A method for preparing gypsum using a salt cavity

By controlling the reaction temperature in the underground salt cavity and generating and processing high-grade calcium sulfate brine in dihydrate, the problem of waste of gypsum resources during the preparation of ammonia alkali method is solved, the strength and resource utilization of salt cavity goaf area are improved, and the utilization rate of the resource is achieved Sustainable development of salt mines.

CN117361600BActive Publication Date: 2024-11-19JIANGSUSHENG JINGSHEN YANYE CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311138063.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-05
Publication Date
2024-11-19
Estimated Expiration
2043-09-05

AI Technical Summary

Technical Problem

The waste liquid and waste residue generated during the preparation of soda ash by the existing ammonia alkali method is low, resulting in long-term storage of gypsum as a by-product in the underground salt cavity, increasing the difficulty of subsequent rock salt resource mining, resulting in resource waste and economic losses.

Method used

By controlling the reaction temperature in the underground salt cavity, the chemical reaction of alkaline calcium liquid and salt nitrate mother liquor is used to generate high-grade calcium sulfate dihydrate brine, which is transported to the ground through the halogen drainage pipeline to avoid gypsum precipitation covering the bottom of the well, and improve the increase of the rock salt in the bottom of the well The strength of the underground salt cavity goaf area reduces resource waste.

Benefits of technology

It effectively improves the solubility and yield of gypsum, reduces the rock salt resources covered by gypsum, promotes the goaf stability of the salt cavity, reduces resource waste and economic losses, and supports the sustainable development of salt mines.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117361600B_ABST
    Figure CN117361600B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of salt products, and discloses a method for preparing gypsum using a salt cavity, and the specific steps are as follows: S1, injecting pretreated alkali-making calcium liquid and salt nitrate mother liquor into the salt cavity through a first brine injection well and a second brine injection well respectively; wherein the injection well temperature of the alkali-making calcium liquid is 80°C-100°C, and the injection well temperature of the salt nitrate mother liquor is 60°C-80°C; S2, the alkali-making calcium liquid and the salt nitrate mother liquor react in the salt cavity to form brine in which calcium sulfate dihydrate is dissolved; S3, the brine is discharged from the salt cavity through a brine discharge well, and processed to obtain calcium sulfate dihydrate. The present invention uses an underground salt cavity as a reaction vessel, controls the solubility of gypsum by controlling the reaction temperature, and transports the brine in which calcium sulfate dihydrate is dissolved to the ground through a brine discharge pipeline to obtain calcium sulfate dihydrate, which not only avoids the calcium sulfate dihydrate precipitation generated in the underground salt cavity covering the bottom of the well, and a large amount of gypsum is stored underground to cause a waste of resources, but also obtains an economic product calcium sulfate dihydrate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of salt products, and in particular to a method for preparing gypsum by utilizing a salt cavity. Background Art

[0002] Ammonia-soda process: in 1861, the Belgian Solvay used salt, limestone and ammonia as raw materials to produce sodium carbonate and calcium chloride.

[0003] The ammonia-soda process has the advantages of simple process, wide distribution and easy acquisition of raw materials, and high product purity. However, the ammonia-soda process has a very big disadvantage, which is that a large amount of waste liquid and waste residue will be generated during the production process. The main components of the waste liquid and waste residue are calcium chloride and sodium chloride. For every ton of soda ash produced, 10m 3 At present, the utilization rate of waste liquid and waste residue is low. Waste liquid is generally discharged and disposed, while waste residue is piled in the open air, which occupies a lot of land resources and pollutes the ecological environment.

[0004] With the advancement of people's understanding and the requirements for environmental protection, the waste residue and waste liquid of soda ash are treated and comprehensively utilized. At present, the more effective method is to inject the waste liquid produced by the ammonia-soda method into the underground salt cavity of rock salt. For example, the invention patent CN101629484A "Resource Utilization Method of Ammonia-Soda Waste Liquid for Sodium Sulfate Salt Mine Injection and Brine Extraction" injects the waste liquid produced by alkali production into the underground salt cavity to obtain high-grade brine with low sodium sulfate content, which not only effectively reduces the sodium sulfate in the brine, but also recycles and utilizes sodium chloride, effectively reducing waste emissions. The invention patent CN102205979B "Salt, Alkali and Calcium Combined Circulation Production Process Using Well Salt" injects the waste liquid from alkali production into the underground salt cavity of the salt mine to extract brine, and obtains brine with a high calcium ion content. As the raw material for salt and calcium co-production, it is injected into the underground salt cavity, and the utilization rate of sodium chloride in the rock salt reaches 100%, and the benefit is maximized.

[0005] The above inventions all inject the waste liquid and waste residue produced by alkali production into the underground salt cavity, and then replace the brine to improve the quality of calcium chloride, and use calcium chloride as an economic product, but ignore the economic value of gypsum as a by-product. Gypsum is a widely used industrial material that can be used to prepare cement retarders, building products, medical food additives, sulfuric acid production, paint fillers, etc. Gypsum is divided into natural gypsum and industrial by-product gypsum. Natural gypsum is gradually decreasing due to various reasons. With the development of social economy, industrial by-product gypsum is continuously produced and is gradually replacing natural gypsum, and even exceeds natural gypsum for large-scale use. There are many types of industrial by-product gypsum, but their core components are all calcium sulfate dihydrate or anhydrous calcium sulfate. The existing industrial by-product gypsum varieties can completely replace natural gypsum. After technical processing, the bonding performance can be greatly improved.

[0006] When injecting alkali-making calcium liquid underground, the mirabilite-type salt resources associated with underground rock salt will react with the calcium liquid to form slightly soluble CaSO4, namely gypsum. The solubility of gypsum is very small, and it can form a cementing filling body with a certain strength in the underground salt cavity, which can effectively improve the strength of the goaf of the underground salt cavity and inhibit the shrinkage of the salt cavity and surface settlement. However, gypsum, as a by-product, has certain economic value. It is stored in the salt cavity for a long time and covers the surface of the rock salt resources, which increases the difficulty of subsequent rock salt resource mining and causes waste of resources and economic losses. Summary of the invention

[0007] Purpose of the invention: In view of the problems existing in the prior art, the present invention provides a method for preparing gypsum using a salt cavity, using the underground salt cavity as a reaction vessel, controlling the solubility of gypsum by controlling the reaction temperature, and transporting the brine dissolving calcium sulfate dihydrate to the ground through a brine discharge pipeline, and obtaining high-grade calcium sulfate dihydrate after treatment. The present invention avoids the waste of gypsum resources caused by the underground storage of a large amount of gypsum, reduces the precipitation of calcium sulfate dihydrate generated in the underground dissolution cavity and covers the rock salt at the bottom of the well, and well solves this technical problem that restricts the green and sustainable development of salt enterprises.

[0008] Technical solution: The present invention provides a method for preparing gypsum using a salt cavity, comprising the following steps:

[0009] S1, injecting the salt nitrate mother liquor and the pretreated alkali calcium liquor into the salt cavity through the first brine injection well and the second brine injection well respectively; the injection well temperature of the alkali calcium liquor is 80°C-100°C, and the injection well temperature of the salt nitrate mother liquor is 60°C-80°C;

[0010] S2, the alkali-making calcium solution and the salt nitrate mother solution react in the salt chamber filled with brine to form brine in which calcium sulfate dihydrate is dissolved, and the reaction temperature is 60°C-80°C;

[0011] S3, discharging the brine from the salt cavity through a brine drainage well, and processing to obtain calcium sulfate dihydrate.

[0012] Preferably, a two-injection-one-discharge method is adopted, the first brine injection well injects alkali-making calcium liquid, the second brine injection well injects salt nitrate mother liquor, and the brine dissolved with calcium sulfate dihydrate is discharged through the middle brine discharge well.

[0013] Furthermore, the brine discharge well is provided with a wellbore pipe for outputting brine, and the first brine injection well and the second brine discharge well are provided with wellbore pipes for inputting the alkali calcium solution and salt nitrate mother solution, and the wellbore pipes all adopt double-layer vacuum insulation casing.

[0014] The wellbore pipe adopts a double-layer vacuum insulation casing with excellent thermal insulation performance, which can effectively reduce heat loss during brine injection and production.

[0015] Furthermore, in S1, the salt cavity is located 1,600 meters below the surface, with sediment accumulated at the bottom and filled with saturated brine at the top. It has no series connection with other well groups, and the temperature of the saturated brine in the salt cavity is above 60°C.

[0016] Among them, salt cavity refers to the underground dissolution cavity formed in the process of water-soluble mining of rock salt deposits. It is generally mined by connected well water-soluble mining, and two salt cavities form a connected space underground.

[0017] Furthermore, the brine discharge well is located between the first brine injection well and the second brine injection well.

[0018] Furthermore, the distance between the first brine injection well and the second brine injection well is 150m-200m.

[0019] Furthermore, in S1, the alkali-making calcium liquid comes from waste residue and waste liquid produced by alkali plant production, and its main component is calcium chloride, and its calcium chloride content is 90-120 g / L, preferably 90-100 g / L, more preferably 100-110 g / L, and most preferably 110-120 g / L.

[0020] The alkali calcium solution can be the ammonia-alkali waste liquid produced by the production of soda ash. The composition of the ammonia-alkali waste liquid is generally: CaCl2 is generally 90-120g / L (dry basis); NaCl content is generally 40-60g / L (dry basis).

[0021] Furthermore, in S1, the main component of the salt nitrate mother liquor is sodium sulfate, and the sodium sulfate content is 50-60g / L.

[0022] Wherein, the calcium solution may also be a calcium chloride solution.

[0023] Furthermore, in S1, the injection volume ratio of the alkali-making calcium solution and the salt nitrate mother solution is 1:1-1:3.

[0024] Furthermore, in S1, the pretreatment specifically refers to clarifying the alkali-making calcium liquid with a clarification tank and thickening it with a cyclone; the calcium chloride content in the alkali-making calcium liquid after the pretreatment is 90-120 g / L.

[0025] The purpose of the clarifier and cyclone is to thicken the soda ash waste liquid and increase the solid content to more than 25%. The operating pressure of the cyclone is 200KPa, the flow rate is 70m³ / h, and the temperature is 90℃. The clear liquid of the alkali calcium solution overflows from the top of the clarifier to the clear waste liquid pool, and the thick mud enters the mud mixing barrel. The solid content of the mud is about 10%, which is sent to the cyclone by the feed pressure pump and further concentrated and thickened by the cyclone.

[0026] Furthermore, in S3, the processing specifically refers to pumping the brine into a clarification tank, cooling the slurry to thicken the solid content to a concentrated slurry with a solid content of 30%, and washing and filtering the concentrated slurry to obtain a high-quality, high-whiteness gypsum product.

[0027] The clarification tank refers to a Doyle-type clarification tank, the upper clear liquid flows out naturally by overflow, and the lower slurry is discharged from the bottom, and thickening refers to thickening the slurry to a solid content of 30%. The water washing and filtration is to use a vacuum belt filter with spray washing for solid-liquid separation, the vacuum pump pressure is preferably 0.04MPa-0.08MPa, more preferably 0.05MPa-0.07MPa, and the water spray rate is preferably 0.01m 3 / h-0.04m 3 / h, more preferably 0.02m 3 / h-0.04m 3 The washing water is condensed water from salt production, and the mass ratio of condensed water to filter residue is preferably 1.5:1-3:1, more preferably 2:1-2.5:1.

[0028] Theoretical explanation:

[0029] The principle of the present invention is as follows: alkali-making calcium liquid and salt nitrate mother liquid are mixed in an underground salt cavity, and a reaction device for preparing gypsum is used using the chemical reaction mechanism of calcium chloride and sodium sulfate, and the rock salt cavity (salt cavity) in the water-soluble mining process is used as a mixed solution. After sufficient reaction, the gypsum is fully dissolved, and the gypsum brine is discharged to the ground through a brine discharge pipeline.

[0030] The deep salt cavity underground has a huge volume, which can ensure the reaction amount of alkali-making calcium liquid and saltpeter mother liquor, and the amount of gypsum obtained is also considerable.

[0031] The solubility of calcium sulfate first increases with the increase of sodium chloride concentration, then decreases after a maximum value appears in the middle, and the maximum value is about 7g / L; when the brine concentration is 25%, the solubility of calcium sulfate first increases with the increase of temperature, reaches the highest at 70℃, and then decreases. The brine in the salt cavity is close to saturation, and the sodium chloride concentration is about 25%. Therefore, the solubility of gypsum in the salt cavity environment is mainly affected by the reaction temperature. Since brine injection and drainage is a continuous and uninterrupted process, the heat exchange between the formation and the brine is slow in a short time. Ignoring the heat loss during the injection process, the depth of the salt cavity can be controlled, and then the temperature of the brine in the salt cavity can be controlled. Then the reaction temperature in the salt cavity is mainly affected by the injection temperature of the alkali calcium solution and the salt nitrate mother solution. Therefore, according to the gypsum solubility formula, controlling the reaction temperature at 60℃-80℃ can effectively improve the solubility of calcium sulfate dihydrate.

[0032] The solubility of gypsum is calculated according to the following formula:

[0033] ;

[0034] In the formula,

[0035] S——Solubility of calcium sulfate dihydrate, g / L;

[0036] T A ——Reaction temperature, ℃.

[0037] The bottom temperature of the salt cavity is calculated based on the geothermal gradient:

[0038] ;

[0039] Where:

[0040] T C ——Brine bottom temperature, ℃

[0041] T B ——Surface temperature, °C

[0042] K - geothermal gradient

[0043] H——Salt cavity depth, m.

[0044] Beneficial effects: Compared with the prior art, the present invention has the following specific beneficial effects:

[0045] 1. Use the underground salt cavity of rock salt as a reaction container, and control the reaction temperature in the underground cavity by controlling the injection temperature of alkali calcium solution and salt nitrate mother solution, thereby controlling the solubility of gypsum. In addition, the huge reaction space of the salt cavity can obtain a large amount of brine for dissolving gypsum, effectively alleviating the current situation where most of the gypsum covers the rock salt deposits at the bottom of the well, resulting in a large amount of rock salt resource waste.

[0046] 2. By connecting the wells in two rows, the two brine injection wells are respectively injected with alkali-making calcium liquid and salt nitrate mother liquor, which can effectively prevent the reaction products of alkali-making calcium liquid and salt nitrate mother liquor from being attached to the inner wall of the wellbore when they are injected into the same wellbore pipe, causing blockage of the wellbore and adversely affecting subsequent production. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] Figure 1 The present invention is a process flow diagram of a method for preparing gypsum using a salt cavity;

[0048] Figure 2 This is a schematic diagram of the underground salt cavity of the present invention;

[0049] Among them, 1 is the first brine injection well, 2 is the second brine injection well, 3 is the brine extraction well, and 4 is the underground connected salt cavity. DETAILED DESCRIPTION

[0050] The present invention is further described in detail below in conjunction with an example of a rock salt mine: However, this is not a limitation of the present invention. These descriptions are only for further illustrating the features and advantages of the present invention, rather than for limiting the claims. Any equivalent substitutions in the art made according to the disclosure of the present invention are within the protection scope of the present invention.

[0051] Implementation 1:

[0052] This embodiment provides a method for preparing gypsum by controlling the temperature field in a salt chamber, and the method is specifically as follows:

[0053] The target mining area is a salt mine in Huai'an City, Jiangsu Province. The approved production scale of the mine is 1.2 million tons / year, and the mining elevation is -1300m--2460m. The salt mine has been mined and produced for more than 15 years. It mainly produces brine by directional connected well technology. The production time is long. According to production estimates, the volume of underground dissolution cavity is large. A group of salt cavities was selected for in-depth work and systematic evaluation. First, the production situation of this group of salt wells was investigated. The well group's production-injection ratio was stable at about 0.9, the aquifer depth was about 300m, the cavity bottom depth was 1990m, the cavity top position was 1945m, the cavity volume was about 96,000 cubic meters, and there was no series dissolution with other production well groups.

[0054] The alkali calcium liquid that meets the discharge requirements is clarified with a clarification barrel. The clear alkali calcium liquid overflows from the top of the clarification barrel to the clear waste liquid pool. The thick mud enters the mud mixing barrel. The solid content of the mud is about 10%. It is sent to the cyclone through the feed pressure pump. The operating pressure of the cyclone is 200KPa, the flow rate is 70m³ / h, and the temperature is 90℃. The alkali calcium liquid is further concentrated and thickened after passing through the cyclone, and the solid content is more than 25%. The salt nitrate mother liquor (NaSO450g / L, temperature is 65℃) and the pretreated alkali calcium liquid (CaCl2100g / L, PH is 10, temperature is 80℃) are injected into the salt mine through different wellheads and react in the underground salt cavity. The calcium chloride in the pretreated alkali calcium liquid and the sodium sulfate in the salt nitrate mother liquor react in the underground salt cavity. According to calculation, the water addition amount is 10.54 million cubic meters of fresh water, 828,000 tons of calcium sulfate dihydrate are generated, and the extraction-injection ratio is 0.9, which will obtain 15.56 million cubic meters of brine. After 3 hours of injection of brine, the chemical reaction is complete, the concentration of calcium sulfate dihydrate in the brine is 7g / L, and 10,892 tons of calcium sulfate dihydrate are dissolved in the brine. Finally, the brine with calcium sulfate dihydrate dissolved is collected to the ground through the brine well, pumped to the clarification tank, and cooled to thicken the slurry solid content to a thick slurry with a solid content of 30%. The thick slurry is washed and filtered to obtain high-quality, high-whiteness gypsum products.

[0055] Implementation 2:

[0056] This embodiment provides a method for preparing gypsum using a salt cavity, and the method is applied to a connecting well as follows:

[0057] The target mining area is a salt mine in Huai'an City, Jiangsu Province. The approved production scale of the mine is 1.2 million tons / year, and the mining elevation is -1300m--2460m. The salt mine has been in production for more than 15 years, mainly producing brine with directional connected well technology. The production time is long, and the underground cavity volume is large according to production estimates. A group of salt cavities were selected for in-depth work and systematic evaluation. First, the production situation of this group of salt wells was investigated. The well group's production-injection ratio was stable at about 0.9, the aquifer depth was about 250m, the cavity bottom depth was 2066m, the cavity top position was 2001m, the cavity volume was about 81,000 cubic meters, and there was no series dissolution with other production well groups.

[0058] The alkali calcium liquid that meets the discharge requirements is clarified with a clarification barrel, and the clear alkali calcium liquid overflows from the top of the clarification barrel to the clear waste liquid pool. The thick mud enters the mud mixing barrel. The solid content of the mud is about 10%. It is sent to the cyclone through the feed pressure pump. The operating pressure of the cyclone is 200KPa, the flow rate is 70m³ / h, and the temperature is 90℃. The alkali calcium liquid is further concentrated and thickened after passing through the cyclone, and the solid content is more than 25%. The salt nitrate mother liquor (NaSO450g / L, temperature is 70℃) and the pretreated alkali calcium liquid (CaCl2100g / L, PH is 10, temperature is 80℃) are injected into the salt mine through different wellheads and react in the underground salt cavity. The calcium chloride in the pretreated alkali calcium liquid and the sodium sulfate in the salt nitrate mother liquor react in the underground salt cavity. According to calculation, the water addition amount is 10.54 million cubic meters of fresh water, 911,000 tons of calcium sulfate dihydrate are generated, and the extraction and injection ratio is 0.9, which will obtain 15.56 million cubic meters of brine. After 3 hours of injection of brine, the chemical reaction is complete, the concentration of calcium sulfate dihydrate in the brine is 7g / L, and 10,892 tons of calcium sulfate dihydrate are dissolved in the brine. Finally, the brine with calcium sulfate dihydrate dissolved is collected to the ground through the brine well, pumped to the clarification tank, and cooled to thicken the slurry solid content to a concentrated slurry with a solid content of 30%. The concentrated slurry is washed and filtered to obtain high-quality, high-whiteness gypsum products.

[0059] Implementation 3:

[0060] This embodiment provides a method for preparing gypsum using a salt cavity, and the method is specifically as follows:

[0061] The target mining area is a salt mine in Huai'an City, Jiangsu Province. The approved production scale of the mine is 1.2 million tons / year, and the mining elevation is -1300m--2460m. The salt mine has been mined and produced for more than 15 years. It mainly produces brine by directional connected well technology. The production time is long. According to production estimates, the volume of underground dissolved cavities is large. A group of salt cavities was selected for in-depth work and systematic evaluation. First, the production situation of this group of salt wells was investigated. The well group's production-injection ratio was stable at about 0.9, the aquifer depth was about 300m, the cavity bottom depth was 2096m, the cavity top position was 2050m, the cavity volume was about 63,000 cubic meters, and there was no series dissolution with other production well groups.

[0062] The alkali calcium liquid that meets the discharge requirements is clarified with a clarification barrel. The clear alkali calcium liquid overflows from the top of the clarification barrel to the clear waste liquid pool. The thick mud enters the mud mixing barrel. The solid content of the mud is about 10%. It is sent to the cyclone through the feed pressure pump. The operating pressure of the cyclone is 200KPa, the flow rate is 70m³ / h, and the temperature is 90℃. The alkali calcium liquid is further concentrated and thickened after passing through the cyclone, and the solid content is more than 25%. The salt nitrate mother liquor (NaSO460g / L, temperature is 70℃) and the pretreated alkali calcium liquid (CaCl2120g / L, PH is 11, temperature is 70℃) are injected into the salt mine through different wellheads and react in the underground salt cavity. The calcium chloride in the pretreated alkali calcium liquid and the sodium sulfate in the salt nitrate mother liquor react in the underground salt cavity. According to calculation, the water addition amount is 10.54 million cubic meters of fresh water, 994,000 tons of calcium sulfate dihydrate are generated, and the extraction-injection ratio is 0.9, which will obtain 15.56 million cubic meters of brine. After 3 hours of injection of brine, the chemical reaction is complete, the concentration of calcium sulfate dihydrate in the brine is 7g / L, and 10,892 tons of calcium sulfate dihydrate are dissolved in the brine. Finally, the brine with dissolved calcium sulfate dihydrate is collected to the ground through the brine well, pumped to the clarification tank, and cooled to thicken the slurry solid content to a thick slurry with a solid content of 30%. The thick slurry is washed and filtered to obtain high-quality, high-whiteness gypsum products.

[0063] Implementation 4:

[0064] This embodiment provides a method for preparing gypsum using a salt cavity, and the method is specifically as follows:

[0065] The target mining area is a salt mine in Huai'an City, Jiangsu Province. The approved production scale of the mine is 1.2 million tons / year, and the mining elevation is -1030m--1700m. The salt mine has been mined and produced for more than 15 years. It mainly produces brine by directional connected well technology. The production time is long. According to production estimates, the volume of underground dissolved cavities is large. A group of salt cavities was selected for in-depth work and systematic evaluation. First, the production situation of this group of salt wells was investigated. The well group's production-injection ratio was stable at about 0.9, the aquifer depth was about 300m, the cavity bottom depth was 1660m, the cavity top position was 1626m, the cavity volume was about 76,000 cubic meters, and there was no series dissolution with other production well groups.

[0066] The alkali calcium liquid that meets the discharge requirements is clarified with a clarification barrel. The clear alkali calcium liquid overflows from the top of the clarification barrel to the clear waste liquid pool. The thick mud enters the mud mixing barrel. The solid content of the mud is about 10%. It is sent to the cyclone through the feed pressure pump. The operating pressure of the cyclone is 200KPa, the flow rate is 70m³ / h, and the temperature is 90℃. The alkali calcium liquid is further concentrated and thickened after passing through the cyclone, and the solid content is more than 25%. The salt nitrate mother liquor (NaSO460g / L, temperature is 80℃) and the pretreated alkali calcium liquid (CaCl290g / L, PH is 9, temperature is 80℃) are injected into the salt mine through different wellheads and react in the underground salt cavity. The calcium chloride in the pretreated alkali calcium liquid and the sodium sulfate in the salt nitrate mother liquor react in the underground salt cavity. According to calculation, the water addition amount is 10.54 million cubic meters of fresh water, 745,000 tons of calcium sulfate dihydrate are generated, and the extraction-injection ratio is 0.9, which will obtain 15.56 million cubic meters of brine. After 3 hours of injection of brine, the chemical reaction is complete, the concentration of calcium sulfate dihydrate in the brine is 7g / L, and 10,892 tons of calcium sulfate dihydrate are dissolved in the brine. Finally, the brine with calcium sulfate dihydrate dissolved is collected to the ground through the brine well, pumped to the clarification tank, and cooled to thicken the slurry solid content to a concentrated slurry with a solid content of 30%. The concentrated slurry is washed and filtered to obtain high-quality, high-whiteness gypsum products.

[0067] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent transformation or modification made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing gypsum using a salt cavity, characterized in that: The following steps are involved: S1, injecting the salt nitrate mother liquor and the pretreated alkali calcium liquor into the brine in the salt cavity through the first brine injection well and the second brine injection well respectively; the injection well temperature of the alkali calcium liquor is 80°C-100°C, and the injection well temperature of the salt nitrate mother liquor is 60°C-80°C; wherein the saturated brine temperature in the salt cavity is above 60°C, the main component of the salt nitrate mother liquor is sodium sulfate, and the main component of the alkali calcium liquor is calcium chloride; S2, the alkali-making calcium solution and the salt nitrate mother solution react in the brine in the salt chamber to form brine in which calcium sulfate dihydrate is dissolved, and the reaction temperature is 60°C-80°C; S3, discharging the brine containing calcium sulfate dihydrate dissolved in S2 from the salt cavity through a brine discharge well, and processing to obtain calcium sulfate dihydrate; the brine discharge well is located between the first brine injection well and the second brine injection well.

2. The method for preparing gypsum using a salt cavity according to claim 1, characterized in that: In S1, the salt cavity is located 1,600 meters below the surface, with sediment accumulated at the bottom and the cavity filled with saturated brine.

3. The method for preparing gypsum using a salt cavity according to claim 1, characterized in that: The brine discharge well is provided with a wellbore pipe for outputting brine, and the first brine injection well and the second brine discharge well are provided with wellbore pipes for inputting the alkali calcium solution and salt nitrate mother solution. The wellbore pipes are all made of double-layer vacuum insulation casing.

4. The method for preparing gypsum using a salt cavity according to claim 1, characterized in that: The distance between the first brine injection well and the second brine injection well is 150-200m.

5. The method for preparing gypsum using a salt cavity according to claim 1, characterized in that: In S1, the injection volume ratio of the pretreated alkali-making calcium solution and the salt nitrate mother solution is 1:1-1:

3.

6. The method for preparing gypsum using a salt cavity according to claim 1, characterized in that: In S1, the sodium sulfate content in the salt nitrate mother liquor is 50-60 g / L.

7. The method for preparing gypsum using a salt cavity according to claim 1, characterized in that: In S1, the pretreatment specifically refers to clarifying the alkali-making calcium solution with a clarification tank and thickening it with a cyclone.