Method for producing austenitic heat-resistant steel

By controlling the chemical composition and heat treatment conditions of austenitic heat-resistant steel, the problem of difficult to balance creep strength and welding crack resistance is solved, and the improvement of stable creep strength and welding crack resistance at high temperatures is achieved.

CN115461477BActive Publication Date: 2024-10-01NIPPON STEEL CORPORATION
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180031266.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-04-30
Filing Date
2021-04-21
Publication Date
2024-10-01
Estimated Expiration
2041-04-21

AI Technical Summary

Technical Problem

When existing austenitic heat-resistant steel is used at high temperatures, its creep strength is unstable and welding cracks are prone to occur, making it difficult to achieve both stable creep strength and welding crack resistance.

Method used

By controlling the chemical composition and heat treatment conditions of the steel to ensure that the difference between the Nb content and the Nb amount analyzed in the electrolytic extraction residue is within a specific range, solution heat treatment and cooling are performed to optimize the amount of solid solution Nb and the cooling start temperature difference to improve creep. Strength and resistance to weld cracking.

Benefits of technology

It achieves stable creep strength and excellent welding crack resistance when used at high temperatures, improving the overall performance of the steel.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115461477B_ABST
    Figure CN115461477B_ABST
Patent Text Reader

Abstract

A method for producing austenitic heat-resistant steel, wherein the difference between the Nb content and the Nb amount analyzed as electrolytic extraction residue satisfies [0.170≤Nb-Nb ER ≤0.480], the method comprising: a forming step, which processes and forms the steel having a specified chemical composition into a product shape; a solution heat treatment step, which performs heat treatment after the forming step at a heat treatment temperature satisfying the conditions of [-250Nb+1200≤T≤-100Nb+1290] and a heat treatment time satisfying the conditions of [405-0.3T≤t≤2475-1.5T]; and a cooling step, which performs cooling after the solution heat treatment step.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for manufacturing austenitic heat-resistant steel. Background Art

[0002] In thermal power plants, the operating conditions of power generation boilers are becoming higher in temperature and pressure in order to improve power generation efficiency from the perspective of reducing environmental load. In addition, the materials of superheater tubes, reheater tubes, etc. used in power generation boilers are required to have excellent high-temperature strength in addition to characteristics such as corrosion resistance.

[0003] Therefore, conventionally, as a material having excellent high temperature strength, austenitic heat-resistant alloys containing large amounts of Nb and N have been developed. For example, Patent Documents 1 to 6 disclose austenitic steels containing predetermined amounts of Nb and N to improve high temperature strength.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Laid-Open No. 62-133048

[0007] Patent Document 2: Japanese Patent Application Publication No. 2000-256803

[0008] Patent Document 3: International Publication No. 2009 / 044796

[0009] Patent Document 4: International Publication No. 2013 / 073055

[0010] Patent Document 5: Japanese Patent Application Publication No. 2014-1436

[0011] Patent Document 6: Japanese Patent Application Publication No. 2003-268503 Summary of the invention

[0012] Problem that the invention aims to solve

[0013] When the austenitic heat-resistant steels disclosed in Patent Documents 1 to 6 are used at high temperatures, the time until fracture may vary under a certain stress, and there is room for improvement in obtaining stable creep strength. In addition, even if stable creep strength is obtained, cracks are easily generated during welding due to the inclusion of Nb, so there is a technical problem that it is difficult to achieve both stable creep strength and welding crack resistance.

[0014] An object of the present invention is to solve the above-mentioned technical problems and to provide a method for producing an austenitic heat-resistant steel which stably has good creep strength and excellent weld crack resistance when used at high temperatures.

[0015] Solutions for solving problems

[0016] The present invention has been made to solve the above-mentioned technical problems, and the gist of the present invention is a method for producing austenitic heat-resistant steel as described below.

[0017] (1) A method for producing austenitic heat-resistant steel, the method comprising:

[0018] The forming process is to form the steel into a product shape, wherein the chemical composition of the steel is calculated by mass %.

[0019] C: 0.04~0.12%,

[0020] Si: 0.01-0.30%,

[0021] Mn: 0.50-1.50%,

[0022] P: 0.001~0.040%,

[0023] S: 0.0050% or less,

[0024] Cu: 2.2-3.8%,

[0025] Ni: 8.0-11.0%,

[0026] Cr: 17.7~19.3%

[0027] Mo: 0.01~0.55%,

[0028] Nb: 0.400~0.650%,

[0029] B: 0.0010~0.0060%,

[0030] N: 0.050~0.160%,

[0031] Al: 0.025% or less,

[0032] O: 0.020% or less,

[0033] Co: 0-1.00%,

[0034] W: 0~1.00%,

[0035] Ti: 0~0.40%,

[0036] V: 0~0.40%,

[0037] Ta: 0~0.40%,

[0038] Sn: 0~0.0300%,

[0039] Ca: 0~0.0100%,

[0040] Mg: 0~0.0100%,

[0041] REM: 0~0.0800%、

[0042] Balance: Fe and impurities;

[0043] a solution heat treatment step, wherein heat treatment is performed after the molding step at a heat treatment temperature satisfying the following formula (ii) and a heat treatment time satisfying the following formula (iii); and

[0044] A cooling step is performed after the solution heat treatment step.

[0045] 0.170≤Nb-Nb ER ≤0.480 (i)

[0046] -250Nb+1200≤T≤-100Nb+1290 (ii)

[0047] 405-0.3T≤t≤2475-1.5T (iii)

[0048] The element symbols in the above formula represent the content (mass %) of the element contained in the steel, and each symbol in the above formula is defined as follows.

[0049] Nb ER (Mass %): Nb content analyzed as electrolytic extraction residue

[0050] T(℃): Heat treatment temperature

[0051] T (seconds): heat treatment time

[0052] (2) The method for producing austenitic heat-resistant steel according to (1) above, wherein in the cooling step, the cooling is performed by forced cooling.

[0053] The difference between the heat treatment temperature and the temperature of the steel when the forced cooling is started satisfies the following formula (iv).

[0054] 0≤△T≤100Nb-5 (iv)

[0055] The element symbols in the above formula represent the content (mass %) of the elements contained in the steel, and the symbols in the above formula are defined as follows.

[0056] △T (℃): The difference between the heat treatment temperature of the solution heat treatment and the temperature of the steel when forced cooling starts

[0057] (3) The method for producing austenitic heat-resistant steel according to (1) or (2) above, wherein the difference between the Nb content and the Nb amount analyzed as the electrolytic extraction residue satisfies the following formula (v).

[0058] -2B+0.185≤Nb-Nb ER ≤-4B+0.480 (v)

[0059] The symbols of the elements in the above formula refer to the content (mass %) of the elements in the steel. ER It refers to the amount of Nb (mass %) analyzed as the electrolytic extraction residue.

[0060] (4) The method for producing austenitic heat-resistant steel according to any one of (1) to (3) above, wherein the chemical composition contains, in mass %, a

[0061] Co: 0.01~1.00%,

[0062] W: 0.01~1.00%,

[0063] Ti: 0.01~0.40%,

[0064] V: 0.01~0.40%,

[0065] Ta: 0.01~0.40%,

[0066] Sn: 0.0002~0.0300%,

[0067] Ca: 0.0002~0.0100%,

[0068] Mg: 0.0002 to 0.0100%, and

[0069] REM: 0.0005~0.0800%

[0070] One or more of the following.

[0071] (5) The method for producing austenitic heat-resistant steel according to any one of (1) to (4) above, wherein the chemical composition contains, in mass %,

[0072] P: 0.020~0.040%.

[0073] Effects of the Invention

[0074] According to the present invention, it is possible to obtain an austenitic heat-resistant steel which stably has good creep strength and excellent weld crack resistance when used at high temperatures. BRIEF DESCRIPTION OF THE DRAWINGS

[0075] Figure 1It is a figure which shows the groove shape in Example. DETAILED DESCRIPTION

[0076] The present inventors conducted various studies to improve the high temperature strength of austenitic heat-resistant steel containing Nb and N, specifically, to improve creep strength and weld crack resistance, and obtained the following findings (a) to (c).

[0077] (a) It can be seen that the creep strength of steel is strongly affected by the solution heat treatment after the final forming process. Even in the case of the same chemical composition, the creep strength varies depending on the solution heat treatment conditions. Specifically, as the heat treatment temperature becomes higher or the heat treatment time becomes longer, high creep strength is stably obtained.

[0078] Thus, while stably obtaining high creep strength, the amount of precipitation of carbonitrides and nitrides containing Nb is small in the state before use after solution heat treatment and cooling. In addition, when used under exposure to high temperature, carbonitrides and nitrides containing Nb precipitate finely and densely in the grains, and they exist stably for a long time.

[0079] In contrast, in the case of poor creep strength, the amount of precipitation of carbonitrides and nitrides containing Nb observed before use is large. In addition, during use, there are few carbonitrides and nitrides containing Nb that are finely precipitated in the grains, and they are coarsened in advance. Furthermore, for steels with a low Nb content, in order to stably obtain high creep strength, it is necessary to perform solution heat treatment at a higher temperature. Therefore, in order to obtain stable creep strength, it is preferred to fully dissolve Nb in the matrix in advance and precipitate Nb-containing precipitates during the use stage.

[0080] (b) On the other hand, regarding weld crack resistance, it was confirmed that crack sensitivity tends to increase as the heat treatment temperature increases or the heat treatment time increases. In addition, weld cracks occur at the grain boundaries of the weld heat-affected zone, and traces of local melting of the grain boundaries are confirmed on the crack cross-section, resulting in Nb enrichment. Furthermore, for steel containing a large amount of Nb, weld cracks may occur even when solution heat treatment is performed at a lower temperature.

[0081] Nb dissolved in the matrix (hereinafter referred to as "solid solution Nb") has a greater impact on weld crack sensitivity than Nb existing as precipitates. The reason is that solid solution Nb does not need time to be dissolved in the matrix through the welding heat cycle, so Nb is easily enriched at the grain boundary. As a result, weld cracks are easily generated.

[0082] (c) Based on the above, it can be seen that the amount of dissolved Nb has a great influence on both creep strength and weld crack resistance. Therefore, in order to achieve both stable high creep strength and good weld crack resistance, it is necessary to properly control the amount of dissolved Nb and the solution heat treatment conditions that affect it. The amount of dissolved Nb is also affected by the B content, so it is preferred to properly control these ranges. Moreover, on the basis of controlling the amount of dissolved Nb, of course, the Nb content must be adjusted to an appropriate range, and it is hoped that the heat treatment temperature and heat treatment time in the solution heat treatment can be properly managed according to the Nb content.

[0083] The present invention has been accomplished based on the above findings, and as described below, is a method for producing an austenitic heat-resistant steel in which the difference between the Nb content and the Nb amount analyzed as an electrolytic extraction residue satisfies the formula (i) described below.

[0084] 1. Molding process

[0085] 1-1. Molding method

[0086] In the manufacturing method of the present invention, in the forming process, the steel having the chemical composition described below is processed and formed into the final shape, i.e., the product shape. There is no particular limitation on the method for processing and forming, and it can be casting using a mold or plastic processing. In the case of forming by plastic processing, for example, hot rolling, hot forging, cold rolling, cold forging, cold drawing, etc. can be considered as an example, and the processing temperature can be any temperature range of hot working, cold working, and warm working. It should be noted that in the forming process, heat treatment and pickling can be performed as needed.

[0087] In addition, there is no particular limitation on the shape of the product to be processed and formed. For example, the product shape may be a plate, a tube, a rod, a wire, an H shape, an I shape, or a special shape using a casting mold.

[0088] 1-2. Chemical composition of steel

[0089] In the manufacturing method of the present invention, it is also important to control the chemical composition of the steel to be processed and formed. The chemical composition of the steel as the raw material for the above-mentioned plastic forming is controlled by, for example, melting and refining the raw material of a specified chemical composition. In addition, generally, a steel ingot or a bloom is manufactured by casting. Thereafter, the above-mentioned plastic processing such as hot rolling or cold rolling is performed.

[0090] In the following description, the chemical composition of the steel used as the raw material during processing will be described. It should be noted that, in the description, "%" about the content means "mass %" unless otherwise specified.

[0091] C: 0.04~0.12%

[0092] C forms fine carbides while stabilizing the austenite structure, thereby improving the creep strength during high-temperature use. Therefore, the C content is set to 0.04% or more. It is preferred to set the C content to 0.06% or more, and more preferably to 0.07% or more. However, when C is contained in excess, its effect is saturated, and a large amount of carbides precipitate, and creep ductility decreases. Therefore, the C content is set to 0.12% or less. It is preferred to set the C content to 0.10% or less, and more preferably to 0.09% or less.

[0093] Si: 0.01~0.30%

[0094] Si has a deoxidizing effect during manufacturing. In addition, Si is an effective element for improving corrosion resistance and oxidation resistance at high temperatures. Therefore, the Si content is set to 0.01% or more. It is preferred to set the Si content to 0.03% or more, and more preferably to 0.05% or more. However, when Si is contained excessively, the stability of the austenite structure decreases, resulting in a decrease in toughness and creep strength. Therefore, the Si content is set to 0.30% or less. It is preferred to set the Si content to 0.28% or less, and more preferably to 0.25% or less.

[0095] Mn: 0.50~1.50%

[0096] Mn has a deoxidizing effect like Si. In addition, Mn stabilizes the austenite structure and contributes to the improvement of creep strength. Therefore, the Mn content is set to 0.50% or more. It is preferred to set the Mn content to 0.60% or more, and more preferably to 0.70% or more. However, when Mn is contained in excessive amounts, it will cause embrittlement, and then the creep ductility will also decrease. Therefore, the Mn content is set to 1.50% or less. The Mn content is preferably set to 1.30% or less, and more preferably to 1.00% or less.

[0097] P: 0.001~0.040%

[0098] P is an element contained in steel as an impurity, but if it is excessively reduced, the manufacturing cost will increase, so the P content is set to 0.001% or more. It is preferred to set the P content to 0.005% or more, and more preferably to 0.010% or more. In addition, P has the effect of improving creep strength. In order to obtain this effect, it is preferred to set the P content to 0.020% or more.

[0099] However, if P is contained excessively, the crack sensitivity of the heat-affected zone during welding increases. Therefore, the P content is set to 0.040% or less. Preferably, the P content is set to 0.038% or less, and more preferably, it is set to 0.035% or less.

[0100] S: 0.0050% or less

[0101] S is contained in steel as an impurity like P, and increases the crack sensitivity of the weld heat affected zone during welding. Therefore, the S content is set to 0.0050% or less. It is preferred to set the S content to 0.0040% or less, and more preferably to 0.0020% or less. It should be noted that it is preferred to reduce the S content as much as possible, but extreme reduction will lead to increased steelmaking costs. Therefore, it is preferred to set the S content to 0.0001% or more, and preferably to 0.0002% or more.

[0102] Cu: 2.2~3.8%

[0103] Cu improves the stability of the austenite structure and precipitates finely during use, which helps to improve the creep strength. Therefore, the Cu content is set to 2.2% or more. It is preferred to set the Cu content to 2.5% or more, and more preferably to 2.7% or more. However, when Cu is contained excessively, the hot workability decreases. Therefore, the Cu content is set to 3.8% or less. It is preferred to set the Cu content to 3.5% or less, and more preferably to 3.3% or less.

[0104] Ni: 8.0~11.0%

[0105] Ni stabilizes the austenite structure and helps to improve creep strength. Therefore, the Ni content is set to 8.0% or more. It is preferred to set the Ni content to 8.2% or more, and more preferably to 8.5% or more. However, Ni is a high-priced element, and a large amount of it will lead to increased costs. Therefore, the Ni content is set to 11.0% or less. It is preferred to set the Ni content to 10.8% or less, more preferably to 10.5% or less, and further preferably to 10.3% or less.

[0106] Cr: 17.7~19.3%

[0107] Cr helps to improve oxidation resistance and corrosion resistance at high temperatures. In addition, it forms fine carbides, which also helps to ensure creep strength. Therefore, the Cr content is set to 17.7% or more. It is preferred to set the Cr content to 18.0% or more, and more preferably to 18.2% or more. However, when Cr is contained in excess, the stability of the austenite structure is impaired and the creep strength decreases. Therefore, the Cr content is set to 19.3% or less. It is preferred to set the Cr content to 19.0% or less, and more preferably to 18.8% or less.

[0108] Mo: 0.01~0.55%

[0109] Mo is dissolved in the matrix and thus helps to improve creep strength and tensile strength at high temperatures. Therefore, the Mo content is set to 0.01% or more. It is preferred to set the Mo content to 0.03% or more, and more preferably to 0.05% or more. However, when Mo is contained in excess, the above effect is saturated. Furthermore, the stability of the austenite structure is impaired, and the creep strength decreases instead. Furthermore, since it is a high-priced element, it leads to increased costs. Therefore, the Mo content is set to 0.55% or less. It is preferred to set the Mo content to 0.53% or less, more preferably to 0.50% or less, and further preferably to 0.40% or less.

[0110] Nb: 0.400~0.650%

[0111] Nb precipitates as fine carbonitrides and nitrides, which helps to improve creep strength. Therefore, the Nb content is set to 0.400% or more. It is preferred to set the Nb content to 0.420% or more, and more preferably to 0.450% or more. However, when Nb is contained in excess, welding cracks will occur in the heat-affected zone during welding. In addition, carbonitrides and nitrides precipitate in large quantities, thereby reducing the ductility of the material. Therefore, the Nb content is set to 0.650% or less. It is preferred to set the Nb content to 0.630% or less, and more preferably to 0.600% or less.

[0112] It should be noted that the above-mentioned Nb content refers to the total amount of Nb contained in the austenitic heat-resistant steel. That is, it refers to the sum of the amount of dissolved Nb and the amount of Nb present as precipitates. In the manufacturing method of the present invention, in addition to the Nb content, the difference between the amount of dissolved Nb, that is, the amount of Nb content and the amount of Nb analyzed as the electrolytic extraction residue (the amount of Nb present as precipitates) is set to a prescribed range.

[0113] B: 0.0010~0.0060%

[0114] B has the effect of improving creep strength by finely dispersing grain boundary carbides. Therefore, the B content is set to 0.0010% or more. It is preferred to set the B content to 0.0020% or more, and more preferably to 0.0030% or more. However, when B is contained in excess, the crack sensitivity of the heat-affected zone during welding increases. Therefore, the B content is set to 0.0060% or less. It is preferred to set the B content to 0.0055% or less, and more preferably to 0.0050% or less.

[0115] N: 0.050~0.160%

[0116] N stabilizes the austenite structure and helps to improve creep strength by dissolving or precipitating as nitrides. Therefore, the N content is set to 0.050% or more. It is preferred to set the N content to 0.070% or more, and more preferably to 0.090% or more. However, when N is contained excessively, a large amount of fine nitrides precipitate, resulting in decreased creep ductility and toughness. Therefore, the N content is set to 0.160% or less. It is preferred to set the N content to 0.140% or less, and more preferably to 0.120% or less.

[0117] Al: 0.025% or less

[0118] Al has a deoxidizing effect. However, when Al is contained in excess, the cleanliness of the steel deteriorates and the hot workability decreases. Therefore, the Al content is set to 0.025% or less. It is preferred to set the Al content to 0.023% or less, more preferably to 0.020% or less, and further preferably to 0.0017% or less. On the other hand, an extreme reduction in Al will increase the cost of steelmaking and will not achieve the above-mentioned effect. Therefore, it is preferred to set the Al content to 0.001% or more, and more preferably to 0.002% or more.

[0119] O: 0.020% or less

[0120] O is contained in steel as an impurity. When it is contained in excess, hot workability decreases. In addition, toughness and ductility are also impaired. Therefore, the O content is set to 0.020% or less. It is preferred to set the O content to 0.018% or less, and more preferably to 0.015% or less. It should be noted that there is no particular lower limit for the O content, but an extreme reduction in the content will increase the manufacturing cost. Therefore, it is preferred to set the O content to 0.001% or more, and more preferably to 0.002% or more.

[0121] In addition to the above elements, the chemical composition may contain one or more selected from Co, W, Ti, V, Ta, Sn, Ca, Mg and REM within the range shown below. The reasons for limiting each element are explained below.

[0122] Co: 0~1.00%

[0123] Co, like Ni, has the effect of stabilizing austenite structure and improving creep strength. Therefore, it can be contained as needed. However, Co is a very expensive element, and when it is contained in excess, the cost increases. Therefore, the Co content is set to 1.00% or less. It is preferred to set the Co content to 0.90% or less, and more preferably to 0.80% or less. On the other hand, in order to obtain the above-mentioned effect, it is preferred to set the Co content to 0.01% or more, and more preferably to 0.03% or more.

[0124] W: 0~1.00%

[0125] W has the effect of improving creep strength at high temperature by being dissolved in the matrix or forming a fine intermetallic compound phase. Therefore, it can be contained as needed. However, even if W is contained excessively, the above effect will be saturated, and the stability of the austenite structure will be damaged, and the creep strength will decrease instead. Moreover, since it is a high-priced element, the manufacturing cost increases. Therefore, the W content is set to less than 1.00%. It is preferred to set the W content to less than 0.90%, and more preferably to less than 0.80%. On the other hand, in order to obtain the above effect, it is preferred to set the W content to more than 0.01%, and more preferably to more than 0.03%.

[0126] Ti: 0~0.40%

[0127] Ti combines with carbon and nitrogen to form fine carbides and carbonitrides, thereby having the effect of improving creep strength at high temperatures. Therefore, it can be contained as needed. However, when Ti is contained excessively, a large amount of precipitates precipitate, resulting in decreased creep ductility and toughness. Therefore, the Ti content is set to 0.40% or less. It is preferred to set the Ti content to 0.35% or less, and more preferably to 0.30% or less. On the other hand, in order to obtain the above-mentioned effect, it is preferred to set the Ti content to 0.01% or more, and more preferably to 0.02% or more.

[0128] V: 0~0.40%

[0129] V, like Ti, has the effect of forming fine carbides and carbonitrides, thereby improving creep strength at high temperatures. Therefore, it can be contained as needed. However, when V is contained excessively, a large amount of precipitates precipitate, resulting in decreased creep ductility and toughness. Therefore, the V content is set to 0.40% or less. It is preferred to set the V content to 0.35% or less, and more preferably to 0.30% or less. On the other hand, in order to obtain the above-mentioned effect, it is preferred to set the V content to 0.01% or more, and more preferably to 0.02% or more.

[0130] Ta: 0~0.40%

[0131] Ta, like Ti and V, has the effect of forming fine carbides and carbonitrides, thereby improving creep strength at high temperatures. Therefore, it can be present as needed. However, when Ta is contained in excess, a large amount of precipitates precipitate, resulting in decreased creep ductility and toughness. Therefore, the Ta content is set to 0.40% or less. It is preferred to set the Ta content to 0.35% or less, and more preferably to 0.30% or less. On the other hand, in order to obtain the above-mentioned effect, it is preferred to set the Ta content to 0.01% or more, and more preferably to 0.02% or more.

[0132] Sn: 0~0.0300%

[0133] Sn has a good effect of improving weldability. Therefore, it can be contained as needed. However, when Sn is contained excessively, the crack sensitivity of the weld heat affected zone is increased during welding, and the hot workability during manufacturing is impaired. Therefore, the Sn content is set to 0.0300% or less. It is preferred to set the Sn content to 0.0250% or less, and more preferably to 0.0200% or less. On the other hand, in order to obtain the above-mentioned effect, it is preferred to set the Sn content to 0.0002% or more, and more preferably to 0.0005% or more.

[0134] Ca: 0~0.0100%

[0135] Ca has the effect of improving hot workability. Therefore, it can be contained as needed. However, when Ca is contained in excess, it combines with oxygen to significantly reduce the cleanliness and damage the hot workability. Therefore, the Ca content is set to 0.0100% or less. It is preferred to set the Ca content to 0.0080% or less, and more preferably to 0.0060% or less. On the other hand, in order to obtain the above-mentioned effect, it is preferred to set the Ca content to 0.0002% or more, and more preferably to 0.0005% or more.

[0136] Mg: 0~0.0100%

[0137] Mg, like Ca, has the effect of improving hot workability. Therefore, it can be contained as needed. However, when Mg is contained in excess, it combines with oxygen and significantly reduces the cleanliness. As a result, the hot workability is reduced. Therefore, the Mg content is set to 0.0100% or less. It is preferred to set the Mg content to 0.0080% or less, and more preferably to 0.0060% or less. On the other hand, in order to obtain the above-mentioned effect, it is preferred to set the Mg content to 0.0002% or more, and more preferably to 0.0005% or more.

[0138] REM: 0~0.0800%

[0139] REM, like Ca and Mg, has the effect of improving hot workability during manufacturing. Therefore, it can be contained as needed. However, when REM is contained excessively, it combines with oxygen and significantly reduces the cleanliness. As a result, the hot workability is reduced. Therefore, the REM content is set to 0.0800% or less. It is preferred to set the REM content to 0.0600% or less, and more preferably to 0.0500% or less. On the other hand, in order to obtain the above-mentioned effect, it is preferred to set the REM content to 0.0005% or more, and more preferably to 0.0010% or more.

[0140] REM refers to a total of 17 elements including Sc, Y and lanthanoids, and the above REM content refers to the total content of these elements. REM is often added in the form of mixed rare earth metals in industry.

[0141] In the chemical composition of the present invention, the balance is Fe and impurities. Here, "impurities" refer to components mixed in industrial steel production due to various factors such as raw materials such as ore and waste and the production process, and are allowed within the range that does not adversely affect the present invention.

[0142] 2. Solution heat treatment process

[0143] Among the Nb contained in the steel, the Nb existing as precipitates before use contributes to creep strength, but its effect is small. In contrast, when used at high temperatures, solid-solution Nb precipitates finely and densely in the grains for a long time as carbonitrides or nitrides, greatly contributing to creep strength and its stabilization.

[0144] In addition, even if Nb is sufficiently dissolved, if the heat treatment temperature in the solution heat treatment is too low or the heat treatment temperature is too short, the processing deformation introduced in the process so far cannot be fully released, and the carbonitride or nitride will coarsen prematurely during use at high temperature, and its precipitation strengthening effect will disappear prematurely. As a result, the creep strength becomes difficult to stabilize.

[0145] In addition, when welding austenitic heat-resistant steel, Nb segregates at the grain boundaries of the weld heat-affected zone due to the welding heat cycle. Nb lowers the solidus temperature of the steel, so the grain boundaries where Nb segregates are partially melted, causing weld cracks. Moreover, even among the Nb contained in the steel, the solid solution Nb does not require time to be dissolved in the matrix through the welding heat cycle, so it has a great influence on the sensitivity of weld cracks.

[0146] In addition, when the heat treatment temperature in the solution heat treatment is too high or the heat treatment temperature is too long, the grains coarsen during the heat treatment process and the grain boundary area per unit volume decreases. Therefore, the grain boundary segregation amount of Nb during welding increases, and the thermal stress acting on specific grain boundaries increases, thereby increasing the sensitivity of welding cracks.

[0147] Therefore, from the perspective of creep strength, before use, it is necessary to ensure the amount of dissolved Nb effective for precipitation strengthening, and to effectively precipitate carbonitrides and nitrides containing Nb. On the other hand, from the perspective of weld crack resistance, it is necessary to ensure the amount of dissolved Nb required to improve creep strength, and to suppress the grain boundary segregation of Nb. Therefore, after the above-mentioned forming process, a solution heat treatment is performed under the conditions of the heat treatment temperature and time described later.

[0148] Specifically, in the solution heat treatment process, after the molding process, heat treatment is performed under the conditions that the heat treatment temperature satisfies the following formula (ii) and the heat treatment time satisfies the following formula (iii). That is, the heat is maintained at the heat treatment temperature satisfying the following formula (ii) and during the heat treatment time satisfying the following formula (iii).

[0149] -250Nb+1200≤T≤-100Nb+1290 (ii)

[0150] 405-0.3T≤t≤2475-1.5T (iii)

[0151] The element symbols in the above formula represent the content (mass %) of the element contained in the steel, and each symbol in the above formula is defined as follows.

[0152] T(℃): Heat treatment temperature

[0153] t(seconds): heat treatment time

[0154] In the solution heat treatment, when the heat treatment temperature is lower than the value on the left side of formula (ii), the precipitates containing Nb formed by the forming process cannot be fully dissolved in the matrix, and the amount of dissolved Nb cannot be fully ensured. In addition, the processing deformation introduced in the forming process cannot be eliminated by the solution heat treatment. As a result, in an environment of use exposed to high temperature, the carbonitride or nitride containing Nb will not precipitate finely and densely for a long time, and stable creep strength cannot be obtained. Therefore, the heat treatment temperature is set to be above the value on the left side of formula (ii).

[0155] On the other hand, when the heat treatment temperature exceeds the right value of formula (ii), although the amount of solid-soluted Nb is sufficient, the grains are coarsened, which leads to an increase in the weld crack sensitivity of the weld heat-affected zone caused by the grain boundary segregation of Nb. Therefore, the heat treatment temperature is set to be less than the right value of formula (ii).

[0156] Similarly, when the heat treatment time is less than the value on the left side of formula (iii), the precipitate containing Nb cannot be fully dissolved in the matrix, and the amount of dissolved Nb cannot be fully ensured. In addition, the processing deformation introduced in the forming process cannot be eliminated by solution heat treatment. As a result, in an environment exposed to high temperature, the carbonitride or nitride containing Nb will not precipitate finely and densely for a long time, and stable creep strength cannot be obtained. Therefore, the heat treatment time is set to be greater than the value on the left side of formula (iii).

[0157] On the other hand, when the heat treatment time exceeds the right value of formula (iii), although the amount of solid-soluted Nb is sufficient, the grains are coarsened, which increases the weld crack sensitivity of the weld heat-affected zone caused by the grain boundary segregation of Nb. Therefore, the heat treatment temperature is set to be less than the right value of formula (iii).

[0158] Based on the above, in the solution heat treatment, by performing heat treatment under the conditions satisfying the above formulas (ii) and (iii), it is possible to ensure the amount of solid solution Nb, suppress the coarsening of grains and the segregation of Nb at grain boundaries, and eliminate processing deformation. It should be noted that the atmosphere in the solution heat treatment can be conventionally used, for example, the atmospheric atmosphere or bright atmosphere commonly used in the heat treatment of steel products can be considered.

[0159] 3. Cooling process

[0160] In the cooling process, after the solution heat treatment, that is, after the heat treatment temperature and the heat treatment time are maintained, cooling is performed. It should be noted that during cooling, the cooling rate in the temperature range of 1000 to 600°C is preferably set to 0.4°C / s or more, and more preferably to 1.0°C / s or more. There is no particular limitation on the cooling method in the cooling process, but water cooling or forced air cooling is preferred. In addition, it is sufficient to cool to a temperature range of at least 300°C or less.

[0161] As for the cooling method, forced cooling is preferably performed by blowing a refrigerant such as water or air onto the steel. As an example of forced cooling, water cooling and forced air cooling can be cited. Moreover, when forced cooling is performed, it is preferred that the difference between the heat treatment temperature and the temperature of the steel at the start of forced cooling satisfies the following formula (iv). It should be noted that the above-mentioned heat treatment temperature refers to the temperature of the steel during heat treatment, and the temperature of the steel refers to the surface temperature of the steel.

[0162] 0≤△T≤100Nb-5 (iv)

[0163] The element symbols in the above formula represent the content (mass %) of the elements contained in the steel, and the symbols in the above formula are defined as follows.

[0164] △T (℃): The difference between the heat treatment temperature of the solution heat treatment and the temperature of the steel when forced cooling starts

[0165] The temperature difference between the heat treatment temperature of the solution heat treatment and the temperature of the steel when forced cooling starts (hereinafter referred to as "cooling start temperature difference") is preferably 0°C. However, in the manufacture using common manufacturing equipment, such as using an actual machine, it is difficult to make the cooling start temperature difference 0°C. Therefore, the cooling start temperature difference is more preferably 1°C or more, and further preferably 2°C or more.

[0166] On the other hand, when the cooling start temperature difference exceeds the right side value of formula (iv), the precipitates containing Nb are coarsely reprecipitated during the period until the forced cooling starts, the amount of solid-solution Nb decreases, and it becomes difficult to obtain a stable creep strength. Therefore, the cooling start temperature difference is preferably less than the right side value of formula (iv).

[0167] 5. Amount of solid solution Nb

[0168] In the manufacturing method of the present invention, the amount of Nb dissolved in the matrix, i.e., the amount of dissolved Nb, is controlled by solution heat treatment and the subsequent cooling process. Specifically, the difference between the Nb content corresponding to the amount of dissolved Nb and the amount of Nb analyzed as the electrolytic extraction residue needs to satisfy the following formula (i).

[0169] 0.170≤Nb-Nb ER ≤0.480 (i)

[0170] The element symbols in the above formula represent the content (mass %) of the elements contained in the steel, and the symbols in the above formula are defined as follows.

[0171] Nb ER (Mass %): Nb content analyzed as electrolytic extraction residue

[0172] When the amount of dissolved Nb as the intermediate value of formula (i) is less than 0.170%, the carbonitrides and nitrides containing Nb are in a precipitated state before being exposed to the use environment. When used at high temperatures, the carbonitrides and nitrides containing Nb will not precipitate finely in the grains. In addition, these precipitates are coarsened in advance. As a result, the creep strength cannot be improved. Therefore, the amount of dissolved Nb is set to more than 0.170%. It is preferred to set the amount of dissolved Nb to more than 0.180%.

[0173] However, when the amount of dissolved Nb exceeds 0.480%, the weld crack sensitivity of the weld heat affected zone is further increased during welding. Therefore, the amount of dissolved Nb is set to 0.480% or less. Preferably, the amount of dissolved Nb is set to 0.460% or less.

[0174] In addition, it is preferable to adjust the amount of dissolved Nb in combination with the effect of B that is dissolved in carbides and finely precipitated at grain boundaries to improve creep strength. Specifically, the amount of dissolved Nb preferably satisfies the following formula (v).

[0175] -2B+0.185≤Nb-Nb ER ≤-4B+0.480 (v)

[0176] The symbols of the elements in the above formula refer to the content (mass %) of the elements in the steel. ER It refers to the amount of Nb (mass %) analyzed as the electrolytic extraction residue.

[0177] This is because when the amount of dissolved Nb is equal to or greater than the value on the left side of formula (v), carbides in which B is dissolved are finely precipitated at the grain boundaries while ensuring the amount of dissolved Nb, further improving the creep strength. On the other hand, when the amount of dissolved Nb is equal to or less than the value on the right side of formula (v), the weld crack resistance can be improved.

[0178] It should be noted that the Nb content analyzed as the electrolytic extraction residue in the above formula can be measured according to the following procedure. A test piece of a predetermined size is collected from the steel. The constant current electrolysis method using 10 volume % acetylacetone-1 mass % tetramethylammonium chloride methanol solution as the electrolyte is carried out at 20 mA / cm 2 The test piece is dissolved at an anodic current density to extract carbonitrides and nitrides as residues. The extracted residue is decomposed by acid and then subjected to ICP (high frequency inductively coupled plasma) emission analysis to determine the mass of Nb in the residue. The mass of Nb in the residue is divided by the amount of dissolved test material to determine the amount of Nb present as carbonitrides and nitrides. The amount of Nb obtained is the amount of Nb analyzed as electrolytic extraction residue.

[0179] Hereinafter, the present invention will be described in more detail with reference to Examples, but the present invention is not limited to these Examples.

[0180] Example

[0181] Steel ingots were cast by melting materials of steel types A to T having chemical compositions shown in Table 1, and were formed into a thickness of 25 mm by hot forging, a thickness of 18 mm by hot rolling, and a thickness of 12 mm by cold rolling.

[0182] [Table 1]

[0183]

[0184] Then, the cold-rolled billet was machined to produce a plate having a thickness of 12 mm × a width of 100 mm × a length of 100 mm. In addition, for steel types A, C, and E, a plate having a thickness of 15 mm × a width of 100 mm × a length of 100 mm was also machined from the hot-rolled billet. Then, for these plates, the heat treatment temperature and the heat treatment time in each case were changed as shown in Tables 2 to 4, and a solution heat treatment with a soaking hold was performed.

[0185] Then, water cooling or forced air cooling is started from the heat treatment temperature so that the cooling start temperature difference shown in Tables 2 to 4 is obtained. Water cooling or forced air cooling is carried out until the temperature of the steel reaches at least 300°C or less, and a steel with an austenitic structure is obtained as a test material. It should be noted that for the example in which the cooling start temperature difference is 0°C, cooling is shown immediately after the solution heat treatment. Here, in any cooling method, in the temperature range of 1000 to 600°C, the cooling rate is 0.4°C / s or more.

[0186] The obtained test material was subjected to constant current electrolysis to measure the amount of Nb analyzed as the electrolytic extraction residue. Specifically, a test piece of 8 mm square and 40 mm long was collected from the test material and subjected to constant current electrolysis at 20 mA / cm2 using a 10 volume % acetylacetone-1 mass % tetramethylammonium chloride methanol solution as an electrolyte. 2 The test piece is anode-dissolved at a current density of , and carbonitrides and nitrides are extracted as residues. The extracted residue is acid-decomposed and then subjected to ICP (high-frequency inductively coupled plasma) emission analysis to measure the mass of Nb in the residue. The mass of Nb in the residue is divided by the dissolved amount of the test material to determine the amount of Nb present as carbonitrides and nitrides.

[0187] Furthermore, round bar creep test pieces were collected from the obtained test materials and subjected to creep rupture tests. In the evaluation, creep rupture tests were conducted under the conditions of 650°C×216MPa with a target rupture time of 1000 hours for the base material, and test pieces whose rupture time exceeded the target rupture time or whose rupture time satisfied 95% or more of the target rupture time were evaluated as "excellent", test pieces whose rupture time was 90% or more and less than 95% or less were regarded as "acceptable" and evaluated as "qualified", and test pieces whose rupture time was less than 90% were evaluated as "unqualified".

[0188] The obtained test material was reduced to a thickness of 8 mm by machining, and then the end surface in the longitudinal direction was subjected to Figure 1 Groove processing as shown. The groove surface of the test material was butted, and after being restrained all around using a flux-cored electrode specified in A5.11-2005ENiCrFe-3 on a commercially available steel plate equivalent to SM400B specified in JIS G3106:2008 (thickness 20mm, width 150mm, length 150mm), stack welding was performed in the groove by gas tungsten arc welding. During welding, AWS A5.14-2009ERNiCr-3 with an outer diameter of 1.2mm was used as the filler metal, and the heat input was set to about 9 to 12 kJ / cm. In addition, Ar was used as the shielding gas and the back shielding gas, and the flow rate was set to 10L / min.

[0189] Five cross sections were exposed from the obtained welded joints, mirror polished and etched, and then examined under an optical microscope to check whether there were cracks in the welded parts. Welded joints with no cracks observed in all five samples were evaluated as "excellent", welded joints with cracks observed in one sample were evaluated as "acceptable", and welded joints with cracks observed in two or more samples were evaluated as "unacceptable".

[0190] [Table 2]

[0191]

[0192] [Table 3]

[0193]

[0194] [Table 4]

[0195]

[0196] As shown in Tables 2 to 4, by using steels A to F that satisfy the chemical composition specified in the present invention and performing appropriate solution heat treatment, the test body whose intermediate value of formula (i), i.e., the amount of dissolved Nb, satisfies the requirements of the present invention can obtain good creep strength and also has sufficient resistance to welding cracking. In addition, it can be seen that in order to stably obtain these properties, it is preferred that the amount of dissolved Nb satisfies the relationship with the amount of B in formula (v).

[0197] Furthermore, from the comparison between the test piece E1 and the test pieces G1, H1 and K1, it can be seen that the inclusion of more P is preferable for stably obtaining creep strength. In addition, from the comparison between the test pieces A24 and A25, and the test pieces E16 and E19, it can be seen that the cooling start temperature difference preferably satisfies the prescribed range. In addition, from the comparison between the test piece E19 and other examples, it can be seen that when the cooling start temperature difference satisfies the formula (iv), the creep strength is improved.

[0198] In contrast, the heat treatment time of the test pieces A26 and C8 was shorter than the prescribed range, so the elimination of the processing deformation introduced in the forming process became insufficient, and the target creep strength could not be obtained. Furthermore, the heat treatment temperature of the test pieces A8, A19, and E13 was lower than the prescribed range or the heat treatment time was shorter than the prescribed range. In addition, the amount of dissolved Nb was less than the prescribed range, so the precipitation amount in the creep test was insufficient, and the target creep strength could not be obtained.

[0199] In addition, the heat treatment temperature of the test pieces A18, A29, A31 and E12 was higher than the prescribed range, or the heat treatment time was longer than the prescribed range, so the grains were coarsened, and the target weld crack resistance was not obtained. Furthermore, in the test pieces C18 and C20, the amount of solid solution Nb exceeded the prescribed range, so the segregation of Nb caused weld cracks in the weld heat affected zone, and the target weldability was not obtained.

[0200] In the test piece I1 using the symbol I, the Nb content was lower than the range specified in the present invention, so the amount of precipitates containing Nb became insufficient, and the target creep strength could not be obtained. In the test piece J1 using the symbol J, the Nb content exceeded the range specified in the present invention, so the segregation of Nb caused cracks to occur in the weld heat affected zone, and the target weld crack resistance could not be obtained.

[0201] Industrial Applicability

[0202] According to the present invention, it is possible to obtain an austenitic heat-resistant steel which stably has good creep strength and excellent weld crack resistance when used at high temperatures.

Claims

1. A method for producing an austenitic heat-resistant steel, the method comprising: The forming step is to form the steel into a product shape, wherein the chemical composition of the steel is C: 0.04-0.12% by mass, Si: 0.01-0.30%, Mn: 0.50-1.50%, P:0.001~0.040%、 S: 0.0050% or less, Cu: 2.2-3.8%, Ni: 8.0-11.0%, Cr:17.7~19.3%、 Mo: 0.01~0.55%, Nb: 0.400~0.650%, B:0.0010~0.0060%、 N:0.050~0.160%、 Al: 0.025% or less, O: 0.020% or less, Co: 0-1.00%, W:0~1.00%、 Ti: 0~0.40%, V:0~0.40%、 Ta: 0~0.40%, Sn: 0~0.0300%, Ca: 0~0.0100%, Mg: 0~0.0100%, REM: 0~0.0800%、 Balance: Fe and impurities; a solution heat treatment step, wherein heat treatment is performed after the molding step at a heat treatment temperature satisfying the following formula (ii) and a heat treatment time satisfying the following formula (iii); and a cooling step, which is performed after the solution heat treatment step, 0.170≤Nb-Nb ER ≤0.480 (i) -250Nb+1200≤T≤-100Nb+1290 (ii) 405-0.3T≤t≤2475-1.5T (iii) in, The element symbols in the above formula represent the content of the element contained in the steel in mass %, and the symbols in the above formula are defined as follows: Nb ER : The amount of Nb analyzed as the electrolytic extraction residue, that is, the amount of Nb present as precipitates, in mass %; T: heat treatment temperature, in °C; t: heat treatment time, in seconds.

2. The method for producing austenitic heat-resistant steel according to claim 1, wherein: In the cooling step, cooling is performed by forced cooling. The difference between the heat treatment temperature and the temperature of the steel at the start of the forced cooling satisfies the following formula (iv): 0≤△T≤100Nb-5 (iv) The element symbols in the above formula represent the content of the element in steel in mass %, and the symbols in the above formula are defined as follows: ΔT: The difference between the heat treatment temperature of the solution heat treatment and the temperature of the steel when forced cooling starts, in degrees Celsius.

3. The method for producing austenitic heat-resistant steel according to claim 1, wherein: The difference between the Nb content and the Nb amount analyzed as the electrolytic extraction residue satisfies the following formula (v): -2B+0.185≤Nb-Nb ER ≤-4B+0.480 (v) The symbols of the elements in the above formula refer to the content of each element in the steel in mass %, Nb ER It means the amount of Nb in mass % analyzed as the electrolytic extraction residue, that is, the amount of Nb existing as precipitates.

4. The method for producing austenitic heat-resistant steel according to claim 2, wherein: The difference between the Nb content and the Nb amount analyzed as the electrolytic extraction residue satisfies the following formula (v): -2B+0.185≤Nb-Nb ER ≤-4B+0.480 (v) The symbols of the elements in the above formula refer to the content of each element in the steel in mass %, Nb ER It means the amount of Nb in mass % analyzed as the electrolytic extraction residue, that is, the amount of Nb existing as precipitates.

5. The method for producing austenitic heat-resistant steel according to any one of claims 1 to 4, wherein: The chemical composition contains, in mass%, a Co: 0.01~1.00%, W:0.01~1.00%、 Ti: 0.01~0.40%, V:0.01~0.40%、 Ta: 0.01~0.40%, Sn: 0.0002~0.0300%, Ca: 0.0002~0.0100%, Mg: 0.0002 to 0.0100%, and REM: 0.0005~0.0800% One or more of the following.

6. The method for producing austenitic heat-resistant steel according to any one of claims 1 to 4, wherein: The chemical composition contains in mass % P:0.020~0.040%。 7. The method for producing austenitic heat-resistant steel according to claim 5, wherein: The chemical composition contains in mass % P:0.020~0.040%。