An explosion-proof needle auxiliary agent and its preparation method and application

By using explosion-proof needle additives containing silicone oil, ester emulsifiers and water in PU synthetic leather, a stable water-in-oil dispersion system is formed, which solves the problem of 'explosive needle' and silicone oil precipitation, and improves the quality and qualification rate of the product .

CN116289237BActive Publication Date: 2024-11-15江西三越高新材料有限公司 +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310389148.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-12
Publication Date
2024-11-15
Estimated Expiration
2043-04-12

AI Technical Summary

Technical Problem

PU synthetic leather fabrics are prone to 'explosion' during sewing, resulting in a decline in product quality and low pass rate. Existing solutions such as adding dimethyl silicone oil will cause silicone oil to appear on the surface, affecting quality.

Method used

Provide an explosion-proof needle auxiliary, containing silicone oil, ester emulsifier and water, and forms a stable water-in-oil dispersion system through the esterification reaction, which is added to the PU dry mother liquor to disperse evenly to prevent the needle from bringing out of the wet PU layer. substance.

Benefits of technology

It effectively solves the problem of 'explosive needle', and avoids the precipitation of silicone oil, improves the aesthetics and pass rate of the product, and ensures the quality of the synthetic leather.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to the technical field of PU synthetic leather, and provides an anti-explosion needle auxiliary agent, and a preparation method and application thereof. The present invention provides an anti-explosion needle auxiliary agent, comprising the following components in mass percentage: 45-70% silicone oil; 15-40% ester emulsifier; 15-30% water; the ester emulsifier is obtained by esterification reaction of carboxyl-modified silicone oil and long-chain alkyl alcohol polyoxyethylene ether. The present invention forms a stable oil-in-water dispersion system by controlling the type of ester emulsifier and strictly controlling the content of each material. The present invention applies the anti-explosion needle auxiliary agent to the PU slurry, which can be evenly dispersed, and solves the problem of "needle explosion" while overcoming the problem of silicone oil precipitation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of PU synthetic leather, and in particular to an explosion-proof needle auxiliary agent and a preparation method and application thereof. Background Art

[0002] PU synthetic leather fabrics are generally composed of non-woven fabrics, wet PU layers and dry PU layers from bottom to top. During the sewing process of PU synthetic leather fabrics, the sewing needle is easily pulled out of the wet PU layer (commonly known as the "burst needle" phenomenon in the industry). The pulled-out substances remain at the needle hole, affecting the appearance and quality of the sewn products, resulting in low product qualification rate and waste.

[0003] At present, some researchers have added a small amount of dimethyl silicone oil to the synthetic leather dry process mother liquor to solve the "needle burst" problem. However, dimethyl silicone oil has poor compatibility with PU resin, which will cause silicone oil bright spots to appear on the surface of the synthetic leather product, seriously affecting the product quality. Summary of the invention

[0004] In view of the above problems, the purpose of the present invention is to provide an explosion-proof needle auxiliary agent and a preparation method and application thereof. The explosion-proof needle auxiliary agent provided by the present invention is added to the PU dry process mother liquor and can be evenly dispersed, thereby solving the "explosion needle" problem while overcoming the problem of silicone oil precipitation.

[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0006] The present invention provides an explosion-proof needle auxiliary agent, comprising the following components in percentage by mass:

[0007] Silicone oil 45-70%;

[0008] Ester emulsifier 15-40%;

[0009] Water 15-30%;

[0010] The ester emulsifier is obtained by esterification reaction of carboxyl-modified silicone oil and long-chain alkyl alcohol polyoxyethylene ether.

[0011] Preferably, the silicone oil includes one or more of dimethyl silicone oil, hydroxy silicone oil and amino silicone oil;

[0012] The viscosity of the dimethyl silicone oil is 50000-2000000cps;

[0013] The viscosity of the hydroxy silicone oil is 20000-2000000cps;

[0014] The viscosity of the amino silicone oil is 1000-100000 cps, and the ammonia value is 0.2-0.6.

[0015] Preferably, when the silicone oil includes dimethyl silicone oil, hydroxy silicone oil and amino silicone oil, the mass ratio of the dimethyl silicone oil, hydroxy silicone oil and amino silicone oil is 10-60:10-60:1-20.

[0016] Preferably, when the silicone oil includes dimethyl silicone oil and hydroxy silicone oil, the mass ratio of the dimethyl silicone oil to the hydroxy silicone oil is 10-60:10-60.

[0017] Preferably, the long-chain alkyl alcohol polyoxyethylene ether has 10 to 15 carbon atoms.

[0018] Preferably, the molar ratio of the carboxyl-modified silicone oil to the long-chain alkyl alcohol polyoxyethylene ether is 1:2.1-2.3.

[0019] Preferably, the esterification reaction temperature is 130-150°C and the time is 2-4h;

[0020] The esterification reaction is carried out under vacuum conditions; the vacuum degree of the vacuum conditions is ≥0.093MPa.

[0021] The present invention also provides a method for preparing the explosion-proof needle auxiliary agent described in the above technical solution, comprising the following steps:

[0022] Silicone oil, ester emulsifier and water are mixed to obtain explosion-proof needle auxiliary agent.

[0023] Preferably, the mixing equipment is a kneader.

[0024] The present invention also provides the use of the explosion-proof needle auxiliary agent described in the above technical solution or the explosion-proof needle auxiliary agent prepared by the preparation method described in the above technical solution in dry-process PU synthetic leather.

[0025] The present invention provides an explosion-proof needle auxiliary agent, comprising the following components in mass percentage: 45-70% silicone oil; 15-40% ester emulsifier; 15-30% water; the ester emulsifier is obtained by esterification reaction of carboxyl-modified silicone oil and long-chain alkyl alcohol polyoxyethylene ether. The present invention forms a stable oil-in-water dispersion system by controlling the type of ester emulsifier and strictly controlling the content of each material.

[0026] The present invention also provides an application of an explosion-proof needle auxiliary agent in a PU synthetic leather dry process. The present invention utilizes a stable oil-in-water dispersion system and a PU dry process mother liquor to form a homogeneous system. During the sewing process of the prepared PU synthetic leather fabric, the explosion-proof needle auxiliary agent can lubricate the sewing needle. After the sewing needle enters the wet process PU layer and is pulled out, it is not easy to bring out the substances in the wet process PU layer, so that the sewn product is beautiful. While solving the "bursting needle" problem, it overcomes the problem of silicone oil precipitation, and ultimately improves the qualified rate of the product. DETAILED DESCRIPTION

[0027] The present invention provides an explosion-proof needle auxiliary agent, comprising the following components in percentage by mass:

[0028] Silicone oil 45-70%;

[0029] Ester emulsifier 15-40%;

[0030] Water 15-30%;

[0031] The ester emulsifier is obtained by esterification reaction of carboxyl-modified silicone oil and long-chain alkyl alcohol polyoxyethylene ether.

[0032] In the present invention, unless otherwise specified, the components are all commercially available products well known to those skilled in the art.

[0033] In the present invention, the explosion-proof needle auxiliary agent includes silicone oil with a mass fraction of 45-70%, preferably 55-65%. In the present invention, the silicone oil preferably includes one or more of dimethyl silicone oil, hydroxy silicone oil and amino silicone oil; the viscosity of the dimethyl silicone oil is preferably 50000-2000000cps, more preferably 500000-1000000cps; the viscosity of the hydroxy silicone oil is preferably 20000-2000000cps, more preferably 1000000-2000000cps; the viscosity of the amino silicone oil is preferably 1000-100000cps, more preferably 1000-50000cps, and the ammonia value is preferably 0.2-0.6.

[0034] In the present invention, when the silicone oil preferably includes dimethyl silicone oil, hydroxy silicone oil and amino silicone oil, the mass ratio of the dimethyl silicone oil, hydroxy silicone oil and amino silicone oil is preferably 10-60:10-60:1-20. In the present invention, when the silicone oil preferably includes dimethyl silicone oil and hydroxy silicone oil, the mass ratio of the dimethyl silicone oil to the hydroxy silicone oil is preferably 10-60:10-60.

[0035] In the present invention, the explosion-proof needle auxiliary agent includes 15-40% by mass of an ester emulsifier, preferably 20-30% by mass, and the ester emulsifier is obtained by esterification reaction of carboxyl-modified silicone oil and long-chain alkyl alcohol polyoxyethylene ether.

[0036] In the present invention, the carbon number of the long-chain alkyl alcohol polyoxyethylene ether is preferably 10-15, more preferably 12-15; the long-chain alkyl alcohol polyoxyethylene ether preferably includes one or both of linear alkyl alcohol polyoxyethylene ether and branched alkyl alcohol polyoxyethylene ether.

[0037] In the present invention, the linear alkyl alcohol polyoxyethylene ether preferably includes AEO series products, and the AEO series products are preferably from BASF AG, Shell Group, and Sanjiang Chemical Co., Ltd. In a specific embodiment of the present invention, the linear alkyl alcohol polyoxyethylene ether is preferably BASF AEO-7.

[0038] In the present invention, the branched alkyl alcohol polyoxyethylene ether preferably includes isomeric tridecanol polyoxyethylene ether or secondary alcohol polyoxyethylene ether; the isomeric tridecanol polyoxyethylene ether is preferably from BASF AG or Sasol Chemical Co., Ltd.; the secondary alcohol polyoxyethylene ether is preferably from Dow Chemical Co., Ltd. In a specific embodiment of the present invention, the isomeric tridecanol polyoxyethylene ether is specifically Sasol 1380 isomeric tridecanol polyoxyethylene ether; the secondary alcohol polyoxyethylene ether is specifically Dow 15-S-9 secondary alcohol polyoxyethylene ether.

[0039] In the present invention, the carboxyl-modified silicone oil is preferably carboxyl-modified silicone oil X-22-162C produced by Shin-Etsu Chemical Co., Ltd.

[0040] In the present invention, the molar ratio of the carboxyl-modified silicone oil to the long-chain alkyl alcohol polyoxyethylene ether is preferably 1:2.1-2.3, and more preferably 1:2.1-2.2.

[0041] In the present invention, the temperature of the esterification reaction is preferably 130-150°C, more preferably 135-145°C, and the time is preferably 2-4h, more preferably 2-3h. In the present invention, the esterification reaction is preferably carried out under vacuum conditions; the vacuum degree of the vacuum conditions is preferably ≥0.093MPa, more preferably ≥0.095MPa. In the present invention, the esterification reaction is preferably carried out under catalyst conditions, and the catalyst is preferably p-toluenesulfonic acid; the amount of the catalyst is preferably 0.2-0.5% of the total mass of the reactants, more preferably 0.3-0.5%.

[0042] In the present invention, the explosion-proof needle auxiliary agent includes water with a mass fraction of 15 to 30%, preferably 15 to 25%; the water is preferably deionized water.

[0043] The present invention also provides a method for preparing the explosion-proof needle auxiliary agent described in the above technical solution, comprising the following steps:

[0044] Silicone oil, ester emulsifier and water are mixed to obtain explosion-proof needle auxiliary agent.

[0045] In the present invention, the mixing is preferably:

[0046] The silicone oil and the ester emulsifier are first kneaded for 1 to 2 hours, and then water is added dropwise while kneading. After the addition is completed, the kneading is continued for 0.5 to 1.5 hours.

[0047] In the present invention, the water is preferably added dropwise for 2.5 to 3 hours.

[0048] In the present invention, the kneading equipment is preferably a kneader; the rotation speed of the kneader is preferably 35 to 45 rpm.

[0049] The present invention also provides the use of the explosion-proof needle auxiliary agent described in the above technical solution or the explosion-proof needle auxiliary agent prepared by the preparation method described in the above solution in dry PU synthetic leather. The present invention has no special requirements for the specific implementation of the application, and it can be carried out in a manner commonly used by those skilled in the art.

[0050] In a specific embodiment of the present invention, the application method preferably includes the following steps:

[0051] Mix 100 parts of PU dry resin (30% solid content), 100 parts of dimethylformamide, 5 parts of black flakes, 0.3 parts of wetting and leveling agent and 0.8 parts of explosion-proof needle additive to obtain PU dry mother liquor;

[0052] The PU dry process mother liquid is coated on release paper by knife coating, and then transferred to the wet process synthetic leather BASE to obtain dry process PU synthetic leather.

[0053] The present invention has no special limitation on the model of the black flakes and the type of the wetting and leveling agent, and those known to those skilled in the art may be used.

[0054] The present invention has no particular limitation on the process of scraping and transferring, and the process may be carried out using a process well known to those skilled in the art.

[0055] In order to further illustrate the present invention, an explosion-proof needle auxiliary agent provided by the present invention, a preparation method thereof and an application thereof are described in detail below in conjunction with examples, but they should not be construed as limiting the scope of protection of the present invention.

[0056] The kneading machine model used in the embodiment of the present invention is LGNH1000L.

[0057] Example 1

[0058] Preparation of ester emulsifier:

[0059] Carboxyl-modified silicone oil (carboxyl-modified silicone oil X-22-162C produced by Shin-Etsu Chemical Co., Ltd. of Japan), BASF AEO-7 long-chain alkyl alcohol polyoxyethylene ether and p-toluenesulfonic acid (the amount used is 0.3% of the total amount of raw materials) are mixed, and an esterification reaction is carried out at 135°C, the vacuum degree is not less than 0.093MPa, and the reaction time is 3h to obtain an ester emulsifier.

[0060] The molar ratio of carboxyl-modified silicone oil to BASF AEO-7 long-chain alkyl alcohol polyoxyethylene ether is 1:2.2.

[0061] Preparation of explosion-proof needle additives:

[0062] Add 200g of ester emulsifier into the kneader, and then add 250g of dimethyl silicone oil, 250g of hydroxy silicone oil and 100g of amino silicone oil, turn on the power of the kneader, the speed is 40 rpm, knead for 2h, then add 200g of deionized water while kneading, the addition is completed after 3h, and continue kneading for 1h to obtain an explosion-proof needle auxiliary agent, wherein the viscosity of the dimethyl silicone oil is 1000000cps; the viscosity of the hydroxy silicone oil is 2000000cps; the viscosity of the amino silicone oil is 5000cps, and the ammonia value is 0.4.

[0063] Example 2

[0064] Preparation of ester emulsifier:

[0065] Carboxyl modified silicone oil (carboxyl modified silicone oil X-22-162C produced by Shin-Etsu Chemical Co., Ltd. of Japan), Sasol 1380 isomeric tridecanol polyoxyethylene ether and p-toluenesulfonic acid (the amount used is 0.4% of the total amount of raw materials) are mixed, and an esterification reaction is carried out at 140° C., the vacuum degree is not less than 0.093 MPa, and the reaction time is 3 hours to obtain an ester emulsifier;

[0066] The molar ratio of carboxyl modified silicone oil to Sasol 1380 isotridecyl alcohol polyoxyethylene ether is 1:2.15.

[0067] Preparation of explosion-proof needle additives:

[0068] Add 150g of ester emulsifier to the kneader, then add 100g of dimethyl silicone oil and 600g of hydroxy silicone oil, turn on the kneader power, rotate at 40 rpm, knead for 2h, then slowly add 150g of deionized water while kneading, and complete the addition within 2.5h. After adding the deionized water, continue kneading for 1h to obtain an explosion-proof needle auxiliary agent, wherein the viscosity of the dimethyl silicone oil is 500000cps; the viscosity of the hydroxy silicone oil is 1500000cps.

[0069] Example 3

[0070] Preparation of ester emulsifier:

[0071] Carboxyl modified silicone oil (carboxyl modified silicone oil X-22-162C of Shin-Etsu Chemical Co., Ltd. of Japan), Dow 15-S-9 secondary alcohol polyoxyethylene ether and p-toluenesulfonic acid (the amount used is 0.5% of the total amount of raw materials) are mixed, and an esterification reaction is carried out at 145° C., the vacuum degree is not less than 0.095 MPa, and the reaction time is 3 hours to obtain an ester emulsifier;

[0072] The molar ratio of carboxyl-modified silicone oil to Dow 15-S-9 secondary alcohol polyoxyethylene ether is 1:2.1.

[0073] Preparation of explosion-proof needle additives:

[0074] Add 400g of ester emulsifier into a kneader, and then add 100g of dimethyl silicone oil, 100g of hydroxy silicone oil and 100g of amino silicone oil, turn on the kneader power, rotate at 40 rpm, knead for 2h, then slowly add 300g of deionized water while kneading, and add it within 3h. After adding the deionized water, continue kneading for 1h to obtain an explosion-proof needle auxiliary agent, wherein the viscosity of the dimethyl silicone oil is 300000cps; the viscosity of the hydroxy silicone oil is 1000000cps; the viscosity of the amino silicone oil is 50000cps, and the ammonia value is 0.2.

[0075] Application Example 1

[0076] 100 parts of PU dry process resin (30% solid content), 100 parts of dimethylformamide, 5 parts of black flakes, 0.3 parts of wetting and leveling agent and 0.8 parts of explosion-proof needle auxiliary agent obtained in Example 1 were mixed to obtain PU dry process mother liquid;

[0077] The PU dry process mother liquid is scraped onto release paper and then transferred onto a wet process synthetic leather BASE to obtain a dry process PU synthetic leather.

[0078] Application Example 2

[0079] Dry process PU synthetic leather was prepared according to the preparation method of Application Example 1, except that:

[0080] The explosion-proof needle auxiliary agent prepared in Example 1 was used to replace the explosion-proof needle auxiliary agent prepared in Example 2.

[0081] Application Example 3

[0082] Dry process PU synthetic leather was prepared according to the preparation method of Application Example 1, except that:

[0083] The explosion-proof needle auxiliary agent prepared in Example 1 was used to replace the explosion-proof needle auxiliary agent prepared in Example 3.

[0084] Comparative Example 1

[0085] Dry process PU synthetic leather was prepared according to the preparation method of Application Example 1, except that:

[0086] The explosion-proof needle auxiliary agent prepared in Example 1 was replaced with dimethyl silicone oil.

[0087] Comparative Example 2

[0088] Dry process PU synthetic leather was prepared according to the preparation method of Application Example 1, except that:

[0089] No explosion-proof needle additives are added.

[0090] Performance Testing

[0091] The surfaces of the synthetic leathers prepared in Application Examples 1 to 3 and Comparative Examples 1 to 2 were observed to see whether silicone oil was precipitated, and the synthetic leathers were subjected to a sewing test. Each synthetic leather was sewn with 1,000 stitches, and the number of pinholes resulting in needle burst was counted. The synthetic leather samples are shown in Table 1 below:

[0092] Table 1 Performance test results of synthetic leather in Application Examples 1 to 3 and Comparative Examples 1 to 2

[0093] Synthetic leather sample Application Example 1 Application Example 2 Application Example 3 Comparative Example 1 Comparative Example 2 Is there any silicone oil precipitation on the surface? none none none have none Number of pinholes causing pin bursting 0 1 2 2 67

[0094] It can be seen from Table 1 that the synthetic leather prepared in Comparative Example 2 has a needle burst ratio of 6.7%; the dry-process PU synthetic leather prepared in Application Examples 1 to 3 has no silicone oil precipitation on the surface and has an excellent anti-needle burst effect; the dry-process PU synthetic leather prepared in Comparative Example 1 has an excellent anti-needle burst effect, but silicone oil is precipitated on the surface of the synthetic leather, which seriously affects the quality of the synthetic leather.

[0095] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be regarded as the protection scope of the present invention.

Claims

1. An explosion-proof needle auxiliary agent, characterized in that: Specifically, the components are as follows: Silicone oil 45-70%; ester emulsifier 15-40%; water 15-30%; The ester emulsifier is obtained by esterification reaction of carboxyl modified silicone oil and long chain alkyl alcohol polyoxyethylene ether; The carbon number of the long-chain alkyl alcohol polyoxyethylene ether is 12 to 15; The long-chain alkyl alcohol polyoxyethylene ether includes one or two of a straight-chain alkyl alcohol polyoxyethylene ether and a branched-chain alkyl alcohol polyoxyethylene ether; The silicone oil is a mixture of dimethyl silicone oil, hydroxy silicone oil and amino silicone oil, or a mixture of dimethyl silicone oil and hydroxy silicone oil; The viscosity of the dimethyl silicone oil is 50000-2000000cps; The viscosity of the hydroxy silicone oil is 20000-2000000cps; The viscosity of the amino silicone oil is 1000-100000 cps, and the ammonia value is 0.2-0.6; When the silicone oil is a mixture of dimethyl silicone oil, hydroxy silicone oil and amino silicone oil, the mass ratio of the dimethyl silicone oil, hydroxy silicone oil and amino silicone oil is 10-60:10-60:1-20; When the silicone oil is a mixture of dimethyl silicone oil and hydroxy silicone oil, the mass ratio of the dimethyl silicone oil to the hydroxy silicone oil is 10-60:10-60.

2. The explosion-proof needle auxiliary agent according to claim 1, characterized in that: The molar ratio of the carboxyl modified silicone oil to the long-chain alkyl alcohol polyoxyethylene ether is 1:2.1-2.

3.

3. The explosion-proof needle auxiliary agent according to claim 1, characterized in that: The esterification reaction temperature is 130-150°C and the time is 2-4h; The esterification reaction is carried out under vacuum conditions; the vacuum degree of the vacuum conditions is ≥0.093MPa.

4. The method for preparing the explosion-proof needle auxiliary agent according to any one of claims 1 to 3, characterized in that: The following steps are involved: Silicone oil, ester emulsifier and water are mixed to obtain explosion-proof needle auxiliary agent.

5. The preparation method according to claim 4, characterized in that: The mixing equipment is a kneader.

6. Use of the explosion-proof needle auxiliary agent according to any one of claims 1 to 3 or the explosion-proof needle auxiliary agent prepared by the preparation method according to any one of claims 4 to 5 in dry-process PU synthetic leather.