Methods for enhancing porosity and reducing defects in low-dimensional zeolites
The secondary growth process enhances the porosity and reduces defects in low-dimensional zeolites, addressing diffusion limitations and deactivation issues, resulting in improved catalytic performance and extended catalyst lifetime.
Patent Information
- Application Number
- PCT/US2026/028595
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-16
- Filing Date
- 2026-05-18
- Publication Date
- 2026-11-19
AI Technical Summary
Low-dimensional zeolites suffer from severe diffusion limitations and rapid deactivation in catalytic applications due to intrinsic defects and mass transport restrictions, limiting their performance and commercial viability.
A secondary growth process with a low aluminosilicate supersaturated solution is applied to low-dimensional zeolites like ZSM-23, MTT, and MOR, introducing surface roughness and enhancing porosity to improve mass transport properties and reduce defects.
The method significantly increases micropore volume, extends catalyst lifetime, and enhances product selectivity, particularly in methanol-to-hydrocarbon reactions, outperforming conventional zeolites by improving turnover number and maintaining high propylene selectivity without coking.
Smart Images

Figure US2026028595_19112026_PF_FP_ABST
Abstract
Description
Attorney Docket No.: UNIH-322WO (109293.332) PCT PATENT APPLICATION UHID 2025-050METHODS FOR ENHANCING POROSITY AND REDUCING DEFECTS IN LOW¬DIMENSIONAL ZEOLITESBACKGROUND
[0001] This application claims priority to U. S. Provisional Patent Application Serial No. 63 / 806,924, entitled “Methods for Enhancing Porosity and Reducing Defects in Low-Dimensional Zeolites,” filed May 16, 2025, the entire contents of which are incorporated by reference herein.
[0002] This invention was made with government support under grant DE-SC0021384 awarded by the Department of Energy. Tire government has certain rights in the invention.
[0003] Uris disclosure pertains to methods for preparing low-dimensional zeolite crystals with high micropore volume and reduced diffusion limitations.
[0004] Zeolites, owing to their unique pore topologies and shape selectivity, are a common class of catalysts in industries for hydrocarbon processing. Examples include (but are not limited to) the utilization of methanol as feedstock to convert to higher-value hydrocarbons, light naptha cracking, and carbon dioxide utilization. Among the large variety of chemicals that can be obtained industrially using zeolites as catalysts, light olefins (C2- - C4-) are considered as key intermediates for obtaining high-value products or fuels. Light olefins have been traditionally produced by steam cracking processes of light hydrocarbons or naphthas, but utilizing methanol as a feedstock for its direct transformation to hydrocarbons has been widely explored as one option to address the increasing demand for desired light olefins through either methanol-to-propylene (MTP) or methanol-to-olefins (MTO) processes.
[0005] Considering that the methanol-to-hydrocarbons (MTH) reaction proceeds through a very' complex dual-cycle mechanism, including both olefin and aromatic pathways that predominantly generate C3- - Cs= and C2- - C; alkenes, respectively, it is not surprising that the zeolite structure combined with other physicochemical properties (e.g. Si / Al molar ratio and particle size) has a direct impact on catalyst activity and selectivity in the MTH process. In general, three-dimensional (3D) pore zeolites present improved resistance against deactivation owing to their ideal mass transport properties, whereas product selectivity can be fine-tuned by choosing either a small-pore zeolite (e.g. CHA or AEI framework types), which favors light olefins (mostly Cs- in the MTO process), or a medium-pore zeolite (e.g., MFI) that- 1 -50129690Attorney Docket No.: UNIH-322WO (109293.332) PCT PATENT APPLICATION UHID 2025-050can produce gasoline (i.e. aromatics and alkanes, in the MIG process), lire presence of acid sites within the open space of MFI channel intersections facilitates the formation of aromatics and larger alkanes. In contrast, one-dimensional (ID) medium-pore zeolites, such as ZSM-22 (TON) and ZSM-23 (MTT), show better selectivity towards light olefins and linear Cs-Ce- molecules due to the constrained acid sites within the ID medium pore that promote the olefinic cycle. Unfortunately, these low-dimensional materials are highly prone to deactivation due to severe mass transport restrictions, and are, therefore, limited in catalytic applications.
[0006] To overcome diffusion limitations in zeolites, there are two common synthetic approaches that can be used to design more optimal materials based on methods to decrease crystal size or introduce mesopores. There have been numerous attempts to decrease the cry stal size of 3D zeolite frameworks using complex organics or crystal seeds to create sheet-like or hierarchical structures, modifiers, or unique synthesis conditions (e.g., temperature or pre-crystallized zeolites as Si and Al sources) to create nano-sized particles, or secondary growth methods to create core-shells (e.g., elemental Si / Al gradients) or fm-like protrusions (e.g., zeolites MFI, MEL, and FER). The majority of these breakthroughs in zeolite design focus on 3D zeolite frameworks, such as MFI (ZSM-5), where diffusion in all 3 directions allow s for improvements in catalyst performance by tailoring crystal growth along any of its dimensions. On the other hand, the rational design of unidimensional zeolite frameworks (e.g, MTT) is restricted to synthesis methods that alter growth in only one dimension parallel to ID channels.
[0007] The design of hierarchical and nano-sized zeolite catalysts often requires complex synthesis conditions such as hydrofluoric (HF) treatment, long-alkyl chain surfactants, and alkaline etching. These processes can be costly and time-intensive, and produce materials with restricted acidity and small yields, which collectively limit their commercial viability. A major advantage of using secondary growth to introduce ‘Tins” is its versatility for a broad range of framework types with diverse compositions (e.g., Si / Al ratios and heteroatoms).SUMMARY
[0008] The present disclosure relates generally to methods for preparing lowdimensional zeolites having high micropore volume, reduced intrinsic defects, and reduced diffusion limitations.50129690Attorney Docket No.: UNIH-322WO (109293.332) PCT PATENT APPLICATION UHID 2025-050
[0009] One-dimensional zeolites have distinct pore topologies for shape-selective catalysis, yet their performance in conventional reactions is frequently compromised by severe diffusion limitations. This disclosure relates to methods that can be used to optimize the properties and catalytic performance of 1-dimensional (ID) framework zeolites (such as MTT, MTW, and MOR) through a unique mechanism that differs from those reported in prior examples of finned 2D and 3D zeolites.
[0010] Like many other unidirectional materials, zeolite ZSM-23 (MTT) tends to grow with a needle-like shape morphology with a high aspect ratio, where the channel direction is parallel to the longest dimension of the needle (a-direction). ZSM-23 catalysts have been demonstrated to show a high selectivity towards Cs-C6+ products in hydrocarbon upgrading reactions (e.g., MTH, cracking), but with a very low amount of aromatics, thus producing “clean gasoline”. Aromatic formation is limited due to the absence of channel intersections; however, rapid coking leads to pore blockage, which is a major drawback of unidirectional zeolite frameworks. Most of the 10- membered ring containing ID channels, such as ZSM-22, ZSM-23, and EU-1, restrict diffusion of branched isomers and aromatic rings; therefore, their shape selectivities are governed by the combined effects of transition state and product diffusion limitations. Provided that their mass transport restrictions can be overcome, ID zeolites can be considered as potential catalysts to produce linear-chained alkanes or alkenes as desired products.
[0011] There have been numerous attempts to reduce the size of MTT in the a-direction (diffusion direction) by using diquat surfactants as organic structure-directing agents (OSDAs) or the use of organosilanes. Post-synthesis methods, such as mechanochemical treatment and alkali etching, have also been used to reduce particle size or introduce mesopores, respectively. Traditional alkali treatment often has undesirable side effects, such as a notable decrease in acid strength, loss of crystallinity, and reduced product yield. Tlie present disclosure presents an alternative approach using a facile secondary growth procedure to create optimal unidirectional materials (such as ZSM-23) that outperform state-of-the art MTT-type materials,
[0012] ZSM- 12 is a medium-pore zeolite with the MTW topology that features a onedimensional pore system composed of 12-membered rings with dimensions of approximately 5.6 - 6.0 A. It was first synthesized in 1974 using hexamethonium cations as the organic structure-directing agent (OSDA), marking a significant development in the design of shape- selective catalysts. Tire MTW framework is distinguished by its linear, non-intersecting- 3 -50129690Attorney Docket No.: UNIH-322WO (109293.332) PCT PATENT APPLICATION UHID 2025-050channels, which confer unique diffusion and catalytic characteristics. In its proton form (H- ZSM-12), the material has shown considerable promise in various industrially relevant reactions. Mordenite was first structurally elucidated in 1961 and exhibits a predominantly two-dimensional pore system composed of large 12-membered ring channels (~6.5 - 7.0 A) aligned along the c-axis, interconnected by significantly narrower 8-membered ring side pockets (—2.6 * 5.7 A). Due to the restricted dimensions of these secondary’ channels, which are inaccessible to most reactant molecules, mordenite is considered to be a one-dimensional zeolite with respect to molecular transport. The framework’s high internal surface area, well-defined microporosity, and tunable acidity' have made mordenite an important material in catalysis, separations, and purification processes. Its uniform micropore size and robust hydrothermal stability support its use in applications ranging from hydrocracking to isomerization and selective adsorption; however, like many one-dimensional zeolites, mordenite suffers from intrinsic mass transport limitations due to its narrow, isolated channels and low pore interconnectivity. These constraints often lead to diffusion-limited regimes, which negatively impact catalytic activity, selectivity, and long-term stability, particularly under industrial conditions
[0013] lire approach described herein can be applied to any one-dimensional zeolite, including commercial materials taken “off the shelf’ and allows for versatility in the selection of composition (e.g., Si / Al molar ratio). One-dimensional zeolites often have beter olefin selectivity but are known to deactivate at a much faster rates in hydrocarbon catalysis compared to zeolites with 3 -dimensional pore networks. Low-dimensional zeolites also tend to have intrinsic defects. Here the enhanced catalyst performance of secondary' growth is demonstrated, using exemplary zeolites MTT, MTW, and MOR using a reaction that is known to cause rapid deactivation. The modified zeolite enhances catalyst lifetime while maintaining an unusually high propylene selectivity. This technology will improve the preparation of lowdimensional zeolite frameworks for commercial applications that extend beyond MTH to other hydrocarbon upgrading reactions.BRIEF DESCRIPTION OF THE DRAWINGS
[0014] FIG. 1 shows transmission electron micrographs and corresponding SAED patterns of MTT zeolite, including (A) Zeolite MTT crystals prepared from a synthesis that yields disperse anisotropic rods, (B) MTT-sg after secondary growth in a low supersaturation silica solution, w ith Inset: Higher magnification image of MTT-sg clearly showing the presence- 4 -50129690Attorney Docket No.: UNIH-322WO (109293.332) PCT PATENT APPLICATION UHID 2025-050of surface roughness on the MIT crystals, indicating the presence of protrusions, (C) Nano¬ sized MTT (MTT-nano) crystals synthesized using a long chain OSDA, SAED patterns of (D) MTT seed, (E) MTT-sg, and (F) MTT-nano.
[0015] FIG. 2 shows (A) MTT framework diagram long the
[0100] zone axis showing the 10-membered ring pore openings. MTT has an orthorhombic crystal structure (Pmmn space group) with unit cell parameters a = 0.526, b = 2.20, and c = 1.14 nm, (B) Idealized schematic of a ZSM-23 (MTT) crystal after secondary growth, and (C) Hypothetical roughness on exterior {010} surfaces as a result of secondary growth in the form of (i) a single unfinished layer with a step height equal to that of tire b or c unit cell dimension or (ii) step bunches with heights (h) equal to multiples of the unit cell dimensions.
[0016] FIG. 3 show's high-resolution transmission electron microscopy (HR-TEM) images of (A) MTT (seed) and (B - D) MTT-sg samples.
[0017] FIG. 4 shows Ar adsorption / de sorption isotherms for proton form (H-form) seeds (H-MTT) and the sample after secondary growth (H-MTT-sg).
[0018] FIG. 5 shows micropore volumes of ZSM-23 samples found in literature compared w'ith samples MTT and MTT-sg.
[0019] FIG. 6 show's (A) results of the methanol to hydrocarbon (MTH) reaction at 400 °C comparing the performance of H-MTT-sg (circles), parent seed H-MTT (squares), and H-MTT-nano (triangles) and (B) product selectivity (bar graphs) for all three MTT catalysts along with H-ZSM-5 (Si / Al 40) at initial conversion in methanol to hydrocarbon (MTH) reaction at 400 °C.
[0020] FIG. 7 shows powder X-ray diffraction (PXRD) patterns of zeolite (A) MTW and (B) MOR crystals.
[0021] FIG. 8 shows scanning electron micrographs of (A) zeolite MOR crystals purchased from Zeolyst. (B) Modified MOR after secondary growth (MOR-sg) using a low supersaturation aluminosilicate solution. (C - F) MTW crystals with Si / Al = 50 (C) before and (D) after secondary grow'th (MTW-sg). MTW crystals with Si / Al=30 (E) before and (F) after secondary growth (MTW-30-sg).DETAILED DESCRIPTION OF PREFERRED EMBODIMENTS
[0022] Tire present disclosure relates to a post-synthesis treatment methodology for- 5 -50129690Attorney Docket No.: UNIH-322WO (109293.332) PCT PATENT APPLICATIONUHID 2025-050low-dimensional zeolite frameworks that uses a unique secondary growth solution to generate surface roughness, remove intrinsic defects, and / or alter the size of parent crystals to collectively enhance porosity and reduce diffusion limitations. Preferred embodiments relate to the use of this treatment methodology in crystal structures such as ZSM-23 (MTT), mordenite (MOR), and ZSM-12 (MTW).
[0023] Preferred embodiments of the secondary' growth procedure described herein use solutions with an unusually low aluminosilicate supersaturation to create greater access to interior pores of low-dimensional zeolites. The gel composition and synthesis parameters were selected judiciously to prevent nucleation of new cry sials in growth solution and to supply¬ enough material for a small degree of growth on seed crystals. The molar ratio H? O / Si varies between 25-125 in atypical secondary growth solution, and seed concentration varies between 5-20 wt%. Tins composition provides an abnormally low concentration of nutrient (i.e., silica and alumina) and higher surface area of seed crystals compared to compositions reported in literature for seed-assisted zeolite crystallization. The synthesis temperature and time vary between 100-140°C and 1-3 days, respectively. This method significantly increases the micropore volume, indicating the presence of defects in as-synthesized low-dimensional zeolites such as MTT and MOR. This overcomes significant mass transport limitations often associated with one-dimensional zeolites in shape-selective catalysis. High-resolution images for MTT show roughened interfaces comprised of step bunches of unfinished layers with ultrasmall dimensions that present a series of short ID channels. Diffusion measurements reveal that secondary treatment results in higher D / R2 values where D is the effective diffusivity of a probe molecule (e.g., aliphatic C6 molecule) and R is the effective crystal dimension. Benchmark reactions were carried out using methanol to hydrocarbons (MTH) to assess the catalytic performance of as-syntheses and treated zeolites. Measurements reveal dramatic enhancement in turnover number, catalysts lifetime, and significant changes in product selectivity (e.g., higher propen e / ethene ratio) compared to conventional MTH catalysts such as zeolite ZSM-5 (MFI). For certain materials, secondary' growth alters the size / morphology of the parent crystal to create products with much smaller size. This is evident in the secondary growth of zeolite MOR which shows a reduction in particle size to achieve aggregates of smaller crystals.
[0024] Preferred embodiments described herein relate to a method for post-synthesis modification of low-dimensional zeolite frameworks comprising preparation of a secondary'- 6 -50129690Attorney Docket No.: UNIH-322WO (109293.332) PCT PATENT APPLICATION UHID 2025-050growth solution, where the secondary' growth solution comprises framework source precursors that include both a silica source and an alumina source. Preferably, the silica source is SiCh and the alumina source is AI2O3. The secondary / grow th solution also comprises one or more structure-directing agents, a hydroxide source, and water. In preferred embodiments, the structure-directing agents may be pyrrolidine, dimethylformamide, tetraethylammonium hydroxide, 1,8-diammooctane, cyclohexylamine, tetrabutylammonium hydroxide, or combinations thereof. In preferred embodiments, the hydroxide source may be NazO or K2O.
[0025] Preferred embodiments of the method described herein utilize a secondary¬ growth solution with a low aluminosilicate supersaturation. The secondary growth solution preferably has a molar composition ratio of the framework source precursors, including both the silica source and the alumina source, to water of about 0.001-0.05, and about 0.01-0.02 in additional preferred embodiments. In other preferred embodiments, the secondary growth solution has a molar composition ratio of the silica source to the alumina source of about 12-100, and about 70-75 in additional preferred embodiments. In additional preferred embodiments, the secondary' growth solution has a molar composition ratio of the framework source precursors to the structure directing agents of about 0.04-5, and about 1-3 in additional preferred embodiments. In additional preferred embodiments, the secondary growth solution has a molar composition ratio of the framework source precursors to the hydroxide source of about 0.05-100, and about 4-5 in additional preferred embodiments. The secondary' growth solution may be stirred for a period of time, preferably about 12-24 hours, before taking further action.
[0026] In preferred embodiments of the method for post-synthesis modification of low-dimensional zeolite frameworks, zeolite seed crystals are added to the secondary- growth solution, preferably in an amount of about 5-20 weight percent of the secondary- growth solution. The zeolite seed crystals are preferably a low-dimensional zeolite such as ZSM-23 (MTT), mordenite (MOR), or ZSM-12 (MTW). lire secondary growth solution, containing the zeolite seed cry stals, is then preferably heated to a temperature of about 100-140°C for about 1-3 days, then quenched. The resulting modified zeolite crystals are then isolated from the solution. The modified zeolite crystals obtained using this method have surface roughness, reduced intrinsic defects, and enhanced - or more accessible - porosity.
[0027] The methods described herein for post-synthesis modification of lowdimensional zeolites such as ZSM-23 (MTT), ZSM-12 (MTW), and mordenite (MOR)- 7 -50129690Attorney Docket No.: UNIH-322WO (109293.332) PCT PATENT APPLICATION UHID 2025-050dramatically improve their mass transport properties. This is accomplished by a facile secondary growth process that introduces surface roughness on the exterior surfaces of the crystals and creates greater access to interior pores through the putative removal of intrinsic defects. High resolution images show that roughened interfaces are step bunches of unfinished layers with ultra-small dimensions that present a series of short ID channels. Comparison of exemplary’ materials against conventional and nano-sized ZSM-2.3 catalysts using methanol to hydrocarbons as a benchmark reaction reveal dramatic enhancement in turnover number and product selectivity that achieves a much higher propene / ethene ratio than ZSM-5 (MFI) catalysts. The improved mass transport of these catalysts after secondary' growth also markedly' extends their life time at much shorter reactant con tact times -without any observed changes in the mechanism of coking. Collectively, these methods can be used for the production of modified ID zeolites as catalysts for commercial applications.EXAMPLES AND RESULTSEXAMPLE 1.
[0028] Experimental Methods and Materials.
[0029] Materials. Tire follow ing chemicals for zeolite synthesis were purchased from Sigma Aldrich: LUDOX AS-40 (40 wt% suspension in water), tetraethyl orthosilicate (TEOS, > 99.5%), sodium aluminate (57.1% AI2O3 and 37.2% NazO), aluminum nitrate nonahydrate (A1(NO3)3.9H2O, > 98%), aluminum sulfate hydrate (A^SOrrflLO, 98%), tetrapropylammonium hydroxide (TPAOH, 98%), N, N -dimethylformamide (anhydrous, 99.8%), pyrrolidine (99%), sodium hydroxide (>98% pellets, anhydrous), and potassium hydroxide (>85% pellets). For synthesis of HMBr, 1,7-dibromoheptane (97%) and trimethylamine (anhydrous, >99%) were purchased from Sigma-Aldrich; ethanol (>99.8%) and acetone (>99.5%) 'ere purchased from J T Baker. Deionized (DI) water was produced with an Aqua Solutions RODI-C-12A purification system (18.2 MQ). All reagents w'ere used as received without further purification. For reaction testing, methanol w as purchased from J. T. Baker (99.8%), and the argon, oxygen and nitrogen gases 'ere purchased from Praxair with UHP grade (99.999%).
[0030] Synthesis of seed crystals. The ZSM-23 sample used as seeds was prepared with a molar composition of 0.55 DMF (N, N-dimethylformamide): 0.2.5 NazO: 1 SiOz:- 8 -50129690Attorney Docket No.: UNIH-322WO (109293.332) PCT PATENT APPLICATION UHID 2025-0500.014 AI2O3: 29.5 H2O. The mixture was stirred at room temperature for 24 hours. The sol gel was then placed in a 30 ml Teflon-lined acid digestion bomb and heated in an oven at 160 °C under rotation and autogenous pressure for 3 days. The crystalline product was removed from the mother liquor by three cycles of centrifugation and washes with deionized water, using a Beckman Coulter Avanti J-E centrifuge at room temperature and 6,000 ipm for 10 minutes per cycle. The resulting seeds were immediately stored in deionized water without allowing time for the solids to dry.
[0031] Seed directed secondary growth on ZSM-23. A growth solution was prepared with a molar composition of 0.45 pyrrolidine: 0.2Na?. O: 1 SiO?.: 0.014 AI2O3: 90 H2O. The mixture was stirred at room temperature for 24 hours. The prepared ZSM-23 seed was added to this solution at 15% by weight of the solution and placed in a 30 ml Teflon-lined acid digestion bomb and heated in an oven at 140 °C under rotation and autogenous pressure for 2.75 days. Similar to the seed crystals, the crystalline product was removed from the mother liquor by three cycles of centrifugation and washes with deionized water, using a Beckman Coulter Avanti J-E centrifuge at room temperature and 6,000 rpm for 10 minutes per cycle.
[0032] Synthesis of nano-MTT. Nano-sized ZSM-23 zeolite was synthesized as a reference material using a previously reported protocol. In a typical synthesis, sodium hydroxide solution was mixed in Di water until fully dissolved. To this solution aluminum source was added followed by continuous stirring until the mixture was homogenous. Fumed silica was then added, stirred until well mixed and followed by addition of HMBr to the mixture. Similar centrifugation procedure was followed as mentioned above. The centrifuged MTT samples were dried at room temperature in air and then calcined in a muffle furnace at 550 °C using heating and cooling rates of 1 °C min"!for 8 hours. Ion exchange was performed three times using a 1 M NH4NO3 solution (2 wt% of calcined samples in solutions), which was heated at 80 °C under continuous stirring for 2 hours. The exchanged samples were dried and calcined by the same procedure described above to obtain proton form (H-form) zeolites.
[0033] Synthesis of conventional ZSM-5 catalyst. Conventional ZSM-5 catalyst of Si / Al 40 was prepared according to a previously reported protocol except the molar composition was modified to 20 TPAOH: 4 Na2O: 100 SiCh: 1.25 AI2O3: 2500 II2O. The as-synthesized sample was converted to proton form by ion exchange followed by calcination using the same protocol as above._ 9 _50129690Attorney Docket No.: UNIH-322WO (109293.332) PCT PATENT APPLICATIONUHID 2025-050
[0034] OSDA preparation. The heptamethonium bromide (HMBr) was prepared by refluxing 1,7-dibromoheptane with an excess of trimethylamine in ethanol as a solvent overnight. The product was cooled in ice bath before separation using vacuum filtration. The excess amine was removed by extraction with acetone and recrystallizations were performed in methanol-diethyl ether mixtures. After purification, the formation and purity of HMBr was confirmed byXH NMR.
[0035] Materials characterization. Powder X-ray diffraction (PXRD) patterns of dried solids were collected on a Rigaku SmartLab diffractometer with a Cu Ka source (40 kV, 30 mA). SEM images were obtained using ThermoFisher Axia ChemiSEM. HR-TEM images and selected area electron diffraction patterns wzere acquired using a Thermal Fisher Tliemis-Z microscope operated at 300 kV with double aberration correctors and a Gatan Oneview Insitu detector (resolution 4096 x 4096 pixels, pixel size 15 pm). Elemental analysis was performed by electron dispersive X-ray (EDX) spectroscopy. EDX spectra were collected using Axia ChemiSEM at 15 kV and a 15 mm working distance. Textural analysis was performed with a Micromeritics 3 flex instrument using N2 as a probe gas for physisorption. Surface area was calculated from the BET isotherm and micropore volume was estimated by the t-plot method. Argon physisorption measurements were performed at 87.3 K using Micromeritics ASAP 2420, Prior to adsorption tests, the samples were calcined at 873K for one hour and then transferred to the sample tube, followed by vacuum degassed at 573K for one hour. Cumulative pore volume curves and pore size distribution were calculated from the isotherms by applying an advanced NLDFT method. Transient sorption experiments were performed on a Micromeritics ASAP 2020 instrument with 2,2-dimethylbutane, 2,3-dimethylbutane and n-hexane. The collected data was fitted using a previously reported procedure to obtain the characteristic diffusion timescale R? / D.
[0036] Aluminum speciation was determined from27Al MAS NMR spectra collected at a spinning frequency of 12.5 kHz, pulse of 7i / 12, relaxation delay of 0.8 s, and 4 K scans at 11.7T on a JEOL ECA-500 spectrometer. Total number of acid sites were quantified with temperature-programmed desorption of ammonia (NH3-TPD) in a tubular reactor setup equipped with an online mass spectrometer. Approximately 100 mg of catalyst sample was degassed for 1 hour at 600 °C before being cooled down to 150 °C and exposed to an ammonia flow until the sample was saturated. The sample was then purged with Ar overnight to remove excess and weakly adsorbed ammonia. Finally, the temperature was ramped up to 700 °C at a- 10 -50129690Attorney Docket No.: UNIH-322WO (109293.332) PCT PATENT APPLICATION UHID 2025-050rate of 5 °C min-1while concurrently monitoring the desorbed ammonia with the mass spectrometer. To identify the types of acid sites (i.e., Lewis and Bronsted), pyridine-adsorbed Fourier-transform infrared spectroscopy was conducted. Background spectrum was first collected at room temperature for a high temperature cell equipped with KBr windows using a Nicolet 6700 FTIR spectrometer. Subsequently, approximately 20 mg of sample was pelletized and placed in the cell. The configuration was installed in the spectrometer and connected to heated N2 gas lines (150 °C). The cell was heated to 550 °C for 2 hours to eliminate adsorbed moisture in the sample before being cooled down to 200 °C for the adsorption experiment. A parent spectrum was collected before increment of 1 pl anhydrous pyridine (Sigma Aldrich) was injected into the heated N2 stream (Matheson, 50 cm3min-1). Spectra were collected 5 min after each injection until saturation, and the final spectrum was collected after purging for 2 hours with N2. The subtracted results from the final and parent spectra were analyzed using OMNIC software with peaks assigned to Bronsted and Lewis acid sites at 1545 and 1450 cm-1, respectively. The corrected peak area was used to obtain the percentages of Bronsted and Lewis acid sites.
[0037] Catalytic testing. Methanol-to-hydrocarbon (MTH) reactions were carried out in a A ¼ inch stainless-steel tube installed in a resistively heated furnace (Model 3210, Applied Test Systems). The catalyst bed was supported between two plugs of quartz wool. A K-type thermocouple (Omega Engineering) was inserted into the stainless tube to measure the temperature of the catalyst bed. Prior to the reaction, the catalyst bed was pretreated in situ at 550 °C for 3 hours under the flow of dried air (6 cm3min-1of O2, 24 cm3min-1of N2). The catalyst bed was then cooled to the reaction temperature, 400°C. Methanol was fed by a syringe pump (Harvard Apparatus) into a heated inert gas stream of Ar (Matheson). The methanol flow rate and catalyst amount in the reactor were varied depending on the target w'eight hourly space velocity. Reactor effluent was evaluated using an on-stream gas chromatograph (Agilent GC7890A) equipped with a flame ionization detector.
[0038] Postmortem-coke analysis. A UV-Vis Cary 5000 spectrometer equipped with a diffuse reflectance accessory (Praying Mantis Harrick) was used for recording UV-Vis spectra and BaSO₄ was used as a standard for background measurement. Raman spectra were recorded at ambient temperature with 514 nm excitation on a Renishaw inVia Raman spectrometer equipped with a CCD detector.
[0039] Results and Discussion- 11 - 50129690Attorney Docket No.: UNIH-322WO (109293.332) PCT PATENT APPLICATION UHID 2025-050
[0040] ZSM-23 (MTT) crystals were synthesized according to a reported protocol with modifications made to the growth mixture composition (e.g., increased Na+content), temperature, and time of hydrothermal treatment (see above). Table 1 below shows the various ratios of components used in the growth mixtures and other reaction parameters. These changes were introduced to improve the purity of the final product wherein the same organic structuredirecting agent (OSDA), dimethylformamide (DMF), which is commonly used for MTT synthesis was retained. Another important outcome of the modified synthesis conditions was a reduction in crystal aggregation that is more prevalent when using the original recipe. Powder X-ray diffraction (PXRD) of the as-prepared sample confirmed a fully crystalline MTT product without evidence of the most frequently encountered impurity, quartz.Table 1Growth Mixture Molar Ratio Aging time T TimeTrial Final productDMF SiO2Al2O3NaOH H2O (h) (°C) (d)Predominantly 1a0.55 1 0.014 0.36 29.5 24 185 4quartzPredominantly2 0.55 1 0.014 0.35 29.5 24 185 3quartz3b0.55 1 0.014 0.36 29.5 24 160 4 Magadiite4 0.55 1 0.014 0.25 29.5 24 185 4 MTT5 0.55 1 0.014 0.25 29.5 24 160 4 MTT6C0.55 1 0.014 0.25 29.5 24 160 3 MTT7 0.55 1 0.014 0.25 29.5 24 160 5 MTT8 0.55 1 0.014 0.15 29.5 24 160 3 Amorphous9 0.55 1 0.014 0.15 29.5 24 160 5 Amorphous10 0.55 1 0.014 0.15 29.5 24 185 5 Amorphous a. The recipe from literature yields predominantly quartz, b. A composition similar to the reference using a lower temperature yields a hydrous silicate mineral magadiite. c. Sample used as MTT seeds for the manuscript. In general, lowering the Na⁺ content and pH of the growth mixture promotes the formation of MTT (although there is a threshold below which the precursor is unable to crystallize, leading to an amorphous product).
[0041] FIG. 1 shows transmission electron micrographs and corresponding SAED patterns of MTT zeolite, including (A) Zeolite MTT crystals prepared from a synthesis that- 12 - 50129690Attorney Docket No.: UNIH-322WO (109293.332) PCT PATENT APPLICATION UHID 2025-050yields disperse anisotropic rods, (B) MTT-sg after secondary' growth in a low supersaturation silica solution, with Inset: Higher magnification image of MTT-sg clearly showing the presence of surface roughness on the MTT crystals, indicating the presence of protrusions, (C) Nano¬ sized MTT crystals (MTT-nano) synthesized using a long chain OSDA, SAED patterns of (D) MTT seed, (E) MTT-sg, and (F) MTT-nano. The transmission electron microscope (TEM) images of MTT crystals reveal a rod-like morphology (FIG. 1(A)) with an average length of 1 ± 0.5 μm and -width of 50 ± 5 nm where the 1 -dimensional channels are oriented axially along the longest dimension, the
[0100] direction (FIG. 2(A), below), which imposes more restricted mass transport limitations for internal diffusion. Selected area electron diffraction (SAED) of rod-like MTT particles confirms they are single crystals (FIG. 1(D)).
[0042] FIG. 2 shows (A) MTT framework diagram long the
[0100] zone axis showing the 10-membered ring pore openings. MTT has an orthorhombic crystal structure (Pmmn space group) with unit cell parameters::::0.526, b:::2.20, and c:::1.14 nm, (B) Idealized schematic of a ZSM-23 (MTT) crystal after secondary growth, and (C) Hypothetical roughness on exterior {010} surfaces as a result of secondary' growth in the form of (i) a single unfinished layer with a step height equal to that of the b or c unit cell dimension or (ii) step bunches with heights (h) equal to multiples of the unit cell dimensions.
[0043] The synthesis of relatively uniform, non-aggregated MTT crystals was instrumental to the facile screening of effective secondary' growth procedures for introducing roughened interfaces on the exterior surfaces of parent (seed) crystals. A wide range of secondary' growth conditions were tested as show' n in Table 2 below' to identify an optimal set of parameters that yielded MTT-sg crystals with the anticipation of producing the idealized morphology depicted in FIG. 2(B) with protrusions similar to those observed in previous studies of finned 2D and 3D zeolites.Table 2Growth Mixture Molar Ratio Seed T Time FinalTrial OSDA usedOSDA SiO2Al2O3NaOH H2O wt% (°C) (d) product01Diquat 0.15 1 0.014 0.16 40 10 140 1 B2 Diquat 0.15 1 0.014 0.16 40 10 140 3 C3 DMF 0.55 1 0.014 0.25 29.5 10 140 1 A- 13 - 50129690Attorney Docket No.: UNIH-322WO (109293.332) PCT PATENT APPLICATION UHID 2025-0504 DMF 0.55 1 0.014 0.25 29.5 10 140 3 B5 DMF 0.55 1 0.014 0.25 29.5 10 140 4 C6 DMF 0.55 1 0.014 0.25 50 10 130 3 A7 DMF 0.55 1 0.014 0.25 50 20 130 3 A8 Pyrrolidine 0.45 1 0.014 0.2 45 10 130 1 A9 Pyrrolidine 0.45 1 0.014 0.2 45 10 130 3 A10 Pyrrolidine 0.45 1 0.014 0.2 45 10 140 1 A11 Pyrrolidine 0.45 1 0.014 0.2 45 10 140 2 C12 Pyrrolidine 0.45 1 0.014 0.2 45 15 130 1 C13 Pyrrolidine 0.45 1 0.014 0.2 45 15 140 1 C14 Pyrrolidine 0.45 1 0.014 0.2 90 15 140 1 B15 Pyrrolidine 0.45 1 0.014 0.2 90 15 140 2.75 MTT-sga. Products were defined in three different categories: A = amorphous; B = partially amorphous; C = crystalline but partially dissolved.
[0044] One of the most critical parameters was the selection of an alternative organic, pyrrolidine, which is another commonly reported OSDA for MIT synthesis. Based on the complex mechanisms of zeolite crystallization, the secondary’ growth media must be judiciously designed to promote 3-dimensional growth of protrusions (or surface roughness) without inducing seed dissolution or causing secondary nucleation. In select cases it is necessary’ to switch the OSDA, as previously observed for preparation of finned zeolite FER. When considering classical models of crystallization, highly anisotropic morphologies are the byproduct of disparate growth rates along the principal crystallographic directions. For MTT the fastest growth occurs along the
[0100] direction, resulting in high aspect ratio rod-like crystals w’here the largest surface area corresponds to facets with the slowest growth rate of growth, i.e., the
[0010] and
[0001] directions. These facets exhibit higher barriers for 2-dimensional (2D) nucleation of islands, and thus layer-by-layer growth occurs predominantly in-plane due to infrequent nucleation events. Under these conditions, it w’ould be expected to observe unfinished layers with either single unit cell thickness or step bunches with relatively small step heights, as illustrated in FIG. 2(C). Such features would manifest as surface roughness with less uniformity than the protrusions reported for other finned zeolites.
[0045] The idealized scheme of a MTT-sg crystal after secondary growth shown in FIG, 2(B) supports the motivation for introducing small protrusions on the exterior surfaces of- 14 - 50129690Attorney Docket No.: UNIH-322WO (109293.332) PCT PATENT APPLICATION UHID 2025-050rod-like crystals. Each protrusion is a pseudo nanoparticle on the underlying non-porous interface, thus creating a series of shorter channels for improved mass transport; however, TEM images of seed crystals after secondary' growth show that the exterior surfaces of MTT crystals (FIG. 1(B)) are uncharacteristic of those depicted in FIG. 2(B). On the contrary, surface roughening (FIG. 1(B), inset) is evident in high-magnification TEM images. Powder X-ray diffraction (PXRD) confirmed that secondary' growth resulted in a fully crystalline MTT product, whereas SAED patterns (FIG. 1(E)) indicate there is a small degree of misalignment. Herein, these materials are described by the terminology “secondary growth” (or MTT-sg) to refer to samples possessing a high degree of external surface roughness.
[0046] As a benchmark for assessing the enhance mass transport properties of MTT- sg, a third MTT sample was prepared using a protocol to generate nano-sized (ca, 50 nm) cry stallites, which are referred to as MTT-nano. TEM images (FIG. 1(C)) and PXRD confirmed the synthesis of pure zeolite MTT as aggregates of nano-sized crystallites (FIG. 1(C), inset). The polycrystallinity of this sample is evident in SAED analysis (FIG. 1(F)), which produces a diffuse diffraction pattern. The physicochemical properties of all three samples in proton form (H-ZSM-23) are compared in Table 3 below'. All samples have comparable compositions (Si / Al = 35 - 42) with nearly equivalent total acidity (Cacid) from NHs temperature programmed desorption (TPD) and roughly the same percentage of Bronsted acid sites (BAS) determined from pyridine infrared (IR) analysis. Textural analysis of N₂ adsorption / desorption data reveals that samples without secondary' growth (MTT and MTT-nano) exhibit relatively low micropore volume (Vmicro) compared to the sample after secondary growth (MTT-sg), which also exhibits higher BET and external surface areas.T able 3SampleH-MTT 121 53 0.07 42 103 42 0.09H-MTT- 388 136 0.10 38 135 42 0.04 0.7 3.0 sgH-MTT- 264 126 0.06 35 112 54 0.03nanoaBET and external surface areas (SA) and micropore volume (Vmicro) from N₂ physisorption;bElemental analysis of bulk crystal by EDS:cTotal acid site concentration (Cacid) from NH₃-TPD; " Bronsted acid site (BAS) percentage from pyridine-IR;eDiffusion measurements using probe molecules (I) n-hexane, (II) 2,3- 15 - 50129690Attorney Docket No.: UNIH-322WO (109293.332) PCT PATENT APPLICATION UHID 2025-050dimethylbutane, and (III) 2,2 dimethylbutane.
[0047] A previously reported protocol was used for evaluating the mass transport property of each sample. In this study three probe molecules of vary ing kinetic diameter were selected: n-hexane (I: 4.3 A), 2,3-dimethylbutane (II: 5.8 A), and 2,2-dimethylbutane (III: 6.2 A). Time-resolved uptake measurements were performed to estimate the mass transport parameter R² / D (Table 3), where R is a characteristic dimension of the crystals and D is an effective diffusivity. Dimethylbutanes are commonly used to probe diffusion in medium-pore zeolites (e.g., MFI), interestingly, these molecules could not effectively access the pores of both as-synthesized materials (MTT and MTT-nano), whereas they could diffuse through MTT-sg crystals (Table 1), Tire least sterically hindered (linear) isomer, n-hexane, could access all three samples, similar to N2 used for textural analyses. The corresponding R² / D values for MTT-sg and MTT-nano are comparable and significantly smaller than that of the MTT sample, which indicates secondary growth of the seed crystal results in an enhanced material with mass transport properties equivalent to nano-sized crystallites. The inaccessibility of select probe molecules also suggests there are defects in as-synthesized MTT materials, discussed below'.
[0048] FIG. 3 shows high-resolution transmission electron microscopy (HR-TEM) images of (A) MTT (seed) and (B - D) MTT-sg samples. The boxes in FIG. 3(B) highlight regions of apparent disorder (or lower resolution) that could be attributed to a structural characteristic of the underlying seed crystal or an overgrowth on the exterior surface. Tire slight degree of secondary growth misorientation is indicated in FIG. 3(C) and FIG. 3(D) with the lines and labelled angles between lattice fringe orientations in the seed and protrusion. All scale bars equal 10 nm.
[0049] High-resolution transmission electron microscopy' (HR-TEM) images of the MTT seed crystal (FIG. 3(A)) show a perfectly crystalline material with lattice fringes in the a-direction (parallel to the straight channels) and an atomically smooth exterior {010} surface. HR-TEM images of MTT-sg crystals after secondary' growth (FIG. 3(B) - (D)) reveal features similar to step bunches illustrated in FIG. 2(C), There are no apparent defects in the images of MTT seed crystals; however, there are regions within the HR-TEM images of MTT-sg crystals that are seemingly less ordered (FIG. 3(B), boxes). The exact nature of these regions is unknown but could potentially be defects in the crystal structure or areas of overgrowth (regions of surface protrusions) on the top surface that manifest as irregularities in the 2-dimensional projection of the 3D crystal. HR-TEM images also confirm the slight- 16 - 50129690Attorney Docket No.: UNIH-322WO (109293.332) PCT PATENT APPLICATIONUHID 2025-050misorientation of unfinished layers during secondary growth that can result in protrusions with 1 - 10 degree shifts in their crystallographic registry relative to that of the underlying seed crystal (FIG. 3(C), (D)). This is consistent with the slight broadening of electron diffraction patterns for MTT-sg samples (FIG. 1(E)). It should be emphasized, however, that this small degree of misorientation does not significantly block straight channels in the protrusions, thus providing numerous regions on the exterior surfaces of seed cry sials with substantially shorter pathlengths for molecular diffusion.
[0050] Without being bound by theory’, there are several possibilities for the observed increase in micropore volume, Vmicro, after secondary growth. The low value for MTT seed crystals suggests defects. There are several possibilities for defects before and after secondary growth. Textural and diffusion analyses presented in Table 1 indicate that these defects are of two forms: (i) partially-blocked pores that grant access to n-hexane but not its larger isomers; and (ii) fully-blocked pores that render select regions of the seed crystal inaccessible to nitrogen. Pore blockage in zeolite seed crystals could be related to defects in the framework (e.g., silanol groups or framework-associated aluminum sites), extra-framework species, or residual amorphous material. It is not well understood exactly how intrinsic defects within seed crystals are either removed or altered by the secondary growth procedure. Framework defects could either be annealed or dissolved. The latter could either result in the generation of interchannel micropores or channel defects. Removal of extra-framework species or residual amorphous material can result in the restoration of a pristine ID channel. Alternatively, multiple defects within proximity of each other could potentially lead to localized dissolution and the formation of mesopores. Defect removal or formation can be facilitated by the secondary growth mixture, which has the potential to induce dissolution and reprecipitation within the seed crystal in addition to the generation of external surface features.
[0051] The nature of defects was probed by argon adsorption and HR-TEM. FIG. 4 shows Ar adsorption / desorption isotherms for H-form seeds (H-MTT) and the sample after secondary growth (H-MTT-sg). Argon adsorption / desorption profiles for MIT and MTT-sg samples (FIG. 4) do not exhibit signatures of internal mesopores. The hysteresis observed in the MTT-sg profile at high relative partial pressure is more indicative of interparticle voids. This is anticipated since the secondary treatment protocol involves the use of a supersaturated aluminosilicate solution, which differs from methods reported in literature where postsynthesis treatments employ either acids or bases (i.e., undersaturated solutions) to partially- 17 - 50129690Attorney Docket No.: UNIH-322WO (109293.332) PCT PATENT APPLICATION UHID 2025-050dissolve ZSM-23 crystals for the strategic introduction of mesopores. HR-TEM images of MTT and MTT-sg samples (FIG. 3) do not contain explicit evidence of full / partial pore blockage, or any defect features postulated after secondary growth. This does not negate the possibility of their existence. For example, the presence of residual amorphous material may be too small to detect by HR-TEM or alternative techniques, such as PXRD. Moreover, FTIR analysis of samples before and after secondary growth show little evidence of changes in silanol species (vide infra). As previously discussed, there are less ordered regions within HR-TEM images (FIG. 3(B)) that might be associated with channel defects; however, these features are only observed for MTT-sg samples and are not fully resolved. Collectively, the exact nature of defects before and after secondary growth remain elusive.
[0052] Solid-state27Al NMR spectra of all three samples (MTT, MTT-sg, and MTT-nano) revealed the presence of tetrahedrally-coordinated framework Al sites without any evidence of octahedral extra-framework species. Solid-state Fourier transform infrared spectroscopy (FTIR) showed no significant difference in the regions corresponding to silanol groups before and after secondary' growth. Collective deduction of all characterization data presented thus far suggests that the most likely cause for the dramatic increase in BET surface area and Vmicro after secondary' growth is the removal of amorphous material. This also highlights a more general benefit of the secondary growth procedure, w hich is the opening of inaccessible pores in the parent crystal. To this end, a literature survey of ZSM-23 (MTT) materials reported in prior studies was conducted to determine the range of Vmicro values as a function of their Si / Al ratio. FIG. 5 shows micropore volumes of ZSM-23 samples found in literature compared with samples MTT and MTT-sg. Dotted lines are the medians demarcating the boundaries between micropore volumes above and below 0.065 cm3 / g, and compositions (Si / Al ratio) above and below' 50. Triangles represent each data point from literature data. The majority of materials exhibit values less than 0,07 cm3g’1with a surprisingly large fraction reported with values less than 0,03 cm3g’1. Tire Vmicro of MTT-sg is one of the highest reported in literature, with only one case of a more siliceous MTT exhibiting a higher value. One of the most compelling outcomes of the literature survey' is the extensive range of micropore volumes, which suggests defects are a characteristic feature of the one-dimensional MTT structure; however, the exact nature and diversity of these defects remain elusive.
[0053] The methanol-to-hydrocarbon (MTH) reaction w'as used to assess the relative performance of the three MTT samples. MTH is commonly used as a benchmark reaction for- 18 - 50129690Attorney Docket No.: UNIH-322WO (109293.332) PCT PATENT APPLICATION UHID 2025-050probing the extent of mass transport limitations in zeolite catalysts; however, highly restricted diffusion in ID zeolites is typically nonideal for MTH reactions due to rapid inaccessibility of pores as a result of coking, which often necessitates the use of uncharacteristic reaction conditions, such as higher temperatures or much longer contact times (i.e., smaller weight- hourly space velocity, WHSV), to extend catalyst lifetime. For catalyst testing a nominal temperature of 400 °C and a WHSV of 4 h-1was used. Each catalyst was prepared by a reported protocol for converting as-synthesized samples to their respective proton forms (H-ZSM-23) by ion-exchange and calcination (discussed above).
[0054] FIG. 6 shows (A) results of the methanol to hydrocarbon (MTH) reaction at 400 °C comparing the performance of H-MTT-sg (circles), parent seed H-MTT (squares), and H-MTT-nano (triangles). Weight-hourly space velocity (WHSV) of 4 h"!was used for H-MTT and H-MTT-nano, whereas it was increased to 7 h’1for H-MTT-sg to achieve approximately similar initial activity. Lines are interpolated to guide the eye. FIG. 6 also shows (B) product selectivity (bar graphs) for all three MTT catalysts along with H-ZSM-5 (Si / Al 40) at initial conversion in methanol to hydrocarbon (MTH) reaction at 400 °C.
[0055] As seen in FIG, 6(A), the seed (H-MTT) exhibited instantaneous and rapid deactivation upon exposure to the reactant feed, whereas the H-MTT-nano also immediately deactivated but with a rate that was 2-times slower than that of the seed at identical reaction conditions. The H-MTF-sg catalyst, on the other hand, exhibited markedly higher catalyst stability with 100% conversion achieved for more than 10 hours time-on-stream (TOS) before the onset of deactivation. In order to compare product selectivity at similar (subcomplete) conversion, the contact time was decreased (WHSV = 7 h’]), which initiated catalyst deactivation at earlier TOS, consistent with the other two catalysts. Even at reduced contact time, the rate of H-MTT-sg deactivation was markedly slower (FIG. 6A) than either H-MTT or H-MTT-nano. Comparisons were also made on the basis of turnover number, which normalizes the rate of methanol consumption by the total number of Bronsted acid sites (i.e., Cacid multiplied by the product of catalyst mass and percent BAS, Table 1). H-MTT-sg had a 5-fold higher turnover number compared to the other two catalysts that each exhibited relatively similar values.
[0056] The product selectivities listed in FIG. 6(B) compare the results of MTH reaction at early TOS (ca. 10 minutes). The methane generated over H-MTT catalyst was nearly 40%, which is expected on the basis of its rapid deactivation. A similar outcome was observed- 19 - 50129690Attorney Docket No.: UNIH-322WO (109293.332) PCT PATENT APPLICATION UHID 2025-050for H-MTT-nano but after longer TOS. Both of these catalysts exhibited the lowest quantity of light olefins (i.e., ethene, €2=, and propene, €3=) compared to H-MTT-sg. For comparison, the results of a H-ZSM-5 (MFI) catalyst (cs. 500 nm) synthesized with a similar Si / Al ratio as the ZSM-23 samples were included. The H-MTT-sg and H-ZSM-5 catalysts produced similar yields of light olefins, but the ratio of C₃= / C₂= was larger for H-MTT-sg (ca. 5.0) compared to H-ZSM-5 (ca. 2.4). One additional feature of the H-MTT-sg catalyst was a slightly higher fraction of C₄⁺ olefins. When comparing MTT- and MFI-type zeolites, the presence of sinusoidal channels in the latter creates additional mass transport limitations that promotes the aromatic cycle of the hydrocarbon pool mechanism. This leads to a larger fraction of aromatic products in H-ZSM-5 compared to all H-ZSM-23 catalysts. This also explains the higher ethene content for H-ZSM-5, which is a byproduct of the aromatic cycle.
[0057] Prior studies of MFI-type zeolite have shown that the aromatic cycle is promoted in larger cataly sts owing to the increased residence times of reactants and products. The presence of sinusoidal channels in zeolite MFI creates additional mass transport limitations, whereas the intersections between straight and sinusoidal channels are larger voids that putatively facilitate the formation of aromatics. Zeolite MTT lacks sinusoidal channels and pore intersections, but does exhibit long straight channels that are more susceptible to coking and pore blockage, The rapid deactivation of H-MTT (seed) produces aromatics as coke that remain on the catalyst with relatively less aromatics generated in the reactor product stream. Secondary growth of H-MTT-sg leads to a more "‘open” structure that produces a higher aromatics yield, but less than that of ZSM-5.
[0058] The nature of the carbon structures in both deactivated H-MTT materials was evaluated by Raman and UV-Vis spectroscopies, Raman spectroscopy reveals the appearance of similar signals for both deactivated MTT materials, mainly centered between 1200 and 1700 cm-1, which have been assigned in literature to polyaromatic species. It is worth noting that similar signals were observed by Raman spectroscopy for other deactivated 1-D medium pore zeolites (e.g. TON) after their application as catalysts for the MTH reaction. For the UV-Vis data, different bands occur within the UV (250-330 nm) and visible (330-850 nm) regions. Tire bands below 400 nm have been ascribed to cations of monocyclic aromatics or polyenes, while the bands above 400 nm correspond to cationic or neutral polycyclic aromatics. Both materials exhibit similar UV-Vis spectrum profiles above 400 nm, suggesting the formation of analogous bulky carbonaceous species after the MTH reaction, thus indicating a similar deactivation-20 -50129690Attorney Docket No.: UNIH-322WO (109293.332) PCT PATENT APPLICATION UHID 2025-050profile by coke formation for both catalysts, in good agreement with the Raman spectra; however, there are some notable differences, such as the aspect ratio between bands below and above 400 nm, corresponding to the formation of smaller and bulkier carbonaceous species, respectively. This observation could be attributed to the improved diffusional pathways of the sample after secondary growth (H-MTT-sg), which is expected to decrease the rate of coke formation and putatively explains the extended catalyst lifetime (FIG. 6(A)) compared to its parent material (H-MTT).
[0059] In summary, a secondary growth procedure was used to introduce roughened exterior surfaces on a 1 -dimensional MTT zeolite. Large surface area facets of highly anisotropic crystals typically have high energetic barriers for nucleation, which is likely the reason for MTT surfaces exhibiting less uniform, rough features compared to more defined protrusions on finned zeolites reported previously. Secondary growth of MTT seed crystals creates a distribution of unfinished layers on exterior surfaces that possess much shorter diffusion path lengths (10 - 50 nm) compared to the ID pores of the seed crystal (1 pm); however, this procedure also appears to remove intrinsic defects in as-synthesized MTT crystals, resulting in reduced mass transport limitations (e.g., MTT-sg sample). This is reflected in an approximate 45% increase in micropore volume, reaching a value of 0.10 cm3 / g that is significantly higher than most ZSM-23 catalysts reported in literature (particularly those with Si / Al ratios less than 50). Secondary growth seems to remove a majority of defects that either fully or partially block access to micropores in the seed crystal. Here we propose several possibilities of defects and features resulting from secondary growth; however, the exact nature of these species is elusive despite attempts to characterize them by several high-resolution techniques, such as HR-TEM, solid-state NMR, and FTIR.
[0060] Structure-performance relationships for MTT, MTT-sg, and MTT-nano materials were established using the MTH reaction at 400°C as a benchmark for assessing differences in catalyst activity and selectivity. The MTH reaction is not commonly used with ID zeolites owing to their rapid deactivation at short methanol contact times. The enhanced mass transport properties of MTT-sg significantly improve its catalyst lifetime, enabling high methanol conversion to be sustained over much longer time on stream compared to the parent MTT catalyst as well as the current state-of-the-art nanosized material (MTT-nano). Secondary growth resulted in a higher activity of MTT-sg catalysts at shorter contact times (i.e., much higher turnover number). MTT is often used as a surrogate for studying diffusion or reactions- 21 - 50129690Attorney Docket No.: UNIH-322WO (109293.332) PCT PATENT APPLICATION UHID 2025-050in the straight channel of the MFI framework (3D zeolite) owing to the absence of sinusoidal channels and channel intersections in the ID analogue. Here, the catalytic performance of MTT-sg was compared to a conventional ZSM-5 catalyst synthesized with similar Si / Al ratio. Interestingly, the straight channel of MTT results in much higher propene / ethene product selectivity with reduced aromatics yield in comparison to the results with the ZSM-5 catalyst. Although the total turnovers over the 3D zeolite are higher, this work demonstrates generating a 1 D zeolite that is a promising alternative for tailored product distributions without markedly sacrificing catalyst lifetime. This level of catalytic performance in the MTH reaction has not been reported for a ID zeolite. The effects observed for secondary growth of MTT may be generalizable to other ID zeolite frameworks (e.g., MTW, TON, MOR, etc.), or epitaxial growth may lead to protrusions that are more characteristic of those observed in finned 2D (e.g., FER) and 3D (e.g., MFI, MEL) zeolites.EXAMPLE 2.
[0061] Experimental Methods and Materials.
[0062] Materials. The following chemicals for zeolite synthesis were purchased from Sigma Aldrich: LUDOX AS-40 (40 wt% suspension in water), LUDOX SM-30 (30 wt% suspension in water) sodium aluminate (57.1% AI2O3 and 37.2% Na2O), sodium hydroxide solution (50 wt% in -water), methyltriethylammonium chloride (MTEAC1, 97%), tetraethylammonium hydroxide solution (TEAOH, 35 wt%), and tetraethylammonium bromide (TEABr, 98%). Deionized (DI) water was produced with an Aqua Solutions RODI-C-12A purification system (18.2 M ). All reagents were used as received without further purification. For reaction testing, methanol was purchased from J. T. Baker (99.8%), and the argon, oxygen, and nitrogen gases were purchased from Praxair with UHP grade (99.999%).
[0063] Synthesis of MTW seed crystals: The ZSM-12 sample used as seeds was prepared with a molar composition of 60 MTEAC1: 10 Na₂O: 100 SiO₂: 1 Al₂O₃: 5555 H₂O. Silica source used was Ludox AS-40. The mixture was stirred at room temperature for 24 h. The sol gel was then placed in a 30 ml Teflon-lined acid digestion bomb and heated in an oven at 160 °C for 6 days. MTW crystals with Si / Al=30 was prepared using a growth solution of composition of 15 MTEAC1: 4.5 Na₂O: 100 SiO₂: 1.7 Al₂O₃: 2000 H₂O. The sol gel was then placed in a 30 ml Teflon-lined acid digestion bomb and heated in an oven at 160 °C for 7 days. The crystalline products were removed from the mother liquor by three cycles of centrifugation- 22 - 50129690Attorney Docket No.: UNIH-322WO (109293.332) PCT PATENT APPLICATION UHID 2025-050and washes with deionized water, using a Beckman Coulter Avanti J-E centrifuge at room temperature and 6,000 rpm for 10 min per cycle. The resulting seeds were immediately stored in deionized water without allowing time for the solids to dry.
[0064] Seed directed secondary growth on MTW: A growth solution was prepared with a molar composition of 28 TEAOH: 1 Na₂O: 100 SiO₂: 1 Al₂O₃: 2500 H₂O. Silica source used was Ludox AS-40. The mixture was stirred at room temperature for 24 h. The prepared conventional MTW seed was added to this solution at 15% by weight of the solution and placed in a 30 ml Teflon-lined acid digestion bomb and heated in an oven at 110 °C under rotation and autogenous pressure for 3 days. The MTW-30 seed was added to the same growth solution at 10% by weight of the solution and placed at 110 °C under rotation and autogenous pressure for 3 days. Similar to the seed crystals, the crystalline product was removed from the mother liquor by three cycles of centrifugation and washes with deionized water, using a Beckman Coulter Avanti J-E centrifuge at room temperature and 6,000 rpm for 10 min per cycle.
[0065] Seed directed secondary growth on MOR: A growth solution was prepared with a molar composition of 2.64 TEABr: 5 Na₂O: 13 SiO₂: 1 Al₂O₃: 1000 H₂O. Silica source used was Ludox SM-30. The mixture was stirred at room temperature for 24 h. The zeolyst MOR sample was added to this solution at 5% by weight of the solution and placed in a 30 ml Teflon-lined acid digestion bomb and heated in an oven at 110 °C under rotation and autogenous pressure for 1 day. Similar to the seed crystals, the crystalline product was removed from the mother liquor by three cycles of centrifugation and washes with deionized water, using a Beckman Coulter Avanti J-E centrifuge at room temperature and 6,000 rpm for 10 min per cycle.
[0066] The centrifuged samples were dried at room temperature in air and then calcined in a muffle furnace at 550 °C using heating and cooling rates of 1 °C min⁻¹ for 10 h (MOR) and 12 h (MTW).
[0067] Material characterization: Powder X-ray diffraction (PXRD) patterns of dried solids were collected on a Rigaku SmartLab diffractometer with a Cu Ka source (40 kV, 30 mA). A ThermoFisher Axia ChemiSEM was used to obtain scanning electron microscopy (SEM) images and electron dispersive X-ray (EDX) spectroscopy using 15 kV and a 15 mm working distance. Textural analysis was. performed with a Micromeritics 3Flex instrument- 23 - 50129690Attorney Docket No.: UNIH-322WO (109293.332) PCT PATENT APPLICATION UHID 2025-050using N2 as a probe gas for physisorption. Surface area was calculated from the BET isotherm and micropore volume was estimated by the t-plot method. Transient sorption experiments were performed on a Micromeritics ASAP 2020 instrument with 2,2-dimethylbutane, 2,3- dimethylbutane, and n-hexane. The collected data was fitted using a previously reported procedure to obtain the characteristic diffusion timescale R2 / D.
[0068] Results and Discussion
[0069] ZSM-12 (MTW-type) zeolite crystals were synthesized following a previously reported hydrothermal method using methyltriethylammonium chloride (MTEAC1) as the OSDA, yielding phase-pure material with high crystallinity as confirmed with powder X-ray diffraction (PXRD) in FIG. 7(A). FIG. 7 shows PXRD patterns of zeolite (A) MTW and (B) MOR crystals. FIG. 8 shows scanning electron micrographs of (A) Zeolite MOR crystals purchased from Zeolyst, (B) Modified MOR after secondary growth (MOR-sg) synthesized in a low supersaturation aluminosilicate solution, (C) MTW crystals synthesized using a MTEA⁺ as an OSDA yielding disperse rice-grain morphology, and (D) Modified MTW (MTW-sg) exhibiting a hierarchical intergrowth structure.
[0070] Scanning electron microscopy (SEM) images revealed the formation of elongated crystals in agglomerates (FIG. 8), with axial particle dimensions extending beyond several micrometers, ZSM-12 is typically difficult to crystallize with a high quantity of Al using most conventional OSDAs; however, in this work ZSM-12 crystals with a Si / Al ratio of 30, hereafter referred to as MTW-30 seed, were also synthesized by modifying the growth solution composition and growth conditions. Zeolite MOR was purchased from Zeolyst International (CBV 10A) and used as received.
[0071] A set of secondary' growth conditions w'as evaluated. The treatment was done in a low supersaturation aluminosilicate solution. The secondary growth temperature, and the choice of OSDAs proved particularly critical in controlling the outcome of the treatment. For MTW, tetraethylammonium hydroxide (TEAOH) was employed as the OSDA, and for MOR, tetraethylammonium bromide (TEABr) was utilized. The samples after secondary growth are labelled MTW-sg and MOR-sg (where “sg” refers to secondary growth) in FIG. 7(A) and 7(B). Reference patterns w'ere obtained from the International Zeolite Association Structure Database.
[0072] SEM images and PXRD patterns revealed that the structural integrity of both- 24 - 50129690Attorney Docket No.: UNIH-322WO (109293.332) PCT PATENT APPLICATIONUHID 2025-050zeolites was retained following secondary growth. In the case of MOR, the morphology remained largely intact, with individual crystals appearing less agglomerated and more dispersed compared to the untreated sample, suggesting improved accessibility and reduced particle clustering. For ZSM-12, the characteristic rice-grain morphology synthesized using MTEA as the OSDA was preserved; however, crystals after post-treatment exhibited a more complex hierarchical intergrowth structure, indicative of surface recrystallization or overgrowth processes for both materials prepared with Si / AI molar ratios of 50 and 30.
[0073] The modified ZSM-12 and MOR crystals exhibited a marked enhancement in porosity, as confirmed by N2 physisorption measurements shown in Table 4 below. For MTW, it is well-documented that the use of methyltriethylammonium (MTEA) as the structure- directing agent, as was used here to prepare seed crystals, yields crystals with relatively low micropore volume, due to its bulky nature and limited efficiency as an OSDA. In contrast, tetraethylammonium (TEA) is preferred not only for its cost-effectiveness but also for its ability to produce MTW crystals with higher microporosity. However, the choice of OSDA strongly influences crystal morphology as well. When TEAOH or TEABr is used as the ODSA, ZSM- 12 typically forms sheet-like agglomerates with quasi-cubic or elliptical morphology and diameters in the range of 500-900 nm. In contrast, MTEA-directed synthesis favors the formation of rice-like agglomerates with elongated particles exceeding 1 pm in dimension along the axial direction. Here, it was shown that the rice-like morphology can be preserved while enhancing microporosity with carefully tailored secondary treatment, enabling both structural retention and textural improvement. For zeolite MOR, the secondary growth procedure converted portions of micropore volume into accessible mesoporosity, without the need for harsh acid or base leaching steps and without significant dealumination, as confirmed by elemental analysis.Table 4 Physicochemical properties of zeolite MTW and MOR samples.Sample BET SAAExt SAA(m2 / g) (m2 / g)MTW seed 126 80 0.04 0.23 48 0.3 0.85MTW-sg 288 96 0.12 0.26 46 0.2 0.65MTW-30 seed 209 63 0.06 0.19 20MTW-30-sg 293 98 0.08 0.25 29 — —- 25 - 50129690Attorney Docket No.: UNIH-322WO (109293.332) PCT PATENT APPLICATION UHID 2025-050MOR seed 438 37 0.16 0.09 6.5 0.08 0.20MOR-sg 278 56 0.10 0.31 7.6 0.04 0.073Surface areas (SA) and pore volumes (Vi) for micropores and mesopores from N₂ physisorption;bElemental analysis of bulk crystal from EDS;cMeasured from n- hexane uptake;dMeasured from 2,3 dimethylbutane uptake.
[0074] The diffusion properties of both materials were evaluated using rate-of-uptake experiments with isomers of w-hexane as probe molecules (Table 4). Diffusion coefficients were extracted by fitting the uptake curves using a previously reported protocol and are presented as R2 / D values where R is an effective radius (or average dimension) and D is the effective diffusivity of the probe molecule. Notably, the modified samples showed significantly faster uptake rates compared to their as-synthesized or as-purchased counterparts. While n-hexane and 2,3-dimethylbutane are typically employed to probe molecules to assess transport in medium-pore 3D frameworks such as zeolites MFI and MEL, their relatively small kinetic diameters (~4.3 A and 5.6 A, respectively) should not be sterically hindered in large-pore zeolites like zeolites MTW and MOR. Thus, the observed enhancements in diffusion coefficients suggest the presence of substantial intracrystalline transport barriers — likely associated with defects or partially blocked channels — that are alleviated following the secondary growth treatment. These results confirm that improving pore accessibility, even in nominally large-pore systems, is crucial to unlocking their full catalytic potential.- 26 - 50129690
Claims
Attorney Docket No.: UNIH-322WO (109293.332) PCT PATENT APPLICATION UHID 2025-050WHAT IS CLAIMED IS:
1. A method for secondary treatment of low-dimensional zeolites to enhance pore volume and diffusivity, comprising:preparing a secondary growth solution for modification of low-dimensional zeolite seed crystals, wherein the secondary growth solution comprises framework source precursors, one or more structure-directing agents, and a hydroxide source, wherein the framework source precursors comprise a silica source and an alumina source, wherein the secondary growth solution has a molar composition ratio of the silica source to the alumina source of about 20 to about 100, wherein the secondary’ growth solution has a molar composition ratio of the framework source precursors to w'ater of about 0.001 to 0.05 or less, wherein the secondary growth solution has a molar composition ratio of the framework source precursors to the structure directing agents of about 0.04 to 5, and wherein the secondary growth solution has a molar composition ratio of the framework source precursors to the hydroxide source of about 0.05 to 100;adding the low-dimensional zeolite seed crystals to the secondary growth solution in an amount of about 5 to about 20 weight percent of the secondary growth solution to produce a seeded growth solution, wherein the zeolite seed crystals are MTT, MTW, or MOR framework types; heating the seeded growth solution to a temperature of about 100°C to about 140°C for about 1 to 3 days, to produce modified zeolite seed crystals in the seeded growth solution;quenching the seeded growth solution to room temperature to produce a final growth solution; andisolating modified zeolite crystals from the final growth solution, wherein the modified zeolite crystals have enhanced pore volume and diffusivity relative to the zeolite seed crystals.
2. The method of claim 1, wherein the framework source precursors are selected from sodium silicate, tetraethylorthosilicate, colloidal silicate, fumed silica, SiO₂,, aluminum sulfate, aluminum hydroxide, AI2O3, and combinations thereof.- 27 - 50129690Attorney Docket No.: UNIH-322WO (109293.332) PCT PATENT APPLICATION UHID 2025-0503. The method of claim 1, wherein the one or more structure-directing agents are inorganic, organic, or a combination thereof,4. The method of claim 1, wherein the one or more structure-directing agents are selected from pyrrolidine, dimethylformamide, tetraethylammonium hydroxide, 1,8-diaminooctane, cyclohexylamine, tetrabutylammonium hydroxide, and combinations thereof.
5. The method of claim 1, wherein the hydroxide source is Na₂O or K₂O.
6. The method of claim 1, wherein the silica source is SiO₂ and the alumina source is Al₂O₃.
7. The method of claim 1, wherein the secondary growth solution has a molar composition ratio of the framework source precursors to the one or more structure directing agents of about 1 to 3.
8. The method of claim 1, wherein the secondary growth solution has a molar composition ratio of tire framework source precursors to the hydroxide source of about 4 to 5.
9. The method of claim 1, wherein the secondary growth solution has a molar composition ratio of the silica source to the alumina source of about 70 to 75.
10. The method of claim 1, wherein the secondary growth solution has a molar composition ratio of the framework source precursors to water of about 0.01 to 0.02.
11. The modified zeolite crystals prepared by the method of claim 1- 28 - 50129690