Color conversion film with separator layer

By using a partition layer in a liquid crystal display to separate the green luminescent perovskite crystal layer and the red core-shell quantum dot layer, the incompatibility and degradation problems are solved, and a color conversion film with high stability and low heavy metal content is achieved, satisfying the Anti-humidity and anti-oxidation requirements.

CN117956825BActive Publication Date: 2024-11-19AVANTAMA AG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310470322.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2022-10-27
Filing Date
2023-04-27
Publication Date
2024-11-19
Estimated Expiration
2043-04-27

AI Technical Summary

Technical Problem

The luminescent perovskite and core-shell quantum dot levels in existing liquid crystal displays have problems caused by incompatibility, humidity and oxygen, which is difficult to meet the requirements of anti-humidity and anti-oxidation stability. At the same time, the high content of heavy metals violates the RoHS directive.

Method used

Using a color conversion film including a green luminescent perovskite crystal layer and a red core-shell quantum dot layer, separated by a partition layer, and using a poreless, defect-free polymer layer in the partition layer to provide humidity and oxygen barrier and reduce heavy metal content.

Benefits of technology

A color conversion film with green and red light output under blue light excitation is realized, with excellent optical properties, low heavy metal content, high stability to temperature, humidity and oxygen, reducing manufacturing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004203726180000111
    Figure BDA0004203726180000111
  • Figure BDA0004203726180000121
    Figure BDA0004203726180000121
Patent Text Reader

Abstract

The invention discloses a color conversion film, which emits green light and red light under the stimulation of blue light. The film comprises at least one red light-emitting layer, one green light-emitting layer and at least one separation layer sandwiched therebetween.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a color conversion film, which comprises a green perovskite crystal layer and a red core-shell quantum dot layer and a specific spacer layer separating the layers. The present invention further provides a method for manufacturing such a film and a device comprising such a film. Background Art

[0002] The most advanced liquid crystal displays (LCDs) or display components include components based on luminescent crystals (quantum dots). In particular, the backlight components of such LCDs may include RGB backlights consisting of red, blue and green light. Now, luminescent crystals (quantum dots) are often used to produce the backlight colors of such backlight components.

[0003] For example, WO2017 / 108568 discloses a light-emitting component suitable for manufacturing an LCD. The light-emitting component includes a green light-emitting perovskite dispersed in a polymer film and a red light-emitting perovskite dispersed in another polymer film. Although these light-emitting components are suitable, they show relatively high levels of heavy metals. In addition, EP22179215.3 (unpublished) discloses a light-emitting component suitable for manufacturing an LCD. The light-emitting component includes a green light-emitting perovskite dispersed in a polymer film and a red light-emitting core-shell quantum dot dispersed in another polymer film, and the two films are separated by an inorganic layer.

[0004] The manufacture of such components faces various challenges. One of the challenges is embedding the light-emitting crystals into the components. Due to the different chemical properties of the light-emitting crystals, there may be incompatibility between various embedded materials including the light-emitting crystals or even between light-emitting crystals embedded in the same material. This incompatibility may cause degradation of the materials in the display components, and thus the life of such displays may be affected.

[0005] Additionally, components based on light-emitting crystals often face challenges with degradation caused by humidity and / or oxygen. Luminescent perovskite crystals are primarily degraded by the presence of humidity / water, and luminescent core-shell quantum dots are primarily degraded by the presence of oxygen. It is difficult to provide display components including green-emitting perovskite crystals and red-emitting core-shell quantum dots with sufficient stability against humidity and oxygen.

[0006] Furthermore, light-emitting components should comply with legal regulations, such as the RoHS directive. Of particular interest is compliance with the requirements for low heavy metal content in such components while meeting the market's requirements for high luminescence. Light-emitting perovskite crystals contain Pb, which is a heavy metal and is restricted by the RoHS directive. Therefore, the goal is to minimize the amount of light-emitting perovskite crystals per display. Summary of the invention

[0007] The problem to be solved by the present invention is to overcome the shortcomings of the prior art. In particular, the present invention overcomes the shortcomings of the prior art in terms of stability. The present invention relates to a color conversion film, which emits green light and red light under the excitation of blue light. The film includes at least one red light-emitting layer, one green light-emitting layer and at least one separator layer sandwiched therebetween. Unless otherwise specified, the following definitions shall apply to this specification:

[0008] The terms "a", "an", "the" and similar terms used in the context of the present invention should be interpreted as covering the singular and the plural, unless otherwise specified herein or clearly contradicted by the context. The term "comprising" shall be construed to include "including", "consisting essentially of" and "consisting of". Percentages are expressed in weight %, unless otherwise specified herein or clearly contradicted by the context. "Independently" means that a substituent / ion can be selected from one of the specified substituents / ions, or a combination of multiple thereof.

[0009] The term "luminescent crystal" (LC) is known in the art and in the context of the present invention refers to crystals of 2-100 nm made of semiconductor material. The term includes quantum dots, typically 2-10 nm, and nanocrystals, typically 10-100 nm.

[0010] As the term indicates, LC exhibits luminescence. In the context of the present invention, the term luminescent crystal includes single crystal and polycrystalline particles. In the latter case, a particle may include several crystal domains (crystals) connected by crystalline or amorphous phase boundaries. A luminescent crystal is a semiconductor material that exhibits a direct band gap (usually 1.1-3.8 eV, more usually 1.4-3.5 eV, and even more usually 1.7-3.2 eV). When irradiated with electromagnetic radiation equal to or higher than the energy gap, valence band electrons are excited to the conduction band, leaving electron holes in the valence band. The formed excitons (electron-electron hole pairs) then radiatively recombine in the form of photoluminescence, with a maximum intensity centered at the LC energy gap value and exhibiting a photoluminescence quantum yield of at least 1%. When in contact with an external electron and electron hole source, the LC can exhibit electroluminescence.

[0011] The term "quantum dot" (QD) is known and refers in particular to semiconductor nanocrystals, which are typically 2-10 nm in diameter. In this range, the physical radius of the QD is smaller than the bulk excitation Bohr radius, resulting in a dominant quantum confinement effect. Therefore, the electronic state of the QD, as well as the energy gap, is a function of the QD composition and physical size, i.e., the color absorbed / emitted is related to the size of the QD. The optical quality of a QD sample is directly related to its homogeneity (more monodisperse QDs will have a smaller luminescent FWHM). When the QD reaches a size greater than the Bohr radius, the quantum confinement effect is hindered and the sample may no longer emit light, as the non-radiative pathways of exciton recombination may become dominant. Therefore, QDs are a specific subgroup of nanocrystals, particularly defined by their size and size distribution. Typical quantum dot compositions include cadmium or indium, for example in the form of cadmium selenide (CdSe) indium phosphide (InP).

[0012] The term "core-shell quantum dots" is known and relates in particular to quantum dots that typically include an indium-containing or cadmium-containing core, typically a CdSe core or an InP core, with an additional shell typically comprising zinc sulfide (ZnS), zinc selenide (ZnSe), cadmium sulfide (CdS) or a combination thereof. Core-shell quantum dots may include multiple shells or a shell gradient.

[0013] The term "perovskite crystal" is known, in particular, to include a crystalline compound of the perovskite structure. Such a perovskite structure is known per se and is described by the general formula M 1 M 2 Cubic, pseudocubic, tetragonal or orthorhombic crystals of X3, where M 1 is a cation with a coordination number of 12 (cuboctahedral), M 2 is a cation with a coordination number of 6 (octahedral), and X is an anion in a cubic, quasi-cubic, tetragonal or orthorhombic position of the lattice. In these structures, selected cations or anions can be replaced by other ions (randomly or regularly up to 30 atomic %), thereby producing doped perovskites or non-stoichiometric perovskites, but still maintaining their original crystal structure. Preferably, the luminescent perovskite crystals are approximately isometric (such as spherical or cubic). If the aspect ratio (longest: shortest direction) of all 3 orthogonal dimensions is 1-2, the particles are considered to be approximately isometric. Accordingly, the LC assembly preferably contains 50-100% (n / n), preferably 66-100% (n / n), and more preferably 75-100% (n / n) isometric nanocrystals.

[0014] The production of such light-emitting perovskite crystals is known, for example from WO 2018 / 028869.

[0015] The term "polymer" is known and includes synthetic materials containing repeating units ("monomers"). The term polymer includes homopolymers and copolymers. In addition, crosslinked polymers and non-crosslinked polymers are also included. Depending on the context, the term polymer should include its monomers and oligomers. For example, polymers include acrylic polymers, carbonate polymers, sulfone polymers, epoxy polymers, vinyl polymers, urethane polymers, imide polymers, ester polymers, furan polymers, melamine polymers, styrene polymers, olefin polymers (including cycloolefin polymers, such as norbornene polymers) and silazane polymers. According to the practice in the art, polymers may include other materials such as polymerization initiators, stabilizers and fillers.

[0016] The term "matrix" is known in the art and in the context of the present invention means a continuous phase comprising a discontinuous or particulate phase. The continuous material thus encapsulates the particulate phase.

[0017] The present invention First aspect A color conversion film is related to the color conversion film, which emits green light and red light under the excitation of blue light. The film of the present invention comprises multiple layers, wherein one or more layers (preferably one layer) is a green light-emitting polymer layer comprising green light-emitting perovskite crystals; and one or more layers (preferably one layer) is a red light-emitting polymer layer comprising red light-emitting core-shell quantum dots, the red light-emitting quantum dots comprising II-VI or II-V type semiconductors; and wherein the one or more red light-emitting polymer layers and the green light-emitting polymer layer are separated by one or more spacer layers. Suitable spacer layers cover the entire area of ​​the red and / or green light-emitting polymer layer. In addition, the color conversion film may include one or more barrier films attached to the red light-emitting polymer layer and / or the green light-emitting polymer layer. In addition, the color conversion film may include one or more non-emissive polymer layers. In addition, the red light-emitting polymer layer may contain one or more polythiols.

[0018] It was found that these color conversion films, which combine perovskite and core-shell quantum dots in a laminated structure, exhibit excellent optical properties, low heavy metal content, high stability to temperature, humidity and oxygen, and also facilitate low manufacturing costs. This aspect of the invention is described in further detail below.

[0019] Color conversion film:

[0020] Color conversion films are known per se and find widespread use in commercial articles such as displays. According to the present invention, such films partially or completely convert blue light into red and green light. Typically, the blue light is partially converted so that light in the blue, green and red spectrum is emitted. By adjusting the blue light intensity, concentration, film thickness and the amount of green and red material that emits light, the color of the emitted light can be adjusted according to the needs of the customer.

[0021] Such a color conversion film may be described as a laminate structure and identified by its individual layers, such as "red emitting polymer layer", "green emitting polymer layer", "spacer layer" and "cover layer".

[0022] The film thickness of the color conversion film (including all individual layers) is typically 10-500 microns, preferably 20-250 microns, most preferably 30-200 microns.

[0023] The color conversion films of the present invention may be assembled to obtain a display backlight. Thus, the present invention also provides a display backlight comprising a color conversion film as described herein.

[0024] The color conversion films of the present invention can be assembled to obtain a light emitting device, such as a liquid crystal display. Accordingly, the present invention also provides a light emitting device, preferably a liquid crystal display, comprising the color conversion film described herein.

[0025] Separator layer:

[0026] A spacer layer is applied in the color conversion film of the present invention. As the name implies, it allows to spatially separate the two layers. Suitable spacers can be prepared using commercial starting materials and equipment. It was found that the spacer layer sandwiched between the red and green light-emitting layers retains the optical properties and improves the stability / reliability of the color conversion film; specifically, the edge ingress of the red light-emitting layer is improved (reduced).

[0027] In the context of the present invention, the spacer layer completely or substantially completely covers one surface of the first light-emitting polymer layer. In the field of film production, it is well known that sections of the laminated structure bordering the functional layer are not coated to allow or facilitate production ("spare areas"). Even if such non-coated areas are present, the skilled person will understand that, except for the spare areas, the laminated structure (i.e. the color conversion film) is completely covered by the spacer layer. The area of ​​the spare areas is typically less than 5% of the total area of ​​the laminated structure.

[0028] In the context of the present invention, the spacer layer is arranged between the first and second light-emitting layers. The spacer layer and the light-emitting polymer layer may be in direct contact or separated by one or more non-light-emitting polymer layers.

[0029] In the context of the present invention, a separation layer is a continuous layer. As the term further indicates, the layer is non-porous and defect-free.

[0030] In an advantageous embodiment, the barrier layer provides moisture barrier properties. In an embodiment, the water vapor transmission rate (WVTR) of the barrier layer is less than 10 g / m 2 *Day, preferably less than 1g / m 2 *Day, most preferably less than 0.1g / m 2 * Days. WVTR can be determined according to ISO 15106-3:2003 at a temperature / relative humidity of 40°C / 90% rh.

[0031] In an advantageous embodiment, the separator layer provides oxygen barrier properties. In an embodiment, the oxygen transmission rate (OTR) is less than 100 cm 3 / m 2 *Days, preferably less than 10cm 3 / m 2 *days, preferably less than 1 cm 3 / m 2 *Days, most preferably less than 0.1cm 3 / m 2 * Days. OTR is determined according to ISO 15105 at a temperature of 23°C / 90% rh and atmospheric pressure.

[0032] In an embodiment, the separator contains, i.e. comprises or is composed of a third polymer. Suitable organic materials may be selected from polymers. Suitable polymers may be selected from the following: polyesters, poly(meth)acrylates, polystyrenes, polyolefins, epoxy resins, polyurethanes, polyethylene-vinyl alcohol (EVOH), polyvinylidene chloride (PVDC), polyvinylidene fluoride (PVDF), polyamides (PA), polyacrylonitrile (PAN), polysulfones (PSU), polyethersulfones (PESU). Preferably, the third polymer is selected from polyesters (such as PET) and / or ethylene-vinyl alcohol polymers. Typically, the thickness of the organic separator is 1 micron to 200 microns, preferably 3 microns to 100 microns, more preferably 10 microns to 50 microns. Such a separator is easy to process because it is compatible with the equipment used in industry and is also very attractive from a commercial point of view.

[0033] In an embodiment, the spacer layer comprises sulfur, preferably in the form of thiol functional groups and / or thioether functional groups.

[0034] In an embodiment, the separator layer comprises, preferably consists of, a film laminate in which a film of ethylene vinyl alcohol polymer is sandwiched between two or more layers of other films of different polymers. Such films are commercially available, for example for food packaging, and provide good oxygen barrier properties. In an exemplary embodiment, the film laminate structure containing EVOH polymer is selected from the following list:

[0035] PE (polyethylene) / EVOH / PE,

[0036] PA / EVOH / PE,

[0037] PE / PA / EVOH / PA / PE,

[0038] OPET (oriented PET) / PE / EVOH / PE,

[0039] PS (polystyrene) / EVOH / PE,

[0040] PP (polypropylene) / EVOH / PE,

[0041] PET / EVOH / PE,

[0042] PP / EVOH / PP,

[0043] PC (polycarbonate) / EVOH / PP, and

[0044] ·PET / EVOH / PET.

[0045] In an alternative embodiment, the spacer layer contains, preferably consists of, an inorganic material. Suitable inorganic materials may be selected from the group consisting of metal oxides, metal nitrides, silicon oxides and silicon nitrides. Suitable inorganic materials include, but are not limited to, SiO x (x=1.7-2.3), AlO x (x = 1.3-1.7) and Si x N y (x=3 and y=3.5-4.5). Typically, the thickness of the inorganic spacer layer is 1 nm to 10 micrometers, preferably 10 nm to 1 micrometer. Typically, the thickness of this inorganic layer is more than 10 nanometers. This inorganic spacer layer exhibits gas barrier properties, especially barrier properties to oxygen and water vapor, even at very thin film thicknesses.

[0046] It was found that the optical properties were not negatively affected by the inclusion of one or more of the spacer layers discussed herein. Instead, the stability of the film was improved and the favorable optical properties were retained.

[0047] The first and second set of overlays:

[0048] Adjacent to one or more light emitting polymer layers there may be a covering layer. The first set of covering layers and the second set of covering layers may each independently comprise a single layer or multiple layers, whereby these layers may be inorganic or polymeric and non-emissive (meaning that they do not emit light when excited by blue light). The covering layers may have different functions and may be selected from:

[0049] Barrier film / layer

[0050] Intermediate film / layer

[0051] Adhesive film / layer

[0052] Light management film / layer

[0053] Non-luminescent polymer film / layer

[0054] Barrier film / layer:

[0055] In the context of the present invention, a barrier film exhibits a low permeability to oxygen and / or humidity. Such a barrier film may be selected from a 3 / m 2 *Days, preferably less than 1cm 3 / m 2 *Days, most preferably less than 0.1cm 3 / m 2 * Inorganic barrier film or polymer barrier film with an oxygen transmission rate (OTR) of less than 10 g / m 2 *Day, preferably less than 1g / m 2 *Day, most preferably less than 0.1g / m 2 * Water Vapor Transmission Rate (WVTR) of inorganic or polymeric barrier films. WVTR can be measured according to ISO 15106-3:2003 at a temperature / relative humidity of 40°C / 90% rh.

[0056] The inorganic barrier film comprises or consists of a continuous layer of an inorganic material. Typically, the thickness of the layer is from 1 nm to 10 microns, preferably from 10 nm to 1 micron. Suitable inorganic materials include, but are not limited to, SiO x (x=1.7-2.3), AlO x (x = 1.3-1.7) and Si x N y (x=3 and y=3.5-4.5).

[0057] The polymeric barrier film is composed of a polymer or a polymer blend and typically has a thickness of 5-200 microns, preferably 10-100 microns, most preferably 20-50 microns.

[0058] The inorganic barrier films and polymer barrier films may be commercial items and may be supported by an additional polymer substrate.

[0059] Intermediate film / layer:

[0060] Intermediate layers may be applied in color conversion films to further improve the stability of the color conversion material (typically perovskite crystals), to separate specific layers to avoid contact of these specific layers or to facilitate the manufacture of the color conversion film, for example to reduce manufacturing costs.

[0061] The intermediate layer comprises a polymer or consists of a polymer. Suitable polymers are selected from the group consisting of acrylate or methacrylate polymers, epoxy polymers, silazane polymers, cycloolefin copolymers, polyesters, preferably acrylate polymers or methacrylate polymers.

[0062] In an embodiment, the polymer is cross-linked.

[0063] The thickness of the intermediate layer is 5-100 microns, preferably 10-80 microns, most preferably 20-60 microns.

[0064] Adhesive film / layer:

[0065] Such layers are known in the art and may be included in a color conversion film to improve compatibility between layers, or to improve adhesion between layers, or to facilitate manufacturing.

[0066] Typically, such layers are used on barrier films to improve the adhesion of adjacent polymer layers, such as interlayers or light-emitting polymer layers.

[0067] The thickness of such a layer is typically 0.1 - 20 microns, preferably 0.5 - 10 microns, most preferably 1 - 5 microns.

[0068] In an embodiment, such a layer consists of a polymer or a blend of polymers.

[0069] Typical polymers are selected from the following list: acrylate or methacrylate polymers, epoxy polymers, urethane polymers.

[0070] Light regulating film / layer:

[0071] Light regulating films / layers are sometimes used in color conversion films to, for example, increase the light output of the color conversion film or to reflect a specific portion of the light.

[0072] Light-regulating films include prism films, brightness enhancement films, microlens array (MLA) films (such films are provided, for example, by Brightview Technologies), and blue filter films (also called dichroic mirror films; such films transmit blue light and reflect green and red light; such films are provided by 3M and have been used in Apple iPadPro XDR since 2021).

[0073] MLA films are typically 10–50 microns thick.

[0074] Dichroic mirror films are typically 20–100 microns thick.

[0075] Green light-emitting polymer layer:

[0076] The layer comprises green light-emitting perovskite crystals embedded in a matrix comprising or consisting of a first polymer.

[0077] Perovskite: The green light emitting crystal is a perovskite crystal selected from the compounds of formula (I):

[0078] [M 1 A 1 ] a M 2 b X c (I), wherein:

[0079] A 1 represents one or more organic cations, in particular formamidinium cation (FA),

[0080] M 1 represents one or more alkali metals, in particular Cs,

[0081] M 2 Represents one or more except M 1 Other metals, especially Pb,

[0082] X represents one or more anions selected from the group consisting of halides, pseudohalides and sulfides, in particular Br,

[0083] a represents 1-4, b represents 1-2, c represents 3-9, and

[0084] Among them, M 1 , or A 1 , or M 1 and A 1 Both exist.

[0085] In another advantageous embodiment of the present invention, the green light-emitting crystal is a green light-emitting perovskite crystal of formula (I'):

[0086] FAPbBr3(I').

[0087] In particular, formula (I) describes a perovskite light emitting crystal that, after absorbing blue light, emits light in the green spectrum with a wavelength of 500 nm to 550 nm, particularly light in the green spectrum centered at 525-535 nm.

[0088] First polymer: A wide range of suitable polymers can be selected by routine experimentation. In particular, a suitable first polymer can be selected from acrylates and methacrylates. The first polymer forms a matrix for the perovskite crystals of formula (I).

[0089] Red light-emitting polymer layer:

[0090] The layer comprises red emitting core-shell quantum dots embedded in a matrix comprising or consisting of a second polymer.The layer may additionally comprise one or more sulfur-containing compounds (II) as described below.

[0091] Red QDs: Red core-shell quantum dots are known, which emit red light (630 nm + / - 30 nm) in response to excitation with shorter wavelength light. Suitable crystals are selected from II-VI semiconductor compounds (i.e., containing a metal M with a stable oxidation state of +2). 3 , such as Zn, Cd) and III-V semiconductor compounds (i.e. containing metal M with a stable oxidation state of +3 3 ', for example Y).

[0092] In a preferred embodiment, the red emitting core-shell quantum dots have a core comprising indium or cadmium, most preferably indium.

[0093] In another preferred embodiment, the red emitting core-shell quantum dots have a core comprising indium phosphide or cadmium selenide, most preferably indium phosphide.

[0094] The crystal size of red core-shell quantum dots can vary over a wide range, but is typically 1-10 nm. Such crystals are called quantum dots to distinguish them from microcrystals. For II-VI semiconductor compounds, a suitable range is 1-10 nm, preferably 3-8 nm. For III-V semiconductor compounds, a suitable range is 1-8 nm, preferably 2-4 nm.

[0095] Second polymer: A wide range of polymers can be used. Suitable second polymers can be selected from acrylates, methacrylates, epoxies and carbamates. The second polymer forms a matrix for red luminescent core-shell quantum dots. The second polymer can be partially or completely reacted with polythiol (II) (if present).

[0096] Polythiol: Sulfur-containing compounds have been found to have beneficial effects on the red light-emitting layer. Specifically, the edge intrusion of the layer is improved (i.e. reduced) while maintaining other beneficial optical properties. Given the nature of (II) and the second polymer, a chemical reaction may occur between the two. For example, if the second polymer is an acrylate, the double bonds of the polythiol (II) and the acrylate monomer may form a thiol ether before or during the polymerization of the acrylate monomer. Therefore, within the scope of the present invention, the red light-emitting layer comprises:

[0097] Red QDs and a second polymer as defined herein, but without polythiol (II); or

[0098] Red QDs and a second polymer and polythiol (II), each as defined herein;

[0099] The reaction product of red QDs and a second polymer + polythiol (II), each as defined herein;

[0100] The reaction product of red QDs and a second polymer and polythiol (II) and a second polymer + polythiol (II), each as defined herein;

[0101] The reaction product of red QDs and a second polymer + polythiol (II), each as defined herein;

[0102] • The reaction products of red QDs and a second polymer and a second polymer + polythiol (II), each as defined herein.

[0103] The sulfur-containing compound is a compound of formula (II):

[0104] R 2 (SH) y , (II), where

[0105] R 2 is a (hetero)hydrocarbyl group having a valence of y, and

[0106] y is 2-20, preferably 2-10, for example 4.

[0107] The thiol groups of the polythiol may be primary or secondary, preferably primary. The compound of formula (II) may include a mixture of compounds having two or more average functionalities.

[0108] R 2 Any hydrocarbon group is included, including aliphatic and aromatic polythiols having 2 to 50 carbon atoms.

[0109] R 2Includes (hetero)hydrocarbyl groups, i.e., hydrocarbon groups having 2-50 carbon atoms and also comprising one or more functional groups. Functional groups include pendant hydroxyl, acid, ester or cyano groups or catenary (in-chain) ether, urea, carbamate and ester groups.

[0110] In one embodiment, R 2 Includes non-polymeric aliphatic or alicyclic moieties having from 2 to 30 carbon atoms.

[0111] Specific examples of usable polythiols include 2,3-dimercapto-1-propanol, 2-mercaptoethyl ether, 2-mercaptoethyl sulfide, 1,6-hexanedithiol, 1,8-octanedithiol, 1,8-dimercapto-3,6-dithiooctane, propane-1,2,3-trithiol and trithiocyanic acid.

[0112] Another class of useful polythiols includes those obtained by esterification of a polyol with a terminal thiol-substituted carboxylic acid (or a derivative thereof, such as an ester or acid halide), including an α-mercaptocarboxylic acid or a β-mercaptocarboxylic acid, such as thioglycolic acid, β-mercaptopropionic acid, 2-mercaptobutyric acid or an ester thereof.

[0113] Thus, usable examples of commercially available compounds include: ethylene glycol bis(thioglycolate), pentaerythritol tetrakis(3-mercaptopropionate), dipentaerythritol hexa(3-mercaptopropionate), ethylene glycol bis(3-mercaptopropionate), trimethylolpropane tris(thioglycolate), trimethylolpropane tris(3-mercaptopropionate), pentaerythritol tetrakis(thioglycolate) tetrakis(thioglycolate), pentaerythritol tetrakis(3-mercaptopropionate), pentaerythritol tetrakis(3-mercaptobutyrate) and 1,4-bis(3-mercaptobutylyloxybutane), tris[2-(3-mercaptopropionyloxy]ethyl]isocyanurate, trimethylolpropane tris(thioglycolate), 2,4-bis(mercaptomethyl)-1,3,5-triazine-2,4-dithiol, 2,3-di(2-mercaptoethyl)thio)-1-propanethiol, di-mercaptodiethylsufide and ethoxylated trimethylpropane tris(3-mercaptopropionate) trimethyl-propan-tri(3mercaptopropionate)).

[0114] A specific example of a polymeric polythiol is polypropylene ether glycol bis(3-mercaptopropionate), which is obtained by reacting polypropylene ether glycol (e.g., Pluracol TM P201, BASF Wyandotte Chemical Corp.) and esterification of 3-mercaptopropionic acid.

[0115] Useful soluble high molecular weight mercaptans include polyethylene glycol di(2-mercaptoacetate), LP-3 supplied by Morton Thiokol Inc. (Trenton, NJ). TM Resins and Permapol P3 from Products Research & Chemical Corp. (Glendale, CA) TM Resins and compounds such as adducts of 2-mercaptoethylamine and caprolactam.

[0116] Preferred polythiols include the following pentaerythritol derivatives (II-1) to (II-4):

[0117]

[0118] As described herein, this shall also include the corresponding reaction product with a second polymer.

[0119] Preferred polythiols include the following isocyanurate derivatives (II-5) to (II-7):

[0120]

[0121] In the red light-emitting polymer layer, the sulfur-containing compound is present in the form of having unreacted thiol groups, or in the form of thiol groups that are partially or completely reacted to thioether groups. Such thioether groups can be formed after the sulfur-containing compound (polythiol) is added to the liquid coating formulation of the red light-emitting polymer layer or after UV curing of the red light-emitting polymer layer, when reacting, for example, with alkenyl groups (e.g., acrylate monomers or vinyl monomers).

[0122] In a preferred embodiment, the polythiol comprises 4 valences, ie, y=4, such as pentaerythritol tetrakis(3-mercaptopropionate) (CAS 7575-23-7).

[0123] In a preferred embodiment, the polythiol comprises 4 valences, ie, y=4, such as pentaerythritol tetrakis(3-mercaptopropionate) (CAS 7575-23-7), and is present in the red light-emitting polymer layer at a concentration of 20-50 wt%.

[0124] In an alternative embodiment, R 2 It is polymeric and contains polyoxyalkylene, polyester, polyolefin, polyacrylate or polysiloxane polymers having pendant or terminal reactive -SH groups. Useful polymers include, for example, thiol-terminated polyethylene or polypropylene, thiol-terminated poly(alkylene oxide)s and thiol-terminated polyacrylates.

[0125] The amount of the sulfur-containing compound can vary within wide ranges. The amount can be determined based on the amount of the compound of formula (II) or the sulfur content.

[0126] In an embodiment, in the red light emitting polymer layer, the amount of the compound of formula (II) is 2-50 wt%, preferably 4-40 wt%, most preferably 10-30 wt%.

[0127] In an embodiment, in the red light emitting polymer layer, the sulfur concentration is 0.1-5 wt%, preferably 0.2-2.5 wt%, most preferably 0.5-1.5 wt%.

[0128] The films of the present invention can be made using commercially available starting materials and lamination steps known to the skilled person. The examples provided below illustrate such a manufacturing process.

[0129] Advantageous implementations:

[0130] Preferably, the luminescent crystals (perovskites and core-shell QDs) exhibit a monodisperse size distribution. In the context of the present invention, the term "monodisperse" refers to a population of quantum dots wherein at least about 60% of the population, preferably 75% to 90% of the population, or any integer or non-integer therebetween, falls within a specified particle size range. The diameter deviation of a monodisperse population of particles is less than 20% root mean square (rms), more preferably less than 10% rms, and most preferably less than 5% rms. Particle size and particle size distribution can be determined by microscopy.

[0131] In another advantageous embodiment of the present invention, the green light-emitting polymer layer has 2 The concentration of M in the red light emitting polymer layer is 100-1000ppm, preferably 300-1000ppm, most preferably 500-1000ppm 3 +M 3 'The concentration is greater than 300 ppm, preferably greater than 600 ppm, most preferably greater than 1'200 ppm.

[0132] In another advantageous embodiment, the red core-shell quantum dots have a platelet structure and / or the green perovskite crystals have a cubic structure.

[0133] In another advantageous embodiment of the present invention, the specific size of the red core-shell quantum dots is p 1nm≤s p ≤10nm, especially 3mn≤s p ≤8nm, especially 2nm≤s p ≤6nm, especially 2nm≤s p ≤4nm.

[0134] In another advantageous embodiment, the green light-emitting polymer has a molar ratio z of the sum of (oxygen + nitrogen + sulfur + phosphorus) to carbon, wherein z≤0.9, z≤0.75, in particular z≤0.4, in particular z≤0.3, in particular z≤0.25. The z value is a measure of the polarity of the polymer. A value of z≤0.3 indicates a non-polar polymer. It has been found that the polarity of the polymer affects the performance of the film, and a lower polarity of the polymer of the green light-emitting film can improve the performance. Preferably, the z value z of the polymer in the green light-emitting layer is 绿 Lower than the z value of the polymer in the red emitting layer 红 Preferably, z 绿 :z 红 <1:2; more preferably, z 绿 :z 红 <1:5.

[0135] In another advantageous embodiment, the first polymer and / or the second polymer comprises an acrylate or a methacrylate, in particular wherein the first and / or the second polymer comprises a polycyclic acrylate or a polycyclic methacrylate.

[0136] Suitable polymers for the light-emitting layer ("first polymer" and "second polymer") are known and commercially available. Preferred are UV-curable acrylates or methacrylates with high transparency. Such materials are described, for example, in EP 3753994 B1 (as polymer P1 in sections [0039-0056]), which is incorporated herein by reference.

[0137] In an advantageous embodiment, the first or second polymer comprises an acrylate selected from the group consisting of isobornyl acrylate (CAS 5888-33-5), isobornyl methacrylate (CAS 7534-94-3), dicyclopentyl acrylate (CAS 79637-74-4, FA-513AS (Hitachi Chemical, Japan)), dicyclopentyl methacrylate (CAS 34759-34-7, FA-513M (Hitachi Chemical, Japan)), 3,3,5-trimethylcyclohexyl acrylate (CAS 86178-38-3), 3,3,5-trimethylcyclohexyl methacrylate (CAS 7779-31-9), 4-tert-butylcyclohexyl acrylate (CAS 84100-23-2), 4-tert-butylcyclohexyl methacrylate (CAS 46729-07-1).

[0138] In a further advantageous embodiment, the polymers of the green and / or red emitting polymer layer are crosslinked.

[0139] In another advantageous embodiment, the polymers of the green and / or red light-emitting polymer layer ("first polymer" and "second polymer") comprise multifunctional acrylates.

[0140] structure:

[0141] The membranes of the present invention may be implemented in a variety of different configurations.

[0142] In a first embodiment, in addition to the red and green light emitting polymer layers, the film of the present invention comprises a first inorganic barrier film, a second inorganic barrier film and one or more spacer layers. It should be understood that one or more additional layers may be present, such as an intermediate layer, an adhesive layer or other non-light emitting polymer layer.

[0143] In a second embodiment, in addition to the red and green light emitting polymer layers, the film of the present invention comprises a first inorganic barrier film, a second inorganic barrier film and two inorganic spacer layers between the light emitting layers. It should also be understood that one or more additional layers may be present, such as an intermediate layer, an adhesive layer or other non-light emitting polymer layer.

[0144] In a second embodiment, in addition to the red and green light emitting polymer layers, the film of the present invention comprises a first inorganic barrier film, a second inorganic barrier film and two organic spacer layers between the light emitting layers. It should also be understood that one or more additional layers may be present, such as an intermediate layer, an adhesive layer or other non-light emitting polymer layer.

[0145] In a third embodiment, the film of the present invention comprises multiple layers, whereby there is an intermediate layer between one or more inorganic layers and the green and red light emitting polymer layers. In this embodiment, direct contact of the light emitting polymer layer and the inorganic spacer / barrier layer is avoided by introducing one or more non-light emitting polymer layers (e.g., intermediate layers).

[0146] In another embodiment, the film of the invention comprises the following layer sequence: green emitting polymer layer / spacer layer / red emitting polymer layer.

[0147] In another embodiment, the film of the invention comprises the following layer sequence: intermediate layer / green emitting polymer layer / separating layer / red emitting polymer layer.

[0148] In another embodiment, the film of the invention comprises the following layer sequence: intermediate layer / green emitting polymer layer / intermediate layer / separating layer / red emitting polymer layer.

[0149] In another embodiment, the film of the invention comprises the following layer sequence: intermediate layer / green light-emitting polymer layer / PET separator layer / red light-emitting polymer layer.

[0150] In another embodiment, the film of the present invention comprises the following layer sequence: intermediate layer / green light-emitting polymer layer / PET separator layer / adhesive layer / PET separator layer / red light-emitting polymer layer.

[0151] In another embodiment, the film of the invention comprises the following layer sequence: red emitting polymer layer / spacer layer / green emitting polymer layer / spacer layer / red emitting polymer layer.

[0152] In another embodiment, the film of the invention comprises the following layer sequence: green emitting polymer layer / spacer layer / red emitting polymer layer / spacer layer / green emitting polymer layer.

[0153] In another embodiment, the film of the invention comprises the following layer sequence: green light-emitting polymer layer / spacer layer / red light-emitting polymer layer / dichroic mirror film (blue filter film). Example

[0154] Example 1: Preparation of a color conversion film according to the invention having an inorganic spacer layer between a green-emitting polymer layer and a red-emitting polymer layer.

[0155] Formation of green ink: Green perovskite luminescent crystals with formamidinium lead tribromide (FAPbBr3) components were synthesized in toluene by grinding PbBr2 and FABr. That is, 16 mmol PbBr2 (5.87 g, 98% ABCR, Karlsruhe (Germany)) and 16 mmol FABr (2.00 g, Greatcell Solar Materials, Queanbeyan, (Australia)) were ground together with yttrium stabilized zirconia beads (5 mm in diameter) for 6 hours to obtain pure cubic FAPbBr3 as determined by XRD. Orange FAPbBr3 powder was added to oleylamine (80-90, Acros Organics, Hull (Belgium)) (weight ratio FAPbBr3: oleylamine = 100: 15) and toluene (> 99.5%, extra pure, Sigma Aldrich). The final concentration of FAPbBr3 was 1 wt%. The mixture was then dispersed by ball milling with yttrium stabilized zirconia beads with a diameter of 200 μm under ambient conditions (if not otherwise defined, the atmospheric conditions for all experiments were: 35 ° C, 1 atm, in air) for 1 hour to obtain a green luminescent ink.

[0156] Formation of green light-emitting polymer layer: 0.1 g of green ink was mixed with a UV curable monomer / crosslinker mixture (0.7 g FA-513AS, Hitachi Chemical, Japan / 0.3 g Miramer M240, Miwon, Korea) containing 1 wt% of photoinitiator diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide (TCI Europe, Netherlands) and 2 wt% of polymeric scattering particles (organopolysiloxane, ShinEtsu, KMP-590) in a high-speed mixer and toluene was evaporated by vacuum (<0.01 mbar) at room temperature. The resulting mixture was then coated with a 50 μm layer thickness on a 25 μm barrier film (supplier: I-components (Korea); SiOx layer on PET substrate) on the inorganic layer side and then laminated with a second barrier film of the same type, where the inorganic layer side is adjacent to the green light-emitting polymer layer. Afterwards, the laminate was UV cured for 60 seconds (UVAcube 100 equipped with a mercury lamp and a quartz filter, Höller, Germany). The initial properties of the resulting film showed a green emission wavelength of 526 nm and a FWHM of 22 nm.

[0157] Formation of the red emitting polymer layer: 0.1 g of red emitting crystals (i.e., isometric core-shell QDs with InP core and ZnS shell, 1 wt% suspended in toluene) were mixed with a UV curable monomer / crosslinker mixture (0.5 g FA-DCPA, Hitachi Chemical, Japan / 0.5 g Miramer M2372, Miwon, Korea) containing 1 wt% of the photoinitiator diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide (TCI Europe, Netherlands) and 2 wt% of polymeric scattering particles (organopolysiloxane, Shin-Etsu, KMP-590) in a high-speed mixer and toluene was evaporated by vacuum (<0.01 mbar) at room temperature. The resulting mixture was then coated with a 50 μm layer thickness on the PET side of the barrier film for the green emitting film and then laminated with the same type of barrier film used before, with the inorganic layer on one side adjacent to the red emitting polymer layer. Afterwards, the laminate was UV cured for 60 seconds (UVAcube 100 equipped with a mercury lamp and a quartz filter, Höller, Germany). The initial properties of the resulting film showed a red emission wavelength of 630 nm and a FWHM of 45 nm.

[0158] The color conversion film of Example 1 thus obtained includes an inorganic spacer layer, which is a PET / SiO2 layer used between the green light-emitting polymer layer and the red light-emitting polymer layer. x SiO on barrier film x layer.

[0159] Cut pieces of the color conversion film prepared as described above were tested for 1'000 hours in a climate chamber at 60°C and 90% relative humidity for the stability of the color conversion film of Example 1. The so-called edge intrusion of the green and red light-emitting polymer layers was then measured (edge ​​intrusion refers to the dead edges caused by the degradation of perovskite crystals and / or core-shell quantum dots due to the diffusion of oxygen and / or humidity from the edge of the film to the center of the film).

[0160] Edge intrusion results after 1'000 hours at 60°C / 90% rH:

[0161] -Green edge intrusion: 0.7mm

[0162] -Red edge intrusion: 0.5mm

[0163] These results indicate that a color conversion film can be obtained whereby both the green and red light emitting polymer layers exhibit good resistance to edge intrusion under high temperature / high humidity conditions. The green and red emission wavelengths remain unchanged after the high temperature / high humidity test.

[0164] Example 2: Preparation of a color conversion film according to the invention having an organic spacer layer between a green-emitting polymer layer and a red-emitting polymer layer.

[0165] Formation of green ink: Same steps as in Example 1.

[0166] Formation of the green light-emitting polymer layer: 0.1 g of the green ink was mixed with a UV curable monomer / crosslinker mixture (0.7 g FA-513AS, Hitachi Chemical, Japan / 0.3 g Miramer M240, Miwon, Korea) containing 1 wt% of the photoinitiator diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide (TCI Europe, Netherlands) and 2 wt% of polymeric scattering particles (organopolysiloxane, Shin-Etsu, KMP-590) in a high-speed mixer, and toluene was evaporated by vacuum (<0.01 mbar) at room temperature. The resulting mixture was then coated with a 50 μm layer thickness on a 25 μm barrier film (supplier: Aika (Korea); SiOx layer on PET substrate) on the inorganic layer side and then laminated with a 50 μm PET film (which will eventually become the organic separator layer). Afterwards, the laminated structure was UV-cured for 60 seconds (UVAcube 100 equipped with a mercury lamp and a quartz filter, Hoehler, Germany). The initial performance of the resulting film showed a green emission wavelength of 526 nm and a FWHM of 22 nm.

[0167] Formation of the red emitting polymer layer: 0.1 g of red emitting crystals (i.e., isometric core-shell QDs with InP core and ZnS shell, 1 wt% suspended in toluene) were mixed in a high-speed mixer with a UV curable monomer / crosslinker mixture (0.5 g FA-DCPA, Hitachi Chemical, Japan / 0.5 g Miramer M2372, Miwon, Korea) containing 1 wt% of the photoinitiator diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide (TCI Europe, Netherlands) and 2 wt% of polymeric scattering particles (organopolysiloxane, Shin-Etsu, KMP-590) and toluene was evaporated by vacuum (<0.01 mbar) at room temperature. The resulting mixture was then coated with a 50 μm layer thickness on a PET film of the green emitting film and then laminated with a barrier film of the same type used before, whereby one side of the inorganic layer was adjacent to the red emitting polymer layer. Afterwards, the laminate was UV cured for 60 seconds (UVAcube 100 equipped with a mercury lamp and a quartz filter, Höller, Germany). The initial properties of the resulting film showed a red emission wavelength of 630 nm and a FWHM of 45 nm.

[0168] Cut pieces of the color conversion film prepared as described above were tested for 1'000 hours in a climate chamber at 60°C and 90% relative humidity for the stability of the film according to Example 2. The so-called edge intrusion of the green and red emitting polymer layers was then measured (edge ​​intrusion refers to dead edges caused by degradation of the perovskite crystals and / or core-shell quantum dots due to diffusion of oxygen and / or humidity from the edge of the film to the center of the film).

[0169] Edge intrusion results after 1'000 hours at 60°C / 90% rH:

[0170] -Green edge intrusion: 0.7mm

[0171] -Red edge intrusion: 0.6mm

[0172] These results indicate that a color conversion film can be obtained whereby both the green and red light emitting polymer layers exhibit good resistance to edge intrusion under high temperature / high humidity conditions. The green and red emission wavelengths remain unchanged after the high temperature / high humidity test.

[0173] Example 3: Preparation of a color conversion film according to the invention having an organic spacer layer between a green-emitting polymer layer and a red-emitting polymer layer and a sulfur-containing compound in the red-emitting polymer layer.

[0174] Formation of green ink: Same steps as in Example 1.

[0175] Formation of a green light-emitting polymer layer: the same steps as in Example 2.

[0176] Formation of the red emitting polymer layer: 0.1 g of red emitting crystals (i.e., isometric core-shell QDs with InP core and ZnS shell, 1 wt% suspended in toluene) were mixed with a UV curable monomer / crosslinker mixture (0.5 g FA-DCPA, Hitachi Chemical, Japan / 0.5 g Miramer M2372, Miwon, Korea) containing 25 wt% of pentaerythritol tetrakis(3-mercaptopropionate) (CAS 7575-23-7) from Sigma-Aldrich and 1 wt% of the photoinitiator diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide (TCI Europe, The Netherlands) and 2 wt% of polymeric scattering particles (organopolysiloxane, Shin-Etsu, KMP-590) in a high-speed mixer and toluene was evaporated by vacuum (<0.01 mbar) at room temperature. The resulting mixture was then coated with a 50 micron layer thickness on a PET film of green emitting film and then laminated with a barrier film of the same type used before, whereby one side of the inorganic layer was adjacent to the red emitting polymer layer. The laminated structure was then UV cured for 60 seconds (UVAcube 100 equipped with a mercury lamp and a quartz filter, Höller, Germany). The initial properties of the resulting film showed a red emission wavelength of 630 nm and a FWHM of 45 nm.

[0177] Cut pieces of the color conversion films prepared as described above were tested for film stability for 1'000 hours in a climate chamber at 60°C and 90% relative humidity. The so-called edge intrusion of the green and red emitting polymer layers was then measured (edge ​​intrusion refers to dead edges caused by degradation of perovskite crystals and / or core-shell quantum dots due to diffusion of oxygen and / or humidity from the edge of the film to the center of the film).

[0178] Edge intrusion results after 1'000 hours at 60°C / 90% rH:

[0179] -Green edge intrusion: 0.7mm

[0180] -Red edge intrusion: 0.3mm

[0181] These results show that a color conversion film can be obtained, whereby both the green light-emitting polymer layer and the red light-emitting polymer layer exhibit good resistance to edge intrusion under high temperature / high humidity conditions. The green and red emission wavelengths remain unchanged after the high temperature / high humidity test. Compared with Example 2, the addition of the sulfur-containing compound further improves the red edge intrusion.

[0182] Comparative Example 1: A color conversion film was prepared which did not have a separation layer between the green light-emitting polymer layer and the red light-emitting polymer layer.

[0183] The process is the same as that in the previous embodiment 1, except that the following steps are adjusted:

[0184] - The green light emitting polymer layer is laminated with only one barrier film. The second film used for lamination is a PET film.

[0185] - After UV curing of the green emitting polymer layer, the PET film is removed from the sandwich structure.

[0186] - A red light emitting polymer layer is then formed directly on the green light emitting polymer layer and subsequently laminated with a barrier film prior to UV curing of the red layer.

[0187] The emission wavelengths and FWHM of green and red are the same as in Experiment 1.

[0188] Cut pieces of the prepared quantum dot color conversion film were tested for film stability for 1'000 hours in a climate chamber at 60°C and 90% relative humidity. The edge intrusion of the green and red emitting polymer layers was then measured.

[0189] Edge intrusion results after 1'000 hours at 60°C / 90% rH:

[0190] -Green edge intrusion: 0.7mm

[0191] -Red edge intrusion: 2.0mm

[0192] These results indicate that a color conversion film without a separator layer between the green and red emitting polymer layers results in significant edge intrusion into the red emitting polymer layer.

Claims

1. A color conversion film that emits green light and red light under the stimulation of blue light; the film comprises a plurality of layers, wherein: At least one layer is a green light-emitting layer emitting light at a wavelength of 500 nm to 550 nm, comprising green light-emitting perovskite crystals embedded in a matrix comprising a first polymer; and At least one layer is a red light-emitting polymer layer emitting light at a wavelength of 600 nm to 660 nm, comprising red light-emitting core-shell quantum dots selected from II-VI semiconductor compounds and III-V semiconductor compounds, wherein the red light-emitting core-shell quantum dots are embedded in a matrix comprising a second polymer; and at least one layer is a separation layer that separates the at least one red light emitting polymer layer from the at least one green light emitting polymer layer; Characterized in that the separation layer is a continuous layer covering the entire area between the green light-emitting polymer layer and the red light-emitting polymer layer; and Characterized in that the separation layer contains a third polymer, and the third polymer is selected from polyethylene terephthalate; and The perovskite crystal is selected from the compound of formula (I) [M 1 A 1 ] a M 2 b X c (I), wherein: A 1 represents formamidinium cation (FA), M 1 represents Cs, M 2 represents Pb, X represents one or more anions selected from the group consisting of halides, quasi-halides and sulfides, a represents 1-4, b represents 1-2, c represents 3-9, and Among them, M 1 , or A 1 , or M 1 and A 1 both exist; and wherein the green light-emitting polymer layer has M 2 The concentration is 100-1000ppm.

2. The color conversion film according to claim 1, characterized in that The X represents a Br anion.

3. The color conversion film according to claim 1, characterized in that The separator layer provides oxygen barrier properties, wherein the oxygen transmission rate of the separator layer is less than 100 cm 3 / m 2 *Day, measured according to ISO 15105 at 23°C / 90% relative humidity / atmospheric pressure.

4. The color conversion film of claim 1, wherein The separation layer further comprises an inorganic material; and / or The third polymer includes a sulfur-containing compound.

5. The color conversion film according to claim 1, characterized in that The red light-emitting polymer layer further comprises a sulfur-containing compound defined in formula (II) and / or a reaction product thereof with a monomer of the second polymer: R 2 (SH) y (II) in: R 2 represents a hydrocarbon group having 2-50 carbon atoms and having 2-20 valences, or a heterohydrocarbon group having 2-50 carbon atoms and further containing 1 or more functional groups and having 2-20 valences, and y is 2-20; and Each thiol group in formula (II) is a primary thiol group or a secondary thiol group.

6. The color conversion film of claim 5, wherein The sulfur-containing compound is present in the form of an unreacted polythiol according to formula (II), or The sulfur-containing compound is present in the form of a thioether, thereby forming a covalent bond with the second polymer, or A combination of them. The color conversion film of claim 5 , wherein y represents 4.

8. The color conversion film of claim 5, wherein The concentration of the sulfur-containing compound in the red light-emitting polymer layer is 2-50 wt %; and / or The sulfur concentration in the red light-emitting polymer layer is 0.1-5 wt %.

9. The color conversion film according to claim 5, characterized in that: The perovskite crystal is selected from formamidinium lead bromide (FAPbBr3); and / or The core-shell quantum dots are selected from core-shell quantum dots containing indium.

10. The color conversion film of claim 5, having a total film thickness of 10-500 microns.

11. The color conversion film of claim 1, wherein the second polymer has a polarity less than that of the first polymer, wherein the polarity ratio is given by z 绿 :z 红 <1:2; wherein z is determined by the molar ratio of the sum of oxygen, nitrogen, sulfur and phosphorus to carbon.

12. The color conversion film of claim 1, wherein The first polymer is selected from acrylates or methacrylates; and / or The second polymer is selected from acrylates or methacrylates.

13. The color conversion film of claim 1, wherein The perovskite crystal is selected from formamidinium lead bromide (FAPbBr3); and / or The core-shell quantum dots are selected from core-shell quantum dots containing indium.

14. The color conversion film of claim 1, having a total film thickness of 10-500 microns.

15. The color conversion film of claim 1, wherein the layer sequence is: Green light emitting polymer layer / PET separator layer / red light emitting polymer layer; or Intermediate layer / green light emitting polymer layer / / PET separator layer / red light emitting polymer layer; or Intermediate layer / green light emitting polymer layer / intermediate layer / / PET separator layer / red light emitting polymer layer; or Intermediate layer / green light emitting polymer layer / PET separator layer / red light emitting polymer layer; or Intermediate layer / green light-emitting polymer layer / PET separator layer / adhesive layer / PET separator layer / red light-emitting polymer layer.

16. A display backlight assembly comprising the color conversion film of claim 1.

17. A light emitting device comprising the color conversion film according to claim 1.

18. The light emitting device according to claim 17, which is a liquid crystal display.

19. A display backlight assembly comprising the color conversion film of claim 5.

20. A light emitting device comprising the color conversion film according to claim 5.