A method for reducing medium-low titanium vanadium-titanium magnetite in a hydrogen-based shaft furnace
Through medium and low titanium vanadium titanium magnetite, iron concentrate and titanium concentrate ore combination, combined with oxidized pellet preparation and low-temperature high-temperature reduction, the problem of insufficient reduction performance of vanadium titanium magnetite in hydrogen-based vertical furnaces is solved. It has achieved efficient vanadium titanium ore metallization rate and titanium resource recovery, and enhanced the application value of hydrogen-based vertical furnaces.
Patent Information
- Application Number
- CN202411109782.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-14
AI Technical Summary
When reducing medium and low titanium vanadium titanium magnetite in hydrogen-based vertical furnace, there are problems such as low strength, poor low-temperature reduction and powdering effect, slow reduction rate and low metallization rate, which is difficult to meet the needs of hydrogen-based vertical furnace production. Titanium resource recovery rate is low and economic benefits are insufficient.
Using medium and low titanium vanadium titanium magnetite, iron concentrate and titanium concentrate ore combination, the compressive strength and powdering performance of the pellet are optimized to meet the hydrogen-based vertical The furnace production standard provides vanadium titanium ore metallized pellets with metallization rate greater than 85%.
The reduction behavior of medium and low titanium vanadium titanium magnetite is improved and the hydrogen-based vertical furnace production standards are met. The obtained vanadium titanium ore metallized pellets are suitable for electric furnace production, improving the recovery rate and economic benefits of titanium resources.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of iron and steel metallurgy, and in particular to a method for reducing medium-low titanium type vanadium-titanium magnetite in a hydrogen-based vertical furnace. Background Art
[0002] The steel industry has huge carbon emissions, which has seriously affected the progress of carbon emission reduction in my country. The blast furnace process is mainly based on carbon reduction, which causes a large amount of carbon emissions. Therefore, if the hydrogen-based vertical furnace short-process process with hydrogen as the main reducing gas replaces the blast furnace ironmaking process, carbon emissions can be effectively reduced. At present, the output of direct reduced iron (DRI) products produced by hydrogen-based vertical furnaces at home and abroad is increasing year by year, and the construction volume and production capacity of hydrogen-based vertical furnace devices are also gradually increasing. For example, Zhongjin Taihang, Hesteel Group, and Baowu Group have completed the construction of hydrogen-based vertical furnaces and officially put them into production. The problems with the large-scale promotion of hydrogen-based vertical furnaces mainly include high hydrogen costs and high prices of high-grade ore raw materials.
[0003] my country has rich mineral resources, especially vanadium-titanium ore resources, which are widely distributed. my country's vanadium resources are widely distributed in 19 provinces, cities and regions, but are mainly concentrated in Panzhihua, Sichuan and Chengde, Hebei. The use of vanadium-titanium ore resources to prepare oxidized pellets and reduce them in a hydrogen-based vertical furnace to obtain vanadium-titanium ore metallized pellets can not only utilize the iron in the vanadium-titanium ore resources, but also obtain vanadium, titanium and chromium resources, thereby improving the promotion and application value of the hydrogen-based vertical furnace short-process technology. However, due to the low strength of vanadium-titanium ore pellets, poor low-temperature reduction and pulverization effect, slow reduction rate, and low metallization rate of reduced products, it is difficult to meet the production and application of hydrogen-based vertical furnaces. At the same time, for medium and low titanium vanadium-titanium ore resources, the titanium resource recovery rate of the obtained vanadium-titanium ore metallized pellets after refining in an electric furnace is low, and the economic benefits are insufficient, which also hinders the application of vanadium-titanium ore resources in hydrogen-based vertical furnace production. Summary of the invention
[0004] The present invention aims to solve at least one of the technical problems existing in the prior art or related art.
[0005] To this end, the present invention provides a method for reducing medium-low titanium type vanadium-titanium magnetite in a hydrogen-based vertical furnace, comprising:
[0006] Preparation of oxidized pellets: blending medium-low titanium vanadium-titanium magnetite, iron concentrate and titanium concentrate, and mixing with a binder to form pellets, and then oxidizing and roasting to obtain oxidized pellets, wherein the compressive strength of the oxidized pellets is greater than 2000N / piece;
[0007] Low temperature reduction, reducing the oxidized pellets in a hydrogen-based vertical furnace under low temperature conditions to obtain a low temperature reduction product; the low temperature reduction product meets the following requirements: low temperature reduction pulverization performance LTD +6.3 >80%, low temperature reduction powdering performance LTD -3.2 <10% and low temperature reduction powdering performance LTD up>60%;
[0008] High-temperature reduction, reducing the low-temperature reduction product in a hydrogen-based vertical furnace under high-temperature conditions to obtain vanadium-titanium ore metallized pellets; the vanadium-titanium ore metallized pellets meet the following conditions: reduction expansion rate <15%, reduction adhesion index <20% and metallization rate >85%.
[0009] Furthermore, the medium-low titanium vanadium-titanium magnetite, the iron concentrate and the titanium concentrate are blended in a mass ratio of 38-42:47-52:9-11.
[0010] Furthermore, the medium-low titanium vanadium-titanium magnetite has a total iron content of not less than 60%, a TiO2 content of 4% to 8%, a Cr2O3 content of 0.5% to 1%, and a V2O5 content of 0.5% to 1%, calculated by mass fraction.
[0011] Furthermore, the iron concentrate has a total iron content higher than 67% by mass.
[0012] Furthermore, the titanium concentrate has a TiO2 content of 45% to 48% by mass.
[0013] Furthermore, the low-temperature reduction is carried out at a temperature of 470°C to 520°C and a time of 110 min to 130 min.
[0014] Furthermore, the high temperature reduction is carried out at a temperature of 980°C to 1020°C and a time of 100 min to 150 min.
[0015] Furthermore, the low-temperature reduction and the high-temperature reduction are both carried out under the condition of hydrogen-rich reducing gas, and the hydrogen-rich reducing gas includes: H2, CO, N2 and CO2, and the volume satisfies: H2+CO≥75%, H2 / CO≥4, 2%≤CO2≤5%.
[0016] Furthermore, the mass ratio of the sum of the mass of the medium-low titanium vanadium-titanium magnetite, the iron concentrate and the titanium concentrate to the mass ratio of the binder is 98.5%~99.3%:0.7%~1.5%.
[0017] Furthermore, the vanadium-titanium ore metallized pellets are suitable for electric furnace production, with a TiO2 mass fraction greater than 9%, and high-quality pig iron and high-titanium slag system can be obtained after electric furnace refining.
[0018] Compared with the prior art, the present invention has at least the following beneficial effects:
[0019] The method for reducing medium-low titanium vanadium-titanium magnetite in a hydrogen-based vertical furnace provided by the present invention makes the reduction behavior of the medium-low titanium vanadium-titanium magnetite meet the production standard of the hydrogen-based vertical furnace by blending the medium-low titanium vanadium-titanium magnetite, iron concentrate and titanium concentrate, and combining low-temperature reduction with high-temperature reduction; the obtained vanadium-titanium ore metallized pellets have a metallization rate of more than 85% and are suitable for electric furnace production. DETAILED DESCRIPTION
[0020] In order to better understand the above technical solution, the technical solution of the present application is described in detail below through specific embodiments.
[0021] The embodiment of the present invention provides a method for reducing medium-low titanium type vanadium-titanium magnetite in a hydrogen-based vertical furnace, comprising:
[0022] Preparation of oxidized pellets: blending medium-low titanium vanadium-titanium magnetite, iron concentrate and titanium concentrate, and mixing with a binder to form pellets, and then oxidizing and roasting to obtain oxidized pellets, wherein the compressive strength of the oxidized pellets is greater than 2000N / piece;
[0023] Low temperature reduction, reducing the oxidized pellets in a hydrogen-based vertical furnace under low temperature conditions to obtain a low temperature reduction product; the low temperature reduction product meets the following requirements: low temperature reduction pulverization performance LTD +6.3 >80%, low temperature reduction powdering performance LTD -3.2 <10% and low temperature reduction powdering performance LTD up >60%;
[0024] High-temperature reduction, reducing the low-temperature reduction product in a hydrogen-based vertical furnace under high-temperature conditions to obtain vanadium-titanium ore metallized pellets; the vanadium-titanium ore metallized pellets meet the following conditions: reduction expansion rate <15%, reduction adhesion index <20% and metallization rate >85%.
[0025] The method for reducing medium-low titanium vanadium-titanium magnetite in a hydrogen-based vertical furnace provided in an embodiment of the present invention can obtain vanadium-titanium ore pellets whose low-temperature reduction pulverization performance and reduction performance meet the standards of hydrogen-based vertical furnaces through the improvement of the reduction method, thereby solving the difficulty that my country's medium-low titanium vanadium-titanium magnetite resources are difficult to apply to hydrogen-based vertical furnace production.
[0026] Specifically, by combining low- and medium-titanium vanadium-titanium magnetite, iron concentrate and titanium concentrate, and combining low-temperature reduction with high-temperature reduction, the reduction behavior of medium- and low-titanium vanadium-titanium magnetite meets the production standards of hydrogen-based shaft furnaces; the obtained vanadium-titanium ore metallization pellets have a metallization rate of more than 85%, which is suitable for electric furnace production. Among them, the low-temperature reduction pulverization performance LTD -3.2 It refers to the mass proportion of particles with a particle size less than 3.2 mm after the pulverization test. Low temperature reduction pulverization performance LTD +6.3 Refers to the mass proportion of particles with a particle size greater than 6.3 mm after the pulverization experiment.UP It refers to the proportion of unbroken pellets to the total number of pellets after the pulverization experiment. The calculation process of the reduction bonding index is as follows: weigh the mass of the charge that is bonded together after reduction as M0, then drop it from a height of 1m, weigh the mass of the charge that is still bonded after falling as Mi, the number of drops ranges from 1 to 20 times, and the ratio of Mi to M0 obtained each time is the bonding rate. Draw a curve with the bonding rate as the ordinate and the number of drops as the abscissa, and calculate the area under the curve as the bonding index.
[0027] In a feasible implementation manner, the medium-low titanium vanadium-titanium magnetite, the iron concentrate and the titanium concentrate are blended in a mass ratio of 38-42:47-52:9-11.
[0028] Specifically, in order to improve the reduction performance of vanadium-titanium ore resources in a hydrogen-based vertical furnace, especially the low-temperature reduction pulverization performance, it is usually adopted to increase the preheating temperature of oxidative roasting to increase the pellet strength to improve the low-temperature reduction pulverization performance, but for medium-low titanium vanadium-titanium magnetite resources, its low-temperature reduction pulverization performance is difficult to improve, and at the same time, the recovery of titanium resources is difficult to meet the high-efficiency recovery of hydrogen-based vertical furnaces. Therefore, the present invention develops a method for reducing medium-low titanium vanadium-titanium ore resources in a hydrogen-based vertical furnace, and the medium-low titanium vanadium-titanium magnetite is blended. The addition of iron concentrate can improve the reduction performance of vanadium-titanium ore pellets, and the addition of a small amount of titanium concentrate can increase the titanium content in the vanadium-titanium ore pellets. This not only ensures that the medium-low titanium vanadium-titanium ore pellets can be used smoothly in the hydrogen-based vertical furnace, but also ensures the content of TiO2 in the reduced product, and realizes the clean and efficient use of medium-low titanium vanadium-titanium magnetite in the hydrogen-based vertical furnace. Regarding the addition amount of iron concentrate and titanium concentrate, the inventors concluded through many experiments that a mass ratio of 38~42:47~52:9~11 for medium-low titanium vanadium-titanium magnetite, iron concentrate and titanium concentrate can ensure smooth reduction of medium-low titanium vanadium-titanium magnetite in a hydrogen-based vertical furnace, and the TiO2 content of the reduction product meets the electric furnace smelting effect.
[0029] In a feasible implementation, the medium-low titanium vanadium-titanium magnetite has a total iron content of not less than 60%, a TiO2 content of 4% to 8%, a Cr2O3 content of 0.5% to 1%, and a V2O5 content of 0.5% to 1%. The total iron content of the iron concentrate is higher than 67% by mass. The TiO2 content of the titanium concentrate is 45% to 48% by mass.
[0030] It is understandable that for vanadium-titanium magnetite, the lower the titanium content, the greater the impact on the strength and pulverization of the oxidized pellets, which will destroy the degree of hematite crystallization inside the pellets. When the titanium content increases, the titanium hematite will be mutually crystallized after FeTiO3 oxidation, and the degree of crystallization will increase. The pulverization performance will improve after the strength of the oxidized pellets increases. Vanadium-titanium magnetite with a Cr2O3 mass fraction greater than 0.3% is a high-chromium vanadium-titanium magnetite. Low-temperature reduction pulverization index LTD of the pellets after low-temperature reduction +6.3 As the Cr2O3 content increases, the LTD of the reduced pellets decreases. -3.2 It increases with the increase of Cr2O3 content. With the increase of Cr2O3 content, the FeCr2O4 generated by reduction will aggregate, resulting in increased porosity, improved kinetic conditions, and increased reduction efficiency, but increased reduction stress, which aggravates the pulverization of pellets. With the increase of Cr2O3 content, the compressive strength decreases, and the plasticity of the pellets decreases. The ability of the pellets to resist internal stress and crack expansion becomes worse, which eventually leads to the aggravation of the pulverization of pellets. In general, the low titanium content and high chromium content interact with each other to affect the low-temperature reduction pulverization performance of the pellets. Therefore, it is necessary to consider the ore blending to optimize the low-temperature reduction pulverization performance of the pellets.
[0031] Specifically, the inventors optimized the blending of medium- and low-titanium vanadium-titanium magnetite, iron concentrate and titanium concentrate. Among them, the high-grade iron concentrate with a total iron mass fraction of more than 67% has stable metallurgical properties, which can improve the low-temperature reduction pulverization performance and reduction performance of the pellets. The TiO2 mass fraction of the titanium concentrate is 45%~48%, which is used to increase the TiO2 content in the mixed ore.
[0032] In a feasible implementation manner, the low-temperature reduction is carried out at a temperature of 470° C. to 520° C. and for a time of 110 min to 130 min.
[0033] Specifically, the upper part of the hydrogen-based vertical furnace is the low-temperature section. The charge descends from the upper part and passes through the low-temperature section first. The reduction temperature of the low-temperature section is controlled to be 470℃~520℃, and the time is 110min~130min. The low-temperature reduction pulverization performance is required to obtain a low-temperature reduction product that meets the hydrogen-based vertical furnace standard. If the pulverization performance is poor, it will cause uneven airflow distribution in the furnace, affecting smooth production.
[0034] In a feasible implementation manner, the high temperature reduction is carried out at a temperature of 980° C. to 1020° C. and a time of 100 min to 150 min.
[0035] The experiment found that the higher the high-temperature reduction temperature, the higher the bonding index and expansion rate of the obtained vanadium-titanium ore pellets, and the lower the high-temperature reduction temperature, the lower the metallization rate of the vanadium-titanium ore pellets. By controlling the high-temperature reduction temperature, the bonding index, expansion rate and metallization rate of the vanadium-titanium ore pellets after high-temperature reduction can be balanced. The high-temperature reduction temperature is controlled at 980℃~1020℃, so that the metallization rate of the vanadium-titanium ore pellets is greater than 85%, the reduction expansion rate is less than 12%, and the bonding index is less than 20%.
[0036] In a feasible implementation manner, both the low-temperature reduction and the high-temperature reduction are carried out under hydrogen-rich reducing gas conditions; the hydrogen-rich reducing gas includes: H2, CO, N2 and CO2, and the volume satisfies: H2+CO≥75%, H2 / CO≥4, 2%≤CO2≤5%.
[0037] Specifically, we studied the metallurgical properties of medium and low titanium vanadium-titanium magnetite under different atmospheres. When the H2 / CO ratio was lower than 4, the low-temperature reduction pulverization performance deteriorated; when the CO2 volume exceeded 5%, although the low-temperature reduction pulverization performance was excellent, the metallization rate was low; and when the H2+CO ratio was less than 75%, the metallization rate was significantly low; therefore, the reducing gases include: H2, CO, N2 and CO2, and the volumes satisfy: H2+CO≥75%, H2 / CO≥4, 2%≤CO2≤5%.
[0038] In addition, reducing vanadium-titanium ore pellets under reducing gas conditions with a high hydrogen-carbon ratio is not only beneficial to improving the reduction performance of vanadium-titanium ore pellets, but also can further reduce carbon emissions in the steel industry, providing assistance for my country's carbon peak and carbon neutrality goals.
[0039] In a feasible implementation, the mass ratio of the sum of the mass of the medium-low titanium vanadium-titanium magnetite, the iron concentrate and the titanium concentrate to the mass of the binder is 98.5%-99.3%:0.7%-1.5%. The binder can be bentonite.
[0040] In a feasible implementation, the vanadium-titanium ore metallized pellets are suitable for electric furnace production, with a TiO2 mass fraction greater than 9%, and high-quality pig iron and high-titanium slag system are obtained after electric furnace refining.
[0041] Specifically, by optimizing the ore blending and adjusting the reduction method, the vanadium-titanium ore metallized hot pellets are taken out from the hydrogen-based vertical furnace after high-temperature reduction, placed in a closed container, and cooled to room temperature by passing argon gas, to obtain vanadium-titanium ore metallized pellets with a metallization rate greater than 85% and a TiO2 mass fraction greater than 9%. The vanadium-titanium ore metallized pellets are refined in an electric furnace to obtain high-quality pig iron and high-titanium slag system, which increases the added value of hydrogen-based vertical furnace short-process products and improves the competitiveness of hydrogen-based vertical furnaces. It is suitable for electric furnace production.
[0042] In summary, the strength of the vanadium-titanium ore oxide pellets produced by the method of the embodiment of the present invention is 2750~2950N / piece, and the particle size is 8~14 mm, which can meet the hydrogen-based vertical furnace production standards. At the same time, the metallization rate of the produced vanadium-titanium ore metallized pellets is greater than 85%, and TiO2 is greater than 9%. The vanadium-titanium ore metallized pellets produced by this method can provide high-quality raw materials for the electric furnace refining process, produce high-quality pig iron and titanium, vanadium and chromium resources, and provide a process for the efficient and clean application of vanadium-titanium ore resources in my country and the acquisition of high-quality direct reduced iron products.
[0043] Example 1 A method for reducing medium-low titanium vanadium-titanium magnetite in a hydrogen-based shaft furnace
[0044] The chemical compositions of the medium-low titanium vanadium-titanium magnetite, iron concentrate and titanium concentrate of Example 1 are shown in Table 1.
[0045] Table 1 Main chemical composition of vanadium-titanium magnetite, wt / %
[0046]
[0047] A method for reducing medium-low titanium vanadium-titanium magnetite in a hydrogen-based shaft furnace specifically comprises the following steps:
[0048] (1) Preparation of oxidized pellets: medium-low titanium vanadium-titanium magnetite, iron concentrate and titanium concentrate are mixed in a mass ratio of 40:50:10 and fully mixed with a binder to form pellets. After pelletizing, the pellets are preheated at 925°C for 15 min and oxidized and roasted at 1290°C for 30 min to obtain vanadium-titanium ore oxidized pellets with an average compressive strength of 2853 N / piece. The compressive strength of the vanadium-titanium ore oxidized pellets meets the standard of greater than 2000 N / piece for vertical furnace production.
[0049] (2) Low-temperature reduction: the vanadium-titanium ore oxide pellets are placed in a hydrogen-based vertical furnace. Under the conditions of hydrogen-rich reducing gas composition and volume ratio of H265%, CO13%, CO24% and N218%, the temperature is 500℃, and the reduction time is 120min. The low-temperature reduction product obtained meets the low-temperature reduction pulverization standard (low-temperature reduction pulverization performance LTD +6.3 >80%, low temperature reduction powdering performance LTD -3.2 <10% and low temperature reduction powdering performance LTD up >60%).
[0050] (3) High-temperature reduction: The low-temperature reduction product is reduced in the reduction section of a hydrogen-based vertical furnace. Under the conditions of a hydrogen-rich reducing gas composition and a volume ratio of H265%, CO13%, CO24% and N218%, a temperature of 1000°C and a reduction time of 125 min, the obtained vanadium-titanium ore metallized pellets meet the hydrogen-based vertical furnace production standards (reduction expansion rate <15%, reduction adhesion index <20% and metallization rate greater than 85%).
[0051] Example 2
[0052] The difference between Example 2 and Example 1 is that the medium-low titanium vanadium-titanium magnetite, iron concentrate and titanium concentrate are blended in a mass ratio of 38:51:11.
[0053] Example 3
[0054] The difference between Example 3 and Example 1 is that the medium-low titanium vanadium-titanium magnetite, iron concentrate and titanium concentrate are blended in a mass ratio of 42:49:9.
[0055] Example 4
[0056] The difference between Example 4 and Example 1 is that the high-temperature reduction temperature is 980° C. and the reduction time is 140 min.
[0057] Example 5
[0058] The difference between Example 5 and Example 1 is that the high-temperature reduction temperature is 102° C. and the reduction time is 105 min.
[0059] Comparative Example 1
[0060] The chemical composition of the medium-low titanium vanadium-titanium magnetite in Comparative Example 1 is the same as that in Example 1.
[0061] The difference between Comparative Example 1 and Example 1 is that in the preparation of oxidized pellets, the medium-low titanium vanadium-titanium magnetite is not blended with the binder to form pellets.
[0062] Comparative Example 2
[0063] The chemical composition of the medium-low titanium vanadium-titanium magnetite and iron concentrate in Comparative Example 2 is the same as that in Example 1.
[0064] The difference between Comparative Example 2 and Example 1 is that in the preparation of oxidized pellets, medium-low titanium vanadium-titanium magnetite and iron ore concentrate are fully mixed with a binder to form pellets.
[0065] Comparative Example 3
[0066] The difference between Comparative Example 3 and Example 1 is that the reducing gas components have different volumes. The reducing gas components of Comparative Example 3 have volumes of H2=50%, CO=28%, CO2=4%, and N2=18%.
[0067] Comparative Example 4
[0068] The difference between Comparative Example 4 and Example 1 is that the reducing gas components have different volumes. The reducing gas components of Comparative Example 4 have volumes of H2=65%, CO=13%, CO2=8%, and N2=14%.
[0069] Comparative Example 5
[0070] The difference between Comparative Example 5 and Example 1 is that the reducing gas components have different volumes. The reducing gas components of Comparative Example 5 have volumes of: H2=60%, CO=13%, CO2=4%, and N2=23%.
[0071] Comparative Example 6
[0072] The difference between Comparative Example 6 and Example 1 is that the reducing gas components have different volumes. The reducing gas components of Comparative Example 6 have volumes of: H2=55%, CO=7%, CO2=5%, and N2=33%.
[0073] Comparative Example 7
[0074] The difference between Comparative Example 7 and Example 1 is that the high-temperature reduction temperature is different, and the high-temperature reduction temperature of Comparative Example 7 is 950°C.
[0075] Comparative Example 8
[0076] The difference between Comparative Example 8 and Example 1 is that the high-temperature reduction temperature is different, and the high-temperature reduction temperature of Comparative Example 8 is 1050°C.
[0077] Results and Discussion
[0078] The metallurgical properties of the vanadium-titanium ore pellets prepared in Examples 1 to 5 and Comparative Examples 1 to 8 are shown in Table 2, Table 3 and Table 4.
[0079] Table 2 Metallurgical properties of vanadium-titanium ore pellets prepared in Example 1 and Comparative Examples 1-2
[0080]
[0081] Table 3 Metallurgical properties of vanadium-titanium ore pellets under different reducing atmospheres
[0082]
[0083] Table 4 Metallurgical properties of vanadium-titanium ore pellets at different reduction temperatures
[0084]
[0085] It can be seen from Examples 1 to 5 that the process parameters such as the ore proportion, reducing atmosphere and high-temperature reduction temperature are within a reasonable range, which can simultaneously ensure the pellet strength, metallurgical properties and TiO2 content in the metallized pellets.
[0086] It can be seen from Comparative Example 1 that when all medium-low titanium vanadium-titanium magnetite is used, the pellet strength is 2276 N / piece, and the low-temperature reduction powder index LTD +6.3 =30.94%,LTD -3.2 =63.95%,LTD UP=28.10%, the low temperature reduction pulverization performance is difficult to meet the production needs.
[0087] From Comparative Example 2, it can be seen that when the ore ratio is 50% medium-low titanium vanadium-titanium ore and 50% iron concentrate, the pellet strength is 3223 N / piece, and the low-temperature reduction powder index LTD +6.3 =90.31%,LTD -3.2 =9.69%,LTD UP =98.39%, the metallization rate is 88.94%, and other reduction indicators can also meet the requirements of the hydrogen-based vertical furnace. However, after the addition of high-grade ore, the TiO2 content of the vanadium-titanium ore metallized pellets is only 6.53%, which affects the subsequent electric furnace smelting effect.
[0088] It can be seen from Comparative Examples 3 to 6 that we studied the metallurgical properties of medium and low titanium vanadium-titanium magnetite under different reducing atmospheres. After reducing the H2 / CO ratio, the low-temperature reduction pulverization performance deteriorated. When the CO2 ratio was 8%, although the low-temperature reduction pulverization performance was excellent, the metallization rate was low. When the H2+CO ratio was less than 75%, the metallization rate was obviously low and could not meet the production needs.
[0089] It can be seen from Example 1, Example 4, Example 5 and Comparative Examples 7 and 8 that we compared the metallurgical properties of vanadium-titanium ore pellets at different high-temperature reduction temperatures. The low-temperature reduction temperature was 500°C, while the metallization rate of the vanadium-titanium ore pellets at high-temperature reduction at 950°C was only 82.37%. After the high-temperature reduction temperature was increased to 1050°C, the metallization rate increased to 90.41%, but the bonding index reached 37.27%, which was difficult to meet the hydrogen-based vertical furnace production standards.
[0090] It is easy for those skilled in the art to understand that, under the premise of no conflict, the above-mentioned advantageous methods can be freely combined and superimposed. The above are only preferred embodiments of the present application and are not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application. The above are only preferred implementation methods of the present application. It should be pointed out that for ordinary technicians in this technical field, several improvements and variations can be made without departing from the technical principles of the present application, and these improvements and variations should also be regarded as the protection scope of the present application.
Claims
1. A method for reducing medium-low titanium vanadium-titanium magnetite in a hydrogen-based shaft furnace, characterized in that: include: Preparation of oxidized pellets: blending medium-low titanium vanadium-titanium magnetite, iron concentrate and titanium concentrate, and mixing with a binder to form pellets, and then oxidizing and roasting to obtain oxidized pellets, wherein the compressive strength of the oxidized pellets is greater than 2000N / piece; Low-temperature reduction, reducing the oxidized pellets in a hydrogen-based vertical furnace under low-temperature conditions to obtain a low-temperature reduced product; The low temperature reduction product meets the following requirements: low temperature reduction pulverization performance LTD +6.3 >80%, low temperature reduction powdering performance LTD -3.2 <10% and low temperature reduction powdering performance LTD up >60%; High-temperature reduction, reducing the low-temperature reduction product in a hydrogen-based vertical furnace under high-temperature conditions to obtain vanadium-titanium ore metallized pellets; the vanadium-titanium ore metallized pellets meet the following conditions: reduction expansion rate <15%, reduction bonding index <20% and metallization rate >85%; The medium-low titanium vanadium-titanium magnetite, the iron concentrate and the titanium concentrate are blended in a mass ratio of 38-42:47-52:9-11; The low temperature reduction is performed at a temperature of 470°C to 520°C and a time of 110min to 130min; The high temperature reduction is carried out at a temperature of 980°C to 1020°C and a time of 100 min to 150 min; The low-temperature reduction and the high-temperature reduction are both carried out under the condition of hydrogen-rich reducing gas; the hydrogen-rich reducing gas includes: H2, CO, N2 and CO2, and the volume satisfies: H2+CO≥75%, H2 / CO≥4, 2%≤CO2≤5%.
2. The method for reducing medium-low titanium vanadium-titanium magnetite in a hydrogen-based shaft furnace according to claim 1, characterized in that: The medium-low titanium vanadium-titanium magnetite has a total iron content of not less than 60%, a TiO2 content of 4% to 8%, a Cr2O3 content of 0.5% to 1%, and a V2O5 content of 0.5% to 1%, calculated by mass fraction.
3. The method for reducing medium-low titanium vanadium-titanium magnetite in a hydrogen-based shaft furnace according to claim 2, characterized in that: The iron concentrate has a total iron content of higher than 67% by mass.
4. The method for reducing medium-low titanium vanadium-titanium magnetite in a hydrogen-based vertical furnace according to claim 3, characterized in that: The titanium concentrate has a TiO2 content of 45% to 48% by mass.
5. The method for reducing medium-low titanium vanadium-titanium magnetite in a hydrogen-based vertical furnace according to claim 1, characterized in that: The mass ratio of the sum of the mass of the medium-low titanium vanadium-titanium magnetite, the iron concentrate and the titanium concentrate to the mass ratio of the binder is 98.5%~99.3%:0.7%~1.5%.
6. The method for reducing medium-low titanium vanadium-titanium magnetite in a hydrogen-based vertical furnace according to claim 4, characterized in that: The vanadium-titanium ore metallized pellets are suitable for electric furnace production, with a TiO2 mass fraction greater than 9%. After being refined in an electric furnace, high-quality pig iron and a high-titanium slag system are obtained.