Preparation method of novel multi-band response Mo-TiC MXene / MoC-Mo2N electromagnetic wave-absorbing material and product of novel multi-band response Mo-TiC MXene / MoC-Mo2N electromagnetic wave-absorbing material
By forming MoC and Mo2N nanoparticles in situ on the surface of Mo-TiC MXene, the material stacking problem is solved, and the efficient preparation of Mo-TiC MXene/MoC-Mo2N electromagnetic wave absorbing materials with multi-band response is achieved, and the existing technology is overcome poor impedance matching and weak absorption capacity.
Patent Information
- Application Number
- CN202411097161.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-12
AI Technical Summary
The existing Mo-TiC MXene materials are susceptible to the effect of van der Waals forces, which lead to stacking problems, affecting the synthesis and electromagnetic absorption performance of molybdenum-based compounds, and the prior art is difficult to solve the problems of poor impedance matching and weak absorption capacity.
Through in-situ preoxidation and in-situ heat treatment processes, a large number of MoC and Mo2N nanoparticles are formed on the surface of the small layer of Mo-TiC MXene, which regulates the dielectric loss capacity. Dicyandiamide is used to provide carbon and nitrogen elements to form MoC and Mo2N to achieve Multi-band responsive electromagnetic wave absorbing material.
Mo-TiC MXene/MoC-Mo2N electromagnetic wave absorbing material with multi-band absorption capacity and ultra-thin matching thickness was developed, which effectively overcomes the problems of poor impedance matching, weak absorption capacity and large matching thickness, and achieves efficient multi-band response. .
Smart Images

Figure CN118954510A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of electromagnetic microwave absorption technology, and in particular to a preparation method of a novel multi-band responsive Mo-TiCMXene / MoC-Mo2N electromagnetic absorbing material and a product obtained therefrom. Background Art
[0002] Stealth technology is one of the key research and development areas in the field of national defense and military today. This technology can effectively improve the survival, breakthrough and combat capabilities of military equipment. Therefore, stealth technology has become a research focus of the world's major military powers. In addition, with the development of 5G / 6G technology and the continuous evolution of electronic equipment, the problem of electromagnetic pollution is becoming increasingly serious. Therefore, the development of advanced and efficient electromagnetic absorbing materials is of great strategic significance in the fields of national defense, military and civilian use.
[0003] As a typical dielectric loss material, carbide has attracted great attention from researchers due to its good thermal stability, high mechanical strength, oxidation resistance and corrosion resistance. Among them, molybdenum carbide is one of the most widely used metal carbides. It has excellent dielectric properties, chemical stability, and controllable composition and structure, and is widely used in the field of electromagnetic wave absorption. However, impedance mismatch caused by excessive conductivity and agglomeration problems remains an obstacle to the application of single molybdenum carbide materials. Molybdenum nitride, as another molybdenum-based metal compound with good conductivity, is considered to be one of the ideal dielectric materials. At present, it is generally believed that the performance of a material is highly related to its microstructure. Therefore, constructing molybdenum-based compounds with different crystal structures may be a feasible way to optimize impedance matching, and may also provide additional interface polarization and dipole polarization to the material. In addition, studies have shown that the Mo atoms in the Mo-TiC MXene formed by etching Mo2TiAlC2 MAX occupy the outermost layer, which is conducive to the in-situ formation of molybdenum-based compounds such as sulfides, oxides, nitrides and carbides on the surface of Mo-TiC MXene through special processes, while retaining the inherent structure of Mo-TiC MXene. Therefore, it is feasible to synthesize molybdenum-based compounds by utilizing Mo atoms in Mo-TiC MXene, and it helps to solve the agglomeration problem. However, since Mo-TiC MXene itself is a two-dimensional layered structure, it is susceptible to the action of van der Waals forces, which may lead to stacking problems, affect the large-scale synthesis of molybdenum-based compounds, and affect the electromagnetic absorption performance of the material. The existing technology for solving the stacking problem of Mo-TiC MXene is currently mainly to convert the multi-layer structure into a few-layer or single-layer structure through methods such as ultrasound, intercalation, and molten salt. Therefore, it is of great significance to develop Mo-TiC MXene / MoC-Mo2N electromagnetic absorbing materials with excellent performance through few-layer Mo-TiC MXene. In addition, discovering a low-cost, high-yield method for preparing few-layer Mo-TiC MXene materials and finding a simple and effective process for synthesizing molybdenum-based compounds are also one of the technical challenges in the synthesis of this material. Summary of the invention
[0004] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a method for preparing a novel multi-band responsive Mo-TiCMXene / MoC-Mo2N electromagnetic absorbing material. Through in-situ pre-oxidation, in-situ heat treatment and other processes, a large number of MoC and Mo2N nanoparticles are formed on the surface of a few-layer Mo-TiC MXene, thereby using an in-situ phase change strategy to adjust the dielectric loss capacity, providing important technical ideas and approaches for the design of multi-band responsive electromagnetic absorbing materials. Another purpose of the present invention is to provide a product obtained by the method for preparing the novel multi-band responsive Mo-TiC MXene / MoC-Mo2N electromagnetic absorbing material.
[0005] The purpose of the present invention is achieved through the following technical solutions:
[0006] The present invention provides a method for preparing a novel multi-band responsive Mo-TiC MXene / MoC-Mo2N electromagnetic absorbing material, comprising the following steps:
[0007] (1) Preparation of multilayer Mo-TiC MXene
[0008] Mo2TiAlC2 MAX is used as a raw material and hydrofluoric acid with a concentration of 40% is used as an etchant. The raw material: etchant is stirred and mixed according to a mass volume ratio of 0.5-1 g to 20-60 mL, and then the mixture is collected by centrifugation and washed to obtain an undried multilayer Mo-TiCMXene.
[0009] (2) Preparation of few-layer Mo-TiC MXene
[0010] (2-1) The undried multilayer Mo-TiC MXene is used as a material and TMAOH with a concentration of 5 wt% is used as an intercalation agent, and the mixture is stirred and mixed according to a mass volume ratio of material: intercalation agent = 0.5-1.2 g: 20-40 mL, and then the mixture is collected by centrifugation and washed to obtain a few-layer Mo-TiC MXene precursor from which TMAOH is removed;
[0011] (2-2) according to the mass volume ratio of few-layer Mo-TiC MXene precursor: deionized water = 0.7-1.5 g: 20-30 mL, the few-layer Mo-TiC MXene precursor is dispersed again in deionized water and mixed together, and then the supernatant is obtained by centrifugation, and the supernatant collection process is repeated to obtain the few-layer Mo-TiC MXene solution;
[0012] (3) Preparation of few-layer Mo-TiC MXene-O powder
[0013] The few-layer Mo-TiC MXene solution is stirred and condensed under reflux in a constant temperature environment, and then freeze-dried to obtain a few-layer Mo-TiC MXene-O powder; in this way, the few-layer Mo-TiC MXene-O is obtained by an in-situ pre-oxidation process, providing a molybdenum oxide intermediate phase for the formation of MoC and Mo2N in the next in-situ heat treatment process;
[0014] (4) Preparation of Mo-TiC MXene / MoC-Mo2N
[0015] According to the mass ratio of few-layer Mo-TiC MXene-O: dicyandiamide = 1-2: 0.5-4, the few-layer Mo-TiC MXene-O powder and dicyandiamide are placed at both ends of the porcelain boat, respectively, and placed in a tube furnace, wherein dicyandiamide is placed at the air inlet end and the few-layer Mo-TiC MXene-O powder is placed at the air outlet end; argon gas is introduced at a flow rate of 200-400 mL / min, and the temperature is increased to 350-550°C at 2°C / min for heat treatment for 1-4 hours, and then the temperature is increased to 700-850°C at 5°C / min for heat treatment for 1-4 hours, and then the temperature is increased to 700-850°C at 5°C / min for heat treatment for 1-4 hours, so as to obtain a Mo-TiC MXene / MoC-Mo2N electromagnetic wave absorbing material with multi-band response. Among them, dicyandiamide provides a gas-phase carbon source and a nitrogen source for the formation of MoC and Mo2N, and the molybdenum element in the few-layer Mo-TiC MXene-O provides a molybdenum source for the formation of MoC and Mo2N. The few-layer Mo-TiC MXene-O undergoes a two-stage heat treatment process to first form a molybdenum oxide intermediate phase, and then reacts with the gas phase carbon source and nitrogen source to form MoC and Mo2N, respectively.
[0016] Furthermore, in the step (1) of the present invention, the stirring and mixing time is 72 to 96 hours; the speed of centrifugal collection is 3000 to 8000 r / min, and the time of centrifugal collection is 5 to 30 minutes; the washing solution is deionized water, and the pH value is washed to ≥7. In the step (2-1), the stirring and mixing time is 12 to 24 hours, the speed of centrifugal collection is 10000 to 13000 r / min, and the time of centrifugal collection is 5 to 30 minutes; the washing solution is deionized water, and the pH value is washed to ≥7; the speed of centrifugal collection in the step (2-2) is 3000 to 4000 r / min, and the time of centrifugal collection is 30 to 60 minutes; the number of repetitions of the supernatant collection process is 3 to 6 times. In the step (3), the stirring and condensation reflux temperature is 40 to 50°C, and the time is 48 to 72 hours; the freeze-drying time is 48 to 72 hours.
[0017] The product prepared by the preparation method of the novel multi-band responsive Mo-TiC MXene / MoC-Mo2N electromagnetic absorbing material of the present invention has a reflection loss of -14.8 to -65.2 dB at a matching thickness of 1.565 to 5 mm within a frequency range of 2 to 18 GHz.
[0018] The present invention has the following beneficial effects:
[0019] (1) The present invention uses Mo2TiAlC2 MAX and dicyandiamide as raw materials, and combines with an etchant and an intercalation agent, adopts an in-situ pre-oxidation and heat treatment process, and in-situ synthesizes MoC and Mo2N nanoparticles on the surface of a few-layer Mo-TiC MXene nanosheet to regulate the overall dielectric properties of the material. The present invention not only expands the types of electromagnetic absorbing materials, but also develops a new type of electromagnetic absorbing material with multi-band absorption (reflection loss of -14.8 to -65.2 dB) and ultra-thin matching thickness (1.565 to 5 mm). Through the synergistic effect of mechanisms such as conduction loss and multiple interface polarization, the dielectric loss capacity of the material is adjusted, overcoming the problems of poor impedance matching, weak absorption capacity and large matching thickness of the electromagnetic absorbing materials in the prior art.
[0020] (2) The present invention uses hydrofluoric acid as an etchant to etch away the Al layer in Mo2TiAlC2 MAX to form a multilayer Mo-TiC MXene, providing the required multilayer MXene structure for TMAOH intercalation Mo-TiC MXene and providing the prerequisite for the formation of few-layer Mo-TiC MXene nanosheets.
[0021] (3) In the present invention, TMAOH is used as an intercalation agent, and TMA is mixed by magnetic stirring. + The ions are embedded in the interlayers of multilayer Mo-TiC MXene to expand the interlayer spacing, so as to further transform the multilayer structure of Mo-TiC MXene into a few-layer structure. The few-layer Mo-TiC MXene nanosheets prepared by the TMAOH intercalation process have a large specific surface area and a large spacing between sheets, which provides a certain space for the in-situ synthesis of MoC and Mo2N nanoparticles. In addition, the synthesis of nanoparticles can effectively inhibit the reaggregation of few-layer Mo-TiC MXene.
[0022] (4) The present invention uses an in-situ pre-oxidation process, the purpose of which is to introduce a large number of oxygen-containing functional groups into the few-layer Mo-TiC MXene, to provide oxygen elements for the next heat treatment process, so that after the heat treatment process, the few-layer Mo-TiC MXene-O will preferentially form a molybdenum oxide intermediate phase, and then undergo a crystal phase transformation with the carbon and nitrogen elements in dicyandiamide to form MoC and Mo2N respectively. The present invention finds that the in-situ pre-oxidation strategy is indispensable in the entire process flow, and MoC and Mo2N can only be formed after the pre-oxidation process.
[0023] (5) In the reaction system of the present invention, dicyandiamide is used to provide carbon and nitrogen elements required for the synthesis of molybdenum-based compounds, the purpose of which is to transform the molybdenum oxide intermediate phase preferentially formed in the in-situ heat treatment process into MoC and Mo2N. Therefore, precise control of the Mo-TiC MXene / MoC-Mo2N heterostructure can be achieved by adjusting the in-situ heat treatment and in-situ pre-oxidation process parameters, which is conducive to expanding the loss path, promoting interface polarization and improving dielectric loss capacity, and achieving efficient multi-band response, effectively overcoming the problems of poor impedance matching, weak absorption capacity, large matching thickness, and difficulty in taking into account multi-band absorption of electromagnetic absorbing materials in the prior art, and providing a new method for the formation of MoC and Mo2N.
[0024] (6) The process of the present invention has high repeatability, is easy to control, has low cost, and is easy to promote and use. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] The present invention will be further described in detail below with reference to the embodiments and accompanying drawings:
[0026] Figure 1 This is a scanning electron microscope image of a novel multi-band responsive Mo-TiC MXene / MoC-Mo2N electromagnetic absorbing material prepared in an embodiment of the present invention;
[0027] Figure 2 is an X-ray diffraction pattern of a novel multi-band responsive Mo-TiC MXene / MoC-Mo2N electromagnetic absorbing material prepared in an embodiment of the present invention;
[0028] Figure 3 It is a curve diagram of the relationship between reflection loss and frequency of the novel multi-band responsive Mo-TiC MXene / MoC-Mo2N electromagnetic absorbing material prepared in an embodiment of the present invention at different matching thicknesses;
[0029] Figure 4 It is a curve diagram showing the relationship between the optimal reflection loss and frequency of the electromagnetic absorbing materials of the embodiment of the present invention and the comparative example. DETAILED DESCRIPTION
[0030] Example:
[0031] The present invention provides a method for preparing a novel multi-band responsive Mo-TiC MXene / MoC-Mo2N electromagnetic absorbing material, the steps of which are as follows:
[0032] (1) Preparation of multilayer Mo-TiC MXene
[0033] Using Mo2TiAlC2 MAX as raw material and 40% hydrofluoric acid as etchant, 30 mL of etchant was measured into a Teflon liner with a volume of 100 mL, and 1 g of Mo2TiAlC2 MAX was slowly added. After magnetic stirring and mixing at 55 °C for 72 h, the obtained suspension was centrifuged at 6000 r / min for 5 min and washed with deionized water to a pH value ≥ 7 to obtain undried multilayer Mo-TiC MXene;
[0034] (2) Preparation of few-layer Mo-TiC MXene
[0035] (2-1) Using 5 wt% TMAOH as an intercalation agent, 0.8 g of the undried multilayer Mo-TiC MXene was added to 40 mL of the intercalation agent and magnetically stirred at room temperature for 12 h to intercalate TMAOH. + The ions are embedded into the interlayer of Mo-TiC MXene to expand the interlayer spacing; the obtained solution is collected by centrifugation at 10000r / min for 10min, and washed by centrifugation with deionized water until the pH value is ≥7, thereby obtaining a few-layer Mo-TiC MXene precursor with TMAOH removed;
[0036] (2-2) 0.8 g of the above-mentioned few-layer Mo-TiC MXene precursor was dispersed again in 25 mL of deionized water. After shaking and mixing at room temperature for 5 min, the obtained suspension was centrifuged at 3500 r / min for 60 min to obtain a supernatant. The supernatant collection process was repeated 4 times to increase the yield. The combined supernatant of about 100 mL was the few-layer Mo-TiC MXene solution;
[0037] (3) Preparation of few-layer Mo-TiC MXene-O powder
[0038] 40 mL of the above few-layer Mo-TiC MXene solution was measured, and after magnetic stirring and condensation reflux in a 50°C oil bath for 72 hours, it was freeze-dried at -90°C for 48 hours to obtain a few-layer Mo-TiC MXene-O powder; in this way, the few-layer Mo-TiC MXene-O was obtained by an in-situ pre-oxidation process, providing a molybdenum oxide intermediate phase for the formation of MoC and Mo2N in the next in-situ heat treatment process;
[0039] (4) Preparation of Mo-TiC MXene / MoC-Mo2N
[0040] According to the mass ratio of few-layer Mo-TiC MXene-O to dicyandiamide = 1:1, the few-layer Mo-TiC MXene-O powder and dicyandiamide were placed at both ends of a porcelain boat respectively, and placed in the middle of a quartz tube furnace, wherein dicyandiamide was placed at the air inlet end and the few-layer Mo-TiC MXene-O powder was placed at the air outlet end; argon gas was introduced at a flow rate of 200 mL / min, and the temperature was first increased to 400°C at 2°C / min for heat treatment for 2 h, and then increased to 750°C at 5°C / min for heat treatment for 2 h, to obtain a Mo-TiC MXene / MoC-Mo2N electromagnetic absorbing material with multi-band response (see Figure 1 and Figure 2 ).
[0041] The Mo-TiC MXene / MoC-Mo2N multi-band electromagnetic absorbing material prepared in this embodiment has a reflection loss of -65.2dB, -52.2dB, -22.8dB, -14.8dB, -27.2dB, -47.2dB, -17.0dB, -15.1dB and -15.0dB at a matching thickness of 1.565mm, 1.7mm, 2.0mm, 2.245mm, 3.0mm, 3.165mm, 3.975mm, 4.5mm and 5.0mm within a frequency range of 2 to 18GHz, and these reflection losses are all less than -10dB, achieving effective and multi-band electromagnetic absorption. The optimal reflection loss is -65.2dB, and the matching thickness is 1.565mm (see Figure 3 ).
[0042] Comparative Example 1:
[0043] This comparative example adopts the preparation method of the embodiment of the present invention, and the few-layer Mo-TiC MXene-O prepared in step (3) is used as the electromagnetic absorbing material.
[0044] The electromagnetic absorbing material prepared in this comparative example is Mo-TiC MXene-O. In the frequency range of 2 to 18 GHz and the matching thickness of 1.565 to 5 mm, the optimal reflection loss is -13.6 dB, and the matching thickness is 5 mm (see Figure 4 ).
[0045] Comparative Example 2:
[0046] This comparative example adopts the preparation method of the embodiment of the present invention, which is different from the embodiment in that: 0g of dicyandiamide is added in step (4).
[0047] The electromagnetic absorbing material prepared in this comparative example is Mo-TiC MXene-OP. In the frequency range of 2 to 18 GHz and the matching thickness of 1.565 to 5 mm, the optimal reflection loss is -12 dB, and the matching thickness is 5 mm (see Figure 4 ).
[0048] Comparative Example 3:
[0049] This comparative example adopts the preparation method of the embodiment of the present invention, which is different from the embodiment in that: the few-layer Mo-TiC MXene solution obtained in step (2) is freeze-dried to obtain a few-layer Mo-TiC MXene powder; and the few-layer Mo-TiC MXene powder and dicyandiamide are used for preparation in step (4).
[0050] The electromagnetic absorbing material prepared in this comparative example is Mo-TiC MXene-CN-P. In the frequency range of 2 to 18 GHz and the matching thickness of 1.565 to 5 mm, the optimal reflection loss is -5.4 dB, and the matching thickness is 3 mm (see Figure 4 ).
[0051] The Mo-TiC MXene / MoC-Mo2N multi-band electromagnetic absorbing material prepared in the embodiment of the present invention is Figure 1 and 3 As shown in Figure 2, a large number of MoC and Mo2N nanoparticles are in situ synthesized on the surface of a few-layer Mo-TiC MXene, and the dielectric loss capacity of the material is regulated to achieve efficient multi-band electromagnetic absorption; Figure 4 As shown, compared with the electromagnetic absorbing materials of Comparative Examples 1, 2 and 3, the embodiment of the present invention has stronger electromagnetic absorbing ability, thinner matching thickness and wider effective absorption bandwidth.
Claims
1. A method for preparing a novel multi-band responsive Mo-TiC MXene / MoC-Mo2N electromagnetic absorbing material, characterized in that The following steps are involved: (1) Preparation of multilayer Mo-TiC MXene Mo2TiAlC2 MAX is used as a raw material and hydrofluoric acid with a concentration of 40% is used as an etchant. The raw material: etchant is stirred and mixed according to a mass volume ratio of 0.5-1 g to 20-60 mL, and then the mixture is collected by centrifugation and washed to obtain an undried multilayer Mo-TiCMXene. (2) Preparation of few-layer Mo-TiC MXene (2-1) The undried multilayer Mo-TiC MXene is used as a material and TMAOH with a concentration of 5 wt% is used as an intercalation agent, and the mixture is stirred and mixed according to a mass volume ratio of material: intercalation agent = 0.5-1.2 g: 20-40 mL, and then the mixture is collected by centrifugation and washed to obtain a few-layer Mo-TiC MXene precursor from which TMAOH is removed; (2-2) according to the mass volume ratio of few-layer Mo-TiC MXene precursor: deionized water = 0.7-1.5 g: 20-30 mL, the few-layer Mo-TiC MXene precursor is dispersed again in deionized water and mixed together, and then the supernatant is obtained by centrifugation, and the supernatant collection process is repeated to obtain the few-layer Mo-TiC MXene solution; (3) Preparation of few-layer Mo-TiC MXene-O powder The few-layer Mo-TiC MXene solution is stirred and condensed under reflux in a constant temperature environment, and then freeze-dried to obtain a few-layer Mo-TiC MXene-O powder; (4) Preparation of Mo-TiC MXene / MoC-Mo2N According to the mass ratio of few-layer Mo-TiC MXene-O: dicyandiamide=1-2:0.5-4, the few-layer Mo-TiC MXene-O powder and dicyandiamide are respectively placed at both ends of a porcelain boat, which is placed in a tubular furnace, wherein the dicyandiamide is placed at the air inlet end and the few-layer Mo-TiC MXene-O powder is placed at the air outlet end; argon gas is introduced at a flow rate of 200-400 mL / min, the temperature is increased at 2°C / min to 350-550°C for heat treatment for 1-4 hours, and then the temperature is increased at 5°C / min to 700-850°C for heat treatment for 1-4 hours, so as to obtain a Mo-TiC MXene / MoC-Mo2N electromagnetic absorbing material with multi-band response.
2. The method for preparing the novel multi-band responsive Mo-TiC MXene / MoC-Mo2N electromagnetic absorbing material according to claim 1, characterized in that: The stirring and mixing time in step (1) is 72 to 96 hours; the rotation speed of centrifugal collection is 3000 to 8000 r / min, and the time of centrifugal collection is 5 to 30 minutes; the washing solution is deionized water, and the washing is performed until the pH value is ≥7.
3. The method for preparing the novel multi-band responsive Mo-TiC MXene / MoC-Mo2N electromagnetic absorbing material according to claim 1, characterized in that: The stirring and mixing time in the step (2-1) is 12 to 24 hours, the speed of centrifugal collection is 10,000 to 13,000 r / min, the time of centrifugal collection is 5 to 30 minutes, the washing solution is deionized water, and the washing is performed until the pH value is ≥ 7; the speed of centrifugal collection in the step (2-2) is 3,000 to 4,000 r / min, and the time of centrifugal collection is 30 to 60 minutes; the supernatant collection process is repeated 3 to 6 times.
4. The method for preparing the novel multi-band responsive Mo-TiC MXene / MoC-Mo2N electromagnetic absorbing material according to claim 1, characterized in that: The stirring and condensation reflux temperature in step (3) is 40 to 50° C. and the time is 48 to 72 hours; the freeze-drying time is 48 to 72 hours.
5. A product obtained by the method for preparing the novel multi-band responsive Mo-TiC MXene / MoC-Mo2N electromagnetic absorbing material according to any one of claims 1 to 4.
6. The product according to claim 5, characterized in that: The multi-band electromagnetic absorbing material has a reflection loss of -14.8 to -65.2 dB at a matching thickness of 1.565 to 5 mm within a frequency range of 2 to 18 GHz.
Citation Information
Patent Citations
A method for prepare a nitrogen doped carbon nanotube three-dimensional composite material by in-situ growth of a small lay of titanium carbide
CN109167066A
Preparation method of MXene wrinkled nanospheres
CN113387357A
Nanometer nickel elementary substance and graphite carbon modified titanium carbide composite wave-absorbing material and preparation method thereof
CN116179155A
Preparation method and product of novel efficient ultrathin Mo2TiC2 MXene / MoS2 electromagnetic wave absorbing material
CN117303446A
Transition metal carbonitride mxene films for EMI shielding
US20210261415A1