Preparation method of thermoplastic vulcanized rubber material for automobile cooling water pipe
Through the cooperation of ethylene propylene rubber and polypropylene dynamic vulcanization technology and additives, the problem of reducing aging resistance of thermoplastic vulcanized rubber materials is solved, and high-strength, lightweight, and environmentally friendly automotive cooling water pipe materials are achieved, which extends the service life and Reduced production costs.
Patent Information
- Application Number
- CN202411255523.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-09
- Publication Date
- 2024-11-15
AI Technical Summary
During the use of existing thermoplastic vulcanized rubber materials, there is no chemical action between the anti-aging agent and the rubber material matrix, which leads to the migration and removal of the anti-aging agent, which reduces the aging resistance of the material, and thus shortens the service life of the automobile cooling water pipes, causing resources. and economic waste.
Using dynamic vulcanization technology of ethylene propylene rubber and polypropylene, through reasonable formulation and production process design, additives and crosslinking agents are added to form thermoplastic vulcanized rubber materials with high-efficiency antioxidant properties, ensuring the stability and durability of the material under high temperature environment. sex.
It significantly improves the aging resistance, elasticity and compression deformation resistance of thermoplastic vulcanized rubber materials, extends the service life of the material, meets the high-performance needs of automobile cooling water pipes, and reduces production costs.
Smart Images

Figure CN118956064A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of automobile cooling water pipes, and in particular relates to a method for preparing a thermoplastic vulcanized rubber material for automobile cooling water pipes. Background Art
[0002] As an important component of new energy vehicles, the main function of automobile cooling water pipes is to transport coolant inside and outside the battery pack to cool the motor or battery. Affected by the high temperature of the battery pack and the working environment, the manufacturing materials are required to have high resistance to high temperature, cooling water, ozone and weathering, so the requirements for materials are relatively high.
[0003] Thermoplastic vulcanized rubber has good elasticity and resistance to compression deformation, and its environmental and aging resistance are equivalent to EPDM. At the same time, its oil and solvent resistance are comparable to general-purpose chloroprene rubber. Thermoplastic vulcanized rubber can be used in the temperature range of -60℃ to 135℃. Thermoplastic vulcanized rubber does not need to be vulcanized when used, and can be directly processed and formed by extrusion and other methods, which can shorten the processing process and reduce processing costs. At present, the use of thermoplastic vulcanized rubber materials to extrude cooling water pipe products has become the mainstream in the market.
[0004] However, although the thermoplastic vulcanized rubber materials in the prior art have good aging resistance, with the extension of service time and the influence of the external environment, since there is no chemical reaction between the anti-aging agent and the rubber material matrix, the anti-aging agent will gradually migrate and fall out, thereby significantly reducing the aging resistance of the thermoplastic vulcanized rubber material, greatly reducing the service life of the vulcanized rubber material, and also reducing the service life of the automobile cooling water pipe, resulting in a waste of resources and economy. Summary of the invention
[0005] The purpose of the present invention is to overcome the defects of the prior art and provide a method for preparing an extrusion-grade thermoplastic vulcanized rubber material for automobile cooling water pipes.
[0006] The purpose of the present invention can be achieved through the following technical solutions: A method for preparing a thermoplastic vulcanized rubber material for automobile cooling water pipes comprises the following steps: (1) Weigh 100-250 parts of EPDM rubber, 100-250 parts of polypropylene, 20-150 parts of processing oil, 10-80 parts of filler, 0.2-10 parts of vulcanization system, 2-3 parts of antioxidant, 3.5-6.5 parts of lubricant, 2.5-5.5 parts of auxiliary agent, 1-3 parts of accelerator, 3-8 parts of zinc oxide, and 0.5-1 parts of crosslinking agent by weight; (2) EPDM rubber, 45% processing oil, filler, antioxidant, additive, accelerator, zinc oxide and crosslinking agent are mixed in an internal mixer and then extruded into a rubber masterbatch by a single screw extruder; (3) After the rubber masterbatch, polypropylene and lubricant are mixed at high speed in a high-speed mixer for 2-5 minutes, they are transferred to a twin-screw for dynamic vulcanization, and then the intermediate masterbatch is made through a pelletizing device; (4) After the melt blending, the intermediate masterbatch and the vulcanization system are mixed at high speed in a high-speed mixer for 5-10 minutes, and then transferred to the twin-screw again for dynamic vulcanization. 55% of processing oil is added to the rear section of the twin-screw extruder stage to complete the blending and granulation. The feed speed is 20-100 rpm / min, the screw speed is 290-500 rpm / min, the screw aspect ratio is 55-64, and the processing temperature is 150-220°C. The uniformly mixed materials are accurately added to the twin-screw extruder for mixing, drawing, cooling and pelletizing to obtain a thermoplastic vulcanized rubber material.
[0007] Thermoplastic vulcanized rubber materials prepared by dynamic vulcanization of EPDM rubber and polypropylene have very excellent properties and can meet the performance requirements of automobile cooling water pipes.
[0008] The present invention prepares thermoplastic rubber with high strength and excellent extrudability by selecting suitable materials and changing the traditional formula. The produced cooling water pipe has the characteristics of lightweight, environmentally friendly and recyclable materials, and space saving, and is more convenient to assemble the cooling water pipe on the car, thereby improving production efficiency.
[0009] Furthermore, the EPDM rubber is an EPDM rubber with ethylene norbornene as the third monomer.
[0010] Furthermore, the ethylene norbornene content is 2%-10%.
[0011] Furthermore, the EPDM rubber Mooney viscosity ML (1+4) At 125℃, the temperature is 40-60, and the ethylene content is 30%-70%.
[0012] Furthermore, the polypropylene is a copolymer of propylene and other polymer units, and has a melt index of 0.5-3 g / 10 min.
[0013] Furthermore, the other polymerization units are one or more of ethylene, butene, hexene, and octene, and the content of the other polymerization units is less than 50%.
[0014] Furthermore, the processing oil is one or more of paraffin oil, cycloparaffin oil and aromatic oil.
[0015] Furthermore, the filler is one or more of talc powder, calcined clay, calcium carbonate, and mica powder.
[0016] Furthermore, the vulcanization system is a phenolic resin vulcanization system.
[0017] Furthermore, the antioxidant is one or both of antioxidant 1076 and antioxidant B215.
[0018] Furthermore, the lubricant is one or more of PE wax, stearic acid, and liquid lubricant.
[0019] Furthermore, the auxiliary agent is prepared by the following steps: S1. Add cyanuric chloride, antioxidant 4010NA (N-isopropyl-N-phenyl-p-phenylenediamine) and 1,4-dioxane to a dry three-necked flask under nitrogen protection, stir until completely dissolved, add pyridine, and then stir and react for 8 hours in an ice-water bath (0°C). After the reaction, distill under reduced pressure, purify by column chromatography (the eluent is a mixed solvent of benzene and acetone, and the volume ratio of benzene and acetone is 9:1), and distill under reduced pressure to obtain intermediate 1; the dosage ratio of cyanuric chloride, antioxidant 4010NA, pyridine and 1,4-dioxane is 14.8g:19.6g:8.4mL:200mL; Pyridine is used as an acid-binding agent to control the molar ratio of cyanuric chloride to antioxidant 4010NA to be 1:1.05-1.1. The -Cl of cyanuric chloride and the -NH2 of antioxidant 4010NA undergo a nucleophilic substitution reaction. The reaction process is as follows: S2. Under nitrogen protection, the intermediate 1 was dissolved in 1,4-dioxane, and 3-butene-1-ol and triethylamine were added in sequence after stirring evenly. The temperature was raised to 50°C and stirred for 6 hours. After the reaction was completed, the mixture was cooled to room temperature, and the mixture was distilled under reduced pressure. The mixture was purified by column chromatography (a mixed solvent of benzene and ethyl acetate was used as the eluent, and the volume ratio of benzene and ethyl acetate was 8:2). The intermediate 2 was obtained by distillation under reduced pressure. The usage ratio of the intermediate 1, 3-butene-1-ol, triethylamine and 1,4-dioxane was 28.1 g: 6.9 mL: 15.6 mL: 180 mL. Under heating conditions, triethylamine is used as an acid binding agent to control the molar ratio of intermediate 1 and 3-butene-1-ol to be 1:1.05-1.1, and the -Cl of intermediate 1 and the -OH of 3-butene-1-ol undergo a substitution reaction. The reaction process is as follows: S3. In a dry brown three-necked flask under nitrogen protection, add resorcinol, anhydrous aluminum chloride and DMF (N,N-dimethylformamide) in sequence, stir evenly, add intermediate 2, then stir and heat to 115°C, keep warm for 12 hours, after the reaction is completed, slowly pour the reaction mixture into ice water, precipitate solid, filter, and recrystallize to obtain an auxiliary agent; the dosage ratio of intermediate 2, resorcinol, anhydrous aluminum chloride and DMF is 24.6g:7.1mL:4g:200mL.
[0020] The molar ratio of intermediate 2 to resorcinol is controlled to be 1:1.3-1.4, and intermediate 2 and resorcinol undergo Friedel-Crafts acylation reaction under the catalysis of anhydrous aluminum chloride. The reaction process is as follows: The auxiliary agent contains triazine structures and aromatic amine structures. Compared with stabilizers with benzophenone and benzotriazole structures, triazine structures have higher absorption coefficients and can strongly absorb ultraviolet rays of 280nm-400nm. In addition, triazine structures have the advantages of high efficiency, high temperature resistance, light color and good compatibility. The mechanism of action of triazine structures is that the chelate ring formed by intramolecular hydrogen bonds is destroyed after absorbing ultraviolet light, forming unstable high-energy ionic compounds, and then releasing excess energy to restore the original low-energy stable state, thereby absorbing ultraviolet light; the aromatic amine structure in the auxiliary agent of the present invention is a universal antioxidant for synthetic rubber, natural rubber, etc., and has excellent protection performance against ozone cracking and flex cracking. It is also an excellent protective agent for heat, oxygen, light and general aging. At the same time, it can also inhibit the aging effect of variable-valence metal ions, and its protective performance is more comprehensive than antioxidant 4010 and the like.
[0021] In addition, the additive of the present invention also contains carbon-carbon double bonds, which can produce chemical reactions with the unsaturated double bonds of the side chains of the EPDM rubber under the action of the cross-linking agent, and then be grafted onto the EPDM rubber macromolecular chain. Therefore, the additive is not easy to migrate out and fall off, and can fully and stably play its role, thereby making the thermoplastic vulcanized rubber material of the present invention have efficient and lasting anti-ultraviolet effect and anti-aging performance, not easy to age, and greatly prolonging the service life of the thermoplastic vulcanized rubber material of the present invention.
[0022] Furthermore, the cross-linking agent is one or both of dibenzoyl peroxide and thiocyanate.
[0023] Beneficial effects of the present invention: 1. The additive of the present invention contains triazine structures and aromatic amine structures, and has a chemical reaction with EPDM rubber, so the additive is not easy to migrate out and fall off. The thermoplastic vulcanized rubber material prepared by using the additive and dynamic vulcanization technology has excellent and stable aging resistance, elasticity, compression deformation resistance, environmental resistance and coolant resistance. 2. The present invention increases the proportion of polypropylene and processing oil through reasonable formula and production process design to prepare a high-strength, high-fluidity thermoplastic vulcanized rubber material. When used for automobile cooling water pipes, the automobile cooling water pipes have excellent coolant resistance, flexibility and easy assembly characteristics; 3. The thermoplastic vulcanized rubber body prepared by the present invention can be processed by injection molding, blow molding, and extrusion. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] The present invention will be further described below in conjunction with the accompanying drawings.
[0025] Figure 1 This is a diagram of an automobile cooling water pipe made from the vulcanized rubber material of Example 2. DETAILED DESCRIPTION
[0026] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] The brands and sources of raw materials used in all embodiments and comparative examples are shown in Table 1 below: Table 1 Preparation of auxiliary agent, the specific steps are as follows: S1. Under nitrogen protection, 14.8 g of cyanuric chloride, 19.6 g of antioxidant 4010NA and 200 mL of 1,4-dioxane were added to a 500 mL dry three-necked flask, stirred until completely dissolved, 8.4 mL of pyridine was added, and then stirred in an ice-water bath (0°C) for 8 h. After the reaction was completed, it was distilled under reduced pressure, purified by column chromatography (the eluent was a mixed solvent of benzene and acetone, and the volume ratio of benzene and acetone was 9:1), and distilled under reduced pressure to obtain intermediate 1; S2. Under nitrogen protection, 28.1 g of intermediate 1 was dissolved in 180 mL of 1,4-dioxane, and after stirring evenly, 6.9 mL of 3-butene-1-ol and 15.6 mL of triethylamine were added in sequence, and the temperature was raised to 50°C and stirred for 6 h. After the reaction was completed, the mixture was cooled to room temperature, and the mixture was distilled under reduced pressure. The mixture was purified by column chromatography (a mixed solvent of benzene and ethyl acetate was used as the eluent, and the volume ratio of benzene and ethyl acetate was 8:2), and distilled under reduced pressure to obtain intermediate 2. S3. In a 500-mL dry brown three-necked flask under nitrogen protection, add 7.1 mL of resorcinol, 4 g of anhydrous aluminum chloride and 200 mL of DMF in sequence, stir evenly, add 24.6 g of intermediate 2, then stir and heat to 115°C, keep warm for 12 h, and after the reaction is completed, slowly pour the reaction mixture into ice water, precipitate solid, filter, and recrystallize to obtain an auxiliary agent.
[0028] The specific formula for preparing the thermoplastic vulcanized rubber material is shown in Table 2 below: Table 2 Example 2 to Example 5 The two-step method for preparing thermoplastic vulcanized rubber materials is as follows: (1) Weigh the raw materials according to the formula in Table 2; (2) mixing EPDM rubber, 45% processing oil, filler, antioxidant, additive, accelerator, zinc oxide, and crosslinking agent by weight through an internal mixer and then extruding through a single screw extruder to prepare a rubber masterbatch; (3) After mixing the rubber masterbatch, polypropylene and lubricant in a high-speed mixer for 2-5 minutes, the mixture is transferred to a twin-screw for dynamic vulcanization, and then the intermediate masterbatch is prepared by a pelletizing device; wherein the feed speed is 20-100 rpm / min, the screw speed is 290-500 rpm / min, the screw aspect ratio is 55-64, the processing zone 1 temperature is 160°C, the zone 2 temperature is 180°C, the zone 3 temperature is 180°C, the zone 4 temperature is 180°C, the zone 5 temperature is 180°C, the zone 6 temperature is 180°C, the zone 7 temperature is 180°C, the zone 8 temperature is 180°C, the zone 10 temperature is 180°C, the zone 11 temperature is 180°C, the zone 12 temperature is 185°C, and the zone 13 temperature is 185°C.
[0029] (4) After the melt blending, the intermediate masterbatch and the vulcanization system are mixed at high speed in a high-speed mixer for 5-10 minutes, and then transferred to a twin-screw again for dynamic vulcanization, and processing oil is added to the rear section of the twin-screw extruder stage to complete the blending and granulation (feeding speed 20-100 rpm / min, screw speed 290-500 rpm / min, screw aspect ratio 55-64, processing zone 1 temperature 160°C, zone 2 temperature 180°C, zone 3 temperature 185°C, zone 4 temperature 190°C, zone 5 temperature 190°C, zone 6 temperature 190°C, zone 7 temperature 195°C, zone 8 temperature 185°C, zone 10 temperature 185°C, zone 11 temperature 180°C, zone 12 temperature 180°C, zone 13 temperature 180°C), the uniformly mixed materials are accurately added to the twin-screw extruder for mixing, drawing, cooling and pelletizing to obtain a thermoplastic vulcanized rubber material.
[0030] Comparative Example 1 The two-step method for preparing thermoplastic vulcanized rubber materials is as follows: The remaining steps are the same as those in Example 2, except that the auxiliary agent and the cross-linking agent are removed to prepare a thermoplastic vulcanized rubber material.
[0031] Comparative Example 2 The one-step method for preparing thermoplastic vulcanized rubber material includes the following specific steps: (1) Weigh the raw materials according to the formula in Table 2; (2) mixing EPDM rubber, 45% processing oil, filler, antioxidant, additive, accelerator, zinc oxide, and crosslinking agent by weight through an internal mixer and then extruding through a single screw extruder to prepare a rubber masterbatch; (3) After the rubber masterbatch, polypropylene, lubricant and vulcanization system are mixed at high speed in a high-speed mixer for 2-5 minutes, they are transferred to a twin-screw again for dynamic vulcanization and processing oil is added to the rear section of the twin-screw extruder stage to complete the blending and granulation (feeding speed 20-100 rpm / min, screw speed 290-500 rpm / min, screw aspect ratio 55-64, processing zone 1 temperature 160°C, zone 2 temperature 180°C, zone 3 temperature 185°C, zone 4 temperature 190°C, zone 5 temperature 190°C, zone 6 temperature 190°C, zone 7 temperature 195°C, zone 8 temperature 185°C, zone 10 temperature 185°C, zone 11 temperature 180°C, zone 12 temperature 180°C, zone 13 temperature 180°C), the uniformly mixed materials are accurately added to the twin-screw extruder for mixing, drawing, cooling and pelletizing to obtain a thermoplastic vulcanized rubber material.
[0032] Comparative Example 3 to Comparative Example 4 The one-step method for preparing thermoplastic vulcanized rubber material includes the following specific steps: (1) Weigh the raw materials according to the formula in Table 2; (2) mixing EPDM rubber, 45% processing oil, filler, antioxidant, accelerator and zinc oxide by weight through an internal mixer and then extruding through a single screw extruder to prepare a rubber masterbatch; (3) After the rubber masterbatch, polypropylene, lubricant and vulcanization system are mixed at high speed in a high-speed mixer for 2-5 minutes, they are transferred to a twin-screw again for dynamic vulcanization and processing oil is added to the rear section of the twin-screw extruder stage to complete the blending and granulation (feeding speed 20-100 rpm / min, screw speed 290-500 rpm / min, screw aspect ratio 55-64, processing zone 1 temperature 160°C, zone 2 temperature 180°C, zone 3 temperature 185°C, zone 4 temperature 190°C, zone 5 temperature 190°C, zone 6 temperature 190°C, zone 7 temperature 195°C, zone 8 temperature 185°C, zone 10 temperature 185°C, zone 11 temperature 180°C, zone 12 temperature 180°C, zone 13 temperature 180°C), the uniformly mixed materials are accurately added to the twin-screw extruder for mixing, drawing, cooling and pelletizing to obtain a thermoplastic vulcanized rubber material.
[0033] The vulcanized rubber materials obtained in Examples 2-5 and Comparative Examples 1-4 were subjected to UV aging for 120 hours at room temperature, a vertical irradiation distance of 20 cm, and a 30W UV lamp. The tensile strength before and after aging was tested. The test results are shown in Table 3 below: Table 3 The materials obtained in Examples 1-2 and Comparative Examples 3-4 were placed in an oven for drying, and the required test specimens were prepared by an injection molding machine, and the dust cover samples were prepared by a blow molding machine for performance testing. The test results are shown in Table 4 below: Table 4 The above test results show that the vulcanized material prepared in the embodiment of the present invention can obtain a thermoplastic vulcanized rubber material with high strength and good extrusion performance, and can obtain an easy-to-assemble automobile cooling water pipe through blow molding. Figure 1 This is a diagram of an automobile cooling water pipe made from the vulcanized rubber material of Example 2.
[0034] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0035] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A method for preparing a thermoplastic vulcanized rubber material for automobile cooling water pipes, It is characterized in that The following steps are involved: (1) Weigh 100-250 parts of EPDM rubber, 100-250 parts of polypropylene, 20-150 parts of processing oil, 10-80 parts of filler, 0.2-10 parts of vulcanization system, 2-3 parts of antioxidant, 3.5-6.5 parts of lubricant, 2.5-5.5 parts of auxiliary agent, 1-3 parts of accelerator, 3-8 parts of zinc oxide, and 0.5-1 parts of crosslinking agent by weight; (2) EPDM rubber, 45% processing oil, filler, antioxidant, additive, accelerator, zinc oxide and crosslinking agent are mixed in an internal mixer and then extruded into a rubber masterbatch by a single screw extruder; (3) After the rubber masterbatch, polypropylene and lubricant are mixed at high speed in a high-speed mixer for 2-5 minutes, they are transferred to a twin-screw for dynamic vulcanization, and then the intermediate masterbatch is made through a pelletizing device; (4) After the intermediate masterbatch and the vulcanization system are mixed at high speed in a high-speed mixer for 5-10 minutes, they are transferred to a twin-screw again for dynamic vulcanization, and 55% processing oil is added to the rear section of the twin-screw extruder stage to complete the blending and granulation. The feed speed is 20-100 rpm / min, the screw speed is 290-500 rpm / min, the screw aspect ratio is 55-64, and the processing temperature is 150-220°C. The mixed materials are added to a twin-screw extruder for mixing, drawing, cooling and pelletizing to obtain a thermoplastic vulcanized rubber material.
2. A method for preparing a thermoplastic vulcanized rubber material for automobile cooling water pipe according to claim 1, It is characterized in that The auxiliary agent is prepared by the following steps: S1. Add cyanuric chloride, antioxidant 4010NA and 1,4-dioxane into a flask, stir, add pyridine, react at 0°C for 8h, distill under reduced pressure, purify by column chromatography, and distill under reduced pressure to obtain intermediate 1; S2, under nitrogen protection, the intermediate 1 was dissolved in 1,4-dioxane, and then 3-butene-1-ol and triethylamine were added, reacted at 50°C for 6h, distilled under reduced pressure, purified by column chromatography, and distilled under reduced pressure to obtain the intermediate 2; S3. Under nitrogen protection, add resorcinol, anhydrous aluminum chloride and DMF into a flask, add intermediate 2 with stirring, react at 115° C. for 12 h, pour into ice water, precipitate solid, filter, and recrystallize to obtain an auxiliary agent.
3. A method for preparing a thermoplastic vulcanized rubber material for automobile cooling water pipe according to claim 2, It is characterized in that The usage ratio of cyanuric chloride, antioxidant 4010NA, pyridine and 1,4-dioxane in step S1 is 14.8g:19.6g:8.4mL:200mL; the usage ratio of intermediate 1, 3-butene-1-ol, triethylamine and 1,4-dioxane in step S2 is 28.1g:6.9mL:15.6mL:180mL; the usage ratio of intermediate 2, resorcinol, anhydrous aluminum chloride and DMF in step S3 is 24.6g:7.1mL:4g:200mL.
4. A method for preparing a thermoplastic vulcanized rubber material for automobile cooling water pipe according to claim 1, It is characterized in that The EPDM rubber is an EPDM rubber with ethylene norbornene as the third monomer, and the content of ethylene norbornene is 2%-10%.
5. A method for preparing a thermoplastic vulcanized rubber material for automobile cooling water pipe according to claim 1, It is characterized in that The EPDM rubber Mooney viscosity ML (1+4) At 125℃, the temperature is 40-60, and the ethylene content is 30%-70%.
6. A method for preparing a thermoplastic vulcanized rubber material for automobile cooling water pipe according to claim 1, It is characterized in that The polypropylene is a copolymer of propylene and other polymer units, with a melt index of 0.5-3g / 10min, and the other polymer units are one or more of ethylene, butene, hexene, and octene, and the content of the other polymer units is less than 50%.
7. A method for preparing a thermoplastic vulcanized rubber material for automobile cooling water pipe according to claim 1, It is characterized in that The processing oil is one or more of paraffin oil, naphthenic oil, and aromatic oil; the filler is one or more of talcum powder, calcined clay, calcium carbonate, and mica powder; and the vulcanization system is a phenolic resin vulcanization system.
8. A method for preparing a thermoplastic vulcanized rubber material for automobile cooling water pipe according to claim 1, It is characterized in that The antioxidant is one or both of antioxidant 1076 and antioxidant B215; the lubricant is one or more of PE wax, stearic acid, and liquid lubricant; and the crosslinking agent is one or both of dibenzoyl peroxide and thiocyanate.
Citation Information
Cited By
Solvent-resistant TPV (thermoplastic vulcanizate) material with high melt strength and preparation method thereof
CN119708706A
PVC / PU modified material and preparation method thereof
CN120518957A