A defect-rich cluster monolayer MoS2, preparation method and application thereof
By forming a single layer of MoS2 rich in defect clusters by the preparation method in a dual-temperature zone tube furnace, the technical challenges of defect cluster preparation and property regulation in 2D TMDs are solved, and the effective 3FeMo-VS is achieved in the single layer of MoS2. Defect clusters provide new regulatory ideas and improve the electrical performance of electronic devices.
Patent Information
- Application Number
- CN202310291797.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-23
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-03-23
AI Technical Summary
In 2D transition metal chalcogenides (TMDs), especially monolayer MoS2, how to effectively prepare and regulate the formation and properties of defect clusters has not been fully studied, and the prior art is mainly limited to the study of isolated single doping defects.
A preparation method is adopted to use a mixture of iron salt and molybdenum compound and halogen salt as a precursor, and a high-temperature reaction is carried out in a dual-temperature tube furnace. By controlling the temperature and gas flow, a single layer of MoS2 rich in defect clusters is formed. The specific steps include mixing the precursor and sulfur source in the container, passing the inert gas into the furnace tube, and reacting separately in the high and low temperature zones until the reaction is completed and dropped to room temperature.
The 3FeMo-VS defective cluster formed by sub-doped Fe atoms and sulfur vacancy was realized in single-layer MoS2, breaking through the technical bottleneck of the preparation of defective clusters, providing new ideas to regulate the properties of 2D TMDs, and showing that The 3FeMo-VS defective cluster provides hole doping on monolayer MoS2, eliminating the Schottky contact barrier between metal-semiconductors.
Smart Images

Figure CN116354396B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electrical material preparation, and in particular to a defect cluster-rich single-layer MoS2, a preparation method and application thereof. Background Art
[0002] Two-Dimensional Transition Metal Dichalcogenides (2D TMDs), represented by MoS2, have attracted extensive attention in the research of advanced electronic devices in the post-Moore era due to their ultra-thin layered structure and a variety of novel and unique properties. Using defects to regulate the properties of 2D TMDs is an important part of this research field. Substitutional doping is currently a major means of regulating the properties of 2D TMDs (especially monolayer MoS2), but most studies are limited to studying the effects of isolated single doping defects on 2D TMDs. Defect clusters refer to a type of defect form formed by the interaction between adjacent identical or different defects in a material, which has an important influence on the properties of traditional bulk semiconductors (such as ZnO) and ionic conductors (such as CeO2). However, how to effectively prepare defect clusters in 2D TMDs and how defect clusters affect the properties of 2D TMDs have not been fully studied.
[0003] In view of the above-mentioned defects, the inventors of the present invention finally obtained the present invention after a long period of research and practice. Summary of the invention
[0004] The purpose of the present invention is to solve the problem of how to effectively prepare defect clusters formed by substitutional doping-vacancies in 2D TMDs, and provide a single-layer MoS2 rich in defect clusters, a preparation method and its application.
[0005] In order to achieve the above object, the present invention discloses a method for preparing a defect-rich cluster monolayer MoS2, comprising the following steps:
[0006] S1, placing an iron salt, a mixture of a molybdenum-containing compound and a halogen salt, or a mixture of iron molybdate and a halogen salt as a precursor in a container;
[0007] S2, placing a clean growth substrate directly above the container holding the precursor;
[0008] S3, placing a solid sulfur source in another container or using a gaseous sulfur source to sulfurize the precursor;
[0009] S4, place the two containers containing the precursor and the sulfur source in the high temperature zone and the low temperature zone of the double temperature zone tubular furnace respectively, pass the inert gas into the furnace tube, exhaust the air, then reduce the inert gas flow rate and increase the temperature of the high temperature zone, and start heating the low temperature zone when the temperature of the high temperature zone rises to the predetermined temperature. When the high temperature zone rises to the growth temperature, the low temperature zone can just rise to the temperature of the solid sulfur source vaporization, so that the high temperature zone and the low temperature zone react separately. After the reaction is completed, the reaction system is cooled to room temperature to complete the growth of the defect cluster monolayer MoS2.
[0010] In step S1, the iron salt is iron chloride or iron sulfide, and the molybdenum-containing compound is any one of molybdenum powder, molybdenum oxide, molybdenum-containing halide, molybdenum-containing sulfate, molybdenum-containing ammonium salt and molybdenum-containing organic salt.
[0011] The halogen salt in step S1 is any one of all halogen salts formed by fluorine, chlorine, bromine, iodine and lithium, sodium, potassium, and cesium.
[0012] In the step S1, the mass ratio of iron molybdate to halogen salt is 1:1-1:9, and the mass of the precursor is 1-5 mg.
[0013] The growth substrate in step S2 is a SiO2 / Si substrate, a sapphire substrate, a mica substrate or any other material that can be used as a growth substrate, and the container is a ceramic boat, a quartz boat or any other sulfur corrosion-resistant and high-temperature-resistant container.
[0014] The solid sulfur source in step S3 is any one of solid sublimated sulfur powder, sulfur-containing inorganic matter and sulfur-containing organic matter, and the gaseous sulfur source is H2S gas or gaseous CS2.
[0015] The inert gas in step S4 is nitrogen, argon or a mixture of nitrogen and argon.
[0016] In step S4, the predetermined temperature is 350-520° C., the growth temperature is 550-720° C., the heating rates of the high temperature zone and the low temperature zone are 10-25° C. / min, and the high temperature zone is maintained for 5-20 minutes after reaching the growth temperature.
[0017] The present invention also discloses a defect-rich cluster single-layer MoS2 prepared by the above-mentioned preparation method and the application of the defect-rich cluster single-layer MoS2 in electronic devices.
[0018] Compared with the prior art, the present invention has the following beneficial effects: the present invention prepares a single-layer MoS2 film composed of substitutionally doped Fe atoms (Fe Mo ) and sulfur vacancies (V S ) formed by 3Fe Mo -V SThe new defect cluster technology breaks through the technical bottleneck of preparing defect clusters in 2D TMDs and provides a new idea for using defect clusters to control the properties of 2D TMDs. Mo -V S Electrical measurements of defective cluster monolayer MoS2 show that 3Fe Mo -V S The defect clusters provide hole doping (P-type doping) for the monolayer MoS2, which is different from the common isolated Fe Mo The situation of electron doping (N-type doping) in the monolayer MoS2 sample is completely different. Mo -V S The presence of defect clusters enables the single-layer Fe-doped MoS2 sample to form a good ohmic contact with the metal electrode, eliminating the Schottky contact barrier between metal and semiconductor. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 To prepare 3Fe-rich Mo -V S Schematic diagram of the experimental setup for defect cluster monolayer Fe-doped MoS2;
[0020] Figure 2 Rich in 3Fe Mo -V S X-ray Photoelectron Spectroscopy (XPS), Raman spectroscopy and photoluminescence spectroscopy test results of defect cluster monolayer Fe-doped MoS2 and undoped MoS2. (a) 3Fe-rich Mo -V S XPS spectrum of defect cluster monolayer Fe-doped MoS2, (b) 3Fe-rich Mo -V S XPS fine scanning spectrum of Fe element in defect cluster monolayer Fe-doped MoS2, (c) rich in 3Fe Mo -V S Raman spectra of defect cluster monolayer Fe-doped MoS2 and undoped monolayer MoS2, (d) 3Fe-rich Mo -V S Photoluminescence spectra of defect cluster monolayer Fe-doped MoS2 and undoped monolayer MoS2;
[0021] Figure 3 Rich in 3Fe Mo -V S Two types of defects in Fe-doped MoS2 monolayer (isolated Fe Mo Doping defects and 3Fe Mo -V SSpherical aberration-corrected transmission electron micrographs comparing the atomic arrangement of defect clusters and undoped monolayer MoS2. (a) The arrangement of Mo and S atoms without defects in undoped monolayer MoS2. (b) The isolated Fe in Fe-doped monolayer MoS2. Mo Substitutional doping defects, (c) 3Fe in Fe-doped MoS2 monolayer Mo -V S Defect clusters;
[0022] Figure 4 Statistics of the number of defects: (a) the number of defects in a single layer of undoped MoS2, (b) the number of defects in a single layer of Fe-doped MoS2;
[0023] Figure 5 The electrical performance test results of single-layer undoped MoS2 and single-layer Fe-doped MoS2, (a) output curve of single-layer undoped MoS2 sample, (b) output curve of single-layer Fe-doped MoS2 sample, (c) transfer characteristic curve of single-layer undoped MoS2 sample, (d) transfer characteristic curve of single-layer Fe-doped MoS2 sample;
[0024] Figure 6 Optical microscope photo of single layer Fe-doped MoS2;
[0025] Figure 7 Optical microscope photos of samples obtained by changing the quality of raw materials in the preparation conditions. The sample size is small and thick, not a single layer of molecules;
[0026] Figure 8 Optical microscope photograph of the sample obtained during the temperature increase process of changing the preparation conditions, showing poor crystallinity. DETAILED DESCRIPTION
[0027] The above and other technical features and advantages of the present invention are described in more detail below in conjunction with the accompanying drawings.
[0028] Example 1
[0029] Rich in 3Fe Mo -V S The preparation method of defect cluster single layer Fe doped MoS2 sample is as follows: 2.5 mg Fe2Mo3O 12Place the mixture with NaCl in a quartz boat, and place the growth substrate SiO2 / Si directly above the mixture, facing downward. Pass argon (purity 99.999%) into the quartz tube at a flow rate of 400sccm and maintain for 15 minutes, exhaust the air; then start heating the high temperature zone and raise the temperature to 700℃, the heating rate is 20℃ / min, when the temperature of the high temperature zone rises to 540℃, start the low temperature zone heating program and raise the temperature to 160℃, the heating rate is also 20℃ / min. When the temperature of the high temperature zone reaches 700℃, the low temperature zone can just reach 160℃, maintain the growth temperature and the temperature of the low temperature zone for 10 minutes, after the reaction is completed, let the system cool down naturally to room temperature and turn off the argon gas, and complete the growth of Fe-doped MoS2. In the process of heating, keeping warm and cooling, always keep the argon flow rate at 150sccm.
[0030] Figure 6 For the samples prepared using the conditions of the present invention (the obtained samples have uniform size and thickness), if the process conditions are changed, a flat single-layer Fe-doped MoS2 single crystal cannot be synthesized.
[0031] Example 2
[0032] Rich in 3Fe-V S The preparation method of the single-layer Fe-doped MoS2 sample of the defect cluster is as follows: 2.5 mg of a FeS2+MoO3 mixture with a mass ratio of 1:9 and a NaCl mixture are placed in a quartz boat, the molar ratio of FeS2 to MoO3 is 2:5, and the growth substrate SiO2 / Si is placed directly above the mixture, facing downward. Argon (purity 99.999%) is passed through the quartz tube pipeline at a flow rate of 400sccm and maintained for 15min, and the air is exhausted; then the high temperature zone is heated to 700℃, and the heating rate is 20℃ / min. When the temperature of the high temperature zone is heated to 540℃, the low temperature zone heating program is turned on and heated to 160℃, and the heating rate is also 20℃ / min. When the temperature of the high temperature zone reaches 700℃, the low temperature zone can just reach 160℃, and the growth temperature and the temperature of the low temperature zone are maintained for 10min. After the reaction is completed, the system is naturally cooled to room temperature and the argon is turned off to complete the growth of Fe-doped MoS2. During the heating, keeping and cooling process, the flow rate of argon gas was always maintained at 150 sccm.
[0033] After the obtained sample was transferred to a clean silicon wafer, XPS test was performed and the total spectrum was as follows: Figure 2 (a); The measured Fe element fine spectrum is as follows Figure 2 (b) Raman spectroscopy and photoluminescence spectroscopy were performed on the clean silicon wafer. And compared with undoped MoS2, such as Figure 2(c) and (d) The obtained sample was transferred to a microgrid for spherical aberration transmission electron microscope, and the atomic image was taken to observe the defect morphology of the sample and compare it with the atomic image of the single layer of undoped MoS2. The defects contained in the prepared single layer of Fe-doped MoS2 are as follows: Figure 3 (b) and (c), while undoped MoS2 does not contain defects, such as Figure 3 (a). The concentration statistics of two defects in the single-layer Fe-doped MoS2 sample are shown in the following figure. Figure 4 (b), the defect cluster accounts for 1.08% of the total concentration, indicating that the present invention prepares 3Fe-rich Mo -V S Monolayer Fe-doped MoS2 sample with defect clusters.
[0034] Example 3
[0035] 5.5 mg of Fe2Mo3O with a mass ratio of 1:1 12 Place the mixture with NaCl in a quartz boat, and place the growth substrate SiO2 / Si directly above the mixture, facing downward. Pass argon (purity 99.999%) into the quartz tube at a flow rate of 400sccm and maintain for 15 minutes, exhaust the air; then start heating the high temperature zone and raise the temperature to 700°C at a heating rate of 20°C / min. When the temperature of the high temperature zone rises to 540°C, start the heating program for the low temperature zone and raise the temperature to 160°C at the same heating rate of 20°C / min. When the temperature of the high temperature zone reaches 700°C, the low temperature zone can just reach 160°C. Maintain the growth temperature and the temperature of the low temperature zone for 10 minutes. After the reaction is completed, allow the system to cool down naturally to room temperature and turn off the argon. During the heating, insulation and cooling process, always keep the argon flow rate at 150sccm. Figure 7 This is the sample obtained in this embodiment. As can be seen from the figure, the sample obtained in this embodiment is thicker and smaller in size.
[0036] Example 4
[0037] 1.5 mg of Fe2Mo3O with a mass ratio of 1:1 12Place the mixture with NaCl in a quartz boat, and place the growth substrate SiO2 / Si directly above the mixture, facing downward. Pass argon (purity 99.999%) into the quartz tube at a flow rate of 400sccm and maintain for 15 minutes, exhaust the air; then start heating the high temperature zone and raise the temperature to 700°C at a heating rate of 20°C / min. When the temperature of the high temperature zone rises to 640°C, start the heating program of the low temperature zone and raise the temperature to 160°C at the same heating rate of 20°C / min. When the temperature of the high temperature zone reaches 700°C, the low temperature zone fails to reach 160°C. Although the growth temperature and the low temperature zone temperature are maintained for 10 minutes respectively, the reaction time is not enough. After the reaction is completed, the system is naturally cooled to room temperature and the argon is turned off. During the heating, insulation and cooling process, the argon flow rate is always maintained at 150sccm. Figure 8 This is the sample obtained in this embodiment. As can be seen from the figure, the crystallinity of the sample obtained in this embodiment is poor.
[0038] The above description is only a preferred embodiment of the present invention, which is only illustrative and not restrictive of the present invention. Those skilled in the art understand that many changes, modifications, and even equivalents may be made to the present invention within the spirit and scope defined by the claims of the present invention, but all of them will fall within the scope of protection of the present invention.
Claims
1. A method for preparing a defect-rich cluster monolayer MoS2, characterized in that: The following steps are involved: S1, placing an iron salt, a mixture of a molybdenum-containing compound and a halogen salt, or a mixture of iron molybdate and a halogen salt as a precursor in a container; S2, placing a clean growth substrate directly above the container holding the precursor; S3, placing a solid sulfur source in another container or using a gaseous sulfur source to sulfurize the precursor; S4, placing two containers containing the precursor and the sulfur source in the high temperature zone and the low temperature zone of the dual-temperature zone tubular furnace respectively, passing an inert gas into the furnace tube, exhausting the air, then reducing the inert gas flow rate and increasing the temperature of the high temperature zone, and starting to heat the low temperature zone when the temperature of the high temperature zone rises to a predetermined temperature, and when the high temperature zone rises to the growth temperature, the low temperature zone can just rise to the temperature at which the solid sulfur source melts, so that the high temperature zone and the low temperature zone react, and after the reaction is completed, the reaction system is cooled to room temperature to complete the growth of the defect cluster monolayer MoS2; The halogen salt in step S1 is any one of all halogen salts formed by fluorine, chlorine, bromine, iodine and lithium, sodium, potassium, and cesium.
2. The method for preparing a defect-rich cluster monolayer MoS2 according to claim 1, characterized in that: In step S1, the iron salt is iron chloride or iron sulfide, and the molybdenum-containing compound is any one of molybdenum powder, molybdenum oxide, molybdenum-containing halide, molybdenum-containing sulfate, molybdenum-containing ammonium salt and molybdenum-containing organic salt.
3. The method for preparing a defect-rich cluster monolayer MoS2 according to claim 1, characterized in that: In the step S1, the mass ratio of iron molybdate to halogen salt is 1:1-1:9, and the mass of the precursor is 1-5 mg.
4. The method for preparing a defect-rich cluster monolayer MoS2 according to claim 1, characterized in that: The growth substrate in step S2 is a SiO2 / Si substrate, a sapphire substrate, a mica substrate or any other material that can be used as a growth substrate, and the container is a ceramic boat, a quartz boat or any other sulfur corrosion-resistant and high-temperature-resistant container.
5. The method for preparing a defect-rich cluster monolayer MoS2 according to claim 1, characterized in that: The solid sulfur source in step S3 is any one of solid sublimated sulfur powder, sulfur-containing inorganic matter and sulfur-containing organic matter, and the gaseous sulfur source is H2S gas or gaseous CS2.
6. The method for preparing a defect-rich cluster monolayer MoS2 according to claim 1, characterized in that: The inert gas in step S4 is nitrogen, argon or a mixture of nitrogen and argon.
7. The method for preparing a defect-rich cluster monolayer MoS2 according to claim 1, characterized in that: In step S4, the predetermined temperature is 350-520° C., the growth temperature is 550-720° C., the heating rates of the high temperature zone and the low temperature zone are 10-25° C. / min, and the high temperature zone is maintained for 5-20 minutes after reaching the growth temperature.
8. A defect-rich cluster monolayer MoS2 prepared by the preparation method according to any one of claims 1 to 7.
9. A use of the defect-rich cluster monolayer MoS2 as claimed in claim 8 in electronic devices.