Polymer composition for overmolding applications and articles made therefrom

A polymer composition combining semi-aromatic polyamides, halogen-free flame retardants, and non-circular glass fibers addresses the challenges of thermal shock resistance, electrical insulation, and adhesion in metal overmolding, achieving high performance and regulatory compliance.

WO2026241557A1PCT designated stage Publication Date: 2026-11-19CELANESE INTERNATIONAL CORP +5
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/US2026/028239
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-11-18
Filing Date
2026-05-14
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Formulating a nylon composition that is both flame-retardant and suitable for metal overmolding presents significant challenges, compounded by the difficulty of achieving good thermal shock resistance, electrical insulation, and strong adhesion, as traditional flame retardants compromise mechanical properties and adhesion, and thermal stability is compromised by processing conditions and moisture absorption.

Method used

A polymer composition comprising a semi-aromatic polyamide with a high melting temperature, an amorphous semi-aromatic polyamide, halogen-free flame retardants, and reinforcing glass fibers with a non-circular cross-section, achieving a balance of thermal shock resistance, electrical insulation, and strong adhesion.

Benefits of technology

The composition exhibits superior electrical properties, thermal shock resistance, and mechanical strength, meeting stringent regulatory standards with a CTI of at least 500 V and exceeding 200 thermal shock cycles from -40°C to 140°C, suitable for high-performance applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure US2026028239_19112026_PF_FP_ABST
    Figure US2026028239_19112026_PF_FP_ABST
Patent Text Reader

Abstract

A polymer composition is disclosed, particularly a polyamide composition, that has excellent flame resistance and thermal shock resistance. The composition also has excellent electrical insulation properties. The composition contains at least two polyamide polymers, glass fibers having a non-circular cross-sectional shape, and at least one flame retardant.
Need to check novelty before this filing date? Find Prior Art

Description

Attorney Docket No.: CICT-1567-PCT2 (2024P0075)POLYMER COMPOSITION FOR OVERMOLDING APPLICATIONS AND ARTICLES MADE THEREFROMRELATED APPLICATIONS

[0001] The present application is based upon and claims priority to International Patent Application No. PCT / CN2025 / 094940, having a filing date of May 14, 2025, and U.S. Provisional Patent Application Serial No. 63 / 919,824, having a filing date of November 18, 2025, both of which are incorporated herein by reference in their entirety.BACKGROUND

[0002] Nylon-based materials are widely used in various industrial applications due to their excellent mechanical properties, chemical resistance, and ease of processing. In particular, nylon compositions are frequently utilized in overmolding processes, where plastic materials are molded over metal components to enhance structural integrity, provide electrical insulation, and improve aesthetics. However, formulating a nylon composition that is both flame-retardant and suitable for metal overmolding presents significant technical challenges, further compounded by the difficulty of achieving good thermal shock resistance.

[0003] Flame retardancy is a critical requirement for nylon applications in the electrical, automotive, and industrial sectors to enhance safety and comply with stringent regulatory standards such as UL 94 and IEC 60695. Traditional flame retardants, such as halogenated additives, effectively inhibit combustion but often compromise the mechanical properties of the base nylon material. In particular, incorporating flame-retardant additives can lead to increased brittleness and reduced impact strength, which negatively affect the shock resistance required for durable overmolded components. This challenge becomes even more pronounced when considering thermal shock resistance, as sudden temperature fluctuations can induce cracking, delamination, or warping in formulations that lack sufficient resilience.

[0004] Additionally, electrical insulation is a key property for nylon materials used in electronic and electrical applications. Some flame retardants, especially those based on carbon or other conductive fillers, can inadvertently degrade the dielectric performance of the material. Achieving a balance between flameAttorney Docket No.: CICT-1567-PCT2 (2024P0075)retardancy and electrical insulating properties is therefore a significant material formulation challenge.

[0005] Another critical aspect of nylon formulations for metal overmolding is adhesion. Nylon must bond effectively with metal substrates to ensure structural integrity and durability of the overmolded product. However, many flame-retardant additives can alter the surface energy and flow characteristics of the nylon, leading to poor adhesion and potential delamination under mechanical or thermal stress. These adhesion challenges are exacerbated by thermal shock, as repeated exposure to rapid temperature changes can weaken the interface between the nylon and metal, further increasing the risk of failure.

[0006] Moreover, thermal stability and processing conditions further complicate the formulation of a flame-retardant nylon suitable for overmolding. Overmolding involves elevated processing temperatures that can degrade certain flameretardant additives, resulting in discoloration, reduced mechanical properties, or compromised flame retardancy. Additionally, nylon's inherent moisture absorption can impact both mechanical performance and overmolding adhesion, particularly when hydrophilic flame-retardant additives are incorporated. The effects of moisture absorption, combined with thermal expansion mismatches between nylon and metal, can further reduce thermal shock resistance, making the material more susceptible to cracking or structural failure.

[0007] Accordingly, there is a need for an improved nylon composition that provides flame retardancy while maintaining impact resistance, thermal shock resistance, electrical insulation, and strong adhesion in metal overmolding applications. The present disclosure addresses these challenges by providing an optimized material formulation that meets the demanding performance requirements of such applications.SUMMARY

[0008] The present disclosure relates to a polymer composition specifically designed for molding over metals, providing enhanced electrical, thermal, and mechanical properties. The polymer composition comprises a combination of a first and second polyamide polymers, a flame retardant composition, and reinforcing fibers, yielding a material suitable for high-performance applications.

[0009] The first polyamide polymer is a semi-aromatic polyamide with a meltingAttorney Docket No.: CICT-1567-PCT2 (2024P0075)temperature between about 280°C and 350°C, derived from at least one aliphatic diamine and at least one carboxylic acid, including terephthalic acid. The second polyamide polymer is an amorphous semi-aromatic polyamide with a glass transition temperature ranging from about 110°C to 160°C. The combination of these polyamides ensures a balance of thermal shock resistance, rigidity, toughness, and processability.

[0010] The composition further includes a flame retardant system, which is halogen-free, and reinforcing glass fibers dispersed throughout the polymer matrix. These glass fibers have a non-circular cross-section and are present in amounts ranging from about 8% to about 58% by weight. The composition demonstrates superior electrical properties, achieving a comparative tracking index (CTI) of at least 500 V, and a V-0 rating under the Underwriters Laboratories Test 94 Vertical Burn Test at a thickness of 1.6 mm, at a thickness of 0.8 mm, and / or at a thickness of 0.4 mm.

[0011] Additional refinements in the composition provide enhanced performance characteristics. For instance, the polymer composition can achieve a CTI of at least 525 V, with further improvements to at least 600 V. It also exhibits exceptional thermal shock resistance, exceeding 200 cycles in extreme temperature ranges from -40°C to 140°C, with potential performance extending beyond 650 cycles.

[0012] The first polyamide polymer may be a copolymer or terpolymer, including monomeric units such as hexamethylene diamine, 2-methylpentamethylene diamine, terephthalic acid, isophthalic acid, and adipic acid. The second polyamide polymer can be derived from hexamethylene diamine, decamethylene diamine, isophthalic acid, and terephthalic acid.

[0013] In certain embodiments, the polymer composition includes specific ratios of these polyamides, with the first polyamide polymer comprising from about 10% to 55% by weight and the second polyamide polymer comprising from about 5% to 40% by weight of the polymer composition. The glass fibers incorporated into the matrix have a width-to-height ratio of about 2:1 to 6: 1 , preferably about 3:1 to 5: 1 , with average fiber lengths ranging from about 1 mm to 5 mm.

[0014] The flame retardant composition includes a metal phosphinate, such as aluminum diethylphosphinate, in amounts ranging from about 6% to 18% byAttorney Docket No.: CICT-1567-PCT2 (2024P0075)weight. The polymer composition can be free of nitrogen-containing synergists for flame retardancy, ensuring compliance with regulatory and environmental standards.

[0015] Further modifications to the composition include the addition of lubricants, such as calcium salts of montanic acids, and thermal cycling agents like ultrahigh molecular weight silicone, particularly polydimethylsiloxane, which can be introduced as a masterbatch with a polyamide carrier polymer. The polymer composition also demonstrates exceptional dielectric strength at elevated temperatures, maintaining a dielectric strength of greater than 18 kV / mm at 150°C.

[0016] Additionally, the disclosure encompasses a composite structure comprising a metal component in contact with a resinous component made from the polymer composition. The metal component can be overmolded, forming a structure suitable for use in busbars, current sensors, inverter filters, electrical connectors, brushless direct current motors, guide rings, battery cell sealing rings, quick connectors, tees, and interconnectors.

[0017] This novel polymer composition provides a robust solution for high-performance electrical and thermal applications, ensuring reliability and longevity in demanding environments.

[0018] Other features and aspects of the present disclosure are discussed in greater detail below.BRIEF DESCRIPTION OF THE DRAWINGS

[0019] A full and enabling disclosure of the present invention, including the best mode thereof to one skilled in the art, is set forth more particularly in the remainder of the specification, including reference to the accompanying figures, in which:FIG. 1 illustrates an electric vehicle including components that may incorporate a polymer composition as disclosed herein;FIG. 2 illustrates one embodiment of a busbar as may incorporate a polymer composition as disclosed herein;FIG. 3 illustrates a battery assembly that may employ components that may incorporate a polymer composition as disclosed herein;FIG. 4 is a perspective view of one embodiment of a connector that may incorporate a polymer composition as disclosed herein;FIG. 5 is a plan view of the connector of FIG. 4 in which the first andAttorney Docket No.: CICT-1567-PCT2 (2024P0075)second connector portions are disengaged;FIG. 6 is a plan view of the connector of FIG. 4 in which the first and second connector portions are engaged;FIG. 7 illustrates examples of components that may incorporate a polymer composition as disclosed herein;FIG. 8 illustrates additional components that may incorporate a polymer composition as disclosed herein;FIG. 9 illustrates one embodiment of a water pump as may incorporate a polymer composition as disclosed herein;FIGS. 10-13 illustrate sample components that may be used to perform testing for thermal shock resistance as described herein;FIG. 14 is a graphical representation of some of the results obtained in the example below; andFIG. 15 is a graphical representation of some of the results obtained in the example below.

[0020] Repeat use of reference characters in the present specification and drawings is intended to represent the same or analogous features or elements of the present invention.DEFINITIONS

[0021] Comparative Tracking Index ("CTI"): The comparative tracking index (CTI) may be determined in accordance with International Standard I EC 60112-2003 to provide a quantitative indication of the ability of a composition to perform as an electrical insulating material under wet and / or contaminated conditions. In determining the CTI rating of a composition, two electrodes are placed on a molded test specimen. A voltage differential is then established between the electrodes while a 0.1% aqueous ammonium chloride solution is dropped onto a test specimen. The maximum voltage at which five (5) specimens withstand the test period for 50 drops without failure is determined. The test voltages range from 100 to 600 V in 25 V increments. The numerical value of the voltage that causes failure with the application of fifty (50) drops of the electrolyte is the "comparative tracking index." The value provides an indication of the relative track resistance of the material. According to LIL746A, a nominal part thickness of 3 mm is considered representative of performance at other thicknesses.Attorney Docket No.: CICT-1567-PCT2 (2024P0075)

[0022] Thermal Shock Resistance: To test thermal shock resistance, four (4) types of sample components are initially formed using the molds and inserts shown in Figs. 10-13. As shown in Fig. 10, a first mold 100 is shaped to result in a plastic thickness of 1.2 mm and a part size of 63.8 mm x 20 mm x 10.4 mm; a second mold 200 is shaped to result in a plastic thickness of 2.5 mm and a part size of 65.1 mm x 22.6 mm x 13 mm; a third mold 300 is shaped to result in a plastic thickness of 1.2 mm and a part size of 40 mm x 20 mm x 10.4 mm; and a fourth mold 400 is shaped to result in a plastic thickness of 42.6 mm x 22.6 mm x 13 mm. Two circular bores 402 are formed on the cavity side of each of the molds 300 and 400, parallel to the longitudinal edge of the molds. The bores 402 have a diameter of 3.5 mm and are recessed into the cavity side of the molds. The first and second molds 100 and 200 contain metal inserts 105 and 205 (see Fig. 11), respectively, which are formed from an AISI H13 / 440C stainless steel sheet having a size of 62.6 mm x 18 mm x 18 mm that is inserted into the mold in a manner such that no weldline is formed. The inserts 105 and 205 have a single circular bore 502 at their respective ends having a diameter of 5 mm. The third and fourth molds 300 and 400 likewise contain metal inserts 305 and 405 (see Fig. 11), respectively, which are formed from an AISI H13 / 440C stainless steel sheet having a size of 37.6 mm x 18 mm x 18 mm. As shown in Fig. 11 , each of the metal inserts 305 and 405 contain two circular bores 602 that are aligned parallel to the transverse edge of the inserts and recessed into the core side of each respective insert. The bores 602 have a diameter of 2.0 mm and are recessed into the core side of the inert by a depth of 5 mm. When inserted into the molds 300 and 400, a weldline is formed at a line where two flow fronts meet such that there is an inability of the flow fronts to “knit” or “weld” together during the molding process.

[0023] Referring to Figs 10, 12, and 13, a sample component may be formed using the molds described above by initially passing a polymer composition through a sprue 702 having an upper end 704 with a small diameter (i.e. , 6 mm) and a lower end 706 with a diameter greater than the upper end 704 (i.e., 8 mm). The polymer composition may flow through the sprue 702 into a first runner 802 (diameter of 7 mm) and through a gate 804 for the third mold 300 that has a size of 0.8 x 10 mm and through a gate 806 for the fourth mold 400 that has a size of 1.7 x 10 mm. The polymer composition may likewise flow through the sprue 702 into aAttorney Docket No.: CICT-1567-PCT2 (2024P0075)second runner 902 (diameter of 6 mm) and through a gate 904 for the first mold 100 that has a size of 0.8 x 10 mm and through a gate 906 for the fourth mold 400 that has a size of 1.7 x 10 mm. The draft angle for each side of the molds is 1.5°. When forming molded parts, the processing conditions may be selected as is known to those skilled in the art. For example, the melt and nozzle temperature may be 320°C, the injection pressure may be 1250 bar, the peak pressure may be 1146 bar (e.g., for mold 100) and 1120 (e.g., for mold 300), the injection speed may be 80 mm / s and the injection time may be about 0.25 s, the hold pressure may be about 800 bar, the cooling time may be about 15 s, and the total cycle time may be about 23 s.

[0024] A set of twenty (20) sample components may be formed using each of the molds described above. The sample components may then be subjected to a first heating cycle within a thermal shock chamber having a hot zone and a cold zone, such as those commercially available under the name “ShockEvent T / 120 / V2” from Weisstechnik. The hot zone may be heated to a temperature of 140°C and the cold zone may be cooled to a temperature of -40°C. To initiate the first heating cycle, the sample components are placed within the hot zone for 30 minutes and then a product carrier within the chamber moves the sample components from the hot zone to the cold zone for an additional 30 minutes. In this manner, the total time of the first cycle is 1 hour. 24 cycles are conducted each day and 1 hour for each cycle. During the first two weeks, the sample components are visually observed for cracking once a day, and thereafter, the sample components are visually observed for cracking twice per week until all twenty (20) samples crack or a full set of cycles is achieved, which may be either 1 ,500 or 3,000 cycles depending on the testing protocol. When the first sample cracks, the number of cycles achieved prior to cracking is recorded as the “thermal shock resistance value.” If a full set of cycles (1 ,500 or 3,000) is achieved without all samples cracking, the “thermal shock resistance value” is simply recorded as “>1,500” or “>3,000”, depending on the particular testing protocol.

[0025] Unless otherwise specified, Thermal Shock Resistance is measured herein using the first mold 100.

[0026] UL94: A specimen is supported in a vertical position and a flame is applied to the bottom of the specimen. The flame is applied for ten (10) secondsAttorney Docket No.: CICT-1567-PCT2 (2024P0075)and then removed until flaming stops, at which time the flame is reapplied for another ten (10) seconds and then removed. Two (2) sets of five (5) specimens are tested. The sample size is a length of 125 mm, width of 13 mm, and thickness of 0.8 mm. The two sets are conditioned before and after aging. For unaged testing, each thickness is tested after conditioning for 48 hours at 23°C and 50% relative humidity. For aged testing, five (5) samples of each thickness are tested after conditioning for 7 days at 70°C.Vertical RequirementsRatingsSpecimens must not burn with flaming combustion for more than 10 seconds after either test flame application.T otal flaming combustion time must not exceed 50 seconds for each set of 5 specimens.Specimens must not burn with flaming or glowing combustion up to the specimen V-0holding clampSpecimens must not drip flaming particles that ignite the cotton.No specimen can have glowing combustion remain for longer than 30 seconds after removal of the test flame.Specimens must not burn with flaming combustion for more than 30 seconds after either test flame application.Total flaming combustion time must not exceed 250 seconds for each set of 5 specimens.V-1 Specimens must not burn with flaming or glowing combustion up to the specimen holding clampSpecimens must not drip flaming particles that ignite the cotton.No specimen can have glowing combustion remain for longer than 60 seconds after removal of the test flame.Specimens must not burn with flaming combustion for more than 30 seconds after either test flame application.Total flaming combustion time must not exceed 250 seconds for each set of 5 specimens.V-2 Specimens must not burn with flaming or glowing combustion up to the specimen holding clampSpecimens can drip flaming particles that ignite the cotton.No specimen can have glowing combustion remain for longer than 60 seconds after removal of the test flame.Attorney Docket No.: CICT-1567-PCT2 (2024P0075)

[0027] Glass transition temperature and melting temperature: The glass transition temperature and the melting temperature may be determined using differential scanning calorimetry (“DSC”), using, for instance, ISO Test No. 11357-2:2013 (glass transition temperature) and 11357-3:2011 (melting temperature).

[0028] Dielectric strength: Dielectric strength can be measured according to I EC 60243-1. The test can be conducted at room temperature or at elevated temperatures. When conducted at an elevated temperature such as 150°C, a sample is placed in an oven or temperature-controlled test chamber, and a progressively increasing voltage is applied until dielectric breakdown occurs.DETAILED DESCRIPTION

[0029] It is to be understood by one of ordinary skill in the art that the present discussion is a description of exemplary embodiments only and is not intended as limiting the broader aspects of the present invention.

[0030] In general, the present disclosure is directed to a thermoplastic polymer composition that is particularly well suited for forming metal overmolded articles. The metal overmolded articles can comprise various electronic components, such as those used to construct an electric vehicle or hybrid vehicle. Metal overmolded parts made according to the present disclosure can also be used in all different types of electronic devices and systems.

[0031] The polymer composition of the present disclosure is formulated so as to not only display excellent flame resistant properties but also display thermal shock resistance. In addition, the polymer composition can also be formulated to display a high comparative tracking index. Still further, polymer compositions formulated according to the present disclosure can display unexpectedly high dielectric strength, especially at high temperatures.

[0032] In the past, problems were experienced in creating thermoplastic polymer compositions that not only had good flame resistant properties but also had good thermal shock resistance and electrical insulating properties. In particular, when components were added to the polymer composition for improving flame resistance, the components may adversely impact the thermal shock resistance and electrical insulating properties. Similarly, many modifiers used toAttorney Docket No.: CICT-1567-PCT2 (2024P0075)improve thermal shock resistance can significantly degrade the fire resistant properties of the composition. Polymer compositions formulated according to the present disclosure, however, have unexpectedly found to have both excellent flame resistance in combination with excellent thermal shock resistance. In addition, and of significant advantage, the polymer composition can also display a relatively high comparative tracking index.

[0033] Thermal shock resistance is particularly desirable when producing metal overmolded parts in electrical systems. Metal overmolded parts, for instance, are widely used in battery management systems and in electric drive units in electric vehicles. The insulating polymer material that is used to coat a metallic part should provide good thermal shock resistance, which means that the polymer coating should show no cracks and maintain good electrical insulating properties after many thermal shock cycles. Polyamide polymers used in the past, for instance, have displayed a relatively poor thermal shock resistance. The present disclosure, however, overcomes the above problems and can be used to formulate polyamide compositions with excellent thermal shock resistance.

[0034] The polymer composition of the present disclosure generally comprises a thermoplastic polymer, such as one or more polyamide polymers, that form a polymer matrix when molded into an article. The thermoplastic polymer is combined with a flame retardant system that can comprise a metal phosphinate. The polymer composition can also contain reinforcing fibers, such as glass fibers. In accordance with the present disclosure, the polymer composition contains a first polyamide polymer that comprises a semi-aromatic polyamide polymer with excellent strength properties. The first polyamide polymer is blended with a second polyamide polymer comprising an amorphous polymer. The polyamide polymers are combined with the flame retardant system and glass fibers having a non-circular cross-sectional shape. The combination of components is found to produce a polymer composition with excellent electrical insulation properties, strong adhesion in metal overmolding applications, excellent flame resistance, and excellent impact resistance demonstrated by thermal shock resistance.

[0035] Polymer compositions formulated in accordance with the present disclosure, for instance, can display a thermal shock resistance when measured over a temperature range of from -40°C to 140°C of greater than about 200 cycles,Attorney Docket No.: CICT-1567-PCT2 (2024P0075)such as greater than about 250 cycles, such as greater than about 300 cycles, such as greater than about 350 cycles, such as greater than about 400 cycles, such as greater than about 450 cycles, such as greater than about 500 cycles, such as greater than about 550 cycles, such as greater than about 600 cycles, such as greater than about 650 cycles. The shock resistance is generally less than about 3,000 cycles.

[0036] In addition, the polymer composition of the present disclosure can be formulated so as to exhibit a VO rating as determined in accordance with UL 94 at a thickness of only 1.6 mm, such as only 0.8 mm, such as only 0.4 mm.

[0037] In addition to flame retardant properties and / or thermal shock resistance, the polymer composition of the present disclosure can also display excellent comparative tracking index properties. The comparative tracking index (CTI) is the maximum voltage, measured in volts, at which a material withstands 50 drops of contaminated water without tracking. Tracking is defined as the formation of conductive paths due to electrical stress, humidity, and contamination. The comparative tracking index test is an accelerated simulation to determine possible future failures that typically result in a short in electrical equipment using the polyamide polymer composition as an insulating material. Comparative tracking index can be measured according to Test I EC 60112:2020. The flame retardant polymer composition of the present disclosure can be formulated to display a comparative tracking index of 550 volts or more, such as 600 volts or more, such as 650 volts or more, such as 700 volts or more (and less than about 2000 volts).

[0038] Due to the excellent flame resistance properties, excellent thermal shock resistance, excellent electrical insulation properties, and excellent mechanical properties, the polymer composition of the present disclosure is well suited for making all different types of articles and components.

[0039] The polymer composition is particularly well suited for producing all different types of electrical components. Such articles can include high voltage powertrain components and other devices that may be powered using lithium ion batteries. The polymer composition can serve as a housing for encasing the electrical component or can be an insulative component that directly surrounds an electrical contact pin or other conductive member. The present disclosure is particularly well suited for producing metal overmolded articles, such as inverters,Attorney Docket No.: CICT-1567-PCT2 (2024P0075)converters, onboard charger bases, relay box frames, busbars, battery pack components, high voltage connectors, and the like.

[0040] As described above, the polymer composition of the present disclosure contains at least two polyamide polymers in combination with a flame retardant composition and reinforcing fibers having a non-circular cross-sectional shape. The polyamide polymers generally include a first polyamide polymer comprising a semi-aromatic polyamide polymer having a relatively high melting temperature. The first polyamide polymer provides strength, mechanical integrity, increases the dielectric strength, and produces a polymer composition well suited for molding applications. The first polyamide polymer is combined with a second polyamide polymer that is amorphous and, in one embodiment, does not display a melting temperature. The amorphous polyamide polymer can be semi-aromatic and can have a relatively low glass transition temperature. The second polyamide polymer significantly enhances the thermal shock resistance properties of the overall composition.

[0041] The first and second polyamide polymers form a polymer matrix. The one or more thermoplastic polymers can be present in the polymer matrix in an amount from about 30% by weight to about 80% by weight, including all increments of 1% by weight therebetween. For example, one or more thermoplastic polymers can be contained in the polymer composition in an amount greater than about 35% by weight, such as in an amount greater than about 38% by weight, such as in an amount greater than about 40% by weight and generally in an amount less than about 70% by weight, such as in an amount less than about 65% by weight, such as in an amount less than about 60% by weight.

[0042] Polyamides generally have a CO-NH linkage in the main chain and are obtained by condensation of a diamine and a dicarboxylic acid, by ring opening polymerization of lactam, or self-condensation of an amino carboxylic acid. For example, the polyamide may contain aliphatic repeating units derived from an aliphatic diamine, which typically has from 4 to 14 carbon atoms. Examples of such diamines include linear aliphatic alkylenediamines, such as 1,4-tetramethylenediamine, 1 ,6-hexanediamine, 1 ,7-heptanediamine, 1,8-octanediamine, 1,9-nonanediamine, 1 ,10-decanediamine, 1,11 -undecanediamine, 1,12-dodecanediamine, etc.; branched aliphatic alkylenediamines, such as 2-Attorney Docket No.: CICT-1567-PCT2 (2024P0075)methyl-1,5-pentanediamine, 3-methyl-1,5 pentanediamine, 2,2,4-trimethyl-1 ,6-hexanediamine, 2,4, 4-trimethyl- 1 ,6-hexanediamine, 2,4-dimethyl-1 ,6-hexanediamine, 2-methyl-1,8-octanediamine, 5-methyl-1,9-nonanediamine, etc.; as well as combinations thereof. Of course, aromatic and / or alicyclic diamines may also be employed.

[0043] The dicarboxylic acid component used to produce the polyamide polymer in accordance with the present disclosure contains at least one aromatic dicarboxylic acid alone or in combination with aliphatic dicarboxylic acids.Examples of aromatic dicarboxylic acids include terephthalic acid, isophthalic acid, 2,6-naphthalenedicarboxylic acid, 2,7-naphthalenedicarboxylic acid, 1 ,4-naphthalenedicarboxylic acid, 1,4-phenylenedioxy-diacetic acid, 1 ,3-phenylenedioxy-diacetic acid, diphenic acid, 4,4'-oxydibenzoic acid, diphenylmethane-4,4'-dicarboxylic acid, diphenylsulfone-4,4'-dicarboxylic acid, 4,4'-biphenyldicarboxylic acid, and the like. Examples of aliphatic dicarboxylic acids include adipic acid, sebacicacid, and the like.

[0044] Examples of lactams include pyrrolidone, aminocaproic acid, caprolactam, undecanlactam, lauryl lactam, and so forth. Likewise, examples of amino carboxylic acids include amino fatty acids, which are compounds of the aforementioned lactams that have been ring opened by water.

[0045] The first polyamide polymer contained within the polymer composition of the present disclosure, in one aspect, has a relatively high melting temperature. For instance, the melting temperature of the first polyamide polymer can be greater than about 280°C, such as greater than about 285°C, such as greater than about 290°C, such as greater than about 295°C, and less than about 350°C, such as less than about 345°C, such as less than about 340°C, such as less than about 335°C. The first polyamide polymer can be semi-aromatic and can be a homopolymer, a copolymer, or a terpolymer.

[0046] The first polyamide polymer, for instance, can comprise one or more of the following polyamide polymers: poly(tetramethylene terephthalamide / 2-methylpentamethylene terephthalamide) PA4T / DT, poly(tetramethylene terephthalamide / hexamethylene terephthalamide) PA4T / 6T, poly(tetramethylene terephthalamide / decamethylene terephthalamide) PA4T / 10T, poly(tetramethylene terephthalamide / dodecamethylene terephthalamide)PA4T / 12T,Attorney Docket No.: CICT-1567-PCT2 (2024P0075)poly(tetramethylene terephthalamide / 2-methylpentamethylene terephthalamide / hexamethylene terephthalamide) (PA4T / DT / 6T), poly(tetramethylene terephthalamide / hexamethylene terephthalamide / 2-methylpentamethylene terephthalamide) (PA4T / 6T / DT), poly(hexamethylene terephthalamide / 2-methylpentamethylene terephthalamide) (PA6T / DT), poly(hexamethylene hexanediamide / hexamethylene isophthalamide) (PA 6T / 61), poly(hexamethylene terephthalamide / decamethylene terephthalamide) PA6T / 10T, poly(hexamethylene terephthalamide / dodecamethylene terephthalamide) (PA6T / 12T), poly(hexamethylene terephthalamide / 2-methylpentamethylene terephthalamide / poly(decamethylene terephthalamide) (PA6T / DT / 1 OT), poly(hexamethylene terephthalamide / decamethylene terephthalamide / dodecamethylene terephthalamide) (PA6T / 10T / 12T), poly(decamethylene terephthalamide) (PA10T), poly(decamethylene terephthalamide / tetramethylene terephthalamide) (PA10T / 4T), poly(decamethylene terephthalamide / 2-methylpentamethylene terephthalamide) (PA10T / DT), poly(decamethylene terephthalamide / dodecamethylene terephthalamide) (PA10T / 12T), poly(decamethylene terephthalamide / 2-methylpentamethylene terephthalamide / (decamethylene terephthalamide) (PA10T / DT / 12T). poly(dodecamethylene terephthalamide) (PA12T), poly(dodecamethylene terephthalamide) / tetramethylene terephthalamide) (PA12T / 4T), poly(dodecamethylene terephthalamide) / hexamethylene terephthalamide) PA12TI6T, poly(dodecamethylene terephthalamide) / decamethylene terephthalamide) (PA12T / 10T), and poly(dodecamethylene terephthalamide) / 2-methylpentamethylene terephthalamide) (PA12T / DT), poly(hexamethylene terephthalamide / polyhexamethylene adipamide) (PA6T / 66), and mixtures thereof.

[0047] In one particular embodiment, the first polyamide comprises the following:(C12H22N2O2)n(C14H26N2O2)mwherein n and m can independently be from about 5 to about 5000, such as from about 50 to about 1000, such as from about 75 to about 500.Attorney Docket No.: CICT-1567-PCT2 (2024P0075)

[0048] The polyamides described above can be homopolymers, copolymers, or terpolymers. The polyamide polymers are made from structural units, such as diamines and carboxylic acids. The structural units are combined together to form monomers which are used to produce the polymers. The following list exemplifies the abbreviations used to identify the monomers and repeat units in the polyamide polymers.Abbreviation Descriptionhexamethylene diamine (or 6 when used inHMDcombination with a diacid)T Terephthalic acidAA Adipic acidDMD or 10 DecamethylenediamineI Isophthalic acid6I Polymer repeat unit formed from HMD and I MXD meta-xylylene diamine2-MPMD 2-methylpentamethylenediamine4T polymer repeat unit formed from TMD and T6T polymer repeat unit formed from HMD and TDT polymer repeat unit formed from 2-MPMD and T MXD6 polymer repeat unit formed from MXD and AA66 polymer repeat unit formed from HMD and AA10T polymer repeat unit formed from DMD and T polymer repeat unit formed from6€-caprolactampolymer repeat unit formed from1111-aminoundecanoic acidpolymer repeat unit formed from1212-aminododecanoic acid

[0049] The first polyamide polymer is present in the polymer composition generally in an amount from about 10% by weight to about 55% by weight, including all increments of 1% by weight therebetween. For instance, the firstAttorney Docket No.: CICT-1567-PCT2 (2024P0075)polyamide polymer can be present in the polymer composition in an amount greater than about 13% by weight, such as in an amount greater than about 15% by weight, such as in an amount greater than about 17% by weight, such as in an amount greater than about 20% by weight, such as in an amount greater than about 23% by weight, such as in an amount greater than about 25% by weight, and in an amount less than about 53% by weight, such as in an amount less than about 50% by weight, such as in an amount less than about 48% by weight, such as in an amount less than about 45% by weight, such as in an amount less than about 43% by weight, such as in an amount less than about 40% by weight.

[0050] The first polyamide polymer is combined with a second polyamide polymer in accordance with the present disclosure. The second polyamide polymer can be an amorphous polymer, can be a semi-aromatic polyamide polymer, and / or can have a glass transition temperature of less than about 200°C and greater than about 100°C. For instance, the second polyamide polymer can have a glass transition temperature of greater than about 110°C, such as greater than about 115°C, such as greater than about 120°C, and less than about 160°C, such as less than about 155°C, such as less than about 150°C.

[0051] In one aspect, the second polyamide polymer comprises an amorphous semi-aromatic polyamide polymer. Amorphous semi-aromatic polyamide polymers can lack a distinctive crystalline melting point, resulting in a material with excellent dimensional stability and adhesion properties. The second polyamide polymer, for instance, can increase the toughness of the polymer composition and can serve to dramatically improve thermal shock resistance without compromising other properties.

[0052] The second polyamide polymer, for instance, can comprise poly(hexamethylene isophthalamide / hexamethylene terephthalamide) (PA6I / 6T), poly(hexamethylene isophthalamide / decamethylene terephthalamide) (PA6I / 10T), or the like. The second polyamide polymer may also comprise a mixture of amorphous polyamide polymers. For instance, the second polyamide polymer may also comprise poly(hexamethylene isophthalamide)(PA6l) and / or poly(meta-xylylene diamine adipate)(MXD6), or the like. The second polyamide polymer may also comprise a polyamide terpolymer, such as poly(hexamethylene isophthalamide / hexamethylene terephthalamide / hexamethyleneAttorney Docket No.: CICT-1567-PCT2 (2024P0075)hexanediamide)(PA6l / 6T / 66), poly(hexamethylene isophthalamide / hexamethylene terephthalamide / decamethylene terephthalamide)(PA6l / 6T / 1 OT), poly(hexamethylene isophthalamide / hexamethylene terephthalamide / meta-xylylene diamine adipate)(PA6l / 6T / MXD6).

[0053] The second polyamide polymer can generally be present in the polymer composition in an amount from about 5% by weight to about 40% by weight, including all increments of 1% by weight therebetween. For instance, the second polyamide polymer can be present in the polymer composition in an amount greater than about 10% by weight, such as in an amount greater than about 15% by weight, such as in an amount greater than about 17% by weight, such as in an amount greater than about 20% by weight, and in an amount less than about 38% by weight, such as in an amount less than about 35% by weight, such as in an amount less than about 30% by weight, such as in an amount less than about 27% by weight, such as in an amount less than about 25% by weight.

[0054] In addition to one or more thermoplastic polymers, the polymer matrix may also contain a flame retardant system to help achieve the desired flammability performance. In one aspect, the flame retardant system of the present disclosure only contains one flame retardant component, although in other embodiments various other components may be added. Excellent flame resistant properties in combination with excellent melt processing characteristics can be obtained by incorporating into the polymer composition a non-halogen flame retardant.

[0055] In one embodiment, the flame retardant system of the present disclosure contains a metal phosphinate. Such phosphinates are typically salts of a phosphinic acid and / or diphosphinic acid, such as those having the general formula (I) and / or formula (II):Attorney Docket No.: CICT-1567-PCT2 (2024P0075)(II) wherein,R7 and Rs are, independently, hydrogen or substituted or unsubstituted, straight chain, branched, or cyclic hydrocarbon groups (e.g., alkyl, alkenyl, alkynyl, aralkyl, aryl, alkaryl, etc.) having 1 to 6 carbon atoms, particularly alkyl groups having 1 to 4 carbon atoms, such as methyl, ethyl, n-propyl, iso-propyl, n-butyl, or tert-butyl groups;R9 is a substituted or unsubstituted, straight chain, branched, or cyclic C1-C10 alkylene, arylene, arylalkylene, or alkylarylene group, such as a methylene, ethylene, n-propylene, iso-propylene, n-butylene, tert-butylene, n-pentylene, n-octylene, n-dodecylene, phenylene, naphthylene, methylphenylene, ethylphenylene, tert-butylphenylene, methylnaphthylene, ethylnaphthylene, t-butylnaphthylene, phenylethylene, phenylpropylene or phenylbutylene group; Z is Mg, Ca, Al, Sb, Sn, Ge, Ti, Zn, Fe, Zr, Ce, Bi, Sr, Mn, Li, Na, K, and / or a protonated nitrogen base;y is from 1 to 4, and preferably 1 to 2 (e.g., 1);n is from 1 to 4, and preferably 1 to 2 (e.g. 1); andm is from 1 to 4 and preferably 1 to 2 (e.g., 2).

[0056] The phosphinates may be prepared using any known technique, such as by reacting a phosphinic acid with a metal carbonate, metal hydroxide, or metal oxides in aqueous solution. Particularly suitable phosphinates include, for example, metal salts of dimethylphosphinicacid, ethylmethylphosphinic acid, diethylphosphinic acid, methyl-n-propylphosphinic acid, methane-di(methylphosphinic acid), ethane-1 ,2-di(methylphosphinic acid), hexane-1,6-di(methylphosphinic acid), benzene-1 ,4-di(methylphosphinic acid), methylphenylphosphinic acid, diphenylphosphinic acid, hypophosphoric acid, etc. The resulting salts are typically monomeric compounds; however, polymeric phosphinates may also be formed. Particularly suitable metals for the salts may include Al and Zn. For instance, one particularly suitable phosphinate is zincAttorney Docket No.: CICT-1567-PCT2 (2024P0075)diethylphosphinate. Another particularly suitable phosphinate is aluminum diethylphosphinate.

[0057] One or more metal phosphinates can generally be present in the polymer composition in an amount greater than about 6% by weight, such as in an amount greater than about 8% by weight, such as in an amount greater than about 10% by weight. One or more metal phosphinates are generally present in the polymer composition in an amount less than about 20% by weight, such as in an amount less than about 18% by weight, such as in an amount less than about 15% by weight.

[0058] Optionally, the metal phosphinate can be combined with a synergist, such as a nitrogen-containing synergist. The synergist, for instance, can comprise a polyphosphate, such as a melamine polyphosphate. Other nitrogen-containing synergists include melamine and melamine derivatives.

[0059] In one aspect of the present disclosure, however, the flame retardant composition can be formulated so as to only contain the metal phosphinate. The composition can be free of nitrogen-containing synergists and can be free of inorganic compounds typically combined with phosphinates, such as zinc borate. Although unknown, it is believed that formulating the composition without containing any flame retardant synergists can further increase thermal shock resistance.

[0060] The polymer composition of the present disclosure also contains reinforcing fibers, particularly glass fibers having a non-circular cross-sectional shape. The reinforcing fibers are incorporated into the composition in order to further increase shock resistance without compromising the electrical insulating properties.

[0061] Glass fibers with non-circular cross-sectional shapes refer to glass fibers having a cross-section having a major axis lying perpendicular to a longitudinal direction of the glass fiber and corresponding to the longest linear distance in the cross-section (width). The non-circular cross-section has a minor axis corresponding to the longest linear distance in the cross-section in a direction perpendicular to the major axis (height). The non-circular cross-section of the fiber may have a variety of shapes including a cocoon-type shape, a rectangular shape, an elliptical shape, a roughly triangular shape, a polygon shape, a shape of anAttorney Docket No.: CICT-1567-PCT2 (2024P0075)oval, and / or an oblong shape. The ratio of the length of the major axis (width) to that of the minor axis (height) can be from about 1.5:1 to about 7:1, such as from about 2:1 to about 6:1, such as from about 3:1 to about 5:1.

[0062] In one aspect, the glass fibers have an eliptic or oval shape crosssection. The major axis or width can be greater than about 16 microns, such as greater than about 20 microns, such as greater than about 22 microns, such as greater than about 24 microns, and less than about 45 microns, such as less than about 40 microns, such as less than about 32 microns, such as less than about 30 microns. The minor axis or height can be greater than about 3 microns, such as greater than about 4 microns, and less than about 9 microns, such as less than about 8 microns.

[0063] The glass fibers can have an average fiber length of greater than about 0.5 mm, such as greater than about 1 mm, such as greater than about 1.5 mm, such as greater than about 2 mm, such as greater than about 2.5 mm. The average fiber length of the glass fibers is generally less than about 5 mm, such as less than about 4.5 mm, such as less than about 4 mm, such as less than about 3.5 mm.

[0064] The amount of reinforcing fibers contained in the polymer composition can depend upon the particular application and the desired results. In general, reinforcing fibers can be present in the polymer composition in an amount from about 8% by weight to about 58% by weight, including all increments of 1% by weight therebetween. For instance, reinforcing fibers can be present in the polymer composition in an amount greater than about 10% by weight, such as in an amount greater than about 13% by weight, such as in an amount greater than about 18% by weight, such as in an amount greater than about 20% by weight, such as in an amount greater than about 23% by weight, such as in an amount greater than about 25% by weight, such as in an amount greater than about 28% by weight, such as in an amount greater than about 30% by weight, such as in an amount greater than about 35% by weight, such as in an amount greater than about 40% by weight, such as in an amount greater than about 45% by weight. The reinforcing fibers are generally present in an amount less than about 53% by weight, such as in an amount less than about 50% by weight, such as in an amount less than about 48% by weight. In one embodiment, for instance, theAttorney Docket No.: CICT-1567-PCT2 (2024P0075)polymer composition can contain the glass fibers in an amount from about 25% by weight to about 35% by weight. In an alternative embodiment, the reinforcing fibers can be present in the polymer composition in an amount from about 45% by weight to about 55% by weight. Thermal shock resistance can be improved by increasing the amount of glass fibers contained in the composition. The amount of glass fibers contained in the composition, however, can be balanced with the melt processing characteristics of the polymer composition.

[0065] The polymer composition of the present disclosure, in addition to a blend of polyamide polymers, a flame retardant composition, and reinforcing fibers, can contain various other components and ingredients. For instance, the polymer composition can contain a lubricant, a thermal cycling agent especially when greater amounts of reinforcing fibers are present in the composition, coloring agents, and various different stabilizers.

[0066] In one aspect, for instance, the polymer composition can contain a lubricant. The lubricant can be present in the polymer composition in an amount from about 0.01% by weight to about 2% by weight. For instance, the lubricant can be present in an amount greater than about 0.08% by weight, such as in an amount greater than about 0.1 % by weight, such as in an amount greater than about 0.15% by weight, and less than about 1% by weight, such as less than about 0.5% by weight.

[0067] The lubricant may be formed from a fatty acid salt derived from fatty acids having a chain length of from 22 to 38 carbon atoms, and in some embodiments, from 24 to 36 carbon atoms. Examples of such fatty acids may include long chain aliphatic fatty acids, such as montanic acid (octacosanoic acid), arachidic acid (arachic acid, icosanic acid, icosanoic acid, n-icosanoic acid), tetracosanoic acid (lignoceric acid), behenic acid (docosanoic acid), hexacosanoic acid (cerotinic acid), melissic acid (triacontanoic acid), erucic acid, cetoleic acid, brassidic acid, selacholeic acid, nervonic acid, etc. For example, montanic acid has an aliphatic carbon chain of 28 atoms and arachidic acid has an aliphatic carbon chain of 20 atoms. Due to the long carbon chain provided by the fatty acid, the lubricant has a high thermostability and low volatility. This allows the lubricant to remain functional during formation of the desired article to reduce internal and external friction, thereby reducing the degradation of the material caused byAttorney Docket No.: CICT-1567-PCT2 (2024P0075)mechanical / chemical effects.

[0068] The fatty acid salt may be formed by saponification of a fatty acid wax to neutralize excess carboxylic acids and form a metal salt. Saponification may occur with a metal hydroxide, such as an alkali metal hydroxide (e.g., sodium hydroxide) or alkaline earth metal hydroxide (e.g., calcium hydroxide). The resulting fatty acid salts typically include an alkali metal (e.g., sodium, potassium, lithium, etc.) or alkaline earth metal (e.g., calcium, magnesium, etc.). Such fatty acid salts generally have an acid value (ASTM D 1386) of about 20 mg KOH / g or less, in some embodiments about 18 mg KOH / g or less, and in some embodiments, from about 1 to about 15 mg KOH / g. Particularly suitable fatty acid salts for use in the present invention are derived from crude montan wax, which contains straightchain, unbranched monocarboxylic acids with a chain length in the range of C28-C32. Such montanic acid salts are commercially available from Clariant GmbH under the designations Licomont® CaV 102 (calcium salt of long-chain, linear montanic acids) and Licomont® NaV 101 (sodium salt of long-chain, linear montanic acids).

[0069] If desired, fatty acid esters may be used as lubricants. Fatty acid esters may be obtained by oxidative bleaching of a crude natural wax and subsequent esterification of the fatty acids with an alcohol. The alcohol typically has 1 to 4 hydroxyl groups and 2 to 20 carbon atoms. When the alcohol is multifunctional (e.g., 2 to 4 hydroxyl groups), a carbon atom number of 2 to 8 is particularly desired. Particularly suitable multifunctional alcohols may include dihydric alcohol (e.g., ethylene glycol, propylene glycol, butylene glycol, 1 ,3-propanediol, 1,4-butanediol, 1 ,6-hexanediol and 1 ,4-cyclohexanediol), trihydric alcohol (e.g., glycerol and trimethylolpropane), tetrahydric alcohols (e.g., pentaerythritol and erythritol), and so forth. Aromatic alcohols may also be suitable, such as o-, m-and p-tolylcarbinol, chlorobenzyl alcohol, bromobenzyl alcohol, 2,4-dimethylbenzyl alcohol, 3,5-dimethylbenzyl alcohol, 2,3,5-cumobenzyl alcohol, 3,4,5-trimethylbenzyl alcohol, p-cuminyl alcohol, 1 ,2-phthalyl alcohol, 1,3-bis(hydroxymethyl)benzene, 1 ,4-bis(hydroxymethyl)benzene, pseudocumenyl glycol, mesitylene glycol and mesitylene glycerol. Particularly suitable fatty acid esters for use in the present invention are derived from montanic waxes.Licowax® OP (Clariant), for instance, contains montanic acids partially esterifiedAttorney Docket No.: CICT-1567-PCT2 (2024P0075)with butylene glycol and montanic acids partially saponified with calcium hydroxide. Thus, Licowax® OP contains a mixture of montanic acid esters and calcium montanate. Other montanic acid esters that may be employed include Licowax® E, Licowax® OP, and Licolub® WE 4 (all from Clariant), for instance, are montanic esters obtained as secondary products from the oxidative refining of raw montan wax. Licowax® E and Licolub®WE 4 contain montanic acids esterified with ethylene glycol or glycerine.

[0070] Other known waxes may also be employed in a lubricant. Amide waxes, for instance, may be employed that are formed by reaction of a fatty acid with a monoamine or diamine (e.g., ethylenediamine) having 2 to 18, especially 2 to 8, carbon atoms. For example, ethylenebisamide wax, which is formed by the amidization reaction of ethylene diamine and a fatty acid, may be employed. The fatty acid may be in the range from Ci2to C30, such as from stearic acid (Cis fatty acid) to form ethylenebisstearamide wax. Ethylenebisstearamide wax is commercially available from Lonza, Inc. under the designation Acrawax® C, which has a discrete melt temperature of 142°C. Other ethylenebisamides include the bisamides formed from lauric acid, palmitic acid, oleic acid, linoleic acid, linolenic acid, oleostearic acid, myristic acid and undecalinic acid. Still other suitable amide waxes are N-(2-hydroxyethyl)12-hydroxystearamide and N,N'-(ethylene bis)12-hydroxystearamide, which are commercially available from CasChem, a division of Rutherford Chemicals LLC, under the designations Paricin® 220 and Paricin®285, respectively.

[0071] In one embodiment, the polymer composition can optionally further contain a thermal cycling agent, such as a silicone polymer. The thermal cycling agent can not only compatibilize the different ingredients but can also increase the thermal shock resistance properties.

[0072] As described above, the thermal cycling agent can comprise a silicone. The silicone polymer can have any suitable molecular weight. In one aspect, the silicone polymer can be an ultra-high molecular weight silicone. In general, the UHMW-Si can have an average molecular weight of greater than 100,000 g / mol, such as greater than about 200,000 g / mol, such as greater than about 300,000 g / mol, such as greater than about 500,000 g / mol and less than about 3,000,000 g / mol, such as less than about 2,000,000 g / mol, such as less than aboutAttorney Docket No.: CICT-1567-PCT2 (2024P0075)1 ,000,000 g / mol, such as less than about 500,000 g / mol, such as less than about 300,000 g / mol. Generally, the UHMW-Si can have a kinematic viscosity at 40°C measured according to DIN 51562 of greater than 100,000 mm2s’1, such as greater than about 200,000 mm2s'1, such as greater than about 1,000,000 mm2s’1, such as greater than about 5,000,000 mm2s'1, such as greater than about 10,000,000 mm2s'1, such as greater than about 15,000,000 mm2s’1and less than about 50,000,000 mm2S’1, such as less than about 25,000,000 mm2S'1, such as less than about 10,000,000 mm2s'1, such as less than about 1 ,000,000 mm2s'1, such as less than about 500,000 mm2s'1, such as less than about 200,000 mm2s'1.

[0073] The UHMW-Silicone may comprise a siloxane such as a polysiloxane or polyorganosiloxane. In one embodiment, the UHMW-Si may comprise a dialkylpolysiloxane such as a dimethylsiloxane, an alkylarylsiloxane such as a phenylmethylsiloxane, a polysilsesquioxane, or a diarylsiloxane such as a diphenylsiloxane, ora homopolymer thereof such as a polydimethylsiloxane ora polymethylphenylsiloxane, ora copolymer thereof with the above molecular weight and / or kinematic viscosity requirements. The polysiloxane or polyorganosiloxane may also be modified with a substituent such as an epoxy group, a hydroxyl group, a carboxyl group, an amino group or a substituted amino group, an ether group, or a meth(acryloyl) group in the end or main chain of the molecule. The UHMW-Si compounds may be used singly or in combination. Any of the above UHMW-Si compounds may be used with the above molecular weight and / or kinematic viscosity requirements.

[0074] In one aspect, the silicone polymer is incorporated into the polymer composition as a master batch. The master batch can contain the silicone polymer combined with a carrier polymer. The carrier polymer can comprise a polymer compatible with the silicone polymer and compatible with the other polymers present in the composition. In one aspect, for instance, the carrier polymer can comprise a polyamide polymer. For instance, the carrier polymer can comprise an aliphatic polyamide polymer. The carrier polymer, for instance, can comprise polyamide 6, polyamide 66, or mixtures thereof.

[0075] The carrier polymer can be present in the master batch in an amount greater than about 20% by weight, such as in an amount greater than about 30% by weight, such as in an amount greater than about 40% by weight, and in anAttorney Docket No.: CICT-1567-PCT2 (2024P0075)amount less than about 70% by weight, such as in an amount less than about 60% by weight, such as in an amount less than about 50% by weight. The silicone polymer can be present in an amount from about 30% by weight to about 80% by weight, including all increments of 1 % by weight therebetween. For example, the silicone polymer can be present in the master batch in an amount greater than 30% by weight, such as in an amount greater than about 40% by weight, such as in an amount greater than about 50% by weight, and in an amount less than about 80% by weight, such as in an amount less than about 70% by weight.

[0076] The thermal cycling agent or silicone polymer is generally present in the polymer composition in amounts less than about 2% by weight. For instance, the thermal cycling agent can be present in the polymer composition in an amount less than about 1.75% by weight, such as in an amount less than about 1.6% by weight, such as in an amount less than about 1.5% by weight, such as in an amount less than about 1.25% by weight, such as in an amount less than about 1.1% by weight, such as in an amount less than about 0.9% by weight, such as in an amount less than about 0.7% by weight, such as in an amount less than about 0.5% by weight, such as in an amount less than about 0.4% by weight. The thermal cycling agent can be present in the polymer composition in an amount greater than about 0.08% by weight, such as in an amount greater than about 0.1 % by weight, such as in an amount greater than about 0.15% by weight, such as in an amount greater than about 0.175% by weight.

[0077] In one aspect, the polymer composition can further contain at least one stabilizer. The stabilizer can include, for instance, an antioxidant.

[0078] The antioxidant, for instance, can be a phenolic antioxidant. In one embodiment, for instance, the composition can contain a phenolic antioxidant. Examples of such phenolic antioxidants include, for instance, calcium bis(ethyl 3,5-di-tert-butyl-4-hydroxybenzylphosphonate) (Irganox® 1425); terephthalic acid, 1,4-dithio-,S,S-bis(4-tert-butyl-3-hydroxy-2,6-dimethylbenzyl) ester (Cyanox® 1729); triethylene glycol bis(3-tert-butyl-4-hydroxy-5-methylhydrocinnamate); hexamethylene bis(3,5-di-tert-butyl-4-hydroxyhydrocinnamate (Irganox® 259); 1,2-bis(3,5,di-tert-butyl-4-hydroxyhydrocinnamoyl)hydrazide (Irganox® 1024); 4,4'-di-tert-octyldiphenamine (Naugalube® 438R); phosphonic acid, (3,5-di-tert-butyl-4-hydroxybenzyl)-, dioctadecyl ester (Irganox® 1093); 1 ,3,5-trimethyl-2,4,6-tris(3',5'-Attorney Docket No.: CICT-1567-PCT2 (2024P0075)di-tert-butyl-4' hydroxybenzyl)benzene (Irganox® 1330); 2,4-bis(octylthio)-6-(4-hydroxy-3,5-di-tert-butylanilino)-1 ,3,5-triazine (Irganox® 565); isooctyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate (Irganox® 1135); octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate (Irganox® 1076); 3,7-bis(1 ,1 ,3,3-tetramethylbutyl)-10H-phenothiazine (Irganox® LO 3); 2,2'-methylenebis(4-methyl-6-tert-butylphenol)monoacrylate (Irganox® 3052); 2-tert-butyl-6-[1-(3-tert-butyl-2-hydroxy-5-methylphenyl)ethyl]-4-methylphenyl acrylate (Sumilizer® TM 4039); 2-[1-(2-hydroxy-3,5-di-tert-pentylphenyl)ethyl]-4,6-di-tert-pentylphenyl acrylate (Sumilizer® GS); 1,3-dihydro-2H-Benzimidazole (Sumilizer® MB); 2-methyl-4,6-bis[(octylthio)methyl]phenol (Irganox® 1520); N,N'-trimethylenebis-[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionamide (Irganox® 1019); 4-n-octadecyloxy-2,6-diphenylphenol (Irganox® 1063); 2,2'-ethylidenebis[4,6-di-tert-butylphenol] (Irganox® 129); N N'-hexamethylenebis(3,5-di-tert-butyl-4-hydroxyhydrocinnamamide) (Irganox® 1098); diethyl (3,5-di-tert-butyl-4-hydroxybenxyl)phosphonate (Irganox® 1222); 4,4'-di-tert-octyldiphenylamine (Irganox® 5057); N-phenyl-1-napthalenamine (Irganox® L 05); tris[2-tert-butyl-4-(3-ter-butyl-4-hydroxy-6-methylphenylthio)-5-methyl phenyl]phosphite (Hostanox® OSP 1); zinc dinonyidithiocarbamate (Hostanox® VP-ZNCS 1); 3,9-bis[1 ,1-diimethyl-2-[(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy]ethyl]-2,4,8,10-tetraoxaspiro[5.5]undecane (Sumilizer® AG80); pentaerythrityl tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] (Irganox® 1010); ethylene-bis(oxyethylene)bis[3-(5-tert-butyl-4-hydroxy-m-tolyl)-propionate (Irganox® 245); 3,5-di-tert-butyl-4-hydroxytoluene (Lowinox BHT, Chemtura) and the like.In one embodiment, the antioxidant can be a reaction product of 2,4-di-tert-butylphenol, phosphorous trichloride, and 1 , 1 ’-biphenyl. In one aspect, the antioxidant comprises tetrakis(2,4-di-tert-butylphenyl)-4,4biphenyldiphosphonite. In one aspect, the antioxidant may comprises a phosphite. One example of a phosphite stabilizer is tris(2,4-di-tert-butylphenyl) phosphite.

[0079] In one aspect, an antioxidant may be present that is a hindered phenolic antioxidant. The hindered phenolic antioxidant, for instance, may comprise N,N'-(hexane-1,6-diyl)bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propanamide],

[0080] One or more antioxidants can be present in the polymer composition generally in an amount greater than about 0.05% by weight, such as in an amountAttorney Docket No.: CICT-1567-PCT2 (2024P0075)greater than about 0.08% by weight, such as in an amount greater than about 0.1 % by weight, such as in an amount greater than about 0.2% by weight, such as in an amount greater than about 0.4% by weight, and generally less than about 2% by weight, such as less than about 1.5% by weight, such as less than about 1% by weight, such as less than about 0.8% by weight, such as less than about 0.5% by weight, such as less than about 0.4% by weight.

[0081] The composition can optionally include a light stabilizer which may comprise a hindered amine light stabilizer. Examples of light stabilizers that may be incorporated into the present disclosure include a benzenedicarboxamide. In one aspect, the light stabilizer comprises N,N'-Bis(2,2,6,6-tetramethyl-4-piperidinyl)- 1 ,3-benzenedicarboxamide. The light stabilizer may also comprise any compound which is derived from an alkylsubtituted piperidyl, piperidinyl or piperazinone compound or a substituted alkoxypiperidinyl. Other suitable HALS are those that are derivatives of 2,2, 6,6-tetramethyl piperidine. Preferred specific examples of HALS include: —2,2, 6,6-tetramethyl-4-piperidinone, -2,2, 6,6-tetramethyl-4-piperidinol, — bis-(2, 2, 6,6-tetramethyl-4-piperidinyl)-sebacate, -mixtures of esters of 2,2,6,6-tetramethyl-4-piperidinol and fatty acids, ~bis-(2,2,6,6-tetramethyl-4-piperidinyl)-succinate, ~bis-(1-octyloxy-2,2,6,6-tetramethyl-4-piperidinyl)-sebacate, ~bis-(1,2,2,6,6-pentamethyl-4-piperidinyl)-sebacate, ~tetrakis-(2,2,6,6-tetramethyl-4-piperidyl)-1,2,3,4-butane-tetracarboxylate, ~N-butyl-2,2,6,6-tetramethyl-4-piperidinamine, ~N,N'-bis-(2,2,6,6-tetramethyl-4-piperidyl)-hexane-1,6-diamine, ~2.2'-[(2.2.6.6-tetramethyl-4-piperidinyl)-imino]-bis-[ethanol], ~5-(2.2.6.6-tetramethyl-4-piperidinyl)-2-cyclo-undecyl-oxazole), -mixture of: 2, 2, 4, 4 tetramethyl-21-oxo-7-oxa-3.20-diazadispiro [5.1.11.2] heneicosane-20-propionic acid dodecylester and 2.2.4.4 tetramethyl-21-oxo-7; oxa-3,20-diazadispiro [5,1 ,11 ,2]-heneicosane-20-propionic acid; tetradecyl ester, -diacetam 5 (CAS registration number: 76505-58-3), -propanedioic acid, [(4-methoxyphenyl) methylene]-, bis(1 ,2,2,6, 6-pentamethyl-4-piperidinyl) ester, —1,3-benzendicarboxamide, N,N'-bis (2,2,6,6-tetramethyl-4-piperidinyl), ~3-dodecyl-1-(2,2,6,6-tetramethyl-4-piperidyl)-pyrrolidin-2,5-dione, -formamide, N,N'-1 ,6-hexanediylbis [N-(2,2,6,6-tetramethyl-4-piperidinyl, ~3-dodecyl-1-(1 ,2,2, 6,6-pentamethyl-4-piperidyl)-pyrrolidin-2, 5-dione, -1 ,5-Dioxaspiro (5,5) undecane 3,3-dicarboxylic acid, bis (2,2,6,6-tetramethyl-4-peridinyl) ester, ~1,5-Dioxaspiro (5,5)Attorney Docket No.: CICT-1567-PCT2 (2024P0075)undecane 3,3-dicarboxylic acid, bis (1 ,2,2,6, 6-pentamethyl-4-peridinyl) ester, -bis (1 ,2,2,6,6-penta methyl-4-piperidyl)(3,5-di-t-butyl-4-hydroxybenzyl)-butylpropanedioate, ~tetrakis-( 1 ,2,2,6,6-penta-methyl-4-piperidyl)-1 ,2,3,4-butane-tetra- -carboxylate, -1 ,2, 3, 4-butanetetracarboxylic acid, tetrakis(2, 2,6,6-tetramethyl-4-piperidinyl) ester, -1 ,2,3,4-butane-tetracarboxylic acid-1, 2, 3-tris (1 ,2,2,6,6-pentamethyl-4-piperidinyl)-4-tridecylester, ~8-acetyl-3-dodecyl-7, 7,9,9-tetra methyl-1,3,8-triazaspiro (4,5) decane-2, 4-dione, ~N-2,2,6,6-tetrametyl-4-piperidinyl-N-amino-oxamide, ~4-acryloyloxy-1 ,2,2,6,6-pentamethyl-4-piperidine, -1 ,5,8, 12-tetrakis [2',4'-bis (1",2",2",6",6"-pentamethyl-4"-piperidinyl(butyl)amino)-1 ',3',5'-tr- iazi n-6'-y I]- 1 ,5,8,12-tetraazadodecane, -1 , 1 '-( 1 , 2-ethane-d i-y l)-bis-(3 , 3' , 5,5'-tetra-methyl-piperazinone) (Good rite 3034), -propane amide, 2-methyl-N-(2,2,6,6-tetramethyl-4-piperidinyl)-2-[(2,2,6,6-tetramethyl-4-piperidinyl)amino], -oligomer of N-(2-hydroxyethyl)-2,2,6,6-tetramethyl-4-piperidinol and succinic acid, -poly [[6-[(1,1,3,3-tetramethylbutyl)amino]-s-triazine-2,4-diyl][2,2,6,6-tetram- ethyl-4-piperidinyl)im ino] hexamethylene [(2,2,6,6-tetramethyl-4-piperidinyl)imino]], -poly [(6-morfoline-S-triazine-2.4-diyl) [(2.2.6.6-tetramethyl-4-piperidinyl)-imino]hexamethylene-[(2.2.6.6-tetram- ethyl-4-piperidinyl)-imino]], - poly [(6-morpholino-s-triazine-2.4-diyl) [1.2.2.6.6-penta-methyl-4-piperidyl) imino]-hexamethylene [(2, 2, 6, 6 tetra-methyl-4-piperidyl) imino]], -poly methylpropyl-3-oxy-[4(2.2.6.6-tetrametyl)-piperidinyl)]-siloxane copolymer of a-methylstyrene and n-(2.2.6.6-tetramethyl-piperidinyl)-4-maleimide and N-stearyl-maleimide, -1, 2,3,4-butane tetracarboxylic acid, polymer with 8,8,8',8'-tetramethyl-2,4,8, 10-tetraoxaspiro [5,5] undecane-3,9-diethanol, 1,2,2, 6,6-pentamethyl-4-piperidinyl ester, -1,2, 3, 4-butanetetracarboxylic acid, polymer with 8,8,8',8'-tetramethyl-2,4,8,10-tetraoxaspiro [5,5] undecane-3,9-diethanol, 2,2,6,6-tetramethyl-4-piperidinyl ester, -oligomer of 7-Oxa-3,20-diazadispiro [5,1,11,2] heneicosan-21-one, 2,2,4,4-tetramethyl-20-(oxiranylmethyl), -1 ,3,5-Triazine-2,4,6-triamine, N, N"-[1 ,2-ethanediylbis [[[4,6-bis[buty I (1 ,2,2,6,6-pentamethyl-4-iperidinyl)amino]-1 ,3,5-triazine- -2-yl]imino]-3, 1 - propanediyl]]-bis [N. N"-dibutyl-N. N"-bis (1.2.2.6.6-pentamethyl-4-piperidinyl), ~1.3-Propanediamine, N, N-1 ,2-ethanediylbis-, polymer with 2,4,6-trichloro-1 ,3,5-triazine, reaction products with N-butyl-2, 2,6,6-tetramethyl-4-piperidinamine, -1 ,6-Hexanediamine, N,N'-bis (2,2,6,6-tetramethyl-4piperidinyl)-polymer with 2,4,6-trichloro-1 ,3,5-triazine, reaction products with N-Attorney Docket No.: CICT-1567-PCT2 (2024P0075)butyl-1-butanamine and N-butyl-2,2,6,6-tetramethyl-4-piperidinamine, -2,9,11,13,15,22,24,26,27,28-Decaazatricyclo [21 ,3,1,110,14]octacosa-1 (27), 10,12,14(28),23,25-hexaene-12, 25-diamine, N, N '-bis (1,1 ,3,3-tetramethylbutyl)-2,9,15,22-tetrakis (2 , 2 , 6 ,6-tetra m ethy l-4-pi peri di ny I)- , -1,1,1 "-(1 ,3,5-T riazine-2,4,6-triyltris ((cyclohexylimino)-2,1 -ethanediyl) tris (3,3,5,5-tetramethylpiperazinone), -1,1,1 "-(1 ,3,5-T riazine-2,4,6-triyltris((cyclohexylimino)-2, 1 -ethylenediyl) tris(3,3,4,5,5-tetramethylpiperazinone), ~1,6-hexanediamine, N, N'-bis (2, 2,6,6-tetramethyl -4-piperidinyl)-, polymer with 2,4, 6-trichloro-1 ,3, 5-triazine, reaction products with 3-bromo-1 -propene, nbutyl-1-butanamine and N-butyl-2, 2,6,6-tetramethyl-4-piperidinamine, oxidised, hydrogenated, -Alkenes, (C20-24)-4 alpha-, polymers with maleic anhydride, reaction products with 2,2,6,6-tetramethyl-4-piperidinamine, ~N-2,2,6,6-tetramethyl-4-piperidinyl-N-amino-oxamide; 4-acryloyloxy-1 ,2,2,6, 6-pentamethyl-4-piperidine; HALS PB-41 or mixtures thereof.

[0082] One or more light stabilizers can generally be present in the composition in an amount greater than about 0.01 % by weight, such as in an amount greater than about 0.05% by weight, such as in an amount greater than about 0.08% by weight, and generally in an amount less than about 2% by weight, such as in an amount less than about 1% by weight, such as in an amount less than about 0.8% by weight, such as in an amount less than about 0.5% by weight, such as in an amount less than about 0.3% by weight, such as in an amount less than about 0.2% by weight.

[0083] In one embodiment, a coloring agent may optionally be incorporated into the polymer composition. The coloring agent, for instance, can be a black pigment such as carbon black or a black dye. The coloring agent can be present in the polymer composition in an amount greater than about 0.05% by weight, such as in an amount greater than about 0.1% by weight, and in an amount less than about 1.5% by weight, such as in an amount less than about 1 % by weight, such as in an amount less than about 0.9% by weight.

[0084] A shaped part may be formed from the polymer composition using a variety of different techniques. Suitable techniques may include, for instance, injection molding, low-pressure injection molding, extrusion compression molding, gas injection molding, foam injection molding, low-pressure gas injection molding, low-pressure foam injection molding, gas extrusion compression molding, foamAttorney Docket No.: CICT-1567-PCT2 (2024P0075)extrusion compression molding, extrusion molding, foam extrusion molding, compression molding, foam compression molding, gas compression molding, etc. For example, an injection molding system may be employed that includes a mold within which the polymer composition may be injected. The time inside the injector may be controlled and optimized so that polymer matrix is not pre-solidified. When the cycle time is reached and the barrel is full for discharge, a piston may be used to inject the composition to the mold cavity. Compression molding systems may also be employed. As with injection molding, the shaping of the polymer composition into the desired article also occurs within a mold. The composition may be placed into the compression mold using any known technique, such as by being picked up by an automated robot arm. The temperature of the mold may be maintained at or above the solidification temperature of the polymer composition for a desired time period to allow for solidification. The molded product may then be solidified by bringing it to a temperature below that of the melting temperature. The resulting product may be de-molded. The cycle time for each molding process may be adjusted to suit the polymer composition, to achieve sufficient bonding, and to enhance overall process productivity.

[0085] As indicated above, the unique properties of the polymer composition can more readily allow it to be integrally formed with a metal component having a vastly different thermal coefficient of expansion. Thus, if desired, the polymer composition may be employed in a composite structure that contains a metal component that is integrally formed and in contact with a resinous component that includes the polymer composition of the present invention. This may be accomplished using a variety of techniques, such as by an insert molding process in which the polymer composition is molded (e.g., injection molded) onto a portion or the entire surface of the metal component. The metal component may contain any of a variety of different metals, such as aluminum, stainless steel, magnesium, nickel, chromium, copper, titanium, and alloys thereof. Due to its unique properties, the polymer composition can adhere to the metal component by flowing within and / or around surface indentations or pores of the metal component. To improve adhesion, the metal component may optionally be pretreated to increase the degree of surface indentations and surface area. This may be accomplished using mechanical techniques (e.g., sandblasting, grinding, flaring, punching,Attorney Docket No.: CICT-1567-PCT2 (2024P0075)molding, etc.) and / or chemical techniques (e.g., etching, anodic oxidation, etc.). In addition to pretreating the surface, the metal component may also be preheated at a temperature close to, but below the melt temperature of the polymer composition. This may be accomplished using a variety of techniques, such as contact heating, radiant gas heating, infrared heating, convection or forced convection air heating, induction heating, microwave heating or combinations thereof. In any event, the polymer composition is generally injected into a mold that contains the optionally preheated metal component.

[0086] As previously mentioned, the polymer composition, shaped part, and / or composite structure are particularly beneficial for use in components of an electric vehicle. Referring to FIG. 1 , for instance, one embodiment of an electric vehicle 112 that includes a powertrain 110 is shown. The powertrain 110 contains one or more electric machines 114 connected to a transmission 116, which in turn is mechanically connected to a drive shaft 120 and drive wheels 122. Although by no means required, the transmission 116 in this particular embodiment is also connected to an engine 118, though the description herein is equally applicable to a pure electric vehicle. The electric machines 114 may be capable of operating as a motor or a generator to provide propulsion and deceleration capability. The powertrain 110 also includes a propulsion source, such as a battery assembly 124, which stores and provides energy for use by the electric machines 114. The battery assembly 124 typically provides a high voltage current output (e g., DC current at a voltage of from about 400 volts to about 800 volts) from one or more battery cell arrays that may include one or more battery cells.

[0087] The powertrain 110 may also contain at least one power electronics module 126 that is connected to the battery assembly 124 (also commonly referred to as a battery pack) and that may contain a power converter (e.g., converter, etc., as well as combinations thereof). The power electronics module 126 is typically electrically connected to the electric machines 114 and provides the ability to bidirectionally transfer electrical energy between the battery assembly 124 and the electric machines 114. For example, the battery assembly 124 may provide a DC voltage while the electric machines 114 may require a three-phase AC voltage to function. The power electronics module 126 may convert the DC voltage to a three-phase AC voltage as required by the electric machines 114. In aAttorney Docket No.: CICT-1567-PCT2 (2024P0075)regenerative mode, the power electronics module 126 may convert the three-phase AC voltage from the electric machines 114 acting as generators to the DC voltage required by the battery assembly 124. The battery assembly 124 may also provide energy for other vehicle electrical systems. For example, the powertrain may employ a DC / DC converter module 128 that converts the high voltage DC output from the battery assembly 124 to a low voltage DC supply that is compatible with other vehicle loads, such as compressors and electric heaters. In a typical vehicle, the low-voltage systems are electrically connected to an auxiliary battery 130 (e.g., 12V battery). A battery energy control module (BECM) 133 may also be present that is in communication with the battery assembly 124 that acts as a controller for the battery assembly 124 and may include an electronic monitoring system that manages temperature and charge state of each of the battery cells. The battery assembly 124 may also have a temperature sensor 131 , such as a thermistor or other temperature gauge. The temperature sensor 131 may be in communication with the BECM 133 to provide temperature data regarding the battery assembly 124. The temperature sensor 131 may also be located on or near the battery cells within the traction battery 124. It is also contemplated that more than one temperature sensor 131 may be used to monitor temperature of the battery cells.

[0088] In certain embodiments, the battery assembly 124 may be recharged by an external power source 136, such as an electrical outlet. The external power source 136 may be electrically connected to electric vehicle supply equipment (EVSE) that regulates and manages the transfer of electrical energy between the power source 36 and the vehicle 112. The EVSE 138 may have a charge connector 140 for plugging into a charge port 134 of the vehicle 112. The charge port 134 may be any type of port configured to transfer power from the EVSE 138 to the vehicle 112 and may be electrically connected to a charger or on-board power conversion module 132. The power conversion module 132 may condition the power supplied from the EVSE 138 to provide the proper voltage and current levels to the battery assembly 124. The power conversion module 132 may interface with the EVSE 138 to coordinate the delivery of power to the vehicle 112.

[0089] The polymer composition described herein can be included in various components of an electric vehicle as illustrated in FIG. 1. For instance, a busbar,Attorney Docket No.: CICT-1567-PCT2 (2024P0075)one example of which is illustrated in FIG. 2, may be used to electrically connect individual cells of the battery assembly 124. Referring to FIG. 3, for example, the battery assembly 124 can include a number of battery cells 158. The battery cells 158 may be stacked side-by-side to construct a grouping of battery cells, sometimes referred to as a battery array. In one embodiment, the battery cells 158 are prismatic, lithium-ion cells. However, battery cells having other geometries (cylindrical, pouch, etc.) and / or chemistries (nickel-metal hydride, lead-acid, etc.) could alternatively be utilized within the scope of this disclosure. Each battery cell 158 includes a positive terminal (designated by the symbol (+)) and a negative terminal (designed by the symbol (-)). The battery cells 158 are arranged such that each battery cell 158 terminal is disposed adjacent to a terminal of an adjacent battery cell 158 having an opposite polarity. As used herein, the terms “battery”, “cell”, and “battery cell” may be used interchangeably to refer to any type of individual battery element used in a battery system. The batteries described herein typically include lithium-based batteries, but may also include various chemistries and configurations including iron phosphate, metal oxide, lithium-ion polymer, nickel metal hydride, nickel cadmium, nickel-based batteries (hydrogen, zinc, cadmium, etc.), and any other battery type compatible with an electric vehicle. For example, some embodiments may use the 6831 NCR 18650 battery cell from Panasonic®, or some variation on the 18650 form-factor of 6.5 cm x1.8 cm and approximately 45 g.

[0090] The manner in which a busbar connects to individual battery cells of a battery assembly 124, such as shown in FIG. 3, may vary as is known in the art. Referring to FIG. 2, one embodiment of a busbar 10 is shown that includes a conductive body 12. The body 12 includes a conductive material 18, such as copper, aluminum, aluminum alloy, etc., and can generally be in the form of a solid bar, hollow tube, and so forth. The busbar 10 includes a connector portion 14 at either end that is configured to mate with respective terminations of two or more batteries. An insulative portion 16 (e.g., coating or molded material) that includes the polymer composition as described herein may cover a portion of the conductive material of the body 12. To form the busbar 10, the insulative portion 16 can be applied to the surface of the conductive material 18. For instance, a bar or tube of the conductive material 18 can be inserted into a pre-formed tube of theAttorney Docket No.: CICT-1567-PCT2 (2024P0075)insulating coating 16, e.g., an extruded tube sized and cut to the correct proportions, following which the busbar 10 can be shaped to any suitable form. In another embodiment, the insulating coating can be applied to the surface of the conductive material 18 in the melt, and can solidify on the surface of the conductive material in the applied areas.

[0091] Of course, a busbar may be provided in any suitable shape and size. For instance, a busbar may be used as a template for placing the individual battery cells so that they are uniform in each battery assembly manufactured. In such an embodiment, a busbar may hold individual batteries of a battery assembly 124 in place during the manufacturing process and thermal padding or injection-housings, which can be formed of a polymer composition as described herein, can be added without causing the individual battery cells to shift out of position.

[0092] Apart from busbars, other components may also employ the polymer composition of the present disclosure. For example, other components that can include the polymer composition of the present disclosure include current sensors, power electronic components, E-motor busbars, a component in an inverter system, or an electrical connector.

[0093] Referring to FIG. 4, FIG. 5, and FIG. 6, one particular embodiment of a connector 200 is shown for use in an electric vehicle, e.g., in an electric vehicle powertrain. The connector 200 contains a first connector portion 202 and a second connector portion 204. The first connector portion 202 may include one or more electrical pins 206 and the second connector portion 204 may include one or more receptacles 208 for receiving the electrical pins 206. A first insulator member 212 may extend from a base 203 of the first connecting portion 202 to surround the pins 206, and similarly, a second insulator member 218 may extend from a base 201 of the second connecting portion 204 to surround the receptacles 208. In certain cases, the periphery of the first insulator member 212 may extend beyond an end of the electrical pins 203 and the periphery of the second insulator member 218 may extend beyond an end of the receptacles 208. The base 203 and / or the first insulator member 212 of the first connector portion 202, as well as the base 201 and / or the second insulator member 218 of the second connector portion 204, may be formed from the polymer composition of the present invention.

[0094] Although by no means required, the first connector portion 202 may alsoAttorney Docket No.: CICT-1567-PCT2 (2024P0075)include an identification mark 210 secured to or defined by the first protective member 212. The second connecting portion 204 may also optionally define an alignment window 220 sized according to the identification mark 210 to more easily determine when the portions are fully mated. For instance, the identification mark 210 may not be readable unless blockers 221 cover a portion of the identification mark 210. Optionally, the second connecting portion 204 may include a supplemental mark 224 located adjacent to the alignment window 220.

[0095] FIG. 7 and FIG. 8 illustrate yet other examples of components that may employ the polymer composition of the present invention, such as spacers, connectors, insulators and supports as shown in FIG. 7 and that can be formed from the polymer composition. Components as may incorporate a polymer composition illustrated in FIG. 8 include quick connects, tees, and interconnectors, a plurality of which are illustrated at the top of FIG. 8; brushless direct current motors (middle left of FIG. 8), e.g., sealing rings, housings, supports, etc. of a motor; guide rails (middle right of FIG. 8, also illustrating additional examples of busbars in the image); and battery sealing rings (bottom of FIG. 8).

[0096] Systems that can employ the polymer composition of the present invention are in no way limited to only electrical systems. For example, a thermal management system can also beneficially incorporate the polymer composition. A thermal management system of an electric vehicle can generally include multiple different subsystems such as, without limitation, a power train subsystem, a refrigeration subsystem, a battery cooling subsystem, and a heating, ventilation, and cooling (HVAC) subsystem. In some embodiments, one or more subsystems of a thermal management system may in fluid communication with one another, thus allowing hot heat transfer medium to flow from the high temperature circuit into the low temperature circuit, and cooler heat transfer medium to flow from the low temperature circuit into the high temperature circuit.

[0097] One example of a component of a heat management system as may incorporate the polymer composition of the invention is a coolant pump, e.g., an electric water pump, an example of which is illustrated in FIG. 9. As shown, the electric water pump 401 includes an electric motor 410 as a drive source and a hydraulic portion 420 for generating coolant suction and discharge forces. The motor 410 and associated components are retained with in the motor housingAttorney Docket No.: CICT-1567-PCT2 (2024P0075)411. The hydraulic portion 420 includes a volute casing 421 that generally includes a spiral flow space, an inlet 422, and outlet 423, and an impeller (not shown) rotated by the electric motor 410. The pump 401 has an interface including a mechanical seal (not shown), for sealing and separating the water flow space and the motor chamber. Generally, a mounting portion 412 is provided on the motor housing 411 to mount the pump 401 in the vehicle.Components of an electric pump 401 such as housings, casings, interfaces, etc. can incorporate a polymer composition of the invention.

[0098] The present disclosure may be better understood with reference to the following example.Example

[0099] Fiber-reinforced polymer compositions were formulated in accordance with the present disclosure and tested for various properties. In particular, the following compositions were formulated:Sample No. 1 Sample No. 2 Component(wt.%) (wt.%) PA6T / DT resin (polyamide no. 1) 34.80 30.7 PA6I / 6T resin (polyamide no 2) 22.20 9Glass fiber with non-circular cross-section (width30.00 5000 to height ratio is 4:1; average fiber length 3 mm)Aluminum diethylphosphinate 12.00 9.00 Calcium salt of montanic acids (lubricant) 020 0.20 Carbon black masterbatch 080 060 Ultrahigh molecular weight silicone polymer 050100.00 100.00[000100] The above compositions formulated in accordance with the present disclosure were tested for thermal shock resistance. For purposes of comparison, two other commercial formulations were also tested (Sample Nos. 3 and 4). Both commercial formulations contained 30% by weight glass fibers and contained semi-aromatic polyamide polymers. The results are shown in FIG. 14. As shown, the samples made according to the present disclosure displayed a dramatic improvement in thermal shock resistance. None of the competitive samples, for instance, displayed a thermal shock resistance of greater than about 145 cycles,Attorney Docket No.: CICT-1567-PCT2 (2024P0075)wherein the samples of the present disclosure displayed a thermal shock resistance of 288 cycles and 672 cycles respectively.[000101] Sample No. 1 was also tested for comparative tracking index according to Test Method IEC60112. The polymer composition displayed a comparative tracking index of 600 volts.[000102] Sample No. 1 made in accordance with the present disclosure was also tested for dielectric strength at room temperature and at a temperature of 150°C. The test was conducted on samples having a thickness of 1 mm. Sample Nos. 3 and 4 above were also tested. In addition, a commercially available polyamide product was tested that contained polyamide 66 combined with glass fibers in an amount of 25% by weight (Sample No. 5). The results are illustrated in FIG. 15. As shown, Sample No. 1 unexpectedly demonstrated much greater dielectric strength at 150°C in comparison to the other samples.[000103] The glass transition temperature of each sample was also measured. Sample No. 1 had a relatively high glass transition temperature of 132°C. In comparison, Sample No. 3 had a glass transition temperature of 94°C, Sample No.4 had a glass transition temperature of 107°C, and Sample No. 5 had a glass transition temperature of from 60°C to 70°C. The higher glass transition temperature is believed to support the high temperature insulation properties as demonstrated.[000104] These and other modifications and variations of the present invention may be practiced by those of ordinary skill in the art, without departing from the spirit and scope of the present invention. In addition, it should be understood that aspects of the various embodiments may be interchanged both in whole or in part. Furthermore, those of ordinary skill in the art will appreciate that the foregoing description is by way of example only and is not intended to limit the invention so further described in such appended claims.

Claims

1. Attorney Docket No.: CICT-1567-PCT2 (2024P0075)WHAT IS CLAIMED:

1. A polymer composition for molding over metals comprising:a first polyamide polymer, the first polyamide polymer comprising a semiaromatic polyamide polymer having a melting temperature greater than about 280°C and less than about 350°C, the first polyamide polymer being derived from structural units comprising at least one aliphatic diamine and at least one carboxylic acid comprising terephthalic acid;a second polyamide polymer, the second polyamide polymer comprising an amorphous semi-aromatic polyamide polymer having a glass transition temperature of from about 110°C to about 160°C;a flame retardant composition contained within the polymer composition, the flame retardant composition comprising a non-halogen flame retardant;reinforcing fibers dispersed throughout a polymer matrix formed from the first and second polyamide polymers, the reinforcing fibers comprising glass fibers having a non-circular cross-section, the glass fibers being present in the polymer composition in an amount from about 8% by weight to about 58% by weight; and wherein the polymer composition displays:a comparative tracking index of at least 500 V; anda V-0 rating when tested according to Underwriters Laboratories Test 94 according to Vertical Burn Test at a thickness of 1.6 mm.

2. A polymer composition as defined in claim 1 , wherein the polymer composition displays a V-0 rating when tested according to Underwriters Laboratories Test 94 according to Vertical Burn Test at a thickness of 0.4 mm.

3. A polymer composition as defined in claim 1 , wherein the polymer composition displays a comparative tracking index of at least 525 V, such as at least 550 V, such as at least 575 V, such as at least 600 V.

4. A polymer composition as defined in any of the preceding claims, wherein the polymer composition displays a thermal shock resistance of greater than about 200 cycles, such as greater than about 250 cycles, such as greater than about 300 cycles, such as greater than about 400 cycles, such as greater than about 500 cycles, such as greater than about 600 cycles, such as greater than about 650 cycles at a temperature range of from -40°C to 140°C.

5. A polymer composition as defined in any of the preceding claims,Attorney Docket No.: CICT-1567-PCT2 (2024P0075)wherein the first polyamide polymer comprises a polyamide copolymer or a polyamide terpolymer and wherein the at least one aliphatic diamine comprises hexamethylene diamine, 2-methylpentamethylene diamine, or mixtures thereof, and wherein the at least one carboxylic acid comprises terephthalic acid alone or in combination with isophthalic acid and / or adipic acid.

6. A polymer composition as defined in any of the preceding claims, wherein the first polyamide polymer comprises a polyamide copolymer, the polyamide copolymer being formed from a first monomer and a second monomer, the first monomer including structural units derived from hexamethylene diamine and terephthalic acid, the second monomer being derived from structural units comprising 2-methylpentamethylene diamine and terephthalic acid.

7. A polymer composition as defined in any of the preceding claims, wherein the first polyamide polymer is present in the polymer composition in an amount from about 10% by weight to about 55% by weight, such as in an amount from about 13% by weight to about 45% by weight.

8. A polymer composition as defined in any of the preceding claims, wherein the second polyamide polymer is derived from structural units comprising one or more diamines comprising hexamethylene diamine, decamethylene diamine, or mixtures thereof, and from carboxylic acids comprising isophthalic acid and terephthalic acid alone or in combination with adipic acid.

9. A polymer composition as defined in any of the preceding claims, wherein the second polyamide polymer comprises a polyamide copolymer made from first and second monomers, the first monomer being derived from hexamethylene diamine and isophthalic acid, the second monomer being derived from hexamethylene diamine and terephthalic acid, the first monomer being present in the copolymer in an amount greater than the second monomer on a molar basis.

10. A polymer composition as defined in any of the preceding claims, wherein the second polyamide polymer is present in the polymer composition in an amount from about 5% by weight to about 40% by weight.

11. A polymer composition as defined in any of the preceding claims, wherein the glass fibers have a non-circular cross-sectional shape such that a ratio of a width to a height is from about 2: 1 to about 6: 1 , such as from about 3: 1 toAttorney Docket No.: CICT-1567-PCT2 (2024P0075)about 5:1.

12. A polymer composition as defined in any of the preceding claims, wherein the glass fibers have an average fiber length of from about 1 mm to about 5 mm, and wherein the non-circular cross-sectional shape has a width of from about 16 microns to about 45 microns and a height of from about 3 microns to about 9 microns.

13. A polymer composition as defined in any of the preceding claims, wherein the glass fibers are present in the polymer composition in an amount from about 18% by weight to about 55% by weight.

14. A polymer composition as defined in any of the preceding claims, wherein the flame retardant composition comprises a metal phosphinate, such as aluminum diethylphosphinate, and wherein the metal phosphinate is present in the polymer composition in an amount from about 6% by weight to about 18% by weight.

15. A polymer composition as defined in any of the preceding claims, wherein the polymer composition does not contain a nitrogen-containing synergist for the flame retardant.

16. A polymer composition as defined in any of the preceding claims, wherein the polymer composition further contains a lubricant.

17. A polymer composition as defined in claim 16, wherein the lubricant comprises a calcium salt of montanic acids.

18. A polymer composition as defined in any of the preceding claims, wherein the polymer composition further contains a thermal cycling agent comprising an ultrahigh molecular weight silicone comprising a polydimethylsiloxane.

19. A polymer composition as defined in any of the preceding claims, wherein the silicone is added to the polymer composition as a masterbatch comprising the silicone combined with a carrier polymer.

20. A polymer composition as defined in claim 19, wherein the carrier polymer comprises a polyamide.

21. A polymer composition as defined in any of the preceding claims, wherein the polymer composition displays a dielectric strength at 150°C of greaterAttorney Docket No.: CICT-1567-PCT2 (2024P0075)than about 18 kV / mm, such as greater than about 20 kV / mm, such as greater than about 23 kV / mm.

22. A polymer composition as defined in any of the preceding claims, wherein the polymer composition displays a glass transition temperature of greater than about 110°C, such as greater than about 120°C, such as greater than about 130°C, and less than about 160°C.

23. A composite structure comprising a metal component in contact with a resinous component that includes the polymer composition of any of the preceding claims.

24. The composite structure of claim 23, wherein the metal component is over molded with the polymer composition.

25. The composite structure of claim 23, wherein the composite structure comprises a busbar, a current sensor, an inverter filter, an electrical connector, a brushless direct current motor, a guide ring, a battery cell sealing ring, or a combination thereof.

26. The composite structure of claim 23, wherein the composite structure comprises a quick connector, a tee, an interconnector, an electrical connector or a combination thereof.