Composite electrode, preparation method thereof and lithium ion battery

By using the physical contact between the structured lithium layer and the active material layer in the composite electrode of the lithium ion battery, the utilization rate of lithium metal and the cycling performance of the battery cell are improved, and the low utilization rate of lithium metal and dead lithium in lithium ion battery are solved. The problem of increasing impedance improves the battery's charging and discharging efficiency and cycle life.

CN115528325BActive Publication Date: 2024-11-08JIANGSU TIANHE ENERGY STORAGE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211344009.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-31
Publication Date
2024-11-08
Estimated Expiration
2042-10-31

AI Technical Summary

Technical Problem

The low utilization rate of lithium metal in lithium-ion batteries and the dead lithium covered on the surface of the negative electrode sheet increase impedance, resulting in a decrease in the reversible capacity of the battery cell and a shortened cycle life.

Method used

A composite electrode is designed to form an active material layer on the surface of the current collector and composite a structured lithium layer on it. The structured lithium layer includes lithium and structuring additives, such as graphite, soft carbon, hard carbon, etc., additives. The lithium layer penetrates and forms physical contact with the active material layer to improve the utilization rate of lithium metal.

Benefits of technology

The utilization rate of lithium metal has increased from 55% to 90%, the AC impedance of the battery cell has decreased by 25%, the capacity retention rate of 1500cls in 40℃ cycle has increased by 5%, and the charge and discharge efficiency of 0.5P has increased from 94.0% to 94.6%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003917631050000101
    Figure BDA0003917631050000101
  • Figure HDA0003917631060000011
    Figure HDA0003917631060000011
Patent Text Reader

Abstract

The present invention provides a composite electrode, comprising a current collector, an active material layer composited on the surface of the current collector, and a structured lithium layer composited on the surface of the active material layer; the structured lithium layer comprises lithium and a structured auxiliary agent; the structured auxiliary agent penetrates the structured lithium layer and forms physical contact with the active material layer; the structured auxiliary agent is one or more of graphite, soft carbon, hard carbon, conductive carbon black, carbon fiber, acetylene black, Ketjen black, titanium oxide, conductive polymer particles, graphene and carbon nanotubes. The present invention designs a penetration structure in the lithium metal layer, and compared with the existing rolling lithium supplementation method, the lithium metal utilization rate is increased from 55% to 90%, the AC impedance of the battery cell is reduced by 25%, the capacity retention rate of 1500cls cycle at 40°C is increased by 5%, and the 0.5P charge and discharge efficiency is increased from 94.0% to 94.6%. The present invention also provides a preparation method of the composite electrode and a lithium ion battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium ion batteries, and in particular relates to a composite electrode, a preparation method thereof and a lithium ion battery. Background Art

[0002] The gradual depletion of fossil energy and the increasingly serious greenhouse effect have prompted researchers to continuously explore sustainable and clean energy. Since Sony first commercialized lithium-ion batteries in 1991, lithium-ion batteries have been widely used in 3C digital products and power batteries. Since lithium-ion batteries have more advantages than traditional lead-acid batteries in terms of cycle life, volume energy density and mass energy density, many technicians have been committed to the commercialization of lithium-ion batteries in the past 20 years.

[0003] The actual available capacity and cycle life of the whole battery are closely related to the first coulomb efficiency of the lithium-ion battery and the formation of the negative electrode SEI film. The first efficiency of widely used graphite is between 90% and 95%, and the first irreversible efficiency of hard carbon and silicon-carbon materials with higher energy density exceeds 15%. This is mainly due to the consumption of a large amount of active lithium in the process of forming the solid electrolyte membrane (SEI), which causes the reversible gram capacity of the entire battery cell to be greatly reduced relative to the ideal reversible capacity. In addition, due to the repeated expansion and contraction of the negative electrode during the charge and discharge cycle of the battery cell, SEI will continue to be generated, resulting in a continuous and slow consumption of active lithium. This is the most common capacity decay mode of lithium-ion batteries.

[0004] In order to solve this problem, many researchers have proposed various methods of lithium supplementation, which is also one of the current hot topics in research institutes.

[0005] The main ideas for current lithium replenishment are positive electrode lithium replenishment, negative electrode lithium replenishment and third electrode lithium replenishment. Positive electrode lithium replenishment mainly involves compounding a certain proportion of a high-gram capacity single substance or mixture containing lithium in the preparation process of the positive electrode sheet, and activating it through the first cycle of charging, which significantly improves the charging capacity of the positive electrode sheet. Although the first effect of the negative electrode has not changed, the comprehensive reversible capacity has increased. These mainly include lithium-rich compounds, nanocomposites based on conversion reactions, and binary lithium compounds. Negative electrode lithium replenishment is mainly lithium foil or inert lithium powder. After being compounded with the negative electrode, it forms a primary battery with the negative electrode active material after liquid injection to spontaneously provide active lithium to the negative electrode active material. Some also use built-in third-pole lithium metal for active lithium replenishment. In general, additional lithium replenishment can improve the initial efficiency of the battery cell and the total amount of active lithium that can be operated.

[0006] However, after the liquid electrolyte contacts lithium foil and graphite, the utilization rate of the lithium film is only 30% to 60%. At the same time, considering that the dissolution of lithium metal and the formation of SEI will cause the local lithium metal to lose its electronic conductivity, the unconverted lithium that loses its electronic conductivity (called "dead lithium") will accumulate on the surface of the negative electrode, hindering the transmission of lithium ions between the positive and negative electrodes and increasing the impedance. Summary of the invention

[0007] The object of the present invention is to provide a composite electrode, a preparation method thereof and a lithium ion battery. The utilization rate of lithium metal in the composite electrode of the present invention is significantly improved, and the impedance of the battery cell is reduced.

[0008] The present invention provides a composite electrode, comprising a current collector, an active material layer composited on the surface of the current collector, and a structured lithium layer composited on the surface of the active material layer;

[0009] The structured lithium layer includes lithium and a structured auxiliary agent; the structured auxiliary agent penetrates the structured lithium layer and forms a physical contact with the active material layer;

[0010] The structuring auxiliary agent is one or more of graphite, soft carbon, hard carbon, conductive carbon black, carbon fiber, acetylene black, Ketjen black, titanium dioxide, conductive polymer particles, graphene and carbon nanotubes.

[0011] Preferably, the current collector is copper foil or a composite current collector.

[0012] Preferably, the active material layer comprises an active material, a conductive agent and a binder;

[0013] The active material includes one or more of artificial graphite, natural graphite, silicon-based negative electrode, hard carbon and soft carbon.

[0014] Preferably, the mass ratio of the structuring aid to lithium is (0.01-1):1.

[0015] The present invention provides a method for preparing the composite electrode as described above, comprising the following steps:

[0016] A) coating the active material slurry on the surface of the current collector and forming an active material layer after drying;

[0017] B) rolling and compounding the active material layer with the structured lithium layer compounded on the surface of the polymer film, transferring the structured lithium layer to the surface of the active material layer, to obtain a composite electrode; the structured lithium layer compounded on the surface of the polymer film is obtained by coating a structured auxiliary agent on the surface of the polymer film, rolling and compounding the lithium foil with the surface of the polymer film containing the structured auxiliary agent

[0018] or,

[0019] A structural auxiliary agent is coated on the surface of the active material layer to obtain a rough surface; then a lithium layer composited on the surface of a polymer film is composited with the rough surface, and the lithium layer is transferred to the surface of the active material layer to obtain a composite electrode, wherein the lithium layer composited on the surface of the polymer film is obtained by calendering and composite of the polymer film and lithium foil.

[0020] Preferably, the polymer film is a polypropylene film, a polyvinyl chloride film or a polyethylene terephthalate film;

[0021] The thickness of the polymer film is 6-50 μm.

[0022] Preferably, the thickness of the lithium foil is 30 to 1500 μm.

[0023] Preferably, the lithium foil and the polymer film are rolled and composited to a total thickness of 3 to 30 μm.

[0024] The present invention provides a lithium ion battery, comprising a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, wherein the negative electrode sheet is the composite electrode described above.

[0025] Preferably, the electrolyte comprises an organic solvent and a lithium salt, and the organic solvent is one or more of a carbonate-based solvent, an ether-based solvent and a ketone-based solvent.

[0026] The present invention provides a composite electrode, comprising a current collector, an active material layer composited on the surface of the current collector, and a structured lithium layer composited on the surface of the active material layer; the structured lithium layer comprises lithium and a structured auxiliary agent; the structured auxiliary agent penetrates the structured lithium layer and forms physical contact with the active material layer; the structured auxiliary agent is one or more of graphite, soft carbon, hard carbon, conductive carbon black, carbon fiber, acetylene black, Ketjen black, titanium oxide, conductive polymer particles, graphene and carbon nanotubes. The present invention focuses on solving the problem of low utilization rate of lithium metal supplementation and increased impedance of dead lithium covered on the surface of the negative electrode plate. A penetration structure is designed in the lithium metal layer. Compared with the existing rolling lithium supplementation method, the utilization rate of lithium metal is increased from 55% to 90%, the AC impedance of the battery cell is reduced by 25%, the capacity retention rate of 1500cls cycle at 40°C is increased by 5%, and the 0.5P charge and discharge efficiency is increased from 94.0% to 94.6%. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.

[0028] Figure 1is a schematic diagram of the structure of the composite electrode in the present invention,

[0029] Figure 1 In the figure, 1 is a current collector, 2 and 3 are active material layers, and 4 and 5 are structured lithium layers. DETAILED DESCRIPTION

[0030] The present invention provides a composite electrode, comprising a current collector, an active material layer composited on the surface of the current collector, and a structured lithium layer composited on the surface of the active material layer;

[0031] The structured lithium layer includes lithium and a structured auxiliary agent; the structured auxiliary agent penetrates the structured lithium layer and forms a physical contact with the active material layer;

[0032] The structuring auxiliary agent is one or more of graphite, soft carbon, hard carbon, conductive carbon black, carbon fiber, acetylene black, Ketjen black, titanium dioxide, conductive polymer particles, graphene and carbon nanotubes.

[0033] In the present invention, the current collector is preferably copper foil or a composite current collector.

[0034] In the present invention, the active material layer preferably includes an active material, a conductive agent and a binder, and the active material is preferably one or more of artificial graphite, natural graphite, silicon-based negative electrode, hard carbon and soft carbon; the conductive agent is preferably conductive carbon black and / or acetylene black, and the binder is preferably one or more of fluorine-containing resin, polypropylene resin, fiber-type binder, rubber-type binder and polyimide-type binder. The mass ratio of the active material, the conductive agent and the binder is preferably (95.0-96.5): (0.5-2.0): (1.5-3.0), more preferably (95.0-96.5): (1-1.5): (2-2.5), and most preferably (95.5-96): (1-1.5): (2-2.5). In the present invention, the components and proportions of the two active material layers composited on the two surfaces of the current collector may be the same or different.

[0035] In the present invention, two layers of structured lithium are respectively compounded on the surface of two layers of active material, and the structured lithium layer includes metallic lithium and a structured auxiliary agent, which is made by compounding the structured auxiliary agent with lithium foil by calendering, so that the structured auxiliary agent can penetrate the lithium foil and form a good physical contact with the active material layer. The lithium metal of the structured lithium layer is continuous, and some areas are embedded and / or penetrated by the structured auxiliary agent. The structured auxiliary agent can be attached to the surface of the polymer film carrier or the active material layer by spraying or coating, and then compounded with the lithium foil by calendering.

[0036] In the present invention, the structural aid is preferably one or more of graphite, soft carbon, hard carbon, conductive carbon black, carbon fiber, acetylene black, Ketjen black, titanium dioxide, conductive polymer particles, graphene and carbon nanotubes. Specifically, in the embodiments of the present invention, it can be a combination of multiple substances, preferably including structural aids with a relatively large aspect ratio, such as carbon fiber, carbon nanotubes, etc. For example, a mixture of carbon black, multilayer graphene and carbon nanotubes with a relatively large aspect ratio has a better effect than a single type of structural aid. The present invention has no special restrictions on the proportion of each substance in the mixture of the multiple structural aids, which can form a structure that penetrates the metal lithium layer structure; the mass ratio of the structuring aid to the metallic lithium is preferably (0.01-1):1, more preferably (0.05-0.66):1, such as 0.01:1, 0.05:1, 0.1:1, 0.15:1, 0.2:1, 0.25:1, 0.3:1, 0.35:1, 0.4:1, 0.45:1, 0.5:1, 0.55:1, 0.6:1, 0.66:1, 0.7:1, 0.75:1, 0.8:1, 0.85:1, 0.9:1, 0.95:1, 1:1, preferably a range value with any of the above values ​​as the upper or lower limit.

[0037] In the present invention, the components and proportions of the two structured lithium layers may be the same or different.

[0038] The present invention also provides a method for preparing a composite electrode, comprising the following steps:

[0039] A) coating the active material slurry on the surface of the current collector and forming an active material layer after drying;

[0040] B) rolling and compounding the active material layer with the structured lithium layer compounded on the surface of the polymer film, transferring the structured lithium layer to the surface of the active material layer, to obtain a composite electrode; the structured lithium layer compounded on the surface of the polymer film is obtained by coating a structured auxiliary agent on the surface of the polymer film, rolling and compounding the lithium foil with the surface of the polymer film containing the structured auxiliary agent

[0041] or,

[0042] A structural auxiliary agent is coated on the surface of the active material layer to obtain a rough surface; then a lithium layer composited on the surface of a polymer film is composited with the rough surface, and the lithium layer is transferred to the surface of the active material layer to obtain a composite electrode, wherein the lithium layer composited on the surface of the polymer film is obtained by calendering and composite of the polymer film and lithium foil.

[0043] The present invention coats the active material slurry on the two surfaces of the current collector, and rolls it after drying to obtain an initial pole piece composited with an active material layer.

[0044] In the present invention, the active material slurry preferably includes an active substance, a conductive agent, a binder and a solvent, and the solvent is preferably deionized water; the types and amounts of the active substance, conductive agent and binder are consistent with the types and amounts of the active substance, conductive agent and binder described above, and the present invention will not be repeated here.

[0045] In the present invention, the drying temperature is preferably 50 to 80° C., more preferably 60 to 70° C.; the drying time is preferably 5 to 20 min, more preferably 10 to 15 min.

[0046] After obtaining the initial electrode, the present invention uses lithium foil as the lithium source in the structured lithium layer, and uses the polymer film as the carrier for calendering and thinning the lithium foil. The structuring auxiliary agent and the lithium foil are calendered and compounded by a calendering compound method to form a structured lithium layer on the surface of the active material layer. Specifically, in an embodiment of the present invention, the calendering compounding can be performed in any one of the following two ways.

[0047] In one embodiment of the present invention, a structuring auxiliary agent is coated on the surface of a polymer film, and a lithium foil is rolled and composited with the surface of the polymer film containing the structuring auxiliary agent to obtain a structured lithium layer composited on the surface of the polymer film; then the structured lithium layer is rolled and composited with an active material layer, and the structured lithium layer is transferred to the surface of the active material layer to obtain a composite electrode.

[0048] In the present invention, the polymer film is preferably a polypropylene film, a polyvinyl chloride film or a polyethylene terephthalate film; the thickness of the polymer film is preferably 6 to 50 μm, more preferably 10 to 40 μm, such as 6 μm, 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm, preferably a range value with any of the above values ​​as the upper or lower limit.

[0049] In the present invention, the type and amount of the structuring aid are consistent with the type and amount of the structuring aid described above, and the present invention will not be repeated here. The spraying thickness of the structuring aid on the surface of the polymer film is preferably 1 to 15 μm; the thickness of the lithium foil is preferably 30 to 1500 μm, more preferably 100 to 1000 μm, such as 30 μm, 50 μm, 100 μm, 200 μm, 300 μm, 400 μm, 500 μm, 600 μm, 700 μm, 800 μm, 900 μm, 1000 μm, 1100 μm, 1200 μm, 1300 μm, 1400 μm, 1500 μm, preferably a range value with any of the above values ​​as the upper or lower limit.

[0050] In the present invention, the lithium foil and the surface of the polymer film containing the structuring aid are rolled and composited to a total thickness of 3 to 40 μm. In the obtained structured lithium layer, the content of lithium metal is preferably 50 to 95%, more preferably 60 to 80%, such as 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, preferably a range value with any of the above values ​​as the upper or lower limit.

[0051] The surface containing structured lithium metal is called the first surface. The first surface is rolled and composited with two active material layers of the initial negative electrode sheet respectively, so that the structured lithium layer is transferred to the surface of the active material layer to obtain a composite negative electrode.

[0052] In another embodiment of the present invention, the polymer film and lithium foil are rolled and composited to obtain a lithium layer composited on the surface of the polymer film;

[0053] Coating a structuring agent on the surface of the active material layer to obtain a rough surface;

[0054] The lithium layer is rolled and compounded with the rough surface, and the lithium layer is transferred to the surface of the active material layer to obtain a composite electrode.

[0055] In the present invention, the polymer film is preferably a polypropylene film, a polyvinyl chloride film or a polyethylene terephthalate film; the thickness of the polymer film is preferably 6 to 50 μm, more preferably 10 to 40 μm, such as 6 μm, 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm, preferably a range value with any of the above values ​​as the upper or lower limit.

[0056] In the present invention, the thickness of the lithium foil is preferably 30 to 1500 μm, more preferably 100 to 1000 μm, such as 30 μm, 50 μm, 100 μm, 200 μm, 300 μm, 400 μm, 500 μm, 600 μm, 700 μm, 800 μm, 900 μm, 1000 μm, 1100 μm, 1200 μm, 1300 μm, 1400 μm, 1500 μm, preferably a range value with any of the above values ​​as the upper or lower limit.

[0057] In the present invention, the lithium foil and the surface of the polymer film are rolled and composited to a total thickness of 3 to 40 μm.

[0058] In the present invention, the type and amount of the structuring aid are consistent with the type and amount of the structuring aid described above, and the present invention will not repeat them here. The spraying thickness of the structuring aid on the surface of the active material layer is preferably 1 to 15 μm.

[0059] The present invention rolls and compounds the lithium layer with the rough surface to form a structured lithium layer, and at the same time, transfers the structured lithium layer to the surface of the active material layer. In the present invention, in the structured lithium layer, the lithium layer and the rough surface are rolled and compounded.

[0060] The above preparation method in the present invention can be applied to the preparation of the positive electrode or negative electrode of a lithium ion battery. In the embodiments of the present invention, the negative electrode is taken as an example for specific description.

[0061] The present invention also provides a lithium ion battery, comprising a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, wherein the negative electrode sheet is the composite electrode described above.

[0062] In the present invention, the active material in the positive electrode sheet includes at least one of lithium nickel cobalt manganese oxide, lithium cobalt oxide, lithium manganese oxide, lithium-rich manganese-based positive electrode material, lithium iron phosphate and lithium iron manganese phosphate that can embed and extract lithium ions.

[0063] In the present invention, the separator is composed of a sheet or non-woven fabric made of an olefin polymer having chemical resistance and hydrophobicity, such as polypropylene, glass fiber or polyethylene. The pore size of the separator is preferably 0.01 to 10 μm, more preferably 0.1 to 5 μm; the thickness of the separator is preferably 5 to 25 μm, more preferably 10 to 20 μm. When a solid electrolyte such as a polymer is used as the electrolyte, the solid electrolyte can also serve as a separator.

[0064] In the present invention, the electrolyte comprises an organic solvent and a lithium salt, wherein the organic solvent is one or more of a carbonate-based solvent, an ether-based solvent and a ketone-based solvent, and more preferably an aprotic organic solvent, such as propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, γ-butyrolactone, 1,2-dimethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, triester phosphate, trimethylol ester, trimethylol ester, methyl ether ... One or more of oxymethane, dioxolane derivatives, cyclopentane, methyl cyclopentane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ethers, methyl propionate and ethyl propionate; the lithium salt is preferably one or more of LiCl, LiBr, LiI, LiClO4, LiBF4, LiPF6, LiCF3SO3, LiCF3CO2, LiAsF6, LiSbF6, LiAlCl4, CH3SO3Li and (CF3SO2)2NLi.

[0065] The present invention provides a composite electrode, comprising a current collector, an active material layer composited on two surfaces of the current collector, and a structured lithium layer composited on the surface of the active material layer; the structured lithium layer comprises lithium and a structured auxiliary agent; the structured auxiliary agent penetrates the structured lithium layer and forms physical contact with the active material layer; the structured auxiliary agent is one or more of graphite, soft carbon, hard carbon, conductive carbon black, carbon fiber, acetylene black, Ketjen black, titanium oxide, conductive polymer particles, graphene and carbon nanotubes. The present invention focuses on solving the problem of low utilization rate of lithium metal supplementation and increased impedance of dead lithium covered on the surface of the negative electrode plate. A penetration structure is designed in the lithium metal layer. Compared with the existing rolling lithium supplementation method, the utilization rate of lithium metal is increased from 55% to 90%, the AC impedance of the battery cell is reduced by 25%, the capacity retention rate of 1500cls cycle at 40°C is increased by 5%, and the 0.5P charge and discharge efficiency is increased from 94.0% to 94.6%.

[0066] In order to further illustrate the present invention, a composite electrode, a preparation method thereof and a lithium ion battery provided by the present invention are described in detail below in conjunction with embodiments, but they should not be construed as limiting the scope of protection of the present invention.

[0067] Example 1

[0068] (1) Preparation of positive electrode

[0069] LiFePO4, conductive carbon black and polyvinylidene fluoride are dispersed in N-methylpyrrolidone to form a positive electrode active material slurry. Among them, the weight ratio of LiFePO4: conductive carbon black: polyvinylidene fluoride is 96.5%: 1.6%: 1.9%. The slurry is spread on both surfaces of 13μm aluminum foil, and then dried at 90℃ for 10 minutes. The double-sided density of the dried coating is 33.2mg / cm2. After rolling, it is punched into a pole piece with a pole ear of 70.5mm wide and 81.0mm high.

[0070] (2) Preparation of composite negative electrode sheets

[0071] Graphite, conductive carbon black, hydroxymethyl cellulose and styrene butadiene rubber are dispersed in deionized water to form a negative electrode active material slurry. Among them, the weight ratio of graphite: conductive carbon black: hydroxymethyl cellulose: styrene butadiene rubber is 96:0.8::1.2:2. The slurry is coated on both surfaces of copper foil (thickness 8μm), and then dried at 60°C for 10 minutes to form a negative electrode active material layer. The double-sided coating surface density after drying is 16.0mg / cm2. After rolling, it is punched into an initial negative electrode sheet with a 74.5mm wide and 85.0mm high tab. A 50μm initial lithium foil is used as the raw material, and a 30μm polymer film is used as the carrier for lithium foil calendering and thinning. The polymer film is polyethylene terephthalate. First, a mixture of carbon black, carbon nanotubes and multilayer graphene is sprayed on one surface of the polymer film by an electrostatic powder spray gun, and then the initial lithium foil and the surface of the polymer film containing the structural additive are rolled and composited to a total thickness of 38μm to form a structured lithium metal, the lithium metal content in the structured lithium metal is 65%, and the surface containing the structured lithium metal is called the first surface. Finally, the two surfaces of the initial negative electrode sheet are respectively rolled and composited with a first surface, so that the structured lithium metal is transferred to the surface of the active material layer to obtain a composite negative electrode sheet.

[0072] (3) Preparation of lithium secondary batteries

[0073] The positive and negative electrodes and polyethylene diaphragm are laminated into a core package of a lithium ion secondary battery (thickness 5.5mm, width 75.0mm, height 89.5mm), and the core package is encapsulated in an aluminum-plastic film bag. Subsequently, LiPF6 is dissolved in a mixed solvent of EC / PC / EMC=35:5:60 (mass ratio) at a concentration of 1mol / L to form a non-aqueous electrolyte, and finally 2.5% of vinylene carbonate is added as a film-forming additive. The electrolyte is injected into the above aluminum-plastic film bag in an amount of 4.5g / Ah and sealed. After standing for 24h, it is formed at 45℃, and then the gas is extracted under negative pressure and then sealed again, and then charged to 3.65V at 1.0C, constant voltage at 3.65V to a current of 0.05C, and then discharged to 2.5V at 1.0C to obtain an initial discharge capacity C0.

[0074] (4) Cycle test

[0075] The cycle test temperature is 40°C, the process is:

[0076] ①Stay still for 5 minutes

[0077] ②1.0C constant current charging to 3.65V, 3.65V constant voltage to 0.05C

[0078] ③Stay still for 5 minutes

[0079] ④1.0C constant current discharge to 2.5V

[0080] ⑤Stay still for 5 minutes

[0081] ⑥ Repeat steps 2-5 1500 times, and the 1500th discharge capacity is recorded as C 1500

[0082] ⑦1.0C constant current charging to 4.3V, 4.3V constant voltage to 0.05C

[0083] ⑧Stay still for 5 minutes

[0084] ⑨1.0C discharge to 2.5V

[0085] ⑩ Repeat steps 2-5 once, and record the capacity as C j

[0086] Example 2

[0087] A lithium secondary battery is prepared according to the preparation method in Example 1, except that the composite process in this embodiment is changed to: the active material layer is coated on both sides of the current collector and dried and rolled to obtain an initial negative electrode sheet, and a mixture of carbon black, carbon nanotubes and multilayer graphene is sprayed on both surfaces of the initial negative electrode sheet by an electrostatic powder spraying gun to obtain a rough negative electrode sheet. A 50μm initial lithium foil is used as a raw material, and a 30μm polymer film is used as a carrier for calendering and thinning of the lithium foil, and the polymer film is polyethylene terephthalate. The initial lithium foil and one surface of the polymer film are calendered and composited to a total thickness of 38μm, and the surface containing lithium metal is called the first surface. Finally, the two surfaces of the rough negative electrode sheet are calendered and composited with a first surface, so that the lithium metal is transferred to the surface of the active material layer, and the structured auxiliary agent and lithium metal are composited to obtain structured lithium metal. The rest is consistent with Example 1.

[0088] Comparative Example 1

[0089] Compared with Example 1, the negative electrode is directly laminated using the initial negative electrode sheet, the positive electrode sheet and the polyethylene separator, and the rest is consistent with Example 1.

[0090] Comparative Example 2

[0091] A lithium secondary battery is prepared according to the preparation method in Example 1, except that the composite process of this comparative example is changed to: the active material layer is coated on both sides of the current collector, dried and rolled to obtain an initial negative electrode sheet. A 50μm initial lithium foil is used as a raw material, and a 30μm polymer film is used as a carrier for calendering and thinning of the lithium foil, and the polymer film is polyethylene terephthalate. The initial lithium foil and one surface of the polymer film are calendered and composited to a total thickness of 38μm, and the surface containing lithium metal is called the first surface. Finally, the two surfaces of the initial negative electrode sheet are each calendered and composited with a first surface to transfer the lithium metal to the surface of the active material layer. The rest is consistent with Example 1.

[0092] Table 1 Performance data of lithium secondary batteries obtained in the embodiments of the present invention and comparative examples

[0093]

[0094] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a composite electrode, comprising the following steps: A) coating the active material slurry on the surface of the current collector and forming an active material layer after drying; B) rolling and compounding the active material layer with the structured lithium layer compounded on the surface of the polymer film, and transferring the structured lithium layer to the surface of the active material layer to obtain a composite electrode; the structured lithium layer compounded on the surface of the polymer film is obtained by coating a structured auxiliary agent on the surface of the polymer film, and rolling and compounding lithium foil with the surface of the polymer film containing the structured auxiliary agent; or, A structural auxiliary agent is coated on the surface of the active material layer to obtain a rough surface; then a lithium layer composited on the surface of the polymer film is composited with the rough surface, and the lithium layer is transferred to the surface of the active material layer to obtain a composite electrode, wherein the lithium layer composited on the surface of the polymer film is obtained by calendering and composite of the polymer film and lithium foil; The composite electrode comprises a current collector, an active material layer composited on the surface of the current collector, and a structured lithium layer composited on the surface of the active material layer; The structured lithium layer includes lithium and a structured auxiliary agent; the structured auxiliary agent penetrates the structured lithium layer and forms a physical contact with the active material layer; The structural auxiliary agent is one or more of graphite, conductive carbon black, carbon fiber, titanium dioxide, conductive polymer particles, graphene and carbon nanotubes.

2. The preparation method according to claim 1, characterized in that: The current collector is copper foil or a composite current collector.

3. The preparation method according to claim 1, characterized in that: The active material layer includes an active material, a conductive agent and a binder; The active material includes one or more of silicon-based negative electrode material, hard carbon and soft carbon.

4. The preparation method according to claim 1, characterized in that: The mass ratio of the structuring aid to lithium is (0.01~1):

1.

5. The preparation method according to claim 1, characterized in that: The polymer film is a polypropylene film, a polyvinyl chloride film or a polyethylene terephthalate film; The thickness of the polymer film is 6-50 μm.

6. The preparation method according to claim 1, characterized in that: The thickness of the lithium foil is 30-1500 μm.

7. The preparation method according to claim 6, characterized in that: The lithium foil and the polymer film are rolled and compounded to a total thickness of 3 to 30 μm.