Waffle fleece warm knitted fabric and preparation method thereof

By using differentiated polyester yarn and refined yarn all cotton yarn in waffle fabrics, combined with specific process processing, the problems of poor warming effect and insufficient shape of waffle fabrics are solved, achieving a high visual sense. Good warmth and tensile deformation resistance.

CN115595712BActive Publication Date: 2024-11-22NINGBO DAQIAN TEXTILE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211235584.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-10
Publication Date
2024-11-22
Estimated Expiration
2042-10-10

AI Technical Summary

Technical Problem

The existing waffle fabric has poor warmth, insufficient shape and is prone to stretching and deformation.

Method used

The first DTY differentiated polyester yarn and the second DTY differentiated polyester yarn are interwoven, combined with refined yarn all cotton yarn to form a waffle fabric with a double-sided structure, and is washed with flat webs, first woven, dyed, The second woven and reshaping process improves the tightness and warmth of the fabric.

Benefits of technology

It achieves a high visual sense, fashionable feeling and good warmth effect of the fabric, while avoiding stretching and deformation, improving hair grab density and feel comfort.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115595712B_ABST
    Figure CN115595712B_ABST
Patent Text Reader

Abstract

The present invention provides a waffle fleece warm knitted fabric and a preparation method thereof, wherein the fabric has a double-sided structure, one side is a plane structure, and the other side is a waffle structure, wherein the plane is woven with a first DTY differentiated polyester yarn, the yarn count of the first DTY differentiated polyester yarn is 160-200D, and the connecting wire between the waffle and the plane is woven with a second DTY differentiated polyester yarn, the yarn count of the second DTY differentiated polyester yarn is 60-100D. The present invention adopts two differentiated easy-shrink yarns, the first DTY differentiated polyester yarn and the second DTY differentiated polyester yarn, so that the woven fabric is more compact and less likely to deform, and the obtained waffle fabric has better warming performance. The woven fabric is first subjected to an open-width water washing treatment, and the first and second DTY differentiated polyester yarns shrink more evenly after open-width water washing, so that the gaps between the yarns are filled more fully, the fabric is more compact, the warming effect is better, and it is less likely to be stretched and deformed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of knitted fabrics, and in particular to a waffle fleece warm-keeping knitted fabric and a preparation method thereof. Background Art

[0002] The appearance of the napped fabrics on the market is relatively monotonous, lacking in fashion and innovation, and the napped thickness is relatively thin, and the warmth-keeping effect is poor; waffle fabrics have a strong visual and fashion sense, and their surface is rough, with obvious square or diamond-shaped convexities, and are deeply loved by the market, but they do not have a warmth-keeping effect, lack a sense of shape, and are prone to stretching and deformation.

[0003] The prior art with publication number CN212688349U discloses a non-dyed waffle fabric, which is knitted by upper and lower needles for a cycle of 40 loops to form upper and lower sides, each loop includes 16 loops, and the loops 1, 3, 4, 7, 8, 11, 12, 15, and 16 in the loops 1, 5, 9, 13, 17, 21, 25, 29, 33, and 37 are loops, wherein the loop 1 is at the bottom, and the loops 3, 4, 7, 8, The coils of 11, 12, 15, and 16 are on the top; the coils of 1, 2, 3, 5, 6, 7, 9, 10, 11, 13, 14, and 15 in the 3, 7, 11, 15, 19, 23, 27, 31, 35, and 39 are looped, among which the coils of 1, 2, 5, 6, 9, 10, 13, and 14 are on the top, and the coils of 3, 7, 11, and 15 are on the bottom; the coils in the even-numbered circuits are all looped and on the top. The Chinese clothing pattern fabric woven by the prior art has poor warmth retention effect, insufficient shape, and is prone to stretching and deformation. Summary of the invention

[0004] In view of this, the present invention aims to provide a waffle fleece warm knitted fabric and a preparation method thereof, so as to solve the problems of poor warming effect, insufficient shape and easy stretching deformation of the waffle fleece fabric knitted in the prior art.

[0005] To achieve the above object, the technical solution of the present invention is achieved as follows:

[0006] A waffle fleece warm knitted fabric, the fabric having a double-sided structure, one side being a plane structure and the other side being a waffle structure, the plane being woven with a first DTY differentiated polyester yarn, the yarn count of the first DTY differentiated polyester yarn being 160-200D, the connecting wire between the waffle and the plane being woven with a second DTY differentiated polyester yarn, the yarn count of the second DTY differentiated polyester yarn being 60-100D.

[0007] The arrangement adopts two differentiated easily shrinkable yarns, namely the first DTY differentiated polyester yarn and the second DTY differentiated polyester yarn, so that the woven fabric is tighter and the waffle fabric has better warmth retention performance.

[0008] Furthermore, the waffle surface is woven with fine cotton yarn, which makes the waffle surface more soft and improves the comfort of users.

[0009] Furthermore, the fabric consists of 6 loops as a cycle, and is woven into upper and lower surfaces in the order of arrangement from the upper needle disc to the lower needle cylinder. The upper and lower needles on the 1st loop are both looped; the upper, 3rd and 4th needles are tucked together and the lower needle is looped; the upper and 6th needles are looped together and the lower needle is tucked together.

[0010] Furthermore, the yarn woven in the first pass is the second DTY differentiated polyester yarn, the yarn woven in the second, third and fourth passes is the first DTY differentiated polyester yarn, and the yarn woven in the fifth and sixth passes is fine cotton yarn.

[0011] Furthermore, the yarn count of the fine cotton yarn ranges from 25 to 35S.

[0012] A method for preparing a fabric, the method being used to prepare the above-mentioned waffle fleece warm knitted fabric, the method comprising:

[0013] S1: Yarn count preparation;

[0014] S2: fabric weaving;

[0015] S3: fabric pretreatment;

[0016] S4: Dyeing and finishing process.

[0017] Further, step S3 includes:

[0018] S31: open width washing;

[0019] S32: flat retraction;

[0020] S33: First hair pulling;

[0021] Furthermore, the step S4 comprises:

[0022] S41: Predetermined type;

[0023] S42: Dyeing;

[0024] S43: Second roughening;

[0025] S44: Shearing treatment;

[0026] S45: Re-setting.

[0027] Further, step S31, open-width washing includes washing and shrinking the fabric woven in step S2 at an open width, at a temperature of 60-90°C and for 20-30 minutes. The fabric is first subjected to open-width washing and shrinking treatment, and the fabric surface becomes more fluffy after the differential polyester yarn shrinks. The fabric obtained after pretreatment feels firm and fluffy, and is easier to pick up, thereby improving the efficiency of the picking machine.

[0028] Further, in step S33, the first napping includes feeding the fabric after the flat width shrinkage into a napping machine, performing napping treatment on the plane, the napping speed is 8-15 m / min, the tension on the machine is 5-15 N, the napping is reversed, and the napping is continuously pulled 1-5 times. The fabric after the flat width washing and shrinkage is easier to nap, and after the first napping, the fabric feels firm and fluffy, and has a certain warmth-keeping effect.

[0029] The present invention also provides a method for preparing the waffle fleece warm knitted fabric, and the method is used to prepare the waffle fleece warm knitted fabric mentioned above.

[0030] Compared with the prior art, the waffle fleece warm knitted fabric and the preparation method thereof of the present invention have the following advantages:

[0031] 1) The waffle fleece warm knitted fabric described in the present application is interwoven with DTY differentiated polyester yarn and cotton yarn, so that one side has a strong visual sense and a fashionable sense, and its surface is rough with obvious square or diamond-shaped concave and convex feeling, and the other side has good tightness, is not easy to stretch and deform, and has a good warming effect;

[0032] 2) The preparation method of the waffle wool warm knitted fabric described in the present application breaks the conventional process, which is generally to directly grab the wool after dyeing, so that the density, thickness and hair loss of the wool cannot be well taken into account. The present application first performs an open-width water washing and shrinking treatment on the fabric, so that the DTY differentiated polyester yarn is more uniform after the open-width water washing and shrinking, so that the gaps between the yarns are filled more fully, making the fabric more compact, with good warmth retention effect, and not easy to be stretched and deformed;

[0033] 3) The waffle nap warm knitted fabric described in this application is softened by adding a softener during dyeing and a softener in the shaping groove during reshaping, so that the obtained fabric has a better fabric feel and a better nap feel;

[0034] 4) In the present application, the woven fabric is first shrunk and then the hair is picked, which is not only easier to raise, but also has better density and concentration of the picked hair. After the rough is picked, it is subjected to high-temperature shaping and dyeing treatment, and the floating hair will also be processed. After dyeing, the napped surface is fluffed and the floating hair is repaired. The picked hair obtained in this way is not only denser, but also thick and fluffy as a whole, and the hair shedding of the picked hair surface is very good. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 This is a knitting arrangement diagram of the waffle fleece warm knitted fabric of the present invention;

[0036] Figure 2 This is a triangle arrangement diagram of the waffle fleece warm knitted fabric of the present invention. DETAILED DESCRIPTION

[0037] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, specific embodiments of the present invention are described in detail below with reference to the accompanying drawings.

[0038] Example 1

[0039] The invention relates to a waffle fleece warm knitted fabric with a double-sided structure. The fabric is woven by an 18G double-sided machine, and the blank is dropped from the machine into a cylinder to obtain a fabric with one side being a waffle and the other side being a plane. Preferably, the side close to the skin is a plane structure, and the side away from the skin is a waffle structure. The raw material of the plane is a first DTY differentiated polyester yarn, the connecting wire between the waffle and the plane is woven by a second DTY differentiated polyester yarn, and the waffle side is woven by fine yarn pure cotton yarn, wherein DTY is the abbreviation of Draw texturing yarn, which means drawn texturing yarn.

[0040] This setting makes one side have a strong visual sense and fashion sense, its surface is rough, with obvious square or diamond-shaped convex and concave feeling, and the other side has good tightness, is not easy to stretch and deform, and has good warmth retention effect.

[0041] like Figure 1 As shown, the waffle wool warm knitted fabric has a weaving structure with one needle track on the upper needle disk and one needle track on the lower needle cylinder. Specifically, the arrangement relationship of the upper and lower needles is that the upper needles are arranged in a 011 cycle, 0 is a drawn needle, 1 is knitted, and the lower needles are arranged in a 110 cycle.

[0042] like Figure 2 As shown in the figure, the waffle wool warm knitted fabric is woven with 6 loops as one cycle, and the upper and lower sides are formed according to the arrangement order from the upper needle disc to the lower needle cylinder. The upper and lower needles of the first loop are looped; the second, third, and fourth loops are tucked, and the lower needles are looped; the fifth and sixth loops are looped, and the lower needles are tucked. The fabric woven with this setting not only has a three-dimensional checkered effect on the surface, but also has a tighter overall fabric.

[0043] The yarn woven in the first thread is the second DTY differentiated polyester yarn, the yarn woven in the second, third and fourth threads is the first DTY differentiated polyester yarn, and the yarn woven in the fifth and sixth threads is fine cotton yarn.

[0044] Preferably, the yarn count of the first DTY differentiated polyester yarn ranges from 160 to 200D, the yarn count of the second DTY differentiated polyester yarn ranges from 60 to 100D, and the yarn count of the pure cotton yarn ranges from 25 to 35S.

[0045] Specifically, the first thread is woven with 80D / 156F polyester yarn, the second, third and fourth threads are woven with 180D / 156F polyester yarn, and the fifth and sixth threads are woven with 30S fine cotton yarn.

[0046] This setting makes the thickness of polyester yarn and cotton yarn connected on different routes have certain differences, and the stripes on the surface of the fabric formed by knitting have a certain concave-convex feeling, which not only makes the surface of the fabric more compact, but also has a better raising effect on the plane.

[0047] Specifically, the coils include tucking and forming loops, and the length of the coils of the 1st to 4th routes is 20-25 cm / 100 stitches. Preferably, the length of the coils of the 1st to 4th routes is 22 cm / 100 stitches.

[0048] Furthermore, the length of the coils of the 5th and 6th routes is 15 to 20 cm / 100 needles, and preferably, the length of the coils of the 5th and 6th routes is 18 cm / 100 needles.

[0049] The arrangement makes the woven fabric uneven and three-dimensional, with good strength and not easy to deform.

[0050] Example 2

[0051] A method for preparing a waffle fleece warm knitted fabric, the method being used to prepare the fabric described in Example 1, the method comprising the following steps;

[0052] S1: Yarn count preparation;

[0053] S2: fabric weaving;

[0054] S3: fabric pretreatment;

[0055] S4: Dyeing and finishing process.

[0056] Furthermore, in step S1, the yarn count preparation process includes: selecting DTY differentiated polyester yarn and cotton yarn as weaving materials.

[0057] Preferably, in step S1, a first DTY differentiated polyester yarn with a thickness of 160-200D, a second DTY differentiated polyester yarn with a thickness of 60-100D, and a fine cotton yarn with a thickness of 25-35S are selected as the weaving materials.

[0058] More preferably, the flat surface is made of DTY differentiated polyester yarn with a thickness of 160D, the middle connecting yarn is made of DTY differentiated polyester yarn with a thickness of 80D, and the waffle surface is mainly made of fine cotton yarn with a thickness of 30S.

[0059] The fabric obtained by this arrangement has a strong visual sense and a fashionable sense on one side, a rough surface with obvious square or diamond-shaped concave and convex feeling, and a good raising effect and good warmth retention performance on the other side.

[0060] Further, in step S2, the fabric weaving process includes a weaving structure of an upper needle disc and a needle track, and a lower needle cylinder and a needle track. The knitting needles of the fabric are as follows: 6 routes are a cycle, and the upper and lower sides are woven according to the arrangement order from the upper needle disc to the lower needle cylinder. The upper needle and the lower needle on the 1st route are both in loops; the needles on the 2nd, 3rd, and 4th routes are tucked together, and the lower needle is tucked together; the needles on the 5th and 6th routes are tucked together, and the lower needle is tucked together.

[0061] Furthermore, in step S2, the yarn woven in the first pass is the second DTY differentiated polyester yarn, the yarn woven in the second, third and fourth passes is the first DTY differentiated polyester yarn, and the yarn woven in the fifth and sixth passes is fine cotton yarn.

[0062] Specifically, the yarn woven in the first pass is 80D / 156F polyester yarn, the yarn woven in the second, third and fourth passes is 180D / 156F polyester yarn, and the yarn woven in the fifth and sixth passes is 30SJC pure cotton.

[0063] Furthermore, the step S3, fabric pretreatment comprises the following steps:

[0064] S31: open width washing;

[0065] S32: flat retraction;

[0066] S33: First hair pulling;

[0067] Among them, step S31, the blank open-width water washing includes washing and shrinking the fabric woven in step S2 at an open width, at a temperature of 60-90°C and a time of 20 to 30 minutes, so that the fabric can fully shrink. Conventional processes are to directly grab the hair after dyeing, so the density, thickness and hair loss of the grabbed hair cannot be well taken into account. The fabric is first subjected to open-width water washing and shrinkage treatment, and the fabric surface is more fluffy after the differential polyester yarn shrinks. The fabric obtained after pretreatment feels firm and fluffy, and is easier to grab hair, thereby improving the efficiency of the grabbing machine. Preferably, the open-width water washing temperature is 90°C and the time is 20 minutes.

[0068] In this embodiment, step S32, open-width shrinking includes slitting the fabric after the open-width washing in step S31, and then putting it into an open-width dryer for an open-width shrinking, the temperature is 90-130°C, the speed is 10-50m / min, and steam is sprayed in the middle of the dryer to make the surface of the fabric uniform and flat, which is convenient for the subsequent fabric raising. Preferably, the temperature is 110°C and the speed is 30m / min.

[0069] In this embodiment, step S33, the first napping includes that the fabric after the flat width shrinkage is put into the napping machine, the flat surface is napped, the napping speed is 8-15m / min, the tension on the machine is 5-15N, the napping is reversed, and the napping is continuously pulled 1-3 times. This setting makes the fabric easier to nap after the flat width washing and shrinkage, and after the first napping, the fabric feels firm and fluffy, and has a certain warming effect. Preferably, the napping speed is 10m / min, the tension on the machine is 9N, and the napping is continuously pulled 3 times.

[0070] Furthermore, the step S4, dyeing comprises the following steps:

[0071] S41: Predetermined type;

[0072] S42: Dyeing;

[0073] S43: Second roughening;

[0074] S44: Shearing treatment;

[0075] S45: Re-setting.

[0076] In this embodiment, step S41, pre-setting includes, the fabric after the first napping treatment is subjected to high-temperature pre-setting at 160-200°C, the vehicle speed is 15-30m / min, the overfeed is 20%-40%, and the setting machine air volume is 60-90CFM. This setting prevents the fabric from becoming thinner or the napping effect is poor during the subsequent dyeing process, and the fabric stability is poor. Preferably, the pre-setting temperature is 175°C, the vehicle speed is 25m / min, the overfeed is 25%, and the setting machine air volume is 80CFM.

[0077] In this embodiment, step S42, dyeing includes, the fabric after pre-setting treatment enters the dyeing vat, the bath ratio is 1:10, and both polyester and cotton can be dyed. When the softener is treated in the dyeing vat, a bulking agent is added to the fabric, wherein the softener concentration is 10-30g / l, and the bulking agent concentration ratio is 10-15g / l, heated to 50-70°C, and operated for 10-30min. This setting is convenient for subsequent napping and shearing. After dyeing, the fabric is first dehydrated and then dried in a dryer for a second napping. Preferably, the softener concentration is 20g / l, the bulking agent concentration is 12g / l, the heating temperature is 60°C, and the operating time is 20°C.

[0078] In this embodiment, step S43, the second napping includes napping the dyed fabric on a napping machine, wherein the tension of the machine is 5-10N and the speed is 10-15m / min. The napping is repeated 1-3 times to obtain a basic finished fabric. This setting can grind the fibers on the surface of the fabric into a fluffy shape, thereby making the surface of the fabric more fluffy and soft, more skin-friendly, and having a better warming effect. Preferably, the tension of the machine is 7N, the speed is 12m / min, and the napping is repeated twice.

[0079] In this embodiment, step S44, the shearing treatment includes shearing the fabric after the second napping treatment on a shearing machine, with a shearing speed of 10 to 15 m / min, a machine tension of 8 to 12 N, and shearing 1 to 3 times, and shearing off the surface of the napped surface and floating hair on other surfaces to ensure that the final hairiness falls off. Preferably, the shearing speed is 12 m / min, the machine tension is 10 N, and shearing is done once.

[0080] In this embodiment, step S45, re-setting includes setting the shearing process on a setting machine, wherein 10-30 g / l of softener is added to the setting machine groove, the re-setting temperature is 120-150°C, the speed is 20-40 m / min, the overfeed is 20%-40%, the air volume is 70-90 CFM, and the napping process causes the softener to fall off the fabric, and the napping increases the surface roughness of the fabric. When softener is added to the setting machine groove, the fabric is both set and allowed to absorb more softener, thereby obtaining a better fabric feel and a better raised feel. Preferably, the softener concentration is 20 g / l, the re-setting temperature is 150°C, the speed is 25 m / min, the overfeed is 30%, and the air volume is 80 CFM.

[0081] In summary, it is not difficult to conclude that the fabric and preparation method thereof provided in this embodiment have the following advantages:

[0082] First, the waffle fleece warm knitted fabric described in the present application is interwoven with DTY differentiated polyester yarn and cotton yarn, so that one side has a strong visual sense and a sense of fashion, and its surface is rough with obvious square or diamond-shaped convex and concave feeling, and the other side has good tightness, is not easy to stretch and deform, and has a good warming effect.

[0083] Second, the preparation method of the waffle wool warm knitted fabric described in the present application breaks the conventional process, which is generally to directly grab the wool after dyeing, so that the density, thickness and hair loss of the wool cannot be well taken into account. The present application first performs an open-width water washing and shrinkage treatment on the fabric, so that the DTY differentiated polyester yarn is more uniform after open-width water washing, so that the gaps between the yarns are filled more fully, making the fabric more compact, with good warmth retention effect, and not easy to be stretched and deformed;

[0084] Third, the waffle wool warm knitted fabric described in this application has a better fabric feel and a better raised feel by adding a softener during dyeing and adding a softener in the shaping groove during reshaping;

[0085] Fourthly, the present invention washes the woven fabric flat and then plucks it, which not only makes it easier to raise the hair, but also makes the density and concentration of the plucked hair better. After the plucked hair, the blank is subjected to high-temperature shaping and dyeing treatment, and the floating hair will also be processed. After dyeing, the plucked surface is fluffed and the floating hair is repaired. The plucked hair obtained in this way is not only denser, but also thicker and fluffy as a whole, and the hair shedding of the plucked surface is excellent.

[0086] Although the present invention is disclosed as above, the present invention is not limited thereto. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the scope defined by the claims.

Claims

1. A waffle fleece warm knitted fabric, the fabric having a double-sided structure, characterized in that: One side is a flat structure, and the other side is a waffle structure, the flat surface is woven with a first DTY differentiated polyester yarn, the yarn count of the first DTY differentiated polyester yarn is 160-200D, the connecting wire between the waffle and the flat surface is woven with a second DTY differentiated polyester yarn, the yarn count of the second DTY differentiated polyester yarn is 60-100D; the waffle surface is woven with combed cotton yarn, the yarn count of the combed cotton yarn is in the range of 25-35S; the preparation method of the fabric includes: The process includes flat-width washing - flat-width shrinkage - first napping - pre-setting - dyeing; the fabric is woven into an upper and lower surface in the order of the upper needle disc to the lower needle cylinder, wherein the upper and lower needles of the first needle are both looped; the needles of the second, third and fourth needles are tucked and the lower needles are looped; the needles of the fifth and sixth needles are looped and the lower needles are tucked; the yarn woven in the first needle is the second DTY differentiated polyester yarn, the yarn woven in the second, third and fourth needles is the first DTY differentiated polyester yarn, and the yarn woven in the fifth and sixth needles is combed cotton yarn.

2. A method for preparing a fabric, characterized in that: The method is used to prepare the waffle fleece warm knitted fabric according to claim 1, and the method comprises: S1: Yarn count preparation; S2: fabric weaving; S3: fabric pretreatment; S4: Dyeing and finishing process.

3. The preparation method according to claim 2, characterized in that: Step S3 includes: S31: open width washing; S32: flat retraction; S33: First time pulling hair.

4. The preparation method according to claim 2, characterized in that: Step S4 includes: S41: Predetermined type; S42: Dyeing; S43: Second roughening; S44: Shearing treatment; S45: Re-setting.

5. The preparation method according to claim 3, characterized in that: Step S31, fabric open-width water washing, includes washing and shrinking the fabric woven in step S2 at an open width at a temperature of 60-90° C. for 20-30 minutes.

6. The preparation method according to claim 3, characterized in that: Step S33, the first napping includes: the fabric after the flat width is shrunk is put into the napping machine, and the flat surface is napped. The napping speed is 8-15m / min, the tension of the machine is 5-15N, and the napping is done in reverse, and the napping is done continuously for 1-3 times.