Two-dimensional pillared catalyst materials for plastic recycling

Pillared MXene and metal oxide catalysts address the low surface area and porosity issues of conventional catalysts by enhancing polymer-catalyst contact and mass transport, achieving efficient hydrogenolysis of plastic waste into valuable products.

WO2026241519A2PCT designated stage Publication Date: 2026-11-19LUO SONG +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/US2026/028186
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-14
Filing Date
2026-05-14
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Conventional catalysts for hydrogenolysis of polyolefins, such as Ru-based catalysts supported on TiO2, ZrO2, CeO2, and carbon, suffer from low surface areas and porosities, limiting their effectiveness in recycling plastic waste due to polymer-catalyst contact and mass transport issues, especially with high molecular weight polymers.

Method used

Development of two-dimensional (2D) MXene-based catalyst materials with pillared structures, comprising MXene sheets and interlayer pillars, which enhance porosity and surface area, and metal oxide-based catalysts with similar structures, to improve hydrogenolysis efficiency.

Benefits of technology

The pillared MXene and metal oxide materials exhibit improved porosities, higher surface areas, enhanced metal dispersion, and catalytic activities, facilitating efficient hydrogenolysis of plastic waste into valuable fuels and chemicals, overcoming the limitations of conventional catalysts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure US2026028186_19112026_PF_FP_ABST
    Figure US2026028186_19112026_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed herein are two-dimensional catalyst materials possessing pillared structures between MXene sheets and derived metal oxide-based sheets for use in plastic recycling processes. Methods for preparaing these catalyst materials are also disclosed.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] 2101715-001365

[0002] -1- TWO-DIMENSIONAL PILLARED CATALYST MATERIALS FOR PLASTIC RECYCLING

[0003] CROSS-REFERENCE TO RELATED APPLICATION

[0004] This application claims priority to U.S. Provisional Patent Application No. 63 / 805,614 filed on May 14, 2025, and U.S. Provisional Patent Application No. 64 / 041,321 filed on April 16, 2026, the contents of which are incorporated herein by reference in their entireties for all purposes.

[0005] STATEMENT REGARDING FEDERALLY SPONSORED RESEARCH

[0006] This invention was made with government support under DE-SC0021166 awarded by the U.S. Department of Energy, Office of Science, Basic Energy Sciences. The Government has certain rights in the invention.

[0007] FIELD

[0008] The present disclosure relates to two-dimensional catalyst materials possessing pillared structures for use in plastic recycling processes. Methods for preparaing these catalyst materials are also disclosed.

[0009] BACKGROUND

[0010] Since their inception in the early 1900s, synthetic plastics have evolved rapidly to become indispensable to modern life. Polyolefins, such as polyethylene (PE) and polypropylene (PP), are thermoplastics that dominate the plastics market due to their simple yet versatile structures, offering qualities like high strength to weight ratios, transparency, and durability. However, the durability that serves as a strength of polyolefins is also a disadvantage as they are difficult to depolymerize or decompose. In 2015, over 150 million metric tons (Mt) of polyolefin waste were generated, constituting half of total plastic waste produced globally. This contributes to severe effects on the environment and human health. For example, the slow decomposition of plastics leads to the formation of environmentally persistent microplastic particles that infiltrate terrestrial and aquatic environments, thus negatively impacting these ecosystems. The formation of microplastics also poses a threat to human health through bioaccumulation in the food chain, which can increase the risk of cardiovascular or respiratory diseases. Furthermore, uncontrolled incineration of plastic waste leads to release of toxic gases and2101715-001365

[0011] -2-particulate matter, ultimately impacting air quality and the climate through radiative forcing which increases air pollution and greenhouse gas emissions, thereby escalating climate change and increasing the frequency of natural disasters.

[0012] Public awareness and concern over the above impacts of plastic waste have spurred efforts towards plastics recycling. Practices such as mechanical grinding, melt filtration, extrusion, and pelletization have been implemented to produce resins from plastic waste for secondary manufacturing. Despite these efforts, it is anticipated that by 2050, of the cumulative about 33 x 1 o3Mt of plastic waste, only 8.5 x 103Mt of plastics will be recycled while 12.4 x 103Mt will be incinerated for energy recovery. The remaining 12.3 x 103Mt of plastic waste will end up in landfills and thus pose both environmental and human health risks.

[0013] Chemical upcycling methods such as pyrolysis, gasification, solvolysis, cracking, and hydrogenolysis are promising alternative practices for plastic waste recycling as higher mass fractions of plastics can be converted to valuable fuels and chemicals. Of these methods, hydrogenolysis shows a great potential for upgrading waste polyolefins to valued fuels and chemicals of C5-35 under mild conditions (e.g., 200 °C to 250 °C, 1.0 - 3.0 megapascal (MPa) H2), possibly creating a circular lifecycle of synthetic plastics.

[0014] Hydrogenolysis is a catalytic process that cleaves single bonds (e.g., C-C, C-O, C-N, and C-S) using hydrogen to produce two smaller molecules. This process involves the activation of a substrate (e.g., a plastic waste or plastic polymer) and hydrogen on a catalyst surface. Conventional supported metal catalysts containing metals such as Pt, Ni, Co, Ru, and Rh, have been explored for the hydrogenolysis of polyolefins. Among these, Ru-based catalysts have shown superior performance due to a lower activation energy barrier for the rate-determining C-C bond scission step. Common supports for Ru particles include TiOs, ZrOs, CeCh, and carbon. Unfortunately, these catalysts often suffer from low surface areas and / or porosities, which limit their effectiveness due to polymer-catalyst contact and mass transport issues, especially with high molecular weight polymers, such as those present in plastic waste.

[0015] Given the various drawbacks associated with conventional hydrogenolysis catalyst materials, the discovery of new and improved catalytic materials would be2101715-001365

[0016] -3-of great interest to those concerned with reducing pollution and environmental hazards caused by waste plastics.

[0017] MXene materials have recently emerged as promising new catalytic materials. MXenes are two-dimensional (2D) transition-metal carbide and nitride materials with the general formula Mn+ iXnTx, where M is an early transition metal, n = 1 , 2, or 3, X is C and / or N, and Txare surface functional groups (e.g., -O, -OH and / or -F groups). These materials are derived from a parental MAX phase, where A is an A-group element mostly from group 13 and 14 in the periodic table, by selectively etching the A layer as M-X bonds are stronger and less prone to breaking than M-A bonds. MXenes have garnered increasing attention due to their versatile composition, structure, and numerous physicochemical properties. Their electrical conductivity and tunable bandgap, for example, have enabled applications in areas such as energy storage, electrocatalysis, and photocatalysis. Though these materials have seen effective use in various areas, the use of MXenes as catalysts in conventional heterogeneous reactions (e.g., those used in plastic waste recycling) is largely underexplored.

[0018] SUMMARY

[0019] One aspect of the present disclosure is a first catalyst material including (i.e., comprising) (i) at least two MXene sheets, each sheet having a chemical composition according to the following formula Mn+ iXnTx, wherein: M is a transition metal, n is an integer ranging from 1 to 3, X is carbon (C) or nitrogen (N), and Txis a surface functional group; and (ii) an interlayer space residing between the two MXene sheets, wherein the interlayer space comprises one or more pillar structures.

[0020] Another aspect of the present disclosure is a second catalyst material including (i) at least two metal oxide sheets, each sheet having a chemical composition according to the following formula Mn+ iOm(n+i)Xn-aTx, wherein M is a transition metal, n is an integer ranging from 1 to 3, m is an integer ranging from 0 to 2, X is carbon (C) or nitrogen (N), a is an integer ranging from 0 to 2, and Txis a surface functional group; and (ii) an interlayer space residing between the at least two metal oxide sheets, the interlayer space including one or more pillar structures.2101715-001365

[0021] -4- Another aspect of the present disclosure is a method for hydrogenating a plastic waste composition that includes subjecting the plastic waste composition to a hydrogenolysis reaction, wherein the hydrogenolysis reaction occurs in the presence of one or more of the catalyst materials disclosed herein.

[0022] Another aspect of the present disclosure is a method for producing the first catalyst material, wherein the method includes one or more of: intercalating one or more pillar precursors between the at least two MXene sheets and / or hydrolyzing the one or more pillar precursors between the at least two MXene sheets into the one or more pillars structures.

[0023] Another aspect of the present disclosure is a method for producing the second catalyst material, the method including one or more of: calcining a P-MXene material at a temperature ranging from about 250°C to about 550°C, wherein the P-MXene material contains an interlayer space residing between two MXene sheets, the interlayer space including one or more pillar structures.

[0024] BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Other features and advantages of the compositions, devices and methods disclosed herein will be apparent to those skilled in the art reading the following detailed description in conjugation with the exemplary embodiments illustrated in the drawings, wherein:

[0026] FIG. 1 depicts SEM images showing morphologies of a MAX (a) and a MXene (b) material of Example 1 , along with their N2 adsorption / desorption isotherms (c) and XRD patterns (d), respectively.

[0027] FIG. 2 depicts the pore width distribution and cumulative pore volume of the MAX (a) and the MXene (b) materials of Example 1 using the HK method.

[0028] FIG. 3 depicts aTEM image of exemplary 2D MXene layers with an average layer thickness of 0.9 nm.

[0029] FIG. 4 depicts the pore width distribution and cumulative pore volume of a 3.0% Ru-loaded MXene catalyst material (Ru@MXene) using the HK method.

[0030] FIG. 5 depicts the pore width distribution and cumulative pore volume of a 5.0% Ru-loaded MXene catalyst material (Ru@MXene) using the HK method.

[0031] FIG. 6 depicts the pore width distribution and cumulative pore volume of a 7.0% Ru-loaded MXene catalyst material (Ru@MXene) using the HK method.2101715-001365

[0032] -5- FIG. 7 depicts the Ru particle size distribution histograms for different Ru mass fractions (3.0 % (a), 5.0 % (b) and 7.0 % (c)) in Ru@MXene catalysts.

[0033] FIG. 8 depicts H2-TPR profiles of exemplary Ru@MXene catalysts with different Ru loadings.

[0034] FIG. 9 depicts Ru 3d / C 1s XPS spectra of exemplary Ru@MXene catalysts with different Ru loadings.

[0035] FIG. 10 depicts the conversion and yield of different phases (a), and C1-C35 yield (b) in a LDPE hydrogenolysis over bare MXene (24 h) and 5.0 % Ru@MXene (6 h) catalysts. Reaction conditions: LDPE-to-catalyst mass ratio of 20, 250 °C, and 3.0 MPa H2.

[0036] FIG. 11 depicts a representative GC-FID trace characterizing the distribution of soluble products from a LDPE hydrogenolysis over 5.0 % Ru@MXene. Reaction conditions: LDPE-to-catalyst mass ratio of 20, 250 °C, 6 h, and 3.0 MPa H2.

[0037] FIG. 12 depicts the conversion and yield of different phases (a), and C1-C35 yield (b) of a LDPE hydrogenolysis over 5.0 % Ru@MXene catalyst at different reaction temperatures.

[0038] FIG. 13 depicts the conversion and yield of different phases (a), and C1-C35 yield (b) of a LDPE hydrogenolysis over 5.0 % Ru@MXene catalyst at different reaction times.

[0039] FIG. 14 depicts the conversion and yield of different phases (a), and C1-C35 yield (b) of a LDPE hydrogenolysis over 5.0 % Ru@MXene catalyst at different H2 pressures.

[0040] FIG. 15 depicts the conversion and yield of different phases (a), and C1-C35 yield (b) of a LDPE hydrogenolysis over different Ru mass fractions in the Ru@MXene catalysts. Reaction conditions: LDPE-to-catalyst mass ratio of 20, 4 h, 250 °C, and 3.0 MPa H2.

[0041] FIG. 16 depicts the conversion and yield of different phases (a), and C1-C35 yield (b) of a LDPE hydrogenolysis over commercial 5.0 % Ru / C (4 h), 5.0 % Ru@MXene (6 h), and 5.0 % Ru@P-MXene (0.5 h) catalysts. Reaction conditions: LDPE-to-catalyst mass ratio of 20, 250 °C, and 3.0 MPa H2.

[0042] FIG. 17 depicts the conversion and yield of different phases (a), and C1-C35 yield (b) of a LDPE hydrogenolysis over commercial 5.0 % Ru / C catalyst at 1 h, 2 h2101715-001365

[0043] -6-and 4 h. Reaction conditions: LDPE-to-catalyst mass ratio of 20, 250 °C, and 3.0 MPa H2.

[0044] FIG. 18 depicts the conversion and yield of different phases (a), and C1-C35 product yields (b) of a LDPE hydrogenolysis at different reaction conditions (Condition #1 : 2 h, 280 °C, 3.0 MPa H2, Condition #2: 6 h, 250 °C, 3.0 MPa H2, Condition #3: 2 h, 250 °C, 6.0 MPa H2. These three conditions were performed with 5.0 % Ru@MXene; Condition #4: 4 h, 250 °C, 3.0 MPa H2, with 7.0 % Ru@MXene, and Condition #5: 0.5 h, 250 °C, 3.0 MPa H2with 5.0 % Ru@P-MXene. In all reaction conditions LDPE-to-catalyst mass ratio was 20).

[0045] FIG. 19 depicts the conversion and yield of different phases (a), and C1-C35 yield (b) of a LDPE hydrogenolysis over 5.0 % Ru@P-MXene (0.25 h) and 5.0 % Ru@MXene (4 h) catalysts at different reaction times. Reaction conditions: LDPE-to-catalyst mass ratio of 20, 250 °C, and 3.0 MPa H2.

[0046] FIG. 20 depicts the SEM (a), TEM (b), XRD (c), and N2isotherm (d) data of a P-MXene sample.

[0047] FIG. 21 depicts the pore width distribution and cumulative pore volume of an exemplary pillarized MXene material (P-MXene) using the HK method.

[0048] FIG. 22 depicts the pore width distribution and cumulative pore volume of an exemplary P-MXene loaded with 5% Ru using the HK method.

[0049] FIG. 23 depicts the conversion and yield of different phases (a), and C1-C35 yield (b) of a LDPE hydrogenolysis over 5.0 % Ru@P-MXene at different reaction times. Reaction conditions: feed-to-catalyst mass ratio of 20, 250 °C, and 3.0 MPa H2.

[0050] FIG. 24 depicts the conversion and yield of different phases (a), and C1-C35 yield (b) of a PE hydrogenolysis with different molecular weights (4 KDa and 76 KDa) over 5.0 % Ru@MXene (2 h) catalyst. Reaction conditions: LDPE-to-catalyst mass ratio of 20, 250 °C, and 3.0 MPa H2.

[0051] FIG. 25 depicts the conversion and yield of different phases (a), and C1-C35 yield (b) of a PE hydrogenolysis with different molecular weights (4 KDa and 76 KDa) over 5.0 % Ru@P-MXene (0.5 h) catalyst. Reaction conditions: LDPE-to-catalyst mass ratio of 20, 250 °C, and 3.0 MPa H2.2101715-001365

[0052] -7- FIG. 26 depicts the elemental mapping (EDS) spectra of elements over (a) MAX, MXene and P-MXene, and (b) 5.0 % Ru@MXene, and 5.0 % Ru@P-MXene materials.

[0053] FIG. 27 depicts theXPS spectra of (a) MAX, MXene, and P-MXene, (b) 5.0 % Ru@MXene, and 5.0 % Ru@P-MXene materials.

[0054] FIG. 28 depicts XRD patterns of 5.0 % Ru@MXene (a) and 5.0 % Ru@P-MXene (b) samples before and after hydrogenolysis of LDPE.

[0055] FIG. 29 depicts XRD data of exemplary C-P-TiO2 and P-TiO2 materials. FIG. 30 depicts SEM images of exemplary C-P-TiO2 (a) and P-TiO2 (b) materials, and a TEM image of the P-TiO2 (c) material. The region highlighted with a dashed circle in (c) indicates the presence of silica pillars.

[0056] FIG. 31 depicts the N2 adsorption-desorption isotherms of exemplary P-TiO2 and C-P-TiO2 materials.

[0057] FIG. 32 depicts the pore size distributions and accumulative pore volumes of exemplary P-TiO2 and C-P-TiO2 materials.

[0058] FIG. 33 depicts the conversion and product selectivity (a) and product yield distribution (b) of a LDPE hydrogenolysis over exemplary Ru@P-TiC>2 and Ru@C-P-TiO2 catalysts. Reaction conditions: 250 °C, 30 bar H2, LDPE feed / catalyst mass ratio = 20. The reaction time for both catalysts was controlled at 30 min.

[0059] FIG. 34 depicts a schematic of an exemplary vapor phase pillarization (VPP) process.

[0060] FIG. 35 depicts the Raman spectra of exemplary MAX, MXene and P-MXene materials. P-MXene synthesis condition: MXene / DDA / TEOS / F = 1:10:0.5:10 (mass ratio), intercalation at 100 °C, hydrolysis at 80 °C.

[0061] FIG. 36 depicts XRD data of exemplary MAX, MXene and P-MXene materials. P-MXene synthesis condition: MXene / DDA / TEOS / F = 1:10:0.5:10 (mass ratio), intercalation at 100 °C, hydrolysis at 80 °C.

[0062] FIG. 37 depicts SEM images of exemplary MXene (a) and P-MXene (b) materials. TEM images of the exemplary MXene (c) and P-MXene (d) are also shown. The regions highlighted with dashed circles in (d) indicate the presence of silica pillars. P-MXene synthesis condition: MXene / DDA / TEOS / F = 1 :10:0.5:10 (mass ratio), intercalation at 100 °C, hydrolysis at 80 °C.2101715-001365

[0063] -8- FIG. 38 depicts the N2 adsorption-desorption isotherms (a, b) and the corresponding pore size distributions (c, d) of exemplary MXene and P-MXene materials. P-MXene synthesis condition: MXene / DDA / TEOS / F = 1:10:0.5:10 (mass ratio), intercalation at 100 °C, hydrolysis at 80 °C.

[0064] FIG. 39 depicts the textural properties of an exemplary P-MXene material prepared by a VPP process as a function of DDA loading during intercalation, (a) depicts the surface area of exemplary P-MXene material prepared via a VPP process, the surface area being partitioned into micro- and meso-contributions; (b) depicts the corresponding micro-, meso-, and macropore volumes. Samples were synthesized at DDA: MXene mass ratios of 0, 5, 10, and 20. Synthesis conditions: MXene / TEOS / H2O = 1:0.5:10 (mass ratio), intercalation at 100 °C, hydrolysis at 80 °C.

[0065] FIG. 40 depicts the textural properties of an exemplary P-MXene prepared by VPP as a function of TEOS loading during intercalation, (a) depicts the surface area of the P-MXene material partitioned into micro- and meso-contributions; (b) depicts corresponding micro-, meso- and macropore volumes. Samples were synthesized atTEOS:MXene mass ratios of 0.1, 0.5, 1, and 20. Synthesis conditions: MXene / DDA / FhO = 1 :10:10 (mass ratio), intercalation at 100 °C, hydrolysis at 80 °C.

[0066] FIG. 41 depicts the textural properties of an exemplary P-MXene material prepared by a VPP process as a function of water loading during hydrolysis, (a) depicts the surface area of the P-MXene material partitioned into micro- and meso-contributions; (b) depicts corresponding micro-, meso- and macropore volumes. Samples were synthesized at water: MXene mass ratios of 0, 10, and 20. Synthesis conditions: MXene / TEOS / DDA = 1:0.5:10 (mass ratio), intercalation at 100 °C, hydrolysis at 80 °C.

[0067] FIG. 42 depicts the textural properties of an exemplary P-MXene prepared by a VPP process with different swelling agents (HA, DDA, or ODA) during intercalation, (a) depicts the surface area of the P-MXene material partitioned into micro- and meso-contributions; (b) depicts corresponding micro-, meso- and macropore volumes. Synthesis condition: MXene / DDA / TEOS / H2O = 1:10:0.5:102101715-001365

[0068] -9- (mass ratio), intercalation at 100 °C, hydrolysis at 80 °C; for HA and ODA, the molar numbers were controlled the same as DDA.

[0069] FIG. 43 depicts the textural properties of an exemplary P-MXene prepared by a VPP process as a function of TEOS loading during intercalation, (a) depicts the surface area of the P-MXene material partitioned into micro- and mesocontributions; (b) depicts corresponding micro-, meso- and macropore volumes. Samples were synthesized at TEOS:MXene mass ratios of 1 .6, 3.2, 6.4, 10, and 20. Synthesis conditions: MXene / DDA / H2O = 1:0.8:10 (mass ratio), intercalation at 100 °C, hydrolysis at 80 °C.

[0070] FIG. 44 depicts the textural properties of an exemplary P-MXene material prepared by a VPP process as a function of temperature during intercalation, (a) depicts the surface area of the P-MXene material partitioned into micro- and mesocontributions; (b) depicts corresponding micro-, meso- and macropore volumes. Synthesis conditions: MXene / TEOS / DDA / H2O = 1:6.4:0.8:10 (mass ratio), intercalation at 80, 100, 130, or 170 °C, hydrolysis at 80 °C.

[0071] FIG. 45 depicts a schematic illustration of stacked MXene layers with low porosity between layers after freeze drying (a) and with hierarchical wedge-like pores between layers after a VPP pillarization process (b).

[0072] FIG. 46 depicts XRD data of an exemplary P-MXene material after thermal and hydrothermal treatments. P-MXene synthesis condition:

[0073] MXene / DDA / TEOS / H2O = 1:10:0.5:10 (mass ratio), intercalation at 100 °C, hydrolysis at 80 °C. Thermal treatment was performed under 500 °C under N2 (100 mL / min) for 24 h, while hydrothermal treatment was carried out under 500 °C under Ar (50 mL / min) for 24 h with 2 wt.% steam.

[0074] FIG. 47 depicts the textural properties of an exemplary P-MXene, and an exemplary P-MXene after thermal and hydrothermal treatments, (a) depicts the surface area of the P-MXene material partitioned into micro- and mesocontributions; (b ) depicts corresponding micro-, meso- and macropore volumes. P-MXene synthesis condition: MXene / DDA / TEOS / H2O = 1:10:0.5:10 (mass ratio), intercalation at 100 °C, hydrolysis at 80 °C. Thermal treatment was performed under 500 °C under N2 (100 mL / min) for 24 h, while hydrothermal treatment was carried out under 500 °C under Ar (50 mL / min) for24 h with 2 wt.% steam.2101715-001365

[0075] -10- FIG. 48 depicts the conversion and product selectivity (a) and product yield distribution (b) of a LDPE hydrogenolysis over Ru@MXene and Ru@P-MXene catalysts. Reaction conditions: 250 °C, 30 bar H2, LDPE feed / catalyst mass ratio = 20. The reaction time for Ru@MXene and Ru@P-MXene was 2 and 0.5 h, respectively. P-MXene synthesis condition: MXene / DDA / TEOS / FLO = 1:10:0.5:10 (mass ratio), intercalation at 100 °C, hydrolysis at 80 °C.

[0076] DETAILED DESCRIPTION

[0077] All publications, patent applications, patents, and other references mentioned herein are incorporated by reference in their entirety. Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention belongs. In case of conflict, the present specification, including definitions, will control.

[0078] Unless stated otherwise, all percentages, parts, ratios, etc., are by weight. As used herein, the term “exemplary embodiments” refers to specific examples or embodiments of any of the aspects disclosed herein that serve as illustrations to demonstrate the various ways in which the various aspects can be implemented, constructed or practiced.

[0079] When an amount, concentration, or other value or parameter is given as either a range, preferred range or a list of upper preferable values and lower preferable values, this is to be understood as specifically disclosing all ranges formed from any pair of any upper range limit or preferred value and any lower range limit or preferred value, regardless of whether ranges are separately disclosed. Where a range of numerical values is recited herein, unless otherwise stated, the range is intended to include the endpoints thereof, and all integers and fractions within the range. It is not intended that the scope of the invention be limited to the specific values recited when defining a range.

[0080] As used herein, the term “about” refers to a value that is ± 5% of the stated value. In addition, it is understood that reference to a range of a first value to a second value includes the range of the stated values, e.g., a range of about 1 to about 5 also includes the more precise range of 1 to 5. It is also understood that the ranges disclosed herein include any selected subrange within the stated range,2101715-001365

[0081] -11-e.g., a subrange of about 50 to about 60 is contemplated in a disclosed range of about 1 to about 100.

[0082] The present disclosure details the surprising discovery that pillared MXene and pillared metal oxide-based materials can exhibit improved porosities, higher surface areas, enhanced metal dispersion, catalytic activities, stabilities and molecular transport properties when compared to conventional catalyst materials. Without being bound to any theory, a possible explanation for the improved properties of the materials disclosed herein is their unique 2D structures. The 2D structures can serve as precursor materials for the fabrication of pillared structures, in which pillars are inserted between adjacent MXene layers to expand the interlayer spacing and generate mesoporous gallery channels. Such nanoengineering can increase the surface area of the support, improve the transport of bulky species during metal catalyst loading and reaction processes, and mitigate the spatial limitations commonly associated with conventional catalyst supports. Furthermore, the pillared MXene materials disclosed herein can serve as precursors for the synthesis of other pillared 2D materials, such as metal oxides and hybrid 2D metal oxide-carbon structures, through appropriate post- treatment strategies. Various exemplary embodiments of these materials are discussed below.

[0083] One aspect of the present disclosure is a first catalyst material including (i) at least two MXene sheets, each sheet having a chemical composition according to the following formula Mn+ iXnTx, wherein: M is a transition metal, n is an integer ranging from 1 to 3, X is carbon (C) or nitrogen (N), and Tx is a surface functional group; and (ii) an interlayer space residing between the two MXene sheets, wherein the interlayer space comprises one or more pillar structures.

[0084] The transition metal (M) of the MXene sheets can be selected from any transition metal, such as but not limited to, scandium, yttrium, lanthanum, actinium, titanium, zirconium, hafnium, vanadium, niobium, tantalum, chromium, molybdenum, tungsten or any combinations thereof. In exemplary embodiments, at least one of the MXene sheets contains two or more transition metals, e.g., a TiVCTx MXene sheet.2101715-001365

[0085] -12- The Txsurface functional group of the MXene sheets can be selected from, but is not limited to, -O’, -OH, a halogen (e.g., -Cl, -Br, -F) or an amine.

[0086] In exemplary embodiments, the interlayer space of the first catalyst material has a thickness ranging from about 1.0 nm to about 100 nm or higher, about 1.0 nm to about 90 nm, about 1.0 nm to about 80 nm, about 1.0 nm to about 70 nm, about 1.0 nm to about 60 nm, about 1 .0 nm to about 50 nm, about 1.0 nm to about 40 nm, about 1.0 nm to about 30 nm, about 1.0 nm to about 20 nm, about 1.0 nm to about 10 nm, or 3.0 nm to about 5.0 nm.

[0087] In exemplary embodiments, the one or more pillar structures of the first catalyst material contain metal species, inorganic oxide species, ionic species, and / or organic species. The pillar structures can be composed of only one type of metal species, inorganic oxide species, ionic species, and / or organic species, be composed of combinations of different metal species, inorganic oxide species, ionic species, or organic species, or be composed of different metal species, inorganic oxide species, ionic species, and organic species. In exemplary embodiments, at least one of the pillar structures is bimetallic, trimetallic or multiple metallic alloy materials. The metal species can include, but are not limited to, Ru, Ni, Ag, Au, Pt, Pd, Fe, Co, Cu, Ir, Rh, Os. The inorganic oxide species can include, but are not limited to, SiO2, SnO2, TiO2, CoFe2O4, C03O4, FesO4, AI2O3, CeO2, GeOx (amorphous germanium oxide), PdO, and Ag2O. The ionic species can include, but are not limited to, alkali metal ions (e.g., Li+, Na+, K+, Cs+), divalent / trivalent ions (e.g., Mg2+, Ca2+, Fe2+, Al3+, Zn2+, Cu2+) and ionic surfactants (e.g., cetyltrimethylammonium bromide (CTAB) and alkylammonium cations). The organic species can include, but are not limited to, small organic molecules (e.g., isopropyl amine, DMSO, tetrabutylammonium hydroxide (TBAOH), hydrazine), aromatic compounds (e.g., 1,4-benzenediol (HQ), 1,4-benzenedithiol (Th), 1,4-phenylenediamine (PPD)), polymers (e.g., polypyrrole, polyaniline, and 3,4-ethylenedioxythiophene (EDOT)), and amino acids.

[0088] In exemplary embodiments, at least one of the one or more pillar structures located within the interlayer space of the first catalyst material contains metallic particles or alloys. The metallic particles can be, but are not limited to, any of the transition metals belonging to Period 4, Period 5 or Period 6 of the Periodic T able,2101715-001365

[0089] -13-e. g. , iron (Fe) particles, cobalt (Co) particles, nickel (Ni) particles, copper (Cu) particles, chromium (Cr) particles, manganese (Mn) particles, ruthenium (Ru) particles, rhodium (Rh) particles, palladium (Rd) particles, silver (Ag) particles, platinum (Pt), palladium (Pd), gold (Au) particles, iridium (Ir) particles, or combinations thereof. The metallic alloys can possess metals selected from, but not limited to, Fe, Co, Ni, Cu, Cr, Mn, Ru, Rh, Pd, Ag, Pt, Pd, Au, Ir, molybdenum (Mo), aluminum (Al), tin (Sn), vanadium (V), zinc (Zn), antimony (Sb), and bismuth (Bi).

[0090] In exemplary embodiments, the metallic particles of the first catalyst material possess an average particle size ranging from about 0.2 nm to about 1.5 nm or higher, about 0.5 nm to about 50 nm, about 0.5 nm to about 40 nm, about 0.5 nm to about 30 nm, about 0.5 nm to about 20 nm, about 0.5 nm to about 10 nm, about 0.5 nm to about 5 nm, about 0.5 nm to about 1.5 nm, or about 0.5 nm to about 0.8 nm.

[0091] In exemplary embodiments, one or more of the pillar structures located within the interlayer space residing between the two MXene sheets of the first catalyst material is loaded with or contains one or more metallic particles or metallic alloys in an amount, based on the total weight of the first catalyst material, ranging from about 0.01 wt% to about 50 wt%, at least 3 wt%, from about 3 wt% to about 10 wt%, from about 3 wt% to about 50 wt%, from about 10 wt% to about 50 wt%, from about 20 wt % to about 40 wt%, or at most 50 wt%. The metallic particles or metallic alloys can be selected from any one or more of the metallic particles or metallic alloys disclosed herein.

[0092] In exemplary embodiments, the first catalyst material possesses metallic particles or alloys within the interlayer space in an amount, based on the total weight of the first catalyst material, ranging from about 0.01 wt% to about 50 wt%, from about 3 wt% to about 10 wt%, from about 3 wt% to about 50 wt%, from about 10 wt% to about 50 wt%, from about 20 wt % to about 40 wt%, or at most 50 wt%.

[0093] In exemplary embodiments, the first catalyst material is characterized by a small angle X-ray diffraction (SAXS) pattern having peaks at 6.2 to 5.6° 26 or lower. In other exemplary embodiments, the first catalyst material is characterized by a SAXS pattern having a peak at about 2.0° 20 or lower. In exemplary embodiments,2101715-001365

[0094] -14-the first catalyst material is characterized by an X-ray diffraction (XRD) pattern having peaks at about 8.2° and about 6.7° 29.

[0095] SAXS is a powerful, non-destructive technique that analyzes elastic X-ray scattering at very small angles (0.1 to 10°) to determine the nanoscale structure, size, shape, and distribution of particles or materials (e.g., those ranging from 1-100nm). This technique can be applied to various materials — liquids, solids, gels, and powders — without needing crystallization or high vacuum, providing bulk-averaged data.

[0096] XRD is a non-destructive analytical technique used to identify the atomic and molecular structure of materials (e.g., crystalline materials). By bombarding a sample with X-rays and measuring the diffraction angles and intensities, this technique can determine phase composition, crystallinity, crystal strain, and the periodic atomic arrangement of a material.

[0097] In exemplary embodiments, the first catalyst material is characterized by a d-spacing of 1 nm or higher or about 1 nm to about 100 nm, as determined by a SAXS pattern. In exemplary embodiments, the first catalyst material is characterized by a d-spacing of about 0.8 nm to about 2.0 nm or higher, or about 1.4 nm to about 1.6 nm or higher, as determined by a SAXS pattern. In other exemplary embodiments, the first catalyst material is characterized by a d-spacing of about 4.0 nm or higher, as determined by a SAXS pattern.

[0098] In exemplary embodiments, at least one of the MXene sheets of the first catalyst material has an average layer thickness above 1.5 nm or ranging from about 0.5 nm to about 1.5 nm, about 0.7 nm to about 1.5 nm, about 0.5 nm to about 1.2 nm, or about 0.5 nm to about 0.7 nm.

[0099] In exemplary embodiments, the first catalyst material is characterized by a H3-type hysteresis loop at relative pressures (P / Po) of at least 0.5 or ranging between 0.4 to 0.8, as determined by a N2 adsorption / desorption isotherm. In other exemplary embodiments, the first catalyst material is characterized by a H2-type hysteresis loop at P / Poof 0.4 to 0.9, as determined by a N2 adsorption / desorption isotherm. In other exemplary embodiments, the first catalyst material is characterized by a H4-type hysteresis loop at P / Pogreater than 0.8, as determined by a N2 adsorption / desorption isotherm. N2 adsorption / desorption isotherms are a2101715-001365

[0100] -15-critical analysis technique used at 77 K (liquid nitrogen temperature) to determine the surface area, pore size, and pore volume of materials, particularly powders and porous catalysts. This technique involves measuring the volume of N2 gas adsorbed onto a material as the relative pressure (P / Po) increases, then desorbed as pressure decreases, revealing information about the pore structure through hysteresis loops, often analyzed using BET (Brunauer-Emmett-Teller) and BJH (Barrett-Joyner-Halenda) models.

[0101] The BET model is based on a fundamental theory used in physical chemistry to determine the specific surface area of materials by measuring physical gas adsorption. This model extends the Langmuir model to account for multilayer adsorption, allowing for the calculation of the total surface area, including pores, of powders and porous solids using inert gas (typically N2) at cryogenic temperatures. The BJH model is a widely used method in materials science to determine the poresize distribution of porous materials, typically targeting mesopores (2-50 nm) based on N2 adsorption / desorption isotherms. This model applies the Kelvin equation to calculate pore volumes by analyzing capillary condensation and evaporation within the pores, assuming a cylindrical pore model.

[0102] In exemplary embodiments, the first catalyst material possesses a BET surface area ranging from about 30 m2 / g to about 800 m2 / g, about 50 m2 / g to about 800 m2 / g, about 50 m2 / g to about 600 m2 / g, about 50 m2 / g to about 400 m2 / g, about 100 m2 / g to about 400 m2 / g, or about 300 m2 / g to about 500 m2 / g.

[0103] In exemplary embodiments, the first catalyst material possesses a BET surface area that is at least three times higher than a BET surface area of the catalyst material without the one or more pillar structures residing within the interlayer space.

[0104] In exemplary embodiments, the first catalyst material is characterized by a pore-width distribution having a peak at 0.6 nm, as determined by a N2 adsorption / desorption isotherm and the Horvath-Kawazoe (HK) method. The HK method is a semi-empirical model used to calculate the pore size distribution (PSD) of microporous materials, specifically graphitic slit-shaped pores, from adsorption isotherms. This method calculates pore size by relating the relative pressure of2101715-001365

[0105] -16-adsorption to the potential energy interaction between the adsorbate molecules and the pore walls.

[0106] In exemplary embodiments, the first catalyst material is characterized by a mesopore size distribution of about 5 nm to about 35 nm, as determined by a N2 adsorption / desorption isotherm.

[0107] In exemplary embodiments, the first catalyst material is characterized by a H2-TPR profile having distinct reduction peaks at about 340 °C and about 520 °C. In other exemplary embodiments, the first catalyst material is characterized by a H2-TPR profile having distinct reduction peaks at about 70 °C, about 340 °C and about 520 °C. In other exemplary embodiments, the first catalyst material is characterized by a H2-TPR profile having distinct reduction peaks at about 80 °C, about 340 °C and about 520 °C.

[0108] In exemplary embodiments, the first catalyst material is characterized by a C 1s X-ray Photoelectron Spectroscopy (XPS) having a peak at about 282.0 eV. In other exemplary embodiments, the first catalyst material is characterized by a C 1s XPS having peaks at about 280.4 eV, about 280.9 eV, and about 282.1 eV. C 1s XPS is a surface-sensitive technique that analyzes photoelectrons emitted from the carbon 1s orbital (about 285 eV binding energy) to determine the chemical bonding, functional groups, and oxidation states of carbon within the top 5-10 nm of a material. The top 5-10 nm of a material is the most commonly analyzed XPS region since it can help distinguish sp2 / sp3hybridization, identify contaminants (adventitious carbon), and determine polymer chemistry.

[0109] In exemplary embodiments, the first catalyst material is characterized by a Fourier-transformed Extended X-ray Absorption Fine Structure (EXAFS) spectra having a scattering peak at about 2.4 A and optionally at about 1 .8 A.

[0110] In exemplary embodiments, the first catalyst material is characterized by a cumulative pore volume of about 0.10 cm3 / g to about 2.0 cm3 / g or more, about 0.10 cm3 / g to about 1.5 cm3 / g, about 0.10 cm3 / g to about 1.0 cm3 / g, or about 0.50 cm3 / g to about 0.80 cm3 / g.

[0111] Another aspect of the present disclosure is a second catalyst material including (i) at least two metal oxide sheets, each sheet having a chemical composition according to the following formula Mn+ iOm(n+i)Xn-aTx, wherein M is a2101715-001365

[0112] -17-transition metal, n is an integer ranging from 1 to 3, m is an integer ranging from 0 to 2, X is carbon (C) or nitrogen (N), a is an integer ranging from 0 to 2, and Tx is a surface functional group; and (ii) an interlayer space residing between the at least two titanium oxide sheets, the interlayer space including one or more pillar structures.

[0113] In exemplary embodiments, the second catalyst material has at least one metal oxide sheet having a chemical composition according to one of the following formulas Ti3O3mC2-aTx orTisOsmTx, wherein m is an integer ranging from 0 to 2, and a is an integer ranging from 0 to 2.

[0114] The transition metal (M) of the second catalyst material can be any one or combinations of the transition metals used in the MXene sheets of the first catalyst material.

[0115] The Txsurface functional group of the MXene sheets can be selected from, but is not limited to, -O', -OH, a halogen (e.g., -Cl, -Br, -F) or an amine.

[0116] The one or more pillar structures of the second catalyst material can contain any one or combinations of the inorganic oxide species, ionic species, and / or organic species of the first catalyst material.

[0117] The interlayer space of the second catalyst material can have a thickness ranging from about 1.0 nm to about 100 nm or higher, about 1.0 nm to about 90 nm, about 1 .0 nm to about 80 nm, about 1.0 nm to about 70 nm, about 1.0 nm to about 60 nm, about 1.0 nm to about 50 nm, about 1.0 nm to about 40 nm, about 1.0 nm to about 30 nm, about 1.0 nm to about 20 nm, about 1.0 nm to about 10 nm, or 3.0 nm to about 5.0 nm.

[0118] In exemplary embodiments, at least one of the one or more pillar structures located within the interlayer space of the second catalyst material contains one or more metal species (e.g., metallic particles or alloys), inorganic oxide species, ionic species, and / or organic species. The pillar structures can be composed of only one type of metal species, inorganic oxide species, ionic species, and / or organic species, be composed of combinations of different metal species, inorganic oxide species, ionic species, or organic species, or be composed of different metal species, inorganic oxide species, ionic species, and organic species. In exemplary embodiments, at least one of the pillar structures is bimetallic, trimetallic or multiple2101715-001365

[0119] -18-metallic alloy materials. The metallic species can include, but are not limited to, any of the transition metals belonging to Period 4, Period 5 or Period 6 of the Periodic Table, e.g., iron (Fe) particles, cobalt (Co) particles, nickel (Ni) particles, copper (Cu) particles, chromium (Cr) particles, manganese (Mn) particles, ruthenium (Ru) particles, rhodium (Rh) particles, palladium (Pd) particles, silver (Ag) particles, platinum (Pt), palladium (Pd), gold (Au) particles, iridium (Ir) particles, or combinations thereof. The metallic species can also include alloys that possess metals selected from, but not limited to, Fe, Co, Ni, Cu, Cr, Mn, Ru, Rh, Pd, Ag, Pt, Pd, Au, Ir, molybdenum (Mo), aluminum (Al), tin (Sn), vanadium (V), zinc (Zn), antimony (Sb), and bismuth (Bi).

[0120] The pillar structures of the second catalyst material can contain any one or combinations of the metal species, inorganic oxide species, ionic species, and / or organic species contained in the pillar structures of the first catalyst material.

[0121] In exemplary embodiments, the metallic particles of the second catalyst material possess an average particle size ranging from about 0.2 nm to about 1.5 nm or higher, about 0.5 nm to about 50 nm, about 0.5 nm to about 40 nm, about 0.5 nm to about 30 nm, about 0.5 nm to about 20 nm, about 0.5 nm to about 10 nm, about 0.5 nm to about 5 nm, about 0.5 nm to about 1.5 nm, or about 0.5 nm to about 0.8 nm.

[0122] In exemplary embodiments, one or more of the pillar structures located within the interlayer space residing between the two titanium oxide metallic sheets of the second catalyst material is loaded with or contains one or more metallic particles or metallic alloys in an amount, based on the total weight of the second catalyst material, ranging from about 0.01 wt% to about 50 wt%, at least 3 wt%, from about 3 wt% to about 10 wt%, from about 3 wt% to about 50 wt%, from about 10 wt% to about 50 wt%, from about 20 wt % to about 40 wt%, or at most 50 wt%. The metallic particles or metallic alloys can be selected from any one or more of the metallic particles or metallic alloys disclosed herein.

[0123] In exemplary embodiments, the second catalyst material possesses metallic particles or alloys within the interlayer space in an amount, based on the total weight of the second catalyst material, ranging from about 0.01 wt% to about 50 wt%, at least 3 wt%, from about 3 wt% to about 10 wt%, from about 3 wt% to about2101715-001365

[0124] -19- 50 wt%, from about 10 wt% to about 50 wt%, from about 20 wt % to about 40 wt%, or at most 50 wt%.

[0125] In exemplary embodiments, the second catalyst material is characterized by an XRD pattern having peaks 25.5°, 38.1°, 48.1°, and 54.4° 20. In exemplary embodiments, the second catalyst material is characterized by an XRD pattern having a peak at 27.6° 20.

[0126] In exemplary embodiments, the second catalyst material is characterized by a d-spacing of 1 nm or higher or about 1 nm to about 100 nm, as determined by a SAXS pattern. In exemplary embodiments, the second catalyst material is characterized by a d-spacing of about 0.8 nm to about 2.0 nm or higher, or about 1.4 nm to about 1.6 nm or higher, as determined by a SAXS pattern. In other exemplary embodiments, the second catalyst material is characterized by a d-spacing of about 4.0 nm or higher, as determined by a SAXS pattern.

[0127] In exemplary embodiments, at least one of the titanium oxide metallic sheets of the second catalyst material has an average layer thickness above 1.5 nm or ranging from about 0.5 nm to about 1.5 nm, about 0.7 nm to about 1.5 nm, or about 0.5 nm to about 0.7 nm.

[0128] In exemplary embodiments, the second catalyst material is characterized by a H3-type hysteresis loop at P / Poof about 0.48 to about 1.00, as determined by a N2 adsorption / desorption isotherm. In exemplary embodiments, the second catalyst material is characterized by a H3-type hysteresis loop at relative pressures (P / Po) of at least 0.5 or ranging between 0.4 to 0.8, as determined by a N2 adsorption / desorption isotherm. In other exemplary embodiments, the second catalyst material is characterized by a H2-type hysteresis loop at P / Poof 0.4 to 0.9, as determined by a N2 adsorption / desorption isotherm. In other exemplary embodiments, the second catalyst material is characterized by a H4-type hysteresis loop at P / Po greater than 0.8, as determined by a N2 adsorption / desorption isotherm.

[0129] In exemplary embodiments, the second catalyst material is characterized by a hierarchical pore architecture with pore size distribution of micro- (<2 nm), meso-(2-50 nm) and macro-(>50 nm) pores, as determined by a N2 adsorption / desorption isotherm.2101715-001365

[0130] -20- In exemplary embodiments, the second catalyst material has a BET surface area greater than 100 m2 / g, ranging from about 100 m2 / g to about 1000 m2 / g, ranging from about 200 m2 / g to about 800 m2 / g, ranging from about 400 m2 / g to about 600 m2 / g, or ranging from about 300 m2 / g to about 500 m2 / g. In exemplary embodiments, the second catalyst material has a BET surface area of about 30 m2 / g to about 800 m2 / g.

[0131] In exemplary embodiments, the second catalyst material possesses a BET surface area that is at least three times higher than a BET surface area of the catalyst material without the one or more pillar structures residing within the interlayer space.

[0132] In exemplary embodiments, the second catalyst material is characterized by a pore-width distribution having a peak at 0.6 nm, as determined by a N2 adsorption / desorption isotherm and the Horvath-Kawazoe (HK) method.

[0133] In exemplary embodiments, the second catalyst material is characterized by a cumulative pore volume of about 0.10 cm3 / g to about 2.0 cm3 / g or more, about 0.10 cm3 / g to about 1.5 cm3 / g, about 0.10 cm3 / g to about 1.0 cm3 / g, or about 0.50 cm3 / g to about 0.80 cm3 / g.

[0134] Another aspect of the present disclosure is a method for hydrogenating a plastic waste composition that includes subjecting the plastic waste composition to a hydrogenolysis reaction, wherein the hydrogenolysis reaction occurs in the presence of one or more of the catalyst materials disclosed herein.

[0135] In exemplary embodiments, the hydrogenolysis reaction occurs at temperature ranging from about 150°C to about 400°C, about 200°C to about 300°C, or about 250°C to about 350°C.

[0136] In exemplary embodiments, the hydrogenolysis reaction occurs at H2 pressure ranging from about 1 bar to about 300 bar, about 1 bar to about 250 bar, about 1 bar to about 200 bar, about 1 bar to about 150 bar, about 1 bar to about 100 bar, about 1 bar to about 50 bar, or about 1 bar to about 25 bar.

[0137] In exemplary embodiments, the hydrogenolysis reaction occurs under a plastic-to-catalyst material ratio ranging from about 1:1 to about 100:1, about 1:1 to about 50: 1 , about 1 : 1 to about 25: 1 , about 1 : 1 to about 15:1, about 1 : 1 to about 10:1 , about 5:1 to about 25:1 , or about 5:1 to about 15:1 .2101715-001365

[0138] -21- In exemplary embodiments, the hydrogenolysis reaction occurs for at least 1 minute, 5 minutes, at least 10 minutes, at least 15 minutes, at least 30 minutes, at least an hour, at least 2 hours, at least 4 hours, at least 12 hours, or any time required to fully hydrogenolyze the plastic composition. Those of ordinary skill in the art would be ready capable of determining the time required to hydrogenolyze the plastic composition based on the contents of the composition and the amount of catalyst material used in the hydrogenolysis reaction.

[0139] In exemplary embodiments, the plastic composition includes one or more polyolefins (such as polyethylene, polypropylene, polybutene, and ethylenepropylene diene monomer (EPDM)), polyesters (such as polyethylene terephthalate, poly-1, 4-cyclohexylene-dimethylene terephthalate, recycled polyester, polycarbonate, polytetrafluoroethylene, and polybutylene terephthalate), polystyrene, polyvinyl chloride, polyurethane, polyamides and acrylics.

[0140] Another aspect of the present disclosure is a method for producing the first catalyst material, wherein the method includes one or more of: intercalating one or more pillar precursors between the at least two MXene sheets and / or hydrolyzing the one or more pillar precursors between the at least two MXene sheets into the one or more pillars structures.

[0141] In exemplary embodiments, the method is carried out under an autogenous pressure. An autogenous pressure is the internal pressure developed within a sealed vessel, such as an autoclave, caused by heating the contained fluids (liquid solvent and / or reaction products) rather than by external pressure application. In exemplary embodiments, the autogenous pressure ranges from about 1 atm to about 2.5 atm. In other exemplary embodiments, the autogenous pressure ranges from about 1 bar to about 100 bar, about 1 bar to about 50 bar, about 1 bar to about 40 bar, about 1 bar to about 30 bar, about 1 bar to about 20 bar, about 1 bar to about 10 bar, about 10 bar to about 30 bar, or about 10 bar to about 20 bar.

[0142] In exemplary embodiments, the intercalating includes subjecting the at least two MXene sheets to a swelling agent and a pillarization agent.

[0143] In exemplary embodiments, the swelling agent is selected from an amine containing an alkyl chain having one to twelve carbons (such as dodecylamine (DDA), octadecylamine (ODA) or hexylamine (HA)), or more (such as long-chain2101715-001365

[0144] -22-fatty amines like 1-tetradecanamine, 1-hexadecanamine, 1-octadecanamine, or9-octadecen-1 -amine, and branched alkyl amines like 2-hexyldecylamine or 2-octyldodecylamine), organic bases (such as DMSO, tetrabutylammonium hydroxide, and tetramethylammonium hydroxide), metal ions and 1,3,5-trimethylbenzene.

[0145] In exemplary embodiments, the pillarization agent is an oregano precursor of metal oxides (e.g., cobalt oxide, silver oxide, manganese oxide, titanium oxide, zirconium oxide, aluminum oxide, cesium oxide, silicon dioxide and tin oxide), tetraethyl orthosilicate (TEOS), metal ions (e.g., Na+, Li+and K+), organic compounds and carbon nanotubes.

[0146] In exemplary embodiments, the intercalating is performed under a swelling agent to MXene mass ratio of about 0.1:1 to about 25: 1 , about 1 : 1 to about 20: 1 , about 5: 1 to about 15:1, or about 5: 1 to about 10:1.

[0147] In exemplary embodiments, the intercalating is performed under a pillarization agent to MXene mass ratio of about 0.01 :1 to about 50:1, about 0.1:1 to about 50: 1 , about 1 : 1 to about 50: 1 , about 1 : 1 to about 40: 1 , about 1 : 1 to about 20:1, about 1:1 to about 10:1, or about 1 :1 to about 5:1.

[0148] In exemplary embodiments, the intercalating is performed at a temperature ranging from about 50°C to about 300°C, 100°C to about 200°C, or about 100°C to about 150°C.

[0149] In exemplary embodiments, the intercalating is performed in the presence of water. In other exemplary embodiments, the hydrolysis of the intercalated one or more pillar precursors is performed in the presence of water.

[0150] In exemplary embodiments, the intercalating is performed under a mass ratio of MXene:swelling agent: pillarization agentwater. This mass ratio can be expressed as 1 :x:y:z, wherein x = swelling agent mass, y = pillarization agent mass, and z = water mass. In exemplary embodiments, x is 0.5 to 20, y is 0.1 to 20, and z is 0 to 20. In other exemplary embodiments, the intercalating is performed under a mass ratio of MXene:swelling agentpillarization agentwater of about 1:10:0.5:10.

[0151] In exemplary embodiments, no water is added during the hydrolyzing of the one or more pillar precursors.2101715-001365

[0152] -23- In exemplary embodiments, the hydrolyzing is performed under a temperature of about 25°C to about 100°C, about 30°C to about 90°C, or about 50°C to about 70°C.

[0153] In exemplary embodiments, the hydrolyzing is performed under a mass ratio of water to MXene ranging from about 0:1 to about 20:1, about 0.1:1 to about 15:1 , about 0.1:1 to about 10:1, about 0.1:1 to about 5:1 , or about 0.1:1 to about 1:1.

[0154] Another aspect of the present disclosure is a method for producing the second catalyst material, the method including one or more of: calcining a P-MXene material at a temperature ranging from about 250°C to about 550°C, wherein the P-MXene material contains an interlayer space residing between two MXene sheets, the interlayer space including one or more pillar structures.

[0155] In exemplary embodiments, the calcining is performed at a temperature of about 250°C to 450°C, about 300°C to 400°C or about 250°C to 350°C. In other exemplary embodiments, the calcining is performed at a temperature of about 350°C to about 550°C, about 400°C to about 500°C or about 450°C to about 500°C.

[0156] In exemplary embodiments, the calcining is performed under an airflow rate of about 10 to about 500 mL / min, about 50 to about 400 mL / min, about 100 to about 300 mL / min or about 100 to about 200 mL / min.

[0157] In exemplary embodiments, the calcining is performed under atmospheric pressure.

[0158] In exemplary embodiments, the calcining is performed for about 1 to about 24 hours, about 2 to about 16 hours, about 4 to about 12 hours or about 2 to about 8 hours.

[0159] In exemplary embodiments, the method includes impregnating the second catalyst material with at least metallic particle or alloy disclosed herein.

[0160] In exemplary embodiments, the impregnating includes one or more of: adding a stock solution of the at least one metallic particle or alloy to the second catalyst material to create an impregnated catalyst material, drying the impregnated catalyst material under a temperature ranging from about 25°C to about 200°C, and / or reducing the dried, impregnated catalyst material at a temperature ranging from about 150°C to about 450°C.2101715-001365

[0161] -24- Examples

[0162] The present disclosure will be described in more detail with reference to the following Examples, which show exemplary embodiments in accordance with the present disclosure. The present disclosure is not limited to these exemplary embodiments.

[0163] Example 1 :

[0164] This example provides exemplary synthesis methods for, and structural properties of, the catalyst materials disclosed herein. This example also evaluates the ability of the catalyst materials to hydrogenate plastic polymers typically present in plastic waste.

[0165] Materials and Methods of Example 1

[0166] Materials

[0167] Hydrochloric acid (HCI, 37.0%), lithium fluoride (LiF, > 99.9 %), hexaammineruthenium (II) chloride ([Ru(NH3)e]Cl2, 99.9 % trace metals basis), tetraethyl orthosilicate (TEOS, 98 %), low-density polyethylene (LDPE) (Mwabout 4 kDa), polyethylene (LDPE) (Mw about 76 kDa), and methylene chloride (CH2CI2, > 99.9 %) were purchased from Sigma-Aldrich. Ruthenium on carbon support (5.0 mass % Ru, powder) was purchased from Sigma-Aldrich, n-octacosane (C28H58, > 98.0 %) was acquired from TCI Chemicals. The MAX (Ti3AIC2, > 99.9 %) powder was obtained from Tongrun Info Technology Co. Ltd, China. 1 -dodecylamine (DDA, 97 % purity) was acquired from Thermo Fisher Scientific Inc. Deionized (DI) water was used throughout the experiments of this example. All chemicals were used as received without further modification.

[0168] Preparation of MXene and P-MXene Materials

[0169] The MXene material was prepared by etching aluminum (Al) from TisAIC2 MAX phase material following a previously reported method (see Little, J.M. et al., “Noble metal ion-directed assembly of 2D materials for heterostructured catalysts and metallic micro-texturing”, Adv. Funct. Mater. (2023) 33, 2215222). For this example, 1.0 g of TisAIC2 MAX powder was slowly added to a solution containing 40 mL of 9.0 mol L'1HCI solution and 3.0 g LiF. The resulting mixture was stirred at 35 °C and 40 rad s'1for 24 h. The resultant suspension was divided equally into two centrifuge tubes with a volume of 50 mL. The centrifuge tubes were pre-filled2101715-001365

[0170] -25-with 25 mL of cold 2.0 mol L'1HCI solution. After centrifuging at 840 rad s'1for 5 min, the supernatant in each centrifuge tube was replaced with fresh 2.0 mol L'1HCI solution. The centrifugation and washing steps were repeated three times. Afterwards, the solid material was collected by centrifugation and washed by dispersing in DI water. The water washing and centrifugation steps were repeated until the supernatant reached a pH of about 6.0. Finally, the solid residue was dispersed in DI water, sonicated in iced water at 35 kHz for 1 hr in an ultrasonic cleaner (VWR International), and then centrifuged at 315 rad s'1for 30 min. The supernatant, containing the TisC2TxMXene phase, was separated from unreacted MAX phase, which precipitated at the bottom of centrifuge tube, and was transferred into a clean centrifuge tube. A portion of the MXene suspension was lyophilized using a freeze dryer at -85 °C and 1 .0 Pa for 2 days to obtain a dry powder for characterization and pillarization treatment. For simplicity, the MXene (TisC2Tx) product is referred to as MXene throughout the remainder of this example.

[0171] MXene pillarization was conducted following a previously reported procedure (see Maughan, P.A. et al., “Porous silica-pillared MXenes with controllable interlayer distances for long-life Na-ion batteries”, Langmuir (2020) 36, 4370-4382). For this example, 0.5 g of MXene dry powder was mixed with 5.0 g of DDA and 10.0 g TEOS in a glass flask at ambient temperature. The mixture was purged with an argon gas flow for 15 min, then was sealed and kept stirring at 20 rad s'1for 4 hr. Afterward, the suspension was filtered, and the resulting solid residue was dried in a vacuum oven for 18 hr. The dried sample was then dispersed in 25 mL DI water in a centrifuge tube and left at ambient temperature for 18 hr without stirring. The product was collected by filtration, followed by drying at 60 °C in a vacuum oven overnight. Finally, the product underwent heat treatment, with the temperature ramping to 400 °C at a rate of 1.0 °C min-1and maintained at this temperature for 12 hr under N2 with a flow rate of 100 mL min'1, resulting in the formation of pillared MXene which is hereafter referred to as P-MXene in this example.

[0172] Synthesis of Ru@MXene and Ru@P-MXene catalysts

[0173] To prepare the Ru@MXene catalysts, a 0.1 mol L'1stock solution of [Ru(NH3)e]Cl2 was initially prepared by dissolving [Ru(NH3)e]Cl2 in DI water. An appropriate amount of the stock solution was added dropwise to the prepared2101715-001365

[0174] -26- MXene suspension to vary the Ru mass fraction from 3.0 % to 7.0 %. The mixture was stirred at 40 rad s-1for 1 hr, transferred into a sealed petri dish, and immersed in a liquid N2 dewar. The sample was then lyophilized for 2 days to obtain Ru@MXene catalysts, in which Ru mass fraction was varied from 3.0 % to 7.0 %. The Ru@MXene samples were reduced in a tubular furnace at 300 °C for 2 hr (ramp rate 5.0 °C min-1) under a H2 gas flow (a 5.0 % volume fraction of H2 in a N2 mixture, flow rate of 100 mL min'1).

[0175] The preparation of the Ru@P-MXene catalysts utilized an incipient wetness impregnation method. The [Ru(NH3)e]Cl2 stock solution was added dropwise to the prepared P-MXene sample, followed by drying at 60 °C for 2 hr in a vacuum oven. The Ru@P-MXene samples were then reduced following the same procedure as the Ru@MXene samples. All the dry MXene, P-MXene, Ru@MXene and Ru@P-MXene samples were stored in a desiccator prior to property characterization and catalytic reaction tests.

[0176] Material characterization

[0177] Wide-angle (20 > 5.0 °) powder X-ray diffraction (XRD) patterns were obtained on a Bruker D8 diffractometer equipped with Cu Ka radiation source. Small-angle X-ray scattering (SAXS) measurements (0.10< 29 < 5.0 °) were carried out on a Xenocs Xeuss 3.0 instrument equipped with D2+ MetalJet X-ray source (Ga Ka, 9.2 keV, / = 1.341 A). The samples were aligned perpendicular to the direction of the incident X-ray beam (transmission mode) and the scattered beam was recorded on a Dectris Eiger 2R 4M hybrid photon counting detector with a pixel dimension of 75 x 75 pm2, where the X-ray exposure time for each measurement was 600 s. The collected 2D SAXS images were circularly averaged and expressed as absolute intensity versus 29 after transmission correction and subtraction of background scattering. In order to calibrate the measured intensities to absolute scale intensities, we used direct beam intensity. The sample-to-detector distances for SAXS was 900 mm. Nitrogen adsorption / desorption isotherms were measured at a temperature of -196°C with a Micromeritics ASAP 2020 system. Samples were evacuated overnight at 150 °C and 100 Pa. The specific surface area and pore width distribution were calculated using the Brunauer-Emmett-Teller (BET) and Horvath-Kawazoe (HK) methods. BET specific surface area are2101715-001365

[0178] -27-obtained from adsorption branch at relative pressure ratios (P / Po) between 0.1 and 0.3.

[0179] X-ray photoelectron spectra (XPS) were acquired with a Kratos Axis Supra+ spectrometer equipped with an AI(Ka) X-ray source. Binding energies in all spectra were referenced to the C-Ti peak, a characteristic peak of MXene materials, located at 282.0 eV. X-ray absorption fine structure (XAFS) measurements were performed on the Ru K-edge at beamline ISS, 8-ID, and on the Ti K-edge at beamline BMM, 6-BM, at the National Synchrotron Light Source II (NSLS-II). At ISS, X-rays were provided by a damping wiggler and tuned by a Si (111 ) monochromator. Ex situ measurements were made of empirical oxide and metallic standards, whereas in situ catalyst measurements were made with a Clausen cell. Reactions were monitored by mass spectrometry (Hiden Analytical, HPR-20 R&D). At BMM, X-rays were provided by a 3-pole wiggler tuned by a Si(111 ) double crystal monochromator. Here, in situ catalyst measurements were made with a Nashner-Adler cell. Data processing, including normalization and Fourier transform analysis, was performed using the Larch analysis package and followed methods reported elsewhere (see Jahrman, E.P. et al., “X-ray absorption fine structure characterization of a multicomponent spinel catalyst”, X-Ray Spectrom., (2023) 52, 90-101 ; and Newville, M., “Larch: an analysis package for XAFS and related spectroscopies”, J. Phys.: Conf. Ser. (2013) 430, 012007).

[0180] Particle morphologies were characterized by scanning electron microscopy (SEM, Zeiss Auriga 60 CrossBeam, using an accelerating voltage of 3kV) and transmission electron microscopy (TEM, JEOL, JEM-201 OF). The TEM instrument was equipped with a field-emission transmission electron gun operating with an accelerating voltage of 200 kV. For TEM high-angle annular dark field scanning transmission electron microscopy (HAADF-STEM) imaging, the ethanol-dispersed Ru-loaded samples were sonicated for 30 min and drop casted onto lacey carbon grids. Analysis of Ru morphology on catalyst samples were conducted using a JEOL JEM-ARM200F TEM microscope in STEM mode, operating with an accelerating voltage of 200 kV, with a 50 pm condenser aperture size, and 5C spot size. Energy dispersive X-ray spectroscopy mapping (STEM-EDS) was performed using an Oxford XMAXTLE 100 mm2windowless EDS spectrometer mounted on2101715-001365

[0181] -28-the ARM200F microscope. The reducibility of catalyst samples was assessed by H2 temperature-programmed reduction (H2-TPR) using a Micromeritics AutoChem II 2920 instrument. In each experiment, 30 mg of the as-lyophilized Ru@MXene or vacuum-dried (60°C) Ru@P-MXene catalyst was pretreated in a He flow (50 mL min-1) at 300 °C for 2 hr, followed by cooling to 30 °C. H2-TPR profiles were obtained by heating the sample to 900 °C at a ramp rate of 10 °C min-1under a H2 gas flow (a 10 % volume fraction of H2 in an Ar mixture, flow rate of 30 mL min-1) and the data were recorded by a thermal conductivity detector (TCD). The inductively coupled plasma optical emission spectroscopy (ICP-OES, Thermo iCAP 7600) was used to measure the Ru mass fraction in each sample.

[0182] Hydrogenolysis reaction tests

[0183] The catalytic reaction was conducted in a 50 mL stainless steel Parr batch reactor equipped with a pressure gauge and thermocouple. In all experiments, 0.1 g of freshly reduced Ru-loaded catalyst and 2.0 g of low-density polyethylene (LDPE) (i.e., LDPE-to-catalyst mass ratio = 20) were added to the Parr reactor. The catalyst / LDPE mixture was stirred for 2 min using a magnetic stir bar (25.4 mm x 8 mm, coated with polytetrafluoroethylene (PTFE)). Subsequently, the reactor was sealed and purged 5 times with H2 (Keen Gas, grade 5.0) with a pressure of 1.5 MPa. The reactor was then pressurized with H2 to the desired pressure. Afterwards, the reactor was heated to the final temperature using a band heater controlled by a proportional-integral-derivative (PID) controller while stirring at 50 rad s-1. After a specified reaction time, the reactor was removed from the heating source and cooled rapidly in an ice bath to quench the reaction.

[0184] The reaction products were collected once the reactor temperature dropped below 3.0 °C. The gaseous products (C1-4) were extracted from the Parr reactor headspace into a 1 .0 L Tedlar gas sampling bag and analyzed by gas chromatography with flame-ionization detector (GC-FID, Agilent) equipped with a CP-Volamine GC column. The residual solid and oil / liquid mixture inside the Parr reactor were dissolved in about 20 mL of methylene chloride containing 20 mg of n-octacosane as an external standard. The slurry mixture was filtered by Whatman filter paper (GE, 11 pm). The soluble products were categorized as liquid products (C5-35), and the solid residue collected on the filter paper was classified as solid.2101715-001365

[0185] -29- The liquid products were quantified using a GC-FID (Agilent, HP-1 column) and identified with a gas chromatography coupled with mass spectrometry (GC-MS, Agilent) equipped with a DB-1 column. Analytical standard calibration mixtures of C1-35 were employed to determine calibration coefficients and retention times for product identification.

[0186] The yields of liquid and gas products were calculated on a molar basis. The yield of the product group with / carbons ( Y) was calculated as:

[0187] Y =l(Equation 1)

[0188] nfeed

[0189] where n, is the moles of carbon in the product group with / carbons, and nfeed is the moles of carbon in the plastic feed. The conversion (X, %) was defined gravimetrically based on the solid residue collected on the filter paper and calculated as:

[0190]

[0191] where mfeed is the mass of plastic feed and mresidue solidis the mass of the polymer residue collected on the filter paper. The solid yield (Ys) is defined as:

[0192] Ys= 100 - X(° / o) (Equation 3).

[0193] Experiments and Results

[0194] Experiment 1: Investigating Morphology and Textural Properties ofMXene Material

[0195] The morphologies of MXene and its parental MAX material were visualized using SEM imaging. The MAX phase (FIG. 1) exhibits a dense, layered structure, characteristic of its crystalline arrangement. Following the etching of Al during MXene synthesis, this compact structure transforms into thin, flexible, multilayered MXene sheets (FIG. 1 ). These sheets are prone to restacking due to van der Waals interactions. Sliding and reordering of these MXene layers can also occur. To explore the surface area and porosity of these materials, N2 adsorption / desorption isotherms (FIG. 1) were analyzed. The BET specific surface area and cumulative pore volume of MXene were notably higher than those of the MAX phase. The MAX phase showed negligible N2 adsorption over almost the entire relative pressure (P / Po) range. In contrast, MXene exhibited a slight increase in N2 uptake at relative pressure below P / Po < 0.4, indicative of the presence of small amount of2101715-001365

[0196] -30-micropores. Furthermore, MXene showed a distinct H2-type hysteresis loop at P / Po > 0.4, indicating the presence of a pore network structure. The steep desorption branch of the hysteresis loop could be attributed either to pore-blocking / percolation in a narrow range of pore necks or to cavitation-induced evaporation. The pore width distribution (FIG. 2), analyzed by the HK method, revealed a peak at 0.6 nm and several smaller, broader peaks in the 0.9 nm to 3.6 nm range. The broader peaks suggest the presence of nonuniform mesopores, consistent with the H2-type hysteresis loop in FIG. 1. It should be noted that the cumulative pore volume of the MXene material is still relatively low, about 0.04 cm3g-1- XRD patterns (FIG. 1) further illustrate the structural evolution from MAX to MXene. The XRD pattern of the MAX phase (TisAIC2) displayed a characteristic (002) peak corresponding to a c-lattice parameter of 1 .8 nm, confirming the presence of a single MAX phase before MXene synthesis. After conversion to multilayered MXene, the XRD pattern still resembled that of the MAX phase, but the (002) peak broadened and shifted to a lower diffraction angle. Specifically, the (002) peak shifted from 20 = 9.4 ° in the MAX phase to 20 = 8.2 ° in MXene, which corresponds to a c-lattice parameter increase from 1.8 nm to 2.2 nm. TEM imaging of MXene (FIG. 3) was employed to measure the thickness of the sheets, revealing an average layer thickness of 0.9 nm. The average interlayer spacing (i.e., the distance between the surfaces of adjacent layers) in the synthesized MXene can be estimated by subtracting the one-layer thickness (i.e., 0.9 nm) from the d-spacing (i.e., the distance between the centers of adjacent layers, equivalent to half of c-lattice parameter), which is about 0.2 nm.

[0197] Experiment 2: Investigating the Morphology and Textural Properties of Ru@MXene catalysts

[0198] Ru@MXene catalysts were prepared with Ru mass fractions of 3.0 %, 5.0 % and 7.0 %. The wide-angle XRD patterns of these Ru@MXene catalysts displayed the characteristic diffraction peaks of MXene. The absence of peaks associated with Ru species indicates a higher dispersion of Ru particles within the MXene support. The characteristic diffraction peaks of MXene, specifically the (004), (006), (008), and (110) reflections, were observed at 20 = 17.1 °, 25.4 °, 34.5 °, and2101715-001365

[0199] -31- 60.8 °, respectively, demonstrating preservation of the crystalline structure following the incorporation of Ru. However, small-angle XRD data revealed a shift in the (002) peak from 29 = 8.2 ° to 6.2 °, 5.8 ° and 5.6 ° as the Ru mass fraction increased from 3.0 % to 5.0 % and then to 7.0 %. Using Bragg's Law, the d-spacing of the Ru@MXene catalysts were calculated to be 1.4 nm, 1.5 nm, and 1.6 nm, respectively. Previous TEM characterizations determined the layer thickness of MXene to be 0.9 nm. Consequently, the interlayer spacing can be evaluated as 0.5 nm, 0.6 nm, and 0.7 nm by subtracting the average layer thickness from each of the d-spacing. This clearly indicates that the incorporation of Ru metal into the MXene support results in an expansion of the interlayer spacing, which increases with higher metal loading.

[0200] The N2 adsorption / desorption isotherms of Ru@MXene catalysts showed changes in textural properties upon Ru loading. As the Ru mass fraction increased to 3.0 % and 5.0 %, N2 uptake increased at relative pressures of P / Po < about 0.5 (FIG. 3). This suggests an increase in micropore volume due to the presence of metal particles. However, at a 7.0 % Ru mass fraction, the N2 uptake slightly decreased, aligning more closely with 3.0 % sample within this relative pressure range. At P / Po > about 0.5, all Ru@MXene samples exhibited an H3-type hysteresis loop, differing from the H2-type in pristine MXene. This characteristic can be attributed to the non-rigid aggregates of MXene layers, or the presence of incomplete filled large pores by condensate. The increase in N2 uptake at higher relative pressures (i.e. , P / Po > 0.8) followed the Ru loading order, implying the creation of larger pores in the support as more Ru metal is loaded. The BET surface areas of Ru@MXene samples with Ru mass fraction of 3.0 %, 5.0 % and 7.0 % were 22.7 m2g-1, 32.4 m2g-1, and 22.9 m2g-1, respectively, which is 3-4 times higher than that of the pristine MXene and follows the increase and then decrease trend. The cumulative pore volume also showed a volcano type trend with increasing Ru loading in the MXene support.

[0201] MXene features a pore network with small openings. The metal loading appeared to mitigate pore neck blocking and created larger pores. The overloading of metal species also seemed to occupy the pore spaces of MXene, which can lead to a decrease in N2 uptake. The Ru@MXene samples were prepared by mixing the2101715-001365

[0202] -32-metal precursors with dispersed MXene layers in solvent, followed by lyophilization, which could have locked metal species between the MXene layers. Electrostatic interactions between Ru5+ions and the negatively charged TisC2Tx surface groups can also help stabilize the expanded interlayer spacing. The pore width distribution (FIGs. 4-6) showed that a distinct peak at 0.6 nm remained dominant, indicating that the metal loading primarily affected the pore mouth structure. As the Ru mass fraction increased to 5.0 % (FIG. 5), a slight increase in intensity of this peak was observed. At a Ru mass fraction of 7.0 % (FIG. 6), the distinct peak at 0.6 nm remained dominant, which aligns with the increased d-spacing observed in the XRD patterns. Notably, the d-spacing calculated using Bragg's Law was smaller than the spacing inferred from the N2 isotherms. This discrepancy could be caused by the formation of elliptical or oval-shaped pores, where the longest axis aligns with the in-plane direction of the 2D layers, while XRD measures the d-spacing along the out-of-plane direction.

[0203] HAADF-STEM images and STEM-EDS mapping were employed to investigate the morphologies of Ru particles in the Ru@MXene catalysts. The particle size distributions were analyzed using ImageJ software, with measurements of at least about 300 Ru particles taken from multiple STEM images for each sample. In the 3.0 % Ru@MXene sample, the Ru particles were observed to be small, uniform, and nearly spherical. As the Ru mass fraction increased to 5.0 %, a sparse emergence of larger, elongated particles was observed alongside the predominantly smaller spherical ones. At a Ru mass fraction of 7.0 %, the number of large, elongated particles increased significantly. The particle size distribution histograms (FIG. 7) showed broader distributions with increasing Ru loadings. In these histograms, the size of spherical particles was based on their diameter, while the size of elongated particles was determined by their longest dimension. The average Ru particle size increased progressively, from 1.4 nm in the 3.0 % sample to 1.9 nm in the 5.0 % sample, and finally to 2.6 nm in the 7.0 % sample. The formation of larger particles with higher Ru loadings can be explained by the hard and soft acid and base theory. Ru, being a soft acid, tends to accept electrons from soft bases, such as thiolates. However, Ru interacts less favorably with hard bases like hydroxide and / or fluoride, which are present on the MXene2101715-001365

[0204] -33-surface. As a result, with increasing Ru loading, Ru particles tend to aggregate and form larger particles. The in-plane spacing of the 2D MXene layers influenced the shape of the Ru aggregates into elongated structures. This is consistent with the elliptical pores aligned in the in-plane direction of the MXene layers, as estimated from the N2 isotherms and XRD characterizations discussed above.

[0205] Experiment 3: Investigating the Reducibility and Coordination Environment of Ru@MXene Catalysts

[0206] The reducibility of Ru@MXene catalysts was examined using H2-TPR measurements. FIG. 8 shows the H2-TPR profiles for Ru@MXene catalysts with different Ru mass fractions alongside the parental MAX and pristine MXene for comparison. The MAX phase did not exhibit any obvious reduction peaks within the tested temperature range. However, the MXene sample showed two reduction peaks at 630 °C and 805 °C, corresponding to the partial reduction of titanium oxide (i.e., Ti4+-> Ti3+), and Ti-Ox species in the MXene phase. Upon loading 3.0 % Ru into the MXene, two new reduction peaks emerged at 340 °C and 520 °C. The lower temperature peak likely corresponds to the reduction of RuOxspecies to metallic Ru. The higher temperature peak is associated with methane formation, catalyzed by Ru through the activation of carbide species within the MXene layers in the presence of hydrogen. With the increase of Ru loading to 5.0 %, a new peak appeared at 70 °C, which can be attributed to the reduction of RuCh (Ru(lll) to Ru(ll)) and / or RuOx (Ru(ll) to Ru(l) or Ru(ll) to Ru(0)). In the 7.0 % Ru@MXene sample, all peaks related to reduction of Ru species increased intensity and shifted to lower temperatures. This reflects greater reducibility and is consistent with the formation of larger Ru particles as verified by HAADF-STEM analysis.

[0207] XPS spectra of the Ru 3d region were measured for the Ru@MXene catalysts to explore their coordination environment. Due to the overlap between the Ru 3d and C 1s sepectra, deconvolution was performed using CasaXPS software following a previously reported method (see Morgan, D.J., “Resolving ruthenium: XPS studies of common ruthenium materials”, Surf. Interface Anal. (2015) 47, 1072-1079) to distinguish the Ru 3ds / 2 signal from the C 1s spectrum. As shown in FIG. 9, the Ru 3d spectra was deconvoluted into peaks assigned to Ru-CI, Ru-Ru and Ru-0 groups. All spectra were calibrated to C-Ti peak, a characteristic peak of2101715-001365

[0208] -34- MXene materials, located at 282.0 eV. In all Ru@MXene samples, the C 1s XPS spectrum exhibited the characteristic peak at 282.0 eV binding energy, attributed to C atoms residing in the Ti octahedra in MXene confirming successful MAX etching process and MXene formation. Additional peaks at higher binding energies were also observed, corresponding to surface contamination introduced during synthesis or from ambient air. Ru-Ru, Ru-O, and Ru-CI states were located around 280.4 eV, 280.9 eV, and 282.1 eV, respectively. The 3.0% and 5.0% Ru@MXene samples displaed mostly cationic Ru oxidation states which likely originate from RuCb and RuOx species, while the 7.0% Ru@MXene sample exhibited both cationic and metallic Ru states. It should be noted that the Ru@MXene sample was pre-reduced before the XPS measurement. The presence of metallic Ru in the Ru@MXene sample could suggest that metal carbide properties of MXene facilitate the reduction of Ru species.

[0209] To explore the coordination environment of Ru species in the Ru@MXene catalyst during the hydrogenolysis reaction, the 5.0 % Ru@MXene catalyst was selected for in situ XAFS measurement. In this experiment, the pre-reduced 5.0 % Ru@MXene was mixed with LDPE in a ratio of 2:1 by mass, and the mixture was exposed to H2 gas flow (a 5.0 % volume fraction of H2 in an Ar mixture). The temperature was ramped from ambient temperature (about 25 °C) to 250 °C at 5.0 °C min'1. After 1 hr of hold time, the sample was cooled to ambient temperature. The in situ Ru K-edge X-ray absorption near-edge structure (XANES) results reveal that the catalyst maintained a consistent chemical state throughout the reaction, as evidenced by the similar spectral shapes under the three reaction steps (i.e. , pre-reaction, reaction, and post-reaction). In particular, the XANES spectra corresponding to reaction and post-reaction were nearly identical, whereas the H2 environment with ambient temperature (i.e., pre-reaction) only differed in some modest increase in intensity at 22145 eV. Given the proximity of this region to the white line feature of RuC>2, it is likely that this change corresponds to some minor reduction that occurred upon heating. Furthermore, the proximity of the spectral features at 22130 eV and 22155 eV to similar features observed in the spectrum of a metallic Ru foil indicates that the Ru in the catalyst was present in a significantly metallic state. This is consistent with the Fourier-transformed extended2101715-001365

[0210] -35- XAFS (EXAFS) results, which reveal a strong Ru-Ru scattering peak at 2.4 A (EXAFS distances are presented without phase correction). Notably, even after the material was returned to ambient temperature after the reaction, the Ru-Ru scattering peak was considerably less intense than what was observed for the metallic Ru foil. This could indicate an undercoordination related to nanosizing which could contribute to the differences in the XANES spectra of the catalyst and Ru foil. Finally, a scattering peak was also observed at 1.8 A, which could be related to Ru-0 or Ru-CI scattering. This feature may correspond to anchoring of the metal to the MXene support as would be required for some cationic Ru5+surface species. This is consistent with XPS results in the literature, as well as the XPS and H2-TPR results gathered in this example.

[0211] Experiment 4: Hydrogenolysis over Ru@MXene catalysts

[0212] To evaluate the performance of Ru@MXene catalysts, a series of experiments were conducted to investigate the effects of various parameters on the hydrogenolysis of LDPE using a 5.0 % Ru@MXene catalyst. The base conditions were a LDPE-to-catalyst mass ratio of 20, a reaction time of 2 hr, a temperature of 250 °C, and a pressure of 3.0 MPa H2. Each parameter (e.g., temperature, reaction time, and pressure) was independently varied to assess its influence on LDPE conversion and product yields, compared to the base conditions. It is worth noting that the pristine MXene support showed no activity in enabling LDPE deconstruction (FIG. 10). The product primarily consisted of linear alkanes with a minor amount of branched alkanes, and no aromatics were identified. A representative GC-FID spectrum illustrating the product distribution is provided in FIG. 11.

[0213] Effects of reaction temperature: FIG. 12 shows that LDPE conversion increased with rising reaction temperature. The catalyst enabled 4.4 % LDPE conversion at 220 °C, 9.2 % at 250 °C, and 90.9 % at 280 °C. Product yields showed that very little liquid and gas products were formed at 220 °C (i.e., < 1.0 %), while 4.2 % liquid and 1.8 % gas products formed at 250 °C, and 66.1 % liquid and 21.3 % gas products formed at 280 °C. FIG. 12 further illustrates the Ci to C35 product yields from LDPE hydrogenolysis at different temperatures. The majority of products were small hydrocarbons, with methane (Ci) being dominant at 220 °C2101715-001365

[0214] -36-and 250 °C at low conversions (i.e., < 10.0 %). At 280 °C, the majority of products are in the fuel range (C5-C22), yielding 43.0 %. The increase in conversion with temperature can be attributed to two factors. First, the viscosity of the polymer melt decreases as the temperature rises. It has been reported that a 15 °C increase in temperature can reduce the effective viscosity of polyethylene by a factor of 1.8. Lower viscosity facilitates the migration of polymer chains into the catalyst, improving access to the Ru sites for the hydrogenolysis reaction. Second, higher temperatures favor reaction kinetics, as described by the Arrhenius equation. Additionally, methane formation is more favorable at elevated temperatures, as indicated by the increasing methane selectivity among all gas and liquid products. The liquid-to-gas product ratios were 1.7, 2.2, and 3.1 as temperature increased from to 220 °C to 250 °C and finally 280 °C, respectively. However, the methane yield increased from 0.3 % to 1.6 % and then 17.5 % with increasing temperature.

[0215] Effects of reaction time: The effects of reaction time on LDPE hydrogenolysis (i.e., kinetics) were studied with different reaction times ranging from 2 hr to 6 hr. As shown in FIG. 13, after 2 hr, a modest conversion of 9.2 % was observed. However, extending the reaction time to 3 hr increased the conversion to 60.5 %. Further extending the time to 4 hr resulted in a conversion of 77.1 %, and after 6 hr, the conversion reached 89.2 %. The product yield (FIG. 13) mirrored this trend. At 2 hr, minimal liquid (4.2 %) and gas (1.0 %) products were produced, while after 3 hr, 41.6 % liquid and 15.7 % gas products formed. By 4 hr, the liquid yield increased to 58.1 %, and gas to 16.0 %. After 6 hr, the yields reached 63.4 % liquid and 21 .6 % gas. These kinetics followed an “S”-shaped curve when plotting LDPE conversion versus reaction time. Initially, the conversion was low, but as the reaction progressed, the rate accelerated before approaching a plateau. This behavior is characteristic of heterogeneously catalyzed polymer degradation reactions. In the melt phase, LDPE does not form extended chain structures but rather adopts a random coil configuration. In this configuration, only terminal groups of the polymer chains are more labile, making them prone to conformational changes that facilitate their interaction with the active sites in the catalyst. Consequently, the hydrogenolysis rate is slow in the early stages but increases as the degree of polymerization decreases. The formation of liquid2101715-001365

[0216] -37-products (i.e., shorter hydrocarbon chains) serves to lower the system’s viscosity, improving mass transport and catalytic activity. Overtime, the yield of C5-C22 fuel range products also increased, reaching 32.2 % after 3 hr, 39.4 % after 4 hr, and 46.5 % after 6 hr, respectively (FIG. 13). The methane yield increased with increasing reaction time, reaching 17.9 % after 6 hr.

[0217] Effects of hydrogen pressure: LDPE hydrogenolysis was further tested under different H2 pressures. FIG. 14 shows LDPE conversion increased with pressure: 6.7 % at 1.0 MPa H2, 9.2 % at 3.0 MPa H2, and 90.8 % at 6.0 MPa H2. At the highest pressure, the majority of products were in the fuel range, with a yield of 54.2 % (FIG. 14). The product yields showed limited liquid formation at 1.0 MPa H2 (i.e., < 2.0 %), while 4.2 % liquid and 1.8 % gas products were produced at 3.0 MPa H2. In contrast, 68.8 % liquid and 18.5 % gas products formed at 6.0 MPa H2. Product distribution became more uniform at higher pressures compared to lower pressures. Furthermore, high H2 pressure helped to reduce methane formation to 15.1 %.

[0218] Effects ofRu loading in Ru@MXene catalyst: To examine the effects of Ru loading on catalyst performance, the same base reaction conditions as in previous studies were utilized, with the reaction time fixed at 4 hr, and Ru mass loadings adjusted to 3.0 %, 5.0 %, and 7.0 %. As shown in FIG. 15, the 3.0 % Ru@MXene catalyst achieved a conversion of 7.7 %, which increased significantly to 77.1 % with 5.0 % Ru@MXene, and further to 87.5 % with 7.0 % Ru@MXene. The product yields were 2.5 % liquid and 1.7 % gas for the 3.0 % Ru@MXene, 58.1 % liquid and 16.0 % gas for the 5.0 % Ru@MXene, and 61.9 % liquid and 21.3 % gas for the 7.0 % Ru@MXene. The product distribution in FIG. 15 shows that with the 3.0 % Ru@MXene catalyst, most products were below C7, while a broader range of products spanning from Ci to C35 was observed with both the 5.0 % and 7.0 % Ru@MXene catalysts.

[0219] While LDPE conversion increased with Ru loading, the relationship is not linear, suggesting that other factors should contribute to the substantial enhancement in conversions at higher Ru loadings. In this heterogeneous solidliquid-gas system, the accessibility of H2 gas and liquid polymer melt to the solid Ru@MXene catalyst is a key step for the reaction to proceed. As discussed earlier,2101715-001365

[0220] -38-the Ru active sites are likely sandwiched between adjacent MXene layers, making the transport of polymer chains and H2 gas molecules critical for efficient conversion. The kinetic diameter of H2 is about 0.3 nm and the radius of gyration of LDPE is about 2.9 nm. This suggests the transport of polymer into the MXene layers should play a key role in the reaction rate. Textural property characterizations reveal that surface area first increases and then decreases with increasing Ru loading in Ru@MXene catalysts. Notably, while the 3.0 % and 7.0 % Ru@MXene catalysts have similar surface areas, their conversions differ markedly, indicating that surface area alone is not the primary factor influencing performance. Pore widths that allow polymers access to the surface areas seem to be more important. The cumulative pore volume analysis (FIGs. 4-6) shows that Ru@MXene catalysts possess a hierarchical pore structure, with micro-, meso-, and macropores. The 7.0% Ru@MXene catalyst exhibited the higher macropore volume, which likely enhances conversion by facilitating greater polymer access to active sites. FIG. 15 also shows that the gas product yield increased from 16.0 % for the 5.0 % Ru@MXene sample to 21.3 % for the 7.0 % Ru@MXene sample. Methane, in particular, showed a significant increase, with yields rising from 13.3 % to 18.0 %. This elevated methane production may be attributed to the slightly larger Ru particles orclusters, which promote multi-point interactions with LDPE chains, enhancing C-C bond activation. However, this also leads to more extensive hydrogenolysis of C-C bonds, resulting in higher yields of gaseous products, particularly methane.

[0221] The 5.0 % Ru@MXene catalyst’s hydrogenolysis performance was also compared to a commercial 5.0 % Ru / C catalyst. The comparison was conducted under the same conditions as the base conditions used for 5.0 % Ru@MXene catalyst. As shown in FIG. 16, the 5.0 % Ru / C catalyst achieved 98.4 % conversion, with 47.5 % liquid and 46.4 % gas products after 4 hr of reaction.

[0222] Methane was the dominant product, with a yield of 38.1 %. In contrast, the 5.0 % Ru@MXene catalyst achieved 89.2 % conversion after 6 hr of reaction, yielding 63.4 % liquid and 21.6 % gas products, among which 17.9 % methane was detected. The high selectivity toward methane formation over the Ru / C catalyst is not simply due to a greater extent of reaction. Even when the reaction time was2101715-001365

[0223] -39-reduced to 2 hr and 1 hr, the methane selectivity remained higher compared to Ru@MXene at similar conversion levels (FIG. 17). These results indicate that 5.0 % Ru / C is more active than 5.0 % Ru@MXene but is also more selective toward methane formation. Methane formation on Ru catalysts during hydrogenolysis occurs via direct terminal C-C scission and a surface cascade of consecutive C-C scissions, with the latter being sensitive to hydrogen availability and dominant under hydrogen-lean conditions. Enhancing Ru dispersion by confining it within mesoporous materials, such as silica, could improve hydrogen coverage, while incorporating a reducible metal oxide support could facilitate hydrogen storage and supply via reverse hydrogen spillover. The readily available hydrogen on Ru catalysts can hydrogenate and desorb long alkyl surface intermediates, which prevents methane formation through excessive cascading C-C scissions.

[0224] The lower methane yield observed with 5.0 % Ru@MXene in this example likely results from two key effects: (1) confinement by MXene layers which limits polymer chain access to Ru active sites and mitigates excessive surface coverage by polymer chains and thus cascading C-C scissions, and (2) reverse hydrogen spillover from the MXene substrate which hydrogenates reaction intermediates and reduces methane formation. These mechanisms align with the observed suppression of methane selectivity when hydrogen pressure was increased at similar conversions (FIG. 18), Ru particle size was reduced (i.e., by reducing loadings) in MXene support (FIG. 15), or silica pillars were introduced into the MXene substrate (FIGs. 16 and 17). The positioning of Ru particles within MXene layers likely slows mass transport compared to Ru supported on carbon, which leads to the lower activity of 5.0 % Ru@MXene relative to 5.0 % Ru / C. The pillarization of MXene, which increases the interlayer distance (i.e., the formation of P-MXene), effectively addressed this issue. The 5.0 % Ru@P-MXene exhibited significantly higher activity than the 5.0 % Ru / C catalyst (see FIG. 19).

[0225] Experiment 5: Investigating the Ru@P-MXene catalyst in a Hydrogenolysis Reaction

[0226] The hydrogenolysis of LDPE over Ru@MXene catalysts indicated that meso- and macropores are crucial for enhancing the accessibility of LDPE to Ru2101715-001365

[0227] -40-active sites and improving the reaction rate. However, the micropores formed by Ru metal sandwiched between adjacent MXene layers accompanied with large Ru metal particles contributed to increased methane formation. To address these conflicting scenarios, a silica-pillared MXene as a support was utilized and Ru was loaded onto this support by a wetness impregnation to create a Ru@P-MXene catalyst for the hydrogenolysis of LDPE plastic.

[0228] Morphology and textural properties of P-MXene FIG. 20 presents a representative SEM image of P-MXene. The sample has a booklet-like structure, with layers resembling rigid, flat plates compared to the more flexible, curved layers in MXene (FIG. 1). Additionally, the P-MXene surface is rougher and more adorned with smaller particles compared to the smoother surfaces of MXene particles.

[0229] These characteristics arise from the presence of silica particles on the surface and within the interlayer space of MXene layers. The TEM image in FIG. 20 also confirms the layered structure in the P-MXene sample. The XRD pattern (FIG. 20) demonstrates the preservation of characteristic peak of MXene in P-MXene sample. The small-angle XRD pattern in FIG. 20 reveals a significant shift of the (002) peak to a lower angle at 2.0 °, corresponding to a d-spacing of 4.4 nm. After subtracting the MXene layer thickness of 0.9 nm, the interlayer spacing was 3.5 nm, significantly higher than those of Ru@MXene catalysts discussed above.

[0230] The N2 adsorption / desorption isotherm of P-MXene (FIG. 20) depicts the textural property changes induced by the pillaring process. P-MXene exhibited significant N2 uptake across the entire relative pressure range, surpassing that of the MXene support. The isotherm demonstrates characteristics of both type II and type IV isotherms, with the hysteresis loop combining elements of types H2 and H4. At relative pressures P / Po< 0.4, the N2 uptake attributed to micropore adsorption, indicating an increase in microporosity within the P-MXene material. In the P / Porange of 0.4 to 0.8, adsorption was dominated by condensation within the mesopores. At P / Po> 0.8, the hysteresis loop reflects type H4 characteristics, suggesting the presence of macropores that are not fully filled by pore condensates, or that the material contained non-rigid aggregates of plate-like particles. The BET surface area and cumulative pore volume of P-MXene significantly increased to 427.4 m2g-1and 0.77 cm3g-1, respectively. The2101715-001365

[0231] -41-cumulative pore width distribution (FIG. 21) revealed one distinct peak at 0.6 nm, corresponding to micropores, and a broader peak ranging from 2.2 to 5.8 nm. After silica incorporation, the cumulative pore volume drastically increased with formation of a new peak at 3.5 nm, compared to that of the MXene support.

[0232] Morphology and textural properties of Ru@P-MXene: A wetness impregnation method was employed to synthesize the Ru@P-MXene catalyst with a Ru mass fraction of 5.0 %. The XRD patterns (FIG. 20) at both wide and low angles for Ru@P-MXene closely resembled those of P-MXene, indicating that Ru loading did not induce any structural changes in the P-MXene support. No distinct XRD peaks corresponding to Ru species were observed, suggesting that the Ru particles are well dispersed on the support. The N2 adsorption / desorption isotherm of 5.0 % Ru@P-MXene displayed characteristics similar to those of the P-MXene support (FIG. 20). At lower relative pressures (P / Po < 0.1), the N2 uptake remained comparable between the two materials; however, with increasing P / Po from 0.1 to 1.0, the N2 adsorption for Ru@P-MXene began to decrease progressively, with a more pronounced reduction at higher relative pressures. The surface area and cumulative pore volume of 5.0 % Ru@P-MXene decreased to 356.7 m2g_1and 0.61 cm3g’1, respectively, after Ru incorporation. The similarity in N2 uptake at low relative pressures suggests that the Ru species introduced during post-treatment do not primarily reside in the micropores but rather occupied mesopores and larger pores. The cumulative pore volume data (FIG. 22) revealed a distinct reduction in the 2.2-5.8 nm size range, indicating that the Ru particles are predominantly located within this pore width range.

[0233] Compared to the 5.0 % Ru@MXene sample, the Ru particles in 5.0 % Ru@P-MXene were smaller, more uniform, and more spherical in shape. The absence of larger particles suggests better dispersion of Ru particles in the P-MXene support. The particle size distribution histogram indicated a narrower particle size distribution with an average size (i.e., diameter) of 1 .2 nm, in contrast to 1.9 nm of the 5.0 % Ru@MXene sample. The strong interaction between silica (as hard acid) and MXene functional groups (as hard base) facilitates the dispersion of Ru particles by interaction with the silanol group. Isolated silanol groups create anchoring sites for Ru particles to promote metal dispersion.2101715-001365

[0234] -42- The reducibility test for P-MXene showed that P-MXene has three peaks at 570 °C, 710 °C, and 860 °C in the H2-TPR profile. The first two peaks can be attributed to the partial reduction of titanium oxide and Ti-Ox species, as discussed in H2-TPR profile of Ru@MXene sample. However, the peak positions shifted to lower temperatures compared to MXene (i.e. , from 630 °C to 570 °C and from 805 °C to 710 °C), indicating that the titanium within the MXene structure became more accessible for reduction following pillaring. The peak at 860 °C is likely associated with the dehydroxylation of silanol groups (i.e.,

[0235]

[0236] Si-O-Si + H2O). Upon loading 5.0 % Ru into the P-MXene sample, the H2-TPR profile displayed three new reduction peaks at 80 °C, 340 °C, and 520 °C, respectively. The small peak at 80 °C is likely linked to the reduction of RuCh and / or RuOx species. The other two peaks can be assigned to the reduction of RuOx and methane formation, as discussed in H2-TPR profile of Ru@MXene sample. It should be noted that the peak at 520 °C was quite strong compared to other reduction peaks, suggesting the reduction of carbide species is easier in the P-MXene support.

[0237] XPS spectra shows the presence of characteristic peak of C-Ti at 282.0 eV in 5.0 % Ru@P-MXene, which suggests the pillarization did not influence the C-Ti bonding significantly. Additional peaks related to surface contamination were also observed at higher binding energies (285.0 to 289.0 eV). The Ru species only displayed cationic states (i.e., RuCh and RuOx).

[0238] An overview of the physiochemical properties of all of the catalytic materials used in this example can be found in Table 1 below.

[0239] Table 1: Physicochemical properties of

[0240] MAX, MXene, P-MXene, Ru@MXene and Ru@P-MXene Materials

[0241]

[0242] 2101715-001365

[0243] -43-

[0244]

[0245] Hydrogenolysis over Ru@P-MXene catalyst: The 5.0 % Ru@P-MXene catalyst was evaluated for LDPE hydrogenolysis using a LDPE-to-catalyst mass ratio of 20, at 250 °C and 3.0 MPa H2. FIG. 19 shows the catalyst achieved 78.1 % LDPE conversion in just 15 min compared to 77.1 % conversion over 4 hr with 5.0 % Ru@MXene. Notably, the liquid product (i.e., C5-35) formation rate for the 5.0 % Ru@P-MXene reached 914.9 gcs-35 gRu'1IT1, the highest value reported in the literature to date. Product analysis showed 57.2 % liquid and 17.9 % gas yields for the 5.0 % Ru@P-MXene, similar to 58.1 % liquid and 16.0 % gas yields formed over 5.0 % Ru@MXene. FIG. 19 shows the yield of fuel range products slightly decreased from 39.4 % with 5.0 % Ru@MXene to 38.1 % with 5.0 % Ru@P-MXene, while the methane yield increased slightly from 13.3 % to 14.2 %. Overall, both catalysts demonstrated similar hydrogenolysis performance, but the 5.0 % Ru@P-MXene enabled a much faster reaction rate.

[0246] The increased reaction rate can be attributed to the larger interlayer spacing enabled by pillarization of 2D MXene layers, which facilities the diffusion of LDPE polymer chains to access the active sites within the structure. While the Ru particles in the 5.0 % Ru@MXene catalyst are slightly larger on average, both catalysts produced similar methane yields. Typically, larger Ru particle sizes (i.e., > 2.5 nm) are associated with increased methane formation. However, despite the larger particle size distribution in the 5.0 % Ru@MXene, methane formation did not increase significantly. This suggests that particle shape, rather than size alone, may be responsible for the observed performance. Previous studies have indicated2101715-001365

[0247] -44-that 2D flat, disordered Ru particles suppress methane formation. The larger particles in the 5.0 % Ru@MXene appear elongated along the in-plane direction of the MXene layers, with size measurements based on their length. The thickness of the elongated Ru particles in 5.0 Ru@MXene should be smaller, which might be similar to the diameter of spherical Ru particles in 5.0 % Ru@P-MXene. Because Ru particles are sandwiched between the 2D MXene layers, the side of the Ru particles should have a greater chance of interacting with the polymer chains, leading to adsorption and reaction. Therefore, particle thickness may play a more significant role in influencing product yield than particle length.

[0248] Increasing the reaction time to 0.5 hr with the 5.0 % Ru@P-MXene catalyst resulted in 93.3 % LDPE conversion, with 63.0 % liquid, 26.4 % gas, and 47.2 % fuel range products (FIG. 23). Interestingly, the distribution of liquid products was similar to that observed in a 6-hr reaction test with 5.0 % Ru@MXene and in a 4 hr test with 7.0 % Ru@MXene (FIG. 18), except for a slightly higher methane yield. These findings further underscore the influence of Ru particle geometry on hydrogenolysis performance. The confinement of Ru particles in the interlayer spacing along the in-plane direction of 2D MXene should be responsible for particle geometry. The use of P-MXene materials in polyolefin hydrogenolysis has demonstrated significant rate enhancements due to improved mass transport and access to active sites. However, optimization of the Ru particle geometry confined by MXene layers in P-MXene support can be further studied to tune product selectivity.

[0249] The mass transport enhancement through pillarization in the 5.0 % Ru@P-MXene catalyst was further explored by using PE with a molecular weight of 76 KDa, 19 times greater than the 4 KDa LDPE. The same reaction conditions as those used for the 4 KDa LDPE were applied, with 5.0 % Ru@MXene serving as a control catalyst. As shown in FIG. 24, the reaction over 5.0 % Ru@MXene resulted in a conversion of 4.3 % after 2 hr, with product yields of 1.0 % liquid and 2.9 % gas. In contrast, in the 5.0 % Ru@P-MXene catalyst (FIG. 25), the conversion reached 29.2 % after 0.5 hr, with product yields of 14.1 % liquid and 13.4 % gas, of which 8.6 % was methane and 11.3 % were in the fuel range (i.e., C5-22). The conversions of PE with 76 KDa molecular weight in both catalysts were lower than2101715-001365

[0250] -45-the 4 KDa LDPE. PE with a higher molecular weight is likely to experience greater mass transport limitations, which hinder high conversions under the same reaction conditions as LDPE. The pillarization in MXene appears to enhance the mass transport of bulky plastic feedstock to the Ru sites within the MXene layers, thereby improving the conversion compared to the Ru@MXene catalyst.

[0251] Experiment 6: Investigating the Composition and Oxidation Status of MXene from Synthesis to Post-catalysis

[0252] Additional measurements were conducted, including XRD, EDS, XPS, and XANES, along with further analyses on five samples (e.g., MAX, MXene, P-MXene, 5.0 % Ru@MXene, 5.0 % Ru@P-MXene) at different synthesis and testing stages to better understand the composition and Ti-bonding environment of the catalysts. The EDS (FIG. 26) and XPS survey (FIG. 27) of the samples identified the elemental composition of the catalysts. The EDS data showed that MAX contains C, Ti, Al, and O. The presence of C, Ti, and Al is consistent with the expected composition of MAX, while the presence of O was unexpected based on the ideal MAX composition. However, such surface oxidation is an anticipated phenomenon, and could originate from surface oxidation of MAX due to the strong affinity toward oxygen by Ti92or adventitious species introduced during EDS measurements. The transformation of MAX into MXene introduced F and trace amounts of Cl, accompanied by the disappearance of Al, which aligns with its removal via HCI and Li F in the etching process. Upon pillaring MXene to form P-MXene, Si was introduced into the material, while Cl and F signals became very weak. The incorporation of Ru species into the MXene and P-MXene supports resulted in the appearance of Ru signals in the EDS spectra, along with a slight increase in Cl signals due to the use of hexaammineruthenium (II) chloride ([Ru(NHs)6]Cl2) precursor. The XPS survey data confirmed these findings, as shown in FIG. 27.

[0253] To investigate the presence of impurity phases (e.g., TiO2, TiOF2) in the catalysts, XRD measurements were performed on these samples. For comparison, the XRD patterns of TiO2 (e.g., Anatase and Rutile) and TiOF2 were also included. As shown in FIG. 28, MXene, 5.0 % Ru@MXene, and 5.0 % Ru@MXene (after the catalysis test) did not exhibit peaks corresponding to either TiO2 or TiOF2. A similar observation was made for P-MXene, 5.0 % Ru@P-MXene, and 5.0 % Ru@P-2101715-001365

[0254] -46- MXene after the catalysis tests. However, a slight oxidation of Ti was observed which likely originated from the material synthesis process or exposure to air.

[0255] These results indicate that complete oxidation of Ti to TiC>2 did not occur and no bulk phase of TiOs orTiOF2 formed during either the catalyst preparation or the catalytic reaction stages.

[0256] To elucidate the meaning of “T” in MXene (i.e., TisC2Tx), deconvolution of the Ti 2p, O 1s, and C 1s spectra was performed in the XPS data following the method reported by Barsoum et al (Natu, V., Benchakar et al. “A critical analysis of the X-ray photoelectron spectra of TisC2TzMXenes”, Matter (2021 ) 4, 1224-1251). All data were normalized to the binding energy of carbon atoms in the Ti octahedra within the MXene, and P-MXene layers (i.e., 282.0 eV) and to the binding energy of adventitious carbon at 248.8 eV for MAX phase. Given the absence of the TiC impurity phase, as confirmed by XRD data, the spectra were fitted with two asymmetric peaks representing the 2p3 / 2and 2pi / 2 spin-orbit split Ti-C components, where the binding energy depends on local bonding with termination species such as fluorine (F) and oxygen (O). Additionally, two asymmetric peaks were included to represent Ti-0 components (e.g., TiCk). In the MAX phase, these two sets of peaks appeared at 454.6 and 460.6 eV (for Ti-C peaks), as well as 458.7 and 464.4 eV (forTi-0 peaks), respectively. In MXene materials, all four peaks shifted to higher binding energies.

[0257] The first set of peaks (i.e., Ti-C) was further deconvoluted into four pairs, following Barsoum et al., and assigned to C-Ti-O / O / O, C-Ti-O / O / F, C-Ti-O / F / F, and C-Ti-F / F / F octahedra, respectively. In these notations, 7” denotes termination species. The second set of peaks was assigned to TiC>2-xF2x. It is worth noting that the binding energy (BE) of pure TiO2 oxides is reported to be about 458.6 eV, which is significantly lower than the values observed for the samples. This suggests that the TiC>2-xF2x in MXene are not equivalent to the Ti©2 phase. Therefore, the “T” species in the MXene samples contain both Ti-F and Ti-0 bonds. For the P-MXene sample, the peaks associated with C-Ti bonds were very weak, whereas the TiO2-x-related peaks were significantly stronger, with a slight shift to higher BE. The pillarization of MXene introduced SiC>2 species, which diluted the Ti-C signal, making these peaks less prominent.2101715-001365

[0258] -47- To further investigate the oxygen termination species, the O 1s spectra was analyzed. The peaks were assigned to C-Ti-O, C-Ti-OH (or C-Ti-O / F), and adsorbed water. In the MAX phase, the dominant species were C-Ti-O, C-Ti-OH. Upon transformation into MXene, these peaks shifted slightly to higher BE and were assigned to C-Ti-O, TiO2-xF2x, C-Ti-OH\O\F, and adsorbed water. In P-MXene, the peaks further shifted to even higher BE, with the C-Ti-O peak remaining around 530.7 eV. A distinct peak corresponding to the Si-0 bond appeared due to the presence of SiO2 species introduced during the pillarization treatment.

[0259] Both MAX and MXene exhibited a Ti-C peak at 281.5 and 282 eV, respectively. However, in P-MXene, this peak was significantly weaker due to pillarization of MXene with SiO2 species. Other peaks were attributed to adventitious carbon species. Finally, the introduction of Ru species into MXene and P-MXene appear to influence slightly the XPS spectra. As shown Table 2 and 3, the peak positions in Ru-loaded samples slightly shifted to higher BE compared to those of the bare support materials.

[0260] Table 2: Summary of XPS Fittings over 5.0 % Ru@MXene and 5.0 % Ru@P- MXene

[0261]

[0262] 2101715-001365

[0263] -48-

[0264]

[0265] Table 3: Summary of XPS Fittings over 3.0 %, 5.0 %, and 7.0 % Ru@MXene

[0266]

[0267] 2101715-001365

[0268] -49-

[0269]

[0270] The Ti K-edge XAFS spectra in the near-edge region were also measured for as-lyophilized MXene (i.e., Ex Situ: As-Prepared), the as-lyophilized MXene after sample preparation for in situ measurements and under N2 (i.e., In Situ: Pre-reduction), and in situ reduction of as-lyophilized MXene (i.e., In Situ: Reduced), and 5.0 % Ru@MXene in its as-lyophilized (i.e., Ex Situ: As-Prepared), ex-situ reduced, and ex-situ after reaction (Reaction conditions: 4 KDa LDPE-to-catalyst mass ratio of 20, 250 °C, 4 h, and 3.0 MPa H2) stages to understand the bonding environment of Ti species. The Ti K-edge spectrum of as-lyophilized MXene exhibited features similar in position to those exhibited by anatase TiO2, suggesting some similarity in oxidation state between Ti in this MXene sample and those in anatase. Nonetheless, it should be noted that the MXene’s spectral shape is2101715-001365

[0271] -50-distinctfrom anatase, indicating differences in electronic structure, and that its features are similar to other Ti K-edge measurements of MXenes in the literature. These findings are consistent with the XPS results discussed above. The in-situ pre-reduction spectrum of MXene revealed that the sample preparation for the X-ray measurements did not significantly change the chemistry of the sample.

[0272] Interestingly, the MXene sample largely maintained its electronic structure upon exposure to a 5.0 % H2 flow (with the balance being N2) and temperatures of 300 °C for approximately 1 hr, other than slight changes in the pre-edge and shoulder regions.

[0273] The Ti K-edge spectra of 5.0 % Ru@MXene differed significantly. In the presence of Ru, the Ti species in as-lyophilized 5.0 % Ru@MXene appeared more reduced, as indicated by an edge position slightly lower in energy than the previous MXene spectra. Interestingly, the reduced and after reaction samples, which are similar to each other in shape, appeared more oxidized than the as-lyophilized sample and bear some similarity to anatase. This behavior is similar to observations of other MXenes in the literature that have been treated with high temperatures. As reported there, this behavior is likely due to some oxidation of the MXene, though not a complete transformation to TiC>2. Moreover, the lack of oxidation observed in situ, despite higher temperatures and lower hydrogen pressures, indicates that the sample may simply be liable to oxidation under ambient environments after reduction or reaction events rather than oxidized during reaction.

[0274] Across all tested stages, complete oxidation of Ti to TiC>2 did not occur, indicating that Ti primarily remained in the Ti-F / O state during catalytic testing. The observed oxidation features likely originated from the material synthesis process or exposure to air, as MXene is known to undergo gradual oxidation when exposed to air or water. These results suggest that “T” primarily consists of O, F, or -OH species, introduced either during sample preparation or through air exposure. The exposure to hydrogen under a diluted H2 flow did not significantly alter the termination species, but the presence of Ru appears to induce some degree of MXene reduction.

[0275] Conclusions of Example 12101715-001365

[0276] -51- In summary, this example studied 2D MXene-supported Ru catalysts (Ru@MXene) for the hydrogenolysis of LDPE into liquid fuels. The Ru@MXene catalyst was prepared by lyophilizing a solution containing dispersed MXene sheets and Ru precursors, resulting in the incorporation of Ru species into the interlayer spaces of the MXene. This led to the formation of Ru-pillared structures, which expanded the interlayer distance. Increasing the Ru mass fraction promoted the formation of larger Ru particles and shifted the Ru oxidation states towards a more metallic form. The 2D MXene layers confined the Ru particles, leading to elongated particle shapes with their length oriented along the in-plane direction of the MXene layers, when the Ru loading was high.

[0277] Reaction tests examined key parameters, including temperature, H2 pressure, reaction time, and Ru loading, revealing their influence on the efficiency and yield of LDPE hydrogenolysis. However, diffusion limitations that hindered polymer-catalyst interactions posed challenges to catalytic performance. To address these limitations, a silica-pillared MXene-supported Ru catalyst (Ru@P-MXene) was developed. The introduction of silica pillars significantly expanded the interlayer distance, thereby mitigating diffusion constraints and improving access to active sites.

[0278] The Ru@P-MXene catalyst exhibited a remarkably high rate of liquid product formation during LDPE hydrogenolysis. A comparison of methane yields between Ru@P-MXene and Ru@MXene suggests that Ru particles confined within the 2D MXene support predominantly expose their side facets during reactions, which does not enhance methane formation despite their larger size. This indicates that tailoring particle geometry through confinement within the interlayer spacing of MXene could help reduce methane formation while optimizing liquid fuel production. Overall, these findings underscore the potential of the catalytic materials disclosed herein in addressing critical challenges in plastic waste upcycling and advancing the development of efficient, sustainable catalytic processes for the future.

[0279] Example 2:

[0280] This example describes an exemplary pillared TiO2 catalyst support material possessing improved surface areas.2101715-001365

[0281] -52- Materials and Methods of Example 2:

[0282] Chemicals

[0283] Hydrochloric acid (HCI, 37%), lithium fluoride (LiF, >99.9%), dodecylamine (DDA, 98%), and hexaammineruthenium (II) chloride ([Ru(NH3)e]Cl2), and low-density polyethylene (LDPE, Mw about 4kDa) were purchased from Sigma-Aldrich. Ti3AIC2 MAX powder was obtained from Tongrun Info Technology Co. Ltd, China. Tetraethyl orthosilicate (TEOS, 98%) was purchased from Alfa Aesar. Deionized (DI) water was used in this example.

[0284] Material Synthesis

[0285] Synthesis of 2D MXene Material

[0286] TisC2Tx MXene nanosheets were synthesized by selectively etching the Al layer from TisAIC2 MAX phase. Specifically, 1 .0 g of TisAIC2 MAX powder was added to a mixture of 40 mL of 9.0 M HCI solution and 3.0 g of LiF. The mixture was stirred magnetically at 35 °C for 24 hr at 400 rpm. After etching, the resulting suspension was centrifuged at 8000 rpm for 5 min. Following decantation of the supernatant, cold 2.0 M HCI was added to the precipitate and mixed to form a suspension. This centrifugation-decantation-redispersion process in cold HCI was repeated three times to remove residual ions and byproducts. The HCI solution was then replaced with DI water, and the washing process was repeated until the suspension reached a pH of about 6.0. Subsequently, the mixture was sonicated for 60 min to produce delamination, followed by centrifugation at 3000 rpm for 30 min. The delaminated TisC2Txnanosheets (MXene) in the supernatant was collected by lyophilization using a freeze dryer at -85 °C and 101 Pa pressure for further synthesis and characterization.

[0287] Synthesis of pillared MXene (P-MXene)

[0288] In this example, 0.5 g of MXene dry powder was mixed with 5.0 g of DDA and 10.0 g of TEOS in a glass flask at ambient temperature. The mixture was purged with an argon gas flow for 15 min, sealed, and stirred at 200 rpm for 4 hr. Afterward, the suspension was filtered, and the resulting solid residue was dried in a vacuum oven for 18 hr. The dried sample was then dispersed in 25 mL of DI water in a centrifuge tube and left at ambient temperature for 18 hr without stirring. The product was collected by filtration and dried overnight at 60 °C in a vacuum.2101715-001365

[0289] -53- Finally, the product underwent heat treatment, for which the temperature ramped to 400°C at a rate of 1.0 °C min-1and was maintained at this temperature for 12 hr under N2 with a flow rate of 100 mL min-1, resulting in the formation of pillared MXene, which is hereafter referred to as P-MXene in this example.

[0290] Syntheses of pillared T1O2 (P-T1O2) and carbon-containing pillared T1O2 (C-P-TiO2)

[0291] After obtaining P-MXene, the material was calcined under 550 °C (ramped at a rate of 1 .0 °C min-1from room temperature (RT)) for 12 hr under air with a flow rate of 100 mL min-1, or 410 °C for 24 hr under the same airflow rate, to synthesize P-TiO? and C-P-TiO?.

[0292] Syntheses of pillared TiO2 supported Ru (Ru@P-TiC>2) and carbon-containing pillared TiO2 supported Ru (Ru@C-P-TiO2)

[0293] Ru@P-TiO2 and Ru@C-P-TiC>2 catalysts were prepared using an incipient wetness impregnation approach. First, a [Ru(NHs)6]Cl2 stock solution (0.1 mol L-1) was added in a dropwise fashion to the prepared P-TiO2 or C-P-TiC>2, and then the materials were dried under 60 °C in a vacuum oven for 2 hr. Finally, the prepared Ru@P-TiO2 and Ru@C-P-TiO2 samples were reduced in a tubular furnace at 300 °C for 2 hr (ramp rate of 5.0 °C min-1) under a H2 gas flow (a 5.0% volume fraction of H2 in a N2 mixture; flow rate of 100 mL min-1). The Ru loading in Ru@P-TiC>2 and Ru@C-P-TiC>2 are about 5wt%.

[0294] Characterizations

[0295] X-ray diffraction (XRD) measurements were conducted on a Bruker D8 diffractometer with Cu Ko radiation (A =1.54 A) over a 20 range of 15 - 40°. N2 adsorption-desorption isotherms were collected at -196.15 °C using a Micromeritics 3Flex surface characterization analyzer. Prior to measurements, samples were degassed at 130 °C under vacuum for 16 hr. The pore size distribution was determined by density functional theory (DFT) based on the adsorption branch of isotherms. The total surface area was calculated by the Brunauer-Emmett-Teller (BET; using adsorption branch of the N2 isotherm data, P / Po = 0.05-0.35). Morphological features of the samples were characterized by scanning electron microscopy (SEM, Zeiss Merlin) and transmission electron microscopy (TEM, JEOL JEM-201 OF).2101715-001365

[0296] -54- Catalytic Hydrogenolysis Tests

[0297] Hydrogenolysis of LDPE was conducted in a 50 mL stainless steel Parr batch reactor. A total of 0.1 g of the reduced Ru@P-TiC>2 or Ru@C-P-TiO2 catalyst and 2.0 g of LDPE (feed-to-catalyst ratio of 20:1 ) were added to the reactor. The reactor was then sealed, purged 5 times with H2 at 15 bar, and subsequently pressurized to 30 bar H2 at room temperature (about 20 °C). The reactor was placed on a heating stirrer set to 500 rpm and heated to 250 °C. The gaseous products (C1-C4) were collected in a 1 L Tedlar gas sampling bag and analyzed using GC-FID (Agilent CP-Volamine GC column). The residual content in the reactor was treated with about 20 mL of methylene chloride (CH2CI2, HPLC grade, 23 99.9%) containing 20 mg of n-octacosane (C28H58, 5= 98.0%) as an external standard. After filtration, the soluble fraction was defined as the liquid products (Cs-C35), while the unreacted polymer retained on the filter paper was classified as solid residue (>C3s). The liquid products were analyzed by GC-FID (Agilent HP-1 column) and identified by GC-MS (Agilent DB-1 column). Product yields for both gas and liquid phases were calculated on a molar basis. Polymer conversion was determined gravimetrically, based on the mass difference between the initial amount of polymer added and the unreacted residue collected on the filter paper.

[0298] Experiments and Results

[0299] By using thermogravimetric analysis (TGA), Ti was observed to undergo oxidation first at about 300 °C to form TiO2, and C was observed to undergo oxidation at about 550 °C to form CO2. Hence, a temperature of 410 °C was utilized to calcine P-MXene to synthesize C-P-TiO2, while 550 °C was selected to synthesize P-TiO2.

[0300] X-ray diffraction patterns were used to analyze the crystal structures of C-P-TiC>2 and P-TiO2. As shown by FIG. 29, both 410 °C- and 550 °C-treated samples exhibited characteristic reflections assigned to either anatase or rutile phase, indicating P-MXene was successfully converted into TiO2 structures. Under SEM (FIG. 30), both C-P-TiO2 and P-TiO2 showed an irregular morphology (with a crystal size of tens of microns) with a rough surface, and TEM (FIG. 30) displayed a layered structure of P-TiO2, and in addition, silica pillar particles were clearly visible2101715-001365

[0301] -55-within the galleries of P-TiO2, thereby suggesting the pillared structure of P-MXene was retained during the synthetic process for P-TiO2.

[0302] N2 adsorption-desorption isotherms were used to evaluate the textural properties of P-TiCh and C-P-TiO2. As shown in FIG. 31, the adsorption isotherms of both materials rose progressively at low relative pressures (P / Po < 0.48), consistent with micropore filling; the pronounced hysteresis at 0.48 < P / Po < 1.00 arose from capillary condensation in mesopores, and the persistence of the loop approaching P / Po about 1.00 suggests the presence of macropores as well. Both of the isotherms of P-TiO2 and C-P-TiO2 are type II with an H3 hysteresis loop, indicative of existence of wedge-shaped mesopores. The pore size distribution and cumulative pore volume data (FIG. 32) confirmed a hierarchy of micro-, meso-, and macropores in both P-TiO2 and C-P-TiO2, with a dominant pore width of about 67 nm for P-TiO2 (consistent with the TEM observations (FIG. 30), and about 120 nm for C-P-TiO2. However, the cumulative pore volume and BET surface area of P-TiO2were 0.67 cm3 / g and 425.6 m2 / g, respectively, which are both greatly larger than C-P-TiO2 (0.50 cm3 / g and 343.0 m2 / g, respectively), and this might be explained by that the existence of carbon in C-P-TiO2 occupies some of the internal space of the sample. Notably, as compared in Table 4, the surface areas of both P-TiO2and C-P-TiO2are even 2-3 times larger than some of the best commercial TiC>2 supports, indicating the great potential of the synthesized pillared TiO2 catalyst supports in improving the dispersion of loaded catalysts.

[0303] Table 4: Surface Areas of Mesoporous TiO2 catalysts

[0304]

[0305] 2101715-001365

[0306] -56-

[0307]

[0308] The hydrogenolysis of low-density polyethylene (LDPE) was using Ru@P-TiO2 and Ru@C-P-TiO2 catalysts was next explored. The reaction was carried out under 250 °C and 30 bar H2 for 30 min, with a LDPE feed / catalyst mass ratio at 20.2101715-001365

[0309] -57- As shown in FIG. 33, Ru@C-P-TiO2 exhibited a relatively lower activity, achieving a 28.2% conversion after 0.5 hours. The product distribution consisted of 9.2% gas, 14.8% liquid, and 71.5% solid residue, with methane as the dominant gaseous product. In contrast, Ru@P-MXene delivered significantly enhanced performance, reaching 97.2% conversion within the same time. The product distribution shifted markedly toward more volatile products, with 35.8% gas, 60.4% liquid, and 2.4% solid (FIG. 33). Methane again dominated the gaseous fraction. The superior activity of Ru@P-TiO2 stems from the comparatively larger surface area and pore volume, which can alleviate diffusion limitations and enhance the accessibility of polymer chains to Ru active sites.

[0310] Example 2 Conclusion

[0311] This example demonstrated that a MXene-derived strategy was capable of synthesizing high-surface-area, pillared TiO2catalyst supports with well-defined hierarchical porosities. By calcining silica-pillared Ti3C2TxMXene under controlled oxidative conditions, the titanium carbide lattice was successfully converted into crystalline TiO2while preserving the pillared architecture. Two distinct materials were obtained depending on calcination temperature: fully oxidized P-TiO2and carbon-containing C-P-TiO2. Both materials exhibited a combination of micro-, meso-, and macropores, with record-high BET surface areas of 425.6 m2g“1and 343.0 m2g-1, respectively, exceeding those of conventional TiO2supports.

[0312] When evaluated as supports for Ru-catalyzed LDPE hydrogenolysis, P-TiO2enabled markedly enhanced catalytic performance, achieving near-complete polymer conversion under mild reaction conditions. The superior activity was attributed to the large surface area and pore volume, which promoted high Ru dispersion and improved accessibility of polymer chains to active sites. While partial carbon retention in C-P-TiO2reduced accessible porosity and catalytic activity relative to P-TiO2, it offers a tunable platform to further investigate metalsupport interactions and potential hydrogen spillover effects.

[0313] Overall, this study establishes pillared MXene-derived TiO2as a new class of high-performance catalyst supports with unprecedented surface areas and tunable compositions.

[0314] Example 3:2101715-001365

[0315] -58- This example describes an exemplary process for producing the catalyst materials disclosed herein.

[0316] Materials and Methods of Example 3:

[0317] Materials

[0318] Hydrochloric acid (HCI, 37%), lithium fluoride (LiF, > 99.9%), dodecylamine (DDA, 98%), octadecylamine (ODA, 98%), hexylamine (HA, 99%), and hexaammineruthenium (II) chloride ([Ru(NH3)e]Cl2), and low-density polyethylene (LDPE, Mw about 4kDa) were purchased from Sigma-Aldrich. TisAIC2 MAX powder was obtained from Tongrun Info Technology Co. Ltd, China. Tetraethyl orthosilicate (TEOS, 98%) was purchased from Alfa Aesar. Deionized (DI) water was used in the experiment.

[0319] Material synthesis

[0320] Synthesis of 2D MXene Material: TisC2Tx MXene nanosheets were synthesized by selectively etching the Al layer from TisAIC2 MAX phase.

[0321] Specifically, 1 .0 g of TisAIC2 MAX powder was added to a mixture of 40 m L of 9.0 M HCI solution and 3.0 g of LiF. The mixture was stirred magnetically at 35 °C for 24 h at 400 rpm. After etching, the resulting suspension was centrifuged at 8000 rpm for 5 min. Following decantation of the supernatant, cold 2.0 M HCI was added to the precipitate and mixed to form a suspension. This centrifugation-decantation-redispersion process in cold HCI was repeated three times to remove residual ions and byproducts. The HCI solution was then replaced with DI water, and the washing process was repeated until the suspension reached a pH of about 6.0. Subsequently, the mixture was sonicated for 60 min to produce delamination, followed by centrifugation at 3000 rpm for 30 min. The delaminated TisC2Txnanosheets (MXene) in the supernatant was collected by lyophilization using a freeze dryer (Labconco FreeZone) at -85 °C and 101 Pa pressure for further synthesis and characterization.

[0322] Synthesis of 2D P-MXene Material: Proper amounts of MXene and amine swelling agent (0.01 - 1.0g of MXene and 0.01 -20g of amine swelling agent) were added to a glass vial. After mixing the two materials, the vial was transferred into a 50 mL Teflon liner, which was then placed within a stainless-steel autoclave.

[0323] Subsequently, TEOS was added to the Teflon liner, outside the glass vial. The2101715-001365

[0324] -59-autoclave was sealed and placed in a preheated oven at target temperature for 24 h. The autoclave was then removed from the oven and allowed to cool in a fume hood. Proper amount of water was added to the space between the outer wall of the glass vial and the inner wall of the Teflon liner. The autoclave was sealed again and heated in an oven preheated to 80 °C for another 24 h. After cooling, the material in the glass vial was transferred into a furnace for calcination. The calcination process involved ramping from ambient temperature to 400 °C at a rate of 0.8 °C / min, followed by holding at the final temperature for 12 h under a N2 gas (Purity: 99.999%; Airgas) flow of 100 mL / min. This synthesized pillared MXene material is named “P-MXene” in this Example.

[0325] Synthesis of MXene or P-MXene Supported Ru Catalysts’. The MXene-supported Ru catalyst (i.e., Ru@MXene) was synthesized by adding 5.2 g of a 0.1 M hexaammineruthenium (II) chloride solution to 1 g MXene, followed by mixing at 500 rpm stirring for 60 min. The resulting mixture was then lyophilized using a freeze dryer at -85 °C and 101 Pa pressure. After freeze drying, the sample was reduced in a tubular furnace at 300 °C for 2 h with a ramp rate 5 °C / min under a 5% H2 / N2 gas mixture flowing at 100 mL / min. The P-MXene-supported Ru (i.e., Ru@P-MXene) catalyst was prepared using an incipient wetness impregnation approach. First, a [Ru(NH3)e]Cl2 stock solution (0.1 mol L-1) was added in a dropwise fashion to the prepared P-MXene, and then it was dried under 60 °C in a vacuum oven for 2 h. Finally, the prepared Ru@P-MXene sample was also reduced according to the same method as Ru@P-MXene. The Ru loading in Ru@MXene or Ru@P-MXene was 5wt%, and both catalysts were ready for catalytic testing.

[0326] Materials Characterization

[0327] X-ray diffraction (XRD) measurements were conducted on a Bruker D8 diffractometer with Cu Ko radiation (A =1.54 A) over a 20 range of 15 - 40°. For diffraction angles below 15°, small-angle X-ray scattering (SAXS) was performed using a Xenocs Xeuss 3.0 instrument equipped with a D2+ MetalJet X-ray source (Ga Ka, 9.2 keV, A = 1.34 A). N2 adsorption-desorption isotherms were collected at -196.15 °C using a Micromeritics 3Flex surface characterization analyzer. Prior to measurements, samples were degassed at 130 °C under vacuum for 16 h. The pore size distribution and cumulative pore volume were determined by density functional2101715-001365

[0328] -60-theory (DFT) based on the adsorption branch of isotherms. The total and micropore surface areas were calculated by the Brunauer-Emmett-Teller (BET; using adsorption branch of the N2 isotherm data, P / Po = 0.05-0.35) and t-plot methods (P / Po< 0.1), respectively. The mesopore surface area was obtained by subtracting the micropore surface area from the BET surface area. The micropore volume was taken from the cumulative pore volume at pore sizes < 2 nm, the mesopore volume from the cumulative pore volume between 2-50 nm, and the macropore volume from pore sizes > 50 nm, based on the cumulative pore volume distribution.

[0329] Morphological features of the samples were characterized by scanning electron microscopy (SEM, Zeiss Merlin) and transmission electron microscopy (TEM, JEOL JEM-201 OF). Raman spectra were acquired using a Raman spectrometer (LabRAM HR Evolution, Horiba Scientific, Japan), and the measuring conditions include acquisition time of 10 s, three accumulations, RTD time of 1 s, excitation at 532 nm, neutral density filter set to 3.2%, confocal hole size of 200, and a 600 grating (500 nm) in the visible range. The instrument was calibrated using the Si Raman peak at 520.8 cm-1. For the sample preparation, the dried powder was sandwiched between two glass microscope slides and pressed to obtain flat MAX or MXene particles. X-ray photoelectron spectroscopy (XPS) was performed using a Kratos Axis Supra+ spectrometer with an Al Ka X-ray source.

[0330] For the Ru@MXene and Ru@P-MXene samples, a JEOL JEM-ARM200F transmission electron microscope operated in scanning transmission electron microscopy (STEM) mode at 200 kV accelerating voltage was used to analyze the Ru morphologies via high-angle annular dark field (HAADF-STEM) imaging.

[0331] Samples were prepared by dispersing the catalyst powders in ethanol, followed by 30 min of sonication. The resulting suspension was drop-cast onto lacey carbon grids and dried prior to imaging. Elemental mapping was performed using energy-dispersive X-ray spectroscopy (EDS) with an Oxford XMAX TLE 100 mm2windowless EDS detector integrated with the ARM200F microscope.

[0332] Catalytic Hydrogenolysis Tests

[0333] Hydrogenolysis of LDPE was conducted in a 50 mL stainless steel Parr batch reactor. A total of 0.1 g of the reduced Ru@MXene or Ru@P-MXene catalyst and 2.0 g of LDPE (feed-to-catalyst ratio of 20:1) were added to the reactor. The2101715-001365

[0334] -61-reactorwas then sealed, purged 5 times with H2 at 15 bar, and subsequently pressurized to 30 bar H2 at room temperature (about 20 °C). The reactor was placed on a heating stirrer set to 500 rpm and heated to 250 °C. The gaseous products (C1-C4) were collected in a 1 L Tedlargas sampling bag and analyzed using GC-FID (Agilent CP-Volamine GC column). The residual content in the reactor was treated with about 20 ml_ of methylene chloride (CH2CI2, HPLC grade, > 99.9%) containing 20 mg of n-octacosane (C28H58, > 98.0%) as an external standard. After filtration, the soluble fraction was defined as the liquid products (C5-C35), while the unreacted polymer retained on the filter paper was classified as solid residue (>C3s). The liquid products were analyzed by GC-FID (Agilent HP-1 column) and identified by GC-MS (Agilent DB-1 column). Product yields for both gas and liquid phases were calculated on a molar basis. Polymer conversion was determined gravimetrically, based on the mass difference between the initial amount of polymer added and the unreacted residue collected on the filter paper.

[0335] Results and Experiments

[0336] Experiment 1: Exploring the Benefits of Transitioning from Liquid Phase to Vapor-phase Pillarization of MXene

[0337] Silica-pillared MXene has previously been synthesized through liquid-phase processing, which requires large amounts of solvent and multiple operational steps. One report from Shaikh et al. (Al Shaikh, R. et al., “MXene-Based Materials for Proton-Exchange Membrane Fuel Cell Applications”, Cell Rep. Phys. Sci. 2026, 7 (1)) involved co-intercalation of DDA and TEOS, followed by hydrolysis in water. In Shaikh et al., MXene was dispersed in a solution of DDA dissolved in TEOS under an argon (Ar) atmosphere at room temperature, with a typical molar ratio of MXene / DDA / TEOS = 1:6-10:15-20. After filtration and drying, the intercalated MXene was dispersed in water at a MXene / water mass ratio of 1 :50. After drying, the sample at this stage exhibited a surface area of 235 m2 / g and a pore size of about 10 A. The sample was then calcined in Ar at 400 °C to remove trapped DDA while preserving the pillared structure. The surface area was changed to 141 m2 / g with a pore size of about 32 A after calcination.

[0338] Another study by Ruiz-Hitzky et al. (Ruiz-Hitzky, E. et al, “Silica-Ti3C2Tx MXene Nanoarchitectures with Simultaneous Adsorption and Photothermal2101715-001365

[0339] -62- Properties”, Materials 2024, 17 (17)) reported a synthesis process involving intercalation, hydrolysis, and extraction steps. First, MXene was dispersed in a cetyltrimethylammonium bromide (CTAB) solution at a mass ratio of MXene / CTAB / water = 1:0.25:200. After drying, the CTAB-intercalated MXene was redispersed in isopropanol, followed by the addition of tetramethyl orthosilicate (TMOS) for intercalation and a water / methanol mixture forTMOS hydrolysis (molar ratio MXene / TMOS / water / methanol = 1:1:2:2). After centrifugation and drying, CTAB was removed from the sample using a hydrochloric acid / ethanol solution at 70 °C. The final dried material exhibited a surface area of 290 m2 / g with an average pore width of about 120 A.

[0340] In view of these prior liquid-phase pillaring protocols, a vapor-phase operation route was developed that reduces solvent use, minimizes operational steps, and generates less liquid waste for the synthesis of silica-pillared MXene. The reagents used in this Example mirror those used in LPP methods: DDA as the swelling agent, TEOS for intercalation precursor, and water for hydrolysis. To prevent premature interaction between DDA and TEOS before diffusion into MXene, DDA and MXene were co-located in a container while keeping TEOS in a separate compartment (FIG. 34). Because DDA melts at about 27-31 °C but boils near 247-249 °C, an intercalation temperature between its melting and boiling points (e.g., 100 °C) was selected to limit volatilization. Upon heating, the molten DDA was drawn into the MXene galleries by capillary forces. TEOS boils near 168-170 °C, so operating below its boiling point slowed undesired hydrolysis with exterior -OH groups on MXene and allowed deeper penetration into the galleries. Hydrolysis was then carried out in the same setup by replacing the TEOS source with water and lowering the temperature to 80 °C.

[0341] Two VPP regimes were tested: (i) DDA loading comparable to the liquidphase process with reduced TEOS (e.g., mass ratio of MXene / DDA / TEOS = 1 :5-20:0.1-1), and (ii) TEOS loading comparable to the liquid-phase process with reduced DDA (e.g., mass ratio of MXene / DDA / TEOS = 1:0.8:1.6-20). These experiments defined practical reagent windows for producing silica-pillared MXene while substantially lowering overall reagent consumption. For comparison, two trials without DDA and with a MXene / DDA ratio of 10 were conducted, but with DDA2101715-001365

[0342] -63-placed with TEOS together, both staying outside the MXene compartment. In the absence of DDA, the N2 isotherm of the product closely matched that of pristine MXene, indicating minimal interlayer expansion and limited TEOS access. When DDA was added to the TEOS compartment, its high boiling point hindered effective evaporation and diffusion into the MXene galleries, yielding only a slight increase in N2 uptake. Collectively, these results suggest that the identified VPP conditions are appropriate for synthesizing mesoporous P-MXene.

[0343] Experiment 2: Verification of VPP Effectiveness in Synthesizing Silica-pillared MXene

[0344] To evaluate the effectiveness of the VPP process for synthesizing silica-pillared MXene, an intercalation mass ratio of MXene / DDA / TEOS = 1:10:0.5 was first explored. Assuming a MXene composition of TisC2-OH, the corresponding molar ratio of MXene / DDA / TEOS is 1:10:0.9. In the subsequent hydrolysis step, the MXene / FW mass ratio was 1:10, equivalent to a molar ratio of 1 :103. Intercalation was carried out at 100 °C for 24 h, followed by hydrolysis at 80 °C for 24 h. The resulting material was then calcined under a N2 atmosphere at 400 °C for 12 h. These conditions were defined as the baseline for further investigating the effects of VPP parameters on the synthesis of silica-pillared MXene.

[0345] The elemental compositions of MXene and P-MXene were analyzed using energy-dispersive X-ray spectroscopy (EDX) measurements, with the parent MAX phase included for comparison. The MAX showed a stoichiometry of Ti1.6C1.0AI0.9O06. In the etched MXene, Al atomic composition was reduced to 0.4%, confirming successful removal of Al layers (Table 5).

[0346] Table 5: Atomic Compositions for MAX, MXene, and P-MXene measured by

[0347] EDX

[0348]

[0349] * Synthesis condition: VPP, MXene / DDA / TEOS / FhO = 1 :10:0.5:10 (mass ratio), intercalation at 100 °C, hydrolysis at 80 °C.2101715-001365

[0350] -64- ** Synthesis condition: VPP, MXene / DDA / TEOS / F = 1:0.8:6.4:10 (mass ratio), intercalation at 100 °C, hydrolysis at 80 °C.

[0351] The MXene composition is Ti1.5C10AI0.02O15X0.9 (X stands for F and Cl) from the EDX data. The slightly lower Ti / C ratio relative to MAX suggests that minor Ti dissolution during etching, and the presence of F and Cl, and increased O content indicates the formation of surface terminations. After vapor-phase pillarization, the P-MXene exhibited a composition of Tii.iCi.oAlo.oi02.3Xo.3Sio.i, which means Ti and C were largely retained, while the increases in O and Si confirm successful incorporation of silica pillars. The reduced X content points to partial loss of F / CI terminations during VPP. No nitrogen (N) signal was observed, consistent with removal of DDA during calcination.

[0352] Because EDX is insensitive to hydrogen, Raman spectroscopy was used to probe -OH and / or -O surface terminations in MXene and P-MXene (FIG. 35). The MAX precursor showed a sharp band at about 198 cm-1(Ti-O) and a weaker band at about 270 crrr1(Ti-OH). Both features persist in the etched MXene phase. After VPP, the P-MXene retains the about 198 cm-1band, whereas the about 270 cm-1band disappears, consistent with consumption of Ti-OH groups during silica pillar formation. A new band at about 152 cm'1can be assigned to Ti-Si-0 linkage formed during VPP. Additional bands below 1000 cm'1are attributable to overlapping Ti-X vibrations (X = F, Cl). The broad band at 1200 - 1700 cm'1in both MXene and P-MXene indicates the presence of amorphous carbon, likely due to slight overetching of the MAX precursor.

[0353] X-ray diffraction patterns (FIG. 36) were used to analyze the crystal structures of MXene and P-MXene. MXene exhibited characteristic reflections at 20 about 8.4°, 25.3°, and 38.0°, indexed to the (002), (006), and (008) planes, respectively. No diffraction peaks from the parent MAX phase were observed, which indicates successful etching to the MXene phase. Notably, the (002) peak shifts from 20 about 9.5° (MAX) to 8.4° (MXene), evidencing an increased interlayer spacing per Bragg’s law. From the (002) reflection, the calculated d-spacing in MXene is about 1.1 nm. The average interlayer spacing can be estimated by subtracting the layer thickness (i.e. , 0.9 nm, obtained by the TEM result discussed below) from the d-spacing, yielding about 0.2 nm. After VPP, the (002) peak further2101715-001365

[0354] -65-shift to 20 about 6.7°, corresponding to d-spacing of about 1.3 nm and a gallery height of about 0.4 nm. This trend followed previous reports on MXene pillarization via the LPP approach.

[0355] The morphology of MXene and P-MXene was characterized using SEM and TEM imaging. The parent MAX phase exhibited a compact, densely layered structure. After selective Al etching, the resulting MXene displayed thin, flexible, sheet-like morphologies with curled edges (FIG. 37). Following VPP pillarization, the P-MXene retained its sheet-like architecture. However, the sheets appeared narrower, thicker, and with straighter edges (FIG. 37). TEM images further resolved the internal stacking. MXene showed multiple stacked layers with an individual layer thickness of about 0.90 nm and an interlayer spacing of about 0.25 nm (FIG.

[0356] 37), in good agreement with the XRD-derived gallery height (FIG. 36). After VPP, the interlayer spacing of P-MXene increased substantially to about 5-20 nm, while the single-layer thickness remained about 0.90 nm (FIG. 37). Silica pillar particles were clearly visible within the galleries of P-MXene. The broad distribution of interlayer distances indicates that pillars form non-uniformly between adjacent MXene nanosheets.

[0357] N2 adsorption-desorption isotherms were used to evaluate the textural properties of MXene and P-MXene. As shown in FIG. 38, MXene exhibits very limited N2 uptake across the entire relative pressure range. A closer look at FIG. 38 indicates a type II isotherm with an H3-type hysteresis loop, according to IUPAC classification. The hysteresis loop is characteristic of a plate-like layered structure that contains wedge-shaped pores among stacked MXene nanosheets. Overall, MXene displayed a low total pore volume (0.014 cm3 / g) and a low BET surface area (4 m2 / g), as corroborated by the pore size distribution (FIG. 38) and cumulative pore volume data (Table 6).

[0358] Table 6: Surface Areas and Pore Volumes of MXene and P-MXene

[0359] Materials

[0360]

[0361] 2101715-001365

[0362] -66- * Synthesis condition: VPP, MXene / DDA / TEOS / FhO = 1 :10:0.5:10 (mass ratio), intercalation at 100 °C, hydrolysis at 80 °C.

[0363] In contrast, P-MXene displayed markedly higher N2 uptake across the full relative pressure range (FIG. 38). The adsorption isotherm rose progressively at low relative pressures (P / Po < 0.48), consistent with micropore filling. The pronounced hysteresis at 0.48 < P / Po < 1.00 arose from capillary condensation in mesopores. The persistence of the loop approaching P / Po about 1.00 suggests the presence of macropores as well. The isotherm was also type II with an H3 hysteresis loop, indicative of existence of wedge-shaped mesopores. The amount of these pores increased significantly more than the MXene sample. The pore size distribution and cumulative pore volume data (FIG. 38 and Table 6) confirm a hierarchy of micro-, meso-, and macropores in P-MXene, with dominant pore widths in the mesopore range (about 5-35 nm), consistent with TEM observations (FIG. 37). The cumulative pore volume increased dramatically to 0.53 cm3 / g, and the BET surface area rose to 148 m2 / g for P-MXene. Notably, this improvement approached that of SiO2-pillared MXene prepared by a LPP method in the literature (about 141 m2 / g from an initial 4 m2 / g), despite using only about 2.5% of the TEOS amount (MXene / TEOS = 1:0.5 in VPP vs. 1:20 in LPP). This demonstrates the efficiency of VPP in boosting surface area of MXene materials while minimizing precursor consumption and TEOS-related waste.

[0364] Experiment 3: Vapor-phase Pillarization of MXene under High DDA and Low TEOS Conditions

[0365] Beginning with the base composition (mass ratio of MXene:DDA:TEOS:H2O = 1:10:0.5:10) in the VPP, the amount of DDA, the quantity of TEOS, the water content during the hydrolysis step, and the type of swelling agent (e.g., HA and ODA) was systematically varied to examine their influences on the formation of P-MXene. N2 adsorption-desorption isotherms were employed to quantify BET surface area, pore volume, pore-size distributions, and pore geometry. These data were used to compare samples and correlate textural characteristics with synthesis conditions, thereby establishing processing-structure relationships to engineer interlayer mesopores in MXene pillarization.2101715-001365

[0366] -67- The DDA amount during VPP intercalation step was first varied by adjusting the DDA / MXene mass ratio from the base case (i.e. , 10) to 5 and 20. The absence of DDA (i.e., DDA / MXene = 0) in the synthesis was included for comparison. As the ratio increased from 5 to 10, the overall N2 uptake rose, but decreased at a ratio of 20. In all three cases (5, 10, and 20), the resultant P-MXene samples exhibit higher N2 uptake than pristine MXene across the micropore (P / Po<0.50), mesopore (O.5O<P / Po<O.98), and macropore (P / Po>O.98) regions. At a ratio of 5, the isotherm is type IV with an H2b hysteresis loop, indicative of ink-bottle-type mesopores with a broad distribution of neck sizes. At a mass ratio of 10, the isotherm is type II with an H3 hysteresis loop, characteristic of wedge- or slit-shaped pores in layered materials. An abrupt closure of the desorption branch onto the adsorption branch is observed in the mesopore region at P / Po =0.5, consistent with cavitation. At a ratio of 20, the mesopore features resembled those at a ratio of 5, but with more pronounced macroporosity, as evidenced by the increased uptake at P / Po > 0.98.

[0367] The BET surface area followed a volcano-type trend with DDA usage (FIG.

[0368] 39 and Table 7), as do the meso- and macro-pore volumes (FIG. 39 and Table 7).

[0369] Table 7: Surface Areas and Pore Volumes of P-MXene Materials Synthesized with Varying DDA.

[0370]

[0371] * Synthesis condition: VPP, MXene / DDA / TEOS / FEO = 1 :x:0.5:10 (mass ratio), intercalation at 100 °C, hydrolysis at 80 °C.

[0372] The mesopore-size distributions show that P-MXene prepared at DDA: MXene mass ratios of 5, 10, and 20 exhibited pore ranges of 25-350 A, 40-450 A, and 30-400 A, respectively. The ratio of 10 yielded a pronounced increase2101715-001365

[0373] -68-in pores between 100 and 300 A compared with the other samples. Collectively, these results indicate interconnected micro-, meso-, and microporosity in all resultant P-MXene materials, with DDA playing a critical role in tuning texture. At low DDA loadings, DDA could intercalate with a bias toward the stack perimeter, expanding only the edge-adjacent galleries of the MXene bilayer. TEOS vapor can then be confined to these regions and, upon hydrolysis / condensation, form silica pillars that create narrow necks (ink-bottle mesopores). With higher DDA (DDA:MXene=10), the layers can expand more towards the interior of the stack, allowing TEOS to infiltrate the galleries and generate wedge / slit-shaped pores. At excessive DDA (DDA:MXene=20), the galleries can become overfilled with DDA, preventing TEOS from penetrating beyond the edges. Upon calcination, the DDA escapes and the nanosheets partially collapse, yielding only limited increases in surface area and pore volume.

[0374] Furthermore, the effects of DDA intercalation time were studied by conducting a control experiment with extension of the VPP duration from 24 h to 48 h under otherwise identical synthesis conditions (MXene / DDA / TEOS / FW = 1:5:0.5:10 by mass; intercalation at 100 °C and hydrolysis at 80 °C). Prolonging the VPP time does not significantly alter the overall textural properties. The N2 adsorption-desorption isotherms in the micro- and mesopore regions remained nearly unchanged, indicating that the corresponding pore structures were largely preserved. However, extending the treatment to 48 h resulted in a noticeable increase in macroporosity. This increase could have arisen from further accumulation of DDA and TEOS near the edge regions of the MXene galleries, where precursor access is less diffusion-limited. These results suggest that longer reaction times primarily promote macropore development through continued deposition or aggregation of pillaring species at the sheet perimeters, while the micro- and mesoporous structures remain essentially intact. This behavior likely reflects saturation of the swelling agent and silica precursor within the confined interior galleries after an initial equilibration period.

[0375] The effect of TEOS loading during intercalation was next examined by varying the TEOS:MXene mass ratio from the base condition of 0.5 to 0.1 , 1.0 and 20. All samples display type II isotherms with H3 hysteresis loop, indicative of2101715-001365

[0376] -69-wedge / slit-shaped mesopores. The BET surface area increased as the TEOS:MXene ratio rose from 0.1 to 0.5, then decreased to 1.0 and 20.0 (FIG. 40 and Table 8). The meso- and total pore volumes followed the same trend (FIG. 40 and Table 8).

[0377] Table 8: Surface Areas and Pore Volumes of P-MXene Materials Synthesized with Varying TEOS

[0378]

[0379] The hysteresis loops in the mesopore range (O.5<P / Po<O.98) grew substantially, particularly at 0.8<P / Po<0.98, when the ratio increased from 0.1 to 0.5, diminished at higher TEOS loadings, with a pronounced reduction at O.5<P / Po<O.8, consistent with fewer smaller mesopores. The mesopore size distributions spanned about 20-250 A at a ratio of 0.1 with a prominent feature near about 100 A; they broaden to about 40-300 A at 0.5, and narrowed slightly to about 55-300 A at 1.0 with a much weaker peak than at 0.5. The low surface area / porosity at low TEOS loading can be attributed to an insufficient number of silica pillars, while the decrease at high loading likely arises from overfilling of the interlayer galleries by excess silica, causing densification and reduced accessible porosity. Notably, a TEOS:MXene ratio of 20 approximated that used in the LPP method, yet the surface area achieved by VPP under this condition (33 m2 / g) was far lower than that reported for LPP (141 m2 / g). In LPP, excess TEOS is removed by filtration prior to calcination, a step not implemented in VPP. Overall, these results indicate that P-MXene formation via VPP requires reagent compositions distinct from those effective in LPP.

[0380] The effect of water during the VPP hydrolysis step was evaluated by varying the water: MXene mass ratio from 10 in the base condition to 0 and 20. Omission of2101715-001365

[0381] -70-added water (ratio = 0) still yields a higher N2 uptake than pristine MXene, though lower than that obtained at a ratio of 10. The isotherm at ratio of 0 is type IV with an H2b hysteresis loop and a sharp uptake at P / Po > 0.98 indicates the presence of macropores. At a ratio of 20, the overall N2 uptake decreased below even the nowater case, and the high-pressure uptake (P / Po > 0.98) was no longer prominent, while the isotherm remained type IV with H2b hysteresis. Across the tested water: MXene ratios, the BET surface area increased from 0 to 10 and then decreased to 20 (FIG. 41 and Table 9). The mesopore and total pore volume followed the same trend (FIG. 41 and Table 9).

[0382] Table 9: Surface Areas and Pore Volumes of P-MXene Materials Synthesized with Varying Water

[0383]

[0384] * Synthesis condition: VPP, MXene / DDA / TEOS / F = 1 :10:0.5:x (mass ratio), intercalation at 100 °C, hydrolysis at 80 °C.

[0385] The mesopore size distributions showed that the no-water sample (ratio = 0) favors smaller pores (about 25-300 A) compared with the ratio of 10 sample (about 40-450 A). At ratio of 20, the distribution range resembled that at 10 but with uniformly lower intensity. In the presence of water, intercalated TEOS was converted to silica via hydrolysis (Si(OCH2CH3)4 + 4H2O — Si(OH)4 + 4C2H5OH) and condensation (Si(OH)4 — SiO2 + 2H2O) reactions. Assuming TEOS does not react with terminal -OH groups on MXene, the stoichiometric water requirement corresponds to a mass ratio of MXene / TEOS / DDA / H2O =1:0.5:10:0.09. This means about 9 wt% water relative to MXene mass is sufficient for complete TEOS hydrolysis. TGA indicates about 2 wt% water in the as-prepared MXene, explaining why some pillarization occurs even without added water. The decline in N2 uptake at higher water content is plausibly due to disruption of the DDA bilayer between MXene sheets: strong H2O-amine interactions can destabilize the bilayer and2101715-001365

[0386] -71-weaken hydrogen bonding with MXene-OH groups, thereby reducing VPP pillaring efficiency.

[0387] As a swelling agent, DDA comprises a linear C12 hydrocarbon chain terminating in an -NH2 group (CH3-(CH2)n-NH2). Because amines of different hydrocarbon chain lengths are available, the chain length, and thus molecular size, was hypothesized to affect both interlayer expansion and pillarization efficiency. To test this hypothesis, DDA with replaced with hexylamine (HA, CH3-(CH2)s-NH2) and octadecylamine (ODA, CH3-(CH2)i7-NH2) at equal molar loadings in the VPP process, enabling a direct comparison of chain-length effects. The N2 adsorptiondesorption isotherms showed lower overall uptakes for HA- and ODA-derived samples than for DDA. For HA, the isotherm exhibited features of a type IV curve with an H2b hysteresis loop beginning near P / Po = 0.6 and a pronounced high-pressure uptake (P / Po>O.98), indicative of macroporosity. For ODA, the isotherm displayed a clearer type IV profile with an H2b loop, consistent with ink-bottle-type mesopores. Macropore-related uptake at P / Po>0.98 was also evident. BET surface area increased from HA to DDA, then decreased with ODA (FIG. 42 and Table 10). The meso- and total pore volumes followed the same trend (FIG. 42 and Table 10).

[0388] Table 10: Surface Areas and Pore Volumes of P-MXene Materials Synthesized with HA, DDA, or ODA

[0389]

[0390] * Synthesis condition: VPP, MXene / HA, DDA or ODA / TEOS / H2O = 1:10:0.5:10 (mass ratio), intercalation at 100 °C, hydrolysis at 80 °C.

[0391] Pore-size distributions shifted to smaller characteristic sizes for both HA and ODA relative to DDA. These results suggest that HA is too short to substantially expand the MXene interlayer galleries, while ODA, although capable of promoting expansion, occupies excessive volume and limits TEOS access, suppressing pore development. By contrast, the intermediate chain length of DDA provides a more2101715-001365

[0392] -72-favorable balance, facilitating interlayer expansion and TEOS diffusion into interior regions, thereby enhancing formation of well-pillared structures.

[0393] Experiment 4: Vapor-phase Pillarization of MXene under Low DDA and High TEOS Conditions

[0394] A DDA:MXene mass ratio of 10 was hypothesized to preoccupy the interlayer galleries with DDA, thus impeding TEOS intercalation and limiting the formation of highly porous P-MXene. T o test this hypothesis, a second set of VPP experiments were conducted using a lower DDA: MXene ratio (0.8) while increasing TEOS loading. All other conditions matched the base case. Specifically, the TEOS:MXene mass ratio varied stepwise to 1.6, 3.2, 6.4, 10.0, and 20.0. All exhibit type IV isotherms with H2b hysteresis and a pronounced high-pressure uptake at P / Po > 0.98, indicating macroporosity. This behavior contrasts with the first VPP set (higher DDA), which showed more restricted-neck mesoporosity. At lower TEOS loadings (TEOS: MXene = 1.6), the micropore uptakes are comparable and capillary condensation onsets near P / Po about 0.60. Increasing the TEOS loading (TEOS: MXene = 6.4) produced a clear rise in mesopore and macropore uptake. At still higher TEOS loadings (e.g., TEOS:MXene = 10 and 20), both micropore and mesopore uptakes increased further, and the condensation onset shifted to lower relative pressure (P / Po about 0.42), consistent with the formation of small-width mesopores.

[0395] Surface area increased monotonically with TEOS loading, and all samples surpassed those from the first VPP set (FIG. 43 and Table 11). Notably, the TEOS:MXene = 6.4 sample reached 386 m2 / g, more than twice the value reported for liquid-phase pillaring. The total pore volume (FIG. 43 and Table 11 ) shows a non-monotonic trend: it decreases at intermediate TEOS and then rises again at higher TEOS, suggesting that partial occupation of the interlayer galleries by TEOS initially reduces accessible volume, while greater TEOS ultimately enhances pillar formation and restores porosity.

[0396] Table 11 : Surface Areas and Pore Volumes of P-MXene Materials Synthesized with Varying TEOS

[0397]

[0398] 2101715-001365

[0399] -73-

[0400]

[0401] * Synthesis condition: VPP, MXene / DDA / TEOS / F = 1 :0.8:x:10 (mass ratio), intercalation at 100 °C, hydrolysis at 80 °C.

[0402] The pore-size distributions shifted toward smaller mesopore widths at higher TEOS loadings, in agreement with the lower condensation onset. Overall, these results imply that a small amount of DDA is sufficient to swell the MXene layers, creating interlayer space for TEOS intercalation and pillar growth, thereby strengthening the pillaring effect.

[0403] Using the composition (MXene: DDA:TEOS=1.0:0.8:6.4), the effect of intercalation temperature was next examined. This was motivated by the observation that a substantial fraction of TEOS remained unreacted in the external reservoir when intercalation proceeded at the base temperature. Accordingly, intercalation was conducted at 80, 130, and 170 °C, and the resulting VPP-pillared MXene samples were characterized by N2 adsorption-desorption. Mesoporosity was retained at the higher temperatures (130 and 170 °C), but the BET surface areas decreased to 310 and 257 m2 / g, respectively (FIG. 44 and Table 12).

[0404] Table 12: Surface Areas and Pore Volumes of P-MXene Materials Synthesized with Varying Intercalation Temperature

[0405]

[0406] 2101715-001365

[0407] -74- * Synthesis condition: VPP, MXene / DDA / TEOS / FhO = 1 :0.8:6.4: 10 (mass ratio), intercalation at 80, 100, 130, or 170 °C, hydrolysis at 80 °C.

[0408] At 80 °C, the BET surface area also declined to 309 m2 / g. A yellow coloration observed after high-temperature intercalation was consistent with partial DDA decomposition, which would reduce swelling efficacy and hinder TEOS penetration into the galleries. At the lower temperature, reduced TEOS delivery to the interlayer space likely limits pillar formation. Consequently, pillaring performance was compromised at both ends of the temperature range. Notably, the pore volumes (FIG. 44 and Table 12) and the pore size distribution trends fluctuated with temperature, indicating a more complex temperature dependence.

[0409] Experiment 5: Mechanistic Understanding of Hierarchical Porosity Structure Formation

[0410] With an improved understanding of the structure-property evolution of the resultant P-MXene materials under different VPP conditions, a mechanistic model for the development of hierarchical porosity in silica-pillared MXene can be proposed. The synthesis began with freeze drying of delaminated MXene sheets dispersed in suspension, during which partial restacking occured (FIG. 45). During freezing, solvent crystallization and subsequent sublimation induced structural rearrangement of the nanosheets. Although classical capillary stresses associated with liquid evaporation are minimized in freeze drying, van der Waals attractions between adjacent sheets and mechanical stresses generated during ice crystal formation can promote non-uniform interlayer collapse. Central regions of stacked domains experience greater compressive constraint due to limited edge relaxation, leading to heterogeneous gallery spacing. This process produces a wrinkled morphology with spatially varying interlayer distances (FIG. 37). As reflected in the BET analysis (FIG. 38), the resulting structure exhibited limited overall porosity, dominated by microporosity arising from wedge- or slit-like galleries between wrinkled, partially restacked layers, with only minor contributions from meso- and microporosity.

[0411] Upon mixing MXene with DDA and heating above the melting point of DDA, molten DDA was drawn into the interlayer galleries by capillary forces to expand the interlayers apart. The intercalation process was further stabilized by hydrogen2101715-001365

[0412] -75-bonding between the -OH surface terminations of MXene and the -NH2 groups of DDA. Following vapor-phase introduction of the silica precursor (TEOS), nucleation and condensation occurred at regions of enhanced accessibility, surface functionalization (-OH, -O terminations), and structural defects. As a basic amine, DDA also catalyzed TEOS hydrolysis and condensation reactions with surface functional groups on the MXene sheets to form silica pillars. Because perimeter regions are more exposed to both molten DDA and vapor-phase TEOS diffusion, silica pillar growth proceeded more extensively at the sheet edges, resulting in taller pillars in these regions. In contrast, interior galleries experienced diffusionlimited precursor access and stronger mechanical confinement, leading to shorter pillars and narrower interlayer spacing.

[0413] Thus, the resulting architecture consisted of macro- and / or mesopores stabilized by taller edge pillars that prevent large-scale collapse, and micropores formed by interlayer galleries confined by shorter interior pillars or wrinkles regions in restacked MXene layers (FIG. 45). The interconnection between the macro-, meso- and micropores form wedge- or slit-like porosities. Overall, the final structure reflects a balance among capillary-induced collapse during drying, interlayer van der Waals attraction, swelling-induced expansion by DDA, and the mechanical rigidity of silica pillars. This interplay provides a mechanistic basis for the observed hierarchical pore distribution and explains the simultaneous emergence of macro-, meso- and microporosity without requiring intrinsic framework pore formation within individual MXene sheets.

[0414] Experiment 6: Thermal and Hydrothermal Stability of P-MXene Thermal and hydrothermal stability are important considerations for MXene-based materials in catalytic applications, particularly for thermal catalysis. In understanding these properies, both thermal and hydrothermal stability tests were conducted on the P-MXene material prepared from the VPP process. It is reported that MXene-based materials can undergo oxidation in air at temperatures above about 350 °C. Therefore, practical applications of MXene-based materials should generally be limited to temperatures below this temperature in oxidative environments. For completeness, the stability of P-MXene under inert and hydrothermal conditions at elevated temperatures were evaluated. For the thermal2101715-001365

[0415] -76-stability test, the sample (synthesis condition: MXene / DDA / TEOS / F = 1:10:0.5:10 (mass ratio), intercalation at 100 °C, hydrolysis at 80 °C) was treated at 500 °C under flowing N2 (100 ml_ min-1) for 24 h. Hydrothermal stability was evaluated by exposing the sample to 500 °C under flowing 2%steam / 98%Ar (50 ml_ min-1) steam for 24 h. After treatment, N2 adsorption-desorption isotherms and XRD patterns were collected.

[0416] For the hydrothermally treated sample, the XRD pattern (FIG. 46) shows disappearance of the (002) reflection, indicating significant disruption of the layered structure of P-MXene. This observation is consistent with the N2 adsorptiondesorption results, where both the surface area (FIG. 47) and total pore volume (FIG. 47) decreased after hydrothermal treatment. The structural degradation is likely due to collapse of the interlayer architecture upon prolonged exposure of the silica pillars to steam at high temperature. In contrast, for the thermally treated sample under dry N2, the (002) peak was retained (FIG. 46), suggesting that the layered structure remained largely intact. Interestingly, thermal treatment resulted in an increase in surface area and pore volume (FIG. 47). This enhancement can be attributed to further condensation or structural rearrangement of the silica pillars, reducing framework blockage and increasing accessible porosity. Additionally, trace oxygen impurities in the N2 stream can have caused partial oxidation of carbon species in P-MXene, potentially generating additional micro- or macroporosity. Overall, these results indicate that P-MXene exhibits limited stability under high-temperature hydrothermal conditions, while it retains structural integrity more effectively under dry atmospheres. Nevertheless, prolonged exposure to high temperatures, even under inert conditions, can induce structural evolution.

[0417] Therefore, catalytic applications of P-MXene should preferably be conducted at moderate temperatures to ensure structural stability.

[0418] Experiment 7: P-MXene Supported Ru Catalyst for Plastic Hydrogenolysis To evaluate the application potential of P-MXene synthesized via the VPP method, the P-MXene was used as a catalyst support for the chemical upcycling of plastics. Polyolefins, including polyethylene (PE) and polypropylene (PP), are thermoplastic materials that dominate the global plastics market due to their structurally simple yet highly versatile nature. They exhibit advantageous properties2101715-001365

[0419] -77-such as high strength-to-weight ratios, transparency, and excellent durability.

[0420] However, the same chemical stability that underpins their utility also renders them resistant to depolymerization and degradation. Ruthenium, a metal catalyst widely studied for polyolefin hydrogenolysis, has shown superior catalytic performance, largely attributed to their lower activation energy barrier for the rate-determining C-C bond cleavage step. Typical supports for Ru nanoparticles include TiO2, ZrO2, CeO2, and carbon materials. Nevertheless, these catalyst systems often suffer from limited surface area and porosity, which restrict polymer-catalyst interfacial contact and hinder mass transport. Aiming at this issue, Ru was selected as the active phase to prepare the P-MXene-supported Ru catalyst (Ru@P-MXene). For comparison, a MXene-supported Ru catalyst (Ru@MXene) was also synthesized and tested under identical reaction conditions. In both cases, the Ru loading was controlled at 5 wt%.

[0421] Catalyst properties. The morphologies of Ru particles in Ru@MXene and Ru@P-MXene catalysts were examined by HAADF-STEM imaging. On the MXene support, Ru particles exhibited a spherical morphology. The particle size distribution histogram shows an average particle size of Ru particles was about 1.9 nm. On the P-MXene support, no distinct Ru particles were observed. STEM-EDS elemental mapping confirmed the presence of Ru in Ru@P-MXene and revealed significantly improved dispersion compared to Ru@MXene. This enhanced dispersion is attributed to the increased surface area and mesopore volume generated by the VPP process.

[0422] The high-resolution Ru 3d XPS spectra of 5.0% Ru@MXene and 5.0% Ru@P-MXene were measured to provide insights into the coordination environment of Ru species. Deconvolution was performed using CasaXPS software to distinguish the Ru 3d signal from the C 1s spectrum. The C 1s spectra were deconvoluted to adventitious carbon species (C-C / C-H, about 284.8 eV), oxygenated carbons (C-0 and O-C=O, about 286.2-288.9 eV), and carbide-related peaks (C-Ti at about 282.0 eV), and Ru-related species overlapping with the C 1s region. The Ru 3d spectra were deconvoluted to Ru-Ru, Ru-O, and Ru-CI states located around 280.4 eV, 280.9 eV, and 282.1 eV, respectively. For the2101715-001365

[0423] -78- 5.0% Ru@MXene sample, the dominant features of the C-Ti peak confirmed the preservation of the MXene carbide framework after Ru incorporation. Notably, Ru-Cl and Ru-0 species are clearly resolved, suggesting that a substantial fraction of Ru remained in cationic states, derived from residual RuC precursors and oxidized Ru species stabilized on the MXene surface. The presence of Ru-Ru bonding contributions indicated partial reduction of Ru species to metallic Ru. This combination of metallic and oxidized Ru states supports the idea that the MXene substrate promotes both dispersion and partial reduction of Ru, while simultaneously stabilizing cationic species through surface terminations. By contrast, the 5.0% Ru@P-MXene catalyst exhibited a markedly different spectral profile. While the characteristic C-Ti peak remained at about 282.0 eV, confirming structural preservation of the MXene layers after pillarization, the Ru signal was dominated by Ru-0 and Ru-CI states, with little to no contribution from metallic Ru-Ru bonding. This indicates that Ru species are more finely dispersed and stabilized in oxidized form within the expanded interlayer environment created by silica pillars. The absence of metallic Ru features aligns with the observed smaller, more uniform Ru particle sizes from HAADF-STEM in Ru@P-MXene compared to elongated Ru particles in Ru@MXene.

[0424] The high-resolution Ti 2p XPS spectra were deconvoluted to C-Ti-(O\O\O), C-Ti-(O\O\F), and C-Ti-(O\F\F) environments. For 5.0% Ru@MXene, the presence of TiO2-xF2x was also evident, though its contribution is moderate, suggesting partial oxidation of the surface during synthesis or handling. The coexistence of these states indicates that Ti atoms at the MXene surface are distributed among carbide-bonded and oxyfluoride environments. The multiple termination states likely facilitate anchoring of Ru species, stabilizing both cationic and metallic Ru as observed in the Ru 3d spectra. In contrast, the Ti 2p spectrum of 5.0% Ru@P-MXene was dominated by a strong TiO2-xF2x component, with less pronounced contributions from mixed C-Ti-O / F states. The weaker intensity of carbide-related C-Ti peaks imply partial dilution of the Ti-C signal by the silica framework. This structural modification, while reducing the relative prominence of2101715-001365

[0425] -79- Ti-C bonding, creates more accessible sites, which can strongly stabilize dispersed Ru cations.

[0426] Hydrogenolysis of low-density polyethylene: The hydrogenolysis of low-density polyethylene (LDPE) was evaluated under identical conditions using Ru@P-MXene and Ru@MXene catalysts. As shown in FIG. 48, Ru@MXene exhibited limited activity, achieving only 9.16% conversion after 2 hours. The product distribution consisted of 1.85% gas, 4.19% liquid, and 90.84% solid residue, with methane as the dominant gaseous product. In contrast, Ru@P-MXene delivered significantly enhanced performance, reaching 76.57% conversion within 0.5 hours. The product distribution shifted markedly toward more volatile products, with 15.46% gas, 56.36% liquid, and 23.43% solid (FIG. 48). Methane again dominated the gaseous fraction, with a yield of 12.28%. For both catalysts, the high selectivity aligns with the well-established behavior of Ru-based catalysts in hydrogenolysis reactions.

[0427] The low activity of Ru@MXene can be attributed to the low BET surface area, small pore volume, and narrow pore sizes of the MXene support, which restrict accessibility to active sites and hinder mass transport. Moreover, Ru@MXene was synthesized via freeze-drying of MXene dispersed in a Ru precursor solution, a process that likely led to Ru species being intercalated between MXene layers. By contrast, the superior activity of Ru@P-MXene stems from the significantly increased surface area, pore volume, and mesopore sizes provided by the pillared support. These textural improvements alleviate diffusion limitations and enhance the accessibility of polymer chains to Ru active sites. Collectively, these results highlight that P-MXene, with its enhanced textural properties, more effectively harness the catalytic potential of MXene-based materials in heterogeneous thermal catalysis, an emerging application area for this promising class of 2D materials.

[0428] Conclusions of Example 3

[0429] In summary, a vapor-phase pillarization (VPP) strategy was developed to engineer the pore architecture of mesoporous silica-pillared MXene (P-MXene). By optimizing the identity and loading amine swelling agents, the amount of silica precursor (TEOS), and the water content for hydrolysis, P-MXene materials2101715-001365

[0430] -80-exhibiting expanded interlayer spacing, high surface area, and large mesopores were produced. These materials possessed properties comparable to materials produced by liquid-phase pillarization. Moreover, by lowering the DDA loading while increasing TEOS, VPP-derived P-MXene attained more than twice the surface area of its LPP counterpart. The VPP route also improved precursor utilization and minimized liquid waste, offering a more environmentally friendly, cost-effective, and operationally simple alternative to conventional liquid processing. To explore catalysis applications, P-MXene was used as a support for Ru nanoparticles (Ru@P-MXene) in polyethylene hydrogenolysis. The P-MXene support promoted highly dispersed Ru sites and better access for bulky polymer chains, enhancing mass transport in the molten phase and substantially increasing catalytic activity. Overall, this Example shows that MXene-based materials described herein can possess new mesoporous architectures and underscores their promise as heterogeneous catalyst supports for heavy or bulky feedstocks such as plastics.

[0431] It will be appreciated by those skilled in the art that the present disclosure can be embodied in other specific forms without departing from the spirit or essential characteristics thereof. The presently disclosed embodiments are therefore considered in all respects to be illustrative and not restricted. The scope of the disclosure is indicated by the appended claims rather than the foregoing description and all changes that come within the meaning and range and equivalence thereof are intended to be embraced therein.

Claims

2101715-001365-81- CLAIMS:

1. A catalyst material comprising:at least two MXene sheets, each sheet having a chemical composition according to the following formula Mn+ iXnTx, wherein:M is an early transition metal,n is an integer ranging from 1 to 3,X is C or N, andTxis a surface functional group selected from one or more of -O, -OH, ora halogen; andan interlayer space residing between the two MXene sheets, wherein the interlayer space comprises one or more pillar structures, wherein at least one of the pillar structures is loaded with one or more metallic particles and / or metal alloys.

2. The catalyst material of claim 1 , wherein the material is characterized by a small angle X-ray diffraction (XRD) pattern having a peak at about 2.0° 26.

3. The catalyst material of claim 1 , wherein the material is characterized by a d-spacing of about 1 .0 nm or higher, as determined by small angle XRD pattern.

4. The catalyst material of claim 1 , wherein at least one of the MXene sheets has an average layer thickness ranging from about 0.5 nm to about 1.2 nm.

5. The catalyst material of claim 1 , wherein the interlayer space has a thickness ranging from about 1.0 nm to about 100 nm or higher.

6. The catalyst material of claim 1 , wherein the material is characterized by a H2-type hysteresis loop at a P / Po ranging from about 0.4 to about 0.9 and a H4-type hysteresis loop as determined by a N2 adsorption / desorption isotherm.2101715-001365-82- 7. The catalyst material of claim 1 , wherein the material is characterized by a H4-type hysteresis loop at relative pressures (P / Po) greater than 0.8, as determined by a N2 adsorption / desorption isotherm.

8. The catalyst material of claim 1 , wherein the material possesses a BET surface area ranging from about 50 m2 / g to about 800 m2 / g.

9. The catalyst material of claim 1 , wherein the material is characterized by a cumulative pore volume of about 0.10 cm3 / g to about 2.00 cm3 / g.

10. The catalyst material of claim 1 , wherein the one or more metallic particles and / or metal alloys possess an average particle size ranging from about 0.2 nm to about 1.5 nm or higher.

11. The catalyst material of claim 1 , wherein the material is characterized by a C 1s X-ray Photoelectron Spectroscopy (XPS) having a peak at about 282.0 eV.

12. The catalyst material of claim 1 , wherein the material possesses 0.01 wt% to 50 wt% of the one or more metallic particles and / or metal alloys.

13. A method for hydrogenating a plastic composition comprising:subjecting the plastic composition to a hydrogenolysis reaction, wherein the hydrogenolysis reaction occurs in the presence of the catalyst material of claim 1 .

14. The method of claim 13, wherein the hydrogenolysis reaction occurs under a plastic-to- catalyst material ratio ranging from about 1:1 to about 100:1.

15. The method of claim 13, wherein the hydrogenolysis reaction occurs at a temperature ranging from about 150°C to about 400°C.2101715-001365-83- 16. The method of claim 13, wherein the hydrogenolysis reaction occurs for at least 1 minute or higher.

17. The method of claim 13, wherein the hydrogenolysis reaction occurs under a H2 pressure of about 1 bar to about 300 bar.

18. The method of claim 13, wherein the plastic composition comprises one or more of polyolefins, polyesters, polystyrene, polyvinyl chloride, polyurethane, polyamides and acrylics.

19. A method for producing a catalyst material having at least two MXene sheets and one or more pillar structures located between the at least two MXene sheets, wherein each MXene sheet has a chemical composition according to the following formula Mn+ iXnTx, wherein:M is an early transition metal,n is an integer ranging from 1 to 3,X is C or N, andTx is a surface functional group selected from one or more of -O, -OH, or a halogen;the method comprising:- intercalating one or more pillar precursors between the at least two MXene sheets; and- hydrolyzing the one or more pillar precursors between the at least two MXene sheets into the one or more pillar structures,wherein the method is carried out under an autogenous pressure.

20. The method of claim 19, wherein the intercalating comprises:- subjecting the at least two MXene sheets to a swelling agent and a pillarization agent.2101715-001365-84- 21. The method of claim 20, wherein the swelling agent is selected from dodecylamine (DDA), octadecylamine (ODA), hexylamine (HA), or other amine agents.

22. The method of claim 20, wherein the intercalating is performed under a swelling agent to MXene mass ratio of about 0.1 :1 to about 25:1.

23. The method of claim 20, wherein the pillarization agent is selected from an oregano precursor of a metal oxide, tetraethyl orthosilicate (TEOS), metal ions, organic compounds, and carbon nanotubes.

24. The method of claim 20, wherein the intercalating is performed under a pillarization agent to MXene mass ratio of about 0.01 :1 to about 50:1.

25. The method of claim 20, wherein the intercalating is performed at a temperature ranging from about 50°C to about 300°C.

26. The method of claim 20, wherein the hydrolysis of the intercalated one or more pillar precursors is performed in the presence of water.

27. The method of claim 26, wherein the intercalating is performed under a mass ratio of MXene:swelling agent:pillarization agent:water of 1 :x:y:z, wherein: x = swelling agent mass,y = pillarization agent mass,z = water mass, andx is 0.5 to 20, y is 0.1 to 20, and z is 0 to 20.

28. The method of claim 19, wherein no water is added during the hydrolyzing of the one or more silica pillar precursors.

29. The method of claim 19, wherein the hydrolyzing is performed under a temperature of about 25°C to about 100°C.2101715-001365-85-30. The method of claim 19, wherein the hydrolyzing is performed under a mass ratio of water to MXene ranging from 0:1 to about 20:1.

31. A catalyst material produced from the method of claim 34.

32. The catalyst material of claim 31 , wherein the material contains an interlayer spacing region between the at least two MXene sheets and the interlayer spacing region possesses a thickness ranging from about 0.5 to about 100 nm or higher.

33. The catalyst material of claim 31 , wherein the material is characterized by a X-ray diffraction (XRD) pattern having peaks at about 8.2° and about 6.7° 20.

34. The catalyst material of claim 31 , wherein the material is characterized by a d-spacing of about 1.0 nm to about 100 nm or higher, as determined by small angle XRD pattern.

35. The catalyst material of claim 31 , wherein the material is characterized by a H3-type hysteresis loop at relative pressures (P / Po) ranging between 0.4 to 0.8, as determined by a N2 adsorption / desorption isotherm.

36. The catalyst material of claim 31 , wherein the material is characterized by a mesopore size distribution of about 5 nm to about 35 nm, as determined by a N2 adsorption / desorption isotherm.

37. The catalyst material of claim 31 , wherein the material is characterized by a cumulative pore volume of about 0.10 cm3 / g to about 2.0 cm3 / g.

38. The catalyst material of claim 31 , wherein the material possesses a Brunauer-Emmett-Teller (BET) surface area ranging from about 30 m2 / g to about 800 m2 / g.2101715-001365-86- 39. A catalyst material comprising:at least two metal oxide sheets, each sheet having a chemical composition according to the following formula Mn+ iOm(n+i)Xn-aTx, wherein M is a transition metal, n is an integer ranging from 1 to 3, m is an integer ranging from 0 to 2, X is carbon (C) or nitrogen (N), a is an integer ranging from 0 to 2, and Txis a surface functional group; andan interlayer space residing between the at least two metal oxide sheets, wherein the interlayer space comprises one or more pillar structures,wherein the catalyst material has a Brunauer-Emmett-Teller (BET) surface area ranging greater than 100 m2 / g.

40. The catalyst material of claim 39, wherein the material is characterized by a cumulative pore volume of about 0.10 cm3 / g to about 2.00 cm3 / g.

41. The catalyst material of claim 39, wherein the material comprises one or more metallic particles or alloys.

42. The catalyst material of claim 39, wherein the material is characterized by a X-ray diffraction (XRD) pattern having peaks at 25.5°, 38.1°, 48.1°, and 54.4° 20 and / or a peak at 27.6 °20.

43. The catalyst material of claim 39, wherein the material is characterized by a H3-type hysteresis loop at relative pressures (P / Po) of about 0.48 to about 1.00, as determined by a N2 adsorption / desorption isotherm.

44. The catalyst material of claim 39, wherein the material is characterized by a hierarchical pore architecture with pore size distribution of micro- (<2nm), meso- (2-50nm) and macro-(>50nm) pores, as determined by a N2 adsorption / desorption isotherm.

45. A method for creating the catalyst material of claim 39, comprising:2101715-001365-87- calcining a P-MXene material at a temperature ranging from about 250°C to about 550°C,wherein the P-MXene material comprises:at least two MXene sheets, each sheet having a chemical composition according to the following formula Mn+ iXnTx, wherein:M is an early transition metal,n is an integer ranging from 1 to 3,X is C or N, andTx is a surface functional group selected from one or more of -O, -OH, or a halogen; andan interlayer space residing between the two MXene sheets, wherein the interlayer space comprises one or more pillar structures.

46. The method of claim 45, wherein the calcining is performed at a temperature of about 250-450°C.

47. The method of claim 45, wherein the calcining is performed at a temperature of about 350-550°C.

48. The method of claim 45, wherein the calcining is performed under an air flow rate of about 10-500 mL / min and atmospheric pressure.

49. The method of claim 45, wherein the calcining is performed for about 2 to about 24 hours.

50. The method of claim 45, comprising:impregnating the catalyst material with at least one metallic particle or alloy.

51. The method of claim 50, wherein the impregnating comprises one or more of:2101715-001365-88- adding a stock solution of the at least one metallic particle or alloy to the catalyst material to create an impregnated catalyst material;drying the impregnated catalyst material under a temperature ranging from about 25°C to about 200°C; orreducing the dried, impregnated catalyst material at a temperature ranging from about 150°C to about 450°C.

52. A method for hydrogenating a plastic composition comprising:subjecting the plastic composition to a hydrogenolysis reaction, wherein the hydrogenolysis reaction occurs in the presence of the catalyst material of claim 39.

53. The method of claim 52, wherein the hydrogenolysis reaction occurs at temperature ranging from about 150°C to about 300°C.

54. The method of claim 52, wherein the hydrogenolysis reaction occurs at H2 pressure ranging from about 1 bar to about 300 bar.

55. The method of claim 52, wherein the hydrogenolysis reaction occurs under a plastic-to- catalyst material ratio ranging from about 1:1 to about 100:1.