A cosmetic transparent colored cosmetic ingredient that may change color automatically when exposed to ultraviolet light

By combining photochromic molecules with polymers in cosmetics, using transesterification reactions to ensure that cosmetics automatically change their colors under ultraviolet light, it solves the problem that existing cosmetics are difficult to maintain transparency and automatic discoloration, while maintaining moisturizing and beauty functions. The innovative effect of color changes has been achieved.

CN115209869BActive Publication Date: 2024-12-03INTERCOS SPA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180014129.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-02-17
Filing Date
2021-02-15
Publication Date
2024-12-03
Estimated Expiration
2041-02-15

AI Technical Summary

Technical Problem

Existing cosmetics are difficult to remain transparent in all forms and conditions of use, while automatically changing colors under ultraviolet irritation, and the operation of introducing new molecules into cosmetics is complex, which may affect skin safety.

Method used

Using cosmetic ingredients with polymer structure, photochromic molecules are combined with polyurethane polymers or polymers derived from linoleic acid through transesterification reaction, ensuring rapid and reversible conversion of molecules under ultraviolet light, maintaining moisturizing function, and Photochromic molecules are anchored in the polymer to achieve color changes.

Benefits of technology

It realizes the effect of cosmetics automatically changing colors under ultraviolet irritation, while maintaining moisturizing and beauty functions. The cosmetic formula is easy to optimize without affecting other properties such as texture and retention time.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FDA0005089451910000011
    Figure FDA0005089451910000011
  • Figure FDA0005089451910000012
    Figure FDA0005089451910000012
  • Figure GDA0005044784290000041
    Figure GDA0005044784290000041
Patent Text Reader

Abstract

A cosmetic ingredient for use in cosmetics having a polymer structure comprising a light-transmitting emollient or a film-forming cosmetic polymer. An organic chromophore molecule is inserted and chemically linked into the polymer, which molecule may be a fixed color molecule or a photochromic molecule capable of rapidly switching from one color to another. A colored or photochromic molecule is inserted and chemically linked by transesterification into a cosmetic oil having functional groups suitable for chemical anchoring of the molecule and chemical linking to the oil. The cosmetic oil may be a silicone macrodiol functionalized with a photochromic derivative designed to ensure transition between a colorless state and a colored state upon irradiation with ultraviolet light.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a transparent colored cosmetic composition for use in cosmetics, which composition may automatically change color when exposed to ultraviolet rays. Technical Field

[0003] Since ancient times, color has been an essential factor in enhancing beauty, especially feminine beauty.

[0004] In the past, Egyptians used powders and mixtures to decorate their bodies, and warriors used them to shock and intimidate their enemies. Similarly, Native Americans and American Indians have always been accustomed to coloring their skin.

[0005] First impressions were, and still are, an important part of everyday life. Products must engage all the senses to evoke a range of emotional responses in consumers.

[0006] Over time, makeup has acquired a more complex and sophisticated meaning, becoming a cosmetic practice aimed at improving the image of the human body.

[0007] So, while color psychology has a long history, its assessment has only reached a more scientific approach in recent years with the development of models that are able to predict humans’ emotional responses to colors and their combinations.

[0008] The first theories aiming to explain the nature of color date back to the 17th century, when people realized that color is primarily a physical characteristic caused by the interaction between light, matter at the electronic level, and the shape of objects.

[0009] Various dyes have been used in cosmetics and over time attempts have been made to improve their properties, such as gloss, in order to follow current trends and meet consumer demands. The constant development of new trends in the cosmetics market and the continuous development of specific and diverse demands for cosmetics indicate the need to continuously develop new and more complex formulations that produce new benefits and achieve special effects.

[0010] To meet the new demands of consumers, we thought of using the known chemical phenomenon of photochromism to break the static nature of formulated colors to obtain surprising, innovative and exclusive products.

[0011] Photochromism is a physical phenomenon based on a reversible reaction that transforms a molecule from state A to state B after absorption of electromagnetic radiation. The two states A and B are isomers, since photochemical excitation leads to rearrangement of the electronic and nuclear structure of the molecule. Their main difference is in the absorption spectrum. The initial stable state A absorbs in the ultraviolet spectral region, so it is usually colorless, while the higher energy state B absorbs in the visible region and is strongly colored.

[0012] The word "photochromic" comes from the Greek words "phos" (light) and "chroma" (color), which means "color change due to the influence of light." Molecules that can exhibit this special phenomenon are defined as "photochromic".

[0013] These molecules can find applications in industry if they meet certain requirements, such as fast activation of the color change process (also called "switching"), high efficiency and, ultimately, solubility in the matrix to which the molecules are bound.

[0014] Photochromic molecules have been developed, such as spiropyrans and spirooxazines, which change color through UV-A radiation, the most accessible wavelength in the solar spectrum. The high efficiency and remarkable switching speed of these compounds enable their use in the production of photochromic lenses.

[0015] The introduction of new molecules into cosmetics is always a delicate operation, since substances with low molecular weight, such as molecules, can be absorbed by the skin.

[0016] JP S61 275209A describes the synthesis of cosmetic compositions using polyolefin polymers in which chromophore molecules are directly linked to monomers which are repeated throughout the polyolefin chain.

[0017] US 2003 / 193044 A1 describes chromophore compositions comprising crosslinked, non-cosmetic polyurethanes, wherein the chromophore molecules are not chemically linked to the polymer but are merely admixed and are not intended for cosmetic applications.

[0018] No. 5,322,945 A describes a process for preparing linear photochromic polysiloxanes in which chromophore molecules of spirooxazine are chemically linked to monomers which repeat along the entire chain. Summary of the invention

[0019] The object of the present invention is now to provide a cosmetic ingredient for cosmetics which allows the cosmetic to be coloured while being transparent in all its forms and under all conditions of use and which may moreover be capable of automatically changing colour under the stimulation of ultraviolet rays.

[0020] According to the invention, this object is achieved by a cosmetic ingredient having a polymer structure for use in cosmetics as defined in claim 1 .

[0021] The chromophore molecule can be a colored molecule of the static type, ie able to remain colored, or of the dynamic photochromic type, ie able to change color if stimulated by ultraviolet light. If such a chromophore molecule is of the photochromic type, the molecule will ensure a rapid and reversible switch from the internal environment to the external environment.

[0022] The polymer structure of the cosmetic ingredient may include polyurethane-type polymers, polysiloxanes, or polymers derived from linoleic acid having cosmetic film-forming or emollient functions.

[0023] The cosmetic composition according to the invention allows the production of transparent colored cosmetics which have a fixed color or which may change color upon exposure to UV light.

[0024] In order to incorporate colored or photochromic molecules into the interior of the polymer and thus into the cosmetic ingredient, the method as defined in claim 6 may be used.

[0025] In the case of the photochromic molecule, in order to allow insertion into the polymer, a cosmetic oil consisting of bishydroxyethoxypropyl polydimethicone (cosmetic oil) can be functionalized by transesterification with the photochromic molecule, which in turn imparts the necessary functionality, namely anchoring it to the polydimethicone, maintaining the main cosmetic function of the emollient oil. The transesterification synthesis can be carried out in the presence of a tin complex at elevated temperatures (about 140°C) and in the absence of solvents.

[0026] After the transesterification reaction of the photochromic molecule, the molecule itself can be used as a monomer with hydroxyl functional groups for the synthesis of polyurethanes, which can be mainly alkyl or completely silicone. In the first case, according to EP2349197, the synthesis is carried out in the presence of diols, which are usually used to synthesize polyurethanes (such as C12-15 alkyl tartarates), isocyanates, diisocyanates with different structures (such as isophorone diisocyanate-IPDI, 1,6-hexamethylene diisocyanate-HDI, dicyclohexylmethane diisocyanate-M12HDI, 3-isocyanate propyl trimethoxysilane, 3-isocyanate propyl triethoxysilane, etc.). In the second case, according to EP 1588686, the synthesis is carried out in the presence of silicone diols commonly used in cosmetics (such as bishydroxyethoxypropyl polydimethylsiloxane) and diisocyanates with different structures (such as isophorone diisocyanate - IPDI, 1,6-hexamethylene diisocyanate - HD, dicyclohexylmethane diisocyanate - M12HDI, etc.). By appropriately changing the functionality of the initial molecule, the monomer can be used for other types of polymers. The polymerization of polyurethanes can be carried out in the presence of tin and zinc complexes at a temperature of 90 / 95°C.

[0027] The polymers obtained by using silicone oils can be used in fluid cosmetics (such as lip fluids) with the secondary purpose of imparting a color-changing characteristic when exposed to ultraviolet light.

[0028] The polymer can also be added to powder products (such as eye shadow powder) as a binding oil and has a secondary color change purpose.

[0029] As an alternative to photochromic molecules, it is possible to use fixed color molecules (ie, they do not change color but are static in their natural color), which are commercially available under the name Reactint by Milliken and which allow to obtain colored but transparent polyurethane polymers and thus cosmetics having this characteristic. DETAILED DESCRIPTION

[0030] A preferred example of functionalizing a siloxane macrodiol for cosmetic use with a photochromic derivative specifically designed to ensure a transition between a colorless and a colored state upon UV irradiation is now described.

[0031] The best candidates for functionalizing macrodiols are appropriately functionalized molecules belonging to the spiropyran family, such as the derivative FC-C3-Et obtained using the synthesis illustrated below.

[0032]

[0033] The choice of this particular structure was made based on the following characteristics:

[0034] A. Spiropyrans, typical photochromic molecules, ensure the required properties in terms of photochromic contrast.

[0035] B. The functionalized chain inserted onto the indoline nitrogen makes it possible to covalently anchor macromolecular diols via catalytic transesterification.

[0036] C. The presence of nitro and methoxy groups on the phenyl residue ensures the correct position of photoequilibrium and better photochemical stability under irradiated and dark conditions, respectively.

[0037] In order to obtain the derivative FC-C3-Et according to the above procedure, trimethylindoline (CAS 1640-39-7) is alkylated with a lower alcohol ester obtained from a chain ω-bromic acid between C2 (ethyl bromoacetate) and C12 (e.g. ethyl 3-bromopropionate (CAS 539-74-2)) in the absence of a solvent. The reaction is carried out between 80° C. and 140° C. in a nitrogen atmosphere for 1 to 48 hours. The stoichiometric ratio of indoline to the alkylating agent is between 1:1 (mol) and 1:5 (mol), preferably 1:1.5.

[0038] The viscous liquid thus obtained is dissolved in water and extracted with CH2CL2 to a colorless organic aqueous phase. The purpose of the extraction is to remove excess alkylating agent.

[0039] The aqueous phase thus obtained is made alkaline (pH < 12) with 5M NaOH (or other mineral bases), stirred for 2 hours, then extracted with CH2CL2 to obtain an organic phase which is dried over anhydrous salt to produce a viscous red oil consisting of a mixture of the starting indoline and anhydrous base. The indoline is removed by distillation under reduced pressure to obtain pure anhydrous base as a very viscous red oil.

[0040] This is followed by a condensation phase of pure anhydrous base with methoxy-nitroresorcinol (CAS 17028-61-4), which is very critical: (according to the previously illustrated synthesis) two different 0.5 M anhydrous base solutions and aldehyde solutions are prepared in anhydrous ethanol, both solutions being preheated to 60° C. The aldehyde solution is saturated at this temperature. The two solutions are mixed rapidly in a 60° C. bath and kept at this temperature for 120 seconds. The thermostatic bath is removed and the resulting dark blue solution is stirred overnight. A large amount of gray precipitate is thus obtained, which is crystallized twice from anhydrous ethanol.

[0041] The derivative FC-C3-Et thus obtained has a melting point of about 145° C. and is a white crystalline solid which is very soluble in common organic solvents: it is only partially soluble in hot isododecane.

[0042] Subsequent transesterification reactions were performed under a variety of experimental conditions to minimize the amount of organic residues present in the final functionalized macrodiol samples.

[0043] The following parameters were considered:

[0044] A.Solvent

[0045] B. Temperature

[0046] C. Duration

[0047] D. Catalyst Type and Stoichiometry

[0048] E. Purification

[0049] First, the most suitable transesterification catalyst was determined. Considering the cosmetic use of the product, a heterogeneous catalyst based on dibutyltin oxide (CAS 818-08-6) was used. This catalyst works in a heterogeneous phase and can be filtered at the end of the reaction. Unless otherwise stated, all the following tests were performed using a 1:0.0003 mass ratio of catalyst to bis-hydroxyethoxypropyl dimethicone.

[0050] As expected, the derivative FC-C3-Et is insoluble in isododecane, nor in pure bishydroxyethoxypropyl polydimethicone, except at temperatures above 140° C. Considering that the melting temperature of FC-C3-Et is close to the minimum process temperature required to obtain a homogeneous solution of the photochromic in bishydroxyethoxypropyl polydimethicone and isododecane, the reaction was initially carried out using a low-boiling solvent (boiling point below 120° C.-130° C.). Reactions carried out in the presence of solvents are in any case slow and it is difficult to achieve their complete conversion.

[0051] Therefore, a protocol was developed to carry out the reaction without solvent (i.e., using bishydroxyethoxypropyldimethylsiloxane directly as solvent). In this case, the reaction must be carried out under vacuum to simultaneously distill the ethanol released from the photochromic precursor. The distillation temperature was found to vary between 140°C and 160°C for 3 to 6 hours.

[0052] In all cases, this analysis and observation also highlighted the release of bishydroxyethoxypropyl polydimethicone alone, which probably occurred through transesterification. In fact, the molecular weight and viscosity of the material increased. This process is sensitive to time and temperature.

[0053] Therefore, the transesterification scheme was optimized: a suspension of 100g of bis-hydroxyethoxypropyl polydimethylsiloxane. 10g FC-C3-Et and 50mg dibutyltin oxide were placed under vigorous stirring and vacuum. The mixture was heated to about 145°C, and the gradual escape of steam (ethanol) and the gradual dissolution of the precipitate were observed. After about 1 hour, the suspension was converted into a uniform solution. The heating was maintained for another 5 hours and the reaction was monitored at a fixed time by 1H NMR spectroscopy. At the end of the reaction, the resulting blue / green oil was cooled to room temperature, diluted with 100ml of heptane, and placed at -20°C overnight (to precipitate the catalyst and any other insoluble residues). The mixture was then filtered through a folded filter and the solvent was removed under reduced pressure until constant weight. Therefore, the following photochromic raw material shown as sample I was obtained by the transesterification reaction of the derivative FC-C3-Et with the cosmetic oil (bis-hydroxyethoxypropyl polydimethylsiloxane).

[0054]

[0055] The described process may include several variations, the main ones being the following:

[0056] 1. The stoichiometric ratio of bishydroxyethoxypropyl polydimethylsiloxane to photochromic is 4:1 to 50:1, preferably 10:1 (mass ratio).

[0057] 2. Catalyst: dibutyltin oxide or tin oxalate, used in a stoichiometric amount of 1 to 0.00001 wt % relative to bis-hydroxyethoxypropyl polydimethylsiloxane.

[0058] 3. Temperature: 120°C to 180°C, preferably 130°C to 160°C, more preferably 140°C to 150°C.

[0059] 4. Time: 1 to 48 hours, preferably 2 to 8 hours.

[0060] The cosmetic material or ingredient synthesized in this way can be inserted into various cosmetic compositions. The cosmetic composition comprises at least one cosmetic material or ingredient having the function of cosmetic oil or film-forming oil, and the weight percentage thereof ranges from 4wt% to 20wt%. In addition, the cosmetic material or ingredient can have the ability to change color and / or be colored in a fixed manner.

[0061] The following are examples of different cosmetic compositions in which cosmetic oil (Sample 1) is used as a binding oil in different percentages and has the characteristic of changing color with ultraviolet light.

[0062] Example 1: Eyeshadow

[0063]

[0064] Example 2: Eyeshadow

[0065]

[0066] Example 3: Lip Gloss

[0067]

[0068] Example 4: Lip Gloss

[0069]

[0070] Furthermore, an example of a cosmetic composition is reported herein in which at least one cosmetic material according to the invention is used in an amount of 29 wt % (sample II), which has a film-forming function and is characterized by being colored in a fixed manner.

[0071] Example 5: Lip Gloss

[0072]

[0073] The main advantage of the present invention which would not have occurred to a person skilled in the art is that by taking a cosmetic raw material that functions as an emollient or film-forming oil and transesterifying it with a chromophore molecule, the main cosmetic function is maintained and in the case of a photochromic molecule, the ability to change color is increased if the cosmetic is subjected to the ultraviolet component of solar radiation.

[0074] The clear technical advantage is to take a cosmetic formulation that has already been optimized with an emollient oil or an initial film-forming oil, which is easy to implement and can change its color during application without modifying other cosmetic properties (texture, sensory experience, hold time, etc.).

Claims

1. A cosmetic ingredient having a polymer structure for use in cosmetics, characterized in that: The polymer structure includes a cosmetic polymer with an emollient function or a film-forming function, the cosmetic polymer is light-transmissive in both a dry state and a solution state, wherein an organic photochromic molecule is chemically linked in the polymer in a covalent manner through an ester exchange reaction, the cosmetic polymer is a siloxane macromolecular diol, wherein the photochromic molecule has a spiropyran-type chemical structure and can quickly switch from one color to another, wherein the photochromic molecule has the following structure FC-C3-Et:

2. The cosmetic ingredient according to claim 1, characterized in that The polymer having an emollient function is made of polysiloxane.

3. The cosmetic ingredient according to claim 2, characterized in that The polysiloxane is bishydroxyethoxypropyl dimethicone.

4. The cosmetic ingredient according to claim 1, characterized in that The polymer having the cosmetic film-forming function is made of polyurethane.

5. A method for inserting a photochromic molecule into an emollient cosmetic polymer, wherein a cosmetic oil is functionalized by transesterification with a photochromic molecule, the photochromic molecule being provided with a functionality suitable for its polymer anchoring, the functionalized cosmetic oil retaining the cosmetic functionality of the emollient oil, wherein, The photochromic molecule has the following structure FC-C3-Et: The cosmetic oil is a silicone macrodiol.

6. The method according to claim 5, characterized in that The cosmetic oil consists of polysiloxane.

7. The method according to claim 6, characterized in that The polysiloxane is bishydroxyethoxypropyl dimethicone.

8. The method according to claim 5, characterized in that The cosmetic oil consists of polymers derived from linoleic acid.

9. The method according to claim 5, characterized in that The transesterification reaction of the photochromic molecule is carried out in the presence of a tin complex at a high temperature of >100° C. and in the absence of a solvent.

10. The method according to claim 5, characterized in that The siloxane macrodiol is functionalized by photochromic molecules designed to ensure a transition between a colorless state and a colored state upon irradiation with ultraviolet light.

11. The method according to claim 10, characterized in that The macromolecular diol transesterified by the photochromic molecule is used as a monomer for synthesizing polyurethane while maintaining the film-forming function.

12. The method according to claim 11, characterized in that The polyurethane is of alkyl type.

13. The method according to claim 11, characterized in that The polyurethane is of silicone type.

14. The method according to claim 5, characterized in that The photochromic molecule having the structure FC-C3-Et is obtained by the following steps: a) alkylating trimethylindoline with a lower alcohol ester obtained from a chain ω-bromic acid between C2 and C12 in the absence of a solvent, the reaction being carried out at between 80° C. and 140° C. for 1 to 48 hours in a nitrogen atmosphere, the stoichiometric molar ratio of indoline to alkylating agent being between 1:1 and 1:5, until a viscous liquid is obtained; b) dissolving the viscous liquid in water and extracting with CH2Cl2 to remove excess alkylating agent until a colorless organic aqueous extract phase is obtained; c) the aqueous phase is made alkaline, stirred for about 2 hours, and then extracted with CH2Cl2 to obtain an organic phase, which is dried over anhydrous salt to produce a viscous red oil consisting of a mixture of indoline and anhydrous base; d) removing the indoline by distillation under reduced pressure to obtain the pure anhydrous base as a very viscous red oil; e) Condensation of pure anhydrous base with methoxy-nitroresorcinol by preparing two different anhydrous base solutions and aldehyde solutions in ethanol, both solutions being preheated to 60°C, the two solutions being rapidly mixed with each other in a 60°C bath and kept at this temperature for 120 seconds, then removing the constant temperature bath to obtain a solution, stirring the solution overnight until a grey precipitate is obtained, and crystallizing the grey precipitate twice from anhydrous ethanol to obtain a final derivative having a melting point of about 145°C, being a white crystalline solid, being very soluble in common organic solvents, but only partially soluble in hot isododecane.

15. The method according to claim 14, characterized in that The transesterification was carried out according to the following scheme: a) preparing a suspension mixture of bishydroxyethoxypropyl polydimethylsiloxane, a photochromic molecule having the structure FC-C3-Et and a heterogeneous catalyst based on dibutyltin oxide in a solvent, stirring and treating it under vacuum; b) heating the mixture to about 145° C. until the suspension is converted into a homogeneous solution; c) keep heating for about 1 hour until a blue / green oil is obtained; d) cooling the blue / green oil to room temperature, diluting it with heptane, and then standing at about -20°C overnight to allow the catalyst and any other insoluble residues to precipitate, to obtain a resulting mixture free of the catalyst and any other insoluble residues; e) filtering the resulting mixture and removing the solvent until an emollient oil having photochromic capabilities is obtained.