydrocarbons, such as cyclohexane, cycloheptane, methylcyclohexane, methylcycloheptane, and mixtures thereof, such as can be found commercially (Isopar™); perhalogenated hydrocarbons, such as perfluorinated C4-10 alkanes, chlorobenzene, and aromatic and alkylsubstituted aromatic compounds, such as benzene,toluene, mesitylene, and xylene. Suitable solvents also include liquid olefins which may act as monomers or comonomers including ethylene, propylene, 1 -butene, 1 -hexene. 1 -pentene, 3-methyl- 1 -pentene, 4-methyl-l -pentene, 1 -octene, 1 -decene, and mixtures thereof. In some embodiments, aliphatic hydrocarbon solvents are used as the solvent, such as isobutane, butane, pentane, isopentane, hexanes, isohexane, heptane, octane, dodecane, and mixtures thereof; cyclic and alicyclic hydrocarbons, such as cyclohexane, cycloheptane, methylcyclohexane, methylcycloheptane, and mixtures thereof. In another embodiment, the solvent is not aromatic, preferably aromatics are present in the solvent at less than 1 wt%, such as less than 0.5 wt%, such as less than 0 wt% based upon the weight of the solvents.

[0069] In at least one embodiment, the monomer input(s) include a solvent in an amount of about 50 vol% or less, based on the total volume of the of the monomer input. In at least one embodiment, the monomer input(s) include a solvent in an amount of about 50 wt% or less, based on the total weight of the monomer input.

[0070] In some embodiments, the monomer input(s) is introduced to the reaction zone at a rate of about 1x10-5(L / volume of reactor zone) / min (otherwise referred to as “L / volume / min”) to about 3.0 L / volume / min. To obtain the actual monomer flow rate, the “L / volume / min” value is multiplied by the volume of the reactor or volume of the reaction zone in units of Liters. For example, if the monomer flow rate was 2.0 L / volume / min and the volume of the reactor was 0.5 L, then the actual flow rate of the monomer into the reactor would be 1.0 L / min.

[0071] In some embodiments, the monomer input(s) is introduced to the reaction zone at a rate of about 0.1 (g / volume of reactor zone) / min (otherwise referred to as “g / volume / min”) to about 2.0 g / volume / min. To obtain the actual monomer flow rate, the “g / volume / min'’ value is multiplied by the volume of the reactor or the volume of the reaction zone in units of Liters. For example, if the monomer flow rate was 1.5 g / volume / min and the volume of the reactor was 1.0 L, then the actual flow rate of the monomer into the reactor would be 1.5 g / min.

[0072] In some embodiments, the monomer input includes one or more of ethylene, propylene, and an aluminum vinyl compound. Ethylene may be introduced to the reaction zone at a flow rate of about 0.1 L / volume / min to about 2.5 L / volume / min, such as about 0.5 L / volume / min to about 2 L / volume / min, such as about 1 L / volume / min to about 1.5 L / volume / min, alternatively about 0.1 L / volume / min to about 0.5 L / volume / min, alternatively about 0.5 L / volume / min to about 1 L / volume / min. alternatively about1.5 L / volume / min to about 2 L / volume / min, alternatively about 2 L / volume / min to about3 L / volume / min. Propylene may be introduced to the reaction zone at a input rate of about1 (g / volume of reactor) / min (otherwise referred to as ’g / volume / min Jto about25 g / volume / min, such as about 5 g / volume / min to about 20 g / volume / min, such as about 10 g / volume / min to about 1 g / volume / min, alternatively about 1 g / volume / min to about 5 g / volume / min, alternatively about 5 g / volume / min to about 10 g / volume / min, alternatively about 15 g / volume / min to about 20 g / volume / min, alternatively about 20 g / volume / min to about 25 g / volume / min. The aluminum vinyl compound may be introduced to the reaction zone at a flow rate of about 0.01 mL / volume / min to about 4 mL / volume / min, such as about 0.1 mL / volume / min to about 2.5 mL / volume / min, such as about 0.5 mL / volume / min to about2 mL / volume / min, alternatively about 0.01 mL / volume / min to about 0.1 mL / volume / min, alternatively about 0.1 mL / volume / min to about 0.5 mL / volume / min. alternatively about 0.5 mL / volume / min to about 1 mL / volume / min, alternatively about 1 mL / volume / min to about 2 mL / volume / min, alternatively about 2 mL / volume / min to about 2.5 mL / volume / min, alternatively about 2.5 mL / volume / min to about 4 mL / volume / min.

[0073] At operation 104 of the method 100, a catalyst system is introduced to the reaction zone with the monomer input to produce a reaction mixture. A catalyst system may include a catalyst compound and an activator, such as an alumoxane or a non-coordinating anion. The catalyst compound and the activator may be pre-mixed and fed into the reactor, or each component may be fed into the reactor separately. Additionally, the catalyst system may be formed by combining the catalyst compound and the activator with a support structure which is then fed into the reactor.

[0074] In at least one embodiment, the catalyst system includes a bis(phenolate) Lewis base catalyst compound. The bis(phenolate) Lewis base catalyst compound may include a Group 4 transition metal, a tridentate dianionic ligand containing two anionic donor groups, and a neutral heterocyclic Lewis base donor. The heterocyclic donor can be covalently- bonded between the two anionic donors. The tridentate dianionic ligand can coordinate to the metal with two anionic oxygen donors and one neutral heterocyclic nitrogen donor to form a pair of eight-membered metallocycle rings.

[0075] In at least one embodiment, the catalyst compound is represented by Formula (II):wherein:M is a Group 3, 4, 5, or 6 transition metal, or a lanthanide metal (such as Hf, Zr, Ti, Sc, Y, or La);each of E and E' is independently O, S, or NRA, where RAis independently hydrogen. C1-C40 hydrocarbyl, substituted C1-C40 hydrocarbyl, or a heteroatom-containing group, such as O, such as both E and E' are O;Q is group 14, 15, or 16 atom, such as Q is C, O. S, or N, such as Q is C, N, or O, such as Q is N;A’QA1is part of a heterocyclic Lewis base containing 4 to 40 non-hydrogen atoms and links A2to A2via a 3-atom bridge with Q being the central atom of the 3-atom bridge (A'QA1combined with the curved line shown joining A1and A1represents the heterocyclic Lewis base);each of A1and A1' is independently C, N, or C(RB), where RBis selected from hydrogen, C1-C20 hydrocarbyl, and substituted C1-C20 hydrocarbyl(for example, each of A1and A1' are C);adivalent group containing 2 to 40 non-hydrogen atoms and links A1to the E-bonded aryl group via a 2-carbon atom bridge, and A3and A2are combined to form a substituted hydrocarbyl ring, an unsubstituted hydrocarbyl ring, a substituted heterocyclic ring, or an unsubstituted heterocyclic rings each having 5, 6, 7, or 8 ring atoms, and where substitutions on the ring can join to form additional rings, such as A3and A2are combined to form ortho-phenylene, substituted ortho-phenylene, ortho-arene, substituted ortho-arene, indolene, substituted indolene, benzothiophene, substituted benzothiophene, pyrrolene, substituted pyrrolene, thiophene, substituted thiophene;A___A is a divalent group containing 2 to 40 non-hydrogen atoms and links A1' to the E'-bonded aryl group via a 2-carbon atom bridge, and A3and A2are combined to form a substituted hydrocarbyl ring, an unsubstituted hydrocarbyl ring, a substituted heterocyclic ring, or an unsubstituted heterocyclic rings each having 5, 6, 7, or 8 ring atoms, and where substitutions on the ring can join to form additional rings, such as A3and A2are combined to form, such as ortho-phenylene, substituted ortho-phenylene, ortho-arene, substituted orthoarene, indolene, substituted indolene, benzothiophene, substituted benzothiophene, pyrrolene, substituted pyrrolene, thiophene, substituted thiophene;each L is independently a Lewis base;X’ is an anionic ligand;any two L groups may be joined together to form a polydentate (e.g., bidentate) Lewis base;an X’ group may be joined to an L group to form a monoanionic bidentate group; n is 1, 2, or 3;m is 0, 1, or 2;n+m is 4 or less; andeach of R1, R2, R3, R4, R1, R2, R3, and R4is independently hydrogen, C1-C40 hydrocarbyl, substituted C1-C40 hydrocarbyl, a heteroatom or a heteroatom-containing group (such as R1and R1are independently a hydrocarbyl group, such as a tertiary alkyl group, or a cyclic hydrocarbyl group, such as a cyclic tertiary alkyl group), or one or more of R1and R2. R2and R3, R3and R4, R1and R2, R2and R3, R3and R4may be joined to form one or more substituted hydrocarbyl rings, unsubstituted hydrocarbyl rings, substituted heterocyclic rings, or unsubstituted heterocyclic rings each having 5, 6, 7, or 8 ring atoms, and where substitutions on the ring can join to form additional rings.

[0076] The metal, M, is selected from Group 3, 4, 5, or 6 elements, such as Group 4. For example, the metal, M, is a Group 4 metal, such as titanium, zirconium, or hafnium.

[0077] The donor atom Q of the neutral heterocyclic Lewis base (in Formula (I)) can be nitrogen, sulfur, or oxygen. In some embodiments, Q is nitrogen.

[0078] Non-limiting examples of neutral heterocyclic Lewis base groups include pyridine, pyrazine, pyrimidine, triazine, thiazole, imidazole, thiophene, oxazole, thiazole, furan, and substituted variants of thereof. In some embodiments, heterocyclic Lewis base groups can include pyridine, pyrazine, thiazole, or imidazole.

[0079] In some embodiments, each of A1and A1is independently C, N, or C(R5), where R5is selected from hydrogen, C1-C20 hydrocarbyl, and substituted C1-C20 hydrocarbyl. In some embodiments, each of A1and A1' is carbon. When Q is carbon, each of A1and A1can be independently selected from nitrogen and C(R5). When Q is nitrogen, each of A1and A1can be carbon. In some embodiments, Q = nitrogen and A1= A1= carbon. When Q is nitrogen or oxygen, the heterocyclic Lewis base of Formula (II) might not have any hydrogen atoms bound to the A1or A1atoms, which may be preferred because it is thought that hydrogens in those positions may undergo unwanted decomposition reactions that reduce the stability of the catalytically active species.

[0080] In at least one embodiment of Formula (II), Q is carbon and each of A1and A1' isN or C(R5), where R5is selected from hydrogen, C1-C20 hydrocarbyl. substituted C1-C20 hydrocarbyl, a heteroatom or a heteroatom-containing group. In such embodiments, the A'QA1fragment forms part of a cyclic carbene, N-heterocyclic carbene, cyclic amino alkyl carbene, or a substituted variant thereof.

[0081] The heterocyclic Lewis base (of Formula (II)) represented by A^A1combined with the curved line joining A1and A1can be selected from the following structures shown below, with each R25group selected from hydrogen, heteroatoms, C1-C20 alkyls, C1-C20 alkoxides, C1-C20 amides, and substituted C1-C20 alkyls.

[0082] In some embodiments, the heterocyclic Lewis base (of Formula (II)) represented by AxQArcombined with the curved line joining A1and A1is a six-membered ring containing zero, one, or 2 ring heteroatoms or a five-membered ring containing zero, one, two or three ring heteroatoms. Alternately, the heterocyclic Lewis base (of Formula (II)) represented by A^A1combined with the curved line joining A1and A1is not a sixmembered ring containing two or more ring heteroatoms.

[0083] In some embodiments of Formula (II), A^A1is part of a heterocyclic Lewis base containing 2 to 20 non-hydrogen atoms and links A2to A2via a 3-atom bridge with Q being the central atom of the 3-atom bridge. In some embodiments, each A1and A1' is a carbon atom and the AxQArfragment forms part of a pyridine, pyrazine, pyrimidine, triazine, thiazole, imidazole, thiophene, oxazole, thiazole, furan, or a substituted variant of thereof group, or a substituted variant thereof.

[0084] In some embodiments of Formula (II), M is Hf, Zr, Ti, Sc, Y, or La, Q is nitrogen, both A1and A1are carbon, both E and E are oxygen, and both R1and R1are independentlyC4-C20 cyclic tertiary alkyl.

[0085] In some embodiments of Formula (II), M is Hf, Zr, Ti, Sc, Y, or La, Q is nitrogen, both A1and A1are carbon, both E and E are oxygen, and both R1and R1are independently adamantan-l-yl or substituted adamantan-l-yl.

[0086] In some embodiments of Formula (II), M is Hf, Zr, Ti, Sc, Y, or La, Q is nitrogen, both A1and A1are carbon, both E and E are oxygen, and both R1and R1are independently acyclic tertiary alkyl.

[0087] In at least one embodiment, each L of the catalysts represented by Formula (II) can be independently selected from ethers, amines, phosphines, thioethers, esters, Et20, MeO'Bu, EtsN. PhNMe2, MePh2N, tetrahydrofuran, or dimethylsulfide. In at least one embodiment, m of the catalysts represented by Formula (II) is 0. In at least one embodiment, each X the catalysts represented by Formula (II) can be independently selected from methyl, benzyd, trimethylsilyl, neopentyl, ethyl, propyl, butyl, phenyl, hydrido, chloro, fluoro, bromo, iodo, trifluoromethanesulfonate, dimethyl ami do, diethylamido, dipropylamido, or diisopropylamido, such as chloro, such as methyl. In at least one embodiment, n of the catalysts represented by Formula (II) is 2.

[0088] In some embodiments, X is selected from methyl, or benzyl, n is 2, and m is zero.

[0089] In at least one embodiment, the catalyst compound is represented by Formula(HI)wherein:M is a Group 4. transition metal (such as Hf or Zr);each of E and E' is each independently O, S, or NRA, where RAis independently hydrogen, C1-C40 hydrocarbyl, substituted C1-C40 hydrocarbyl, or a heteroatom-containing group, such as both E and E' are O;each L is independently a Lewis base;each X’ is independently an anionic ligand;any two or more L groups may be joined together to form a poly dentate (e.g., bidentate) Lewis base;an X’ group may be joined to an L group to form a monoanionic bidentate group; n is 1, 2, or 3;m is 0, 1, or 2;n+m is 4 or less;each of R7, R8, R9, R10, R7, R8. R9. and R10' is independently hydrogen, C1-C40 hydrocarbyl, substituted C1-C40 hydrocarbyl, a heteroatom or a heteroatom-containing group, or one or more of R7and R8, R8and R9, R9and R10, R7and R8, R8and R9, R9and R10may be joined to form one or more substituted hydrocarbyl rings, unsubstituted hydrocarbyl rings, substituted heterocyclic rings, or unsubstituted heterocyclic rings each having 5, 6, 7, or 8 ring atoms, and where substitutions on the ring can join to form additional rings; and each of R11, R12, R13, R14, R11, R12, R13, R14, R15, R16, and R17is independently hydrogen, C1-C40 hydrocarbyl, substituted C1-C40 hydrocarbyl, a heteroatom or a heteroatomcontaining group, or one or more of R11and R12, R12and R13. R13and R14, R11and R12, R12and R13, R13and R14, R15and R16, or R16and R17may be joined to form one or more substituted hydrocarbyl rings, unsubstituted hydrocarbyl rings, substituted heterocyclic rings, or unsubstituted heterocyclic rings each having 5, 6, 7, or 8 ring atoms, and where substitutions on the ring can join to form additional rings.

[0090] In Formula (III), E and E’ are each independently selected from oxygen or NRA, where RAis independently hydrogen, C1-C40 hydrocarbyl, substituted C1-C40 hydrocarbyl, or a heteroatom-containing group. In some embodiments, E and E' are oxygen. When E and / or E’ are NRA, RAcan be selected from Ci to C20 hydrocarbyls, alkyls, or aryls. In one embodiment, E and E’ are each independently selected from O, S, N(alkyl), or N(aryl), where the alkyl can be a Ci to C20 alk l, such as methyl, ethyl, propyl, buty l, pentyd, hexyl, octyl, nonyl, decy l, undecyl, dodecyl, and the like, and aryl is a Ce to C40 aryl group, such as phenyl, naphthalenyl, benzyl, methylphenyl, and the like.

[0091] In some embodiments of catalyst compounds of Formula (II) or (HI), when E and E’ are oxygen, each phenolate group can be substituted in the position that is next to the oxygen atom (e.g., R1and R1in Formula (II) or R7and R7in Formula (III)). Thus, when E and E' are oxygen, each of either R1and R1of Formula (II) or R7and R7of Formula (III) is independently a C1-C40 hydrocarbyl, a substituted C1-C40 hydrocarbyl, a heteroatom, or a heteroatom-containing group, such as each of R1and R1is independently a non-aromatic cyclic alkyl group with one or more five- or six-membered rings (such as cyclohexy l, cyclooctyl, adamantyl, or 1 -methylcyclohexyl, or substituted adamantyl). such as anon-aromatic cyclic tertiary alkyl group (such as 1 -methylcyclohexyl, adamantyl. or substituted adamantyl).

[0092] In some embodiments of the catalyst compound of Formula (II) or (III), each of either R1and R1of Formula (II) or R7and R7of Formula (III) is independently a tertiary hydrocarbyl group. In other embodiments of Formula (II) or (III), each of either R1and R1of Formula (II) or R7and R7of Formula (III) is independently a (substituted or unsubstituted) cyclic tertiary hydrocarbyl group. In other embodiments of the catalyst compound of Formula (II) or (HI), each of either R1and R1of Formula (II) or R7and R7of Formula (III) is independently a (substituted or unsubstituted) polycyclic tertiary hydrocarbyl group.

[0093] In some embodiments of catalyst compounds of Formula (II) or (HD- when E and E’ are oxygen, each phenolate group can be substituted in the position that is para to the oxygen atom (e.g, each of either R3and R3of Formula (II) or R9and R9of Formula (III)).Thus, when E and E' are oxygen, each of either R3and R3of Formula (II) or R9and R9of Formula (III) is independently a C1-C40 hydrocarbyl, a substituted C1-C40 hydrocarbyl. a heteroatom, or a heteroatom-containing group, such as each of either R3and R3of Formula (II) or R9and R9of Formula (III) is independently C1-C20 alkyd, such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, or an isomer thereof. Alternatively, each of either R3and R3of Formula (II) or R9and R9of Formula (III) is independently a non-aromatic cyclic alkyl group with one or more five- or six-membered rings (such as cyclohexyl, cyclooctyl, adamantyl, or 1 -methylcyclohexyl, or substituted adamantyl), such as anon-aromatic cyclic tertiary alkyl group (such as 1 -methylcyclohexyl, adamantyl, or substituted adamantyl).

[0094] In some embodiments of the catalyst compound of Formula (II) or (III), each of either R3and R3of Formula (II) or R9and R9of Formula (III) is independently a (substituted or unsubstituted) C1-C20 alkyl, such as methyl, ethyl, propyl, butyl, pentyl, hexyl, hepty l, octyd, nonyl, decyl, or isomers thereof. In some embodiments of the catalyst compound of Formula (II) or (III), each of either R3and Ryof Formula (II) or R9and R9of Formula (III) is independently a (substituted or unsubstituted) acyclic tertiary hydrocarbyl group. In other embodiments of Formula (II) or (III), each of either R3and R3of Formula (II) or R9and R9of Formula (III) is independently a tert-butyl.

[0095] In some embodiments, one or more of R7, R8, R9, R10, R7, R8, R9, R10, R11, R12, R13, R14, R11, R12, R13; R14, R15, R16. or R17of Formula (III) are independently hydrogen or Ci to C20 alkyl, such as methyl, ethyl, propyl, buty l, pentyl, hexyl, heptyl, octyl, nonyl, decyl,undecyl, dodecyl, tridecyl, tetradecyl, pentadecyl, hexadecyl, heptadecyl, octadecyl, nonadecyl, eicosyl, or an isomer thereof, such as isopropyl, etc.

[0096] In some embodiments of Formula (II) and / or (III), M is Group 4 metal, such as Ti, Hf, or Zr.

[0097] In some embodiments of Formula (II) and / or (III), each of E and E' is O.

[0098] In some embodiments of Formula (II) and / or (III), each of either R1, R2, R3, R4, R1. R2. R3, and R4of Formula (II) or R7, R8, R9, R10. R7. R8, R9, and R10' of Formula (III) is independently selected from hydrogen, methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, undecyl, dodecyl, tridecyl, tetradecyl, pentadecyl, hexadecyl, heptadecyl, octadecyl, nonadecyl, eicosyl, heneicosyl, docosyl, tricosyl, tetracosyl, pentacosyl, hexacosyl, heptacosyl, octacosyl, nonacosyl, triacontyl, phenyl, substituted phenyl (such as methylphenyl and dimethylphenyl), benzyl, substituted benzyl (such as methylbenzyl), naphthalenyl, cyclohexyl, cyclohexenyl, methylcyclohexyl, and isomers thereof.

[0099] In embodiments of Formula (II) and / or (III), each X’ is, independently, selected from hydrocarbyl radicals having from 1 to 20 carbon atoms (such as alkyls or aryls), hydrides, amides, alkoxides, sulfides, phosphides, halides, alkyl sulfonates, and a combination thereof, such as each X’ is independently selected from halides, aryls, and Ci to Cs alkyl groups, such as each X’ is independently a hydrido, dimethylamido, di ethylamido, bis(dimethylsilyl)amido, bis(trimethylsilyl) amido, methylenetrimethylsilyl, neopentyl, phenyl, benzyl, methyl, ethyl, propyl, butyl, pentyl, fluoro, iodo, bromo, or chloro group. In some embodiments, each X’ is independently selected from bis(dimethylsilyl)amido, bis(trimethylsilyl) amido, and methylenetrimethylsilyl.

[0100] Alternatively, eachX’ may be, independently, a halide, a hydride, an alky l group, or an alkenyl group.

[0101] In some embodiments of Formula (II) and / or (III), each L is a Lewis base, independently, selected from ethers, thio-ethers, amines, nitriles, imines, pyridines, halocarbons, and phosphines, such as ethers, thioethers, or a combination thereof, optionally two or more L's may form a part of a fused ring or a ring system, such as each L is independently selected from ether or thioether groups, such as each L is an ethyl ether, tetrahydrofuran, dibutyl ether, or dimethylsulfide group.

[0102] In some embodiments of Formula (II) and / or (III), each of either R1and R1of Formula (I) or R7and R7of Formula (III) is independently cyclic tertiary alkyl groups.

[0103] In some embodiments of Formula (II) and / or (III), m is 0, 1 or 2, such as 0.

[0104] In some embodiments of Formula (II) and / or (III), each of either R1and R1ofFormula (I) or R7and R7of Formula (III) is not hydrogen.

[0105] In some embodiments of Formula (II) and / or (III), each of either R3and R3ofFormula (I) or R9and R9of Formula (III) is not hydrogen.

[0106] In some embodiments of Formula (II) and (III), M is Zr, Sc, Y, or La, each of E and E' is O; either R1and R1of Formula (II) or R7and R7of Formula (III) is independently a C1-C40 hydrocarbyl, a substituted C1-C40 hydrocarbyl. a heteroatom or a heteroatomcontaining group, and each of either R2, R \ R4, R2, R ’, and R4of Formula (II) or R8, R9, R10, R8, R9, and R10of Formula (III) is independently hydrogen, C1-C20 hydrocarbyl, or substituted C1-C20 hydrocarbyl.

[0107] In some embodiments of Formula (III), each of R11. R12, R13, R14. R11, R12, R13. R14, R15, R16, and R17is independently hydrogen, methyl, ethyl, propyl, butyl, pentyl, hexyl, or an isomer thereof.

[0108] In some embodiments of Formula (III), each of R11, R12, R13, R14, R11, R12, R13,R14, R15, R16, and R17is independently selected from hydrogen, methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, undecyl, dodecyl, tridecyl, tetradecyl, pentadecyl, hexadecyl, heptadecyl, octadecyl, nonadecyl, eicosyl, heneicosyl, docosyl, tricosyl, tetracosyl, pentacosyl, hexacosyl, heptacosyl, octacosyl, nonacosyl, triaconty l, phenyl, substituted phenyl (such as methylphenyl and dimethylphenyl), benzy l, substituted benzy l (such as methylbenzyl), naphthalenyl, cyclohexyl, cyclohexenyl, methylcyclohexyl, or isomers thereof.

[0109] In some embodiments of Formula (III), M is Hf or Zr, each of E and E' is O; each of R7and R7' is independently a C1-C40 hydrocarbyl, a substituted C1-C40 hydrocarbyl, a heteroatom or a heteroatom-containing group; each of R9and R9' is independently a C1-C40 hydrocarbyl, a substituted C1-C40 hydrocarbyl, a heteroatom or a heteroatom-containing group; each of R7, R8, R9, R7', R8, and R9' is independently hydrogen, C1-C20 hydrocarbyl, substituted C1-C20 hydrocarbyl, a heteroatom or a heteroatom-containing group, or one or more of R7and R8, R8and R9, R9and R10, R7and R8, R8and R9, R9and R10may be joined to form one or more substituted hydrocarbyl rings, unsubstituted hydrocarbyl rings, substituted heterocyclic rings, or unsubstituted heterocyclic rings each having 5, 6, 7, or 8 ring atoms, and where substitutions on the ring can join to form additional rings; each X’ is independently selected from substituted or unsubstituted: hydrocarbyl radicals having from 1 to 20 carbon atoms (such as alkyls or aryls), hydrides, amides, alkoxides, sulfides, phosphides, halides, dienes, amines, phosphines, ethers, and a combination thereof, (two ormore X’s may form a part of a fused ring or a ring system); n is 2; m is 0; and each of R11, R12, R13, R14. R11, R12, R13. R14, R15. R16, and R17is independently hydrogen, C1-C20 hydrocarbyl, substituted C1-C20 hydrocarbyl, a heteroatom or a heteroatom-containing group, or one or more adjacent R groups may be joined to form one or more substituted hydrocarbyl rings, unsubstituted hydrocarbyl rings, substituted heterocyclic rings, or unsubstituted heterocyclic rings each having 5, 6, 7, or 8 ring atoms, and where substitutions on the ring can join to form additional rings, such as each of R11, R12. R13, R14. R11, R12, R13, R14, R15, R16, and R17is independently selected from hydrogen, methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, undecyl, dodecyl, tridecyl, tetradecyl, pentadecyl, hexadecyl, heptadecyl, octadecyl, nonadecyl, eicosyl, heneicosyl, docosyl, tricosyl, tetracosyl, pentacosyl, hexacosyl, heptacosyl, octacosyl, nonacosyl, triacontyl, phenyl, substituted phenyl (such as methylphenyl and dimethylphenyl), benz l, substituted benz l (such as methylbenzyl), naphthyl, cyclohexyl, cyclohexenyl, methylcyclohexyl, and isomers thereof.

[0110] In some embodiments of Formula (III), M is Hf or Zr. both E and E are oxygen, both R7and R7are independently C4-C20 cyclic tertiary alkyl, and both R9and R9are independently C1-C10 alkyl.[OlH] In some embodiments of Formula (III), M is Hf or Zr, both E and E are oxygen, both R7and R7are adamantan-l-yl or substituted adamantan-l-yl, and both R9and R9are independently C1-C10 alkyl.

[0112] In some embodiments of Formula (III), M is Hf or Zr, both E and E are oxygen, and each of R7, R7, R9and R9are independently adamantan-l-yl or substituted adamantan-l-yl.

[0113] In at least one embodiment of the present disclosure, the catalyst systems include the product of the combination of one or more support materials. In some embodiments, a support material is a porous support material, for example, talc, and inorganic oxides. Other support materials include zeolites, clays, organoclays, or any other organic or inorganic support material, or mixtures thereof. As used herein, "support" and “support material” are used interchangeably.

[0114] The terms “cocatalyst” and “activator” are used herein interchangeably.

[0115] As previously discussed, catalyst systems described herein can typically include a catalyst complex as described above and an activator such as alumoxane or a noncoordinating anion and may be formed by combining the catalyst components described herein with activators in any manner known from the literature including combining themwith supports, such as silica. The catalyst systems may also be added to or generated in solution polymerization or bulk polymerization (in the monomer). Catalyst systems of the present disclosure may have one or more activators and one, two or more catalyst components. Activators are defined to be any compound which can activate any one of the catalyst compounds described above by converting the neutral metal compound to a catalytically active metal compound cation. Non-limiting activators, for example, include alumoxanes, aluminum alkyls, ionizing activators, which may be neutral or ionic, and conventional-type cocatalysts. Suitable activators typically include alumoxane compounds, modified alumoxane compounds, and ionizing anion precursor compounds that abstract a reactive, o-bound, metal ligand making the metal compound cationic and providing a chargebalancing noncoordinating or weakly coordinating anion, e.g., a non-coordinating anion.

[0116] In at least one embodiment, a catalyst system includes one or more catalyst compounds represented by Formula (II) and / or (III) as described above, and an activator compound. Activator compounds can include, but are not limited to, an alumoxane catalyst, an ionizing / non-coordinating anion activator, and combinations thereof.

[0117] Alumoxane activators can be utilized as activators in the catalyst systems described herein. Alumoxanes are generally oligomeric compounds containing -Al(R')O- sub-units, where R1is an alkyl group. Examples of alumoxanes include methylalumoxane (MAO), modified methylalumoxane (MMAO), ethylalumoxane and isobutylalumoxane. Alkylalumoxanes and modified alkylalumoxanes are suitable as catalyst activators, particularly when the abstractable ligand is an alkyl, halide, alkoxide or amide. Mixtures of different alumoxanes and modified alumoxanes may also be used. A visually clear methylalumoxane can be used. A cloudy or gelled alumoxane can be filtered to produce a clear solution or clear alumoxane can be decanted from the cloudy solution. A useful alumoxane is a modified methyl alumoxane (MMAO) cocatalyst type 3 A (commercially available from Akzo Chemicals, Inc. under the trade name Modified Methylalumoxane type 3 A. covered under patent number U. S. Patent No. 5,041,584). Another useful alumoxane is solid polymethylalumoxane as described in US 9,340,630; US 8,404,880; and US 8,975,209.

[0118] When the activator is an alumoxane (modified or unmodified), at least one embodiment selects the maximum amount of activator typically at up to about a 5,000-fold molar excess Al / M over the catalyst compound (per metal catalytic site). The minimum activator-to-catalyst-compound is about a 1: 1 molar ratio. Alternative suitable ranges include a molar ratio from about 1: 1 to about 500: 1, alternatively from 1: 1 to 200: 1, alternativelyfrom about 1:1 to about 100:1, or alternatively from about 1:1 to about 50:1. In an alternative embodiment, little or no alumoxane is used in the polymerization processes described herein. For example, alumoxane is present at about zero mole %, alternatively the alumoxane is present at a molar ratio of aluminum to catalyst compound transition metal less than or about 500: 1, such as less than or about 300: 1, such as less than or about 100: 1, such as less than or about 1:1.

[0119] The term "non-coordinating anion" (NCA) means an anion which either does not coordinate to a cation or which is only weakly coordinated to a cation thereby remaining sufficiently labile to be displaced by a Lewis base. " Compatible" non-coordinating anions are those which are not degraded to neutrality when the initially formed complex decomposes. Further, the anion will not transfer an anionic substituent or fragment to the cation so as to cause it to form a neutral transition metal compound and a neutral byproduct from the anion. Non-coordinating anions useful in accordance with the present disclosure are those that are compatible, stabilize the transition metal cation in the sense of balancing its ionic charge at +1, and yet retain sufficient labi li ty to permit displacement during polymerization. Ionizing activators useful herein typically comprise an NCA, particularly a compatible NCA.

[0120] In some embodiments, the activator is an ionizing activator, neutral or ionic. In some embodiments of the present disclosure, neutral or ionic activators can be used alone or in combination with alumoxane or modified alumoxane activators.

[0121] In some embodiments, the catalyst systems of the present disclosure can include at least one non-coordinating anion (NCA) activator. In at least one embodiment, boron containing NCA activators can be used, wherein the boron containing NCA activator is represented by the formula:(ZW-)wherein: Z is (L-H) or a reducible Lewis acid; L is a Lewis base; H is hydrogen; (L-H) is a Bronsted acid; Ad-is a boron containing non-coordinating anion having the charge d-; d is 1, 2, or 3.

[0122] The cation component, Zd + may include Bronsted acids such as protons or protonated Lewis bases or reducible Lewis acids capable of protonating or abstracting a moiety, such as an alkyl or aryl, from the bulky ligand transition metal catalyst precursor, resulting in a cationic transition metal species.

[0123] The activating cation Zd + may also be a moiety such as silver, tropylium, carbeniums, ferroceniums and mixtures, such as carbeniums and ferroceniums. Zd+can be triphenyl carbenium. Reducible Lewis acids can be a triaryl carbenium (where the aryl can be substituted or unsubstituted, such as those represented by the formula: (ArsC+), where Ar is ary l or ary l substituted with a heteroatom, a Ci to C40 hydrocarbyl, or a substituted Ci to C40 hydrocarbyl), such as the reducible Lewis acids " Z" may include those represented by the formula: (Ph;, C). where Ph is a substituted or unsubstituted phenyl, such as substituted with Ci to C40 hydrocarbyls or substituted a Ci to C40 hydrocarbyls, such as Ci to C20 alky ls or aromatics or substituted Ci to C20 alkyls or aromatics, such as Z is a triphenylcarbenium. When Za+ is the activating cation (L-H)d+, it can be a Bronsted acid, capable of donating a proton to the transition metal catalytic precursor resulting in a transition metal cation, including ammoniums, oxoniums, phosphoniums, silyliums, and mixtures thereof, such as ammoniums of methylamine, aniline, dimethylamine, diethylamine, N-methylaniline, diphenylamine, trimethylamine, triethylamine, N, N-dimethylaniline, methyldiphenylamine, pyridine, p-bromo N, N-dimethylaniline, p-nitro-N, N-dimethylaniline, dioctadecylmethylamine, phosphoniums from triethylphosphine, triphenylphosphine, and diphenylphosphine, oxoniums from ethers such as dimethyl ether diethyl ether, tetrahydrofuran and dioxane, sulfoniums from thioethers, such as diethyl thioethers, tetrahydrothiophene, and mixtures thereof.

[0124] The anion component Ad-includes those having the formula [Mk+Qn]d-where k is 1, 2, or 3; n is 1, 2, 3, 4, 5, or 6 (such as 1, 2, 3, or 4); n-k=d; M is an element selected from Group 13 of the Periodic Table of the Elements, such as boron or aluminum, and Q is independently a hydride, bridged or unbridged dialkylamido, halide, alkoxide, aryloxide, hydrocarbyl, substituted hydrocarbyl, halocarbyl, substituted halocarbyl, and halosubstituted-hydrocarbyl radicals, said Q having up to 20 carbon atoms with the proviso that in not more than 1 occurrence is Q a halide. Each Q can be a fluorinated hydrocarbyl group having 1 to 20 carbon atoms, such as each Q is a fluorinated ary l group, and such as each Q is a pentafluoryl ary l group. Examples of suitable Ad-also include diboron compounds as disclosed in U. S. Pat. No. 5,447.895, which is fully incorporated herein by reference.

[0125] Illustrative, but not limiting, examples of boron compounds which may be used as an activating cocatalyst are the compounds described as (and particularly those specifically listed as) activators in U. S. Pat. No. 8,658,556, which is incorporated by reference herein.

[0126] The ionic stoichiometric activator Zd+(Ad-) can be one or more ofN, N-dimethylanilinium tetrakis(perfluorophenyl) borate, N, N-dimethylaniliniumtetrakis(perfluoronaphthyl) borate, dioctadecylmethylammonium tetrakis(perfluorophenyl)borate, N, N-dimethylanilinium tetrakis(perfluorobiphenyl)borate. N, N-dimethylanilinium tetrakis(3,5-bis(trifluoromethyl)phenyl)borate, triphenylcarbenium tetrakis(perfluoronaphthyl)borate, triphenylcarbenium tetrakis(perfluorobiphenyl)borate, triphenylcarbenium tetrakis(3,5-bis(trifluoromethyl)phenyl)borate, or triphenylcarbenium tetra(perfluorophenyl)borate.

[0127] Alternately, the activator compounds are represented by Formula (IV):[R41R42R43EH] / [M*+Qn]<y’ (IV) wherein:E is nitrogen or phosphorous, preferably nitrogen;d is 1, 2 or 3 (preferably 3); k is 1, 2, or 3 (preferably 3); n is 1, 2, 3, 4, 5, or 6 (preferably 4, 5, or 6); n-k=d (preferably dis 1, 2 or 3; k is 3; n is 4, 5, or 6, preferably when M is B, n is 4);each of R41, R42, and R43is independently H, optionally substituted C1-C40 alkyl (such as branched or linear alkyl), or optionally substituted C5-C50 ary l (alternately each of R41, R42, and R43is independently unsubstituted or substituted with at least one of halide, C5-C50 ary l, C6-C35 arylalkyl, C6-C35 alky lary l and, in the case of the C5-C50 aryl, C1-C50 alkyl);wherein R41, R42, and R43together comprise 15 or more carbon atoms (such as 18 or more carbon atoms, such as 20 or more carbon atoms, such as 22 or more carbon atoms, such as 25 or more carbon atoms, such as 30 or more carbon atoms, such as 35 or more carbon atoms, such as 37 or more carbon atoms, such as 40 or more carbon atoms, such as 45 or more carbon atoms), preferably at least one of R41, R42, and R43is a C3 to C40 hydrocarbyl, (such as a C3-C40 alkyl, alternately such as a C7-C40 alkyl);M is an element selected from group 13 of the Periodic Table of the Elements, such as B or Al, andeach Q is independently a hydride, bridged or unbridged dialkylamido, halide, alkoxide, aryloxide, hydrocarbyl, substituted hydrocarbyl, halocarbyl, substituted halocarbyl, or halosubstituted-hydrocarbyl radical, such as a fluorinated aryl group, such as a fluorophenyl or fluoro-naphthyl, such as perfluorophenyl or perfluoronaphthyl.

[0128] In some embodiments of Formula (IV), each of R41, R42, and R43are independently selected from a substituted linear alkyl, a substituted branched alkyl, a substituted arylalkyl, a substituted silyl group, a substituted alkoxy group, a halogen, a halogen containing group, and combinations thereof.

[0129] In some embodiments, substituted linear alky ls can include, but a not limited to methyl, ethyl, n-propyl, n-butyl, n-pentyl, n-hexyl, n-heptyl, n-octyl, n-nonyl, n-decyl, n-undecyl, n-dodecyl, n-tridecyl, n-tetradecyl, n-pentadecyl, n-hexadecyl, n-heptadecyl, n-octadecyl, n-nonadecyl, n-icosyl, n-henicosyl, n-docosyl, n-tricosyl, n-tetracosyl, n-pentacosyl, n-hexacosyl, n-heptacosyl, n-octacosyl, n-nonacosyl, n-triacontyl. and any isomer thereof.

[0130] In some embodiments, a substituted branched alkyl can include, but is not limited to, alkylbutyl, alkyl-pentyl, alkyl-hexyl, alkyl-heptyl, alkyl-octyl, alkyl-nonyl, alkyl-decyl, alkyl-undecyl, alkyl-dodecyl, alkyl-tridecyl, alkyl-tetradecyl, alkyl-pentadecyl, alkyl-hexadecyl, alkyl-heptadecyl, alkyloctadecyl, alkyl-nonadecyL alkyl-eicosyl, and isomers thereof. In some embodiments, the substituted branched alkyl is a multi-alkyl analog, such as dialkyl-butyl, dialkyl-pentyl, dialkyl-hexyl, dialkyl-heptyl, dialkyl-octyl, dialkylnonyl, dialkyl-decyl, dialkyl-undecyl, dialkyl-dodecyl, dialkyl-tridecyl, dialkyl-butadecyl, dialkylpentadecyl, dialkyl-hexadecyl, dialkyl-heptadecyl, dialky 1-octadecyl, dialkyl-nonadecyl, dialkyl-icosyl, trialkyl-butyl, trialkyl-penty 1, trialkyl-hexyl, trialkyl-heptyl, trialkyloctyl, trialkyl -nonyl, trialkyl-decyl, trialkyl-undecyl, trialkyl-dodecyl, trialkyl-tridecyl. trialkyl-butadecyl, trialkyl-pentadecyl, trialkyl-hexadecyl, trialky 1 -heptadecyl, trialkyl-octadecyl, trialkyl -nonadecyl, trialkyl-icosyl, and isomers thereof. In some embodiments, substituted branched alkyl is independently a Ci to C40 linear, branched or cyclic alkyl group, such as C2 to C30 linear, branched or cyclic alkyd group, such as C3 to C20 linear, branched or cyclic alkyd group. In some embodiments, the alkyl group of the substituted branched alkyl is methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octy l, nonyl, decyl, undecyl, dodecyl, tridecyl, tetradecyl, pentadecyl, hexadecyl, heptadecyl, octadecyl, nonadecyl, icosyl, henicosyl, docosyl, tricosyl, tetracosyl, pentacosyl, hexacosyl, heptacosyl, octacosyl, nonacosyl, tricontyl, and isomers thereof.

[0131] In some embodiments, a substituted arylalkyl include methylphenyl, ethylphenyl, propylphenyl, butylphenyl, pentylphenyl, hexylphenyl, heptylphenyl, octylphenyl, nonylphenyl, decylpheny 1, undecylpheny 1, dodecylphenyl, tridecylphenyl, tetradecylphenyl, pentadecylphenyl, hexadecylphenyl. heptadecylphenyl, octadecylphenyl, nonadecylphenyl, icosylphenyl, henicosylphenyl, docosylphenyl, tricosylphenyl, tetracosylphenyl, pentacosylphenyl, hexacosylphenyl, heptacosylphenyl, octacosylphenyl, nonacosylphenyl, triacontylphenyl, (3,5,5-trimethylhexyl)phenyl, dioctylphenyl, (3,3,5-trimethylhexyl)phenyl, (2, 2, 3, 3, 4 pentamethylpentyl)phenyl, and isomers thereof.

[0132] In some embodiments, a substituted silyl group include a trialkylsilyl group, wherein each alkyl is independently a substituted Ci to C20 alkyl, such as trimethylsilyl, triethylsilyl, tripropylsilyl, tributylsilyl, trihexylsilyl, triheptylsilyl, trioctylsilyl, trinonylsilyl, tridecylsilyl, triundecylsilyl, tridodecylsilyl, tri-tridecylsilyl, tri-tetradecylsilyl,tri-pentadecylsilyl, trihexadecylsilyl, tri-heptadecylsilyl, tri-octadecylsilyl, tri-nonadecylsilyl, tri-icosylsilyl, and isomers thereof.

[0133] In some embodiments, a substituted alkoxy group can be represented by the Formula -OR*, where R* includes a substituted Ci to C20 alkyl or aryl group, such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, undecyl, dodecyl, tridecyl, tetradecyl, pentadecyl, hexadecyl, heptadecyl, octadecyl, nonadecyl, icosyl, phenyl, naphthyl, anthracenyl, and combinations thereof. In some embodiments, R* can include an alkylphenyl group, such as methyl phenyl, propyl phenyl, and isomers thereof.

[0134] In some embodiments, a halogen includes Br and Cl. In some embodiments, a halogen containing group includes bromomethyl and bromophenyl.

[0135] In some embodiments, the NCA can include one or more of:N, N-di(hydrogenated tallow)methylammonium [tetrakis(perfluorophenyl)borate],N-methyl-4-nonadecyl-N-octadecylanilinium [tetrakis(perfluorophenyl)borate],N-methyl-4-hexadecyl-N-octadecylanilinium [tetrakis(perfluorophenyl)borate],N-methyl-4-tetradecyl-N-octadecylanilinium [tetrakis(perfluorophenyl)borate].N-methyl-4-dodecyl-N-octadecylanilinium [tetrakis(perfluorophenyl)borate].N-methyl-4-decyl-N-octadecylanilinium [tetrakis(perfluorophenyl)borate],N-methyl-4-octyl-N-octadecylanilinium [tetrakis(perfluorophenyl)borate],N-methyl-4-hexyl-N-octadecylanilinium [tetrakis(perfluorophenyl)borate],N-methyl-4-butyl-N-octadecylanilinium [tetrakis(perfluorophenyl)borate],N-methyl-4-octadecyl-N-decylanilinium [tetrakis(perfluorophenyl)borate],N-methyl-4-nonadecyl-N-dodecylanilinium [tetrakis(perfluorophenyl)borate],N-methyl-4-nonadecyl-N-tetradecylanilinium [tetrakis(perfluorophenyl)borate],N-methyl-4-nonadecyl-N-hexadecylanilinium [tetrakis(perfluorophenyl)borate],N-ethyl-4-nonadecyl-N-octadecylanilinium [tetrakis(perfluorophenyl)borate],N-methyl-N, N-dioctadecylammonium [tetrakis(perfluorophenyl)borate],N-methyl-N, N-dihexadecylammonium [tetrakis(perfluorophenyl)borate],N-methyl-N, N-ditetradecylammonium [tetrakis(perfluorophenyl)borate],N-methyl-N, N-didodecylammonium [tetrakis(perfluorophenyl)borate],N-methyl-N, N-didecylammonium [tetrakis(perfluorophenyl)borate],N-methyl-N. N-dioctylammonium [tetrakis(perfluorophenyl)borate],N-ethyl-N, N-dioctadecylammonium [tetrakis(perfluorophenyl)borate],N, N-di(octadecyl)tolylammonium [tetrakis(perfluorophenyl)borate],N, N-di(hexadecyl)tolylammonium [tetrakis(perfluorophenyl)borate],N, N-di(tetradecyl)tolylammonium [tetrakis(perfluorophenyl)borate],N, N-di(dodecyl)tolylammonium [tetrakis(perfluorophenyl)borate],N-octadecyl-N-hexadecyl-tolylammonium [tetrakis(perfluorophenyl)borate].N-octadecyl-N-hexadecyl-tolylammonium [tetrakis(perfluorophenyl)borate],N-octadecyl-N-tetradecyl-tolylammonium [tetrakis(perfluorophenyl)borate],N-octadecyl-N-dodecyl-tolylammonium [tetrakis(perfluorophenyl)borate],N-octadecyl-N-decyl-tolylammonium [tetrakis(perfluorophenyl)borate],N-hexadecyl-N-tetradecyl-tolylammonium [tetrakis(perfluorophenyl)borate],N-hexadecyl-N-dodecyl-tolylammonium [tetrakis(perfluorophenyl)borate],N-hexadecyl-N-decyl-tolylammonium [tetrakis(perfluorophenyl)borate],N-tetradecyl-N-dodecyl-tolylammonium [tetrakis(perfluorophenyl)borate],N-tetradecyl-N-decyl-tolylammonium [tetrakis(perfluorophenyl)borate],N-dodecyl-N-decyl-tolylammonium [tetrakis(perfluorophenyl)borate],N-methyl-N-octadecylanilinium [tetrakis(perfluorophenyl)borate],N-methyl-N-hexadecylanilinium [tetrakis(perfluorophenyl)borate],N-methyl-N-tetradecylanilinium [tetrakis(perfluorophenyl)borate],N-methyl-N-dodecylanilinium [tetrakis(perfluorophenyl)borate],N-methyl-N-decylanilinium [tetrakis(perfluorophenyl)borate], andN-methyl-N-octylanilinium [tetrakis(perfluorophenyl)borate].

[0136] In at least one embodiment, the activator is selected from one or more of dimethylanilinium tetrakis(pentafluorophenyl)borate, dimethylanilinium tetrakis(heptafluoro-2-naphthalenyl)borate, N, N-di(hydrogenated tallow)methylammonium tetrakis(perfluorophenyl)borate, N, N-di (hydrogenated tallow)methylammonium tetrakis(heptafluoro-2-naphthalenyl)borate, N-methyl-4-nonadecyl-N-octadecylanilinium tetrakis(perfluorophenyl)borate, N-methyl-4-nonadecyl-N-octadecylanilinium tetrakis(heptafluoro-2-naphthalenyl)borate, N-methyl-N, N-dioctadecylammonium tetrakis(perfluorophenyl)borate, N-methyl-N, N-dioctadecylammonium tetrakis(heptafluoro-2-naphthalenyl)borate, N-methyl-N, N-dihexadecylammonium tetrakis(perfluorophenyl)borate, N-methyl-N, N-dihexadecylammonium tetrakis(heptafluoro-2-naphthalenyl)borate, N-methyl-N-octadecyl-4-(octadecyloxy)aniliniumtetrakis(perfluorophenyl)borate, and N-methyl-N-octadecyl-4-(octadecyloxy)anilinium tetrakis(heptafluoro-2-naphthalenyl)borate.

[0137] In some embodiments, the activator is selected from one or more of a triaryl carbenium compounds including triphenylcarbenium tetraphenylborate, triphenylcarbenium tetrakis(pentafluorophenyl)borate, triphenylcarbenium tetrakis-(2, 3, 4, 6-tetrafluorophenyl)borate. triphenylcarbenium tetrakis(perfluoronaphthyl)borate, triphenylcarbenium tetrakis(perfluorobiphenyl)borate, triphenylcarbenium tetrakis(3,5-bis(trifluoromethyl)phenyl)borate.

[0138] In another embodiment, the activator is selected from one or more of trialkylammonium tetrakis(pentafluorophenyl)borate, N, N-dialkylanilinium tetrakis(pentafluorophenyl)borate, dioctadecylmethylammonium tetrakis(perfluoronaphthyl)borate, N, N-dimethyl-(2,4,6-trimethylanilinium) tetrakis(pentafluorophenyl)borate, trialkylammonium tetrakis-(2, 3,4,6-tetrafluorophenyl)borate, N, N-dialkylanilinium tetrakis-(2,3,4,6-tetrafluorophenyl)borate, trialkylammonium tetrakis(perfluoronaphthyl)borate, N, N-dialkylanilinium tetrakis(perfluoronaphthyl) borate, trialkylammonium tetrakis(perfluorobiphenyl)borate, N, N-dialkylanilinium tetrakis(perfluorobiphenyl)borate, trialkylammonium tetrakis(3,5-bis(trifluoromethyl)phenyl)borate, N, N-dialkylanilinium tetrakis(3,5-bis(trifluoromethyl)phenyl)borate, N, N-dialkyl-(2,4,6-trimethylanilinium) tetrakis(3,5-bis(trifluoromethyl)phenyl)borate. di-(i-propyl)ammonium tetrakis(pentafluorophenyl)borate, N-methyl-4-nonadecyl-Noctadecylanilinium tetrakis(perfluoronaphthalen-2-yl)borate, N-methyl-4-nonadecyl-N-octadecylanilinium tetrakis(perfluorophenyl)borate.

[0139] Suitable activator-to-catalyst ratio for catalyst systems having NCA activators, an activator-to-catalyst ratio may be about a 1: 1 molar ratio. In some embodiments, the activator-to-catalyst ratio ranges from about 0.1: 1 to about 100: 1, such as from about 0.5:1 to about 200: 1, such as from about 1: 1 to about 500: 1, such as about 1: 1 to about 1000: 1. In some embodiments, the activator-to-catalyst ratio is from about 0.5: 1 to about 10:1, such as about 1: 1 to about 5:1.

[0140] In some embodiments, any one or more catalyst compounds, one or more alumoxanes, one or more NCA, and one or more activators may be combined in any amount or ratio to form a catalyst system to produce a desired result, such as, but not limited to, a polymer having a desired architecture, molecular weight, physical properties, thermal properties, and combinations thereof.

[0141] In addition to the activators, scavengers, chain transfer agents or co-activators may be used. Aluminum alkyl or organoaluminum compounds which may be utilized as co-activators include, for example, trimethylaluminum, triethylaluminum, triisobutylaluminum, tri-n-hexylaluminum, tri-n-octylaluminum, diethyl zinc,tri-n-butylaluminum, diisobutylaluminum hydride, or combinations thereof.

[0142] In at least one embodiment, the catalyst systems can additionally comprise one or more scavenging compounds. Here, the term “scavenger’7means a compound that removes polar impurities from the reaction environment. These impurities adversely affect catalyst activity and stability. For example, the scavenging compound will be an organometallic compound such as the Group-13 organometallic compounds of U. S. Pat. Nos. 5,153,157; 5,241,025; and WO 1991 / 009882; WO 1994 / 003506; WO 1993 / 014132; and that of WO 1995 / 007941. Exemplary' compounds include triethyl aluminum, triethyl borane, tri-iso-butyl aluminum, methyl alumoxane, iso-butyl alumoxane, and tri-n-octyl aluminum. Those scavenging compounds having bulky or C6-C20 linear hydrocarbyl substituents connected to the metal or metalloid center usually minimize adverse interaction with the active catalyst. Examples include triethyl aluminum, and bulky compounds such as tri-iso-butyl aluminum, tri-iso-prenyl aluminum, and long-chain linear alkyl-substituted aluminum compounds, such as tri-n-hexyl aluminum, tri-n-octyl aluminum, or tri-n-dodecyl aluminum. When alumoxane is used as the activator, any excess over that needed for activation will scavenge impurities and additional scavenging compounds may be unnecessary’.Alumoxanes also may be added in scavenging quantities with other activators, e.g., [Me2HNPh]+[B(pfp)4]‘ or B(pfp)4(perfluorophenyl = pfp = CeFs).

[0143] Exemplary aluminum scavengers can include those where there is oxygen present. That is, the material per se or the aluminum mixture used as a scavenger, includes an aluminum / oxygen species, such as an alumoxane or alkylaluminum oxides, e.g., dialkyaluminum oxides, such as bis(diisobuty laluminum) oxide. In at least one aspect, aluminum containing scavengers can be represented by the formula ((Rz-Al-)yO-)x. wherein z is 1-2, y is 1-2, x is 1-100, and R is a C1-C12 hydrocarbyl group. In another aspect, the scavenger has an oxygen to aluminum (O / Al) molar ratio of from about 0.25 to about 1.5, more particularly from about 0.5 to about 1. Aluminum alkyl or organoaluminum compounds which may be utilized as scavengers or co-activators include, for example, trimethyl aluminum, triethylaluminum, triisobutylaluminum, tri-n-hexylaluminum, tri-n-octylaluminum, and diethyl zinc.

[0144] Chain transfer agents may be used in the compositions and / or processes described herein. Useful chain transfer agents are typically alkylalumoxanes. a compound represented by the formula AlR3, ZnR2(where each R is, independently, a C1-C8aliphatic radical, such as methyl, ethyl, propyl, butyl, pentyl, hexyl, octyl or an isomer thereof) or a combination thereof, such as diethyl zinc, methylalumoxane, trimethylaluminum, triisobutylaluminum, trioctylaluminum, or a combination thereof.

[0145] In some embodiments, the monomer input includes a solvent and / or diluent. Suitable diluents / solvents include non-coordinating, inert liquids. In at least one embodiment, a solvent / diluent includes straight and branched-chain hydrocarbons, such as isobutane, butane, pentane, isopentane, hexanes, isohexane, heptane, octane, dodecane, and mixtures thereof; cyclic and alicyclic hydrocarbons, such as cyclohexane, cycloheptane, methylcyclohexane, methylcycloheptane, and mixtures thereof, such as can be found commercially (Isopar™); perhalogenated hydrocarbons, such as perfluorinated C4-10 alkanes, chlorobenzene, and aromatic and alkylsubstituted aromatic compounds, such as benzene, toluene, mesitylene, and xylene. Suitable solvents also include liquid olefins which may act as monomers or comonomers including ethylene, propylene, 1 -butene, 1 -hexene, 1 -pentene, 3-methyl- 1 -pentene, 4-methyl-l -pentene, 1-octene, 1 -decene, and mixtures thereof. In some embodiments, aliphatic hydrocarbon solvents are used as the solvent, such as isobutane, butane, pentane, isopentane, hexanes, isohexane, heptane, octane, dodecane, and mixtures thereof; cyclic and alicyclic hydrocarbons, such as cyclohexane, cycloheptane, methylcyclohexane, methylcycloheptane, and mixtures thereof. In another embodiment, the solvent is not aromatic, preferably aromatics are present in the solvent at less than 1 wt%, such as less than 0.5 wt%, such as less than 0 wt% based upon the weight of the solvents.

[0146] In some embodiments, the catalyst system is introduced to the reaction zone at a rate of about 5.0 (μg / volume of reactor) / min (otherwise referred to as “ug / volume / min”). To obtain the actual catalyst flow rate, the “ug / volume / min” value is multiplied by the volume of the reactor or volume of the reaction zone in units of Liters. For example, if the catalyst flow rate was 20.0 μg / volume / min and the volume of the reactor was 0.5 L, then the actual flow rate of the catalyst into the reactor would be 10.0 μg / min (1 g = 1,000,000 μg). In at least one embodiment, the catalyst system is introduced to the reaction zone at a rate of about 5.0 μg / volume / min to about 1,000 μg / volume / min, such as about 10 μg / volume / min to about 500 μg / volume / min, such as about 20 μg / volume / min to about 400 μg / volume / min, alternatively about 30 μg / volume / min to about 200 μg / volume / min, alternatively about40 μg / volume / min to about 100 μg / volume / min, alternatively about 50 μg / volume / min to about 90 μg / volume / min, alternatively about 60 μg / volume / min to about 80 μg / volume / min.

[0147] At operation 106 of the method 100, the reaction mixture is polymerized such that the monomeric components of the monomer input react to form a polymer mixture.Generally, the polymerization process is conducted through contacting the monomer input with the catalyst system, as described above. Each of the components of the monomer input and catalyst system may be combined in any suitable order, sequence, or processes known to one of ordinary skill in the art. In at least one embodiment, the catalyst system is fully prepared prior to contacting with the monomer input.

[0148] Polymerization processes of the present disclosure can be carried out in any suitable manner. Any suitable suspension, homogeneous, bulk, solution, slurry, or gas phase polymerization process can be used. Such processes can be run in a batch, semi-batch, or continuous mode. Homogeneous polymerization processes and slurry processes can be used. A bulk homogeneous process can be used. Alternately, no solvent or diluent is present or added in the reaction medium, (except for the small amounts used as the carrier for the catalyst system or other additives, or amounts found with the monomer; e.g., propane in propylene). In another embodiment, the process is a slurry process. As used herein, the term ’’slurry polymerization process” means a polymerization process where a supported catalyst is employed and monomers are polymerized on the supported catalyst particles. At least 95 wt% of polymer products derived from the supported catalyst are in granular form as solid particles (not dissolved in the diluent).

[0149] The polymerization process can be run at any temperature and / or pressure suitable to obtain the desired polymers. Suitable temperatures and / or pressures include a temperature of about 0°C to about 300°C, such as about 20°C to about 200°C. such as about 35°C to about 160°C, such as about 80°C to about 160°C, such as about 85°C to about 140°C.Polymerizations can be run at a pressure of about 0.1 MPa to about 25 MPa, such as about 0.45 MPa to about 6 MPa, or about 0.5 MPa to about 4 MPa.

[0150] In some embodiments, the run time of the polymerization reaction can be up to about 1,500 minutes, such as about 1,200 minutes, such as about 300 minutes, such as about 5 minutes to about 250 minutes, such as about 10 minutes to about 120 minutes, such as about 20 minutes to about 90 minutes, such as about 30 minutes to about 60 minutes. In a continuous process, the run time may be the average residence time of the reaction components within the reactor and / or reaction zone. In at least one embodiment, the run time of the reaction is up to about 180 minutes.

[0151] In some embodiments, an inert gas may be introduced to the polymerization reaction zone during the polymerization. Inert gas(es) can include nitrogen, hydrogen, or a combination thereof. In at least one embodiment, hydrogen is present in the polymerization reaction zone at a partial pressure of about 0.001 psig to about 50 psig (0.007 kPa to 345 kPa), such as about 0.01 psig to about 25 psig (0.07 kPa to 172 kPa), such as about 0.1 psig to about 10 psig (0.7 kPa to 70 kPa). In at least one embodiment, the hydrogen content is about 0.0001 ppm to about 2,000 ppm. such as about 0.0001 ppm to about 1,500 ppm, such as about 0.0001 ppm to about 1,000 ppm, such as about 0.0001 ppm to about 500 ppm.Alternately, hydrogen can be present at zero ppm.

[0152] A "polymerization reaction zone" also referred to as a "polymerization zone" is a vessel where polymerization takes place, for example a stirred-tank reactor or a loop reactor. When multiple reactors are used in a continuous polymerization process, each reactor is considered as a separate reaction zone. For a multi-stage polymerization in a batch polymerization process, each polymerization stage is considered as a separate polymerization zone. In at least one embodiment, the polymerization occurs in one reaction zone. Room temperature is 23°C unless otherwise noted.

[0153] Other additives may also be used in the polymerization, as desired, such as one or more scavengers, hydrogen, aluminum alkyls, or chain transfer agents such as alkylalumoxanes, a compound represented by the formula AlR3or ZnR2 (where each R is, independently, a C1-C8aliphatic radical, such as methyl, ethyl, propyl, butyl, pentyl, hexyl octyl or an isomer thereof) or a combination thereof, such as diethyl zinc, methylalumoxane, trimethylaluminum, triisobutylaluminum, trioctylaluminum, or a combination thereof.

[0154] In some embodiments, the polymerization process is a solution phase polymerization process. A solution polymerization is a polymerization process in which the polymer is dissolved in a liquid polymerization medium, such as an inert solvent or monomer(s) or their blends. A solution polymerization is typically homogeneous. A homogeneous polymerization is one where the polymer product is dissolved in the polymerization medium. Such systems are not turbid as described in Oliveira, J. V. et al. (2000) Ind. Eng. Chem. Res. v.39, pg. 4627. Solution polymerization may involve polymerization in a continuous reactor in which the polymer formed, the monomer input and catalyst system materials supplied are agitated to reduce or avoid concentration gradients and in which the monomer acts as a diluent or solvent or in which a hydrocarbon is used as a diluent or solvent. Suitable processes can operate at temperatures from about 0°C to about 250°C, such as from about 50°C to about 170°C, such as from about 80°C to about 150°C,and / or at pressures of about 0.1 MPa or more, such as 0.5 MPa or more. The upper pressure limit is not critically constrained but can be about 200 MPa or less, such as 120 MPa or less, such as 30 MPa or less. Temperature control in the reaction zone can be obtained by balancing the heat of polymerization and with reactor cooling by reactor jackets or cooling coils to cool the contents of the reaction zone, auto refrigeration, pre-chilled feeds, vaporization of liquid medium (diluent, monomers or solvent) or combinations of all three. Adiabatic reactors with pre-chilled feeds can also be used. The purity, type, and amount of solvent can be optimized for the maximum catalyst productivity for a particular type of polymerization. The solvent can be also introduced as a catalyst carrier. The solvent can be introduced as a gas phase or as a liquid phase depending on the pressure and temperature. Advantageously, the solvent can be kept in the liquid phase and introduced as a liquid. Solvent can be introduced in the input to the polymerization reaction zones.

[0155] A process described herein can be a solution polymerization process that may be performed in a batchwise fashion (e.g., batch; semi-batch) or in a continuous process.Suitable reaction zones may include tank, loop, and tube designs. In at least one embodiment, the process is performed in a continuous fashion and dual loop reactors in a series configuration are used. In at least one embodiment, the process is performed in a continuous fashion and dual continuous stirred-tank reactors (CSTRs) in a series configuration are used. Furthermore, the process can be performed in a continuous fashion and a tube reactor can be used. In another embodiment, the process is performed in a continuous fashion and one loop reactor and one CSTR are used in a series configuration. The process can also be performed in a batchwise fashion and a single stirred tank reactor can be used.

[0156] In some embodiments, the polymer mixture produced from the polymerization reaction of the method of operation 106 includes a terpolymer composed of the monomer compounds of the monomer input. The olefin monomers of the monomer input can include ethylene and one or more olefin compounds (e.g., propylene). For the sake of brevity, the one or more olefin compounds, from here on, will be referred to as / by propylene. That is to say that any one or more olefin compounds may be substituted in place of propylene for the remainder of the disclosure. In at least one embodiment, the terpolymer can be represented by Formula (V):wherein each of x, y, and z are independently an integer greater than 1. In at least one embodiment, the terpolymer is composed of ethylene units, propylene units, and aluminum containing monomer units. The terpolymer may include a number of ethylene units, wherein the number of ethylene units is denoted by x. The terpolymer may include a number of propylene units, wherein the number of propylene units is denoted by y. The terpolymer may include a number of aluminum containing monomer units, wherein the number of aluminum containing monomer units is denoted by z.

[0157] In some embodiments, the efficiency of the polymerization reaction can be described in terms of catalyst activity (e.g., amount of polymer produced per amount of catalyst introduced to the polymer system) and overall polymer yield. In at least one embodiment, the catalyst activity is about 100,000 g polymer / g catalyst (g / g) to about 2,500,000 g / g, such as about 150,000 g / g to about 2,000,000 g / g, such as about 250,000 g / g to about 1,000,000 g / g, alternatively about 100,000 g / g to about 150,000 g / g, alternatively about 150,000 g / g to about 250,000 g / g, alternatively about 250,000 g / g to about 500,000 g / g, alternatively about 500,000 g / g to about 1,000,000 g / g, alternatively about 1,000,000 g / g to about 2,000,000 g / g, alternatively about 2.000,000 g / g to about 2.500,000 g / g. In some embodiments, the polymer yield of the polymerization reaction is about 100 g to about 5,000 g, such as about 150 g to about 1,000 g, such as about 250 g to about 500 g, alternatively about 100 g to about 150 g, alternatively about 150 g to about 250 g, alternatively about 500 g to about 1,000 g, alternatively about 1,000 g to about 5,000 g.

[0158] At operation 108 of the method 100, the polymer mixture is transferred from the first reaction zone to a second reaction zone. The polymer mixture may be transferred from the first reaction zone to the second reaction zone via any one or more processes known to one of ordinary skill in the art, such as pumping, conveying, flowing, and the like. In at least one embodiment, the polymer mixture may be transferred from the first reaction zone to the second reaction zone via a '‘free-flowing” mechanism, by which gravitational force isoperating mechanism progressing the polymer mixture from the first reaction zone to the second reaction zone.

[0159] At operation 110 of the method 100, an oxygen or sulfur containing reagent is introduced to the second reaction zone, and is reacted with the polymer mixture at operation 112 to produce a polymer composition. The oxygen or sulfur containing reagent may be introduced to the second reaction zone with the polymer mixture and / or subsequently after the polymer mixture has been introduced to the second reaction zone. In some embodiments, the oxygen containing reagent is selected from oxygen (O2), carbon dioxide (CO2), ozone (O3), compressed dry air, dry air, air vented in from outside the second reaction zone, an organic peroxide, peroxyacetic acid, meta-chloroperoxybenzoic acid, or a combination thereof. In at least one embodiment, the oxygen or sulfur containing reagent is selected from O2, CO2, CS2, peroxyacectic acid, meta-chloroperoxybenzoic acid, and combinations thereof. In some embodiments, the oxygenated reagent is added as a gas, for example, O2, CO2, compressed dry air, dry air, or air vented in from outside the second reaction zone. In some embodiments, the oxygenated reagent is solubilized in a hydrocarbon liquid that has been saturated with an oxygenated gas such as O2, CO2, and / or dry air. In some embodiments, the oxygenated reagent is solubilized in a hydrocarbon liquid to form a solution containing an organic peroxide, peroxyacectic acid, meta-chloroperoxybenzoic acid, and combinations thereof. In some embodiments, O2 is preferred. In other embodiments, compressed dry air. or dry air is preferred.

[0160] In some embodiments, the second reaction zone is free of, or substantially free of, water, alcohols, salts of alcohols, organic acids, inorganic acids, or any combination thereof.

[0161] In some embodiments, the temperature within the second reaction zone during and / or throughout operation 110 of the method 100 is about 50°C to about 250°C, such as about 100°C to about 200°C, such as about 125°C to about 175°C, alternatively about 50°C to about 100°C, alternatively about 100°C to about 125°C, alternatively about 125°C to about 150°C, alternatively about 150°C to about 175°C, alternatively about 175°C to about 200°C, alternatively about 200°C to about 250°C.

[0162] Reacting the polymer mixture with the oxygen containing gas quenches the polymerization reaction and / or promotes the formation of anion alkenyl moiety from the aluminum containing pendant groups present along the polymer chain. In other words, metal alkenyl moieties of a terpolymer of the present disclosure are converted into anion alkenyl moieties to form an ionomer composition. In at least one embodiment, the polymer composition includes a terpolymer represented by Formula (VI):wherein each of x, y, and z are independently an integer greater than 1. In at least one embodiment, the terpolymer is composed of ethylene units, propylene units, and aluminum containing monomer units. The terpolymer may include a number of ethylene units, wherein the number of ethylene units is denoted by x. The terpolymer may include a number of propylene units, wherein the number of propylene units is denoted by y. The terpolymer may include a number of aluminum containing monomer units, wherein the number of aluminum containing monomer units is denoted by z.

[0163] As previously discussed, terpolymers formed via method(s) described herein include ethylene units, a-olefin units, and aluminum containing units. In some embodiments, the terpolymer has a weight average molecular weight (Mw) of about 5,000 g / mol or greater, such as about 5,000 g / mol to about 2,000,000 g / mol, such as about 10,000 g / mol to about 1,000,000 g / mol, such as about 10,000 g / mol to about 500,000 g / mol, such as about 10,000 g / mol to about 300,000 g / mol, such as about 20.000 g / mol to about 200,000 g / mol, such as about 20.000 g / mol to about 100,000 g / mol. such as about 30,000 g / mol to about 90.000 g / mol, such as about 40,000 g / mol to about 80,000 g / mol, such as about 50,000 g / mol to about 70,000 g / mol, such as about 55,000 g / mol to about 65,000 g / mol, such as about 60,000 g / mol to about 65,000 g / mol.

[0164] In at least one embodiment, the terpolymer has a number average molecular weight (Mn) of about 1,000 g / mol or greater, such as about 1,000 g / mol to about 400,000 g / mol, such as about 1,000 g / mol to about 200,000 g / mol, such as about 1,000 g / mol to about 100,000 g / mol, such as about 1,000 g / mol to about 50,000 g / mol, such as about 5,000 g / mol to about 40,000 g / mol, such as about 10,000 g / mol to about 30,000 g / mol, such as about 15,000 g / mol to about 25,000 g / mol, such as about 18,000 g / mol to about 20.000 g / mol.

[0165] In at least one embodiment, terpolymers of the present disclosure can have an Mw / Mn (polydispersity index) value of about 1 to about 10, such as from about 2 to about 5, such as from about 3 to about 4.

[0166] In at least one embodiment, the terpolymer includes one or more ethylene units, one or more additional a-olefin units, and one or more aluminum containing units. The terpolymer may include an ethylene content of about 0.1 wt% to about 50 wt% based on the weight of the terpolymer, such as about 1 wt% to about 50 wt%, such as about 10 wt% to about 50 wt%, such as about 20 wt% to about 50 wt%, such as about 30 wt% to about 50 wt%, such as about 40 wt% to about 50 wt%, such as about 45 wt% to about 50 wt%. In some embodiments, the terpolymer has an ethylene content of less than about 50 wt%, such as less than about 30 wt%, such as less than about 20 wt%, such as less than about 18 wt%. The terpolymer may include the one or more additional a-olefin units in an amount of about 50 \\t% to about to about 99.9 wt% based on the weight of the terpolymer, such as about 50 wt% to about 99 wt%, such as about 50 wt% to about 90 wt%, such as about 50 wt% to about 80 wt%, such as about 50 wt% to about 70 wt%, such as about 50 wt% to about 60 wt%, such as about 50 wt% to about 55 wt%, alternatively about 0.1 wt% to about 50 wt%, alternatively about 1 wt% to about 50 wt%, alternatively about 10 wt% to about 50 wt%, alternatively about 20 wt% to about 50 wt%, alternatively about 30 wt% to about 50 wt%, alternatively about 40 wt% to about 50 wt%, alternatively about 45 wt% to about 50 wt%. The terpolymer may include the one or more aluminum containing units in an amount of about 0.01 wt% to about 20 wt% based on the weight of the terpolymer, such as about 0.1 wt% to about 10 wt%, such as about 0.1 wt% to about 5 wt%, such as about 0.3 wt% to about 3 wt%, such as about 0.5 wt% to about 1.5 wt%.

[0167] In at least one embodiment, the terpolymer includes about 0.1 wt% to about 50 wt% ethylene based on the weight of the terpolymer, such as about 1 wt% to about 50 wt%, such as about 10 wt% to about 50 wt%, such as about 20 wt% to about 50 wt%, such as about 30 wt% to about 50 wt%, such as about 40 wt% to about 50 wt%, such as about 45 wt% to about 50 wt%. The terpolymer may also include about 50 wt% to about to about 99.9 wt% propylene based on the weight of the terpolymer, such as about 50 wt% to about 99 wt%, such as about 50 wt% to about 90 wt%, such as about 50 wt% to about 80 wt%, such as about 50 wt% to about 70 wt%, such as about 50 wt% to about 60 wt%, such as about 50 wt% to about 55 wt%. The terpolymer may also include the one or more aluminum containing units in an amount of about 0.01 wt% to about 20 wt% based on the weight of the terpolymer, suchas about 0.1 wt% to about 10 wt%, such as about 0.1 wt% to about 5 wt%, such as about 0.3 wt% to about 3 wt%. such as about 0.5 wt% to about 1.5 wt%.

[0168] In some embodiments, the weight ratio of ethylene to the one or more additional a-olefin units in the terpolymer composition is about 1:99 to about 35:65, such as about 20:80 to about 30:70. In at least one embodiment, the weight ratio of ethylene to propylene is about 1:99 to about 35:65, such as about 20:80 to about 30:70.

[0169] In some embodiments, the terpolymer has a melt flow rate of about 0.01 to about 150 at a temperature of about 230°C, such as about 0.1 to about 50, such as about 0.1 to about 10, such as about 0.1 to about 5. In at least one embodiment, the terpolymer has a complex viscosity (T|) of about 90 kPa*s to about 200 kPa*s at 150°C, such as about 100 kPa*s to about 180 kPa*s. such as about 110 kPa*s to about 150 kPa*s. In at least one embodiment, the terpolymer has a complex viscosity of greater than about 100 kPa*s at 150°C. In at least one embodiment, the terpolymer has a shear elastic modulus (G’) of about 200 Pa to about 1,000 Pa at 150°C, such as about 200 Pa to about 600 Pa, such as about 200 Pa to about 400 Pa. In at least one embodiment, the terpolymer has a shear elastic modulus (G ) of greater than about 350 Pa at 150°C. In at least one embodiment, the terpolymer has a tan 6 of about 1 to about 5, such as about 1 to about 4, such as about 1 to about 3. In at least one embodiment, the terpolymer has a strain hardening ratio at 150°C of about 1.1 to about 5, such as about 1.2 to about 4.8, such as about 1.3 to about 4.6. In some embodiments, the terpolymer has a strain hardening ratio (SHR) of about 1.1 or greater, alternatively. 1,2 or greater, alternatively 1,3 or greater, alternatively 1.4 or greater, alternatively 1.5 or greater, alternatively 1.7 or greater.

[0170] In some embodiments, the terpolymer has a glass transition temperature (Tg) of about -40°C to about 0°C, such as about -40°C to about -10°C, such as about -35°C to about -15°C. In some embodiments, the terpolymer has a melting temperature (Tm) of about 30°C to about 130°C, such as about 35°C to about 100°C, such as about 40°C to about 75°C. In some embodiments, the terpolymer is amorphous and exhibits no melting temperature.EXAMPLES

[0171] The foregoing discussion can be further described with reference to the following non-limiting examples. Catalyst A can be prepared as described in US 11,254,763. Activator 1, dimethylanilinium tetrakis (pentafluorophenyl)borate, is commercially available from Boulder Scientific and other suppliers. Tri(n-octyl)aluminum (TNOAL, neat) can be purchased from Nouryon, and was used as a 25 wt% solution in hexane solvent. Solvents, and1,7-octadiene (available from Sigma Aldrich) were purified by filtering through a plug of neutral alumina (Sigma Aldrich) under an N2 atmosphere.Example 1: Preparation of aluminum containing monomer (AV 18)

[0172] To a 2000 mL round bottom flask containing 1,7-octadiene (1194 mL, 8080 mmol) at 60°C was added diisobutylaluminium hydride (DIBAL-H; 320 mL, 1796 mmol) dropwise over 1 hour. After addition, 1.7-octadiene was distilled off at 60°C under reduced pressures, leaving behind a colorless liquid. The colorless liquid was further dried under reduced pressures at ambient temperatures for at least 3 hours, affording 7-octenyldiisobutylaluminum (AV18) as a colorless oil (520 mL, 445.6 g, 98% yield).NMR (400 MHz, benzene-d6):5 = 5.78 (m, 1H, =CH), 5.01 (m. 2H, =CH2), 1.95 (m, 4H, -CH2), 1.54 (m. 2H, iBu-CH), 1.34 (m, 6H, -CH2), 1.04 (d, 12H, iBu-CH3), 0.49 (t, 2H, A1-CH2), 0.27 (d, 4H, iBu-CH2) ppm.Example 2: Preparation of aluminum containing monomer solution

[0173] The aluminum containing monomer (AV 18; 20 mL) was added to a round bottom flask containing 780 mL toluene in an N2 glovebox. The mixture was allowed to stir at ambient temperatures for 10 minutes before use.Example 3: Preparation of polymerization catalyst solution

[0174] Catalyst A (20.0 mg; shown below) and dimethylanilinium tetrakis (pentafluorophenyl)borate (Activator 1; 17.9 mg) were added to a round bottom flask containing 900 mL toluene in an N2 glovebox. The mixture was allowed to stir at ambient temperatures for 10 minutes before use. The mixture is referred to as “catalyst solution” hereafter.Example 4: General process for the preparation of terpolymers

[0175] Polymerizations described in the example below were carried out in a continuous stirred tank reactor system. A 1 -liter Autoclave reactor was equipped with a stirrer, a pressure controller, and a water cooling / steam heating element with a temperature controller. The reactor was operated in liquid fill condition at a reactor pressure in excess of the bubbling point pressure of the reactant mixture, keeping the reactants in liquid phase.Isohexane and propylene were pumped into the reactors by Pulsa feed pumps. All flow rates of liquid were controlled using Coriolis mass flow controller (Quantim series from Brooks). Ethylene flowed as a gas under its own pressure through a Brooks flow controller. Ethylene, propylene and the aluminum containing monomer solution (AV 18) feeds were combined into one stream and then mixed with a pre-chilled isohexane stream that had been cooled to at least 0°C. The mixture was then fed to the reactor through a single line. The tri(n-octyl)aluminum solution was added to the combined solvent and monomer stream just before they entered the reactor. The catalyst solution was fed to the reactor using an ISCO syringe pump through a separate line.

[0176] The polymer produced in the first reactor exited to a second IL reactor where the polymer stream was quenched with either dry air (21% O2, referred to as '‘air” in Table 1) at a flow rate of 100 mL / min. The polymer stream then exited the second reactor through a back pressure control valve that reduced the pressure to atmospheric. This caused the unconverted monomers in the solution to flash into a vapor phase which was vented from the top of a vapor liquid separator. The liquid phase, comprising mainly polymer and solvent, was collected for polymer recovery. The collected samples were first air-dried in a hood to evaporate most of the solvent, and then dried in a vacuum oven at a temperature of about 90°C for about 12 hours. The vacuum oven dried samples were weighed to obtain yields.

[0177] The results of polymerization reactions are summarized in Table 1.Table 1. Summary of polymerization conditions and resulting polymer compositions of terpolymers. Activated cat solution was prepared by mixing Catalyst Complex A (20 mg) and Activator 1 (17.9 mg) in 450 mL of toluene. TNOAL solution (25 wt% in hexane) was maintained at a flow rate of 2.4 mL / min. Isohexane was maintained at a flow rate of 45 g / min. Dry air was used as the quench reagent in the second reactor at a flow rate of 100 mL / min.Table 1 - Part 1Table 1 - Part 2

[0178] As can be observed from the data provided in Table 1, each of the monomer input rates, catalyst input rates, and the reaction temperature affect the resulting terpolymer composition and melt flow rate. It was further determined that the temperature at which the polymerization reaction and the catalyst input rate influences the melt flow rate of the resulting terpolymers. For instance, at catalyst input rates of about 1 mL / min or greater and reaction temperatures of about 95°C or greater, the melt flow rate of the resulting terpolymer greatly increases. Without being bound by theory, the increase in the melt flow rate is indicative of a lack of integration of the aluminum containing monomer into the terpolymer composition.

[0179] After oxidation of the terpolymer by introducing an oxidizing agent to the second reactor, an ionomer can be formed having an a-olefin content and an anion alkenyl content (e.g., aluminum containing monomer). In other words, metal alkenyl moieties of the terpolymers are transformed into anion alkenyl moieties to form an ionomer, where the terpolymers can have any comonomer composition described herein. Properties of the ionomers may be influenced by ion content. In that regard, ion content can be increased by atleast one of: increasing an aluminum vinyl unit content in the terpolymer composition, increasing an extent of an oxidizing reaction to increase a conversion of aluminum pendant groups to alkoxide, carboxylate, thiocarboxylate anions, increasing an extent of ion exchange to promote ionomer conversion or combination(s) thereof. In any case, an ionic content can be increased, thereby forming a stronger ionic network. As previously noted, and without being bound by theory, the increase in the melt flow rate is indicative of a lack of integration of the aluminum containing monomer into the terpolymer composition.Example 5: Representative synthetic example of Sample 7

[0180] Sample 1 was prepared in two continuous stirred-tank one-liter reactors in series. The first reactor A (one liter) was continuously supplied with isohexane (45 g / min), ethylene (1.6 liter / min), propylene (14 g / min), TNOAL solution (25 wt% in hexane. 2.4 mL / min). and activated catalyst solution (Catalyst A / Activator 1, 0.3 mL / min). The total pressure was maintained at 350 psi. The temperature was 85°C. The stir rate was 1000 rpm. The polymerization reaction mixture exited reactor A and entered reactor B (one liter) which was supplied with dry air (21% O2. 100 mL / min). The polymerization reaction mixture then exited reactor B, and the polymer solution was collected in a beaker. The total polymerization time was 40 minutes. The polymer was then dried under reduced pressure at 90°C for 8 hours.Yield: 381.4 g.Example 6: Representative synthetic example of Sample 2

[0181] Sample 2 was prepared in two continuous stirred-tank one-liter reactors in series. The first reactor A (one liter) was continuously supplied with isohexane (45 g / min), ethylene (1.6 liter / min), propylene (14 g / min), AV18 solution (1.2 mL / min), TNOAL solution (2.4 mL / min), and activated catalyst solution (Catalyst A / Activator 1, 0.6 mL / min). The total pressure was maintained at 350 psi. The temperature was 85°C. The stir rate was 1000 rpm. The polymerization reaction mixture exited reactor A and entered reactor B (one liter) which was supplied with dry air (21% O2, 100 mL / min). The polymerization reaction mixture then exited reactor B, and the polymer solution was collected in a beaker. The total polymerization time was 40 minutes. The polymer was then dried under reduced pressure at 90°C for 8 hours.Yield: 173.4 g.Polymer Characterization Methods4D Gel permeation chromatograph (4D GPC)

[0182] Unless otherwise indicated, the distribution and the moments of molecular weight (Mw, Mn, Mz, Mw / Mn, etc.) and the comonomer content are determined by using a high temperature Gel Permeation Chromatography (Polymer Char GPC-IR) equipped with a multiple-channel band-filter based Infrared detector IR5 with a multiple-channel band filter based infrared detector ensemble IR5 with band region covering about 2700 cm’1to about 3000 cm’1(representing saturated C-H stretching vibration), an 18-angle light scattering detector and a viscometer. Three Agilent PLgel 10-pm Mixed-B LS columns are used to provide polymer separation. Reagent grade 1, 2, 4-tri chlorobenzene (TCB) (from Sigma-Aldrich) comprising-300 ppm antioxidant BHT can be used as the mobile phase at a nominal flow rate of -1.0 mL / min and a nominal injection volume of -200 pL. The whole system including transfer lines, columns, and detectors can be contained in an oven maintained at ~145°C. A given amount of sample can be weighed and sealed in a standard vial with -10 pL flow marker (heptane) added thereto. After loading the vial in the auto-sampler, the oligomer or polymer may automatically be dissolved in the instrument with -8 mL added TCB solvent at ~160°C with continuous shaking. The sample solution concentration can be from -0.2 to -2.0 mg / ml, with lower concentrations used for higher molecular weight samples. The concentration, c, at each point in the chromatogram can be calculated from the baseline-subtracted IR5 broadband signal, I, using the equation:c=al, where a is the mass constant determined with polyethylene or polypropylene standards. The mass recovery can be calculated from the ratio of the integrated area of the concentration chromatography over elution volume and the injection mass which is equal to the predetermined concentration multiplied by injection loop volume. The conventional molecular weight (IR MW) is determined by combining universal calibration relationship with the column calibration which is performed with a series of monodispersed polystyrene (PS) standards ranging from 700 to 10M gm / mole. The MW at each elution volume is calculated with following equation:where the variables with subscript “PS” stand for polystyrene while those without a subscript are for the test samples. In this method, aps = 0.67 and Kps = 0.000175, a and K for other materials are as calculated by GPC ONE™ software (Polymer Characterization, S. A., Valencia, Spain). Concentrations are expressed in g / cm3, molecular weight is expressed ing / mole, and intrinsic viscosity (hence Kin the Mark-Houwink equation) is expressed in dL / g unless otherwise noted.

[0183] The comonomer composition is determined by the ratio of the IR5 detector intensity corresponding to CH2 and CH3 channel calibrated with a series of PE and PP homo / copolymer standards whose nominal value are predetermined by NMR or FTIR. In particular, this provides the methyls per 1000 total carbons (CH3 / 1000TC) as a function of molecular weight. The short-chain branch (SCB) content per 1000TC (SCB / 1000TC) is then computed as a function of molecular weight by applying a chain-end correction to the CH3 / 1000TC function, assuming each chain to be linear and terminated by a methyl group at each end. The weight % comonomer is then obtained from the following expression in which f is 0.3, 0.4, 0.6. 0.8, and so on for C3, C4, C6, C8, and so on co-monomers. respectively:w2 = f * SCB / 1000TCThe bulk composition of the polymer from the GPC-IR and GPC-4D analyses is obtained by considering the entire signals of the CH and CH2 channels between the integration limits of the concentration chromatogram. First, the following ratio is obtainedArea of CH3signal within integration limitsBulk IR ratio = - — — —: -; — — —: -: - - — —Area of CH2signal within integration limitsThen the same calibration of the CH3 and CH2signal ratio, as mentioned previously in obtaining the CH3 / 1000TC as a function of molecular weight, is applied to obtain the bulk CH3 / 1000TC. A bulk methyl chain ends per 1000TC (bulk CH3end / 1000TC) is obtained by weight-averaging the chain-end correction over the molecular-weight range. Then w2b = f * bulk SCB / 1000TCbulk SCB / 1000TC = bulk CH3 / 1000TC - bulk CH3end / 1000TC and bulk SCB / 1000TC is converted to bulk iv2 in the same manner as described above.

[0184] The LS detector is the 18-angle Wyatt Technology High Temperature DAWN HELEOSII. The LS molecular weight (M) at each point in the chromatogram is determined by analyzing the LS output using the Zimm model for static light scattering (Light Scattering from Polymer Solutions,' Huglin, M. B., Ed.; Academic Press, 1972 ):

[0185] Here, AR(0) is the measured excess Rayleigh scattering intensity at scattering angle 6, c is the polymer concentration determined from the IR5 analysis, A2 is the secondvirial coefficient, P(0) is the form factor for a monodisperse random coil, and Ko is the optical constant for the system:where NA is Avogadro’s number, and (dn / dc) is the refractive index increment for the system,n = 1.500 for TCB at 145°C and = 665 nm. For analyzing polyethylene homopolymers, ethylene-hexene copolymers, and ethylene-octene copolymers, dn / dc = 0.1048 ml / mg and A2 = 0.0015; for analyzing ethylene-butene copolymers, dn / dc = 0.1048*(1-0.00126*w2) ml / mg and A2 = 0.0015 where w2 is weight percent butene comonomer.

[0186] A high temperature Agilent (or Viscotek Corporation) viscometer, which has four capillaries arranged in a Wheatstone bridge configuration with two pressure transducers, is used to determine specific viscosity. One transducer measures the total pressure drop across the detector, and the other, positioned between the two sides of the bridge, measures a differential pressure. The specific viscosity, ps, for the solution flowing through the viscometer is calculated from their outputs. The intrinsic viscosity, [η], at each point in the chromatogram is calculated from the equation [η]= η / c, where c is concentration and is determined from the IR5 broadband channel output. The viscosity MW at each point is calculated as M=KpsMaps+1 / [η] where aps is 0.67 and Kps is 0.000175.

[0187] The branching index (g'vis) is calculated using the output of the GPC-IR5-LS-VIS method as follows. The average intrinsic viscosity, [η]avg of the sample is calculated by:[η]avg = Σ(ci[η]i) / Σciwhere the summations are over the chromatographic slices, i, between the integration limits. The branching index g'vis is defined aswhere Mv is the viscosity-average molecular weight based on molecular weights determined by LS analysis and the K and α are for the reference linear polymers are calculated by GPC ONE™ 2019f software (Polymer Characterization, S. A., Valencia, Spain). Concentrations are expressed in g / cm3, molecular weight is expressed in g / mole, and intrinsic viscosity (hence K in the Mark-Houwink equation) is expressed in dL / g unless otherwise noted.Calculation of the w2b values is as discussed above.Differential scanning calorimetry (DSC)

[0188] Glass transition temperature (Tg) and melting temperature (or melting point, Tm) are measured using Differential Scanning calorimetry (DSC) on a commercially available instrument (e.g., TA Instruments 2920 DSC or TA Instruments 2900 DSC). Typically, 6 mg to 10 mg of molded polymer or plasticized polymer are sealed in an aluminum pan and loaded into the instrument at room temperature. Melting data (first heat) is acquired by heating the sample to at least 30°C above its melting temperature, typically 200°C for polypropylene, at a heating rate of 10°C / min. The sample is held for at least 5 minutes at this temperature to destroy its thermal history. Crystallization data are acquired by cooling the sample from the melt to at least 50°C below the crystallization temperature at a cooling rate of 10°C / min. The sample is held at this temperature for at least 5 minutes, and finally heated at 10°C / min. to acquire additional melting data (second heat). The endothermic melting transition (first and second heat) and exothermic crystallization transition are analyzed according to standard procedures. The melting temperatures reported are the peak melting temperatures from the second heat unless otherwise specified. For Tg determination herein, temperature ramps from -150°C to 150°C with a 10°C / min. heating rate were carried out using a DSC2500™ (TA Instruments™).

[0189] For polymers displaying multiple peaks, the melting temperature is defined to be the peak melting temperature from the melting trace associated with the largest endothermic calorimetric response (as opposed to the peak occurring at the highest temperature).Likewise, the crystallization temperature is defined to be the peak crystallization temperature from the crystallization trace associated with the largest exothermic calorimetric response (as opposed to the peak occurring at the highest temperature).1H Nuclear Magnetic Resonance Spectroscopy (NMR)

[0190] Proton NMR spectra are collected using a suitable instrument, e.g., a 500 MHz Varian pulsed Fourier transform NMR spectrometer equipped with a variable temperature proton detection probe operating at 120°C. Typical measurement of the NMR spectrum include dissolving of the polymer sample in l,l,2,2-tetrachloroethane-d2 (" TCE-d2") and transferring into a 5 mm glass NMR tube. Typical acquisition parameters are a sweep width of 10 KHz, pulse width of 30 degrees, acquisition time of 2 seconds, acquisition delay of 5 seconds and number of scans was 120. Chemical shifts are determined relative to the TCE-d2 signal, which was set to 5.98 ppm.Rheological properties of terpolymers

[0191] Rheological data such as “Complex shear viscosity (q*),” reported in Pascal seconds, can be measured at 0.01 rad / sec and 100 rad / sec. Complex shear viscosity and other rheological measurements can be obtained from small angle oscillatory shear (SAGS) experiments.

[0192] For instance, complex shear viscosity can be measured with a rotational rheometer such as an Advanced Rheometrics Expansion System (ARES-G2 model) or Discovery Hybrid Rheometer (DHR-3 Model) using parallel plates (diameter=25 mm) in a dynamic mode under nitrogen atmosphere. The rheometer can be thermally stable at 190°C for at least 20 minutes before inserting compression-molded specimen onto the parallel plates. To determine the specimen’s viscoelastic behavior, a frequency sweep in the range from 0.01 to 628 rad / s can be carried out at a temperature of 190°C under constant strain that does not affect the measured viscoelastic properties. The sweep frequencies are equally spaced on a logarithmic scale, so that 5 frequencies are probed per decade. Depending on the molecular weight and temperature, strains of 3% can be used and linearity of the response is verified. A nitrogen stream is circulated through the oven to minimize chain extension or cross-linking during the experiments. The specimens can be compression molded at 190°C, without stabilizers. A sinusoidal shear strain can be applied. If the strain amplitude is sufficiently small the material behaves linearly. As those of ordinary skill in the art will be aware, the resulting steady-state stress will also oscillate sinusoidally at the same frequency but will be shifted by a phase angle 5 with respect to the strain wave. The stress leads the strain by 5. For purely elastic materials 8=0° (stress is in phase with strain) and for purely viscous materials, 8=90° (stress leads the strain by 90° although the stress is in phase with the strain rate). For viscoelastic materials. 0< 8 <90. Complex viscosity, loss modulus (G") and storage modulus (G') as function of frequency are provided by the small amplitude oscillatory shear test. Dynamic viscosity is also referred to as complex viscosity or dynamic shear viscosity. The phase or the loss angle 8, is the inverse tangent of the ratio of G" (shear loss modulus) to G' (shear storage modulus). The shear thinning slope (STS) can be measured using plots of the logarithm (base ten) of the dynamic viscosity versus logarithm (base ten) of the frequency. The slope is the difference in the log(dynamic viscosity) at a frequency of 100 s ' and the log(dynamic viscosity) at a frequency of 0.01 s ’ divided by 4. The complex shear viscosity (q*) versus frequency (co) curves can be fitted using the Carreau-Yasuda model:η*- η∞ = (η₀ - η∞)*(1 + (λω)ᵃ)^((n-1) / a).

[0193] The five parameters in this model are: r|o. the zero-shear viscosity; X, the relaxation time; and n, the power-law index; r|co the infinite rate viscosity’; and a. the transition index. The zero-shear viscosity is the value at a plateau in the Newtonian region of the flow curve at a low frequency, where the dynamic viscosity’ is independent of frequency. The relaxation time corresponds to the inverse of the frequency at which shear-thinning starts. The power-law exponent describes the extent of shear-thinning, in that the magnitude of the slope of the flow curve at high frequencies approaches n-1 on a log(η*)-log(ω) plot. For Newtonian fluids, n=l and the dynamic complex viscosity is independent of frequency.

[0194] In addition to dynamic and complex viscosity (each in Pascal seconds), at each frequency sweep in the SAGS experiment, various other parameters are collected, including storage modulus (Pa), Loss modulus (Pa), Complex Modulus (Pa), tan(delta), and phase angle. Charting the phase angle versus the complex shear modulus from the rheological experiment yields Van Gurp Palmen plots useful to extract some information on the molecular characteristics, for example, linear vs. long chain branched chains, type of long chain branching, polydispersity (Dealy, M. J., Larson, R. G., ‘" Structure and Rheology of Molten Polymers”, Carl Hanser Verlag, Munich pp. 182-183 (2006). It has been also suggested that Van Gurp Palmen plots can be used to reveal the presence of long chain branching in polyethylene. See Trinkle, S., Walter, P., Friedrich, C. “Van Gurp-Palmen plot II — Classification of long chain branched polymers by their topology”, in 41 Rheol. Acta pp. 103-113 (2002).

[0195] “Strain Hardening Ratio” (SHR), also known strain hardening coefficient (Münstedt, Rheol. Acta (2023) 62:333-363), is defined as the ratio between the extensional viscosity measured at a Hencky strain (εH) of 3 and a Hencky strain rate (ἐH) of 1 s⁻¹ in the linear viscoelastic envelop (LVE), e.g., SHR = ηE+(εH= 3) / ηLVE(εH= 3). The extensional viscosity (p^) is measured using a Sentamanat Extensional rheometer (SER, Xpansion Instruments) mounted on a rotational rheometer (ARES-G2, TA Instruments). Start-up transient extensional viscosity measurements are carried out at 150°C using four Hencky strain rates of 0.01, 0.1, L0, and 10 s'1(shown in FIG. 3). LVE measurements correspond to the transient shear viscosity measured during a start-up shear flow experiment at 150°C with a shear rate of 0.001 s'1. The LVE viscosity’ ( ]LVE, dotted line in figure below) is equal to the transient shear viscosity (?]+) multiplied by 3 (i.e.. TJLVE= 3 X TJ+). FIG. 3 shows the transient extensional viscosity of Sample 3, measured at 150°C and Henck ’ strain rates of 0.01, 0.01, 1.0 and 10 s'1, as indicated. Dotted line corresponds to the linear viscoelasticenvelope. The SHR is computed with the indicated values of η+and ηLVE, measured at εH= 3 (SHR = η+(εH= 3) / ηLVE(εH= 3)).Thermal and thermomechanical properties of terpolymers

[0196] The thermal and thermomechanical properties of select terpolymer samples, as formulated herein, were determined in accordance with the above specified procedures and methods. The resulting terpolymer properties were compared to those of various copolymer made up of ethylene and propylene units. That is to say that the effects of having the aluminum containing monomer present in the terpolymer composition was comparatively analyzed with copolymers formed under similar polymerization conditions. The results of such analysis are summarized in Table 2.Table 2. Summary of the thermal and thermomechanical properties of terpolymers. C2 wt% was determined by the FTIR method.aComplex viscosity (|T]*|) measured at 150°C and at an angular frequency (to) of 0.01 s'1.bG’ is the storage modulus, and tan 5 is the ratio between storage and loss moduli (G’’), i.e., tan 5 = G’7G’. G’ and tan 5 are measured at 150°C and at an angular frequency (co) of 0.01 s'1.cComparative copolymers 48 to 51 are commercial Vistamaxx™ copolymers available from ExxonMobil.

[0197] The thermal and thermomechanical properties of various terpolymers and comparative copolymers are summarized in Table 2. As such, it has been determined that the composition of each of the terpolymers and copolymer affect such properties. For instance, terpolymer samples having about 20 wt% or greater ethylene content (<?.g., samples 2, 9-11, and 14) exhibit amorphous material properties. In contrast, terpolymer samples having about 10 wt% or less ethylene content exhibit melting temperatures of about 80°C or greater. Furthermore, the data presented in Table 2 suggests that the terpolymer composition may be tuned to obtain the desired thermal and thermomechanical properties, such as properties similar to that of the comparative copolymer compositions while also exhibiting increased melt stability. As previously described, the increased melt stability can be attributed to the ion formation of the aluminum containing monomer units in the terpolymer composition. Rheological analysis of select terpolymers

[0198] Rheological analysis was conducted on Samples 1, 13, 8, and 3 to determine the effects of changing the input rate of the aluminum containing monomer of the polymerization reaction on the resulting storage modulus (FIG. 3A) and complex viscosity (FIG. 3B) as afunction of angular frequency. As can be observed, terpolymers formed using higher input rates of the aluminum containing monomer exhibit increased storage modulus and complex viscosity. Such increases can be attributed to increased amounts of the aluminum containing monomer within the terpolymer composition allowing for greater ion formation.Furthermore, it is observed that the transient extensional viscosity (FIG. 3C) of terpolymers also increases as a function of increasing the input rate of the aluminum containing monomer.

[0199] Overall, the present disclosure provides a method for the continuous production of terpolymers composed of ethylene, one or more additional a-olefin monomers, and aluminum containing monomer units. More specifically, the method disclosed herein utilizes a first reactor for the polymerization reaction and a second reactor for the oxidation reaction. Bifurcating the two reactions into two different reactors allows for the development of a continuous process, which can increase production efficiency and decrease cost. Furthermore, an investigation into reactor conditions and input ratios was conducted to determine their effects on the resulting material’s thermal and thermomechanical properties. From such investigation, it was determined that the ability for ion formation of the aluminum containing monomer units in the terpolymer composition increased the melt strength of the terpolymer compositions without sacrificing other desired thermal and thermomechanical properties.

[0200] The phrases, unless otherwise specified, "consists essentially of and "consisting essentially of do not exclude the presence of other steps, elements, or materials, whether or not, specifically mentioned in this specification, so long as such steps, elements, or materials, do not affect the basic and novel characteristics of the present disclosure, additionally, they do not exclude impurities and variances normally associated with the elements and materials used.

[0201] For the sake of brevity, only certain ranges are explicitly disclosed herein.However, ranges from any lower limit may be combined with any upper limit to recite a range not explicitly recited, as well as, ranges from any lower limit may be combined with any other lower limit to recite a range not explicitly recited, in the same way, ranges from any upper limit may be combined with any other upper limit to recite a range not explicitly recited. Additionally, within a range includes every point or individual value between its end points even though not explicitly recited. Thus, every point or individual value may serve as its own lower or upper limit combined with any other point or individual value or any other lower or upper limit, to recite a range not explicitly recited.

[0202] All documents described herein are incorporated by reference herein, including any priority documents and or testing procedures to the extent they are not inconsistent withthis text. As is apparent from the foregoing general description and the specific embodiments, while forms of the present disclosure have been illustrated and described, various modifications can be made without departing from the spirit and scope of the present disclosure. Accordingly, it is not intended that the present disclosure be limited thereby. Likewise, the term “comprising” is considered synonymous with the term “including” for purposes of United States law. Likewise, whenever a composition, an element or a group of elements is preceded with the transitional phrase “comprising,” it is understood that we also contemplate the same composition or group of elements with transitional phrases “consisting essentially of,” “consisting of,” “selected from the group of consisting of,” or “is” preceding the recitation of the composition, element, or elements and vice versa.

[0203] While the present disclosure has been described with respect to a number of embodiments and examples, those skilled in the art, having benefit of this disclosure, will appreciate that other embodiments can be devised which do not depart from the scope and spirit of the present disclosure.

Claims

CLAIMSWhat is claimed is:

1. A method for preparing a terpolymer, comprising:introducing two or more different α-olefin monomers and an aluminum vinyl monomer to a first reaction zone;introducing a catalyst system to the first reaction zone to form a reaction mixture; polymerizing the reaction mixture to form a polymer mixture;transferring the polymer mixture from the first reaction zone to a second reaction zone;introducing a reagent to the second reaction zone, wherein the reagent comprises an oxygen containing reagent, a sulfur containing reagent, or a combination thereof; and reacting the polymer mixture with the reagent to form a polymer composition comprising the terpolymer.

2. The method of claim 1, wherein the aluminum vinyl monomer is represented by the formula:5wherein each R is independently a Ci-Cio hydrocarbyl, and n is an integer from 3 to 10.

3. The method of claim 3, wherein each R is isobutyl and n is an integer from 6 to 8.

4. The method of claim 1, wherein the α-olefin monomers are selected from the group consisting of ethylene, propylene, butene, pentene, hexene, heptene, octene, nonene, decene, undecene, dodecene, isomers thereof, and any combination thereof.

5. The method of claim 4, wherein(i) the α-olefin monomers comprise ethylene and propylene;(ii) the α-olefin monomers comprise ethylene and 1-hexene; or,(iii) the α-olefin monomers comprise ethylene and 1-octene.

6. The method of claim 1, wherein the monomer feed is substantially free of diene.2025EM073-WQ / 050930-08007. The method of claim 1, wherein the reagent comprises CO2, CS2, O2, O3, dry’ air, organic peroxide, or any combination thereof.

8. The method of claim 10, wherein the reagent(i) is selected from the group consisting of peroxy acetic acid, metachloroperoxybenzoic acid, and a combination thereof;(ii) is selected from the group consisting of O2, dry’ air, an organic peroxide, and any combination thereof; or(iii) is CS2.

9. The method of claim 1, wherein the catalyst system comprises a bis(phenolate) Lewis base catalyst compound that comprises a Group 4 transition metal, a tridentate dianionic ligand containing two anionic donor groups and a neutral heterocyclic Lewis base donor, wherein the heterocyclic donor is covalently bonded between the two anionic donors, and wherein the tridentate dianionic ligand coordinates to the metal with two anionic oxygen donors and one neutral heterocyclic nitrogen donor to form a pair of eight-membered metallocycle rings.

10. The method of claim 9, wherein the catalyst system comprises a catalyst compound represented by the formula:wherein:M is a Group 4 metal;each of E and E' is each independently O, S, or NRA, where RAis independently hydrogen, C1-C40 hydrocarbyl, substituted C1-C40 hydrocarbyl, or a heteroatom-containing group;each L is independently a Lewis base;X’ is independently an anionic ligand, C1-C40 hydrocarbyl. substituted C1-C40 hydrocarbyl, or a heteroatom-containing group;any two or more L groups are optionally joined together to form a poly dentate Lewis base;the X’ group are optionally joined to an L group to form a monoanionic bidentate group;n is 1, 2, or 3;m is 0, 1, or 2;n + m is 4 or less;each of R7, R8, R9, R10, R7, R8, R9, and R10is independently hydrogen, C1-C40 hydrocarbyl, substituted C1-C40 hydrocarbyl, a heteroatom or a heteroatom-containing group, or one or more of R7and R8, R8and R9, R9and R10, R7and R8, R8and R9, R9and R10are joined to form one or more substituted hydrocarbyl rings, unsubstituted hydrocarbyl rings, substituted heterocyclic rings, or unsubstituted heterocyclic rings each having 5, 6, 7, or 8 ring atoms; andeach of R11, R12, R13, R14, R11, R12, R13, R14, R15, R16, and R17is independently hydrogen, C1-C40 hydrocarbyl, substituted C1-C40 hydrocarbyl, a heteroatom or a heteroatomcontaining group, or one or more of R11and R12, R12and R13, R13and R14, R11and R12, R12and R13, R13and R14, R15and R16, or R16and R17are joined to form one or more substituted hydrocarbyl rings, unsubstituted hydrocarbyl rings, substituted heterocyclic rings, or unsubstituted heterocyclic rings each having 5, 6, 7, or 8 ring atoms.

11. The method of claim 10, wherein M comprises Hf or Zr, E and E’ is O, and R7and R7’ are independently a C1-C40 hydrocarbyl, substituted C1-C40 hydrocarbyl. or a heteroatomcontaining group.

12. The method of claim 10, wherein R7and R7’ are independently a C4-C40 tertiary hydrocarbyl group, or a C4-C40 cyclic tertiary hydrocarbyl group.

13. The method of claim 10, wherein the catalyst compound is represented by the formula:

14. The method of claim 1, wherein the catalyst system comprises an activator selected from the group consisting of dimethylanilinium tetrakis(pentafluorophenyl)borate, dimethy lanilinium tetraki s(heptafluoro-2-naphthalenyl)borate,N, N-di(hydrogenated tallow)methylammonium tetrakis(perfluorophenyl)borate,N, N-di (hydrogenated tallow)methylammonium tetrakis(heptafluoro-2-naphthalenyl)borate,N-methyl-4-nonadecyl-N-octadecylanilinium tetrakis(perfluorophenyl)borate,N-methyl-4-nonadecyl-N-octadecylanilinium tetrakis(heptafluoro-2-naphthalenyl)borate, N-methyl-N, N-dioctadecylammonium tetrakis(perfluorophenyl)borate,N-methyl-N, N-dioctadecylammonium tetrakis(heptafluoro-2-naphthalenyl)borate,N-methyl-N, N-dihexadecylammonium tetrakis(perfluorophenyl)borate,N-methyl-N, N-dihexadecylammonium tetrakis(heptafluoro-2-naphthalenyl)borate,N-methyl-N-octadecyl-4-(octadecyloxy)anilinium tetrakis(perfluorophenyl)borate,N-methyl-N-octadecyl-4-(octadecyloxy)anilinium tetrakis(heptafluoro-2-naphthalenyl)borate, and any combination thereof.

15. The method of claim 1, wherein the catalyst system is introduced to the first reaction zone at an input rate of about 0.1 mL / volume / min to about 2.5 mL / volume / min.

16. The method of claim 1, wherein the aluminum vinyl monomer is introduced to the first reaction zone at an input rate of about 0.01 mL / volume / min to about 4 mL / volume / min.

17. The method of claim 16, wherein as the aluminum vinyl monomer input rate is increased(i) the complex viscosity (r]*o.oi) at 150°C of the polymer composition comprising the terpolymer increases;(ii) the shear elastic modulus (G’o.oi) at 150°C of the polymer composition comprising the terpolymer increases; or,(iii) the strain hardening ratio at 150°C of the polymer composition comprising the terpolymer increases.

18. The method of claim 1, wherein the two or more different a-olefm monomers and the aluminum vinyl monomer are continuously introduced to the first reaction zone.

19. The method of claim 1, wherein the second reaction zone is substantially free of one or more of water, alcohols, salts of alcohols, organic acids, or inorganic acids.

20. The method of claim 1, wherein the polymer composition comprises about 50 wt% or less of ethylene.

21. The method of claim 20, wherein the polymer composition comprises about 18 wt% or less of ethylene.

22. The method of claim 1, wherein the polymer composition a compositional weight ratio of ethylene to propylene of about 1:99 to about 35:65.

23. The method of claim 1, wherein the polymer composition has an ethylene content of 25 wt% or less, a complex viscosity (T]*O. OI) of about 100 kPa*s or more at 150°C, a shear elastic modulus (G’o.oi) of about 300 Pa or more at 150°C, and a strain hardening ratio greater than 1.1 at 150°C.

24. A polymer composition comprising a terpolymer, wherein the terpolymer comprises ethylene, propylene, and an aluminum vinyl monomer that has reacted with an oxygen containing reagent, wherein the terpolymer comprises:an ethylene content of 25 wt% or less;a complex viscosity (i]*o.oi) of about 100 kPa*s or more at 150°C;a shear elastic modulus (G’o.oi) of about 300 Pa or more at 150°C; anda strain hardening ratio greater than 1.1 at 150°C.

25. The polymer composition of claim 24, wherein the ethylene content of the terpolymer is 18 wt% or less.

26. The polymer composition of claim 24, wherein the strain hardening ratio of the terpolymer is greater than 1.5 at 150°C.