Aromatic amphiphilic polyelectrolyte complexes and related membrane materials

A composite membrane with cationic and anionic aromatic copolymers forms tighter pores, addressing the challenges of selectivity and fouling resistance, enhancing performance in water treatment and chemical processing.

WO2026241629A1PCT designated stage Publication Date: 2026-11-19TRUSTEES OF TUFTS COLLEGE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/US2026/028352
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-16
Filing Date
2026-05-15
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Existing membrane technologies face challenges in achieving high selectivity, permeability, and fouling resistance simultaneously, particularly in applications such as water treatment and chemical processing.

Method used

A composite membrane is developed comprising a porous support and a selective layer made of a first copolymer with cationic aromatic repeat units and a second copolymer with anionic aromatic repeat units, which self-assemble into structurally confined domains to form tighter pores and enhance selectivity, using copolymers like styrene and vinylbenzyl trimethylammonium chloride and styrenesulfonic acid sodium salt.

Benefits of technology

The composite membrane exhibits improved salt rejections, especially for divalent salts, maintains high selectivity between monosaccharides and disaccharides, and demonstrates excellent pH resistance and fouling resistance, outperforming conventional membranes in water treatment and chemical processing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure US2026028352_19112026_PF_FP_ABST
    Figure US2026028352_19112026_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed are composite membranes comprising a porous support and a selective layer comprising a first copolymer and a second copolymer wherein: the first copolymer comprises a plurality of first hydrophobic repeat units and a plurality of cationic repeat units, wherein the first plurality of hydrophobic repeat units, the plurality of cationic repeat units, or both comprise aromatic or heteroaromatic moieties; and the second copolymer comprises a plurality of second hydrophobic repeat units and a plurality of anionic repeat units, wherein the second plurality of hydrophobic repeat units, the plurality of anionic repeat units, or both comprise aromatic or heteroaromatic moieties. Also disclosed are methods of fabricating and using the composite membranes.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] TUV- 19925

[0002] AEOMATLCAMPHLPHLLLC POLYELECTEOLYTE COMPLEXES AND EELATED MEMBEANE MATERIALS

[0003] RELATED APPLICATION

[0004] This application claims the benefit of priority to U. S. Provisional Application No.

[0005] 63 / 807,142, filed May 16, 2025; the contents of which is incorporated by reference in its entirety.

[0006] BACKGROUND

[0007] Membrane-based separation processes have become increasingly important in various industries, including water treatment, chemical processing, and biotechnology. These processes offer advantages such as energy efficiency, scalability, and the ability to separate components at the molecular level. However, existing membrane technologies often face challenges in achieving high selectivity, permeability, and fouling resistance simultaneously. Accordingly, there is an ongoing, unmet need for new membranes and methods of making said membranes.

[0008] SUMMARY OF THE INVENTION

[0009] In some aspects, the present disclosure provides a composite membrane, comprising: a porous support; and a selective layer comprising a first copolymer and a second copolymer; wherein:

[0010] the first copolymer comprises a plurality of first hydrophobic repeat units and a plurality of cationic repeat units, wherein the plurality of first hydrophobic repeat units and / or the plurality of cationic repeat units comprises aromatic or heteroaromatic moieties; and the second copolymer comprises a plurality of second hydrophobic repeat units and a plurality of anionic repeat units, wherein the plurality of second hydrophobic repeat units and / or the plurality of anionic repeat units comprises aromatic or heteroaromatic moieties.

[0011] In some aspects, the present disclosure provides a method of separating a solute from a solution, comprising contacting the solution with a composite membrane disclosed herein.

[0012] In some aspects, the present disclosure provides a method of fabricating a composite membrane disclosed herein, comprising: applying to a porous support a first copolymer comprising a plurality of first hydrophobic repeat units and a plurality of cationic repeat units, wherein the plurality of first hydrophobic repeat units and / or the plurality of cationic repeat units comprises

[0013] - 1 - FH30004399.6

[0014] TUV- 19925

[0015] aromatic or heteroaromatic moieties; and applying to the porous support a second copolymer comprising a plurality of second hydrophobic repeat units and a plurality of anionic repeat units, wherein the plurality of second hydrophobic repeat units and / or the plurality of anionic repeat units comprises aromatic or heteroaromatic moieties.

[0016] BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1. NMR spectrum of PSA+ chemical structure indicating copolymerization of the two monomer units.

[0018] Figure 2. NMR spectrum of PSS- chemical structure indicating copolymerization of the two monomer units.

[0019] Figure 3. FRP synthesis scheme of the APEs. (Left) styrene as the hydrophobic monomer (black), copolymerized with either TMAC as the cationic monomer (red) or SSAS as the anionic monomer (blue). (Right) Resulting random amphiphilic copolymers after synthesis.

[0020] Figure 4. Formation of self-assembled APEC bilayer TFC membranes, (a) Schematic structure of oppositely charged APEs. (b) Schematic of manufacturing procedure. Here, (1) cationic APE solution is coated first on top of a support membrane. (2) After solvent evaporation, anionic APE solution is coated as the second layer, (c) Hypothesized cross-sectional structure of a self-assembled APEC bilayer TFC membrane, where oppositely charged ionic segments form the hydrophilic domains as effective nanochannels. Hydrophobic domains provide pore walls, confining permeation into the ionic nanopores.

[0021] Figure 5. Cross-sectional SEM images of (a) Uncoated support membrane and (b) A+ single layer, (c) AS bilayer, (d) S- single layer, and (e) SA bilayer on top of the support (10,000x magnification) fabricated using 5 wt% casting solutions of PSA+ and PSS-.

[0022] Figure 6. Cross-sectional SEM images of membranes with different concentration of top-layer casting solutions in two orders of casting (AS and SA) and post-treated AS membranes (AS Heat and AS Salt). (10,000x magnification, except for AS Salt with ll,000x magnification).

[0023] Figure 7. ATR-FTIR spectra of uncoated support membrane (PS35), A+, AS, S-, and SA membranes fabricated with 5 wt% casting solutions of PSA+ and PSS-, along with AS1, AS 0.2, SAI, SA 0.2, AS Salt, and AS Heat membranes fabricated with different top layer casting solution concentrations and post-treatment methods, highlighting characteristic peaks of the copolymers in the regions.

[0024] - 2 - FH30004399.6

[0025] TUV- 19925

[0026] Figure 8. Water permeance for membranes fabricated using 5 wt% casting solutions of PSA+ and PSS-.

[0027] Figure 9. Stabilization of permeance for AS and SA bilayer membranes fabricated using 5 wt% casting solutions of PSA+ and PSS-.

[0028] Figure 10. Water permeance of AS membrane fabricated using 5 wt% casting solutions of PSA+ and PSS- before and after annealing.

[0029] Figure 11. Stabilization of Rb rejection for AS and SA bilayer membranes fabricated using 5 wt% casting solutions of PSA+ and PSS-.

[0030] Figure 12. Rejections of neutral solutes with varying size. VB12, Rb, Sucrose, and Glucose rejections for bilayer (AS and SA) and single layer (A+ and S-) fabricated using 5 wt% casting solutions of PSA+ and PSS-, along with support membrane (PS35) and a commercial NF membrane as a benchmark (NP030, Microdyn Nadir).

[0031] Figure 13. Rejection of neutral solutes vs Stokes diameter for AS and SA bilayer membranes fabricated using 5 wt% casting solutions of PSA+ and PSS-. Solid lines show fits to the Donnan Steric Pore Model to calculate the effective pore diameter.

[0032] Figure 14. Rejection of VB12 and Rb and fitted pore sizes of AS membrane fabricated using 5 wt% casting solutions of PSA+ and PSS- before and after annealing.

[0033] Figure 15. Salt rejections at different concentrations for membranes fabricated using 5 wt% casting solutions of PSA+ and PSS-: Na2SC>4, MgSCb, MgCh. NaCl, along with some monovalent salts rejections for AS membrane.

[0034] Figure 16. Rejection of Na₂SO₄, MgSO₄, MgCl₂, and NaCl salts at different concentrations for AS membrane fabricated using 5 wt% casting solutions of PSA+ and PSS- before and after annealings.

[0035] Figure 17. Stable sugars rejections in the presence of salts and stable salts rejections in the presence of sugars for AS and SA bilayer TFC membranes fabricated using 5 wt% casting solutions of PSA+ and PSS-.

[0036] Figure 18. (a) Glucose / sucrose separation factors and rejections of sucrose and glucose when filtering mixture solutions of 4000 and 10,000 ppm containing 1:1 ratio of sucrose and glucose at applied pressures of 40 and 60 psi for AS bilayer APEC TFC membrane fabricated using 5 wt% casting solutions of PSA+ and PSS-. The x-axis shows the difference between the

[0037] - 3 - FH30004399.6

[0038] TUV- 19925

[0039] applied pressure (AP) and the osmotic pressure of the feed solutions (An) (b) Glucose / Sucrose selectivity of AS membrane compared to those reported in the literature.

[0040] Figure 19. Comparison of the ATR FTIR spectra for AS membrane fabricated using 5 wt% casting solutions of PSA+ and PSS- at different pH solutions showing chemical stability.

[0041] Figure 20. Comparison of the ATR FTIR spectra for SA membrane fabricated using 5 wt% casting solutions of PSA+ and PSS- at different pH solutions showing chemical stability.

[0042] Figure 21. Flux recovery ratios (FRR) for dead-end filtration of (a) oil-in-water emulsion through AS and SA bilayer TFC membranes fabricated using 5 wt% casting solutions of PSA+ and PSS- after 2 days DIW compaction, and commercial NF membranes (NP030), (b) organic mixture through AS, (c) BSA in IX PBS through AS, and (d) lysozyme in IX PBS through AS.

[0043] Figure 22. Contact angle of the fabricated membranes.

[0044] Figure 23. Saccharide content (wt% of total solids) of 42 DE corn syrup in the feed and permeate streams. The permeate stream is enriched in glucose, but maltose, maltotriose, and DP4+ are retained, exhibiting saccharide fractionation by AS bilayer APEC TFC membrane fabricated using 5 wt% casting solutions of PSA+ and PSS-.

[0045] DESCRIPTION OF THE INVENTION

[0046] According to an aspect of the present disclosure, a membrane is provided. The membrane comprises a porous support layer and a selective layer. The selective layer comprises a first copolymer and a second copolymer, as further described herein. The first copolymer has a first charge and the second copolymer has a second charge opposite to the first charge. The first copolymer and the second copolymer may be blended to form the selective layer, or may be present in distinct layers to provide the selective layer as a multilayer (e.g., a bilayer).

[0047] The membranes disclosed herein may include one or more of the following features. The first amphiphilic polyelectrolyte may be a copolymer comprising styrene and vinylbenzyl trimethylammonium chloride monomers. The second amphiphilic poly electrolyte may be a copolymer comprising styrene and styrenesulfonic acid sodium salt monomers. The first layer may be in direct contact with the porous support layer and the second layer may be in direct contact with the first layer. Alternatively, the second layer may be in direct contact with the porous support layer and the first layer may be in direct contact with the second layer. The selective layer may have a thickness of about 0.5 pm to about 2 pm. The membrane may have a water permeance of

[0048] - 4 - FH30004399.6

[0049] TUV- 19925

[0050] about 0.5 L / m2-h-bar to about 10 L / m2-h-bar. The membrane may exhibit a rejection of at least 80% for at least one solute (e.g., sucrose, riboflavin, and / or vitamin B12). The membrane may exhibit a rejection of at least 70% for at least one salt (e.g., Na2SO4 and MgSCb). The membrane may exhibit a rejection of less than 50% for NaCl. The membrane may exhibit an oil fouling resistance characterized by maintaining at least 80% of initial water flux after 14 hours of exposure to a 1500 ppm oil-in-water emulsion.

[0051] In certain embodiments, the membrane may be a thin film composite (TFC) membranes, where a thin “selective layer” is coated onto a porous support. The selective layer comprises a combination of at least two copolymers:

[0052] 1. A first copolymer, also referred to herein as a “cationic aromatic amphiphilic polyelectroyte (APE)”, which is a copolymer comprising at least two types of repeat units: a first hydrophobic repeat unit (e.g., whose homopolymer would be insoluble in water), and a cationic repeat unit which becomes at least partially positively charged when in water, at least one of which includes aromatic or heteroaromatic groups.

[0053] 2. A second copolymer, also referred to herein as an “anionic aromatic APE”, which is a copolymer comprising at least two types of repeat units: a second hydrophobic repeat unit (which may be the same or different as the first hydrophobic repeat unit, and whose homopolymer would be insoluble in water), and an anionic repeat unit which becomes at least partially negatively charged when in water, at least one of which includes aromatic or heteroaromatic groups.

[0054] These two copolymers may be deposited onto the porous support to form a selective layer by various methods including:

[0055] 1. Sequential coating of each copolymer onto the support, creating at least one layer of anionic copolymer and one layer of cationic copolymer on the support. This family of membranes will be termed “bilayer membranes” below, though in principle a higher number of layers is also possible.

[0056] 2. Creating a mixture, or blend, of the two copolymers by dissolving both in the same solvent, then coating this blend onto the support, creating the selective layer. This family of membranes will be termed “blend membranes”.

[0057] In each case, the support membrane’s effective pore size is significantly higher than that of the TFC membrane; the selective layer significantly changes the rejection properties of the support.

[0058] - 5 - FH30004399.6

[0059] TUV- 19925

[0060] In certain embodiments, the membranes disclosed herein exhibit unexpected performance features such as:

[0061] • Tighter pore sizes than non- aromatic APECs of similar charged monomer content, likely associated with tighter chain packing;

[0062] • Higher salt rejections, particularly for divalent salts. Importantly and unlike commercial membranes, these salt rejections do not decrease at higher salinities, providing reliable performance. This is promising for water softening applications;

[0063] • Very high selectivity between monosaccharides and disaccharides; and / or

[0064] • Excellent pH resistance.

[0065] In contrast to non-aromatic amphiphilic poly electrolytes, which tend to form loosely packed, swellable networks with broad pore size distributions, the aromatic copolymers disclosed herein self-assemble into structurally confined domains that yield tighter pores and enhanced selectivity.

[0066] Accordingly, the present disclosure provides a composite membrane, comprising a porous support; and a selective layer comprising a first copolymer and a second copolymer; wherein: the first copolymer comprises a plurality of first hydrophobic repeat units and a plurality of cationic repeat units, wherein the plurality of first hydrophobic repeat units, the plurality of cationic repeat units, or both comprise aromatic or heteroaromatic moieties; and the second copolymer comprises a plurality of second hydrophobic repeat units and a plurality of anionic repeat units, wherein the plurality of second hydrophobic repeat units, the plurality of anionic repeat units, or both comprise aromatic or heteroaromatic moieties.

[0067] As used herein, the term “hydrophobic”, when referring to a repeat unit or monomeric unit, means that the repeat unit has a low affinity for water and tends to preferentially associate with non-aqueous phases rather than dissolve in or interact strongly with water. Hydrophobic repeat units may reduce the overall water affinity of a polymer and may promote phase separation, aggregation, or self-association in aqueous environments. Hydrophobic repeat units typically include non-polar or weakly polar moieties, such as hydrocarbon or aromatic groups, and do not independently impart water solubility to a polymer. A polymer containing hydrophobic repeat units may nonetheless be dispersible or soluble in water due to the presence of hydrophilic or ionic repeat units.

[0068] - 6 - FH30004399.6

[0069] TUV- 19925

[0070] In certain embodiments, the plurality of first hydrophobic repeat units and the plurality of second hydrophobic repeat units each comprise aromatic moieties.

[0071] In certain embodiments, the plurality of first hydrophobic repeat units and the plurality of second hydrophobic repeat units each independently comprises repeat units derived from styrene, a substituted styrene, an aryl acrylate, an aryl methacrylate, or an aryl acrylamide. In certain embodiments, the second plurality of hydrophobic repeat units comprises repeat units derived from styrene, a substituted styrene, an aryl acrylate, an aryl methacrylate, or an aryl acrylamide. In certain embodiments, the plurality of first hydrophobic repeat units and the plurality of second hydrophobic repeat units each comprise repeat units derived from styrene or a substituted derivative thereof.

[0072] In certain embodiments, the plurality of cationic repeat units comprises repeat units derived from acrylate, acrylamide, styrene, or vinyl monomers substituted with amine, pyridinium, imidazolium, phosphonium, or pyrrolidinium. In certain embodiments, the plurality of cationic repeat units comprises repeat units derived from [2-(methacryloyloxy)ethyl] trimethylammonium chloride (MAETA), [3-(methacryloylamino)propyl] trimethylammonium chloride, [2-(acryloyloxy)ethyl] trimethylammonium chloride, (3-acrylamidopropyl)trimethylammonium chloride, 4-vinylbenzyl(triphenyl)phosphonium chloride, (vinylbenzyl)trimethylammonium chloride methacrylate, 3-vinylaniline, 4-vinylaniline, 2-isopropenylaniline, N-(3-aminopropyl)methacrylamide hydrochloride, N-vinylimidazolium, l-allyl-3-vinylimidazoliums, l-allyl-2methyl-5-vinyl-pyridinium, l-allyl-5-vinyl-pyridinium, or 1 -Methyl- 1-(1-vinylcyclohexyl)pyrrolidinium iodide. In certain embodiments, the plurality of cationic repeat units comprises repeat units derived from styrene.

[0073] In certain embodiments, the plurality of cationic repeat units comprises repeat units derived from aryl (meth)acrylate, aryl (meth)acrylamide, styrene, or vinyl aromatic monomers substituted with amine, pyridinium, imidazolium, phosphonium, or pyrrolidinium.

[0074] In certain embodiments, the plurality of cationic repeat units comprises repeat units derived from vinylbenzyl ammonium salts, including vinylbenzyl trimethylammonium chloride, vinylbenzyl trimethylammonium bromide, vinylbenzyl trimethylammonium iodide, vinylbenzyl triethylammonium chloride, vinylbenzyl triethylammonium bromide, vinylbenzyl tributylammonium chloride, vinylbenzyl tributylammonium bromide, vinylbenzyl dimethylethylammonium chloride, vinylbenzyl diethylmethylammonium chloride, vinylbenzyl

[0075] - 7 - FH30004399.6

[0076] TUV- 19925

[0077] pyridinium chloride, vinylbenzyl dimethylethylammonium bromide, vinylbenzyl diethylmethylammonium bromide, or vinylbenzyl pyridinium bromide. In certain embodiments, the plurality of cationic repeat units comprises repeat units derived from amino- substituted styrenes, including 2-vinylaniline, 3-vinylaniline, 4-vinylaniline, N-methyl-4-vinylaniline, N, N-dimethyl-4-vinylaniline, or N, N-diethyl-4-vinylaniline. In certain embodiments, the plurality of cationic repeat units comprises repeat units derived from heteroaryl-substituted styrenes, including vinylbenzyl imidazolium salts. In certain embodiments, the plurality of cationic repeat units comprises repeat units derived from vinylbenzyl phosphonium salts, including vinylbenzyl(triphenyl)phosphonium chloride or vinylbenzyl(tributyl)phosphonium chloride. In certain embodiments, the plurality of cationic repeat units comprises repeat units derived from vinylbenzyl trimethylammonium chloride. In certain embodiments, the plurality of cationic repeat units can comprise repeat units derived from a heteroaromatic monomer such as 2-vinylpyridine, 3-vinylpyridine, 4-vinylpyridine, and the like.

[0078] In certain embodiments, the plurality of anionic repeat units comprises repeat units derived from (meth)acrylate, (meth)acrylamide, styrene, or vinyl monomers substituted with an anionic group selected from carboxylate, sulfonate, sulfonic acid, phosphonate, phosphonic acid, phosphate, or phosphate ester groups. In certain embodiments, the plurality of anionic repeat units comprises repeat units derived from aryl (meth)acrylate, aryl (meth)acrylamide, styrene, or vinyl aromatic monomers substituted with an anionic group selected from carboxylate, sulfonate, sulfonic acid, phosphonate, phosphonic acid, phosphate, or phosphate ester groups.

[0079] In certain embodiments, the plurality of anionic repeat units comprises repeat units derived from styrenic monomers bearing anionic substituents, including styrenesulfonic acid, styrenesulfonic acid salts, styrene phosphonic acid derivatives, styrene carboxylic acid derivatives, or styrenic monomers comprising a spacer linking the styrene moiety and the anionic group. In certain embodiments, the plurality of anionic repeat units comprises repeat units derived from styrenesulfonic acid or salts thereof, including styrenesulfonic acid sodium salt, styrenesulfonic acid potassium salt, or styrenesulfonic acid in protonated form. In certain embodiments, the plurality of anionic repeat units comprises repeat units derived from styrene phosphonic or phosphonate derivatives, including (4-ethenylphenyl)methylphosphonic acid, styrene phosphonic acid, styrene phosphonate salts, or styrenic monomers comprising a phosphonic acid or phosphonate group separated from the styrene ring by an alkylene or oxyalkylene spacer. In certain

[0080] - 8 - FH30004399.6

[0081] TUV- 19925

[0082] embodiments, the plurality of anionic repeat units comprises repeat units derived from styrene carboxylic acid derivatives, including 2-vinylbenzoic acid, 3-vinylbenzoic acid, 4-vinylbenzoic acid, or 4-(2-propenyl)benzoic acid. In certain embodiments, the plurality of anionic repeat units comprises repeat units derived from methacrylic acid (MAA), acrylic acid, 2-carboxyethyl acrylate, mono-2-(methacryloyloxy)ethyl succinate, mono-2-(methacryloyloxy)ethyl maleate, 2-sulfoethyl methacrylate (SEMA), 2-acrylamido-2-methylpropane sulfonic acid, 2-acrylamido-2-methyl-l -propanesulfonic acid, 2-acrylamido-2-methyl-l -propanesulfonic acid sodium salt, 3-sulfopropyl acrylate potassium salt, 3-sulfopropyl methacrylate potassium salt, vinylsulfonic acid sodium salt, or 2-methyl-2-propene-l -sulfonic acid sodium salt.

[0083] In certain embodiments, the plurality of anionic repeat units comprises repeat units derived from amino-acid-based acrylamides or methacrylamides, including L- or

[0084] D-tryptophan-methacrylamide, L- or D-tryptophan-acrylamide, L- or D-alanine-methacrylamide,

[0085] L- or D-alanine-acrylamide, L- or D-valine-methacrylamide, L- or D-valine-acrylamide, L- or

[0086] D-isoleucine-methacrylamide, L- or D-isoleucine-acrylamide, L- or

[0087] D-allo-isoleucine-methacrylamide, L- or D-allo-isoleucine-acrylamide, L- or

[0088] D-methionine-methacrylamide, L- or D-methionine-acrylamide, L- or

[0089] D-phenylalanine-methacrylamide, L- or D-phenylalanine-acrylamide, L- or

[0090] D-tyrosine-methacrylamide, L- or D-tyrosine-acrylamide, L- or D-histidine-methacrylamide, L- or

[0091] D-histidine-acrylamide, L- or D-glutamic acid-methacrylamide, L- or D-glutamic acid-acrylamide, L- or D-aspartic acid-methacrylamide, or L- or D-aspartic acid-acrylamide.

[0092] In certain embodiments, the plurality of anionic repeat units comprises repeat units derived from styrene substituted with an anionic group selected from carboxylate, sulfonate, sulfonic acid, phosphonate, phosphonic acid, phosphate, or phosphate ester groups. In certain embodiments, the plurality of anionic repeat units comprises repeat units derived from styrenesulfonic acid sodium salt.

[0093] In certain embodiments, the first copolymer and the second copolymer may be statistical copolymers. In certain embodiments, the first copolymer and the second copolymer may be random copolymers. For example, the first copolymer can be a statistical copolymer comprising repeat units derived from styrene and vinylbenzyl trimethylammonium chloride; and the second copolymer comprising repeat units derived from styrene and styrenesulfonic acid sodium salt. In certain embodiments, the first copolymer is a statistical copolymer of styrene and vinylbenzyl

[0094] - 9 - FH30004399.6

[0095] TUV- 19925

[0096] trimethylammonium chloride; and the second copolymer is a statistical copolymer of styrene and styrenesulfonic acid sodium salt.

[0097] In certain embodiments, the composite membrane is a thin film composite membrane. For example, the thin film composure membrane can have a thickness of about 20 pm to about 1,000 pm, for example 50 pm to 200 pm.

[0098] In certain embodiments, the first copolymer and the second copolymer are essentially insoluble in water (e.g., under operating conditions). As used herein, the term “essentially insoluble in water” refers to a material that does not dissolve in water to a significant extent under operating or ambient conditions and instead remains predominantly in a separate, undissolved phase. A material that is essentially insoluble in water may swell, disperse, or form a heterogeneous suspension in water but does not form a true molecular solution. For example, a material that is essentially insoluble in water may have a solubility in water of less than about 1 g / L, less than about 0.5 g / L, or less than about 0.1 g / L at 20-25 °C.

[0099] In certain embodiments, the first copolymer comprises about 5 to 60 mol% of the plurality of cationic repeat units, based on total moles of the first copolymer. In certain embodiments, the first copolymer comprises about 20 to 60 mol% of the plurality of cationic repeat units. In certain embodiments, the first copolymer comprises about 5 to 50 mol%, or 20 to 50 mol%, or 5 to 40 mol%, or 5 to 30 mol%, or 5 to 20 mol% of the plurality of cationic repeat units. In certain embodiments, the first copolymer comprises about 5 to 60 wt% of the plurality of cationic repeat units. In certain embodiments, the first copolymer comprises about 20 to 60 wt% of the plurality of cationic repeat units. In certain embodiments, the first copolymer comprises about 5 to 50 wt%, or 20 to 50 wt%, or 5 to 40 wt%, or 5 to 30 wt%, or 5 to 20 wt% of the plurality of cationic repeat units.

[0100] In certain embodiments, the second copolymer comprises about 5 to 60 mol% of the plurality of anionic repeat units, based on total moles of the second copolymer. In certain embodiments, the second copolymer comprises about 20 to 60 mol% of the plurality of anionic repeat units. In certain embodiments, the second copolymer comprises about 5 to 50 mol%, or 20 to 50 mol%, or 5 to 40 mol%, or 5 to 30 mol%, or 5 to 20 mol% of the plurality of anionic repeat units. In certain embodiments, the second copolymer comprises about 5 to 60 wt% of the plurality of anionic repeat units. In certain embodiments, the second copolymer comprises about 20 to 60 wt% of the plurality of anionic repeat units. In certain embodiments, the second copolymer

[0101] - 10 - FH30004399.6

[0102] TUV- 19925

[0103] comprises about 5 to 50 wt%, or 20 to 50 wt%, or 5 to 40 wt%, or 5 to 30 wt%, or 5 to 20 wt% of the plurality of anionic repeat units.

[0104] In certain embodiments, the first copolymer has an average molar mass of at least 20,000 g / mol, or at least 30,000 g / mol. In certain embodiments, the first copolymer has an average molar mass of at least 50,000 g / mol. In certain embodiments, the first copolymer has an average molar mass of at least 100,000 g / mol. In certain embodiments, the first copolymer has an average molar mass of up to 3,000,000 g / mol, or up to 2,000,000 g / mol, or up to 1,500,000 g / mol, or up to 1,000,000 g / mol, or up to 500,000 g / mol. In certain embodiments, the first copolymer can have a molar mass of 20,000 g / mol to about 3,000,000 g / mol, or 30,000 g / mol to about 3,000,000 g / mol, or 50,000 g / mol to about 3,000,000 g / mol, or 20,000 to 1,500,000 g / mol, or 30,000 to 1,500,000 g / mol, or 50,000 to 1,500,000 g / mol, or 100,000 to 1,500,000 g / mol. In certain embodiments, the first copolymer has an average molar mass of 100,000 g / mol to about 500,000 g / mol.

[0105] In certain embodiments, the second copolymer has an average molar mass of at least 20,000 g / mol, or at least 30,000 g / mol. In certain embodiments, the second copolymer has an average molar mass of at least 50,000 g / mol. In certain embodiments, the second copolymer has an average molar mass of at least 100,000 g / mol. In certain embodiments, the second copolymer has an average molar mass of up to 3,000,000 g / mol, or up to 2,000,000 g / mol, or up to 1,500,000 g / mol, or up to 1,000,000 g / mol, or up to 500,000 g / mol. In certain embodiments, the second copolymer can have a molar mass of 20,000 g / mol to about 3,000,000 g / mol, or 30,000 g / mol to about 3,000,000 g / mol, or 50,000 g / mol to about 3,000,000 g / mol, or 20,000 to 1,500,000 g / mol, or 30,000 to 1,500,000 g / mol, or 50,000 to 1,500,000 g / mol, or 100,000 to 1,500,000 g / mol. In certain embodiments, the second copolymer has an average molar mass of 100,000 g / mol to about 500,000 g / mol.

[0106] Molar mass (e.g., molecular weight) as used herein for the first copolymer and the second copolymer refers to the number average molecular weight (Mn) of the copolymers. Number average molecular weight can be determined by, for example, by determining copolymer composition using gel permeation chromatography (GPC) and calculating an average molar mass.

[0107] In certain embodiments, the first copolymer and the second copolymer comprise predominantly aromatic repeat units, such that the amount of non-aromatic repeat units in the copolymers is minimized. In certain embodiments, the first copolymer and the second copolymer exclude non-aromatic repeat units, and do not comprise repeat units derived from aliphatic or

[0108] - 11 - FH30004399.6

[0109] TUV- 19925

[0110] non-aromatic monomers. In certain embodiments, at least a portion of the anionic repeat units and the cationic repeat units comprise aromatic or heteroaromatic moieties. In certain embodiments, at least about 50 mol% of the anionic repeat units or cationic repeat units comprise aromatic moieties. In certain embodiments, at least about 60 mol%, at least about 70 mol%, or at least about 80 mol% of the anionic repeat units or cationic repeat units comprise aromatic moieties. In certain embodiments, the aromatic moieties are phenyl or substituted phenyl groups derived from styrenic monomers. In certain embodiments, less than about 20 mol%, or less than 10 mol%, or less than 5 mol%, or less than 1 mol% of the anionic repeat units or cationic repeat units are non-aromatic. As used herein, mole percentage refers to the molar fraction of the noted repeat units in the copolymer backbone.

[0111] In certain embodiments, the selective layer can comprise the first copolymer and the second copolymer sequentially layered on the porous support (e.g., the first copolymer and the second copolymer have been applied to the porous support layer sequentially), thereby forming a bilayer membrane. In certain embodiments, the first copolymer is in direct contact with the porous support and the second copolymer is layered on the first copolymer. In other embodiments, the second copolymer is in direct contact with the porous support and the first copolymer is layered on the second copolymer. In other embodiments, the selective layer comprising first copolymer and the second copolymer blended or intermingled on the porous support to provide a blended layer (e.g., the first copolymer and the second copolymer form a homogenous layer on the porous support). As used herein, the term “intermingled” means that the first copolymer and the second copolymer are present in overlapping spatial regions within the blended layer, without requiring chemical bonding between the copolymers. Intermingled copolymers may be physically mixed, co-distributed, or interpenetrated within the blended layer.

[0112] In certain embodiments, the selective layer has a thickness of about 30 nm to about 10 pm. In certain embodiments, the selective layer can have a thickness of at least 50 nm, or at least 75 nm, or at least 100 nm, or at least 150 nm, or at least 200 nm, or at least 250 nm, or at least 300 nm, or at least 350 nm, or at least 400 nm, or at least 450 nm, or at least 500 nm, or at least 550 nm, or at least 600 nm. In certain embodiments, the selective layer has a thickness of about 0.1 pm to about 8 pm, or 0.1 to 5 pm, or 0.1 to 2 pm.

[0113] - 12 - FH30004399.6

[0114] TUV- 19925

[0115] In certain embodiments, the composite membrane has a water permeance of about 0.5 L / m2-h-bar to about 30 L / m2-h-bar, for example 1 L / m2-h-bar to about 30 L / m2-h-bar, or 5 L / m2-h-bar to about 30 L / m2-h-bar.

[0116] In certain embodiments, the selective layer exhibits a rejection of at least 80% for at least one neutral solute selected from sucrose, riboflavin, and vitamin B12. In certain embodiments, the selective layer exhibits a rejection of at least 70% for at least one divalent salt selected from Na2SO4and MgSCh. In certain embodiments, the selective layer exhibits a rejection of less than 50% for NaCl. In certain embodiments, the selective layer exhibits different rejections for monosaccharides and disaccharides. In certain embodiments, the selective layer exhibits a D-glucose / sucrose separation factor of greater than 10, or greater than 15, or greater than 18.

[0117] In certain embodiments, the selective layer has an effective pore size of about 0.5 nm to about 2 nm. In certain embodiments, the effective pore size of the composite membrane is less than the effective pore size of a membrane prepared by coating only the first copolymer or only the second copolymer on the same porous support. As used herein, the term “effective pore size” refers to a characteristic pore dimension of a membrane that governs the transport and rejection of solutes during filtration, taking into account the membrane’s internal pore structure, pore shape, and interactions between the solute and the membrane. The effective pore size represents an apparent pore size inferred from separation performance, rather than a direct physical measurement of individual pore diameters. The effective pore size may be estimated using solute rejection data, molecular weight cut-off measurements, or transport models, and does not require direct imaging or physical measurement of individual pores.

[0118] In certain embodiments, the selective layer exhibits oil fouling resistance characterized by maintaining at least 80% of initial water flux after exposure to a 1500 ppm oil-in-water emulsion for at least 14 hours. In certain embodiments, the selective layer exhibits pH stability over a range of pH 2 to pH 12. As used herein, “stability”, when referring to a membrane over a specified pH range, means that the membrane retains its structural integrity upon exposure to aqueous environments within that pH range and does not undergo dissolution, disintegration, or catastrophic mechanical failure. For example, a stable membrane does not undergo substantial chemical degradation of the polymer layers or pendant functional groups sufficient to compromise membrane integrity when exposed to aqueous solutions having a pH from 2 to 12.

[0119] - 13 - FH30004399.6

[0120] TUV- 19925

[0121] In certain embodiments, the selective layer exhibits size-based selectivity between uncharged organic molecules. In certain embodiments, the selective layer exhibits salt rejections for divalent salts that do not substantially decrease at higher salinities.

[0122] In certain embodiments, the porous support comprises a polymeric membrane suitable for pressure-driven water treatment processes, including ultrafiltration, nanofiltration, or reverse osmosis. In certain embodiments, the porous support comprises a polymeric ultrafiltration membrane formed from materials including, but not limited to, polysulfone (PS), polyethersulfone (PES), polyvinylidene fluoride (PVDF), polyacrylonitrile (PAN), cellulose acetate, cellulose triacetate, polyamide, polypropylene, polyethylene, polyether ether ketone (PEEK), or combinations thereof. In certain embodiments, the porous support comprises a polymeric nanofiltration or reverse osmosis support layer, including support layers used in thin-film composite membranes. In certain embodiments, the porous support is an ultrafiltration membrane. In certain embodiments, the porous support is a polysulfone ultrafiltration membrane.

[0123] In some aspects, the present disclosure provides methods of separating a solute from a feed solution. The method comprises contacting the feed solution with a composite membrane as disclosed herein. In certain embodiments, the feed solution is passed (e.g., filtered) through the composite membrane to provide a first stream having a lower concentration of the solute relative to the feed solution. In certain embodiments, the solute is a salt, a sugar, a protein, a dye, a vitamin, or an oil. In certain embodiments, the method is used for water softening, water treatment, reverse osmosis pretreatment, or food wastewater treatment.

[0124] In some aspects, the present disclosure provides methods of fabricating the composite membrane disclosed herein, comprising: applying to a porous support a first copolymer comprising a plurality of first hydrophobic repeat units and a plurality of cationic repeat units, wherein the plurality of first hydrophobic repeat units and / or the plurality of cationic repeat units comprises aromatic or heteroaromatic moieties; and applying to the porous support a second copolymer comprising a plurality of second hydrophobic repeat units and a plurality of anionic repeat units, wherein the plurality of second hydrophobic repeat units and / or the plurality of anionic repeat units comprises aromatic or heteroaromatic moieties, thereby fabricating the composite membrane.

[0125] In certain embodiments, the first copolymer and the second copolymer are applied to the porous support sequentially, thereby forming a bilayer membrane. In certain embodiments, the first copolymer is applied first, and the second copolymer is applied second. In certain

[0126] - 14 - FH30004399.6

[0127] TUV- 19925

[0128] embodiments, the second copolymer is applied first, and the first copolymer is applied second. In other embodiments, the first copolymer and the second copolymer are applied to the porous support as a blend (e.g., the first copolymer and second copolymer are mixed before application), thereby forming a blend membrane.

[0129] In certain embodiments, the first copolymer and the second copolymer can each independently be dissolved in a suitable organic solvent prior to application. Exemplary solvents can include polar organic solvents such as Ci-6 alkyl alcohols (e.g., methanol, ethanol, and the like). In certain embodiments, the applying step comprises coating each copolymer solution onto the porous support. Any suitable coating technique can be used, for example including, but not limited to, film rod application, blade coating, slot-die coating, knife-over-roll coating, gravure coating, reverse-roll coating, spray coating, dip coating, or other continuous or semi-continuous coating processes suitable for laboratory-scale preparation or large-scale membrane manufacturing. In certain embodiments, the method further comprises removing solvent from the selective layer after deposition. In some aspects, the method can include a solvent evaporation period between sequential coating steps.

[0130] Definitions

[0131] Unless otherwise defined herein, scientific and technical terms used in this application shall have the meanings that are commonly understood by those of ordinary skill in the art. Chemistry terms used herein, unless otherwise defined herein, are used according to conventional usage in the art, as exemplified by “The McGraw-Hill Dictionary of Chemical Terms”, Parker S., Ed., McGraw-Hill, San Francisco, C. A. (1985).

[0132] All ranges disclosed herein are inclusive of the endpoints, and the endpoints are independently combinable with each other. “Combinations” is inclusive of blends, mixtures, alloys, reaction products, and the like. The terms “first,” “second,” and the like, do not denote any order, quantity, or importance, but rather are used to distinguish one element from another. The terms “a” and “an” and “the” do not denote a limitation of quantity, and are to be construed to cover both the singular and the plural, unless otherwise indicated herein or clearly contradicted by context. “Or” means “and / or” unless clearly stated otherwise. As used herein, the term “about,” when used to modify a numerical value, means within ±10%, or within ±5% of the stated value, unless a different tolerance is apparent from the context or would be understood by a person of ordinary skill in the art based on measurement uncertainty or experimental variability. In all cases,

[0133] - 15 - FH30004399.6

[0134] TUV- 19925

[0135] variations encompassed by the term “about” are those that do not materially affect the structure or performance of the described embodiment.

[0136] All of the above, and any other publications, patents and published patent applications referred to in this application are specifically incorporated by reference herein. In case of conflict, the present specification, including its specific definitions, will control.

[0137] As used herein, the terms “optional” or “optionally” mean that the subsequently described event or circumstance may occur or may not occur, and that the description includes instances where the event or circumstance occurs as well as instances in which it does not. For example, “optionally substituted alkyl” refers to the alkyl may be substituted as well as where the alkyl is not substituted.

[0138] It is understood that substituents and substitution patterns on the compounds of the present invention can be selected by one of ordinary skilled person in the art to result chemically stable compounds which can be readily synthesized by techniques known in the art, as well as those methods set forth below, from readily available starting materials. If a substituent is itself substituted with more than one group, it is understood that these multiple groups may be on the same carbon or on different carbons, so long as a stable structure results.

[0139] As used herein, the term “optionally substituted” refers to the replacement of one to six hydrogen radicals in a given structure with the radical of a specified substituent including, but not limited to: hydroxyl, hydroxyalkyl, alkoxy, halogen, alkyl, nitro, silyl, acyl, acyloxy, aryl, cycloalkyl, heterocyclyl, amino, aminoalkyl, cyano, haloalkyl, haloalkoxy, -C(O)-CH2-O-alkyl, -OP(O)(O-alkyl)2 or -CH2-OP(O)(O-alkyl)2. Preferably, “optionally substituted” refers to the replacement of one to four hydrogen radicals in a given structure with the substituents mentioned above. More preferably, one to three hydrogen radicals are replaced by the substituents as mentioned above. It is understood that the substituent can be further substituted.

[0140] As used herein, the term “alkyl” refers to saturated aliphatic groups, including but not limited to C1-C10 straight-chain alkyl groups or C1-C10 branched-chain alkyl groups. Preferably, the “alkyl” group refers to Ci-Ce straight-chain alkyl groups or Ci-Ce branched-chain alkyl groups. Most preferably, the “alkyl” group refers to C1-C4 straight-chain alkyl groups or C1-C4 branched-chain alkyl groups. Examples of “alkyl” include, but are not limited to, methyl, ethyl, 1-propyl, 2-propyl, n-butyl, sec-butyl, tert-butyl, 1-pentyl, 2-pentyl, 3-pentyl, neo-pentyl, 1-hexyl, 2-hexyl, 3-hexyl, 1-heptyl, 2-heptyl, 3-heptyl, 4-heptyl, 1-octyl, 2-octyl, 3-octyl or 4-octyl and the like.

[0141] - 16 - FH30004399.6

[0142] TUV- 19925

[0143] Moreover, the term “alkyl” as used throughout the specification, examples, and claims is intended to include both unsubstituted and substituted alkyl groups, the latter of which refers to alkyl moieties having substituents replacing a hydrogen on one or more carbons of the hydrocarbon backbone, including haloalkyl groups such as trifluoromethyl and 2,2,2-trifluoroethyl, etc.

[0144] As used herein, the term “alkylene” refers to a bivalent saturated aliphatic groups, including but not limited to C1-C10 straight-chain alkyl groups or C1-C10 branched-chain alkylene groups. Preferably, the “alkylene” group refers to Ci-Ce straight-chain alkylene groups or Ci-Ce branched-chain alkyl groups. Most preferably, the “alkylene” group refers to C1-C4 straight-chain alkyl groups or C1-C4 branched-chain alkylene groups. Examples of “alkylene” include, but are not limited to, methylene, ethylene, 1 -propylene, 2-propylene, n-butylene, sec -butylene, tert-butylene, 1 -pentylene, 2-pentylene, 3-pentylene, neo-pentylene, 1 -hexylene, 2-hexylene, 3-hexylene, 1-heptylene, 2-heptylene, 3-heptylene, 4-heptylene, 1 -octylene, 2-octylene, 3-octylene or 4-octylene and the like. The “alkylene” group may be optionally substituted.

[0145] The term “acyl” is art-recognized and refers to a group represented by the general formula hydrocarbylC(O)-, preferably alkylC(O)-.

[0146] The term “acylamino” is art-recognized and refers to an amino group substituted with an acyl group and may be represented, for example, by the formula hydrocarbylC(O)NH-.

[0147] The term “acyloxy” is art-recognized and refers to a group represented by the general formula hydrocarbylC(O)O-, preferably alkylC(O)O-.

[0148] The term “alkoxy” refers to an alkyl group having an oxygen attached thereto. Representative alkoxy groups include methoxy, ethoxy, propoxy, tert-butoxy and the like.

[0149] The term “alkoxyalkyl” refers to an alkyl group substituted with an alkoxy group and may be represented by the general formula alkyl-O- alkyl.

[0150] The term “Cx.y” or “Cx-Cy”, when used in conjunction with a chemical moiety, such as, acyl, acyloxy, alkyl, alkenyl, alkynyl, or alkoxy is meant to include groups that contain from x to y carbons in the chain. Coalkyl indicates a hydrogen where the group is in a terminal position, a bond if internal. A Ci-ealkyl group, for example, contains from one to six carbon atoms in the chain.

[0151] The term “alkylamino”, as used herein, refers to an amino group substituted with at least one alkyl group.

[0152] - 17 - FH30004399.6

[0153] TUV- 19925

[0154] The term “alkylthio”, as used herein, refers to a thiol group substituted with an alkyl group and may be represented by the general formula alkylS-.

[0155] The term “amido”, as used herein, refers to a group

[0156]

[0157] wherein R9and R10each independently represent a hydrogen or hydrocarbyl group, or R9and R10taken together with the N atom to which they are attached complete a heterocycle having from 4 to 8 atoms in the ring structure.

[0158] The terms “amine” and “amino” are art-recognized and refer to both unsubstituted and substituted amines and salts thereof, e.g., a moiety that can be represented by

[0159]

[0160] wherein R9, R10, and R10’ each independently represent a hydrogen or a hydrocarbyl group, or R9and R10taken together with the N atom to which they are attached complete a heterocycle having from 4 to 8 atoms in the ring structure.

[0161] The term “aminoalkyl”, as used herein, refers to an alkyl group substituted with an amino group.

[0162] The term “aralkyl”, as used herein, refers to an alkyl group substituted with an aryl group.

[0163] The term “aryl” as used herein include substituted or unsubstituted single-ring aromatic groups in which each atom of the ring is carbon. Preferably the ring is a 5- to 7-membered ring, more preferably a 6-membered ring. The term “aryl” also includes polycyclic ring systems having two or more cyclic rings in which two or more carbons are common to two adjoining rings wherein at least one of the rings is aromatic, e.g., the other cyclic rings can be cycloalkyls, cycloalkenyls, cycloalkynyls, aryls, heteroaryls, and / or heterocyclyls. Aryl groups include benzene, naphthalene, phenanthrene, phenol, aniline, and the like.

[0164] The term “carbamate” is art-recognized and refers to a group

[0165]

[0166] wherein R9and R10independently represent hydrogen or a hydrocarbyl group.

[0167] - 18 - FH30004399.6

[0168] TUV- 19925

[0169] The term “carbocyclylalkyl”, as used herein, refers to an alkyl group substituted with a carbocycle group.

[0170] The term “carbocycle” includes 5-7 membered monocyclic and 8-12 membered bicyclic rings. Each ring of a bicyclic carbocycle may be selected from saturated, unsaturated and aromatic rings. Carbocycle includes bicyclic molecules in which one, two or three or more atoms are shared between the two rings. The term “fused carbocycle” refers to a bicyclic carbocycle in which each of the rings shares two adjacent atoms with the other ring. Each ring of a fused carbocycle may be selected from saturated, unsaturated and aromatic rings. In an exemplary embodiment, an aromatic ring, e.g., phenyl, may be fused to a saturated or unsaturated ring, e.g., cyclohexane, cyclopentane, or cyclohexene. Any combination of saturated, unsaturated and aromatic bicyclic rings, as valence permits, is included in the definition of carbocyclic. Exemplary “carbocycles” include cyclopentane, cyclohexane, bicyclo[2.2.1]heptane, 1,5-cyclooctadiene, 1,2,3,4-tetrahydronaphthalene, bicyclo[4.2.0]oct-3-ene, naphthalene and adamantane. Exemplary fused carbocycles include decalin, naphthalene, 1,2,3,4-tetrahydronaphthalene, bicyclo[4.2.0]octane, 4,5,6,7-tetrahydro-lH-indene and bicyclo[4.1.0]hept-3-ene. “Carbocycles” may be substituted at any one or more positions capable of bearing a hydrogen atom.

[0171] The term “carbocyclylalkyl”, as used herein, refers to an alkyl group substituted with a carbocycle group.

[0172] The term “carbonate” is art-recognized and refers to a group -OCO2-.

[0173] The term “carboxy”, as used herein, refers to a group represented by the formula -CO2H.

[0174] The term “cycloalkyl” includes substituted or unsubstituted non-aromatic single ring structures, preferably 4- to 8-membered rings, more preferably 4- to 6-membered rings. The term “cycloalkyl” also includes polycyclic ring systems having two or more cyclic rings in which two or more carbons are common to two adjoining rings wherein at least one of the rings is cycloalkyl and the substituent (e.g., R100) is attached to the cycloalkyl ring, e.g., the other cyclic rings can be cycloalkyls, cycloalkenyls, cycloalkynyls, aryls, heteroaryls, and / or heterocyclyls. Heteroaryl groups include, for example, pyrrole, furan, thiophene, imidazole, oxazole, thiazole, pyrazole, pyridine, pyrazine, pyridazine, pyrimidine, denzodioxane, tetrahydroquinoline, and the like.

[0175] The term “ester”, as used herein, refers to a group -C(O)OR9wherein R9represents a hydrocarbyl group.

[0176] - 19 - FH30004399.6

[0177] TUV- 19925

[0178] The term “ether”, as used herein, refers to a hydrocarbyl group linked through an oxygen to another hydrocarbyl group. Accordingly, an ether substituent of a hydrocarbyl group may be hydrocarbyl-O-. Ethers may be either symmetrical or unsymmetricaL Examples of ethers include, but are not limited to, heterocycle-O-heterocycle and aryl-O-heterocycle. Ethers include “alkoxyalkyl” groups, which may be represented by the general formula alkyl-O-alkyl.

[0179] The terms “halo” and “halogen” as used herein means halogen and includes chloro, fluoro, bromo, and iodo.

[0180] The terms “hetaralkyl” and “heteroaralkyl”, as used herein, refers to an alkyl group substituted with a hetaryl group.

[0181] The terms “heteroaryl” and “hetaryl” include substituted or unsubstituted aromatic single ring structures, preferably 5- to 7-membered rings, more preferably 5- to 6-membered rings, whose ring structures include at least one heteroatom, preferably one to four heteroatoms, more preferably one or two heteroatoms. The terms “heteroaryl” and “hetaryl” also include polycyclic ring systems having two or more cyclic rings in which two or more carbons are common to two adjoining rings wherein at least one of the rings is heteroaromatic, e.g., the other cyclic rings can be cycloalkyls, cycloalkenyls, cycloalkynyls, aryls, heteroaryls, and / or heterocyclyls. Heteroaryl groups include, for example, pyrrole, furan, thiophene, imidazole, oxazole, thiazole, pyrazole, pyridine, pyrazine, pyridazine, and pyrimidine, and the like.

[0182] The term “heteroatom” as used herein means an atom of any element other than carbon or hydrogen. Preferred heteroatoms are nitrogen, oxygen, and sulfur.

[0183] The term “heterocyclylalkyl”, as used herein, refers to an alkyl group substituted with a heterocycle group.

[0184] The terms “heterocyclyl”, “heterocycle”, and “heterocyclic” refer to substituted or unsubstituted non-aromatic ring structures, preferably 3- to 10-membered rings, more preferably 3- to 7-membered rings, whose ring structures include at least one heteroatom, preferably one to four heteroatoms, more preferably one or two heteroatoms. The terms “heterocyclyl” and “heterocyclic” also include polycyclic ring systems having two or more cyclic rings in which two or more carbons are common to two adjoining rings wherein at least one of the rings is heterocyclic, e.g., the other cyclic rings can be cycloalkyls, cycloalkenyls, cycloalkynyls, aryls, heteroaryls, and / or heterocyclyls. Heterocyclyl groups include, for example, piperidine, piperazine, pyrrolidine, morpholine, lactones, lactams, and the like.

[0185] - 20 - FH30004399.6

[0186] TUV- 19925

[0187] The term “hydrocarbyl”, as used herein, refers to a group that is bonded through a carbon atom that does not have a =O or =S substituent, and typically has at least one carbon-hydrogen bond and a primarily carbon backbone, but may optionally include heteroatoms. Thus, groups like methyl, ethoxyethyl, 2-pyridyl, and even trifluoromethyl are considered to be hydrocarbyl for the purposes of this application, but substituents such as acetyl (which has a =O substituent on the linking carbon) and ethoxy (which is linked through oxygen, not carbon) are not. Hydrocarbyl groups include, but are not limited to aryl, heteroaryl, carbocycle, heterocycle, alkyl, alkenyl, alkynyl, and combinations thereof.

[0188] The term “hydroxyalkyl”, as used herein, refers to an alkyl group substituted with a hydroxy group.

[0189] The term “lower” when used in conjunction with a chemical moiety, such as, acyl, acyloxy, alkyl, alkenyl, alkynyl, or alkoxy is meant to include groups where there are ten or fewer atoms in the substituent, preferably six or fewer. A “lower alkyl”, for example, refers to an alkyl group that contains ten or fewer carbon atoms, preferably six or fewer. In certain embodiments, acyl, acyloxy, alkyl, alkenyl, alkynyl, or alkoxy substituents defined herein are respectively lower acyl, lower acyloxy, lower alkyl, lower alkenyl, lower alkynyl, or lower alkoxy, whether they appear alone or in combination with other substituents, such as in the recitations hydroxyalkyl and aralkyl (in which case, for example, the atoms within the aryl group are not counted when counting the carbon atoms in the alkyl substituent).

[0190] The terms “polycyclyl”, “polycycle”, and “polycyclic” refer to two or more rings (e.g., cycloalkyls, cycloalkenyls, cycloalkynyls, aryls, heteroaryls, and / or heterocyclyls) in which two or more atoms are common to two adjoining rings, e.g., the rings are “fused rings”. Each of the rings of the polycycle can be substituted or unsubstituted. In certain embodiments, each ring of the poly cycle contains from 3 to 10 atoms in the ring, preferably from 5 to 7.

[0191] The term “sulfate” is art-recognized and refers to the group -OSO3H, or a pharmaceutically acceptable salt thereof.

[0192] The term “sulfonamide” is art-recognized and refers to the group represented by the general formulae

[0193]

[0194] - 21 - FH30004399.6

[0195] TUV- 19925

[0196] wherein R9and R10independently represents hydrogen or hydrocarbyl.

[0197] The term “sulfoxide” is art-recognized and refers to the group-S(O)-.

[0198] The term “sulfonate” is art-recognized and refers to the group SO3H, or a pharmaceutically acceptable salt thereof.

[0199] The term “sulfone” is art-recognized and refers to the group -S(O)2-.

[0200] The term “substituted” refers to moieties having substituents replacing a hydrogen on one or more carbons of the backbone. It will be understood that “substitution” or “substituted with” includes the implicit proviso that such substitution is in accordance with permitted valence of the substituted atom and the substituent, and that the substitution results in a stable compound, e.g., which does not spontaneously undergo transformation such as by rearrangement, cyclization, elimination, etc. As used herein, the term “substituted” is contemplated to include all permissible substituents of organic compounds. In a broad aspect, the permissible substituents include acyclic and cyclic, branched and unbranched, carbocyclic and heterocyclic, aromatic and non-aromatic substituents of organic compounds. The permissible substituents can be one or more and the same or different for appropriate organic compounds. For purposes of this invention, the heteroatoms such as nitrogen may have hydrogen substituents and / or any permissible substituents of organic compounds described herein which satisfy the valences of the heteroatoms. Substituents can include any substituents described herein, for example, a halogen, a hydroxyl, a carbonyl (such as a carboxyl, an alkoxycarbonyl, a formyl, or an acyl), a thiocarbonyl (such as a thioester, a thioacetate, or a thioformate), an alkoxyl, a phosphoryl, a phosphate, a phosphonate, a phosphinate, an amino, an amido, an amidine, an imine, a cyano, a nitro, an azido, a sulfhydryl, an alkylthio, a sulfate, a sulfonate, a sulfamoyl, a sulfonamide, a sulfonyl, a heterocyclyl, an aralkyl, or an aromatic or heteroaromatic moiety. It will be understood by those skilled in the art that the moieties substituted on the hydrocarbon chain can themselves be substituted, if appropriate.

[0201] The term “thioalkyl”, as used herein, refers to an alkyl group substituted with a thiol group.

[0202] The term “thioester”, as used herein, refers to a group -C(O)SR9or -SC(O)R9wherein R9represents a hydrocarbyl.

[0203] The term “thioether”, as used herein, is equivalent to an ether, wherein the oxygen is replaced with a sulfur.

[0204] The term “urea” is art-recognized and may be represented by the general formula

[0205] - 22 - FH30004399.6

[0206] TUV- 19925

[0207] o

[0208] c£ 11 pi o

[0209] N^N'R

[0210] R9R9?

[0211] wherein R9and R10independently represent hydrogen or a hydrocarbyl.

[0212] Many of the compounds useful in the methods and compositions of this disclosure have at least one stereogenic center in their structure. This stereogenic center may be present in a R or a S configuration, said R and S notation is used in correspondence with the rules described in Pure Appl. Chem. (1976), 45, 11-30. The disclosure contemplates all stereoisomeric forms such as enantiomeric and diastereoisomeric forms of the compounds, salts, prodrugs or mixtures thereof (including all possible mixtures of stereoisomers). See, e.g., WO 01 / 062726.

[0213] Furthermore, certain compounds which contain alkenyl groups may exist as Z (zusammen) or E (entgegen) isomers. In each instance, the disclosure includes both mixture and separate individual isomers.

[0214] EXAMPLES

[0215] The invention now being generally described, it will be more readily understood by reference to the following examples which are included merely for purposes of illustration of certain aspects and embodiments of the present invention and are not intended to limit the invention.

[0216] Example 1: Synthesis of Poly (styrene)-random- poly (Vinylbenzyl trimethyl ammonium chloride) (PSA+) and Poly (styrene) -random- poly (Styrenesulfonic acid sodium salt) (PSS-) used as an Amphiphilic Polyelectrolyte Complex (APEC) bilayer

[0217] Synthesis of PSA+ (P(TMAC-r-Styrene)). Synthesis has been done by Free Radical Polymerization (FRP). For a 60:40 monomer ratio, styrene (6.00 g, 57.61 mmol) and vinylbenzyl trimethyl ammonium chloride (TMAC, 4.00 g, 18.89 mmol) were dissolved in dimethyl sulfoxide (DMSO) (40 mL). Azobisisobutyronitrile (AIBN) (0.01 g), the thermal initiator, was added. The flask was sealed, and nitrogen was bubbled through the reaction mixture for 20 min to purge dissolved oxygen. It was then placed in an oil bath at 65°C with stirring at 300 rpm for 21 hours. The flask was removed from the oil bath and unsealed, and 0.2 g of 4-methoxyphenol (MEHQ) was added to terminate the reaction. The reaction mixture was then precipitated in acetone (500 ml) and purified by stirring three more fresh portions of acetone for at least 3 hours. Then three

[0218] - 23 - FH30004399.6

[0219] TUV- 19925

[0220] fresh portions of 5:95 deionized water (DIW) to acetone volume ratio for at least 5 hours were used to wash the copolymer. Finally, the copolymer was dried in the vacuum oven for 48 hours at 60°C. The composition of the copolymer was calculated from the 'H-NMR spectrum (Figure 1), using the ratio of protons from the two different monomer units. The calculated composition was 49.2 wt% Styrene and 50.8 wt% TMAC. The final yield of this reaction was -55%.

[0221] Synthesis of PSS- (P(Styrene-r-SSAS)). PSS- was synthesized via FRP. For a 60:40 monomer ratio, 4- Styrenesulfonic acid sodium salt (SSAS, 4.00g, 19.4 mmol), and Styrene (6.00 g, 57.61 mmol) were dissolved in DMSO (40 mL). AIBN (0.01g) was added to the flask. The flask was sealed, and nitrogen was bubbled through the reaction mixture for 20 minutes to purge any dissolved oxygen. The flask was then placed in an oil bath set to 65° C, while stirring at 300 rpm for 21 hours. The flask was removed from the oil bath and unsealed, and 0.2 g of MEHQ was added to terminate the reaction. The reaction mixture was then precipitated in acetonitrile and purified by stirring three more fresh portions of acetonitrile for at least 3 hours. Then three fresh portions of DIW for at least 5 hours were used to wash the copolymer. Finally, the copolymer was dried in the vacuum oven for 48h at 60 °C. The composition of the copolymer was calculated from the 'H-NMR spectrum (Figure 2), using the ratio of protons from the two different monomer units. The calculated composition was 61.7 wt% Styrene and 38.3 wt% SSAS. The final conversion of this reaction was -25%.

[0222] Moreover, PSA+ and PSS- were synthesized using the same procedures described above but this time with 70:30 monomers ratio by just changing the amounts of styrene monomer and charged monomers dissolved in DMSO (7 gr styrene and 3 gr TMAC or SSAS) to study the hydrophobic content effects. The conversions for these reactions for PSA+ and PSS- with higher hydrophobic content were -47% and -5%, respectively. For PSA+, the calculated composition from the ’H-NMR spectrum was 59 wt% Styrene and 41 wt% TMAC (Figure 1). For PSS-, the calculated composition from the ’H-NMR spectrum was 84 wt% Styrene and 16 wt% SSAS (Figure 2).

[0223] Example 2: Membrane preparation of Poly (styrene)-random- poly (Vinylbenzyl trimethyl ammonium chloride) (PSA+) and Poly (styrene)-random- poly (Styrenesulfonic acid sodium salt) (PSS-) used as an Amphiphilic Polyelectrolyte Complex (APEC) bilayer

[0224] - 24 - FH30004399.6

[0225] TUV- 19925

[0226] After both syntheses in Example 1, thin film composite (TFC) membranes were fabricated using both PSA+ and PSS- copolymers (with 60:40 hydrophobic: charged monomers ratio). Each copolymer (0.25 g) was dissolved separately in methanol (4.75 g) to get 5 wt% casting solutions at approximately 25° C. Both copolymer solutions were passed through 0.45 micrometer syringe filters (Whatman) and degassed in a vacuum oven for at least 1 hour. The membranes were prepared by coating consecutive thin layers of each copolymer solution one at a time on top of each other as a bilayer coating on top of a commercial porous ultrafiltration (UF) membrane support using a film applicator rod (Figure 4). In between coatings, we adopted a 30-minute solvent evaporation period at room temperature. PS35 (PSf) UF membrane was used as the support membrane which was purchased from Solecta (Oceanside, Calif.). Membranes with the “AS” configuration were prepared by first coating a layer of PSA+ on a support, followed by a layer of PSS-. For “SA” configuration, we reversed the order of coatings and PSS- was coated first. We also made membranes with only one layer as controls, S- and A+ (Table 1). After coatings and 30-minute drying time, the membranes were immersed in a DIW bath at room temperature and stored until use.

[0227] Table 1. Fabricated TFC membranes with 5 wt% casting solutions of PSA+ and PSS-.

[0228]

[0229] PSf N.-'A N / A N / A N / A

[0230] To fabricate membranes with different top layer concentrations, separate casting solutions containing 5, 1, and 0.2 wt.% of each APEs (with 60:40 hydrophobic: charged monomers ratio) in

[0231] - 25 - FH30004399.6

[0232] TUV- 19925

[0233] methanol were prepared. APEC bilayer TFC membranes in both AS and SA order of casting were fabricated by first coating a layer of one APE 5 wt% casting solution onto the support and allowing it to dry at room temperature for 30 minutes, followed by coating a second layer of the other oppositely charged APE solution on top with the desired concentration of 1 or 0.2 wt% using the same casting procedure described earlier (Table 2).

[0234] Table 2. Fabricated TFC membranes with different top layer concentration.

[0235]

[0236] AS 0.2 A+ 5 S- 0.2

[0237] AS 1 Af 5 S- 1

[0238] SA 0.2 S- 5 A+ 0.2

[0239] SA 1 S- 5 A4- 1

[0240] To study the effects of post-treatment on membrane properties, salt annealing was performed by immersing the AS bilayer TFC membrane fabricated with 5 wt% PSS- on top of a 5 wt% PSA+ casting solutions (using APEs with 60:40 hydrophobic: charged monomer weight ratio) in a 1 M NaCl aqueous solution for 24 hours, followed by rinsing with DI water prior to testing. Heat annealing was conducted by placing the membrane in DI water and keeping it at 45 °C in an oven for 24 hours (Table 3).

[0241] Table 3. Fabricated TFC membrane with different post treatment methods.

[0242]

[0243] AS Beat A* $ $* S

[0244] AS Salt A* 5 S- $

[0245] We investigated the selective layers cross-sectional morphology and thickness using scanning electron microscopy (SEM) to image the freeze-fractured cross-sections of the membranes. In Figure 5, SEM images of the fabricated membranes using 5 wt% casting solutions of PSA+ and PSS- (described above) could be seen. The bilayers can be observed with a total

[0246] - 26 - FH30004399.6

[0247] TUV- 19925

[0248] thickness of about 1 micrometer. In Figure 6, SEM images of the fabricated membranes with different top layer casting solution concentrations and post-treatment methods (described above) could be seen.

[0249] The presence and chemistry of coated layers on TFC membranes and their chemical properties were characterized by Attenuated total reflectance fourier transform infrared (ATR-FTIR) spectroscopy using an FT / IR-6200 spectrophotometer (JASCO Corp) equipped with a ZnSe crystal. Before analysis, the membranes were allowed to air dry for 10 minutes and then dried in a vacuum oven at room temperature for 24 hours. Each spectrum was averaged across 32 scans in the in the range of 4000-600 cm-1with a resolution of 4 cm-1.

[0250] The peaks at the wavenumbers of -950-960 cm1, -1040 cm1, -700 cm1, and -1400-1600 cm'1are attributed to C-N+stretching from quaternary ammonium (PSA+), S=O stretching from the sulfonate group (PSS-), aromatic C-H out-of-plane bending of styrene backbone, and styrene aromatic C=C stretching, respectively, characteristic peaks we anticipated for APE copolymers (Figure 7). The SEM and ATR- FTIR results show successful coatings on the support membrane.

[0251] Example 3: Water permeance of Poly (styrene)-random- poly (Vinylbenzyl trimethyl ammonium chloride) (PSA+) and Poly (styrene)-random- poly (Styrenesulfonic acid sodium salt) (PSS-) used as an Amphiphilic Polyelectrolyte Complex (APEC) bilayer

[0252] In this example, the pure water permeances through the membranes fabricated using 5 wt% casting solutions of PSA+ and PSS- described in Example 2 were measured. PS35 support membrane and a commercial nanofiltration membrane of a relatively similar pore size, NP030, have permeances of 430 ± 43 L / m2.h.bar and 0.97 ± 0.05 L / m2.h.bar, respectively. Membranes performance was characterized using dead-end stirred cell experiments with 10 mL Amicon 8010 (Millipore) cells with 4.1 cm2filtration area. A 40 psi transmembrane pressure was applied, and cells were stirred at 500 rpm. Two separate membrane disks were tested for each membrane. The water flux (J, L.m^.h1), which is the volume of water passing through the membrane per experiment time normalized by the membrane area, was measured by recording the mass of the permeate collected in a container on a scale connected to a computer. The membrane permeance (Lp, L.m^.h bbar1), defined as the flux normalized by applied transmembrane pressure (AP, bar), was calculated as Lp= J / AP (Figure 8). To monitor the equilibration of the membranes described in Example 2, DIW permeance was monitored (Figure 9) which stabilized after 2-3 days, including

[0253] - 27 - FH30004399.6

[0254] TUV- 19925

[0255] over several weeks of additional testing. When just placed in DIW, stabilization takes ~3 months. This change may arise from the slow molecular rearrangement of the aromatic moieties in APEC layers to reach a more tightly packed equilibrium state. Some of the change may also be due to the gaps sealing between the layers and between the coating and the support under pressure. So, for all calculations, after a stabilization period of at least 2 days, a sample of the permeate was collected over 60 minute and weighed. These membranes have permeances comparable to nanofiltration and ultrafiltration commercial membranes.

[0256] Measuring water permeance for the post-treated AS bilayer TFC membranes was done similar to the procedure described earlier. Results for annealing process on AS membrane with 5 wt% S- on top of a 5 wt% A+ show that it affects membrane stabilization and performance. Heat annealing promoted structural equilibration and compaction of the selective layer, resulting in performance comparable to what achieved after ~2 days of pressurization. This effect appears to be irreversible. In contrast, salt annealing had minimal effect on membrane performance, with DI water permeance remaining essentially unchanged, indicating that salt exposure does not significantly affect pore structure (Figure 10).

[0257] Example 4: Neutral solute rejections of of Poly (styrene)-random- poly (Vinylbenzyl trimethyl ammonium chloride) (PSA+) and Poly (styrene) -random- poly (Styrenesulfonic acid sodium salt) (PSS-) used as an Amphiphilic Polyelectrolyte Complex (APEC) bilaver

[0258] In this example, the membranes prepared using 5 wt% casting solutions of PSA+ and PSS-as described in Example 2 were used in experiments aimed at identifying their effective pore size or size cut-off. We used colored vitamins / dyes and sugars to probe this property. The rejection experiments were performed using an Amicon 8010 stirred, dead-end filtration cell (Millipore) with 10 mF cell volume and 4.1 cm2effective filtration area. The cell was stirred at 500 rpm to minimize concentration polarization effects, and the test was performed at 40 psi. Two separate membrane disks were tested for each membrane. Rejection (R, %) of a given solute is defined as R% = 100 * fl —Cp«rmeatewhere Creed and Cpenneate are the feed and permeate concentrations (-Feed

[0259] (mM), respectively. The rejection performance equilibration of the membranes was monitored by running DIW through the membrane for at least 2 days, similar to what was mentioned in Example 3, and measuring the rejection of a neutral solute, Rb over time (Figure 11) which stabilized after 2-3 days, including over several weeks of additional testing. So, for all calculations after a

[0260] - 28 - FH30004399.6

[0261] TUV- 19925

[0262] stabilization period of at least 2 days, to avoid pure water contamination after filtering solutes of interest, the first milliliter of filtrate was discarded, and the next 1 milliliter was utilized to measure rejection (Figures 12). Sucrose, glucose, and glycerol rejections were measured using 4000 ppm solutions; their concentrations were quantified by COD kits (K-7365, CHEMetrics). Glycerol rejection was tested only for AS and SA membranes and the results were 22.8% and 20%, respectively. Rejections of colored vitamins / dyes, riboflavin (Rb) and vitamin B 12 (VB12), were measured using 0.1 mM feed concentrations and quantified by UV-visible spectroscopy (GenesyslO, ThermoScientific). The cell was rinsed several times with water and DIW was filtered through the membrane until the permeate was completely clear before switching to a new solute. The bilayer membranes have the pore size of ~1 nm (Figure 13).

[0263] Results for annealing process on AS bilayer TFC membranes with 5 wt% PSS- on top of a 5 wt% PSA+ show that it affects membrane stabilization and separation performance. Heat annealing promoted structural equilibration and compaction of the selective layer, resulting in performance comparable to what achieved after ~2 days of pressurization. This effect appears to be irreversible. In contrast, salt annealing had minimal effect on membrane performance, with uncharged solute rejection remaining essentially unchanged, indicating that salt exposure does not significantly affect pore structure (Figure 14). Furthermore, subsequent pressurization of salt-annealed membranes resulted in comparable pore size and performance to non-annealed membranes after pressurization, demonstrating that salt annealing does not prevent compaction. Overall, these findings indicate that heat annealing is an effective technique for accelerating membrane stabilization, whereas salt annealing primarily preserves membrane integrity while not significantly altering structure or performance.

[0264] Example 5: Salt rejections of Poly (styrene)-random- poly (Vinylbenzyl trimethyl ammonium chloride) (PSA+) and Poly (styrene)-random- poly (Styrenesulfonic acid sodium salt) (PSS-) used as an Amphiphilic Polyelectrolyte Complex (APEC) bilayer

[0265] In this example, the membranes prepared using 5 wt% casting solutions of PSA+ and PSS-as described in Example 2 were used in experiments to understand separation capabilities and mechanisms and characterize the membranes salt rejection properties. Two concentrations of salts (Na2SO4, MgSO4, MgCh. NaCl, KC1, NaF, EiCl, Nal, and NaCICb) were filtered: 1 mM and 10 mM. Permeate concentrations were measured by a standard conductivity meter probe. The

[0266] - 29 - FH30004399.6

[0267] TUV- 19925

[0268] rejection tests were performed using dead-end stirred cell experiments with 10 mL Amicon 8010 (Millipore) cells with 4.1 cm2filtration area. A 40 psi transmembrane pressure was applied, and cells were stirred at 500 rpm to minimize concentration polarization effects. Two separate membrane disks were tested for each membrane. These salt rejection tests were done after stabilization process mentioned in Example 3 and Example 4. When filtering the salts solutions, after discarding the first 1 mL to avoid pure water contamination, enough volume was collected for analysis by the conductivity probe and the salt rejection (%) was calculated (Figure 15, a-e). The cell was rinsed several times with water and DIW was filtered through the membrane before switching to a new salt solution.

[0269] The findings also imply that annealing affects surface charge and ion transport behavior of AS membrane made with 5 wt% PSS- on top of a 5 wt% PSA+ by changing polymer chain arrangement and charged groups distribution at the interface (Figure 16). The salt rejection data demonstrate that heat annealing and pressurization lead to similar results and promote copolymer intermixing and lower charge heterogeneity. Salt annealing on its own shows limited effect on charge redistribution or pore structure, as evidenced by the minimal change in salt rejection. In symmetric salts (e.g., MgSCb and NaCl), annealing-induced densification and reduced pore size have a greater impact on transport behavior. In asymmetric salts (e.g., MgCL and Na2SC>4), electrostatic effects are more pronounced.

[0270] Example 6: Sugars and salts multicomponent mixture separation of Poly (styrene)-random-poly (Vinylbenzyl trimethyl ammonium chloride) (PSA+) and Poly (styrene)-random- poly (Styrenesulfonic acid sodium salt) (PSS-) used as an Amphiphilic Polyelectrolyte Complex (APEC) bilayer

[0271] In this example, AS and SA bilayer TFC membranes prepared using 5 wt% casting solutions of PSA+ and PSS- as described in Example 2 were used in experiments to explore the membranes multicomponent rejection properties. Novel membrane characterization typically involves single-solute solution filtration; however, rejection can vary with feed composition due to solute-membrane and solute-solute interactions. For example, in PA TFC membranes, the amount of salt in feed causes the barrier layer to change in swelling and pore sizes to enlarge, leading to decreased organics rejections. Also, there are applications where a solution as the wastewater with high organics load including sugars, needs to be treated and an extra salty retentate

[0272] - 30 - FH30004399.6

[0273] TUV- 19925

[0274] is not desired, so it is aimed to reject as high organics as possible, while passing salts like NaCl through. Prescence of salts do not harm the environment, but organics cause imbalance in natural reactions. Also, in such applications it is aimed to not waste energy for separating salts and maybe reuse the retentate which is concentrated sugar. Here, we examined how the presence of salt affects the neutral organic solutes rejections and vice versa in bilayer membranes. Membrane performance was characterized using dead-end stirred cell experiments with 10 mL Amicon 8010 (Millipore) cells with 4.1 cm2filtration area. A 40 psi transmembrane pressure was applied, and cells were stirred at 500 rpm. Two separate membrane disks were tested for each membrane. These rejection tests were done after stabilization process mentioned in Example 3 and Example 4. When filtering the solutions, after discarding the first 1 mL to avoid pure water contamination, enough volume was collected for measurements by a standard conductivity meter probe and COD kits (K-7365, CHEMetrics), and the salt and sugar rejections (%) were calculated (Figure 17). The cell was rinsed several times with DIW and DIW was filtered through the membrane before switching to a new solution. Through filtering 4000 ppm binary mixtures of sucrose or glucose with NaCl or MgSO4 at 1 mM or 10 mM, results showed no significant change in rejections compared to single solute solutions (Figure 17). This indicates that AS and SA membranes maintain stable and predictable performance when filtering multicomponent mixtures. The high DIW permeance and organics removal (sugars, especially glucose) of membranes, and their relatively high divalent ions rejection while not very high NaCl rejection, make them useful in applications such as water softening, RO pre-treatment, and food wastewater treatment where ion and small organic content separations are highly relevant, decreasing the required pressure (energy consumption) for running such processes.

[0275] Table 4. shows data for the rejection of sugars in presence of salts.

[0276] - 31 - FH30004399.6

[0277] TUV- 19925

[0278]

[0279] DIW 96.4* 0.2 77,1 * i.5 97,3*0.6 - 74.5*3.7

[0280] NaCl l mM 97.4 > 0.3 80*. < -.4 97.1*0.6 71.6*6.6 aCUO M %.7*0.3 0.1017 71.5* 1.4 04561 96.1*0.6 0.1561 69,7*2.8 0-3679

[0281] MgSO mM 94.7*0.4 724* 1.7 95.5* 1.3 73.5*3.2

[0282] MgSChlftmM 91.8*0.5 0.1561 63.7*2.5 0.1561 94.1*0.8 04561 68*3,2 0.1801

[0283] *Kruskal-Waliis test showed that there were so statistically significoBt differences in between the different study groups (rejection of sugars with diSerenl sails solutions and with DIW solutions).

[0284] Example 7: Sugars multicomponent mixture separation of Poly (styrene)-random- poly (Vinylbenzyl trimethyl ammonium chloride) (PSA+) and Poly (styrene)-random- poly (Styrenesulfonic acid sodium salt) (PSS-) used as an Amphiphilic Polyelectrolyte Complex (APEC) bilaver

[0285] In this example, the AS membrane prepared using 5 wt% casting solutions of PSA+ and PSS- as described in Example 2 was used in the experiment to further explore the membrane’s multicomponent rejection properties. Membrane performance was characterized using dead-end stirred cell experiments with 10 mL Amicon 8010 (Millipore) cells with 4.1 cm2filtration area. Two separate membrane disks were tested for membrane and cells were stirred at 500 rpm. This rejection test was done after stabilization process mentioned in Example 3 and Example 4. When filtering the solution, after discarding the first 1 mL to avoid pure water contamination, enough volume was collected for measurements. After the test, the cell was rinsed several times with DIW and DIW was filtered through the membrane for washing purposes.

[0286] An important feature of the APEC bilayer membranes is their exceptional size-based selectivity for uncharged organic solutes, especially mono- and di-saccharides, attributed to tight pores and a narrow pore size distribution resulting from the self-assembled structure formed when two oppositely charged APEs meet at the layers interface. The effects of filtration applied pressure and total solution concentration on the separation of sugars, particularly sucrose and glucose were examined here. Two feed model mixtures with sugar concentrations of 4000 ppm and 10,000 ppm in a 1: 1 mass ratio of sucrose and glucose in DIW were used and the concentrations were analyzed

[0287] - 32 - FH30004399.6

[0288] TUV- 19925

[0289] using High-Performance Liquid Chromatography (HPLC). An Agilent 1260 Infinity binary pump HPLC (Agilent Technologies, Palo Alto, CA) was used equipped with an Agilent 7.7 x 300 mm Hi-Plex Na column and an Agilent 1260 Infinity refractive index detector (RID). Isocratic 100% HPLC-grade water (Sigma Aldrich) at a flow rate of 0.2 mL.min-1was used as the mobile phase and each injection was 60 minutes long. The auto sampler was set to an injection volume of 10 pl and column was kept at 80 °C using an Agilent 1260 Infinity thermostatted column compartment. The 4000 ppm solution was tested at 40 psi and 60 psi pressures to assess pressure impact, whereas the 10,000 ppm solution was tested only at 60 psi as it requires higher operating pressure (AP) to overcome the osmotic pressure effects (An). The glucose separation factor (SF) was calculated to evaluate glucose purification from sucrose, indicating that a SF deviating from unity signifies successful separation. It shows how the composition of the permeate changed in comparison to the initial glucose to sucrose ratio in the feed:

[0290] Separation Factor

[0291]

[0292] where Cg,pand CS,Pare the concentrations of glucose and sucrose in permeate (ppm), respectively. Cg,f and Cs,f are the concentrations of glucose and sucrose in the feed (ppm), respectively. Rgis the rejection of glucose and Rsis the rejection of sucrose.

[0293] AS bilayer membrane showcased high sugars rejections at high flux for a mixture of sucrose and glucose at 4000 ppm and 60 psi, achieving a separation factor exceeding 18, indicative of uniform pore size that contribute to the very precise sharp cutoff (Figure 18 a). The permeate is practically just glucose and our membrane could separate sucrose and glucose almost completely. Since AS and SA exhibited similar rejection behaviors, only AS was tested for saccharide selectivity studies, and we believe that findings apply to both membranes with different casting orders. The separation factor of the membrane filtering mixture of sugars increased which compared to when single sugars were filtered which is associated with the pores confinement. When only one molecule can fit in the pores, this phenomenon happens which agrees with the previous studies.

[0294] NF membranes have shown promise for membrane-based sugar separations for complex streams as a feasible technology. A significant challenge for large-scale effective sugar purification

[0295] - 33 - FH30004399.6

[0296] TUV- 19925

[0297] is the trade-off between separation factor and flux in current commercial membranes. The AS bilayer TFC membrane notably outperforms other NF membranes by achieving higher water permeation and separation factor, effectively separating monosaccharides while retaining disaccharides (Figure 18b). High-purity sugar fractions, particularly monosaccharide-rich permeates like glucose, are valuable for applications where purifying sugars selectively is desirable such as fermentation, bioprocessing, pharmaceutical applications, food industry, dairy, conversion of agricultural feedstocks into bio-based sweeteners and biofuel, and biochemicals manufacturing uses. This highlights our membrane potential in enhancing resource efficiency and product purity as a sustainable intensification technique for upgrading purposes and biorefinery processes.

[0298] As illustrated in Figure 18 a, the effective driving force, defined by the difference between applied operating pressure and osmotic pressure of the feed solutions shown in x-axis, influences rejections. When filtering a 4000 ppm feed solution, with an increase in pressure (AP-An) or permeate flux, sucrose rejection increased from approximately 98% at 40 psi to 99% at 60 psi, while glucose rejection increased from about 82% to 84%. The glucose / sucrose separation factor also increased from around 13 to over 18. However, at a higher feed concentration of 10,000 ppm and 60 psi, sucrose and glucose rejections observed to be 97% and 83%, respectively. The results are consistent with previous studies noting on increased rejections as pressure increased or reduced rejections with increased feed concentration.

[0299] Example 8: pH stability of Poly (styrene) -random- poly (Vinylbenzyl trimethyl ammonium chloride) (PSA+) and Poly (styrene) -random- poly (Styrenesulfonic acid sodium salt) (PSS-) used as an Amphiphilic Polyelectrolyte Complex (APEC) bilayer

[0300] Attenuated total reflectance Fourier transform infrared (ATR-FTIR) spectroscopy was done using an FT / IR-6200 spectrophotometer (JASCO Corp) equipped with a ZnSe crystal. ATR-FTIR spectra (4000-600 cm-1, 4 cm-1resolution, 32 scans) were collected for the dried APEC membranes fabricated using 5 wt% casting solutions of PSA+ and PSS- in Example 2 and PS35 support membrane. Afterwards, we put membranes in aqueous solutions at different pHs of 2, 4, 7, 10, and 12 for the period of one week and then after drying them overnight, performed the ATR-FTIR spectroscopy again to compare membranes chemical properties before and after exposure to different pHs. In Figure 19 and Figure 20, the peaks at the wavenumbers of -950-960 cm1, -1040 cm1, -700 cm1, and -1400-1600 cm'1are attributed to C-N+stretching from quaternary

[0301] - 34 - FH30004399.6

[0302] TUV- 19925

[0303] ammonium (PSA+), S=O stretching from the sulfonate group (PSS-), aromatic C-H out-of-plane bending of styrene backbone, and styrene aromatic C=C stretching, respectively. Accordingly, characteristic peaks remained unchanged and both AS and SA membrane showed excellent stability when exposing to this wide range of highly acidic to highly basic pHs over one week. They exhibit constant intensities, no new peaks, no loss of the existing peaks, and consistent peak locations, suggesting no structural change or chemical degradation.

[0304] Example 9: Fouling resistance of Poly (styrene)-random- poly (Vinylbenzyl trimethyl ammonium chloride) (PSA+) and Poly (styrenel-random- poly (Styrenesulfonic acid sodium salt) (PSS-) used as an Amphiphilic Polyelectrolyte Complex (APEC) bilayer

[0305] In this example, to characterize the fouling behavior of styrene-based APEC membranes with different foulants, we tested AS membrane prepared using 5 wt% casting solutions of PSA+ and PSS- with different fouling solutions having positive, negative, and neutral charges. Foulants were selected based on the composition of targeted applications feed. We started with testing AS because of its negative top layer. Having a net anionic surface is a common practice in commercial membranes to improve hydrophilicity and delay fouling. The experiments were performed in an Amicon 8010 stirred, dead-end filtration cell (Millipore) with a cell volume of 10 mL and an effective filtration area of 4.1 cm2and the cell was stirred at 500 rpm. SA membrane prepared using 5 wt% casting solutions of PSA+ and PSS- was also used in one experiment to determine its oil-emulsion fouling resistance properties. The same experiment was done on NP030 commercial membrane for comparison.

[0306] Oil was chosen as a common membrane foulant for our investigation because the oil, petroleum, and manufacturing sectors generate large amounts of oily wastewaters, and properly disposing of or treating them is still quite challenging. 1500 ppm oil-in-water emulsion with a 9:1 ratio of vegetable oil to DC 193 surfactant (non-ionic surfactant, obtained from Dow-Corning) was used to serve as the representative fouling solution to resemble challenging oily wastewater streams; prepared by blending the oil, water, and surfactant using a blender in high rpm for 3 min. Positive and negative charge proteins were used to assess the effect of surface charge and foulantmembrane electrostatic interactions on fouling. The experiments were performed using lysozyme and bovine serum albumin (BSA) solutions by dissolving 1 g / L of one of the proteins in IX phosphate buffered saline (PBS, pH 7.4). Proteins are challenging foulants because of their

[0307] - 35 - FH30004399.6

[0308] TUV- 19925

[0309] amphiphilic properties and pH-dependent net charge. At this pH, lysozyme has a net positive surface charge whereas BSA has a net negative surface charge. Proteins are also typical foulants in wastewater treatment operations, particularly in food and beverage, agricultural, and municipal wastewater streams. Dissolved / natural organic matter are deemed to be the main contributor to fouling among foulants in natural water (e.g., surface water, ground water, seawater) and wastewater streams. Organic mixture fouling test was performed using the fouling solution containing 500 ppm humic acid, 500 ppm sodium alginate, 9.5 mM NaCl and 0.5 mM CaCb. This is a solution of common organic foulants with their concentrations found in surface water and wastewater effluent streams from secondary treatment. Humic acid and sodium alginate are two major biomacromolecules causing fouling and CaCb has been shown to increase the fouling propensity of anionic polymeric organics by forming complexes with calcium. It can bridge humic acid and alginate chains and attach them to a membrane surface with carboxylate and sulfonate groups.

[0310] The dead-end filtration system serves as a "stress test" for membranes as the feed concentration rises during the experiment and is not typical of most industrial systems. Thus, membranes showing high fouling resistance in such experiments probably will perform even better in more realistic crossflow systems. To ensure a steady initial flux, DI water was first filtered through the membranes and the pure water flux was measured. The fouling feed solution was then filtered for 14 hours and the flux during its filtration was monitored. Then, the fouling solution was removed from the cell and membranes was rinsed with DI water to mimic a physical cleaning, and the DI water flux was measured once more. For all fouling tests, the Flux Recovery Ratio (FRR) was calculated using:

[0311] 100

[0312]

[0313] where fena! is the final DI water flux after the fouling test and a gentle rinse, and Jinitiai is the initial DI water flux before the fouling test. Results for fouling tests are provided in Figure 21.

[0314] Oil-in-water emulsion fouling test: A commercial polyether sulfone (PES)-based NF membrane, NP030 (Microdyn Nadir), was utilized as a benchmark due to its similar salt rejection performance. Adjustments were made to the transmembrane pressure for each membrane to achieve same initial flux of ~ 4 L.m’2.h_1, ensuring uniform hydrodynamics during the experiments. Excellent fouling

[0315] - 36 - FH30004399.6

[0316] TUV- 19925

[0317] resistance was established by the AS membrane and it showed just a minimal decline in flux throughout the fouling test and following water rinsing after oil-in-water emulsion filtration, while the commercial membrane showed -60% irreversible initial flux loss. For this membrane, a chemical cleaning procedure would be necessary for any flux recovery, as this loss could not be recovered by a water rinse. The SA showed 68% flux recovery. This shows that APECs are very promising materials for producing fouling-resistant membranes and how self-assembled layers that are chemically designed have a superior performance compared to commercial membranes with fixed chemistries that often require surface modifications to enhance fouling resistance.

[0318] Organic mixture fouling test: AS showed minimal flux decline when exposing to fouling solution, but the flux was fully recovered after water rinse. It is remarkable that it shows no flux reduction after exposure to the fouling solution and shows it is possible to create a fouling resistant layer using APECs.

[0319] Protein fouling tests: The initial DI water flux of AS membrane was measured until it stabilized. Then, IX PBS, which was the background matrix used to dissolve the proteins without aggregation / denature, was filtered through the membrane until the flux stabilized. The cell and reservoir were filled with one of the prepared protein fouling solutions, which was filtered through the membrane for 14 h. Afterwards, membrane was gently rinsed with IX PBS to simulate a physical cleaning and then it was filtered through the membrane. Then, the final DIW flux was measured again. Physical cleaning did not cause a significant flux recovery, and a 35% decline of the water flux after filtering lysozyme solution was observed. This implies that the foulant layer is strongly bound to the membrane surface likely associated with adsorptive fouling of lysozyme cationic protein on the AS’s negative top layer. AS membrane showed excellent fouling resistance with no water flux decline after anionic protein BSA test, showing that there was no irreversible fouling by this foulant solution. Therefore, any adsorptive fouling was cleaned without any harsh chemicals use. According to these results, AS can perform protein filtrations dependent on protein charge. Therefore, these tests verified that we were able to successfully control our membrane’s surface charge through specific order of casting of APE layers (e.g. cationic APE first and anionic APE next for AS bilayer membrane).

[0320] The results also show that AS almost retained its permeance even during the filtration of increasingly concentrated foulant solutions throughout dead-end experiments. These results are

[0321] - 37 - FH30004399.6

[0322] TUV- 19925

[0323] promising and show the potential of this class of self-assembled membranes to perform challenging separations. One potential application for APEC bilayer TFC membranes is the industrial wastewater treatment, where the retention of oils, sugars, and other biological components can be beneficial both on the feed side by producing organic feedstock and on the permeate side by eliminating pollutants.

[0324] Example 10: Water uptake of Poly (styrene)-random- poly (Vinylbenzyl trimethyl ammonium chloride) (PSA+) and Poly (styrene)-random- poly (Styrenesulfonic acid sodium salt) (PSS-) and their mixture compositions used in the respective membranes as an Amphiphilic Polyelectrolyte Complex (APEC) bilayer

[0325] For single copolymer layer films (S- and A+), water uptake measurements (Table 5) were carried out using films made by drop casting and drying 0.5 mL of a 5 wt% copolymers solution in methanol on a 1 cm diameter dish at room temperature. In order to simulate bilayer films for the water uptake experiment, 0.25 mL of PSA+ at 5 wt% was drop cast and allowed to dry at room temperature. The PSS- solution (0.25 mL) was then poured on top and allowed to dry at room temperature. To get the water uptake measurements for each film, the films were initially equilibrated in DIW at room temperature for overnight. After putting the films on a Kimwipe for five seconds to remove extra water, the samples were weighed. The dry weight was obtained after drying the same samples overnight in a vacuum oven set at 60°C.

[0326]

[0327] Table 5. Water uptake of copolymers films.

[0328]

[0329] Water uptake (%) 86 ±8 105 3 N / A 271 ±35

[0330] Example 11: Contact angle of Poly (styrene)-random- poly (Vinylbenzyl trimethyl ammonium chloride) (PSA+) and Poly (styrene)-random- poly (Styrenesulfonic acid sodium salt) (PSS-) used as Amphiphilic Polyelectrolyte single layers and Amphiphilic Polyelectrolyte Complex (APEC) bilayer membrane coatings

[0331] - 38 - FH30004399.6

[0332] TUV- 19925

[0333] Two types of contact angle measurements were performed on all membranes fabricated in Example 2: water-in-air (sessile drop) and air-in-water (captive bubble). Sessile drop contact angle was measured utilizing a Rame-Hart contact angle goniometer (Succasunna, NJ) on dried membranes cut and taped onto glass plates (Figure 22). 15 seconds after carefully applying a 10 pl DI water droplet onto the sample, the measurements were taken. For captive bubble measurements utilizing the same instrument, a transparent rectangular plastic chamber was placed on the sample stage and filled completely with DIW. Membrane samples were attached to a glass slide using double- sided tape and placed upside down in the chamber with the membrane totally submerged in water and the sample edges barely supported by small plastic caps and were let to remain in DIW chamber for 30 minutes to get equilibrated. An inverted needle was used to introduce 10 pF of air bubbles onto the sample (Figure 22). 15 seconds after carefully applying an air bubble onto the sample, the measurements were taken. Three measurements were made for each membrane and the calculated standard deviation of the three measurements is the error.

[0334] Example 12: Demonstration of sugar selectivity with a complex mixture of Poly (styrene)-random- poly (Vinylbenzyl trimethyl ammonium chloride) (PSA+) and Poly (styrene)-random- poly (Styrene sulfonic acid sodium salt) (PSS-) used as an Amphiphilic Polyelectrolyte Complex (APEC) bilaver

[0335] In this example, the AS membrane fabricated using 5 wt% casting solutions of PSA+ and PSS- was used in the experiment. Only AS bilayer membrane was examined, and the result is intended to represent both bilayer membranes with varying casting orders. We demonstrate the capability of APEC membranes in a specific application through fractionating corn syrup, a complex mixture of mono- and higher saccharides, to simulate production of a monosaccharide-enriched permeate (e.g., glucose) under more realistic conditions. While this is shown as one demonstration, the developed membrane technology is applicable to other separations requiring high permeance and selective transport of neutral organics. In contrast to traditional sugar processing, which relies on producing saccharides by hydrolyzing polysaccharides and extensive purification methods like chromatography using ion-exchange resins, particularly simulated moving bed chromatography (SMB), membrane separations present an eco-friendly solution that reduces energy demand and effluent generation through avoiding phase change or extensive

[0336] - 39 - FH30004399.6

[0337] TUV- 19925

[0338] chemical treatments, enhancing cost efficiency and supporting process intensification for producing value-added fractions in bioprocessing and food systems.

[0339] For the saccharide fractionation demonstration experiment, a 1 wt% solution of 42 DE corn syrup in DI water was prepared as a complex sugar mixture model feed, containing dry solid content of 20% glucose (monosaccharide), 13% maltose (disaccharide), 12% maltotriose (trisaccharide, DP3), and 55% higher saccharides (DP4+). Membrane performance was characterized using dead-end stirred cell experiments with 10 mL Amicon 8010 (Millipore) cells with 4.1 cm2filtration area. Two separate membrane disks were tested, and cells were stirred at 500 rpm. This rejection test was done after stabilization process mentioned in Example 3 and Example 4. When filtering the solution, after discarding the first 1 mL to avoid pure water contamination, enough volume was collected for measurements. Filtration test was conducted at 60 psi and sugar concentrations measured via HPLC described in Example 7. The corn syrup needed dilution to 1 wt% due to limitations in filtration cell operating pressure to overcome the osmotic pressure difference across the membrane effectively.

[0340] AS membrane showed clear size exclusion, allowing selective permeation of monosaccharides while retaining disaccharides and higher saccharides, resulting in two streams with distinctly different composition (Table 6). Figure 23 depicts compositional changes, with normalized fractions in feed and permeate streams. The permeate primarily consisted of glucose (-92%), with minor contributions from maltose and maltotriose (-3% each) and negligible DP4+ (<1%), indicating effective discrimination between simple and complex sugars. This mechanism aligns with the upgrading pathway for producing food-grade sweeteners and valorizing biomass-derived sugars. Additionally, the permeate's compositional profile closely resembles that of a 95 DE corn syrup, demonstrating that a single filtration step with AS membrane successfully upgraded the initial 42 DE feed to a higher Dextrose Equivalent (DE) grade, which enhances sweetness, solubility, and fermentability.

[0341] Table 6. Concentrations and % of total solids for the feed and permeate streams, together with rejection values when filtering a 1 wt% 42 DE corn syrup solution in DI water using AS membrane fabricated using 5 wt% casting solutions of PSA+ and PSS-.

[0342] -40 - FH30004399.6

[0343] TUV- 19925

[0344]

[0345] Glucose 180 1630 20 233 92 86± 0

[0346] Maltose 342 1051 13 8.9 3.5 > 99.1± 0

[0347] Maltotriose 504 987 12 8.9** 3.5 >99.1

[0348] DP4+ -830* 4644 55 2.2** 1 > 99.9

[0349] * The DP4+ mixture is treated as averaging to a DP5 sugar.

[0350] ** Limit of Quantification of the calibration curves (LOQ = 10*(standard error of predicted values) / slope of the curve) used as an estimation for maltotriose and DP4+ in the permeate. They were very low and could not be measured by integration, implying that their amounts in the permeate is even below the LOQ values.

[0351] The disclosure further encompasses the following embodiments, which are non-limiting.

[0352] Embodiment 1: A composite membrane, comprising: a porous support; and a selective layer comprising a first copolymer and a second copolymer; wherein: the first copolymer comprises a plurality of first hydrophobic repeat units and a plurality of cationic repeat units, wherein the plurality of first hydrophobic repeat units, the plurality of cationic repeat units, or both comprise aromatic or heteroaromatic moieties; and the second copolymer comprises a plurality of second hydrophobic repeat units and a plurality of anionic repeat units, wherein the plurality of second hydrophobic repeat units, the plurality of anionic repeat units, or both comprise aromatic or heteroaromatic moieties.

[0353] Embodiment 2: The composite membrane of embodiment 1, wherein the plurality of first hydrophobic repeat units and the plurality of cationic repeat units comprise aromatic or heteroaromatic moieties; and the plurality of second hydrophobic repeat units and the plurality of anionic repeat units comprise aromatic or heteroaromatic moieties.

[0354] Embodiment 3: The composite membrane of embodiment 1 or 2, wherein the plurality of first hydrophobic repeat units and the plurality of second hydrophobic repeat units each comprise

[0355] - 41 - FH30004399.6

[0356] TUV- 19925

[0357] repeat units derived from styrene, a substituted styrene, an aryl (meth)acrylate, or an aryl (meth)acrylamide.

[0358] Embodiment 4: The composite membrane of any one of the preceding embodiments, wherein the plurality of first hydrophobic repeat units and the plurality of second hydrophobic repeat units each independently comprise repeat units derived from styrene or a substituted styrene.

[0359] Embodiment 5: The composite membrane of any one of the preceding embodiments, wherein the plurality of cationic repeat units comprises repeat units derived from aryl (meth)acrylate, aryl (meth)acrylamide, styrene, or vinyl aromatic monomers substituted with an amine, a pyridinium, an imidazolium, a phosphonium, or a pyrrolidinium.

[0360] Embodiment 6: The composite membrane of any one of the preceding embodiments, wherein the plurality of cationic repeat units comprises repeat units derived from vinylbenzyl trimethylammonium chloride, 4-vinylaniline, 2-vinylaniline, N, N-dimethyl-4-vinylaniline, 4-vinylpyridine, or 4-vinylbenzyl(triphenyl)phosphonium.

[0361] Embodiment 7: The composite membrane of any one of the preceding embodiments, wherein the plurality of cationic repeat units comprises repeat units derived from vinylbenzyl trimethylammonium chloride.

[0362] Embodiment 8: The composite membrane of any one of the preceding embodiments, wherein the plurality of anionic repeat units comprises repeat units derived from aryl (meth)acrylate, aryl (meth)acrylamide, styrene, or vinyl aromatic monomers substituted with a carboxylic acid, a sulfonate, or a phosphate.

[0363] Embodiment 9: The composite membrane of any one of the preceding embodiments, wherein the plurality of anionic repeat units comprises repeat units derived from styrenesulfonic acid or salts thereof, styrene phosphonic acid derivatives, styrene phosphonate salts, vinylbenzoic acid derivatives, or styrenic monomers comprising a spacer between a styrene ring and an anionic group.

[0364] Embodiment 10: The composite membrane of any one of the preceding embodiments, wherein the plurality of anionic repeat units comprises repeat units derived from styrenesulfonic acid sodium salt.

[0365] Embodiment 11: The composite membrane of any one of the preceding embodiments, wherein the first copolymer is a statistical copolymer of styrene and vinylbenzyl

[0366] - 42 - FH30004399.6

[0367] TUV- 19925

[0368] trimethylammonium chloride, and the second copolymer is a statistical copolymer of styrene and styrenesulfonic acid sodium salt.

[0369] Embodiment 12: The composite membrane of any one of the preceding embodiments, wherein the first copolymer comprises about 5 - 60 mol% of the plurality of cationic repeat units, preferably 5 to 50 mol% of the plurality of cationic repeat units, or 5 to 40 mol% of the plurality of cationic repeat units, and wherein the second copolymer comprises about 5 - 60 mol% of the plurality of anionic repeat units, preferably 5 to 50 mol% of the plurality of anionic repeat units, or 5 to 40 mol% of the plurality of anionic repeat units.

[0370] Embodiment 13: The composite membrane of any one of the preceding embodiments, wherein the first copolymer and the second copolymer each independently have an average molar mass of 20,000 g / mol to 3,000,000 g / mol.

[0371] Embodiment 14: The composite membrane of any one of the preceding embodiments, wherein each of the first copolymer and the second copolymer is a random copolymer.

[0372] Embodiment 15: The composite membrane of any one of the preceding embodiments, wherein the selective layer comprises the first copolymer and the second copolymer sequentially layered on the porous support to provide a bilayer.

[0373] Embodiment 16: The composite membrane of embodiment 15, wherein a first layer comprising the first copolymer is in direct contact with the porous support and a second layer comprising the second copolymer is on the first layer on a side opposite the porous support.

[0374] Embodiment 17: The composite membrane of embodiment 15, wherein a second layer comprising the second copolymer is in direct contact with the porous support and a first layer comprising the first copolymer is on the second layer on a side opposite the porous support.

[0375] Embodiment 18: The composite membrane of any one of the preceding embodiments, wherein the selective layer comprises the first copolymer and the second copolymer as a blended layer on the porous support.

[0376] Embodiment 19: The composite membrane of any one of the preceding embodiments, wherein the selective layer has a thickness of about 30 nm to about 8 pm, preferably 0.1 pm to 2 pm, and an effective pore size of about 0.5 nm to about 2 nm.

[0377] Embodiment 20: The composite membrane of any one of the preceding embodiments, wherein the composite membrane has a water permeance of about 0.5 L / m2-h-bar to about 30 L / m2-h-bar.

[0378] - 43 - FH30004399.6

[0379] TUV- 19925

[0380] Embodiment 21: The composite membrane of any one of the preceding embodiments, wherein the selective layer exhibits one or more of: a rejection of at least 80% for at least one neutral solute selected from sucrose, riboflavin, and vitamin B 12; a rejection of at least 70% for at least one divalent salt selected from NazSCh and MgSCh; a rejection of less than 50% for NaCl; oil fouling resistance characterized by maintaining at least 80% of initial water flux after exposure to a 1500 ppm oil-in-water emulsion for at least 14 hours; a D-glucose / sucrose separation factor of greater than 10; and stability over a range of pH 2 to pH 12.

[0381] Embodiment 22: The composite membrane of any one of the preceding embodiments, wherein the porous support is a porous polymeric support.

[0382] Embodiment 23: A method of separating a solute from a feed solution, the method comprising contacting the feed solution with a composite membrane of any one of the preceding embodiments thereby providing a first stream having a lower concentration of the solute relative to the feed solution.

[0383] Embodiment 24: The method of embodiment 23, comprising passing the feed solution through the composite membrane to provide the first stream.

[0384] Embodiment 25: The method of embodiment 23 or 24, wherein the solute is a salt, a sugar, a protein, a dye, a vitamin, or an oil.

[0385] Embodiment 26: A method of fabricating the composite membrane of any one of embodiments 1 to 22, the method comprising: applying to a porous support a first copolymer comprising a plurality of first hydrophobic repeat units and a plurality of cationic repeat units, wherein the plurality of first hydrophobic repeat units, the plurality of cationic repeat units, or both comprises aromatic or heteroaromatic moieties; and applying to the porous support a second copolymer comprising a plurality of second hydrophobic repeat units and a plurality of anionic repeat units, wherein the plurality of second hydrophobic repeat units, the plurality of anionic repeat units, or both comprises aromatic or heteroaromatic moieties.

[0386] Embodiment 27: The method of embodiment 26, wherein the first copolymer and the second copolymer are applied to the porous support sequentially, thereby forming a bilayer membrane.

[0387] Embodiment 28: The method of embodiment 26, wherein the first copolymer and the second copolymer are applied to the porous support simultaneously, thereby forming a blend.

[0388] - 44 - FH30004399.6

[0389] TUV- 19925

[0390] Embodiment 29: The method of any one of embodiments 26 to 28, wherein the first copolymer and the second copolymer are each independently dissolved in a polar organic solvent prior to application, and the method further comprises removing solvent from the selective layer.

[0391] INCORPORATION BY REFERENCE

[0392] All U. S. and PCT patent application publications and U. S. patents mentioned herein are hereby incorporated by reference in their entirety as if each individual publication or patent was specifically and individually indicated to be incorporated by reference. In case of conflict, the present application, including any definitions herein, will control.

[0393] EQUIVALENTS

[0394] While specific embodiments of the subject invention have been discussed, the above specification is illustrative and not restrictive. Many variations of the invention will become apparent to those skilled in the art upon review of this specification and the claims below. The full scope of the invention should be determined by reference to the claims, along with their full scope of equivalents, and the specification, along with such variations.

[0395] -45 - FH30004399.6

Claims

TUV- 19925CLAIMSWe claim:

1. A composite membrane, comprising: a porous support; and a selective layer comprising a first copolymer and a second copolymer; wherein:the first copolymer comprises a plurality of first hydrophobic repeat units and a plurality of cationic repeat units, wherein the plurality of first hydrophobic repeat units, the plurality of cationic repeat units, or both comprise aromatic or heteroaromatic moieties; and the second copolymer comprises a plurality of second hydrophobic repeat units and a plurality of anionic repeat units, wherein the plurality of second hydrophobic repeat units, the plurality of anionic repeat units, or both comprise aromatic or heteroaromatic moieties.

2. The composite membrane of claim 1, whereinthe plurality of first hydrophobic repeat units and the plurality of cationic repeat units comprise aromatic or heteroaromatic moieties; andthe plurality of second hydrophobic repeat units and the plurality of anionic repeat units comprise aromatic or heteroaromatic moieties.

3. The composite membrane of claim 1, wherein the plurality of first hydrophobic repeat units and the plurality of second hydrophobic repeat units each independently comprises repeat units derived from styrene, a substituted styrene, an aryl (meth)acrylate, or an aryl (meth)acrylamide.

4. The composite membrane of claim 1, wherein the plurality of first hydrophobic repeat units and the plurality of second hydrophobic repeat units each independently comprises repeat units derived from styrene or a substituted styrene.

5. The composite membrane of claim 1, wherein the plurality of cationic repeat units comprises repeat units derived from aryl (meth)acrylate, aryl (meth) acrylamide, styrene, or vinyl aromatic monomers, each independently substituted with an amine, a pyridinium, an imidazolium, a phosphonium, or a pyrrolidinium.- 46 - FH30004399.6TUV- 199256. The composite membrane of claim 1, wherein the plurality of cationic repeat units comprises repeat units derived from vinylbenzyl trimethylammonium chloride, 4-vinylaniline, 2-vinylaniline, N, N-dimethyl-4-vinylaniline, 4-vinylpyridine, or 4-vinylbenzyl(triphenyl)phosphonium.

7. The composite membrane of claim 1, wherein the plurality of cationic repeat units comprises repeat units derived from vinylbenzyl trimethylammonium chloride.

8. The composite membrane of claim 1, wherein the plurality of anionic repeat units comprises repeat units derived from aryl (meth)acrylate, aryl (meth) acrylamide, styrene, or vinyl aromatic monomers, each independently substituted with a carboxylic acid, a sulfonate, or a phosphate.

9. The composite membrane of claim 1, wherein the plurality of anionic repeat units comprises repeat units derived from styrenesulfonic acid or salts thereof, styrene phosphonic acid derivatives, styrene phosphonate salts, vinylbenzoic acid derivatives, or styrenic monomers comprising a spacer between a styrene ring and an anionic group.

10. The composite membrane of claim 1, wherein the plurality of anionic repeat units comprises repeat units derived from styrenesulfonic acid sodium salt.

11. The composite membrane of claim 1, wherein the first copolymer is a statistical copolymer of styrene and vinylbenzyl trimethylammonium chloride, and the second copolymer is a statistical copolymer of styrene and styrenesulfonic acid sodium salt.

12. The composite membrane of claim 1, wherein the first copolymer comprises about 5 to 60 mol% of the plurality of cationic repeat units, preferably 5 to 50 mol% of the plurality of cationic repeat units, or 5 to 40 mol% of the plurality of cationic repeat units, and wherein the second copolymer comprises about 5 to 60 mol% of the plurality of anionic repeat units, preferably 5 to 50 mol% of the plurality of anionic repeat units, or 5 to 40 mol% of the plurality of anionic repeat units.- 47 - FH30004399.6TUV- 1992513. The composite membrane of claim 1, wherein the first copolymer and the second copolymer each independently has an average molar mass of 20,000 g / mol to 3,000,000 g / mol.

14. The composite membrane of claim 1, wherein each of the first copolymer and the second copolymer is a random copolymer.

15. The composite membrane of claim 1, wherein the selective layer comprises the first copolymer and the second copolymer sequentially layered on the porous support to provide a bilayer.

16. The composite membrane of claim 15, wherein a first layer comprising the first copolymer is in direct contact with the porous support and a second layer comprising the second copolymer is on the first layer on a side opposite the porous support.

17. The composite membrane of claim 15, wherein a second layer comprising the second copolymer is in direct contact with the porous support and a first layer comprising the first copolymer is on the second layer on a side opposite the porous support.

18. The composite membrane of claim 1, wherein the selective layer comprises the first copolymer and the second copolymer as a blended layer on the porous support.

19. The composite membrane of claim 1, wherein the selective layer has a thickness of about 30 nm to about 8 pm, preferably 0.1 pm to 2 pm, and an effective pore size of about 0.5 nm to about 2 nm.

20. The composite membrane of claim 1, wherein the composite membrane has a water permeance of about 0.5 L / m2-h-bar to about 30 L / m2-h-bar.

21. The composite membrane of claim 1, wherein the selective layer exhibits one or more of:a rejection of at least 80% for at least one neutral solute selected from sucrose, riboflavin, and vitamin B12;a rejection of at least 70% for at least one divalent salt selected from NazSCh and MgSCh;- 48 - FH30004399.6TUV- 19925a rejection of less than 50% for NaCl;oil fouling resistance characterized by maintaining at least 80% of initial water flux after exposure to a 1500 ppm oil-in-water emulsion for at least 14 hours;a D-glucose / sucrose separation factor of greater than 10; andstability over a range of pH 2 to pH 12.

22. The composite membrane of any one of the preceding claims, wherein the porous support is a porous polymeric support.

23. A method of separating a solute from a feed solution, the method comprising contacting the feed solution with a composite membrane of claim 1, thereby providing a first stream having a lower concentration of the solute relative to the feed solution.

24. The method of claim 23, comprising passing the feed solution through the composite membrane to provide the first stream.

25. The method of claim 23, wherein the solute is a salt, a sugar, a protein, a dye, a vitamin, or an oil.

26. A method of fabricating the composite membrane of claim 1, the method comprising: applying to a porous support a first copolymer comprising a plurality of first hydrophobic repeat units and a plurality of cationic repeat units, wherein the plurality of first hydrophobic repeat units, the plurality of cationic repeat units, or both comprises aromatic or heteroaromatic moieties; and applying to the porous support a second copolymer comprising a plurality of second hydrophobic repeat units and a plurality of anionic repeat units, wherein the plurality of second hydrophobic repeat units, the plurality of anionic repeat units, or both comprises aromatic or heteroaromatic moieties.

27. The method of claim 26, wherein the first copolymer and the second copolymer are applied to the porous support sequentially, thereby forming a bilayer membrane.- 49 - FH30004399.6TUV- 1992528. The method of claim 26, wherein the first copolymer and the second copolymer are applied to the porous support simultaneously, thereby forming a blend.

29. The method of claim 26, wherein the first copolymer and the second copolymer are each independently dissolved in a polar organic solvent prior to application, and the method further comprises removing solvent from the selective layer.- 50 - FH30004399.6