2D perovskite compound and preparation method and multicolor long afterglow luminescence application thereof
By synthesizing 2D perovskite compound SL-1, using HOF network structure and nano-scale particle composite technology, the problems of high cost and low stability of existing materials are solved, and multi-color long afterglow luminescence and stable anti-counterfeiting effect are achieved. for multi-color fluorescence and encryption applications.
Patent Information
- Application Number
- CN202411360494.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-27
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-09-27
AI Technical Summary
The existing high-efficiency inorganic long afterglow luminescence materials contain expensive rare metals, resulting in high cost and low stability, and the inability to effectively achieve the multi-color long afterglow luminescence effect.
The 2D perovskite compound SL-1 was synthesized by solvothermal reaction method using ligand L and cadmium chloride. The HOF network structure was used to inhibit non-radiative transitions, forming a stable spatial structure, achieving excitation-dependent multi-color fluorescence and phosphorescence characteristics, and Anti-counterfeiting films are prepared by composited nano-scale particles with polymers.
It achieves stable multi-color long afterglow luminescence performance, and the luminous color can be adjusted from blue to yellow, improving the stability and environmental friendliness of the material, and is suitable for a wide range of anti-counterfeiting and encryption applications.
Smart Images

Figure BDA0005064817540000021 
Figure BDA0005064817540000072 
Figure BDA0005064817540000081
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of multi-color anti-counterfeiting, and specifically relates to a 2D perovskite compound, a preparation method thereof, and multi-color long afterglow luminescence application. Background Art
[0002] Long afterglow luminescence (LAL) materials have attracted the attention of researchers because of their broad application prospects in optoelectronic devices, bioimaging, afterglow lighting, etc. To date, most high-efficiency inorganic LAL materials contain expensive rare metals and lanthanides, which hinder their further commercial application. In order to overcome these shortcomings, low-cost and easy-to-synthesize organic materials have been further developed. However, the spin-orbit coupling (SOC) in organic molecules is usually too weak to effectively break the spin band gap of the triplet-singlet transition, resulting in poor quantum yield of phosphorescent emission. Recently, organic-inorganic hybrid perovskites have become one of the most promising luminescent materials due to their environmental friendliness, superior optoelectronic properties, and easy availability.
[0003] Here, a typical intraligand charge transfer (ILCT) ligand was preliminarily designed and synthesized. This electrically neutral ligand, on the one hand, contains abundant carbonyl groups, which can be protonated and provide hydrogen bonding sites, thereby co-crystallizing with metal halide polyhedra to produce abundant intermolecular interactions. On the other hand, the abundant N-heteroatoms and carbonyl groups in the ligand are conducive to n-п transitions and achieve effective LAL. Using ILCT ligands and CdCl2 self-assembly, a two-dimensional organic-metal halide perovskite (SL-1) was carefully constructed, in which the organic part formed a HOF network through hydrogen bonding and the inorganic metal halide formed an infinite inorganic layer. This also further protected the triplet excitons, thereby significantly improving the room temperature phosphorescence efficiency of the perovskite hybrid material. Therefore, it is of great significance to study HOF-based organic-inorganic hybrid perovskites. Summary of the invention
[0004] The purpose of the present invention is to provide a 2D perovskite compound and its preparation method and multi-color long afterglow luminescence application. SL-1 has excitation-dependent fluorescence and phosphorescence characteristics, and its fluorescence and phosphorescence colors can range from blue to green and cyan to yellow. More interestingly, when different excitation light sources are removed, the 2D perovskite compound (hereinafter referred to as compound SL-1) can emit a long afterglow with adjustable color from cyan to yellow. At the same time, the nano-scale particles prepared by grinding, ultrasound and other methods can be uniformly compounded with polymers such as polymethyl methacrylate to prepare a stable luminescent anti-counterfeiting film to achieve the purpose of anti-counterfeiting. The technical problem to be solved is to overcome the low stability and short life of two-dimensional organic-inorganic hybrid perovskites.
[0005] In order to achieve the above object, the technical solution adopted by the present invention is:
[0006] An organic ligand L, with the molecular formula of C30H26N4O4, belongs to the monoclinic system, the P21 / c space group, and has the following structure:
[0007]
[0008] The preparation method of the ligand L comprises the following steps:
[0009] 4-Hydroxypyridine and K2CO3 were added to ethanol. After stirring at 80°C for 4h, 1,2,4,5-tetra(bromomethyl)benzene was added to the mixture. After stirring at 80°C overnight, a yellow precipitate was formed. The solvent was removed to obtain a light yellow ligand mixture, which was washed three times with ether. A mixture of the obtained light yellow ligand mixture, DMF, distilled water and CH3CN was added to a glass bottle. The mixture was sealed and placed in an oven and heated at 90°C for 2 days, and then gradually cooled to room temperature at a rate of 5°C / h. Finally, the colorless block crystals were collected by filtration to obtain ligand L.
[0010] Furthermore, the molar ratio of 4-hydroxypyridine, potassium carbonate and 1,2,4,5-tetrabromomethylbenzene is 4:2.5:1 to 4:3:1.
[0011] Wherein, preferably, the molar ratio of 4-hydroxypyridine, potassium carbonate and 1,2,4,5-tetrabromomethylbenzene is 4:2.5:1.
[0012] Furthermore, the usage ratio of ethanol to 4-hydroxypyridine is 15 ml:2 mmol to 20 ml:2 mmol.
[0013] Wherein, preferably, the usage ratio of ethanol and 4-hydroxypyridine is 15ml:2mmol.
[0014] Furthermore, the dosage ratio of the DMF to ligand L mixture is 2 ml:1 mmol to 4 ml:1 mmol.
[0015] Wherein, preferably, the dosage ratio of the DMF and ligand L mixture is 4 ml:1 mmol.
[0016] Furthermore, the usage ratio of DMF, distilled water and CH3CN is 1:1:1 to 1:2:2.
[0017] Among them, preferably, the usage ratio of DMF, distilled water and CH3CN is 1:1:1.
[0018] As an optional embodiment, the preparation method of the ligand L comprises the following steps: 4-hydroxypyridine (4mmol, 0.6g) and potassium carbonate (2.5mmol, 0.9g) are added to ethanol (30mL), and after stirring at 80°C for 4h, 1,2,4,5-tetrabromomethylbenzene (1mmol, 0.5g) is added. After stirring at 80°C overnight, a yellow precipitate is formed. The solvent is removed to obtain a light yellow solid, which is washed 3 times with ether. A mixture of the obtained light yellow ligand mixture, DMF (1ml), distilled water (1ml) and CH3CN (1ml) is added to a glass bottle. The mixture is sealed and placed in an oven and heated at 90°C for 2 days, and then gradually cooled to room temperature at a rate of 5°C / h. Finally, the colorless block crystals are collected by filtration to obtain ligand L.
[0019] A compound SL-1 has a molecular weight of 1604.06, belongs to the monoclinic crystal system, has a space group of P21 / c, and has a molecular formula of C30H40Cd5Cl12N4O10.
[0020] The compound SL-1 is prepared using L and cadmium chloride as raw materials.
[0021] The preparation method of the compound SL-1 comprises the following steps:
[0022] S1. Mix cadmium chloride and organic L in a molar ratio of 1 to 5:1, put into a reaction flask, and add methanol, acetonitrile and hydrochloric acid in a volume ratio of 1 to 2:1 to 3:1 into a reaction kettle;
[0023] S2. The sealed pressure reactor is placed in an oven, the program is set, and the heating is performed for 1 to 2 hours, the temperature is raised from room temperature to 100 to 120 ° C, and the temperature is maintained for 40 to 60 hours, and then cooled after 8 to 12 hours;
[0024] S3. After cooling to room temperature, white block crystals were obtained, which were filtered and washed with methanol to obtain pure crystals.
[0025] Furthermore, in step S1, the molar ratio of cadmium chloride to L is 5:1.
[0026] Furthermore, in step S1, the volume ratio of methanol, acetonitrile and (0.1 mol / L) hydrochloric acid is 1:1:1.
[0027] Furthermore, in step S2, the oven program is set to heat for 2 hours to raise the temperature from room temperature to 90° C., maintain this temperature for 48 hours, and then cool down to room temperature after 10 hours.
[0028] As an optional implementation scheme, the preparation method of the compound SL-1 comprises the following steps: adding 10 mg, 0.02 mmol of L and 18 mg, 0.1 mmol of cadmium chloride into a reaction bottle, then adding 1 mL of methanol, 1 mL of acetonitrile and 1 mL (0.1 mol / L) of hydrochloric acid, and gently shaking the reactor to mix evenly; then placing the reactor in an oven, and setting the oven program to heat for 2 hours to raise the temperature from room temperature to 90°C, keeping this temperature for 48 hours, and then cooling to room temperature after 10 hours; finally filtering the resulting mixture, and washing with methanol to obtain a white single crystal of the coordination compound SL-1.
[0029] The present invention has the following beneficial effects:
[0030] (1) The present invention provides a stable spatial structure formed by using HOF-type organic ligands to suppress non-radiative transitions, thereby obtaining a long-lasting coordination compound with good performance and stability;
[0031] (3) Compound SL-1 has stable luminescence performance; it has excitation-dependent fluorescence and phosphorescence properties, its luminescence color can range from blue to green, it is easy to recycle, and it is environmentally friendly;
[0032] (4) Anti-counterfeiting and encryption materials prepared based on compound SL-1 have a wide range of applications and can be reused. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 The crystal structure of SL-1. a) Asymmetric unit and coordination environment of metal ions; b, c) 2D structure formed by self-assembly of metal and L; d) 2D layered structure formed by hydrogen bond interaction.
[0034] Figure 2 is the infrared spectrum of SL-1.
[0035] Figure 3 PXRD spectra of simulated and synthesized SL-1.
[0036] Figure 4 The instantaneous and delayed emission spectra of L and SL-1 at room temperature.
[0037] Figure 5 The fluorescence and phosphorescence lifetime decay curves of L and SL-1.
[0038] Figure 6 Time-resolved emission spectrum of SL-1.
[0039] Figure 7 The excitation-related instantaneous and delayed emission spectra of SL-1 under ambient conditions and the corresponding CIE coordinates.
[0040] Figure 8 are the excitation spectra of SL-1 at 450, 490, 520 and 620 nm respectively.
[0041] Fig. 9 Instantaneous (a, b) and delayed (c, d) emission spectra of SL-1 crystals before and after grinding.
[0042] Fig.10 The temperature-dependent emission spectra and lifetime decay curves were performed in the range of 300-77K.
[0043] Fig.11 LAL spectra of SL-1 under UV irradiation with different excitation wavelengths removed.
[0044] Fig.12 CIE coordinates of SL-1 under UV irradiation with different excitation wavelengths removed.
[0045] Fig.13 and LAL photographs of SL-1 under UV illumination with different excitation wavelengths removed.
[0046] Fig.14 This is a schematic diagram of the anti-counterfeiting of the material. DETAILED DESCRIPTION
[0047] The present invention is further described below in conjunction with the accompanying drawings and specific examples, but the examples do not limit the present invention in any form. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.
[0048] Unless otherwise specified, the reagents and materials used in the following examples are commercially available.
[0049] Example 1 Preparation of ligand L
[0050] 4-Hydroxypyridine (4mmol, 0.6g) and potassium carbonate (2.5mmol, 0.9g) were added to ethanol (30mL), and after stirring at 80°C for 4h, 1,2,4,5-tetrabromomethylbenzene (1mmol, 0.5g) was added. After stirring at 80°C overnight, a yellow precipitate was formed. The solvent was removed to obtain a light yellow solid, which was washed 3 times with ether. A mixture of the obtained light yellow ligand mixture, DMF (1ml), distilled water (1ml) and CH3CN (1ml) was added to a glass bottle. The mixture was sealed and placed in an oven and heated at 90°C for 2 days, and then gradually cooled to room temperature at a rate of 5°C / h. Finally, the colorless block crystals were collected by filtration to obtain ligand L.
[0051] Example 2 Preparation of SL-1
[0052] Preparation of compound SL-1:
[0053] L (10 mg, 0.02 mmol), cadmium chloride (18 mg, 0.1 mmol), 1 mL of methanol, 1 mL of acetonitrile and 1 mL of 0.1 mol / L hydrochloric acid solution were added to the reaction bottle, and the reactor was slightly shaken to mix evenly; then the reactor was placed in an oven, and the oven program was set to heat for 2 hours to raise the temperature to 100°C, maintain this temperature for 48 hours, and then cool to room temperature after 10 hours; finally, the resulting mixture was filtered and washed with methanol to obtain a single crystal of a white compound.
[0054] Example 3 Crystal structure determination of SL-1
[0055] With Mo target Single crystal X-ray diffraction data of SL-1 were collected on a Rigaku-Oxford Supernova X-ray diffractometer system at 50 kV and 0.80 mA.
[0056] The structure was solved by direct method and refined by full matrix least squares method using SHELXL-2014 package. All hydrogen atoms were obtained by theoretical hydrogenation method and refined along the anisotropic direction; the relevant crystallographic data of SL-1 are shown in Table 1 below.
[0057] Table 1 shows the crystallographic data of compound SL-1
[0058]
[0059]
[0060]
[0061] The present invention has prepared a 2D perovskite compound after a lot of research and exploration. The present invention uses ligand L and cadmium chloride to synthesize compound SL-1 by solvothermal reaction method, and the molecular formula is: C30H40Cd5Cl12N4O10. Select crystals of suitable size for single crystal diffraction, and the results show that SL-1 crystallizes in the monoclinic system and belongs to the P21 / c space group. The asymmetric unit consists of 1 / 2 protonated L, 5 / 2 Cd ions, 6 Cl ions, 2 coordinated water molecules and 1 free water molecule. In SL-1, there are three different types of Cd2+ ions, and all are hexacoordinated, wherein Cd1 is coordinated with 1 oxygen atom and 5 chloride ions, Cd2 is directly coordinated with six chlorine atoms, and Cd3 is coordinated with two oxygen atoms and four chloride ions. Among them, the organic cation forms a stable rigid HOF structure through intermolecular hydrogen bonds and π-π stacking. This stacking method can effectively improve the rigidity of the molecule, inhibit the rotational vibration of the molecule, and thus improve the luminescence performance. Furthermore, the organic HOF layer and the inorganic halide layer are arranged alternately to form a tightly stacked three-dimensional framework structure, which significantly improves the afterglow performance of SL-1.
[0062] SL-1 infrared spectrum Figure 2 The phase purity was verified by powder x-ray diffraction (PXRD), and the results showed that the synthesis and simulation results matched perfectly, further proving the good phase purity ( Figure 3 ).
[0063] Example 4 Photophysical properties of SL-1
[0064] To better understand the luminescence properties at room temperature, the steady-state and transient spectra of L and SL-1 were studied in the solid state ( Figure 4 ). The results show that the instantaneous emission of SL-1 has a single emission peak at 450nm, while the main emission peak of L is at 500nm, and there is a shoulder emission at 470nm, and the corresponding decay curve lifetimes are 1.20 and 4.26ns, respectively. The delayed spectrum results show that the emission peak of the ligand L (1ms) at a short wavelength disappears, and a new emission peak appears at 500nm. In contrast, the gating spectrum of SL-1 delayed by 1ms showed a double emission peak (490nm and 520nm). The decay curve gives their lifetimes at different peaks as 14.83 (L: 500nm), 35.40 (SL-1: 490nm) and 37.10ms (SL-1: 520nm), respectively. The former belongs to fluorescence, while the latter can be attributed to phosphorescence. In addition, the time-resolved emission spectrum further confirmed the existence of long-lived phosphorescence of SL-1 ( Figure 6 ).
[0065] Interestingly, SL-1 exhibits excitation-dependent properties under ambient conditions, e.g. Figure 7 As shown. When the excitation wavelength increases from 270nm to 450nm in increments of 20nm, SL-1 achieves tunable fluorescence from blue to cyan to green. Similarly, excitation-related time-gated spectra with a delay of 1ms were collected to study the phosphorescent properties of the material. As the excitation energy decreases, the emission peak of SL-1 shows a red shift. Specifically, the emission peak moves from 470nm to 530nm, and the CIE diagram shows that SL-1 emits cyan to yellow-green phosphorescence under different excitations ( Figure 7 ). It is worth noting that when the excitation wavelength is 450nm, the spectral shape changes significantly, and a new phosphorescence peak appears at 620nm. The excitation spectrum verifies that these emission peaks originate from two triplet states ( Figure 8 ). We speculate that the phosphorescence at 490nm and 520nm can be attributed to the room temperature phosphorescence induced by the ligand L, and the emission peak at 620nm may be the self-trapped exciton (STE) emission generated by the distortion of the inorganic layer metal halide under ultraviolet light irradiation. This can be proved by the following photophysical properties. Fig. 9 As shown, the emission spectrum shape and wavelength of the microcrystalline powder are very similar to those of the bulk crystal, with only a slight decrease in intensity, which excludes the possibility that the emission near 620nm is related to permanent defects.
[0066] It is well known that temperature is one of the factors that affect the luminescence of MOFs. Therefore, emission spectra and time-resolved decay tests were performed between 300 and 77 K. The intensity of SL-1 decreases with increasing temperature, as shown in Figure 2. Fig.10 The lifetime decay curves show similar changes at different temperatures. The improvement of phosphorescence lifetime and luminescence intensity at lower temperatures may be due to the suppression of triplet non-radiative transitions at low temperatures, thereby enhancing phosphorescence emission.
[0067] Benefiting from the long phosphorescence lifetime of the material, SL-1 exhibits bright LAL emission after the excitation source is removed. Six representative wavelengths of 275, 311, 365, 385, 405 and 450 nm were selected as excitation sources. Fig.11 ,12 and 13, the changes in the LAL emission spectrum are similar to those of the phosphorescence emission spectrum. As the excitation energy decreases, the LAL color of SL-1 changes from cyan to yellow. Furthermore, when these different excitation sources are removed, the LAL can be captured using a camera, demonstrating the excitation-dependent color tuning of the LAL.
[0068] Example 5 Application of SL-1 complex
[0069] like Fig.14As shown in a, a fingerprint pattern was printed on A4 paper using SL-1 ink, and under 275nm and 405nm light, the pattern showed multi-color LAL (cyan and green). Impressively, after removing the 365nm UV lamp, dynamic LAL color changes were observed with the naked eye. This also means that the password was successfully unlocked and the encrypted information was obtained. In addition, CdCL2, L and SL-1 were selectively filled into the grooves. By converting the binary code into ASCII (American Standard Code for Information Interchange) code, a dot matrix pattern (4×8) for information encryption and decryption was formed. It can be imagined that the pattern will show dynamic evolution at different delay times. As shown Fig.14 As shown in b, if the dot is excited, the output is "1", otherwise the output is "0". Under the excitation of ultraviolet light (365nm), all dots are blue and the output is invalid binary code. When the time is extended to 0.1 seconds, the new binary code can be decoded as "SUST" according to ASCII. In addition, the code that appears at 1 second is decoded as "3534" according to decimal. Therefore, according to ASCII and decimal, these codes should eventually be decoded as "SUST 3534". At the same time, these three materials were selected to jointly design a multi-level dynamic three-dimensional anti-counterfeiting code ( Fig.14 c). The security code will display an "error" message under sunlight and 365nm ultraviolet light. When the 365nm ultraviolet light is removed, the first level of encrypted information (EI) begins to appear. After 1 second, EI-1 continues to transform into "EI-2". However, SL-1's color change ability acts as an additional variable to stimulate EI-3, thereby strengthening its anti-counterfeiting complexity. Compared with traditional anti-counterfeiting and encryption materials, SL-1 has higher flexibility and complexity, and can meet the needs of high-security anti-counterfeiting fields.
Claims
1. An organic ligand L, characterized in that The ligand L is named as 1,1',1",1"'-(benzene-1,2,4,5-tetra(methylene))tetra(pyridin-4(1H)-one), and has the molecular formula: C30H26N4O4, belongs to the monoclinic system, P21 / c space group, and its structure is as follows:
2. A compound SL-1, characterized in that The molecular weight is 1604.06, it belongs to the monoclinic crystal system, the space group is P21 / c, and its molecular formula is C30H40Cd5Cl12N4O10.
3. An organic ligand L according to claim 1, characterized in that: The preparation method of the organic ligand L comprises the following steps: Step 1, 4-hydroxypyridine and K2CO3 are added to ethanol, and after stirring at 80°C for 4 hours, 1,2,4,5-tetrakis(bromomethyl)benzene is added to the mixture, and after stirring at 80°C overnight, a light yellow ligand mixture is formed; Step 2: Remove the solvent to obtain a light yellow ligand mixture, and wash it with ether three times. Add the obtained light yellow ligand mixture, DMF, distilled water and CH3CN into a glass bottle; seal the mixture, put it into an oven and heat it at 90°C for 2 days, then gradually cool it to room temperature at a rate of 5°C / h. Finally, collect the colorless block crystals by filtration to obtain ligand L.
4. The method for preparing an organic ligand L according to claim 3, characterized in that: The method comprises the following steps: adding 4-hydroxypyridine (4mmol, 0.6g) and potassium carbonate (2.5mmol, 0.9g) to ethanol (30mL), stirring at 80°C for 4h, and then adding 1,2,4,5-tetrabromomethylbenzene (1mmol, 0.5g). After stirring at 80°C overnight, a yellow precipitate is formed. The solvent is removed to obtain a light yellow solid, which is washed with ether 3 times. A mixture of the obtained light yellow ligand mixture, DMF (1ml), distilled water (1ml) and CH3CN (1ml) is added to a glass bottle. The mixture is sealed and placed in an oven and heated at 90°C for 2 days, and then gradually cooled to room temperature at a rate of 5°C / h. Finally, the colorless block crystals are collected by filtration to obtain ligand L.
5. A compound SL-1 according to claim 2, characterized in that: The compound SL-1 uses organic ligand L and cadmium chloride as raw materials, and its preparation method comprises the following steps: S1. Mix cadmium chloride and organic ligand L in a molar ratio of 1 to 5:1, put into a reaction flask, and add methanol, acetonitrile and hydrochloric acid in a volume ratio of 1 to 2:1 to 3:1 into a reaction kettle; S2. The sealed pressure reactor is placed in an oven, the program is set, and the heating is performed for 1 to 2 hours, the temperature is raised from room temperature to 100 to 120 ° C, and the temperature is maintained for 40 to 60 hours, and then cooled after 8 to 12 hours; S3. After cooling to room temperature, white block crystals were obtained, which were filtered and washed with methanol to obtain pure crystals.
6. The method for preparing compound SL-1 according to claim 5, characterized in that: The following steps are included 10 mg, 0.02 mmol of L and 18 mg, 0.1 mmol of cadmium chloride were added to the reaction bottle, and then 1 mL of methanol, 1 mL of acetonitrile and 1 mL (0.1 mol / L) of hydrochloric acid were added, and the reactor was slightly shaken to mix evenly; then the reactor was placed in an oven, and the oven program was set to heat for 2 hours to increase the temperature from room temperature to 90°C, and this temperature was maintained for 48 hours, and then cooled to room temperature after 10 hours; finally, the resulting mixture was filtered and washed with methanol to obtain a white single crystal of the coordination compound SL-1.
Citation Information
Patent Citations
Cadmium-based two-dimensional hybrid perovskite long afterglow material and preparation method and application thereof
CN114316951A
Cd < 2 + >-based coordination compound SUST-WJ-12 as well as preparation method and application thereof
CN114891029A
Amino-functionalized metal organic framework MOFs long-afterglow coordination compound SUST-WZ-1 and preparation and application of amino-functionalized metal organic framework MOFs long-afterglow coordination compound SUST-WZ-1
CN114957696A
Metal organic complex-inorganic hybrid perovskite with multicolor adjustable continuous luminescence and cold white light emission
CN117417359A
Construction of adjustable multi-phosphorescence and long-lasting luminescence metal organic halide based on pyridine solvent
CN117466919A