A coated glass tube and its preparation method and application
By applying a coating coating on soda-lime glass tubes, including zinc oxide and other components, the problems of poor acid and alkali resistance and high preparation cost are solved, and the acid resistance and alkali resistance are improved and cost reduction are achieved.
Patent Information
- Application Number
- CN202211105060.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-09
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2042-09-09
AI Technical Summary
The existing soda lime glass has poor acid and alkali resistance and high preparation cost of pharmaceutical glass, which limits its application in drug production.
The coating of glass tube is made of zinc oxide, silicon oxide, aluminum oxide, aluminum oxide, alkali metal oxide and alkaline earth metal oxide. The coating technology forms a spray angle of 20-50 degrees on the surface of the glass tube substrate to achieve coating coating. The uniform coverage and tight bonding of the layers reduce the preparation cost.
It improves the acid resistance and alkali resistance of coated glass tubes, complies with the Level 1 standard, and reduces the preparation cost, avoiding the high usage of boron trioxide in the glass tube matrix.
Smart Images

Figure CN116217090B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of preparation of medicinal glass tubes, and in particular to a coated glass tube and a preparation method and application thereof. Background Art
[0002] At present, pharmaceutical injection bottles and ampoules are all produced using pharmaceutical glass tubes. Therefore, the quality of pharmaceutical glass tubes has an important impact on medical effects. Pharmaceutical glass tubes are mainly divided into soda-lime glass and borosilicate glass. Borosilicate glass has a low thermal expansion coefficient, good water resistance and acid / alkali resistance, so it has gradually become the preferred material for pharmaceutical glass. However, due to the complex production technology and high production cost of borosilicate glass, it is difficult to promote, which has led to an increase in the production cost of drugs.
[0003] CN113860729A discloses a medium borosilicate pharmaceutical glass, the chemical composition of which includes: Al2O3 content of 2-4wt%; B2O3 content of 8-9wt%; Al2O3+B2O3 content of 11-12wt%; ZnO content of 2-4wt%; ZrO2 content of 1-2wt%; ZnO+ZrO2 content of 3-6wt%; Li2O+Na2O+K2O content of 6-8wt%, Li2O:Na2O:K2O=3:6:1; CaO+SrO content of 2-4wt%, CaO:SrO is (6-8):(2-4), and the rest is SiO2. Although the medium borosilicate pharmaceutical glass has the advantages of high chemical stability, low melting temperature, low B2O3 volatilization, and low thermal expansion coefficient. However, in production, the introduction of large amounts of boron trioxide will result in excessively high costs for preparing pharmaceutical glass.
[0004] However, soda-lime glass does not contain expensive borax pentahydrate (the source of boron trioxide), and its production cost is relatively low compared to borosilicate glass.
[0005] However, the alkali metal ions in soda-lime glass will react with H + An exchange reaction occurs, which destroys the Si-O-Si network structure in the glass, causing the soda-lime glass to be easily corroded and have a short lifespan.
[0006] Therefore, reducing the preparation cost of pharmaceutical glass and improving the water resistance and acid and alkali resistance of soda-lime glass materials are areas worthy of research at present, which will help promote the application of soda-lime glass and reduce the cost of the pharmaceutical production industry. Summary of the invention
[0007] The purpose of the present invention is to overcome the defects of the existing soda-lime glass, namely, poor acid and alkali resistance and high preparation cost of the pharmaceutical glass.
[0008] In order to achieve the above-mentioned object, a first aspect of the present invention provides a coated glass tube, the coated glass tube comprising a glass tube substrate and a coating provided on the surface of the glass tube substrate;
[0009] The coating contains the following components which are stored independently or in combination:
[0010] Based on 100 parts by weight of the total weight of the coating, the content of zinc oxide is 30-35 parts by weight, the content of silicon dioxide is 25-35 parts by weight, the content of boron trioxide is 17-20 parts by weight, the content of aluminum oxide is 2-3 parts by weight, the content of alkali metal oxide is 9-14 parts by weight, the content of alkaline earth metal oxide is 4.5-11 parts by weight, and the content of zirconium dioxide is 1-2 parts by weight;
[0011] The coating is sprayed on the surface of the glass tube substrate at a spraying angle of 20-50 degrees to the wall of the glass tube substrate.
[0012] Preferably, the content of zirconium dioxide is 1.5-2 parts by weight.
[0013] Preferably, the thickness of the coating is 10-30 μm.
[0014] Preferably, the alkali metal oxide is sodium oxide and / or potassium oxide.
[0015] Preferably, the alkaline earth metal oxide is at least one of calcium oxide, magnesium oxide and barium oxide.
[0016] Preferably, the glass tube substrate is a soda-lime glass tube.
[0017] Preferably, the coating is sprayed onto the surface of the glass tube substrate at a spraying angle of 30-45 degrees to the wall of the glass tube substrate.
[0018] A second aspect of the present invention provides a method for preparing the coated glass tube according to the first aspect, the method comprising the following steps:
[0019] (1) melting the components of the coating of the coated glass tube according to the first aspect to obtain a coating melt;
[0020] (2) clarifying, annealing, and grinding the coating melt in sequence to obtain a coating powder;
[0021] (3) spraying the coating powder onto the surface of a dried glass tube substrate to obtain a glass tube covered with the coating powder;
[0022] (4) Sintering the glass tube covered with the coating powder to obtain the coated glass tube.
[0023] Preferably, in step (1), the melting conditions at least meet the following conditions: temperature of 1100-1200° C. and time of 240-480 min.
[0024] Preferably, in step (2), the conditions of the clarification treatment at least meet the following requirements: temperature of 850-900° C. and time of 60-120 min.
[0025] Preferably, in step (2), the annealing treatment conditions at least meet the following conditions: the annealing temperature is 480-520° C., and the annealing time is not less than 30 min.
[0026] Preferably, in step (3), the spraying conditions at least meet the following conditions: the spraying speed is 50-100 g / min, and the thickness of the coating after spraying is 10-30 μm.
[0027] In step (4), the sintering conditions at least meet the following requirements: sintering temperature is 560-610° C., and sintering time is 20-40 min.
[0028] Preferably, in step (2), the average particle size of the coating powder is less than 50 μm, and the moisture content is less than 3 wt %.
[0029] Preferably, the method further comprises: before performing the step (3), firstly performing a cleaning treatment and a drying treatment on the glass tube substrate to be used in sequence, and then using the glass tube substrate after the drying treatment in the step (3) to perform the spraying;
[0030] The steps of the cleaning process include:
[0031] (A) performing a first washing on the glass tube substrate to be used with a 0.4-0.6 wt % alkaline solution under elution and / or ultrasonic immersion conditions to obtain an alkaline-washed glass tube substrate;
[0032] (B) performing a second washing on the alkali-washed glass tube with a 0.4-0.6 wt % acidic solution to obtain an acid-washed glass tube substrate;
[0033] (C) performing a third washing on the acid-washed glass tube substrate with water.
[0034] Preferably, in the first washing, the alkaline solution is a sodium hydroxide solution.
[0035] Preferably, in the second washing, the acidic solution is a hydrochloric acid solution.
[0036] Preferably, the first washing is performed under ultrasonic immersion conditions.
[0037] Preferably, the conditions for the ultrasonic immersion cleaning at least meet the following requirements: the ultrasonic frequency is 30-50 KHz, the temperature of the first washing is 40-50° C., and the immersion time is 30-60 s.
[0038] Preferably, the conditions in the second washing at least meet: the temperature of the second washing is 40-50° C., and the washing time is 80-100 s.
[0039] Preferably, in the third washing, the acid-washed glass tube substrate is first washed with deionized water for 80-100 seconds, and then washed with distilled water until the conductivity of the washing solution is less than 5.1 μs / cm.
[0040] The third aspect of the present invention provides the use of the coated glass tube described in the first aspect in the field of medicinal injection bottles and ampoules.
[0041] The coated glass tube prepared by the method provided by the present invention has excellent acid resistance and alkali resistance, wherein the acid resistance meets the requirements of level 1 and the alkali resistance meets the requirements of level 1. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1 It is a process flow chart for preparing coated glass tube;
[0043] Figure 2 It is a process flow chart of spraying coating. DETAILED DESCRIPTION
[0044] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0045] As mentioned above, the first aspect of the present invention provides a coated glass tube, the coated glass tube comprising a glass tube substrate and a coating provided on the surface of the glass tube substrate;
[0046] The coating contains the following components which are stored independently or in combination:
[0047] Based on 100 parts by weight of the total weight of the coating, the content of zinc oxide is 30-35 parts by weight, the content of silicon dioxide is 25-35 parts by weight, the content of boron trioxide is 17-20 parts by weight, the content of aluminum oxide is 2-3 parts by weight, the content of alkali metal oxide is 9-14 parts by weight, the content of alkaline earth metal oxide is 4.5-11 parts by weight, and the content of zirconium dioxide is 1-2 parts by weight;
[0048] The coating is sprayed on the surface of the glass tube substrate at a spraying angle of 20-50 degrees to the wall of the glass tube substrate.
[0049] It should be noted that the spraying angle is the acute angle formed by the straight line where the spray gun is located and the wall of the glass tube substrate.
[0050] Preferably, in the coating, based on the total weight of the coating being 100 parts by weight, the content of zinc oxide is 30-34 parts by weight, the content of silicon dioxide is 26-30 parts by weight, the content of boron trioxide is 17-19 parts by weight, the content of aluminum oxide is 2.5-3 parts by weight, the content of alkali metal oxide is 11-13 parts by weight, the content of alkaline earth metal oxide is 6.5-9 parts by weight, and the content of zirconium dioxide is 1.5-2 parts by weight. The inventors of the present invention have found that in this preferred case, the obtained coated glass tube has better acid resistance and alkali resistance.
[0051] In addition, the inventors found that the addition of zirconium dioxide can improve the alkali resistance of the coated glass tube, and when the content of zirconium dioxide is 1.5-2 parts by weight, the alkali resistance of the coated glass tube obtained by the scheme of the present invention can reach level 1, and glass crystallization will not occur.
[0052] Preferably, the thickness of the coating is 10-30 μm.
[0053] Preferably, the alkali metal oxide is sodium oxide and / or potassium oxide.
[0054] More preferably, the alkali metal oxides are sodium oxide and potassium oxide, and the content of the sodium oxide is 7-8 parts by weight, and the content of the potassium oxide is 4-5 parts by weight.
[0055] Preferably, the alkaline earth metal oxide is selected from at least one of calcium oxide, magnesium oxide and barium oxide.
[0056] More preferably, the alkaline earth metal oxides are calcium oxide, magnesium oxide and barium oxide, and the content of the calcium oxide is 2-3 parts by weight, the content of the magnesium oxide is 4-5 parts by weight, and the content of the barium oxide is 0.5-1 part by weight.
[0057] According to a preferred embodiment, the glass tube substrate is a soda-lime glass tube. More preferably, the glass tube substrate contains the following components: based on 100 parts by weight of the total weight of the glass tube substrate, the content of silicon dioxide is 65-75 parts by weight, the content of aluminum oxide is 0-5 parts by weight, the content of sodium oxide is 9-18 parts by weight, the content of potassium oxide is 0-5 parts by weight, the content of calcium oxide is 2-10 parts by weight, the content of magnesium oxide is 2-5 parts by weight, the content of lithium oxide is 0-2 parts by weight, and the content of zinc oxide is 0-2 parts by weight.
[0058] As mentioned above, the second aspect of the present invention provides a method for preparing the coated glass tube according to the first aspect, the method comprising the following steps:
[0059] (1) melting the components of the coating of the coated glass tube according to the first aspect to obtain a coating melt;
[0060] (2) clarifying, annealing, and grinding the coating melt in sequence to obtain a coating powder;
[0061] (3) spraying the coating powder onto the surface of a dried glass tube substrate to obtain a glass tube covered with the coating powder;
[0062] (4) Sintering the glass tube covered with the coating powder to obtain the coated glass tube.
[0063] According to a preferred embodiment, Figure 1 As shown, the method also includes: before performing the melt treatment in step (1), first mixing the components in the coating to be treated until the uniformity reaches more than 95%, and then drying to make the moisture content less than 3wt% to obtain a mixture, and then using the mixture for the melt treatment in step (1) to obtain a coating melt.
[0064] Furthermore, if Figure 1 As shown, the method also includes: drying the obtained coating powder after the spraying treatment in step (2); spraying the dried coating powder on the surface of the cleaned and dried glass tube substrate to obtain a glass tube covered with the coating powder; sintering and annealing the glass tube covered with the coating powder to obtain the coated glass tube.
[0065] According to a preferred embodiment, Figure 1 As shown, specifically including:
[0066] Preparing the coating: mixing, drying and melting the components of the coating to obtain a coating melt; clarifying and annealing the coating melt in sequence; and then grinding and drying to obtain a coating powder;
[0067] Preparing a glass tube matrix: mixing and melting the components of the glass tube matrix; clarifying and homogenizing the glass liquid I in sequence to obtain glass liquid II; drawing the glass liquid II into a shape, and annealing to obtain the glass tube matrix;
[0068] Preparation of coated glass tube: cleaning and drying the glass tube substrate; spraying the coating powder on the surface of the dried glass tube substrate, and obtaining a glass tube covered with coating powder after sintering and annealing.
[0069] It should be noted that there is no specific requirement for the uniformity test in the present invention, and it can be performed using means known in the art, such as using a conductivity test method.
[0070] The glass tube substrate of the present invention can be purchased or made by a method known in the art, and the present invention has no special requirements for this. Figure 1 A method for preparing a glass tube substrate is illustratively provided, such as Figure 1 As shown, the method includes:
[0071] S1: Mix and melt the components of the glass tube matrix:
[0072] The coating components including silicon dioxide, aluminum oxide, sodium oxide, potassium oxide, calcium oxide, magnesium oxide, lithium oxide and zinc oxide are mixed and melted at 1650-1700° C. for 240-480 min to obtain glass liquid I;
[0073] S2: Clarification and homogenization:
[0074] The glass liquid I is clarified and homogenized in sequence to obtain glass liquid II, wherein the clarification temperature is 1400-1600° C. and the time is 50-70 min;
[0075] S3: Drawing and annealing:
[0076] The glass liquid II is drawn into a shape by adopting the Dana process, and annealed at a temperature of 550-570° C. for at least 30 minutes to obtain the glass tube matrix.
[0077] According to a preferred embodiment, the method further comprises: before the melting treatment in step (1), mixing the components in the coating until the uniformity reaches more than 95%, and then drying to make the moisture content less than 3wt%.
[0078] The present invention has no special requirements on the specific operation method of the Dana process, and those skilled in the art can use known technical means to carry out the process.
[0079] Preferably, in step (1), the melting conditions at least meet the following conditions: temperature of 1100-1200° C. and time of 240-480 min.
[0080] Preferably, in step (2), the conditions of the clarification treatment at least meet the following requirements: temperature of 850-900° C. and time of 60-120 min.
[0081] Preferably, in step (2), the annealing treatment conditions at least meet the following conditions: the annealing temperature is 480-520° C., and the annealing time is not less than 30 min.
[0082] Preferably, in step (3), the spraying conditions at least meet the following conditions: the spraying speed is 50-100 g / min, and the thickness of the coating after spraying is 10-30 μm.
[0083] Preferably, in step (2), the coating melt is clarified, annealed, cooled to room temperature, and then ground.
[0084] According to a preferred embodiment, the method further comprises: in step (2), drying the ground coating powder to a moisture content of less than 3 wt %.
[0085] The present invention does not specifically limit the spraying method, and those skilled in the art can use known technical means to carry out the spraying. In order to make the obtained coating powder more closely bonded to the glass substrate, the present invention is combined with Figure 2 A preferred specific spraying method is provided.
[0086] like Figure 2 As shown, after the coating powder passes through the meter, the compressed gas is pressed into the electrostatic spray gun to spray the surface of the glass tube substrate to obtain the glass tube covered with the coating powder, wherein the pressure of the compressed gas is 0.02-0.025Mpa, and the head of the electrostatic spray gun is provided with a discharge needle or an annular metal discharge nozzle for generating high-voltage static electricity, and the distance between the nozzle of the electrostatic spray gun and the spraying center of the surface of the glass tube substrate is 12-15cm, and during the spraying process, the glass tube substrate is placed horizontally and rotated continuously at a rotation speed of 5-10r / min, so as to achieve uniform spraying.
[0087] Furthermore, if Figure 2 As shown, the method also includes: sintering and annealing the glass tube covered with the coating powder to obtain a coated glass tube.
[0088] According to a preferred embodiment, Figure 2 As shown, the method also includes: in the step (3), the coating powder residue generated during the spraying process is collected in time and discharged to the coating powder recovery device to continue to be used in the spraying of the glass tube substrate, thereby further reducing the preparation cost.
[0089] According to a preferred embodiment, Figure 2 As shown, the method further includes: after the coating powder passes through the meter, compressed gas is pressed into the electrostatic spray gun to spray the surface of the glass tube substrate to obtain the glass tube covered with the coating powder, and the glass tube covered with the coating powder is sintered and annealed to obtain the coated glass tube. It also includes timely collecting the coating powder residue generated during the spraying process and discharging it to the coating powder recovery device to continue to be used in the spraying of the glass tube substrate.
[0090] Preferably, in step (4), the sintering conditions at least meet the following conditions: the sintering temperature is 560-610° C., and the sintering time is 20-40 min.
[0091] According to a preferred embodiment, the method further comprises: before performing the sintering step in step (4), first raising the temperature from room temperature to the sintering temperature at a rate of 2-4°C / min, then performing sintering, and annealing to room temperature after sintering to obtain the coated glass tube.
[0092] In the present invention, unless otherwise specified, the room temperature is 25±5°C.
[0093] The present invention has no particular requirements on the specific method of annealing, and it can be performed using methods known in the art.
[0094] Preferably, in step (2), the average particle size of the coating powder is less than 50 μm, and the moisture content is less than 3 wt %.
[0095] Preferably, the method further comprises: before performing the step (3), firstly performing a cleaning treatment and a drying treatment on the glass tube substrate to be used in sequence, and then using the glass tube substrate after the drying treatment in the step (3) to perform the spraying;
[0096] The steps of the cleaning process include:
[0097] (A) performing a first washing on the glass tube substrate to be used with a 0.4-0.6 wt % alkaline solution under elution and / or ultrasonic immersion conditions to obtain an alkaline-washed glass tube substrate;
[0098] (B) performing a second washing on the alkali-washed glass tube with a 0.4-0.6 wt % acidic solution to obtain an acid-washed glass tube substrate;
[0099] (C) performing a third washing on the acid-washed glass tube substrate with water.
[0100] Preferably, in the first washing, the alkaline solution is a sodium hydroxide solution.
[0101] Preferably, in the second washing, the acidic solution is a hydrochloric acid solution.
[0102] Preferably, the first washing is performed under ultrasonic immersion conditions.
[0103] Preferably, the conditions for the ultrasonic immersion cleaning at least meet the following requirements: the ultrasonic frequency is 30-50 KHz, the temperature of the first washing is 40-50° C., and the immersion time is 30-60 s.
[0104] Preferably, the conditions in the second washing at least meet the following requirements: the temperature of the second washing is 40-50° C., and the washing time is 80-100 s.
[0105] The inventors have found that the control of the first washing and second washing temperatures in the present invention can improve the cleaning effect and is less likely to cause corrosion to the glass tube substrate wall.
[0106] Preferably, in the third washing, the water is deionized water and distilled water. More preferably, in the third washing, the acid-washed glass tube substrate is first washed with deionized water for 80-100 seconds, and then washed with distilled water until the conductivity of the washing solution is less than 5.1 μs / cm.
[0107] The inventors have found that the cleaning method provided by the present invention can make the coating layer and the glass tube substrate tightly bonded, thereby further improving the stability of the coated glass tube.
[0108] The third aspect of the present invention provides the use of the coated glass tube described in the first aspect in the field of medicinal injection bottles and ampoules.
[0109] The present invention is described in detail below by way of examples. Unless otherwise specified, the raw materials used are all common commercially available products.
[0110] The glass tube substrate meets the requirements of: YBB00282003-2015 Medicinal Soda-lime Glass Tube.
[0111] In the following examples, unless otherwise specified, each "part" or each "part by weight" means 100 g.
[0112] Electrostatic spraying equipment: Model KCI, purchased from Jining New Coordinate Machinery Equipment Co., Ltd.
[0113] Preparation of glass tube substrate:
[0114] Refer to the composition and addition amount of the glass tube matrix in Table 1.
[0115] S1: Mix and melt the components of the glass tube matrix:
[0116] The coating components including silicon dioxide, aluminum oxide, sodium oxide, potassium oxide, calcium oxide, magnesium oxide, lithium oxide and zinc oxide are mixed and melted at 1670° C. for 300 minutes to obtain glass liquid I;
[0117] S2: Clarification and homogenization:
[0118] The glass liquid I is clarified and homogenized in sequence to obtain glass liquid II, wherein the clarification temperature is 1500° C. and the time is 60 min;
[0119] S3: Drawing and annealing:
[0120] The glass liquid II is drawn into a shape by adopting the Dana process, and annealed at a temperature of 560° C. for 30 minutes to obtain the glass tube matrix.
[0121] Unless otherwise specified, the following examples use Figure 1 and Figure 2 The process flow shown in is carried out.
[0122] Preparation Example 1: Preparation of coated glass tube, numbered P1
[0123] This preparation example is used to illustrate that the coated glass tube described in the present invention is prepared according to the following method.
[0124] The components and addition amounts in the coating are shown in Table 2.
[0125] Preparation of coated glass tube:
[0126] (1) mixing and drying the components of the coating, and then introducing them into a kiln for melting to obtain a coating melt;
[0127] The components in the coating were mixed to a uniformity of 97%, dried to a moisture content of 2 wt%, and melted at a temperature of 1100°C for 240 min.
[0128] (2) clarifying, annealing, grinding and drying the coating melt in sequence to obtain the coating powder;
[0129] The clarification treatment was performed at a temperature of 900°C for 60 minutes; annealing was performed at a temperature of 480°C for 30 minutes, and cooling was performed to room temperature after annealing, and the coating powder was ground to an average particle size of 45 μm, and then dried to a moisture content of 2 wt%;
[0130] Before carrying out step (3), the glass tube substrate to be used is first cleaned and dried in sequence, and then the dried glass tube substrate is sprayed;
[0131] The cleaning process includes:
[0132] (A) Under ultrasonic immersion conditions, the glass tube substrate to be used is first washed with a 0.5wt% sodium hydroxide solution to obtain an alkali-washed glass tube substrate;
[0133] The ultrasonic immersion conditions are as follows: the ultrasonic frequency is 40 KHz, the temperature of the first washing is 45°C, and the immersion time is 30 seconds;
[0134] (B) performing a second washing on the alkali-washed glass tube using a 0.5 wt % hydrochloric acid solution to obtain an acid-washed glass tube substrate;
[0135] The temperature of the second washing is 40°C and the washing time is 90s;
[0136] (C) washing the acid-washed glass tube substrate for a third time with water;
[0137] The acid-washed glass tube substrate was first washed with deionized water for 90 seconds, and then washed with distilled water until the conductivity of the washing solution was 4.1 μs / cm;
[0138] (3) spraying the coating powder onto the surface of the dried glass tube substrate to obtain a glass tube covered with the coating powder;
[0139] Wherein, after the coating powder passes through the meter, it is pressed into the electrostatic spray gun by compressed gas to spray the surface of the glass tube substrate, the pressure of the compressed gas is 0.02Mpa, the spraying angle is 30 degrees, and the head of the electrostatic spray gun is provided with a discharge needle for generating high-voltage static electricity, the distance between the nozzle of the electrostatic spray gun and the spraying center of the surface of the glass tube substrate is 14cm, the spraying speed is 50g / min, the thickness of the coating after spraying is 20μm, and during spraying, the glass tube substrate is placed horizontally and rotated continuously at a rotation speed of 10r / min; during the spraying process, the excess coating powder residue is discharged to the coating powder recovery device and continued to be used in the spraying of the glass tube substrate;
[0140] (4) after raising the temperature from room temperature to the sintering temperature, the glass tube covered with the coating powder is sintered to obtain a coated glass tube;
[0141] Among them, the heating rate is 3°C / min, the sintering temperature is 565°C, and the sintering time is 30min.
[0142] Preparation Example 2: Preparation of coated glass tube, numbered P2
[0143] The coated glass tube was prepared according to the following method, wherein the components and addition amounts in the coating are shown in Table 2.
[0144] Preparation of coated glass tube:
[0145] (1) mixing and drying the components of the coating, and then introducing them into a kiln for melting to obtain a coating melt;
[0146] The components in the coating were mixed to a uniformity of 96%, dried to a moisture content of 2.5 wt%, and melted at a temperature of 1180°C for 300 min.
[0147] (2) clarifying, annealing, grinding and drying the coating melt in sequence to obtain the coating powder;
[0148] The clarification treatment was performed at a temperature of 880°C for 85 minutes; annealing was performed at a temperature of 480°C for 40 minutes, and cooling was performed to room temperature after annealing, and then the coating powder was ground to an average particle size of 40 μm, and then dried to a moisture content of 2.5 wt%;
[0149] Before carrying out step (3), the glass tube substrate to be used is first cleaned and dried in sequence, and then the dried glass tube substrate is sprayed;
[0150] The cleaning process includes:
[0151] (A) Under ultrasonic immersion conditions, the glass tube substrate to be used is first washed with a 0.5wt% sodium hydroxide solution to obtain an alkali-washed glass tube substrate;
[0152] The ultrasonic immersion conditions are as follows: the ultrasonic frequency is 30 KHz, the temperature of the first washing is 50° C., and the immersion time is 60 s;
[0153] (B) performing a second washing on the alkali-washed glass tube using a 0.5 wt % hydrochloric acid solution to obtain an acid-washed glass tube substrate;
[0154] The temperature of the second washing is 50°C and the washing time is 90s;
[0155] (C) washing the acid-washed glass tube substrate for a third time with water;
[0156] The acid-washed glass tube substrate was first washed with deionized water for 90 seconds, and then washed with distilled water until the conductivity of the washing solution was 4.6 μs / cm;
[0157] (3) spraying the coating powder onto the surface of the dried glass tube substrate to obtain a glass tube covered with the coating powder;
[0158] Wherein, after the coating powder passes through the meter, it is pressed into the electrostatic spray gun by compressed gas to spray the surface of the glass tube substrate, the pressure of the compressed gas is 0.025Mpa, the spraying angle is 45 degrees, and the head of the electrostatic spray gun is provided with a discharge needle for generating high-voltage static electricity, the distance between the nozzle of the electrostatic spray gun and the spraying center of the surface of the glass tube substrate is 12cm, the spraying speed is 80g / min, the thickness of the coating after spraying is 15μm, and during spraying, the glass tube substrate is placed horizontally and rotated continuously at a rotation speed of 7r / min; during the spraying process, the excess coating powder residue is discharged to the coating powder recovery device and continued to be used in the spraying of the glass tube substrate;
[0159] (4) after raising the temperature from room temperature to a sintering temperature, sintering the glass tube covered with the coating powder to obtain a coated glass tube;
[0160] Among them, the heating rate is 4°C / min, the sintering temperature is 300°C, and the sintering time is 25min.
[0161] Preparation Example 3: Preparation of coated glass tube, numbered P3
[0162] The coated glass tube was prepared according to the following method, wherein the amount of zirconium dioxide added to the coating was 1 part by weight, and the other components and addition amounts were shown in Table 2. The coating was sprayed on the surface of the glass tube substrate at a spraying angle of 30 degrees to the wall of the glass tube substrate.
[0163] Preparation of coated glass tube:
[0164] (1) mixing and drying the components of the coating, and then introducing them into a kiln for melting to obtain a coating melt;
[0165] The components in the coating are mixed to a uniformity of 98%, dried to a moisture content of 2 wt%, and melted at a temperature of 1180°C for 400 min.
[0166] (2) clarifying, annealing, grinding and drying the coating melt in sequence to obtain the coating powder;
[0167] The clarification treatment was performed at a temperature of 860°C for 100 minutes; annealing was performed at a temperature of 500°C for 60 minutes, and cooling was performed to room temperature after annealing, and the coating powder was ground to an average particle size of 45 μm, and then dried to a moisture content of 2.5 wt%;
[0168] Before carrying out step (3), the glass tube substrate to be used is first cleaned and dried in sequence, and then the dried glass tube substrate is sprayed;
[0169] The cleaning process includes:
[0170] (A) Under ultrasonic immersion conditions, the glass tube substrate to be used is first washed with a 0.6wt% sodium hydroxide solution to obtain an alkali-washed glass tube substrate;
[0171] The ultrasonic immersion conditions are as follows: the ultrasonic frequency is 30 KHz, the temperature of the first washing is 50° C., and the immersion time is 60 s;
[0172] (B) performing a second washing on the alkali-washed glass tube using a 0.4 wt % hydrochloric acid solution to obtain an acid-washed glass tube substrate;
[0173] The temperature of the second washing is 45°C and the washing time is 80s;
[0174] (C) washing the acid-washed glass tube substrate for a third time with water;
[0175] The acid-washed glass tube substrate was first washed with deionized water for 100 seconds, and then washed with distilled water until the conductivity of the washing solution was 4.6 μs / cm;
[0176] (3) spraying the coating powder onto the surface of the dried glass tube substrate to obtain a glass tube covered with the coating powder;
[0177] Wherein, after the coating powder passes through the meter, it is pressed into the electrostatic spray gun by compressed gas to spray the surface of the glass tube substrate, the pressure of the compressed gas is 0.025Mpa, the spraying angle is 30 degrees, and the head of the electrostatic spray gun is provided with a discharge needle for generating high-voltage static electricity, the distance between the nozzle of the electrostatic spray gun and the spraying center of the surface of the glass tube substrate is 12cm, the spraying speed is 80g / min, the thickness of the coating after spraying is 15μm, and during spraying, the glass tube substrate is placed horizontally and rotated continuously at a rotation speed of 7r / min; during the spraying process, the excess coating powder residue is discharged to the coating powder recovery device and continued to be used in the spraying of the glass tube substrate;
[0178] (4) after raising the temperature from room temperature to a sintering temperature, sintering the glass tube covered with the coating powder to obtain a coated glass tube;
[0179] Among them, the heating rate is 4°C / min, the sintering temperature is 300°C, and the sintering time is 25min.
[0180] Preparation Example 4: Preparation of coated glass tube, numbered P4
[0181] This preparation example was carried out in the same manner as in Preparation Example 1, except that the amount of zirconium dioxide added was 1 part by weight. See Table 2 for other components and amounts added.
[0182] A coated glass tube is obtained.
[0183] Preparation Example 5: Preparation of coated glass tube, numbered P5
[0184] This preparation example is carried out in the same manner as Preparation Example 2, except that the coating is sprayed on the surface of the glass tube substrate at a spraying angle of 25 degrees to the wall of the glass tube substrate. The composition and addition amount of the coating are shown in Table 2.
[0185] A coated glass tube is obtained.
[0186] Comparative Example 1
[0187] The same method as Preparation Example 1 was used, except that the components and addition amounts of the coating used to prepare the coated glass tube were different, wherein the addition amount of zirconium dioxide was 2.5 parts by weight. The rest was the same as Preparation Example 1, see Table 2 for details.
[0188] The coated glass tube was obtained and numbered DP1.
[0189] Comparative Example 2
[0190] The same method as Preparation Example 1 was used, except that the components and addition amounts of the coating used to prepare the coated glass tube were different, wherein the addition amount of zinc oxide was 20 parts by weight. The rest was the same as Preparation Example 1, see Table 2 for details.
[0191] The coated glass tube was obtained, numbered DP2.
[0192] Comparative Example 3
[0193] The same method as Preparation Example 1 was followed, except that the coating was sprayed on the surface of the glass tube substrate at a spraying angle of 55 degrees to the wall of the glass tube substrate.
[0194] The components and addition amounts of the coating for preparing the coated glass tube are shown in Table 2.
[0195] The coated glass tube was obtained, numbered DP3.
[0196] Comparative Example 4
[0197] The same method as Preparation Example 1 was used, except that the glass tube substrate was prepared according to the components and addition amounts of the glass tube substrate in Table 1, but the prepared glass tube substrate was not subsequently sprayed with a coating. The glass tube substrate was a soda-lime glass tube, numbered DP4.
[0198] Table 1
[0199] Glass tube matrix components Added amount, weight parts <![CDATA[SiO2]]> 70 <![CDATA[Al2O3]]> 5 <![CDATA[Na2O]]> 10 <![CDATA[K2O]]> 1 <![CDATA[Li2O]]> 3 MgO 3 CaO 7 ZnO 1
[0200] Table 2
[0201] Coating composition / weight Preparation Example 1 Preparation Example 2 Preparation Example 3 Preparation Example 4 Preparation Example 5 ZnO 31 34 35 Same as Preparation Example 2 Same as Preparation Example 1 <![CDATA[SiO2]]> 28 34 27 Same as Preparation Example 2 Same as Preparation Example 1 <![CDATA[B2O3]]> 17.5 20 18 Same as Preparation Example 2 Same as Preparation Example 1 <![CDATA[Al2O3]]> 2.7 2 2 Same as Preparation Example 2 Same as Preparation Example 1 <![CDATA[K2O]]> 5 13 4 Same as Preparation Example 2 Same as Preparation Example 1 <![CDATA[Na2O]]> 6 0 6 Same as Preparation Example 2 Same as Preparation Example 1 CaO 2 3 2 Same as Preparation Example 2 Same as Preparation Example 1 BaO 3 5 2 Same as Preparation Example 2 Same as Preparation Example 1 MgO 3 2 3 Same as Preparation Example 2 Same as Preparation Example 1 <![CDATA[ZrO2]]> 1.8 1.5 1 Same as Preparation Example 2 1 Spraying angle / ° 30 45 Same as Preparation Example 1 25 Same as Preparation Example 1
[0202] Table 2 continued
[0203]
[0204]
[0205] Test Example 1
[0206] In the following tests, the performance involved was tested using the following methods:
[0207] (1) Alkali resistance: tested with reference to "YBB00352004-2015 Determination of glass resistance to corrosion by boiling mixed alkali aqueous solution";
[0208] (2) Acid resistance: Tested according to "YBB00342004-2015 Determination of glass resistance to boiling hydrochloric acid erosion";
[0209] (3) Characteristic temperature points: Tm (melting temperature), Tg (softening temperature), Ts (transition point temperature) through differential scanning calorimetry (DSC);
[0210] (4) Measurement of CTE (coefficient of thermal expansion): The glass sample was cut and ground into a sample strip of 4 mm*4 mm*25.40 mm, and its coefficient of thermal expansion was measured. The coefficient of thermal expansion of the glass was determined by the differential method using a DIL2012STD dilatometer.
[0211] In this test example, the performance (characteristic temperature point, thermal expansion coefficient, alkali resistance, acid resistance) of the products prepared in the above preparation examples and comparative examples was tested. The results are shown in Table 3.
[0212] Table 3
[0213]
[0214] It can be seen from the above results that the comprehensive performance of the coated glass tube prepared by the method provided by the present invention is greatly improved compared with that of soda-lime glass, wherein the acid resistance meets level 1 and the alkali resistance meets level 1; and in the present invention, since the relatively expensive borax pentahydrate (the source of boron trioxide) is only added when preparing the coating and is not used in the glass tube matrix, the amount of boron trioxide used is very low, thereby reducing the preparation cost.
[0215] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A coated glass tube, characterized in that: The coated glass tube comprises a glass tube substrate and a coating layer arranged on the surface of the glass tube substrate; The coating material contains the following components which are stored separately or in combination: Based on 100 parts by weight of the total weight of the raw materials for the coating, the content of zinc oxide is 30-34 parts by weight, the content of silicon dioxide is 26-30 parts by weight, the content of boron trioxide is 17-19 parts by weight, the content of aluminum oxide is 2.5-3 parts by weight, the content of alkali metal oxide is 11-13 parts by weight, the content of alkaline earth metal oxide is 6.5-9 parts by weight, and the content of zirconium dioxide is 1.5-1.8 parts by weight; The coating is sprayed on the surface of the glass tube substrate at a spraying angle of 30-45 degrees to the wall of the glass tube substrate.
2. The coated glass tube according to claim 1, wherein: The thickness of the coating is 10-30 μm; and / or The alkali metal oxide is sodium oxide and / or potassium oxide; and / or The alkaline earth metal oxide is at least one of calcium oxide, magnesium oxide and barium oxide; and / or The glass tube substrate is a soda-lime glass tube.
3. A method for preparing the coated glass tube according to claim 1 or 2, characterized in that: The method comprises the following steps: (1) Melting the components of the raw material for the coating of the coated glass tube according to claim 1 or 2 to obtain a coating melt; (2) clarifying, annealing, and grinding the coating melt in sequence to obtain a coating powder; (3) spraying the coating powder onto the surface of a dried glass tube substrate to obtain a glass tube covered with the coating powder; (4) Sintering the glass tube covered with the coating powder to obtain the coated glass tube.
4. The method according to claim 3, wherein: In step (1), the melting conditions at least meet the following conditions: temperature of 1100-1200°C and time of 240-480 min; and / or In step (2), the conditions of the clarification treatment at least meet the following requirements: the temperature is 850-900°C and the time is 60-120 min; the conditions of the annealing treatment at least meet the following requirements: the annealing temperature is 480-520°C and the annealing time is not less than 30 min; and / or In step (3), the spraying conditions at least meet the following requirements: the spraying speed is 50-100 g / min, and the thickness of the coating after spraying is 10-30 μm; and / or In step (4), the sintering conditions at least meet the following requirements: sintering temperature is 560-610° C., and sintering time is 20-40 min.
5. The method according to claim 3 or 4, wherein: In step (2), the average particle size of the coating powder is less than 50 μm and the moisture content is less than 3 wt %.
6. The method according to claim 3 or 4, wherein: The method further comprises: before performing the step (3), firstly performing a cleaning treatment and a drying treatment on the glass tube substrate to be used in sequence, and then using the glass tube substrate after the drying treatment in the step (3) to perform the spraying; The steps of the cleaning process include: (A) performing a first washing on the glass tube substrate to be used with a 0.4-0.6 wt % alkaline solution under elution and / or ultrasonic immersion conditions to obtain an alkaline-washed glass tube substrate; (B) performing a second washing on the alkali-washed glass tube with a 0.4-0.6 wt % acidic solution to obtain an acid-washed glass tube substrate; (C) performing a third washing on the acid-washed glass tube substrate with water.
7. The method according to claim 6, wherein: In the first washing, the alkaline solution is a sodium hydroxide solution; and / or In the second washing, the acidic solution is a hydrochloric acid solution.
8. The method according to claim 6, wherein: The first washing is performed under ultrasonic immersion conditions; and / or The conditions for the ultrasonic immersion cleaning at least meet the following requirements: the ultrasonic frequency is 30-50 kHz, the temperature of the first washing is 40-50° C., and the immersion time is 30-60 s.
9. The method according to claim 6, wherein: The conditions in the second washing at least meet: the temperature of the second washing is 40-50° C., and the washing time is 80-100 s; and / or In the third washing, the acid-washed glass tube substrate is first washed with deionized water for 80-100 seconds, and then washed with distilled water until the conductivity of the washing solution is less than 5.1 μs / cm.
10. Use of the coated glass tube according to claim 1 or 2 in the field of medicinal injection bottles and ampoules.