Optical glass, optical element and optical instrument

By adjusting the composition ratio of optical glass, especially controlling the content of SiO2, TiO2, Na2O, etc., the problem of crystallization in optical glass during precision molding was solved, and optical glass with high refractive index and high Abbe number was made to have excellent anti-crystallization performance.

CN118930039APending Publication Date: 2024-11-12CDGM OPTICAL GLASS

Patent Information

Application Number
CN202411128061.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing optical glass is prone to crystallization during precision molding, which leads to a decline in quality. In particular, optical glass with a refractive index of 1.65 to 1.72 and an Abbe number of 27 to 34 has poor resistance to crystallization.

Method used

By adjusting the composition ratio of optical glass, including the content of SiO2, TiO2, Na2O, K2O, etc., and controlling (SiO2+ZrO2)/TiO2 to be 1.0 to 2.2, the composition ratio is optimized to ensure that the glass does not crystallize below 980℃, while maintaining a refractive index of 1.65 to 1.72 and an Abbe number of 27 to 34.

Benefits of technology

This technology significantly improves the anti-crystallization properties of optical glass while maintaining high refractive index and high Abbe number, thereby enhancing the quality and production efficiency of optical glass.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004997045910000131
    Figure BDA0004997045910000131
  • Figure BDA0004997045910000151
    Figure BDA0004997045910000151
  • Figure BDA0004997045910000161
    Figure BDA0004997045910000161
Patent Text Reader

Abstract

The invention provides optical glass, which comprises the following components in percentage by weight: 36 to 49 percent of SiO2; 21 to 37 percent of TiO2; 6 to 20 percent of Na2O; 3%-15% of K2O; zrO2: 0-5%, wherein the ratio of (SiO2 + ZrO2) / TiO2 is 1.0-2.2. Through reasonable component design, the optical glass obtained by the invention has an expected refractive index and Abbe number, and also has excellent devitrification resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to optical glass, in particular to optical glass with excellent anti-crystallization performance. Background Art

[0002] In recent years, with the advancement of science and technology, the continuous updating of optoelectronic information products, the demand for optical glass has gradually increased, and at the same time, higher requirements have been put forward for the performance of optical glass. At present, the mainstream method of manufacturing optical glass into optical components is precision molding (including direct molding and secondary molding). The use of precision molding technology to manufacture optical components reduces the consumption of raw materials, reduces the cost of manpower and material resources, and reduces environmental pollution. This technology can produce optical components in large quantities at low cost. The so-called precision molding is to mold glass preforms with high-precision molds with a predetermined product shape under a certain temperature and pressure, so as to obtain glass products with the final product shape and optical functions. Various optical glass products can be manufactured through precision molding technology, such as spherical lenses, aspherical lenses, prisms and diffraction gratings.

[0003] In the prior art, optical glasses with a refractive index of 1.65 to 1.72 and an Abbe number of 27 to 34 generally have poor anti-crystallization performance. For example, Chinese patent CN114599617A discloses an optical glass with a refractive index of 1.70000 to 1.80000 and an Abbe number of 30.00 to 40.00, which has a high liquidus temperature. During the production process of the optical glass or the process of manufacturing optical elements by a precision molding method, crystallization is easily generated in the optical glass, resulting in a decrease in the quality of the optical glass or even scrapping. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide an optical glass with excellent anti-crystallization performance.

[0005] The technical solution adopted by the present invention to solve the technical problem is:

[0006] (1) Optical glass, the components of which, expressed in weight percentage, contain: SiO2: 36-49%; TiO2: 21-37%; Na2O: 6-20%; K2O: 3-15%; ZrO2: 0-5%, wherein (SiO2+ZrO2) / TiO2 is 1.0-2.2.

[0007] (2) The optical glass according to (1), wherein the components, expressed in weight percentage, further contain: BaO: 0-10%; and / or Li2O: 0-8%; and / or ZnO: 0-10%; and / or SrO: 0-5%; and / or CaO: 0-5%; and / or MgO: 0-5%; and / or B2O3: 0-4%; and / or Ln2O3: 0-4%; and / or Nb2O5: 0-4%; and / or WO3: 0-4%; and / or Al2O3: 0-4%; and / or P2O5: 0-4%; and / or clarifier: 0-1%; and / or F: 0-3%, wherein Ln2O3 is one or more of La2O3, Gd2O3, Y2O3, and Yb2O3, and the clarifier is one or more of Sb2O3, SnO2, SnO, and CeO2.

[0008] (3) Optical glass, comprising SiO2, TiO2, Na2O and K2O, wherein the composition, expressed in weight percentage, contains 0 to 5% ZrO2, wherein (SiO2 + ZrO2) / TiO2 is 1.0 to 2.2, and the refractive index of the optical glass is n d 1.65~1.72, Abbe number ν d The temperature is 27 to 34, and the upper limit of crystallization temperature is 980°C or lower.

[0009] (4) The optical glass according to (3), wherein the components, expressed in weight percentage, are: SiO2: 36-49%; and / or TiO2: 21-37%; and / or Na2O: 6-20%; and / or K2O: 3-15%; and / or BaO: 0-10%; and / or Li2O: 0-8%; and / or ZnO: 0-10%; and / or SrO: 0-5%; and / or CaO: 0-5%; and / or MgO: 0-5%; and / or B2 O3: 0-4%; and / or Ln2O3: 0-4%; and / or Nb2O5: 0-4%; and / or WO3: 0-4%; and / or Al2O3: 0-4%; and / or P2O5: 0-4%; and / or clarifier: 0-1%; and / or F: 0-3%, wherein Ln2O3 is one or more of La2O3, Gd2O3, Y2O3, and Yb2O3, and the clarifier is one or more of Sb2O3, SnO2, SnO, and CeO2.

[0010] (5) The optical glass according to any one of (1) to (4), wherein the components thereof, expressed in weight percentage, satisfy one or more of the following 10 conditions:

[0011] 1) (SiO2 + ZrO2) / TiO2 is 1.1 to 2.0, preferably (SiO2 + ZrO2) / TiO2 is 1.2 to 1.8, and more preferably (SiO2 + ZrO2) / TiO2 is 1.2 to 1.6;

[0012] 2) (Nb2O5+WO3) / BaO is less than 1.0, preferably (Nb2O5+WO3) / BaO is less than 0.8, more preferably (Nb2O5+WO3) / BaO is less than 0.5, and further preferably (Nb2O5+WO3) / BaO is less than 0.2;

[0013] 3) Li2O / BaO is 0.15 to 5.0, preferably Li2O / BaO is 0.2 to 3.0, more preferably Li2O / BaO is 0.3 to 2.0, and further preferably Li2O / BaO is 0.4 to 1.5;

[0014] 4) TiO2 / BaO is 3.0 to 30.0, preferably TiO2 / BaO is 4.0 to 15.0, more preferably TiO2 / BaO is 5.0 to 10.0, and further preferably TiO2 / BaO is 5.5 to 9.0;

[0015] 5) SiO2 / (BaO+SrO+CaO+MgO+ZnO+Nb2O5) is 4.5 to 40.0, preferably SiO2 / (BaO+SrO+CaO+MgO+ZnO+Nb2O5) is 6.0 to 30.0, more preferably SiO2 / (BaO+SrO+CaO+MgO+ZnO+Nb2O5) is 7.0 to 20.0, and further preferably SiO2 / (BaO+SrO+CaO+MgO+ZnO+Nb2O5) is 8.6 to 12.0;

[0016] 6) (Nb2O5+ZrO2) / Li2O is less than 1.8, preferably (Nb2O5+ZrO2) / Li2O is less than 1.5, more preferably (Nb2O5+ZrO2) / Li2O is less than 1.0, and further preferably (Nb2O5+ZrO2) / Li2O is less than 0.5;

[0017] 7) (Li2O+Na2O+K2O) / TiO2 is 0.4 to 2.0, preferably (Li2O+Na2O+K2O) / TiO2 is 0.4 to 1.5, more preferably (Li2O+Na2O+K2O) / TiO2 is 0.5 to 1.3, and further preferably (Li2O+Na2O+K2O) / TiO2 is 0.7 to 1.0;

[0018] 8) BaO / K2O is less than 0.95, preferably BaO / K2O is 0.1 to 0.9, more preferably BaO / K2O is 0.2 to 0.8, further preferably BaO / K2O is 0.3 to 0.7, and further preferably BaO / K2O is 0.46 to 0.65;

[0019] 9) (SiO2+BaO) / Li2O is 5.0 to 39.0, preferably (SiO2+BaO) / Li2O is 8.0 to 35.0, more preferably (SiO2+BaO) / Li2O is 10.0 to 30.0, and further preferably (SiO2+BaO) / Li2O is 15.0 to 26.0;

[0020] 10) ZnO / Li2O is 6.0 or less, preferably ZnO / Li2O is 5.0 or less, more preferably ZnO / Li2O is 0.1 to 3.0, further preferably ZnO / Li2O is 0.1 to 1.5, and further preferably ZnO / Li2O is 0.2 to 1.0.

[0021] (6) The optical glass according to any one of (1) to (4), wherein the components are expressed in weight percentage, wherein: SiO2: 38-47%, preferably SiO2: 40-45%; and / or TiO2: 25-35%, preferably TiO2: 27-33%; and / or Na2O: 8-18%, preferably Na2O: 10.5-16%; and / or K2O: 5-12%, preferably K2O: 6.5-10%; and / or BaO: 0.5-8%, preferably BaO: 1-4 .5%; and / or Li2O: 0.1-6%, preferably Li2O: 0.5-4%; and / or ZnO: 0.1-8%, preferably ZnO: 0.5-6.5%; and / or SrO: 0-3%, preferably SrO: 0-2%, more preferably no SrO; and / or CaO: 0-3%, preferably CaO: 0-2%, more preferably no CaO; and / or MgO: 0-3%, preferably MgO: 0-2%, more preferably no MgO; and / or B2O3: 0-3 %, preferably B2O3: 0-2%, more preferably no B2O3; and / or Ln2O3: 0-3%, preferably Ln2O3: 0-2%, more preferably no Ln2O3; and / or ZrO2: 0-3%, preferably ZrO2: 0-2%; and / or Nb2O5: 0-3%, preferably Nb2O5: 0-2%, more preferably no Nb2O5; and / or WO3: 0-3%, preferably WO3: 0-2%, more preferably no WO3; and / or Al2O3: 0-3%, preferably WO3: 0-2%, more preferably no WO3; 3%, preferably Al2O3: 0-2%; and / or P2O5: 0-3%, preferably P2O5: 0-1%, more preferably no P2O5; and / or clarifier: 0-0.5%, clarifier: 0-0.2%; and / or F: 0-2%, preferably F: 0-1%, more preferably no F, the Ln2O3 is one or more of La2O3, Gd2O3, Y2O3, Yb2O3, and the clarifier is one or more of Sb2O3, SnO2, SnO, and CeO2.

[0022] (7) The optical glass according to any one of (1) to (4), wherein the refractive index n d 1.65 to 1.72, preferably 1.66 to 1.71, more preferably 1.67 to 1.70; Abbe number ν d It is 27-34, preferably 28-33, and more preferably 29-32.

[0023] (8) The optical glass according to any one of (1) to (4), wherein λ 80 420nm or less, preferably λ 80 415nm or less, preferably λ 80 is 410 nm or less, and more preferably λ 80 405nm or less; and / or λ5 is 385nm or less, preferably λ5 is 380nm or less, more preferably λ5 is 375nm or less, and further preferably λ5 is 370nm or less; and / or water resistance stability D W 2 or more, preferably 1; and / or acid resistance stability D A is 2 or more, preferably 1; and / or the crystallization upper limit temperature is 980°C or less, preferably 950°C or less, more preferably 920°C or less, and further preferably 900°C or less; and / or the thermal expansion coefficient α 100 / 300℃ 150×10 -7 / K or less, preferably 140×10 -7 / K or less, more preferably 135×10 -7 / K or less; and / or density ρ is 3.20g / cm 3 Below, preferably 3.10 g / cm 3 Below, more preferably 3.00g / cm 3 Below, more preferably 2.95 g / cm 3 Below; and / or transition temperature T g The temperature is 540°C or lower, preferably 530°C or lower, more preferably 520°C or lower, and further preferably 515°C or lower; and / or the weather resistance CR is 2 or higher, preferably 1; and / or the bubble degree is A or higher, preferably A0 or higher, and more preferably A 00 and / or the stripe degree is C level or above, preferably B level or above, more preferably A level.

[0024] (9) A glass preform made of the optical glass described in any one of (1) to (8).

[0025] (10) An optical element, made of the optical glass described in any one of (1) to (8), or made of the glass preform described in (9).

[0026] (11) An optical instrument comprising the optical glass described in any one of (1) to (8) and / or the optical element described in (10).

[0027] The beneficial effect of the present invention is that, through reasonable component design, the optical glass obtained by the present invention has a desired refractive index and Abbe number and also has excellent anti-crystallization performance. DETAILED DESCRIPTION

[0028] The following is a detailed description of the embodiments of the optical glass of the present invention, but the present invention is not limited to the following embodiments and can be implemented with appropriate changes within the scope of the purpose of the present invention. In addition, although there are appropriate omissions of the description of the repeated description, the main purpose of the invention will not be limited thereby. In the following content, the optical glass of the present invention is sometimes referred to as glass.

[0029] [Optical glass]

[0030] The following is an explanation of the range of each component (ingredient) of the optical glass of the present invention. In the present invention, unless otherwise specified, the content, total content, and total content of each component are all expressed in weight percentage (wt%), that is, the content, total content, and total content of each component are expressed in weight percentage relative to the total amount of glass material converted into oxide composition. Here, the "composition converted into oxide" means that when the oxides, complex salts, hydroxides, etc. used as raw materials for the optical glass components of the present invention decompose and transform into oxides during melting, the total amount of the oxide material is taken as 100%.

[0031] Unless otherwise indicated in specific circumstances, the numerical ranges listed herein include upper and lower limits, and "above" and "below" include endpoint values, as well as all integers and fractions within the range, without being limited to the specific values ​​listed when the range is defined. "And / or" as used herein is inclusive, for example, "A and / or B" means only A, or only B, or both A and B.

[0032] <Essential Components and Optional Components>

[0033] SiO2 is a network former component of glass, which can increase the viscosity of molten glass, improve the thermal stability of glass, increase the resistance to devitrification, and reduce the corrosion of molten glass on refractory materials; but if its content is too high, the melting difficulty of glass increases and the transition temperature rises. Therefore, the content of SiO2 in the present invention is 36-49%, preferably 38-47%, and more preferably 40-45%.

[0034] TiO2 has the effect of increasing the refractive index and dispersion of glass, improving the resistance to devitrification and the thermal expansion coefficient. In the present invention, the above effects are obtained by containing more than 21% of TiO2. If the content of TiO2 exceeds 37%, the coloring degree of the glass increases and the transition temperature rises. Therefore, the content of TiO2 in the present invention is 21-37%, preferably 25-35%, and more preferably 27-33%.

[0035] Li2O can reduce the transition temperature of glass and improve the melting property of glass, but its high content is not good for the striation degree and anti-crystallization performance of glass. Therefore, the content of Li2O in the present invention is 0-8%, preferably 0.1-6%, and more preferably 0.5-4%.

[0036] Na2O can improve the chemical stability of glass, reduce the transition temperature and partial dispersion ratio of glass, and improve the secondary compression molding anti-crystallization performance of glass. If the content of Na2O is too high, the refractive index of glass will be difficult to meet the design requirements. Therefore, the content of Na2O is 6-20%, preferably 8-18%, and more preferably 10.5-16%.

[0037] K2O can adjust the optical constants of glass, which is beneficial to improving the weather resistance of glass; however, when its content is too high, it is not conducive to glass molding and the stripe degree of glass is reduced. Therefore, the content of K2O in the present invention is 3-15%, preferably 5-12%, and more preferably 6.5-10%.

[0038] In some embodiments, the ratio of the total content of Li2O, Na2O, and K2O, Li2O+Na2O+K2O, to the content of TiO2, (Li2O+Na2O+K2O) / TiO2, is within the range of 0.4 to 2.0, which can improve the chemical stability of the glass and reduce the density and thermal expansion coefficient of the glass. Therefore, preferably (Li2O+Na2O+K2O) / TiO2 is 0.4 to 2.0, more preferably (Li2O+Na2O+K2O) / TiO2 is 0.4 to 1.5, further preferably (Li2O+Na2O+K2O) / TiO2 is 0.5 to 1.3, and further preferably (Li2O+Na2O+K2O) / TiO2 is 0.7 to 1.0.

[0039] BaO can improve the thermal expansion coefficient and high temperature viscosity of glass. If its content is too high, the chemical stability and devitrification resistance of glass will be deteriorated. Therefore, the content of BaO is 0-10%, preferably 0.5-8%, and more preferably 1-4.5%.

[0040] In some embodiments, the ratio of Li2O to BaO (Li2O / BaO) is controlled within the range of 0.15 to 5.0, which can reduce the glass transition temperature while improving the striation and bubble degree of the glass. Therefore, Li2O / BaO is preferably 0.15 to 5.0, more preferably 0.2 to 3.0, further preferably 0.3 to 2.0, and further preferably 0.4 to 1.5.

[0041] In some embodiments, the ratio (SiO2+BaO) / Li2O between the total content of SiO2 and BaO SiO2+BaO and the content of Li2O is controlled within the range of 5.0 to 39.0, which can improve the striation degree and light transmittance of the glass. Therefore, preferably (SiO2+BaO) / Li2O is 5.0 to 39.0, more preferably (SiO2+BaO) / Li2O is 8.0 to 35.0, further preferably (SiO2+BaO) / Li2O is 10.0 to 30.0, and further preferably (SiO2+BaO) / Li2O is 15.0 to 26.0.

[0042] In some embodiments, the ratio of TiO2 to BaO is controlled within the range of 3.0 to 30.0, which can improve the weather resistance and bubble degree of the glass and prevent the transition temperature from increasing. Therefore, preferably TiO2 / BaO is 3.0 to 30.0, more preferably TiO2 / BaO is 4.0 to 15.0, further preferably TiO2 / BaO is 5.0 to 10.0, and further preferably TiO2 / BaO is 5.5 to 9.0.

[0043] In some embodiments, the ratio of BaO content to K2O content, BaO / K2O, is controlled below 0.95, which is beneficial to lowering the transition temperature of the glass and improving the weather resistance of the glass. Therefore, it is preferred that BaO / K2O is below 0.95, more preferably BaO / K2O is 0.1 to 0.9, further preferably BaO / K2O is 0.2 to 0.8, and further preferably BaO / K2O is 0.3 to 0.7. Furthermore, controlling BaO / K2O within the range of 0.46 to 0.65 can further optimize the striation degree of the glass. Therefore, it is further preferred that BaO / K2O is 0.46 to 0.65.

[0044] SrO can increase the refractive index of glass and improve the resistance to devitrification, but if its content is too high, the chemical stability of the glass will decrease. Therefore, the SrO content is 0 to 5%, preferably 0 to 3%, and more preferably 0 to 2%. In some embodiments, it is further preferred that SrO is not contained.

[0045] CaO can increase the refractive index of glass and optimize the abrasiveness of glass, but if the content of CaO is too high, the anti-crystallization performance of glass will decrease. Therefore, the content of CaO is 0-5%, preferably 0-3%, and more preferably 0-2%. In some embodiments, it is further preferred that CaO is not contained.

[0046] MgO can adjust the optical constants of glass and improve the chemical stability of glass. If its content is too high, the devitrification resistance of glass decreases. Therefore, the MgO content is 0 to 5%, preferably 0 to 3%, and more preferably 0 to 2%. In some embodiments, it is further preferred that MgO is not contained.

[0047] B2O3 has the effect of improving the melting property of glass, but when its content is too high, the chemical stability and devitrification resistance of glass decrease. Therefore, the content of B2O3 in the present invention is 0 to 4%, preferably 0 to 3%, and more preferably 0 to 2%. In some embodiments, it is further preferred that B2O3 is not contained.

[0048] Ln2O3 (Ln2O3 is one or more of La2O3, Gd2O3, Y2O3, and Yb2O3) can improve the refractive index and chemical stability of glass, and is an optional component in the optical glass of the present invention. By controlling the content of Ln2O3 to be below 4%, the devitrification resistance of the glass can be prevented from decreasing. Therefore, in the optical glass of the present invention, the upper limit of the Ln2O3 content range is 4%, preferably 3%, and more preferably 2%. In some embodiments, it is further preferred that Ln2O3 is not contained.

[0049] ZrO2 can increase the refractive index and devitrification resistance of glass, improve the chemical stability and mechanical properties of glass. If its content is too high, the melting difficulty of glass increases, which may lead to inclusions inside the glass and reduce the light transmittance, and reduce the anti-crystallization performance of glass. Therefore, the ZrO2 content is 0-5%, preferably 0-3%, and more preferably 0-2%.

[0050] In some embodiments, the ratio (SiO2+ZrO2) / TiO2 between the total content of SiO2 and ZrO2 SiO2+ZrO2 and the content of TiO2 is controlled within the range of 1.0 to 2.2, which can improve the anti-crystallization performance of the glass and optimize the light transmittance and density of the glass. Therefore, preferably (SiO2+ZrO2) / TiO2 is 1.0 to 2.2, more preferably (SiO2+ZrO2) / TiO2 is 1.1 to 2.0, further preferably (SiO2+ZrO2) / TiO2 is 1.2 to 1.8, and further preferably (SiO2+ZrO2) / TiO2 is 1.2 to 1.6.

[0051] Nb2O5 is a high refractive and high dispersion component, which can improve the resistance of glass to devitrification and reduce the thermal expansion coefficient of glass. If the content of Nb2O5 is too high, the weather resistance and light transmittance of the glass will decrease, and the transition temperature of the glass will increase. Therefore, the content of Nb2O5 in the present invention is 0 to 4%, preferably 0 to 3%, and more preferably 0 to 2%. In some embodiments, it is further preferred that Nb2O5 is not contained.

[0052] In some embodiments, the ratio (Nb2O5+ZrO2) / Li2O between the total content of Nb2O5 and ZrO2, Nb2O5+ZrO2, and the content of Li2O is controlled to be below 1.8, which can improve the chemical stability of the glass and prevent the deterioration of the anti-crystallization and striae of the glass. Therefore, it is preferred that (Nb2O5+ZrO2) / Li2O is below 1.8, more preferably (Nb2O5+ZrO2) / Li2O is below 1.5, further preferably (Nb2O5+ZrO2) / Li2O is below 1.0, and further preferably (Nb2O5+ZrO2) / Li2O is below 0.5.

[0053] WO3 can improve the refractive index and dispersion of glass. If its content is too high, the light transmittance of the glass will decrease, and the secondary pressing anti-crystallization performance will deteriorate. Therefore, the WO3 content in the present invention is 0-4%, preferably 0-3%, and more preferably 0-2%. In some embodiments, it is further preferred that WO3 is not contained.

[0054] In some embodiments, by controlling the ratio of the total content of Nb2O5 and WO3, Nb2O5+WO3, to the content of BaO, (Nb2O5+WO3) / BaO, to be below 1.0, the chemical stability and light transmittance of the glass can be improved, and the transition temperature of the glass can be prevented from increasing. Therefore, preferably (Nb2O5+WO3) / BaO is below 1.0, more preferably (Nb2O5+WO3) / BaO is below 0.8, further preferably (Nb2O5+WO3) / BaO is below 0.5, and further preferably (Nb2O5+WO3) / BaO is below 0.2.

[0055] ZnO can improve the chemical stability of glass and reduce the high temperature viscosity and transition temperature of glass. However, if the content of ZnO is too much, the anti-crystallization performance of glass will decrease, and the high temperature viscosity will be too small, which will make it difficult to form glass. Therefore, the content of ZnO is 0-10%, preferably 0.1-8%, and more preferably 0.5-6.5%.

[0056] In some embodiments, the ratio ZnO / Li2O between the content of ZnO and the content of Li2O is controlled to be below 6.0, so that the glass can obtain a lower transition temperature while improving the striation degree of the glass. Therefore, it is preferred that ZnO / Li2O is below 6.0, and it is more preferred that ZnO / Li2O is below 5.0. Furthermore, controlling ZnO / Li2O within the range of 0.1 to 3.0 can further optimize the anti-crystallization performance and bubble degree of the glass. Therefore, it is further preferred that ZnO / Li2O is 0.1 to 3.0, and it is further preferred that ZnO / Li2O is 0.1 to 1.5, and it is further preferred that ZnO / Li2O is 0.2 to 1.0.

[0057] In some embodiments, the ratio of SiO2 content to the total content of BaO, SrO, CaO, MgO, ZnO, and Nb2O5 (BaO+SrO+CaO+MgO+ZnO+Nb2O5) is SiO2 / (BaO+SrO+CaO+MgO+ZnO+Nb2O5) in the range of 4.5 to 40.0, which can improve the anti-crystallization property and bubble degree of the glass and reduce the thermal expansion coefficient of the glass. Therefore, the preferred SiO2 / (BaO+SrO+CaO+MgO+ZnO+Nb2O5) is 4.5~40.0, the more preferred SiO2 / (BaO+SrO+CaO+MgO+ZnO+Nb2O5) is 6.0~30.0, the further preferred SiO2 / (BaO+SrO+CaO+MgO+ZnO+Nb2O5) is 7.0~20.0, and the further preferred SiO2 / (BaO+SrO+CaO+MgO+ZnO+Nb2O5) is 8.6~12.0.

[0058] In the present invention, Al2O3 has the effect of reducing the thermal expansion coefficient of glass and improving the thermal stability of glass; however, if the Al2O3 content is too high, the glass transition temperature will increase, and the high temperature viscosity of the glass will increase, and bubbles will be difficult to eliminate. Therefore, the content of Al2O3 is 0-4%, preferably 0-3%, and more preferably 0-2%.

[0059] P2O5 can improve the devitrification resistance of glass, but if its content is too high, the chemical stability of glass will deteriorate. Therefore, the content of P2O5 is 0 to 4%, preferably 0 to 3%, and more preferably 0 to 1%. In some embodiments, it is further preferred that P2O5 is not contained.

[0060] In the present invention, by containing 0-1% of one or more components of Sb2O3, SnO2, SnO, and CeO2 as clarifiers, the clarification effect of the glass and the bubble degree of the glass can be improved. The preferred content of the clarifier is 0-0.5%, and the more preferred content of the clarifier is 0-0.2%.

[0061] F can be used to adjust the refractive index of glass and reduce the temperature coefficient of refractive index. However, its volatilization during the production process creates environmental load problems. At the same time, it will volatilize from the glass surface in the molding operation temperature range to form an inhomogeneous part, reducing the glass quality and consistency of optical constants. Therefore, the content of F is 0-3%, preferably 0-2%, and more preferably 0-1%. In some embodiments, it is further preferred that F is not contained.

[0062] <Components that should not be contained>

[0063] In the glass of the present invention, even if oxides of transition metals such as V, Cr, Mn, Fe, Co, Ni, Cu, Ag and Mo are contained alone or in combination in small amounts, the glass will be colored and absorption will occur at specific wavelengths in the visible light region, thereby weakening the property of the present invention of improving the visible light transmittance. Therefore, it is preferably substantially free of oxides of transition metals such as V, Cr, Mn, Fe, Co, Ni, Cu, Ag and Mo, especially for optical glasses that require transmittance at wavelengths in the visible light region.

[0064] The oxides of Th, Cd, Tl, Os, Be and Se have a tendency to be controlled in recent years as harmful chemical substances, and environmental protection measures are necessary not only in the manufacturing process of glass, but also in the processing process and the disposal after productization. Therefore, in the case of paying attention to the impact on the environment, it is preferred that they are actually not contained except for being inevitably mixed in. Thus, the optical glass actually does not contain substances that pollute the environment. Therefore, even if special environmental countermeasures are not taken, the optical glass of the present invention can also be manufactured, processed and discarded. At the same time, in order to achieve environmental friendliness, the optical glass of the present invention preferably does not contain As2O3 and PbO.

[0065] The "does not contain" and "0%" recorded in this article mean that the compound, molecule or element is not intentionally added as a raw material to the optical glass of the present invention; however, as raw materials and / or equipment for producing optical glass, there will be certain impurities or components that are not intentionally added, which will be contained in a small amount or trace amount in the final optical glass, and this situation is also within the scope of protection of the patent of this invention.

[0066] The properties of the optical glass of the present invention will be described below:

[0067] <Refractive Index and Abbe Number>

[0068] The refractive index of optical glass (n d ) and the Abbe number (ν d ) Tested according to the method specified in GB / T 7962.1-2010.

[0069] In some embodiments, the refractive index (n d) has an upper limit of 1.72, a preferred upper limit of 1.71, and a more preferred upper limit of 1.70.

[0070] In some embodiments, the refractive index (n d ) has a lower limit of 1.65, a preferred lower limit is 1.66, and a more preferred lower limit is 1.67.

[0071] In some embodiments, the Abbe number (ν d ) has an upper limit of 34, a preferred upper limit of 33, and a more preferred upper limit of 32.

[0072] In some embodiments, the Abbe number (ν d ) has a lower limit of 27, a preferred lower limit of 28, and a more preferred lower limit of 29.

[0073] <Color>

[0074] The short-wave transmission spectrum characteristics of the optical glass of the present invention are expressed by the coloring degree (λ 80 and λ5). 80 It refers to the wavelength when the glass transmittance reaches 80%. 80 The measurement is to use a glass with a thickness of 10±0.1mm and two opposite planes parallel to each other and optically polished, and measure the spectral transmittance in the wavelength range from 280nm to 700nm and the wavelength at which the transmittance is 80%. The so-called spectral transmittance or transmittance is the wavelength at which the incident intensity I is perpendicular to the above surface of the glass. in Light of intensity I passes through the glass and emerges from a plane out The light of the case through I out / I in λ is a quantity that also includes the transmittance of the surface reflection loss on the above surface of the glass. The higher the refractive index of the glass, the greater the surface reflection loss. Therefore, λ 80 A small value of means that the glass itself is less colored and has a high light transmittance.

[0075] The same applies to λ5.

[0076] In some embodiments, the λ of the optical glass of the present invention is 80 420nm or less, preferably λ 80 415nm or less, preferably λ 80 is 410 nm or less, and more preferably λ 80 Below 405nm.

[0077] In some embodiments, the optical glass of the present invention has a λ5 of 385 nm or less, preferably λ5 of 380 nm or less, more preferably λ5 of 375 nm or less, and further preferably λ5 of 370 nm or less.

[0078] <Water resistance stability>

[0079] Water resistance stability of optical glass (D W ) (Powder method) Tested in accordance with the method specified in GB / T 17129.

[0080] In some embodiments, the water resistance stability (D W ) is 2 or more types, preferably 1 type.

[0081] <Acid resistance stability>

[0082] Acid resistance stability of optical glass (D A ) (Powder method) Tested in accordance with the method specified in GB / T 17129.

[0083] In some embodiments, the acid resistance stability (D A ) is 2 or more types, preferably 1 type.

[0084] <Crystallization upper limit temperature>

[0085] The anti-crystallization performance of optical glass is measured by the gradient temperature furnace method. The glass is made into a 180×10×10mm sample, the side is polished, and it is placed in a furnace with a temperature gradient (10℃ / cm) and a maximum temperature zone of 1200℃ for 4 hours. After that, it is taken out and naturally cooled to room temperature. The crystallization of the glass is observed under a microscope. The highest temperature corresponding to the appearance of crystals in the glass is the upper limit temperature of crystallization of the glass. The lower the upper limit temperature of crystallization of the glass, the better the anti-crystallization performance.

[0086] In some embodiments, the optical glass of the present invention has a crystallization upper limit temperature of 980° C. or lower, preferably 950° C. or lower, more preferably 920° C. or lower, and further preferably 900° C. or lower.

[0087] <Coefficient of Thermal Expansion>

[0088] Thermal expansion coefficient of optical glass (α 100 / 300℃ ) The data at 100-300℃ were tested according to the method specified in GB / T7962.16-2010.

[0089] In some embodiments, the thermal expansion coefficient (α 100 / 300℃ ) is 150×10 -7 / K or less, preferably 140×10 -7 / K or less, more preferably 135×10 -7 / K or less.

[0090] <density>

[0091] The density (ρ) of optical glass is tested according to the method specified in GB / T7962.20-2010.

[0092] In some embodiments, the density (ρ) of the optical glass of the present invention is 3.20 g / cm 3 Below, preferably 3.10 g / cm 3 Below, more preferably 3.00g / cm 3 Below, more preferably 2.95 g / cm 3 the following.

[0093] <Transition Temperature>

[0094] Transition temperature of optical glass (T g ) Tested according to the method specified in GB / T7962.16-2010.

[0095] In some embodiments, the transition temperature (T g ) is 540°C or lower, preferably 530°C or lower, more preferably 520°C or lower, and further preferably 515°C or lower.

[0096] <Weather resistance>

[0097] The test method for weather resistance (CR) of optical glass is as follows: place the sample in a test box with a saturated water vapor environment of 90% relative humidity, alternately cycle every 1 hour at 40-50°C, and cycle for 15 cycles. The weather resistance category is divided according to the change in turbidity before and after the sample is placed. The weather resistance classification is shown in Table 1:

[0098] Table 1.

[0099]

[0100] In some embodiments, the weather resistance (CR) of the optical glass of the present invention is Class 2 or higher, preferably Class 1.

[0101] <Bubble Degree>

[0102] The bubble degree of optical glass is tested according to the method specified in GB / T7962.8-2010.

[0103] In some embodiments, the bubble degree of the optical glass of the present invention is above grade A, preferably above grade A0, and more preferably above grade A1. 00 class.

[0104] <Striation Degree>

[0105] The striation degree of the glass of the present invention is tested by the following method: using a striation meter composed of a point light source and a lens, the striation degree is compared with the standard sample from the direction where the striation is most easily visible, and is divided into 4 levels, namely, A, B, C, and D. Level A means no striations visible to the naked eye under the specified test conditions, level B means fine and dispersed striations under the specified test conditions, level C means slight parallel striations under the specified test conditions, and level D means coarse striations under the specified test conditions.

[0106] In some embodiments, the striae of the optical glass of the present invention is C-level or higher, preferably B-level or higher, and more preferably A-level.

[0107] [Manufacturing method]

[0108] The manufacturing method of the optical glass of the present invention is as follows: the glass of the present invention is produced by conventional raw materials and processes, including but not limited to using oxides, hydroxides, fluorides, boric acid, various salts (carbonates, nitrates, sulfates, phosphates, metaphosphates) and the like as raw materials, and after mixing the materials according to conventional methods, the prepared furnace materials are put into a melting furnace (such as platinum, gold or platinum alloy crucible) at 1000-1400° C. for melting, and after clarification and homogenization, a homogeneous molten glass without bubbles and undissolved substances is obtained, and the molten glass is cast in a mold and annealed. Those skilled in the art can appropriately select raw materials, process methods and process parameters according to actual needs.

[0109] [Glass preforms and optical components]

[0110] The prepared optical glass can be used to make a glass preform by means of direct drop molding, grinding, or compression molding such as hot press molding. That is, the molten optical glass can be directly precision drop molded into a glass precision preform, or the glass preform can be made by mechanical processing such as grinding and grinding, or the preform for compression molding made of the optical glass can be made by hot press molding and then grinding. It should be noted that the means for preparing the glass preform are not limited to the above means.

[0111] As described above, the optical glass of the present invention is useful for various optical elements and optical designs, and it is particularly preferred to form a preform from the optical glass of the present invention and use the preform to perform re-hot pressing, precision stamping, etc. to produce optical elements such as lenses and prisms.

[0112] The glass preform and optical element of the present invention are both formed of the optical glass of the present invention. The glass preform of the present invention has the excellent properties of optical glass; the optical element of the present invention has the excellent properties of optical glass, and can provide various optical elements such as lenses and prisms with high optical value.

[0113] Examples of the lens include various lenses having spherical or aspherical lens surfaces, such as a concave meniscus lens, a convex meniscus lens, a biconvex lens, a biconcave lens, a plano-convex lens, and a plano-concave lens.

[0114] [Optical instruments]

[0115] The optical element formed by the optical glass of the present invention can be used to manufacture optical instruments such as photographic equipment, video equipment, projection equipment, display equipment, vehicle-mounted equipment and monitoring equipment.

[0116] Example

[0117] <Optical Glass Example>

[0118] In order to further clearly illustrate and describe the technical solution of the present invention, the following non-limiting examples are provided.

[0119] This embodiment adopts the above optical glass manufacturing method to obtain optical glasses having the compositions shown in Tables 2 to 4. In addition, the properties of each glass are measured by the testing method described in the present invention, and the measurement results are shown in Tables 2 to 4.

[0120] Table 2.

[0121]

[0122]

[0123] Table 3.

[0124]

[0125]

[0126] Table 4.

[0127]

[0128]

[0129]

[0130] <Glass Preform Example>

[0131] The glass obtained from optical glass examples 1 to 21# is used, for example, by grinding processing, or by molding methods such as hot pressing, precision stamping, etc., to make preforms of various lenses, prisms, etc., such as concave meniscus lenses, convex meniscus lenses, biconvex lenses, biconcave lenses, plano-convex lenses, and plano-concave lenses.

[0132] <Optical Element Embodiment>

[0133] The preforms obtained in the above-mentioned glass preform embodiments are annealed to reduce the deformation inside the glass and perform fine adjustments so that the optical properties such as the refractive index reach the desired values.

[0134] Next, each preform is ground and polished to produce various lenses and prisms such as concave meniscus lenses, convex meniscus lenses, biconvex lenses, biconcave lenses, plano-convex lenses, and plano-concave lenses. The surface of the obtained optical element may be coated with an anti-reflection film.

[0135] <Optical Instrument Embodiment>

[0136] The optical element obtained by the above-mentioned optical element embodiment is optically designed to form an optical component or optical assembly by using one or more optical elements. It can be used in, for example, imaging equipment, sensors, microscopes, medical technology, digital projection, communications, optical communication technology / information transmission, optics / lighting in the automotive field, lithography technology, excimer lasers, wafers, computer chips, and integrated circuits and electronic devices including such circuits and chips, or in camera equipment and devices in the vehicle field.

Claims

1. Optical glass, It is characterized in that Its components are expressed in weight percentage and contain: SiO 2 :36~49%;TiO 2 :21~37%;Na 2 O: 6-20%; K 2 O: 3-15%; ZrO 2 :0~5%, among which (SiO 2 +ZrO 2 ) / TiO 2 It is 1.0~2.

2.

2. The optical glass according to claim 1, It is characterized in that Its components, expressed in weight percentage, also contain: BaO: 0-10%; and / or Li 2 O: 0-8%; and / or ZnO: 0-10%; and / or SrO: 0-5%; and / or CaO: 0-5%; and / or MgO: 0-5%; and / or B 2 O 3 : 0~4%; and / or Ln 2 O 3 :0~4%;and / or Nb 2 O 5 : 0-4%; and / or WO 3 : 0-4%; and / or Al 2 O 3 :0~4%;and / or P 2 O 5 : 0-4%; and / or clarifier: 0-1%; and / or F: 0-3%, the Ln 2 O 3 For La 2 O 3 , Gd 2 O 3 , Y 2 O 3 , Yb 2 O 3 One or more of the following, the clarifier is Sb 2 O 3 SnO 2 , SnO, CeO 2 One or more of .

3. Optical glass, It is characterized in that Its components contain SiO 2 、TiO 2 、Na 2 O and K 2 O, its composition is expressed in weight percentage, containing 0-5% ZrO 2 , where (SiO 2 +ZrO 2 ) / TiO 2 The refractive index n of the optical glass is 1.0 to 2.

2. d 1.65~1.72, Abbe number ν d The temperature is 27 to 34, and the upper limit of crystallization temperature is 980°C or lower.

4. The optical glass according to claim 3, It is characterized in that Its components are expressed in weight percentage and contain: SiO 2 :36~49%;and / or TiO 2 :21~37%;and / or Na 2 O: 6-20%; and / or K 2 O: 3-15%; and / or BaO: 0-10%; and / or Li 2 O: 0-8%; and / or ZnO: 0-10%; and / or SrO: 0-5%; and / or CaO: 0-5%; and / or MgO: 0-5%; and / or B 2 O 3 : 0~4%; and / or Ln 2 O 3 :0~4%;and / or Nb 2 O 5 : 0-4%; and / or WO 3 : 0-4%; and / or Al 2 O 3 :0~4%;and / or P 2 O 5 : 0-4%; and / or clarifier: 0-1%; and / or F: 0-3%, the Ln 2 O 3 For La 2 O 3 , Gd 2 O 3 , Y 2 O 3 , Yb 2 O 3 One or more of the following, the clarifier is Sb 2 O 3 SnO 2 , SnO, CeO 2 One or more of .

5. The optical glass according to any one of claims 1 to 4, It is characterized in that Its components are expressed in weight percentage and meet one or more of the following 10 conditions: 1)(SiO 2 +ZrO 2 ) / TiO 2 1.1 to 2.0, preferably (SiO 2 +ZrO 2 ) / TiO 2 1.2 to 1.8, more preferably (SiO 2 +ZrO 2 ) / TiO 2 1.2~1.6; 2)(Nb 2 O 5 +WO 3 ) / BaO is 1.0 or less, preferably (Nb 2 O 5 +WO 3 ) / BaO is 0.8 or less, and more preferably (Nb 2 O 5 +WO 3 ) / BaO is 0.5 or less, and more preferably (Nb 2 O 5 +WO 3 ) / BaO is less than 0.2; 3)Li 2 O / BaO is 0.15 to 5.0, preferably Li 2 O / BaO is 0.2 to 3.0, and Li 2 O / BaO is 0.3 to 2.0, and Li 2 O / BaO is 0.4~1.5; 4) TiO 2 / BaO is 3.0 to 30.0, preferably TiO 2 / BaO is 4.0 to 15.0, and TiO is more preferred 2 / BaO is 5.0 to 10.0, and TiO is more preferred 2 / BaO is 5.5 to 9.0; 5)SiO 2 / (BaO+SrO+CaO+MgO+ZnO+Nb 2 O 5 ) is 4.5 to 40.0, preferably SiO 2 / (BaO+SrO+CaO+MgO+ZnO+Nb 2 O 5 ) is 6.0 to 30.0, more preferably SiO 2 / (BaO+SrO+CaO+MgO+ZnO+Nb 2 O 5 ) is 7.0 to 20.0, and SiO 2 / (BaO+SrO+CaO+MgO+ZnO+Nb 2 O 5 ) is 8.6~12.0; 6)(Nb 2 O 5 +ZrO 2 ) / Li 2 O is 1.8 or less, preferably (Nb 2 O 5 +ZrO 2 ) / Li 2 O is 1.5 or less, and more preferably (Nb 2 O 5 +ZrO 2 ) / Li 2 O is 1.0 or less, and more preferably (Nb 2 O 5 +ZrO 2 ) / Li 2 O is less than 0.5; 7)(Li 2 O+Na 2 O+K 2 O) / TiO 2 is 0.4 to 2.0, preferably (Li 2 O+Na 2 O+K 2 O) / TiO 2 is 0.4 to 1.5, more preferably (Li 2 O+Na 2 O+K 2 O) / TiO 2 is 0.5 to 1.3, and more preferably (Li 2 O+Na 2 O+K 2 O) / TiO 2 0.7~1.0; 8)BaO / K 2 O is less than 0.95, preferably BaO / K 2 O is 0.1 to 0.9, more preferably BaO / K 2 O is 0.2 to 0.8, and BaO / K is more preferred. 2 O is 0.3 to 0.7, and BaO / K is more preferred. 2 O is 0.46-0.65; 9)(SiO 2 +BaO) / Li 2 O is 5.0 to 39.0, preferably (SiO 2 +BaO) / Li 2 O is 8.0 to 35.0, more preferably (SiO 2 +BaO) / Li 2 O is 10.0 to 30.0, and more preferably (SiO 2 +BaO) / Li 2 O is 15.0-26.0; 10) ZnO / Li 2 O is 6.0 or less, preferably ZnO / Li 2 O is 5.0 or less, and ZnO / Li is more preferred 2 O is 0.1 to 3.0, and ZnO / Li is more preferred. 2 O is 0.1 to 1.5, and ZnO / Li is more preferred 2 O is 0.2~1.

0.

6. The optical glass according to any one of claims 1 to 4, It is characterized in that Its components are expressed in weight percentage, among which: SiO 2 : 38-47%, preferably SiO 2 : 40-45%; and / or TiO 2 : 25-35%, preferably TiO 2 :27~33%;and / or Na 2 O: 8-18%, preferably Na 2 O: 10.5-16%; and / or K 2 O: 5-12%, preferably K 2 O: 6.5-10%; and / or BaO: 0.5-8%, preferably BaO: 1-4.5%; and / or Li 2 O: 0.1-6%, preferably Li 2 O: 0.5-4%; and / or ZnO: 0.1-8%, preferably ZnO: 0.5-6.5%; and / or SrO: 0-3%, preferably SrO: 0-2%, more preferably no SrO; and / or CaO: 0-3%, preferably CaO: 0-2%, more preferably no CaO; and / or MgO: 0-3%, preferably MgO: 0-2%, more preferably no MgO; and / or B 2 O 3 : 0-3%, preferably B 2 O 3 : 0 to 2%, preferably no B 2 O 3 ; and / or Ln 2 O 3 : 0-3%, preferably Ln 2 O 3 : 0 to 2%, preferably no Ln 2 O 3 ; and / or ZrO 2 : 0-3%, preferably ZrO 2 :0~2%;and / or Nb 2 O 5 : 0-3%, preferably Nb 2 O 5 : 0 to 2%, preferably no Nb 2 O 5 ; and / or WO 3 : 0-3%, preferably WO 3 : 0-2%, preferably no WO 3 ; and / or Al 2 O 3 : 0-3%, preferably Al 2 O 3 :0~2%;and / or P 2 O 5 : 0~3%, preferably P 2 O 5 : 0 to 1%, preferably no P 2 O 5 and / or clarifier: 0-0.5%, clarifier: 0-0.2%; and / or F: 0-2%, preferably F: 0-1%, more preferably no F, the Ln 2 O 3 For La 2 O 3 , Gd 2 O 3 , Y 2 O 3 , Yb 2 O 3 One or more of the following, the clarifier is Sb 2 O 3 SnO 2 , SnO, CeO 2 One or more of .

7. The optical glass according to any one of claims 1 to 4, It is characterized in that The refractive index n of the optical glass d 1.65 to 1.72, preferably 1.66 to 1.71, more preferably 1.67 to 1.70; Abbe number ν d It is 27-34, preferably 28-33, and more preferably 29-32.

8. The optical glass according to any one of claims 1 to 4, It is characterized in that The λ of the optical glass 80 420nm or less, preferably λ 80 415nm or less, preferably λ 80 is 410 nm or less, and more preferably λ 80 is below 405nm; and / or λ 5 385nm or less, preferably λ 5 380nm or less, preferably λ 5 is 375 nm or less, and more preferably λ 5 370nm or less; and / or water resistance stability D W 2 or more, preferably 1; and / or acid resistance stability D A is 2 or more, preferably 1; and / or the crystallization upper limit temperature is 980°C or less, preferably 950°C or less, more preferably 920°C or less, and further preferably 900°C or less; and / or the thermal expansion coefficient α 100 / 300℃ 150×10 -7 / K or less, preferably 140×10 -7 / K or less, more preferably 135×10 -7 / K or less; and / or density ρ is 3.20g / cm 3 Below, preferably 3.10 g / cm 3 Below, more preferably 3.00g / cm 3 Below, more preferably 2.95 g / cm 3 Below; and / or transition temperature T g The temperature is 540°C or lower, preferably 530°C or lower, more preferably 520°C or lower, and further preferably 515°C or lower; and / or the weather resistance CR is 2 or higher, preferably 1; and / or the bubble degree is A or higher, preferably A 0 Grade A or above, preferably A 00 and / or the stripe degree is C level or above, preferably B level or above, more preferably A level.

9. Glass preforms, It is characterized in that Made of the optical glass described in any one of claims 1 to 8.

10. Optical components, It is characterized in that The optical glass is made of the optical glass described in any one of claims 1 to 8, or the glass preform described in claim 9.

11. Optical instruments, It is characterized in that Contains the optical glass according to any one of claims 1 to 8, and / or contains the optical element according to claim 10.

Citation Information

Patent Citations

  • Optical glass, preform and optical element

    CN114599617A