Aluminum-manganese intermetallic compound and preparation method thereof
Through vacuum induction furnace smelting and ball milling processes, the manganese content and purity of the aluminum-manganese intermediate alloy are improved, and the problems of low manganese content and difficult to remove Fe impurities in the prior art are solved, thereby achieving low-cost and efficient aluminum alloy production.
Patent Information
- Application Number
- CN202411138503.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-26
AI Technical Summary
The existing aluminum-manganese intermediate alloy has a low manganese content, high production costs, and is prone to oxidation and aluminum volatilization when melted by non-vacuum induction furnaces, resulting in reduced purity and difficult removal of Fe impurities.
Al8Mn5, aluminium-manganese intermediate alloy is melted by a vacuum induction furnace, and heat, stir, cast, crush and ball mill in a vacuum induction furnace through high-purity aluminum ingots and high-purity electrolytic manganese sheets. KCl or NaCl is used as a cover agent and filled with high-purity argon. Gas protects it to reduce Fe impurities.
The content of manganese in aluminum alloy is significantly improved, production costs are reduced, the purity and corrosion resistance of aluminum alloy are improved, the process flow is simplified, and the effective removal of Fe impurities is achieved.
Smart Images

Figure CN119020629A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of aluminum alloy smelting master alloy, in particular to an aluminum-manganese intermetallic compound and a preparation method thereof. Background Art
[0002] Adding an appropriate amount of manganese to aluminum alloys can not only improve the mechanical properties of the alloy, but also increase the recrystallization temperature of the aluminum alloy, reduce the embrittlement of the iron-containing phase, and neutralize the adverse effects of iron in the aluminum alloy. Usually in the production process of aluminum alloys, manganese is mostly added in the form of aluminum-manganese master alloys to achieve the required chemical composition; on the other hand, impurity iron elements are inevitably mixed in the production process of electrolytic aluminum, which causes the embrittlement of the aluminum alloy and greatly reduces the corrosion resistance. In the alloying process of aluminum, a high content of aluminum-manganese master alloy should be added to reduce the iron content.
[0003] The so-called aluminum-manganese master alloy is an intermediate transition alloy used to adjust the alloy composition in the production of aluminum alloy casting, which is composed of aluminum and manganese. At present, the most widely used master alloy on the market is AlMn10, whose chemical composition implements the standards of YS / T282-2000 and GB / T 27677-2017, in which the content of manganese element is 9.0-11.0wt.%. However, the manganese content of the master alloy is low, which makes the input amount large and the production cost increased, and it can no longer meet the needs of the industry. As an important alloying element, it is hoped that the content of the main element manganese in the aluminum-manganese master alloy added can be as high as possible under the premise of ensuring the demand for manganese element, thereby reducing the input and use amount of aluminum-manganese content, achieving the purpose of reducing costs, and reducing the content of harmful impurity iron, thereby improving product quality. Therefore, the development of an aluminum-manganese master alloy with a high manganese content has become an industry development trend.
[0004] At present, the production of aluminum-manganese master alloys mostly uses medium-frequency or industrial-frequency induction furnaces for smelting. This type of production has the advantage of a high degree of alloy Al homogenization, but has the disadvantages of low labor productivity, high energy consumption, and high production costs.
[0005] Through searching, it was found that: Application No. 201710036862.3 published "An aluminum-manganese two-element master alloy and its preparation method". The alloy was heated and melted in a non-vacuum induction furnace, and the furnace temperature was heated to 1700℃. After the charge was melted, the temperature was maintained at 1600℃, and it was boiled for 10-15 minutes to allow the charge to melt and mix evenly, and then cast to obtain an aluminum-manganese two-element master alloy ingot. The obtained aluminum-manganese two-element master alloy ingot was dried, crushed after drying, and then the aluminum-manganese two-element master alloy with qualified particle size was screened out. However, this master alloy is mainly used for the smelting production of TiAl alloy, and is smelted in a non-vacuum induction furnace. The aluminum-manganese master alloy is easily oxidized to form oxide inclusions. When it is kept at 1600℃ for a long time, the aluminum element is easy to volatilize, resulting in a greatly reduced yield.
[0006] Application publication number CN110241342A introduces a high manganese content aluminum-manganese master alloy and a preparation method thereof. The patent adopts a medium frequency induction heating furnace. The technical problem to be solved is that the manganese content of the existing aluminum-manganese master alloy is low, the production cost is high, and the melting point of the high manganese content aluminum-manganese master alloy is too high, which is inconvenient to use. However, when heating in a medium frequency induction furnace, aluminum is easily oxidized to form inclusions, which affects the purity of the obtained aluminum-manganese master alloy, and further affects the efficiency of subsequent aluminum alloy smelting and the effect of removing Fe impurities.
[0007] Application publication number CN114985745A introduces a preparation method and application of an aluminum-manganese intermetallic compound. The preparation method comprises the following steps: smelting in an electric arc furnace protected by high-purity argon (99.99%), crushing the obtained alloy ingot into coarse powder with a particle size of less than 0.5 mm, and using ethanol as a protective agent, milling the alloy coarse powder for 10-20 hours using a planetary ball mill under the experimental conditions of a mass ratio of zirconium oxide to coarse powder of 15:1 and a rotation speed of 400 r / min, to obtain an aluminum-manganese intermediate alloy powder with an average particle size of 3 μm. However, the patent adopts an electric arc furnace for smelting, and the temperature of the electric arc furnace is difficult to control and the temperature rises too fast. It is generally used for the smelting of steel. In addition, the patent selects zirconium oxide balls in the ball milling process at a high cost, and the protective agent ethanol is volatile and has a poor cooling effect.
[0008] High-quality aluminum alloys generally require Fe content below 0.4wt.%, such as high-speed rail box aluminum welding wire SAL5087, and SAL2319 requires Fe content to be controlled below 0.3wt.%. The aluminum-manganese alloys provided by the above patented methods cannot better remove or effectively reduce the Fe impurity element in the aluminum alloy. Summary of the invention
[0009] The purpose of the present invention is to provide an aluminum-manganese intermetallic compound and a preparation method thereof. The aluminum-manganese intermediate alloy Al8Mn5 is smelted in a vacuum induction furnace. It not only contains a high content of Mn elements, but also can significantly reduce the Fe impurity elements in the aluminum alloy. The preparation process has low production cost and is simple and easy to control.
[0010] In order to achieve the above object, the present invention adopts the following technical solutions:
[0011] The present invention provides a method for preparing an aluminum-manganese intermetallic compound, comprising the following steps:
[0012] S1: Place a high-purity aluminum ingot in a crucible of a vacuum induction furnace, add a covering agent, evacuate the furnace, and heat until the aluminum ingot melts;
[0013] S2: adding high-purity electrolytic manganese flakes, continuing to heat up, stirring, and keeping warm, then filling the vacuum induction furnace with protective gas, cooling down, and obtaining aluminum-manganese alloy liquid;
[0014] S3: The aluminum-manganese alloy liquid is cast into a slag form, and then crushed and ball-milled to obtain aluminum-manganese intermetallic compound powder.
[0015] Further, based on the above technical solution, the raw materials of the aluminum-manganese intermetallic compound include 55-66% of high-purity aluminum ingots and 34-45% of high-purity electrolytic manganese sheets in terms of mass percentage;
[0016] And / or, the purity of the high-purity aluminum ingot is ≥99.9%, and the purity of the high-purity electrolytic manganese sheet is ≥99.9%.
[0017] Further, based on the above technical solution, the covering agent is one or more of KCl or NaCl;
[0018] Preferably, the added amount of the covering agent is 10-15% of the total mass of the raw materials.
[0019] Further, based on the above technical solution, in step S1, the crucible of the vacuum induction furnace is a graphite crucible;
[0020] And / or, the crucible is preheated to 180-220° C. and then a high-purity aluminum ingot is placed therein;
[0021] And / or, in step S1, the vacuuming and heating until the aluminum ingot is melted specifically comprises:
[0022] Evacuate to 0.05-0.1Pa, raise the temperature to 700-780℃, and keep it warm for 3-5min to melt the aluminum ingot.
[0023] Further, based on the above technical solution, step S2 specifically includes the following steps:
[0024] Add high-purity electrolytic manganese flakes, continue to heat up to 1350-1500°C, stir, keep warm for 25-30 minutes, fill the vacuum induction furnace with protective gas, and cool down to 800-850°C;
[0025] And / or, the protective gas is argon or helium with a purity of ≥99.99%, preferably argon.
[0026] Furthermore, based on the above technical solution, step S3 specifically includes the following steps: when the pressure in the vacuum induction furnace is ≥1 atmosphere, the upper cover of the vacuum furnace is opened, the slag is removed and the liquid covering agent is poured out, the alloy liquid is poured into an ingot mold for casting, and the alloy block is cooled with the furnace.
[0027] Further, based on the above technical solution, in step S3, the crushing includes:
[0028] The obtained alloy block is placed in a mechanical crusher and crushed into coarse powder;
[0029] Preferably, the particle size of the coarse powder is 5-10 mm.
[0030] Further, based on the above technical solution, in step S3, the ball milling includes:
[0031] The coarse powder is placed in a ball mill, liquid nitrogen is introduced as a protective agent, and a stainless steel ball with a diameter of 25-30 mm is used for ball milling to obtain aluminum-manganese intermetallic compound powder;
[0032] And / or, the powder particles have a diameter of 3-5 μm;
[0033] And / or, the ball milling time is 15-20 hours, and the ball milling speed is 300-400 rpm.
[0034] The present invention also provides an aluminum-manganese intermetallic compound prepared by the preparation method of the aluminum-manganese intermetallic compound as described above, which comprises the following components by mass percentage: 34-45% Mn and 0.1-0.8% trace elements, and the balance is Al;
[0035] The aluminum-manganese intermetallic compound is calculated as Al8Mn5 according to the molecular formula.
[0036] Furthermore, based on the above technical solution, the trace elements include Fe, O, N, Si, Mg and Ti.
[0037] The present invention provides an aluminum-manganese intermetallic compound and a preparation method thereof, and the beneficial effects are as follows:
[0038] (1) The aluminum-manganese master alloy prepared by the present invention has a high Mn content (34-45wt.%), which significantly reduces the production cost of aluminum alloy;
[0039] (2) The aluminum-manganese master alloy preparation process of the present invention has low production cost, is simple and easy to control, is cheap, and is easy to realize industrial production;
[0040] (3) The aluminum-manganese master alloy powder of the present invention has a single phase, uniform particle size distribution, and a simple production method;
[0041] (4) The aluminum-manganese intermediate alloy prepared by the present invention can significantly reduce the Fe impurity element in the aluminum alloy. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0043] Figure 1 This is a scanning electron microscope photograph of the aluminum-manganese master alloy powder prepared in Example 1 of the present invention;
[0044] Figure 2 This is the XRD spectrum of the aluminum-manganese intermediate alloy powder prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0045] In order to make the purpose, technical scheme and advantages of the present invention clearer, the technical scheme in the embodiment of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention. The process parameters of the following embodiments that do not specify specific conditions are usually based on conventional conditions.
[0046] The endpoints and any values of the ranges disclosed in the present invention are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be regarded as specifically disclosed in the present invention.
[0047] According to a first aspect of the present invention, there is provided a method for preparing the above-mentioned aluminum-manganese intermetallic compound, comprising the following steps:
[0048] S1: Place a high-purity aluminum ingot in a crucible of a vacuum induction furnace, add a covering agent, evacuate the furnace, and heat until the aluminum ingot melts;
[0049] S2: adding high-purity electrolytic manganese flakes, continuing to heat up, stirring, and keeping warm, then filling the vacuum induction furnace with protective gas, cooling down, and obtaining aluminum-manganese alloy liquid;
[0050] S3: After the aluminum-manganese alloy liquid is slag-discharging, the aluminum-manganese alloy liquid is cast into a mold, and then crushed and ball-milled to obtain aluminum-manganese intermetallic compound powder.
[0051] As a preferred embodiment of the present invention, the raw material of the aluminum-manganese intermetallic compound includes 55-66% (such as 57%, 59%, 61%, 63%, etc.) of high-purity aluminum ingots and 34-45% (such as 37%, 39%, 41%, 43%, etc.) of high-purity electrolytic manganese flakes by mass percentage;
[0052] And / or, the purity of the high-purity aluminum ingot is ≥99.9%, and the purity of the high-purity electrolytic manganese sheet is ≥99.9%.
[0053] As a preferred embodiment of the present invention, the covering agent is one or more of KCl or NaCl;
[0054] Preferably, the added amount of the covering agent is 10-15% (eg, 10%, 12%, 13%, 14% or 15%, etc.) of the total mass of the raw materials.
[0055] Specifically, the covering agent can effectively isolate the aluminum-manganese alloy liquid from the furnace environment, prevent the aluminum liquid from gasifying during the smelting process, reduce the burning loss of the alloy liquid during the smelting process, and maintain the stability of the alloy composition; and the covering agent has a cleaning effect on the surface oil and oxides entering the aluminum-manganese alloy liquid, which can reduce the degree of contamination of the alloy liquid and improve the purity of the alloy; further, in the aluminum-manganese alloy smelting process, the covering agent is used in combination, and attention is paid to controlling the aluminum liquid temperature and reducing the moisture content in the furnace, so as to achieve a better refining effect, especially the covering agent helps to remove hydrogen and reduce the hydrogen content in the alloy; further, the covering agent can effectively prevent the slag from adhering to the ladle, the furnace lining and entering the casting, reduce the slag inclusion defects of the casting, thereby protecting the smelting equipment and extending its service life; further, after the covering agent forms a covering layer on the surface of the alloy liquid, it also has a certain heat preservation effect, which can reduce the heat loss of the alloy liquid and improve the smelting efficiency.
[0056] As a preferred embodiment of the present invention, in step S1, the crucible of the vacuum induction furnace is a graphite crucible;
[0057] And / or, the crucible is preheated to 180-220° C. (190° C., 200° C., 210° C., etc.) and then the high-purity aluminum ingot is placed therein.
[0058] Specifically, the purpose of preheating the crucible to 180-220° C. in the present invention is to remove moisture in the crucible and dry the crucible.
[0059] As a preferred embodiment of the present invention, in step S1, the vacuuming and heating until the aluminum ingot is melted specifically includes:
[0060] Evacuate to 0.05-0.1Pa (such as 0.06Pa, 0.07Pa, 0.08Pa, 0.09Pa, etc.), heat to 700-780℃ (such as 720℃, 740℃, 760℃, etc.), keep warm for 3-5min (such as 3.5min, 4min, 4.5min, etc.) to melt the aluminum ingot.
[0061] Specifically, preliminary heating of the aluminum ingot at 700-780° C. can control the melting rate of the aluminum ingot, which helps to reduce the probability of formation of AlFe harmful phases.
[0062] As a preferred embodiment of the present invention, step S2 specifically includes the following steps:
[0063] Add high-purity electrolytic manganese flakes, continue to heat up to 1350-1500°C (1400°C, 1420°C, 1440°C, 1460°C, 1480°C, etc.), stir, keep warm for 25-30 minutes (such as 26 minutes, 27 minutes, 28 minutes, 29 minutes, etc.), and then cool down to 800-850°C (820°C, 830°C, 840°C, etc.).
[0064] Specifically, the temperature between 1350°C and 1500°C is most favorable for the melting of the electrolytic manganese sheet. If the temperature is higher than 1500°C, the electrolytic manganese sheet will be oxidized; if the temperature is lower than 1350°C, the melting of the electrolytic manganese sheet will be insufficient.
[0065] Further cooling to 800-850℃ can not only ensure that the metal in the alloy liquid is completely melted and avoid the appearance of unmelted solid particles, but also improve the fluidity of the metal liquid, which is beneficial to subsequent casting, molding and other processes, and can promote the separation and removal of impurities in the metal and improve the purity of the metal.
[0066] As a preferred embodiment of the present invention, the protective gas is argon or helium with a purity of ≥99.99%, preferably argon.
[0067] Specifically, the shielding gas cannot be nitrogen because smelting in a nitrogen atmosphere will result in nitrogen doping and forming inclusions in the melt, resulting in reduced purity of the smelted alloy.
[0068] As a preferred embodiment of the present invention, step S3 specifically includes the following steps: when the pressure in the vacuum induction furnace is ≥1 atmosphere, the upper cover of the vacuum furnace is opened, the slag is removed and the liquid covering agent is poured out, the alloy liquid is poured into an ingot mold for casting, and the alloy block is cooled with the furnace.
[0069] Specifically, during the refining process, proper stirring is used to promote the floating of impurities and gases. After stirring, the covering agent and scum (including oxides, inclusions, etc.) will combine together to form a thick layer of liquid scum; after the refining is completed, the liquid scum layer is removed from the melt surface by slag removal.
[0070] As a preferred embodiment of the present invention, in step S3, the pulverizing includes:
[0071] The obtained alloy block is placed in a mechanical crusher and crushed into coarse powder;
[0072] Preferably, the particle size of the coarse powder is 5-10 mm (such as 6 mm, 7 mm, 8 mm, 9 mm, etc.).
[0073] Specifically, the particle size of the coarse powder is 5-10 mm to facilitate subsequent ball milling.
[0074] As a preferred embodiment of the present invention, in step S3, the ball milling includes:
[0075] The coarse powder is placed in a ball mill, liquid nitrogen is introduced as a protective agent, and a stainless steel ball with a diameter of 25-30 mm is used for ball milling to obtain aluminum-manganese intermetallic compound powder;
[0076] And / or, the powder particle diameter is 3-5 μm (such as 3.5 μm, 4 μm, 4.5 μm, etc.);
[0077] And / or, the ball milling time is 15-20h (such as 16h, 17h, 18h, 19h, etc.), and the ball milling speed is 300-400rpm (such as 320rpm, 340rpm, 360rpm, 380rpm, etc.).
[0078] According to a second aspect of the present invention, there is provided an aluminum-manganese intermetallic compound, comprising the following components, by mass percentage: 34-45% (e.g., 35%, 36%, 38%, 40%, 42%, 44%, etc.) of Mn and 0.1-0.8% (e.g., 0.15%, 0.2%, 0.25%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, etc.) of trace elements, and the balance is Al;
[0079] The aluminum-manganese intermetallic compound is calculated as Al8Mn5 according to the molecular formula.
[0080] Specifically, the aluminum-manganese intermediate alloy Al8Mn5 has a high solid solubility in Fe element (up to 31at.%). The Fe impurity elements in the Al melt are dissolved into the Al8Mn5 phase to form a large amount of Al8(Fe,Mn)5 phase, which greatly reduces the probability of forming AlFe harmful phases and the harmful effect of iron-rich phases on aluminum alloys. At the same time, it effectively reduces the electrode potential of the iron-containing phase and reduces the potential difference between it and the surrounding aluminum matrix, thereby significantly improving the corrosion resistance of the aluminum alloy.
[0081] As a preferred embodiment of the present invention, the trace elements include Fe, O, N, Si and Ti. More preferably, the trace elements include Fe, O, N, Si, Mg and Ti.
[0082] The present invention will be further described in detail below with reference to specific embodiments and comparative examples.
[0083] Example 1
[0084] Prepare raw materials by mass percentage, high-purity aluminum ingots account for 55%, and high-purity electrolytic manganese flakes account for 45%; the purity of the high-purity aluminum ingots is 99.9%, and the purity of the high-purity electrolytic manganese flakes is 99.9%;
[0085] A vacuum induction melting furnace is used, with a built-in graphite crucible. After the power is turned on and the graphite crucible is preheated to 200°C, a high-purity aluminum ingot is placed therein, and KCl accounting for 10% of the total mass of the high-purity aluminum ingot and the high-purity electrolytic manganese sheet is sprinkled therein. The upper cover of the vacuum furnace is closed, the vacuum is evacuated to 0.1 Pa, and the temperature is raised to 750°C and kept for 4 minutes to fully melt the aluminum ingot.
[0086] Add high-purity electrolytic manganese flakes, start electromagnetic stirring, continue to heat up to 1400℃, keep warm for 25 minutes, so that the electrolytic manganese flakes are completely melted;
[0087] Gradually reduce the power supply, introduce argon (purity of 99.99%), cool down to 800℃, wait until the pressure in the vacuum induction furnace reaches 1 atmosphere, open the upper cover of the vacuum furnace, pour out the slag and liquid covering agent, and cast the alloy liquid into alloy blocks;
[0088] After the alloy block is cooled to room temperature, the obtained alloy ingot is mechanically crushed into coarse powder with a particle size of 5-10 mm;
[0089] The coarse powder was poured into a ball mill, liquid nitrogen was introduced as a protective agent, and stainless steel balls with a diameter of 25-30 mm were used for ball milling for 20 hours at a speed of 400 rpm to obtain aluminum-manganese intermediate alloy powder with a particle diameter of 3-5 μm. Figure 1 As shown in FIG. 1 , it can be seen from the SEM morphology that the final powder product prepared in Example 1 of the present invention is spherical particles with uniform particle size and an average particle size of about 3-5 μm; Figure 2As shown, it was further confirmed by XRD that the phase composition of the powder was mainly Al8Mn5.
[0090] Example 2
[0091] The raw materials are prepared by mass percentage, wherein the high-purity aluminum ingots account for 55% and the high-purity electrolytic manganese flakes account for 45%; the purity of the high-purity aluminum ingots is 99.9%, and the purity of the high-purity electrolytic manganese flakes is 99.9%;
[0092] A vacuum induction melting furnace is used, with a built-in graphite crucible. After the power is turned on and the graphite crucible is preheated to 180°C, a high-purity aluminum ingot is placed therein, and a covering agent NaCl accounting for 15% of the total mass of the high-purity aluminum ingot and the high-purity electrolytic manganese sheet is sprinkled therein. The upper cover of the vacuum furnace is closed, the vacuum is evacuated to 0.05Pa, and the temperature is raised to 780°C and kept for 5 minutes to fully melt the aluminum ingot.
[0093] Add high-purity electrolytic manganese flakes, start electromagnetic stirring, continue to heat up to 1350°C, and keep warm for 30 minutes to completely melt the electrolytic manganese flakes;
[0094] Gradually reduce the power supply, introduce argon (purity of 99.99%), cool down to 850°C, wait until the pressure in the vacuum induction furnace reaches 1 atmosphere, open the upper cover of the vacuum furnace, pour out the slag and liquid covering agent, and cast the alloy liquid into alloy blocks;
[0095] After the alloy block is cooled to room temperature, the obtained alloy ingot is mechanically crushed into coarse powder with a particle size of 5-10 mm;
[0096] The coarse powder was poured into a ball mill, liquid nitrogen was introduced as a protective agent, stainless steel balls with a diameter of 25-30 mm were used for ball milling for 15 hours, and the ball mill speed was 400 rpm to obtain aluminum-manganese intermediate alloy powder with a powder particle diameter of 3-5 μm.
[0097] Example 3
[0098] The raw materials are prepared by mass percentage, wherein the high-purity aluminum ingots account for 55% and the high-purity electrolytic manganese flakes account for 45%; the purity of the high-purity aluminum ingots is 99.9%, and the purity of the high-purity electrolytic manganese flakes is 99.9%;
[0099] A vacuum induction melting furnace is used, with a built-in graphite crucible. After the power is turned on and the graphite crucible is preheated to 220°C, a high-purity aluminum ingot is placed in it, and a covering agent KCl accounting for 12% of the total mass of the high-purity aluminum ingot and the high-purity electrolytic manganese sheet is sprinkled in. The upper cover of the vacuum furnace is closed, the vacuum is evacuated to 0.08Pa, and the temperature is raised to 700°C and kept for 3 minutes to fully melt the aluminum ingot.
[0100] Add high-purity electrolytic manganese flakes, start electromagnetic stirring, continue to raise the temperature to 1500°C, and keep warm for 28 minutes to completely melt the electrolytic manganese flakes;
[0101] Gradually reduce the power supply, introduce argon (purity of 99.99%), cool down to 820°C, wait until the pressure in the vacuum induction furnace reaches 1 atmosphere, open the upper cover of the vacuum furnace, pour out the slag and liquid covering agent, and cast the alloy liquid into alloy blocks;
[0102] After the alloy block is cooled to room temperature, the obtained alloy ingot is mechanically crushed into coarse powder with a particle size of 5-10 mm;
[0103] The coarse powder was poured into a ball mill, liquid nitrogen was introduced as a protective agent, stainless steel balls with a diameter of 25-30 mm were used for ball milling for 15 hours, and the ball mill speed was 400 rpm to obtain aluminum-manganese intermediate alloy powder with a powder particle diameter of 3-5 μm.
[0104] Example 4
[0105] The implementation steps of this embodiment are the same as those of Embodiment 1, except that: the raw materials are prepared by mass percentage, with high-purity aluminum ingots accounting for 60% and high-purity electrolytic manganese flakes accounting for 40%; the purity of the high-purity aluminum ingots is 99.9%, and the purity of the high-purity electrolytic manganese flakes is 99.9%.
[0106] Example 5
[0107] The implementation steps of this embodiment are the same as those of Embodiment 1, except that: the raw materials are prepared by mass percentage, with high-purity aluminum ingots accounting for 65% and high-purity electrolytic manganese flakes accounting for 35%; the purity of the high-purity aluminum ingots is 99.9%, and the purity of the high-purity electrolytic manganese flakes is 99.9%.
[0108] Example 6
[0109] The implementation steps of this embodiment are the same as those of Example 1. The raw materials are prepared by mass percentage, with high-purity aluminum ingots accounting for 60% and high-purity electrolytic manganese flakes accounting for 40%; the purity of the high-purity aluminum ingots is 99.9%, and the purity of the high-purity electrolytic manganese flakes is 99.9%.
[0110] The difference from Example 1 is that high-purity electrolytic manganese flakes are added, electromagnetic stirring is turned on, the temperature is continued to be raised to 1350° C., and the temperature is kept for 25 minutes to completely melt the electrolytic manganese flakes.
[0111] Example 7
[0112] The implementation steps of this embodiment are the same as those of Example 1. The raw materials are prepared by mass percentage, with high-purity aluminum ingots accounting for 60% and high-purity electrolytic manganese flakes accounting for 40%; the purity of the high-purity aluminum ingots is 99.9%, and the purity of the high-purity electrolytic manganese flakes is 99.9%.
[0113] The difference from Example 1 is that high-purity electrolytic manganese flakes are added, electromagnetic stirring is turned on, the temperature is continued to be raised to 1450° C., and the temperature is kept for 20 minutes to completely melt the electrolytic manganese flakes.
[0114] Comparative Example 1
[0115] The steps of this comparative example are the same as those of Example 1, except that a medium frequency induction furnace is used for heating; the alloy block is tested by chemical analysis method, and the composition is shown in Table 1.
[0116] Comparative Example 2
[0117] The steps of this comparative example are the same as those of Example 1, except that high-purity electrolytic manganese flakes are added, electromagnetic stirring is turned on, the temperature is continued to be raised to 1550° C., and the temperature is kept for 25 minutes; the composition of the alloy block is tested by chemical analysis method, see Table 1.
[0118] Comparative Example 3
[0119] The steps of this comparative example are the same as those of Example 1, except that high-purity electrolytic manganese flakes are added, electromagnetic stirring is turned on, the temperature is continued to be raised to 1300° C., and the temperature is kept for 25 minutes; the composition of the alloy block is tested by chemical analysis method, see Table 1.
[0120] The components of the aluminum-manganese intermetallic compound powders prepared in Examples 1-7 and Comparative Examples 1-3 are shown in Table 1.
[0121] Table 1 Chemical composition of Al8Mn5 master alloy (wt.%)
[0122]
[0123]
[0124] According to Table 1, compared with Example 1, in Comparative Example 1, since the medium frequency induction furnace is used for heating, aluminum is easily oxidized to form inclusions, which affects the purity of the obtained aluminum-manganese intermediate alloy, resulting in an excessively high oxygen content in the prepared aluminum-manganese intermetallic compound powder, and the content of other impurities also increases accordingly.
[0125] According to Table 1, compared with Example 1, in Comparative Example 2, after adding the high-purity electrolytic manganese sheet, the temperature is raised to 1550° C. for melting, and the temperature is too high, resulting in severe burnout of aluminum and manganese, which leads to a significant increase in the content of other impurities in the prepared aluminum-manganese intermetallic compound powder.
[0126] According to Table 1, compared with Example 1, in Comparative Example 3, after adding the high-purity electrolytic manganese sheet, the temperature is raised to 1300° C. for melting, and the temperature is too low, resulting in an increase in the content of other impurities in the prepared aluminum-manganese intermetallic compound powder.
[0127] Implementation effect comparison example 1
[0128] Select a well-known brand of 5087 aluminum alloy ingot, its chemical composition is shown in Table 2:
[0129] Table 2 Chemical composition of 5087 aluminum alloy (wt.%)
[0130] Al Mn Cu Si Mg Cr Zn Ti Fe Zr Be other 0.25 0.4 0.05 0.7-1.1 4.5-5.2 0.05-0.25 0.25 0.15 margin 0.10-0.20 0.0003 0.15
[0131] A vacuum induction melting furnace is used with a built-in graphite crucible. The graphite crucible is preheated to 200°C and then the 5087 aluminum alloy ingot is placed in it. The upper cover of the vacuum furnace is closed, the vacuum is evacuated to 0.1 Pa, and the temperature is raised to 740°C and kept for 10 minutes to fully melt the aluminum ingot.
[0132] 1% by mass of the Al8Mn5 master alloy powder prepared in Example 1 was added, electromagnetic stirring was turned on, and the temperature was kept at room temperature for 15 minutes to completely melt the melt in the crucible;
[0133] Gradually reduce the power supply, introduce argon (purity of 99.99%), wait until the pressure in the vacuum induction furnace reaches 1 atmosphere, open the upper cover of the vacuum furnace, and cast the alloy liquid into alloy blocks;
[0134] After the alloy block is naturally cooled to room temperature, the composition of the alloy block is tested by chemical analysis method, see Table 3.
[0135] Implementation effect comparison example 2
[0136] The steps of this comparative example are the same as those of comparative example 1, except that the added aluminum-manganese master alloy powder is commercially available AlMn10 powder that complies with the GB / T 27677-2017 standard. The composition of the alloy block is tested by chemical analysis method, see Table 3.
[0137] Implementation effect comparison example 3
[0138] The steps of this comparative example are the same as those of comparative example 1, except that the added aluminum-manganese master alloy powder is commercially available Al6Mn powder that complies with the GB / T 27677-2017 standard. The alloy block is tested by chemical analysis method and the composition is shown in Table 3.
[0139] Implementation effect comparison example 4
[0140] The steps of this comparative example are the same as those of comparative example 1, except that the added aluminum-manganese master alloy powder is commercially available AlMn powder that complies with the GB / T 27677-2017 standard. The alloy block is tested by chemical analysis method and the composition is shown in Table 3.
[0141] Table 3 Chemical composition of aluminum alloy after adding aluminum-manganese master alloy (wt.%)
[0142]
[0143] As can be seen from Table 3, Al8Mn5 has a relatively obvious effect of reducing the content of Fe elements, and has no effect on the contents of other alloy elements, and can be stably used in the smelting production of aluminum alloys. Implementation effect comparison example 2, implementation effect comparison example 3 and implementation effect comparison example 4 show that AlMn10, Al6Mn and AlMn have limited effects on reducing the content of Fe elements, and the content of Fe elements increases instead, which may be due to the presence of Fe impurity elements in the aluminum-manganese master alloy.
[0144] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing an aluminum-manganese intermetallic compound, characterized in that: The steps include: S1: Place a high-purity aluminum ingot in a crucible of a vacuum induction furnace, add a covering agent, evacuate the furnace, and heat until the aluminum ingot melts; S2: adding high-purity electrolytic manganese flakes, continuing to heat up, stirring, and keeping warm, then filling the vacuum induction furnace with protective gas, cooling down, and obtaining aluminum-manganese alloy liquid; S3: The aluminum-manganese alloy liquid is cast into a slag form, and then crushed and ball-milled to obtain aluminum-manganese intermetallic compound powder.
2. The method for preparing the aluminum-manganese intermetallic compound according to claim 1, characterized in that: The raw materials of the aluminum-manganese intermetallic compound include 55-66% of high-purity aluminum ingots and 34-45% of high-purity electrolytic manganese flakes by mass percentage; And / or, the purity of the high-purity aluminum ingot is ≥99.9%, and the purity of the high-purity electrolytic manganese sheet is ≥99.9%.
3. The method for preparing the aluminum-manganese intermetallic compound according to claim 2, characterized in that: The covering agent is one or more of KCl or NaCl; Preferably, the added amount of the covering agent is 10-15% of the total mass of the raw materials.
4. The method for preparing the aluminum-manganese intermetallic compound according to claim 1, characterized in that: In step S1, the crucible of the vacuum induction furnace is a graphite crucible; And / or, the crucible is preheated to 180-220° C. and then a high-purity aluminum ingot is placed therein; And / or, in step S1, the vacuuming and heating until the aluminum ingot is melted specifically comprises: Evacuate to 0.05-0.1Pa, raise the temperature to 700-780℃, and keep it warm for 3-5min to melt the aluminum ingot.
5. The method for preparing the aluminum-manganese intermetallic compound according to claim 1, characterized in that: Step S2 specifically includes the following steps: Add high-purity electrolytic manganese flakes, continue to heat up to 1350-1500°C, stir, keep warm for 25-30 minutes, fill the vacuum induction furnace with protective gas, and cool down to 800-850°C; And / or, the protective gas is argon or helium with a purity of ≥99.99%, preferably argon.
6. The method for preparing the aluminum-manganese intermetallic compound according to claim 1, characterized in that: Step S3 specifically includes the following steps: when the pressure in the vacuum induction furnace is ≥ 1 atmosphere, the upper cover of the vacuum furnace is opened, the slag is removed and the liquid covering agent is poured out, the alloy liquid is poured into an ingot mold for casting, and the alloy block is cooled with the furnace.
7. The method for preparing the aluminum-manganese intermetallic compound according to claim 1, characterized in that: In step S3, the crushing includes: The obtained alloy block is placed in a mechanical crusher and crushed into coarse powder; Preferably, the particle size of the coarse powder is 5-10 mm.
8. The method for preparing the aluminum-manganese intermetallic compound according to claim 7, characterized in that: In step S3, the ball milling includes: The coarse powder is placed in a ball mill, liquid nitrogen is introduced as a protective agent, and a stainless steel ball with a diameter of 25-30 mm is used for ball milling to obtain aluminum-manganese intermetallic compound powder; And / or, the powder particles have a diameter of 3-5 μm; And / or, the ball milling time is 15-20 hours, and the ball milling speed is 300-400 rpm.
9. An aluminum-manganese intermetallic compound obtained by the method for preparing an aluminum-manganese intermetallic compound according to any one of claims 1 to 8, characterized in that: Calculated by mass percentage, it includes the following components: 34-45% Mn and 0.1-0.8% trace elements, and the balance is Al; The aluminum-manganese intermetallic compound is calculated as Al8Mn5 according to the molecular formula.
10. The aluminum-manganese intermetallic compound according to claim 9, characterized in that The trace elements include Fe, O, N, Si, Mg and Ti.
Citation Information
Patent Citations
High-manganese-content aluminum-manganese intermediate alloy and preparation method thereof
CN110241342A
Aluminum-manganese intermetallic compound as well as preparation method and application thereof
CN114985745A
Intermediate Al-Mn alloy and method of manufacturing the same
CN101509087A
Preparation method of high-purity aluminum-manganese intermediate alloy
CN102162042A
Aluminum-manganese dielement intermediate alloy and preparing method thereof
CN108315601A