Optical glass, preforms and optical components
By adjusting the content ratio of SiO2, Nb2O5, ZrO2, Li2O and Ln2O3, the balance problem of optical glass between low dispersion ratio and high devitrification resistance is solved, and high devitrification resistance and good reheating and pressing molding are achieved. , suitable for the production of optical components, reducing the impact of chromatic aberration.
Patent Information
- Application Number
- CN202080075029.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-11-07
- Filing Date
- 2020-09-18
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2040-09-18
AI Technical Summary
It is difficult for existing optical glasses to find a balance between low dispersion ratio and high devitrification resistance, and the reheating pressing moldability is poor, affecting the performance of optical components.
By adjusting the content ratios of SiO2, Nb2O5, ZrO2, Li2O and Ln2O3 in optical glass, the specific partial dispersion ratio and Abbe number relationship are met, and the liquid phase temperature is controlled below 1150℃ to improve the devitrification resistance of the glass and the re-resolution Heating pressing characteristics.
Optical glass with a partial dispersion ratio within the required range is achieved, with high devitrification resistance and good reheating press molding, which is suitable for the production of optical components and reduces the influence of chromatic aberration.
Smart Images

Figure CN114599617B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to optical glass and an optical element. Background Art
[0002] In the optical systems of digital cameras and video cameras, blurring called aberration exists in all images, although the degree of blurring varies. This aberration is classified into monochromatic aberration and chromatic aberration, and chromatic aberration in particular strongly depends on the material properties of the lens used in the optical system.
[0003] Generally, chromatic aberration can be corrected by combining a low-dispersion convex lens and a high-dispersion concave lens, but this combination can only correct the aberrations in the red and green regions, and the aberrations in the blue region still remain. The aberrations in the blue region that are not completely removed are called secondary spectrum. In order to correct the secondary spectrum, it is necessary to consider the trend of the g line (435.835nm) in the blue region for optical design. At this time, the partial dispersion ratio (θg, F) is used as an indicator of optical characteristics that are of concern in optical design. In the above-mentioned optical system in which a low-dispersion lens is combined with a high-dispersion lens, the secondary spectrum can be well corrected by using an optical material with a larger partial dispersion ratio (θg, F) for the lens on the low-dispersion side and an optical material with a smaller partial dispersion ratio (θg, F) for the lens on the high-dispersion side.
[0004] In recent years, in optical design, there is an increasing demand for glass with a small partial dispersion ratio (θg, F).
[0005] The partial dispersion ratio (θg, F) is expressed by the following equation (1).
[0006] θg,F=(n g -n F ) / (n F -n C )······(1)
[0007] In optical glass, the partial dispersion ratio (θg, F) and the Abbe number (ν d ) has a nearly linear relationship. The straight line representing this relationship is a line with the vertical axis representing the partial dispersion ratio (θg, F) and the horizontal axis representing the Abbe number (ν d ), the partial dispersion ratios of NSL7 and PBM2 and the Abbe number are plotted on the orthogonal coordinates of , and the straight line connecting the two points is represented and called the standard line. The standard glass used as the basis for the standard line varies depending on the optical glass manufacturer, but each company uses roughly the same slope and intercept to define it (NSL7 and PBM2 are optical glasses manufactured by Ohara Co., Ltd., and the Abbe number of PBM2 (ν d) is 36.3, the partial dispersion ratio (θg, F) is 0.5828, and the Abbe number (ν d ) is 60.5, and the partial dispersion ratio (θg, F) is 0.5436. )
[0008] As methods for making optical elements from optical glass, for example, there are known methods of grinding and polishing a blank or glass block formed of optical glass to obtain the shape of an optical element; a method of reheating a blank or glass block formed of optical glass and molding it (reheating and pressing) to obtain a glass molded body, and grinding and polishing the glass molded body; and a method of molding a preformed body obtained from a blank or glass block in a mold obtained by ultra-precision processing (precision press molding) to obtain the shape of an optical element. In any of the methods, it is required that stable glass can be obtained when the blank or glass block is formed from molten glass raw materials. Among them, when the stability (devitrification resistance) of the glass constituting the blank or glass block obtained against devitrification is reduced and crystallization occurs inside the glass, glass suitable for use as an optical element can no longer be obtained.
[0009] Prior art literature
[0010] Patent Literature
[0011] Patent Document 1: Japanese Patent Application Publication No. 2006-248897
[0012] Patent Document 2: Japanese Patent Application Publication No. 2012-240909
[0013] It is difficult to obtain the glass of Patent Document 1 having a small partial dispersion ratio (θg, F), and the devitrification property is also likely to be poor.
[0014] The glass of Patent Document 2 has the same technical problem to be solved, that is, to reduce the partial dispersion ratio (θg, F), but due to the inclusion of Ta 2 O 5 Since the component is an essential component, not only the production cost is high, but also the moldability is poor due to poor meltability. Summary of the invention
[0015] Technical problem to be solved by the invention
[0016] The present invention has been made in view of the above-mentioned technical problems, and an object of the present invention is to obtain an optical glass having a partial dispersion ratio (θg, F) within a desired range, high resistance to devitrification, and good reheating press moldability.
[0017] More specifically, it is to obtain a partial dispersion ratio (θg, F) and the Abbe number (ν d ) and satisfy (-0.00162×ν d+0.624≤(θg,F)≤(-0.00162×ν d +0.654), and the liquidus temperature is below 1150°C, and the reheating press moldability is good.
[0018] Solutions to technical problems
[0019] The inventors have conducted in-depth experimental research to solve the above technical problems and found that 2 Composition and Nb 2 O 5 In the glass with the same composition, by adjusting Ln 2 O 3 Composition and LiO 2 The relationship between the contents of the components enables production of an optical glass having a low partial dispersion ratio, high resistance to devitrification, and good reheating pressing characteristics, thereby completing the present invention.
[0020] (1) An optical glass comprising, in terms of mass % of oxide-converted composition:
[0021] 10.0~35.0%SiO 2 Element,
[0022] 10.0~40.0% Nb 2 O 5 Element,
[0023] 1.0~15.0% ZrO 2 Element,
[0024] 1.0~15.0%Li 2 O component, and
[0025] 1.0~20.0%Ln 2 O 3 component (wherein Ln is one or more selected from the group consisting of La, Y, Gd, and Yb),
[0026] Mass ratio (Li 2 O+La 2 O 3 ) / SiO 2 is 0.35 or more,
[0027] Mass ratio Li 2 O / (Li 2 O+Na 2 O+K 2 O) is 0.50 or more,
[0028] Partial dispersion ratio (θg, F) and Abbe number (ν d) and satisfy (-0.00162×ν d +0.624≤(θg,F)≤(-0.00162×ν d +0.654).
[0029] (2) The optical glass according to (1), which contains, in terms of mass % of the oxide conversion composition:
[0030] 0~20.0%B 2 O 3 Element,
[0031] 0~20.0%La 2 O 3 Element,
[0032] 0~20.0% CaO content,
[0033] 0~20.0% SrO component,
[0034] 0~20.0% BaO component,
[0035] 0~10.0% Na 2 O ingredient.
[0036] (3) The optical glass according to (1) or (2), wherein:
[0037] With B 2 O 3 Compared with the ingredients, it contains more SiO 2 Element,
[0038] Mass ratio (ZnO+TiO 2 +P 2 O 5 ) / (ZrO 2 +La 2 O 3 +LiO 2 ) is less than 0.15,
[0039] The mass and BaO+CaO+SrO are 5.0~20.0%.
[0040] (4) The optical glass according to any one of (1) to (3), wherein the refractive index (n d ) is 1.70000~1.80000, and the Abbe number (ν d ) is 30.00~40.00.
[0041] (5) The optical glass according to any one of (1) to (4), wherein the liquidus temperature is 1150° C. or lower.
[0042] (6) An optical element made of the optical glass described in any one of (1) to (5).
[0043] (7) A preform for grinding and / or precision press molding, made of the optical glass described in any one of (1) to (5).
[0044] (8) An optical device comprising the optical element described in (6) or (7).
[0045] According to the present invention, it is possible to obtain an optical glass having a low partial dispersion ratio (θg, F), a low liquidus temperature, and good reheating press moldability. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] Figure 1 The partial dispersion ratio (θg, F) and the Abbe number (ν d )’s relationship diagram. DETAILED DESCRIPTION
[0047] Hereinafter, the embodiments of the optical glass of the present invention will be described in detail, but the present invention is not limited to the following embodiments, and can be appropriately changed and implemented within the scope of the purpose of the present invention. It should be noted that the description of the repeated parts may be appropriately omitted, which will not limit the purpose of the invention.
[0048] [Glass composition]
[0049] The composition range of each component constituting the optical glass of the present invention is as follows. In this specification, unless otherwise specifically denied, the content of each component is expressed in terms of mass % of the oxide-converted composition relative to the total mass of the glass. Here, the "oxide-converted composition" means that the composition of each component contained in the glass electrolyte is expressed by assuming that the oxides, complex salts, metal fluorides, etc. used as raw materials of the glass composition components of the present invention are all decomposed and converted into oxides during melting, and the total mass of the generated oxides is recorded as 100 mass %.
[0050] <About essential ingredients and optional ingredients>
[0051] SiO 2 The component is an essential component, and can promote stable glass formation and reduce devitrification (generation of crystals) which is undesirable as an optical glass.
[0052] In particular, by making SiO 2 When the content of SiO is 10.0% or more, the partial dispersion ratio can be greatly improved and the devitrification resistance can be excellent. In addition, the liquidus temperature can be lowered. 2The lower limit of the content is preferably 10.0% or more, more preferably 13.0% or more, still more preferably 15.0% or more, further preferably 18.0% or more, and most preferably 20.0% or more.
[0053] On the other hand, by making SiO 2 The content of the component is 35.0% or less, which can suppress the increase of the partial dispersion ratio. 2 The upper limit of the content of the component is preferably 35.0% or less, more preferably 33.0% or less, and most preferably 31.0% or less.
[0054] Nb 2 O 5 The component is an essential component, and can increase the refractive index and reduce the Abbe number.
[0055] In particular, by making Nb 2 O 5 The content of Nb is 10.0% or more, which can increase the refractive index. 2 O 5 The lower limit of the content of the component is preferably 10.0% or more, more preferably 12.0% or more, still more preferably 15.0% or more, further preferably 20.0% or more, and most preferably 23.0% or more.
[0056] On the other hand, by making Nb 2 O 5 The content of Nb is 40.0% or less, which can provide thermal stability and reduce the material cost of glass. Furthermore, it can reduce the devitrification of glass. 2 O 5 The upper limit of the content of the component is preferably 40.0% or less, more preferably 38.0% or less, still more preferably 36.0% or less, and most preferably 34.0% or less.
[0057] ZrO 2 The component is a necessary component, which can increase the refractive index and Abbe number of the glass and reduce the partial dispersion ratio.
[0058] In particular, by making ZrO 2 The content of the component is 1.0% or more, which can reduce the partial dispersion ratio and obtain stable glass. 2 The lower limit of the content of the component is preferably 1.0% or more, more preferably 2.0% or more, still more preferably 3.0% or more, further preferably 5.0% or more, and most preferably 6.0% or more.
[0059] On the other hand, by making ZrO 2The content of the component is 15.0% or less, which can reduce devitrification and make it easier to obtain more homogeneous glass. 2 The upper limit of the content of the component is preferably 15.0% or less, more preferably 12.0% or less, still more preferably 11.0% or less, further preferably 10.0% or less, and most preferably 9.0% or less.
[0060] Li 2 The O component, unlike other alkali metals, is an essential component capable of reducing the partial dispersion ratio.
[0061] In particular, by making Li 2 The content of O component is 1.0% or more, which can improve the melting property of glass and reduce the partial dispersion ratio. 2 The lower limit of the content of the component O is preferably 1.0% or more, more preferably 1.5% or more, still more preferably 2.0% or more, and most preferably 2.5% or more.
[0062] On the other hand, by making Li 2 The content of the O component is 15.0% or less, and devitrification due to excessive content can be reduced, and devitrification during reheating and pressing can also be reduced.
[0063] Therefore, Li 2 The upper limit of the content of the component O is preferably 15.0% or less, more preferably 12.0% or less, still more preferably 10.0% or less, further preferably 9.0% or less, and most preferably 8.0% or less.
[0064] B 2 O 3 The component is an optional component, and can promote stable glass formation, lower the liquidus temperature, improve the devitrification resistance, and improve the solubility of the glass raw material.
[0065] In particular, by making B 2 O 3 The content of the component is 0% or more, which can suppress the increase of liquidus temperature. 2 O 3 The lower limit of the content of the component is preferably 0% or more, more preferably greater than 0%, still more preferably 0.1% or more, further preferably 0.2% or more, and most preferably 0.3% or more.
[0066] On the other hand, by making B 2 O 3 The content of the component is 20.0% or less, which can suppress the decrease of the refractive index and the increase of the partial dispersion ratio. 2 O 3The upper limit of the content of the component is preferably 20.0% or less, more preferably 18.0% or less, still more preferably 16.0% or less, still more preferably 14.0% or less, further preferably 12.0% or less, and most preferably 11.0% or less.
[0067] With B 2 O 3 Compared with the components, it is preferred to contain more SiO 2 Ingredients. 2 O 3 Composition ratio SiO 2 When there are many components, the partial dispersion ratio will increase, so by 2 O 3 Contains more SiO than 2 composition, which can stabilize the glass and reduce the partial dispersion ratio at the same time.
[0068] La 2 O 3 The component is a component that can reduce devitrification and decrease the partial dispersion ratio. The inclusion of this component can produce effects different from other rare earth components that are prone to devitrification.
[0069] In particular, by making La 2 O 3 The content of the component is 0% or more, the refractive index can be increased, and by adjusting within the range of the components of the present invention, the anomalous dispersion can be reduced. 2 O 3 The lower limit of the content of the component is preferably 0% or more, more preferably 1.0% or more, still more preferably 2.0% or more, further preferably 3.0% or more, further preferably 4.0% or more, and most preferably 5.0% or more.
[0070] On the other hand, by making La 2 O 3 The content of the component is 20.0% or less, which can suppress the increase of the Abbe number, reduce devitrification, and reduce coloration. 2 O 3 The upper limit of the content of the component is preferably 20.0% or less, more preferably 19.0% or less, still more preferably 17.0% or less, and most preferably 16.0% or less.
[0071] G 2 O 3 Ingredients, Y 2 O 3 Ingredients and Yb 2 O 3 The components are arbitrary components, and when the content of any one of them is at least greater than 0%, the refractive index can be increased and the partial dispersion ratio can be reduced.
[0072] On the other hand, Gd 2 O 3 Ingredients, Y 2 O 3 Ingredients and Yb 2 O 3 Components, when contained in large quantities, will lower the liquidus temperature and cause the glass to lose clarity.
[0073] In particular, by making Gd 2 O 3 Ingredients,Y 2 O 3 Ingredients and Yb 2 O 3 The content of each component is 10.0% or less, which can reduce devitrification and coloration. 2 O 3 Ingredients,Y 2 O 3 Ingredients and Yb 2 O 3 The upper limit of the content of each component is preferably 10.0% or less, more preferably 8.0% or less, further preferably 5.0% or less, and most preferably 3.0% or less.
[0074] Na 2 O component and K 2 The O component is an optional component. When the content thereof is greater than 0%, the meltability of the glass raw material can be improved and coloring can be reduced.
[0075] On the other hand, Na 2 O component and K 2 When the component O is contained in a large amount, the stability of the glass deteriorates and the devitrification resistance decreases.
[0076] On the other hand, by making Na 2 O component and K 2 The content of O component is 10.0% or less, which can reduce devitrification. 2 O component and K 2 The upper limit of the content of the component O is preferably 10.0% or less, more preferably 8.0% or less, still more preferably 7.0% or less, further preferably 6.0% or less, and most preferably 5.0% or less.
[0077] The MgO component is an arbitrary component that can improve solubility and lower the liquidus temperature. However, when the MgO component is contained in a large amount, the glass will devitrify.
[0078] On the other hand, devitrification can be reduced by making the content of the MgO component 10.0% or less. Therefore, the upper limit of the content of the MgO component is preferably 10.0% or less, more preferably 8.0% or less, still more preferably 5.0% or less, further preferably 3.0% or less, and most preferably 2.0% or less.
[0079] The CaO component is an optional component, and can improve the stability of glass.
[0080] In particular, the melting property can be improved by making the content of the CaO component 0% or more. Therefore, the lower limit of the content of the CaO component is preferably 0% or more, more preferably 0.1% or more, still more preferably 0.5% or more, further preferably 1.0% or more, and most preferably 2.0% or more.
[0081] On the other hand, by making the content of the CaO component 20.0% or less, the press moldability becomes better and the increase of the partial dispersion ratio can be suppressed. Therefore, the upper limit of the content of the CaO component is preferably 20.0% or less, more preferably 17.0% or less, still more preferably 14.0% or less, further preferably 12.0% or less, and most preferably 10.0% or less.
[0082] The SrO component is an optional component, and can improve the stability of glass.
[0083] On the other hand, by making the content of the SrO component 20.0% or less, the press moldability becomes better and the increase of the partial dispersion ratio can be suppressed. Therefore, the upper limit of the content of the SrO component is preferably 20.0% or less, more preferably 17.0% or less, still more preferably 14.0% or less, further preferably 12.0% or less, and most preferably 10.0% or less.
[0084] The BaO component is an optional component, and can improve the stability of glass.
[0085] On the other hand, by making the content of BaO component 20.0% or less, press moldability becomes better and the increase of partial dispersion ratio can be suppressed. Therefore, the upper limit of the content of BaO component is preferably 20.0% or less, more preferably 17.0% or less, still more preferably 14.0% or less, further preferably 12.0% or less, and most preferably 10.0% or less.
[0086] TiO 2 The component is any component that can increase the refractive index and reduce the Abbe number. 2 When a large amount of components is contained, the partial dispersion ratio becomes larger.
[0087] In particular, by making TiO 2The content of the component is 10.0% or more, which can suppress the increase of the partial dispersion ratio and reduce the Abbe number. 2 The upper limit of the content of the component is preferably 10.0% or less, more preferably 5.0% or less, still more preferably 3.0% or less, and most preferably 2.0% or less.
[0088] The ZnO component is an optional component that is inexpensive and can adjust the glass to a high dispersion side. On the other hand, when the ZnO component is contained in a large amount, the partial dispersion ratio increases.
[0089] In particular, by making the content of the ZnO component 10.0% or less, devitrification and coloring can be reduced. Therefore, the upper limit of the content of the ZnO component is preferably 10.0% or less, more preferably 5.0% or less, still more preferably less than 3.0%, and most preferably 1.0% or less.
[0090] Ta 2 O 5 The component is an arbitrary component, and can increase the refractive index, reduce the Abbe number and the partial dispersion ratio, and improve the resistance to devitrification.
[0091] In particular, by making Ta 2 O 5 The content of the component is less than 10.0%, which can reduce Ta, a rare mineral resource. 2 O 5 The amount of components used is reduced, and the glass is also easier to melt at a lower temperature, so the production cost of the glass can be reduced. In addition, this can reduce Ta 2 O 5 The excess content of the component causes the devitrification of the glass. 2 O 5 The upper limit of the content of the component is preferably 10.0% or less, more preferably 5.0% or less, still more preferably 3.0% or less, and most preferably 1.0% or less. In particular, from the viewpoint of reducing the material cost of the glass, it is most preferred not to contain Ta. 2 O 5 Element.
[0092] WO 3 The component is an arbitrary component that can increase the refractive index and reduce the Abbe number, and can also improve the solubility of the glass raw material. 3 The content of the component is 10.0% or less, which can make the partial dispersion ratio of the glass difficult to increase, reduce the coloring of the glass and improve the internal transmittance. 3 The upper limit of the content of the component is preferably 10.0% or less, more preferably 5.0% or less, still more preferably 3.0% or less, and most preferably 1.0% or less.
[0093] P 2 O 5 The component is an arbitrary component that can improve the stability of the glass.
[0094] On the other hand, by making P 2 O 5 The content of the component is less than 10.0%, which can reduce P 2 O 5 The excess content of the component leads to an increase in the partial dispersion ratio. 2 O 5 The upper limit of the content of the component is preferably 10.0% or less, more preferably 5.0% or less, still more preferably 3.0% or less, further preferably less than 2.0%, and most preferably 1.0% or less.
[0095] GeO 2 The component is an arbitrary component that can increase the refractive index and reduce devitrification. 2 The content of the component is less than 10.0%, which can reduce the expensive GeO 2 The amount of components used can reduce the material cost of glass. 2 The upper limit of the content of the component is preferably 10.0% or less, more preferably 5.0% or less, still more preferably 3.0% or less, and most preferably 1.0% or less.
[0096] Al 2 O 3 The component is an optional component, and can increase the refractive index and improve the resistance to devitrification.
[0097] On the other hand, by making Al 2 O 3 The content of the component is 10.0% or less, which can reduce Al 2 O 3 The excess content of Al leads to devitrification. 2 O 3 The upper limit of the content of the component is preferably 10.0% or less, more preferably 5.0% or less, still more preferably 3.0% or less, and most preferably 1.0% or less.
[0098] Ga 2 O 3 The component is an optional component, and can increase the refractive index and improve the resistance to devitrification.
[0099] On the other hand, by making Ga 2 O 3 The content of the component is 10.0% or less, which can reduce Ga 2 O 3The excess content of the component causes devitrification. 2 O 3 The upper limit of the content of the component is preferably 10.0% or less, more preferably 5.0% or less, still more preferably 3.0% or less, and most preferably 1.0% or less.
[0100] Bi 2 O 3 The component is an arbitrary component that can increase the refractive index and reduce the Abbe number, and can also reduce the glass transition point. 2 O 3 The content of the component is 10.0% or less, which can make the partial dispersion ratio difficult to increase, reduce the coloring of the glass and improve the internal transmittance. 2 O 3 The upper limit of the content of the component is preferably 10.0% or less, more preferably 5.0% or less, still more preferably 3.0% or less, and most preferably 1.0% or less.
[0101] TeO 2 The component is an arbitrary component that can increase the refractive index, reduce the partial dispersion ratio, and reduce the glass transition point. 2 The content of the component is 10.0% or less, which can reduce the coloring of the glass and improve the internal transmittance. In addition, by reducing the expensive TeO 2 The use of TeO can produce glass with lower material cost. 2 The upper limit of the content of the component is preferably 10.0% or less, more preferably 5.0% or less, still more preferably 3.0% or less, and most preferably 1.0% or less. In particular, from the viewpoint of reducing the material cost of the glass, TeO may not be contained. 2 Element.
[0102] SnO 2 It is an optional component that can clarify (defoam) the molten glass and improve the visible light transmittance of the glass. 2 The content of SnO is less than 1.0%, which can make it difficult for the glass to be colored or devitrified due to the reduction of the molten glass. 2 Alloying with melting equipment (especially precious metals such as Pt) can extend the life of the melting equipment. 2 The upper limit of the content is preferably 1.0% or less, more preferably 0.5% or less, and further preferably 0.1% or less.
[0103] Sb 2 O 3The component can promote the defoaming of the glass and make the glass clear, and is an arbitrary component in the optical glass of the present invention. 2 O 3 The content of the component relative to the total mass of the glass is 1.0% or less, which can make it difficult for excessive foaming to occur during glass melting and can make Sb 2 O 3 The components are difficult to alloy with melting equipment (especially precious metals such as Pt). Therefore, the Sb content compared to the total mass of the glass in terms of oxide conversion composition is 2 O 3 The upper limit of the content of the component is preferably 1.0% or less, more preferably 0.5% or less, still more preferably 0.3% or less, and most preferably 0.1% or less.
[0104] It should be noted that the components that make the glass clear and defoaming are not limited to the above-mentioned Sb 2 O 3 As the component, a clarifier, a defoamer or a combination thereof known in the glass manufacturing field can be used.
[0105] In Ln 2 O 3 When the sum (mass sum) of the contents of the components (wherein Ln is one or more selected from the group consisting of La, Y, Gd, and Yb) is 1.0% or more, the refractive index can be increased and the partial dispersion ratio can be reduced. 2 O 3 The lower limit of the total amount of the components is preferably 1.0% or more, more preferably 3.0% or more, further preferably 5.0% or more, and most preferably 7.0% or more.
[0106] On the other hand, by making Ln 2 O 3 The sum of the contents (mass sum) of the components is 20.0% or less to reduce devitrification caused by excess content. Therefore, the upper limit is preferably 20.0% or less, more preferably 18.0% or less, still more preferably 17.0% or less, and most preferably 16.0% or less.
[0107] In R 2 When the total content (mass sum) of the O component (wherein Rn is one or more selected from the group consisting of Li, Na, and K) is 1.0% or more, the stability of the glass can be improved. 2 The lower limit of the sum of the O components is preferably 1.0% or more, more preferably 2.5% or more, further preferably 3.0% or more, and most preferably 3.5% or more.
[0108] On the other hand, by making Rn 2The sum of the contents (mass sum) of the O components is 15.0% or less, which can suppress the decrease in refractive index and reduce devitrification caused by excessive content. Therefore, the upper limit is preferably 15.0% or less, more preferably 14.0% or less, still more preferably 13.0% or less, and most preferably 12.0% or less.
[0109] When the sum of the contents of RO components (wherein R is one or more selected from the group consisting of Mg, Ca, Sr, and Ba) is 5.0% or more, the low temperature melting property can be improved. Therefore, the sum of the contents of RO components preferably has a lower limit of 5.0%, more preferably 5.3% or more, further preferably 5.8% or more, and most preferably 6.0% or more.
[0110] On the other hand, the sum of the contents of the RO components is preferably 20.0% or less in order to suppress the reduction in devitrification resistance due to excessive content. Therefore, the upper limit of the mass sum of the RO components is preferably 20.0% or less, more preferably 19.0% or less, still more preferably 18.0% or less, and most preferably 16.0% or less.
[0111] When the mass sum of BaO+CaO+SrO is 5.0% or more, the low temperature melting property can be improved. Therefore, the mass sum of BaO+CaO+SrO preferably has a lower limit of 5.0% or more, more preferably 5.3% or more, further preferably 5.8% or more, and most preferably 6.0% or more.
[0112] On the other hand, when the content of BaO+CaO+SrO is excessive, the refractive index and dispersion will increase, it will be difficult to obtain the desired optical properties, and the devitrification will deteriorate, so it is preferably 20.0% or less. Therefore, the upper limit of the content of BaO+CaO+SrO is preferably 20.0% or less, more preferably 19.0% or less, further preferably 18.0% or less, and most preferably 16.0% or less.
[0113] In the mass ratio (Li 2 O+La 2 O 3 ) / SiO 2 When the mass ratio (Li) is 0.35 or more, the glass can be stabilized and the partial dispersion ratio can be reduced. 2 O+La 2 O 3 ) / SiO 2 The lower limit is preferably 0.35 or more, more preferably 0.36 or more, further preferably 0.38 or more, and most preferably 0.40 or more.
[0114] On the other hand, the mass ratio (Li 2 O+La 2O 3 ) / SiO 2 , in order to suppress the increase of liquidus temperature, it is preferably less than 1.00. 2 O+La 2 O 3 ) / SiO 2 The upper limit is preferably 1.00 or less, more preferably 0.90 or less, further preferably 0.88 or less, and most preferably 0.85 or less.
[0115] In mass ratio Li 2 O / (Li 2 O+Na 2 O+K 2 When the value of LiO is 0.50 or more, the LiO 2 The effect of the component is the best, which can increase the solubility and inhibit devitrification. 2 O / (Li 2 O+Na 2 O+K 2 O), the lower limit of which is preferably 0.50 or more, more preferably 0.52 or more, further preferably 0.54 or more, and most preferably 0.55 or more.
[0116] In mass ratio (SiO 2 +B 2 O 3 +Ln 2 O 3 ) / Rn 2 When the mass ratio (SiO) is 3.50 or more, devitrification can be suppressed and the liquidus temperature can be lowered. 2 +B 2 O 3 +Ln 2 O 3 ) / Rn 2 O, and its lower limit is preferably 3.50 or more, more preferably 3.55 or more, further preferably greater than 3.58, and most preferably 3.60 or more.
[0117] On the other hand, in the mass ratio (SiO 2 +B 2 O 3 +Ln 2 O 3 ) / Rn 2 When O is 12.0 or less, the Abbe number (ν d ). Therefore, the mass ratio (SiO 2 +B 2 O 3 +Ln 2 O3 ) / Rn 2 O, and the upper limit thereof is preferably 12.0 or less, more preferably 11.80 or less, further preferably 11.50 or less, and most preferably 11.20 or less.
[0118] In the mass ratio (ZnO+TiO 2 +P 2 O 5 ) / (ZrO 2 +La 2 O 3 +LiO 2 ) is less than 0.15, it is possible to suppress the ZnO component, TiO 2 Ingredients and P 2 O 5 Therefore, the mass ratio (ZnO+TiO 2 +P 2 O 5 ) / (ZrO 2 +La 2 O 3 +LiO 2 ), the upper limit of which is preferably less than 0.15, more preferably below 0.12, further preferably below 0.10, and most preferably below 0.08.
[0119] <About ingredients that should not be contained>
[0120] Next, components that should not be contained in the optical glass of the present invention and components that are preferably not contained are described.
[0121] Other components can be added as needed within the range that does not impair the characteristics of the glass of the present invention. However, in addition to Ti, Zr, Nb, W, La, Gd, Y, Yb, and Lu, various transition metal components such as V, Cr, Mn, Fe, Co, Ni, Cu, Ag, and Mo have the property of coloring the glass even in a small amount when contained alone or in a composite form, and absorbing light of a specific wavelength in the visible light region. Therefore, it is preferably substantially not contained in optical glasses using wavelengths in the visible light region.
[0122] In addition, lead compounds such as PbO and As 2 O 3 Arsenic compounds such as these are components that have a high environmental burden, and therefore, they are preferably not substantially contained, that is, not contained at all except for unavoidable contamination.
[0123] In addition, Th, Cd, Tl, Os, Be and Se are each considered harmful chemical substances and are therefore avoided in recent years. Environmental measures must be taken not only in the glass manufacturing process but also in the processing process and until the waste treatment after the glass is manufactured. Therefore, when the environmental impact is important, it is preferred that these components are not substantially contained.
[0124] [Manufacturing method]
[0125] The optical glass of the present invention can be produced, for example, as follows. For example, the above raw materials are uniformly mixed so that each component is within a specified content range, and the thus produced mixture is placed in a platinum crucible, a quartz crucible or an alumina crucible for rough melting, and then placed in a gold crucible, a platinum crucible, a platinum alloy crucible or an iridium crucible, and melted at a temperature range of 1000 to 1400° C. for 2 to 5 hours, and then stirred for homogenization and defoaming, etc., and then the temperature is lowered to 950 to 1250° C., and fine stirring is performed to remove grains, and then the mixture is cast into a mold and slowly cooled to produce the glass.
[0126] <Physical Properties>
[0127] The optical glass of the present invention has a refractive index (n d ) and the Abbe number (ν d ).
[0128] The refractive index (n d ), the lower limit of which is preferably 1.70000 or more, more preferably 1.73000 or more, and further preferably 1.75000 or more. The upper limit of the refractive index is preferably 1.80000 or less, and more preferably 1.79000 or less.
[0129] The Abbe number (ν d ), the lower limit of which is preferably 30.00 or more, more preferably 32.00 or more, and still more preferably 33.00 or more. On the other hand, the Abbe number (ν d ), and its upper limit is preferably 40.00 or less, more preferably 38.00 or less, and further preferably 37.00 or less.
[0130] The optical glass of the present invention having such a refractive index and Abbe number is useful in optical design, and in particular, can realize high imaging characteristics and also can realize miniaturization of the optical system, thereby increasing the degree of freedom in optical design.
[0131] The optical glass of the present invention has a relatively low partial dispersion ratio (θg, F).
[0132] More specifically, the partial dispersion ratio (θg, F) of the optical glass of the present invention is preferably 0.560 or more, more preferably 0.565 or more, although the lower limit thereof is not particularly limited. On the other hand, the upper limit of the partial dispersion ratio (θg, F) of the optical glass of the present invention is preferably 0.600 or less, more preferably 0.595 or less, and further preferably 0.593 or less. In addition, the partial dispersion ratio (θg, F) of the optical glass of the present invention is related to the Abbe number (ν d ), preferably satisfying (-0.00162×ν d +0.624)≤(θg,F)≤(-0.00162×ν d +0.654).
[0133] Thus, the optical glass of the present invention contains a large amount of SiO 2 Composition and Nb 2 O 5 Compared with conventionally known glasses having a composition of 1.5-1.5 nm, the optical glass has a lower partial dispersion ratio (θg, F). Therefore, an optical element formed of the optical glass can be suitably used for correcting chromatic aberration.
[0134] Here, the Abbe number (ν d ) is related to the partial dispersion ratio (θg, F), and although its lower limit is not particularly limited, it is preferably within (-0.00162×ν d +0.624) or more, more preferably (-0.00162×ν d +0.627) or more, and more preferably (-0.00162×ν d On the other hand, the optical glass of the present invention has an Abbe number (ν d The upper limit of the partial dispersion ratio (θg, F) is preferably (-0.00162×ν d +0.654) or less, more preferably (-0.00162×ν d +0.651) or less, and more preferably (-0.00162×ν d +0.648) or less.
[0135] The optical glass of the present invention preferably has a high visible light transmittance, particularly a high transmittance of light on the short wavelength side of visible light, and thus has little coloration.
[0136] In particular, the optical glass of the present invention, when expressed in terms of glass transmittance, has a wavelength (λ 80 ), and its upper limit is preferably below 420nm, more preferably below 417nm, and further preferably below 410nm.
[0137] In addition, the shortest wavelength (λ) of the optical glass of the present invention when the spectral transmittance of the sample having a thickness of 10 mm is 5% 5 ), and its upper limit is preferably below 345nm, more preferably below 343nm, and further preferably below 342nm.
[0138] Thus, since the absorption edge of the glass is located near the ultraviolet region and the transparency of the glass to visible light is improved, the optical glass can be preferably used as an optical element that transmits light, such as a lens.
[0139] The optical glass of the present invention preferably has a high resistance to devitrification, and more specifically, preferably has a low liquidus temperature.
[0140] That is, the upper limit of the liquidus temperature of the optical glass of the present invention is preferably 1150°C or lower, more preferably 1148°C or lower, and even more preferably 1145°C or lower. Thus, even if the melted glass is discharged at a lower temperature, the crystallization of the produced glass is reduced, so that devitrification when the glass is formed from a molten state can be reduced, and the influence on the optical characteristics of the optical element using the glass can be reduced. In addition, even if the melting temperature of the glass is low, the glass can be molded, so the energy consumed when the glass is molded can be reduced, and thus the manufacturing cost of the glass can be reduced.
[0141] [Preform and optical element]
[0142] For example, a glass molded body can be produced from the produced optical glass by using a compression molding method such as reheating compression molding or precision compression molding. That is, a preform for compression molding is produced from the optical glass, and the preform is reheated and compression molded, and then ground to produce a glass molded body; or, for example, a preform produced by grinding is precision-pressed to produce a glass molded body. In addition, the method for producing a glass molded body is not limited to the above methods.
[0143] The glass molded body produced in this way can be used for various optical elements, and can be used for optical elements such as lenses and prisms, among which it is particularly preferred. As a result, the color blurring caused by chromatic aberration in the transmitted light of the optical system provided with the optical element can be reduced. Therefore, when the optical element is used in a camera, the photographic object can be more accurately represented, and when the optical element is used in a projector, the desired image can be projected more clearly.
[0144] Example
[0145] The compositions of the embodiments (No. 1 to No. 20) of the present invention and the comparative example A, and the refractive index (n d ), Abbe number (νd ), partial dispersion ratio (θg, F), liquidus temperature, transmittance λ 5 and λ 80 The results are shown in Tables 1 and 2. It should be noted that the following examples are only for illustration and are not limited to these examples.
[0146] The glasses of the embodiments and comparative examples are prepared using high-purity raw materials such as oxides, hydroxides, carbonates, nitrates, fluorides and metaphosphate compounds corresponding to the components thereof, which are commonly used in optical glasses. These raw materials are weighed and uniformly mixed in the proportions of the compositions of the embodiments and comparative examples shown in the table, and then put into a stone crucible (a platinum crucible or an alumina crucible may also be used depending on the solubility of the glass). After being melted in an electric furnace for 0.5 to 5 hours at a temperature range of 1100 to 1400°C depending on the melting difficulty of the glass composition, the glass is transferred to a platinum crucible for stirring and homogenization and defoaming, etc. The temperature is then lowered to 1000 to 1200°C and, after stirring and homogenization, is cast into a mold and slowly cooled to produce glass.
[0147] The refractive index (n d ), Abbe number (ν d ) and partial dispersion ratio (θg, F) are measured in accordance with the V-block method specified in JIS B 7071-2:2018. Here, the refractive index (n d ), expressed as the measured value of the d line (587.56nm) of a helium lamp. In addition, the Abbe number (ν d ), using the refractive index for the d-line of a helium lamp (n d ), the refractive index (n F ), the refractive index (n C ) value, according to the Abbe number (ν d )=[(n d -1) / (n F -n C )] is calculated using the formula of θg, F. In addition, the partial dispersion ratio (θg, F) is calculated using the refractive index (n g ), the refractive index (n F ), the refractive index (n C ) value, according to the partial dispersion ratio (θg, F) = (n g -n F ) / (n F -n C ) is calculated using the formula. These refractive indices (n d ), Abbe number (νd ) and the partial dispersion ratio (θg, F) are obtained by measuring the glass obtained at a slow cooling rate of -25°C / hr.
[0148] And, according to the Abbe number (ν d ) and the value of the partial dispersion ratio (θg, F), and the relationship (θg, F) = -a 2 ×ν d +b 2 The slope a 2 The intercept b is 0.00162 2 .
[0149] The transmittance of the glass of the embodiment and the comparative example is measured according to the standard JOGIS02-2003 of the Japan Optical Glass Industry Association. In addition, in the present invention, by measuring the transmittance of the glass, the presence and degree of coloration of the glass can be obtained. Specifically, according to JIS Z8722, the spectral transmittance of the parallel grinding piece with a thickness of 10 ± 0.1 mm from 200 nm to 800 nm is measured, and the wavelength (λ) at which the spectral transmittance is 80% and 5% is obtained. 80 , 5 ).
[0150] The liquidus temperature of the glass of the embodiment and the comparative example was measured by placing the crushed glass sample on a platinum plate at intervals of 10 mm, keeping it in a furnace with a temperature gradient from 800°C to 1200°C for 30 minutes, taking it out, and observing the glass sample with a microscope with a magnification of 80 times for the presence or absence of crystallization after cooling. At this time, the optical glass was crushed into particles with a diameter of about 2 mm as a sample.
[0151]
Table 1
[0152]
[0153]
Table 2
[0154]
[0155] As shown in the table, the optical glass of the embodiments of the present invention has a refractive index (n d ) are all above 1.70000 and all below 1.80000, within the required range.
[0156] In addition, the optical glass of the embodiment of the present invention has an Abbe number (ν d ) are all above 30.00 and below 40.00, which is within the required range.
[0157] As shown in the table, the optical glass of the embodiments of the present invention has an Abbe number (ν d) and the partial dispersion ratio (θg, F) satisfy the relationship (-0.00162×ν d +0.624)≤(θg,F)≤(-0.00162×ν d +0.654).
[0158] As shown in the table, the liquidus temperature of the optical glass of the embodiment of the present invention is below 1150° C. It can also be inferred that the optical glass of the embodiment of the present invention has better reheating press moldability due to its low liquidus temperature.
[0159] As shown in the table, the wavelength (λ 80 ) are all below 420nm, and the wavelength (λ 5 ) are all below 345nm.
[0160] The glass of Comparative Example A, mass ratio (Li 2 O+La 2 O 3 ) / SiO 2 Less than 0.35, so devitrification is serious and vitrification fails.
[0161] Although the present invention has been described in detail above for the purpose of illustration, the purpose of this embodiment is only for illustration, and it should be fully understood that those skilled in the art can make many changes to the present invention without departing from the spirit and scope of the present invention.
[0162] The disclosures of the documents described in this specification and the Japanese application specification that is the Paris priority basis of the present application (including the specification, drawings, and claims) are all incorporated herein by reference.
Claims
1. An optical glass, wherein: In terms of mass % of oxide conversion composition, it contains: 10.0~30.00% SiO2 content, 10.0~40.0% Nb2O5 composition, 1.0~15.0% ZrO2 composition, 1.0-15.0% Li2O content, and 1.0 to 20.0% of Ln2O3 (wherein Ln is at least one selected from the group consisting of La, Y, Gd, and Yb), and The mass ratio (Li2O + La2O3) / SiO2 is 0.53 or more and 0.83 or less, The mass ratio Li2O / (Li2O+Na2O+K2O) is 0.50 or more, The mass ratio (SiO2 + B2O3 + Ln2O3) / Rn2O is 3.60 or more and 6.77 or less, wherein Rn is at least one selected from the group consisting of Li, Na, and K, The mass ratio (ZnO + TiO2 + P2O5) / (ZrO2 + La2O3 + Li2O) is less than 0.04, The liquidus temperature is below 1126°C. Abbe number (ν d ) is 35.20~40.00, Partial dispersion ratio (θg, F) and Abbe number (ν d ) and satisfy (-0.00162×ν d +0.624)≤(θg,F)≤(-0.00162×ν d +0.654).
2. The optical glass according to claim 1, wherein: In terms of mass % of oxide conversion composition, it contains: 0~20.0% B2O3 content, 0~20.0% La2O3 composition, 0~20.0% CaO content, 0~20.0% SrO composition, 0 to 20.0% BaO content, and 0~10.0% Na2O content.
3. The optical glass according to claim 1 or 2, wherein: Compared with B2O3, it contains more SiO2. The mass and BaO+CaO+SrO are 5.0~20.0%.
4. The optical glass according to claim 1 or 2, wherein: Refractive index (n d ) is 1.70000~1.80000.
5. The optical glass according to claim 3, wherein: Refractive index (n d ) is 1.70000~1.80000.
6. An optical element made of the optical glass according to any one of claims 1 to 5.
7. A preform for grinding and / or precision press molding made of the optical glass according to any one of claims 1 to 5.
8. An optical device comprising the optical element according to claim 6.
Citation Information
Patent Citations
Optical glass, glass gob for press molding and optical element
JP2006248897A
Optical glass, preform and optical element
JP2012240909A
High refraction and low dispersion optical glass
CN101386469A
Optical Glass And Optical Element
CN102372430A
Optical glass and optical component
CN104926110A