Anti-static coating material and preparation method thereof as well as anti-static coating and generation method thereof
By using a combination of strong electron-supply and strong electron-absorbing organic matter, an anti-static coating material that can be closely combined with a variety of substrate materials is prepared, which solves the problem of poor universality of existing anti-static materials and realizes the use of various scenarios effective electrostatic dissipation effect.
Patent Information
- Application Number
- CN202411114245.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-19
AI Technical Summary
Existing antistatic materials are poorly universal in some application scenarios, which limits the selection and use range of materials, especially in environments filled with dust or flammable gases, which are prone to explosions.
Using a combination of strong electron-supplying organic substances and strong electron-going organic substances, containing amino groups and fluorine ions, an anti-static coating material that can be closely linked to a variety of substrate materials is prepared by forming a composite solution and adding anhydrous ethanol to balance the charge to satisfy the Electrostatic dissipation requirements.
It improves the universality and stability of anti-static coating materials to base materials, expands the scope of application, can effectively eliminate or reduce static charge accumulation, and meets the electrostatic dissipation needs of different application scenarios.
Smart Images

Figure CN118978860A_ABST
Abstract
Description
Technical Field
[0001] The embodiments of the present disclosure relate to the field of material technology, and in particular, to an antistatic coating material, a method for preparing the antistatic coating material, an antistatic coating, and a method for generating the antistatic coating. Background Art
[0002] Contact electrification is one of the most common physical phenomena in life. Contact electrification plays an important role in energy collection, particle separation, chemical synthesis and other fields. However, contact electrification may also cause some unpleasant feelings or even serious disasters. If this discharge occurs in a dusty factory or a space with flammable gas, it is very likely to cause an explosion. Therefore, in these application scenarios, the use of antistatic materials or surfaces plays a very important role.
[0003] The existing antistatic strategies mainly include the following: the first is to increase the electrostatic charge diffusion rate of the material to avoid excessive charge accumulation, such as doping the material with highly conductive fillers, free radical scavenging molecules or surface hydrophilic modification. Another antistatic strategy is to avoid the generation of charge, which is generally achieved through chemical modification.
[0004] However, the above-mentioned bulk-modified copolymerization method limits the selection of materials and is not widely applicable. Summary of the invention
[0005] The purpose of the present disclosure is to provide an antistatic coating material, a preparation method of the antistatic coating material, an antistatic coating and a method for generating an antistatic coating, thereby at least to a certain extent overcoming the problem of poor universality of the antistatic coating material to the substrate material due to the limitations and defects of the relevant technology.
[0006] According to one aspect of the present disclosure, an antistatic coating material is provided, the components of the antistatic coating material comprising: a strong electron-donating organic substance, a strong electron-withdrawing organic substance, and anhydrous ethanol;
[0007] The strong electron-donating organic matter contains amino groups, and the strong electron-withdrawing organic matter contains fluorine ions.
[0008] In an exemplary embodiment of the present disclosure, the strong electron donating organic matter includes one or more of N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, diethylenetriaminopropyltrimethoxysilane, N-aminoethyl-3-aminopropyltriethoxysilane, and N-methyl-3-aminopropyltrimethoxysilane.
[0009] In an exemplary embodiment of the present disclosure, the strong electron-withdrawing organic matter includes one or more of trimethoxy (1H, 1H, 2H, 2H-tridecafluorooctyl) silane, 1H, 1H, 2H, 2H-perfluorodecyltriethoxysilane, trimethoxy (1H, 1H, 2H, 2H-heptadecafluorodecyl) silane, trimethoxy (1H, 1H, 2H, 2H-nonafluorohexyl) silane, triethoxy-1H, 1H, 2H, 2H-tridecafluorooctylsilane, and 1H, 1H, 2H, 2H-perfluorododecyltriethoxysilane.
[0010] In an exemplary embodiment of the present disclosure, the molar percentage of the strong electron donating organic matter to the strong electron withdrawing organic matter is determined according to the ratio of positive charge to negative charge in the composite solution, and the composite solution includes the strong electron donating organic matter and the strong electron withdrawing organic matter.
[0011] In an exemplary embodiment of the present disclosure, the molar percentage of the strong electron donating organic matter and the strong electron withdrawing organic matter is adjusted according to the bonding force between the antistatic coating material and the base material.
[0012] According to one aspect of the present disclosure, a method for preparing an antistatic coating material is provided. The antistatic coating material is any one of the antistatic coating materials described above. The method for preparing the antistatic coating material comprises:
[0013] Mixing a strong electron-donating organic substance and a strong electron-withdrawing organic substance to obtain a composite solution, wherein the composite solution contains amino groups and fluoride ions;
[0014] Anhydrous ethanol is added to the composite solution to obtain the antistatic coating material.
[0015] According to one aspect of the present disclosure, an antistatic coating is provided, which is prepared according to any one of the antistatic coating materials described above.
[0016] According to one aspect of the present disclosure, a method for producing an antistatic coating is provided, for preparing the antistatic coating as described in any one of the above, comprising:
[0017] Cleaning the base material to form a base material with a clean surface;
[0018] Treating the base material according to any one of the above antistatic coating materials to obtain a base material containing the antistatic coating material;
[0019] The base material containing the antistatic coating material is dried to obtain an antistatic coating.
[0020] In an exemplary embodiment of the present disclosure, the base material containing the antistatic coating material is obtained by immersion or spraying.
[0021] In an exemplary embodiment of the present disclosure, the soaking duration of the soaking method is 30-50 minutes, and the number of spraying times of the spraying method is 3-10 times.
[0022] In the technical solution provided in the embodiment of the present disclosure, the components of the antistatic coating material include: strong electron donating organic matter, strong electron withdrawing organic matter and anhydrous ethanol; wherein, the strong electron donating organic matter contains amino groups, and the strong electron withdrawing organic matter contains fluoride ions. On the one hand, the strong electron donating organic matter contains amino groups, and the strong electron withdrawing organic matter contains fluoride ions. The silane present in the two components enables it to have a strong chemical bond to many base materials, increases the binding force between the antistatic coating material and the base material, improves the universality of the antistatic coating material to the base material, and increases the scope of application. On the other hand, using strong electron donating organic matter and strong electron withdrawing organic matter containing strong electron withdrawing groups and strong electron donating groups as balanced charges can meet the electrostatic dissipation requirements of the antistatic coating material, and will not limit the choice of materials, and has a wide range of applicability.
[0023] It is to be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present disclosure. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] The accompanying drawings herein are incorporated into the specification and constitute a part of the specification, illustrate embodiments consistent with the present disclosure, and together with the specification are used to explain the principles of the present disclosure. Obviously, the accompanying drawings described below are only some embodiments of the present disclosure, and for ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without creative work.
[0025] Figure 1 A schematic flow chart of a method for preparing an antistatic coating material in an embodiment of the present disclosure is schematically shown.
[0026] Figure 2 A flowchart schematically illustrates a method for generating an antistatic coating in an embodiment of the present disclosure.
[0027] Figure 3 The test results of the antistatic coating prepared according to Example 1 are schematically shown.
[0028] Figure 4 The test results of the antistatic coating prepared according to Example 2 are schematically shown. DETAILED DESCRIPTION
[0029] Example embodiments will now be described more fully with reference to the accompanying drawings. However, example embodiments can be implemented in a variety of forms and should not be construed as being limited to the examples set forth herein; on the contrary, these embodiments are provided so that the present disclosure will be more comprehensive and complete, and the concepts of the example embodiments are fully conveyed to those skilled in the art. The described features, structures, or characteristics may be combined in one or more embodiments in any suitable manner. In the following description, many specific details are provided to provide a full understanding of the embodiments of the present disclosure. However, those skilled in the art will appreciate that the technical solutions of the present disclosure may be practiced while omitting one or more of the specific details, or other methods, components, devices, steps, etc. may be adopted. In other cases, known technical solutions are not shown or described in detail to avoid obscuring various aspects of the present disclosure.
[0030] The terms "a", "an", "the" and "said" used in this specification are used to indicate the presence of one or more elements / components, etc.; the terms "including" and "having" are used to express an open-ended inclusion and mean that there may be additional elements / components, etc. in addition to the listed elements / components, etc.; the terms "first" and "second" etc. are used only as labels and are not intended to limit the quantity of their objects.
[0031] Contact electrification is one of the most common physical phenomena in life. On the one hand, contact electrification plays an important role in energy collection, particle separation, chemical synthesis and other fields, but on the other hand, contact electrification may also cause some unpleasant feelings or even serious disasters. If this discharge occurs in a dusty factory or a space with flammable gas, it is very likely to cause an explosion. Therefore, in these application scenarios, the use of antistatic materials or surfaces plays a very important role.
[0032] There are two main antistatic strategies. The first is to increase the electrostatic charge diffusion rate of the material to avoid excessive charge accumulation, such as doping the material with highly conductive fillers, free radical scavenging molecules, or surface hydrophilic modification. Another antistatic strategy is to avoid the generation of charge, which is generally achieved through chemical modification. However, this bulk modified copolymerization method limits the choice of materials and is not widely applicable.
[0033] Considering that contact electrification is an interfacial phenomenon, antistatic can be achieved only by chemical modification of the surface. Existing antistatic surfaces are mainly modified by patterned coatings, which generally include two areas. During friction, the two areas generate positive and negative charges respectively. By controlling the size and proportion of these two areas, equal amounts of positive and negative charges can be obtained, thereby achieving the effect of an overall zero charge. At this stage, with the increasing demand for material performance, it is necessary to provide an antistatic coating material that meets both the requirements of static dissipation and material universality.
[0034] In the embodiment of the present disclosure, an antistatic coating material is first provided, and the components of the antistatic coating material include: a strong electron-donating organic substance, a strong electron-absorbing organic substance, and anhydrous ethanol; wherein the strong electron-donating organic substance contains amino groups, and the strong electron-absorbing organic substance contains fluoride ions. The antistatic coating material is mixed with the strong electron-donating organic substance to form a composite solution, and then anhydrous ethanol is added to form a composite solution.
[0035] The antistatic coating material provided in the present disclosure embodiment, on the one hand, with the strong electron-withdrawing organic matter containing a strong electron-withdrawing group and the strong electron-donating organic matter containing a strong electron-donating group as the substrate for balancing the charge, the electrostatic dissipation requirement of the coating can be met. On the other hand, the strong electron-donating organic matter contains amino groups, so that the antistatic coating material can be closely adhered to a variety of base materials, ensuring the universality of the antistatic coating material to the base material. Therefore, by configuring the antistatic coating material comprising a strong electron-donating group and a strong electron-withdrawing group, the antistatic coating material can be coated on any base material, improving the material universality of the antistatic coating material, increasing the scope of application.
[0036] Next, the antistatic coating material in the embodiment of the present disclosure is described in detail.
[0037] Strong electron donating organic compounds refer to organic compounds that contain strong electron donating groups in their molecular structures. Strong electron withdrawing organic compounds refer to organic compounds that contain strong electron withdrawing groups in their molecular structures.
[0038] In some embodiments, the strong electron donating organic matter in the antistatic coating material contains an amino group, and the strong electron donating organic matter may include one or more of N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, diethylenetriaminopropyltrimethoxysilane, N-aminoethyl-3-aminopropyltriethoxysilane, and N-methyl-3-aminopropyltrimethoxysilane.
[0039] Strong electron-withdrawing organic matter in antistatic coating materials contains fluoride ions. Strong electron-withdrawing organic matter includes one or more of trimethoxy (1H, 1H, 2H, 2H-tridecafluorooctyl) silane, 1H, 1H, 2H, 2H-perfluorodecyl triethoxy silane, trimethoxy (1H, 1H, 2H, 2H-heptadecafluorodecyl) silane, trimethoxy (1H, 1H, 2H, 2H-nonafluorohexyl) silane, triethoxy-1H, 1H, 2H, 2H-tridecafluorooctyl silane, and 1H, 1H, 2H, 2H-perfluorododecyl triethoxy silane.
[0040] Exemplarily, the molar percentage of the strong electron donating organic matter and the strong electron withdrawing organic matter can be determined according to the electrostatic dissipation performance. Electrostatic dissipation performance refers to the use of eliminating or reducing the charge accumulation on the surface of the material, releasing the charge on the surface of the material, thereby achieving the elimination of static electricity. The electrostatic dissipation performance of the antistatic coating material can be improved with the balance of positive and negative charges in the strong electron donating organic matter and the strong electron withdrawing organic matter, that is, when the ratio of positive and negative charges in the strong electron donating organic matter and the strong electron withdrawing organic matter is 1:1, the electrostatic dissipation performance of the antistatic coating material is the largest.
[0041] On this basis, the molar percentage of strong electron donating organic matter and strong electron withdrawing organic matter can be determined according to the ratio of positive charge to negative charge in the strong electron donating organic matter and the strong electron withdrawing organic matter being 1:1.
[0042] Exemplarily, the strong electron donating organic matter and the strong electron withdrawing organic matter can be mixed to form a composite solution, and the molar percentage of the strong electron donating organic matter and the strong electron withdrawing organic matter can be determined according to the ratio of positive charge to negative charge in the composite solution. Among them, the ratio of positive charge to negative charge in the composite solution can be 1:1. Therefore, the molar percentage of the strong electron donating organic matter and the strong electron withdrawing organic matter can be any value between 0-1, for example, it can be determined according to the ratio when the ratio of positive charge to negative charge is 1:1, and is not specifically limited here.
[0043] Furthermore, after determining the molar percentage of the strong electron donating organic matter and the strong electron withdrawing organic matter, the molar percentage of the strong electron donating organic matter and the strong electron withdrawing organic matter can be adjusted according to the bonding force between the antistatic coating material and the substrate material.
[0044] Exemplarily, when the bonding force between the antistatic coating material and the substrate material is the first level, the molar percentage of the amino-containing organic matter can be increased, that is, the molar percentage of the strong electron-donating organic matter is increased. When the bonding force between the antistatic coating material and the substrate material is the second level, the molar percentage of the strong electron-donating organic matter and the strong electron-withdrawing organic matter can be determined according to the ratio of positive charge to negative charge in the composite solution of 1:1, that is, the molar percentage of the strong electron-donating organic matter is not increased, and the molar percentage determined according to the ratio of positive charge to negative charge in the composite solution is kept unchanged. Among them, the first level can be greater than the second level, that is, the bonding force represented by the first level is greater than the bonding force represented by the second level. In the disclosed embodiment, the antistatic coating material includes strong electron-donating organic matter and strong electron-withdrawing organic matter, which avoids the restriction of material selection in the related art, and solves the problem of poor stability of the current antistatic coating material while ensuring excellent electrostatic dissipation performance, improves the universality of the substrate material, and also improves the stability and reliability of the antistatic coating material.
[0045] In the embodiment of the present disclosure, a method for preparing an antistatic coating material is also provided. Figure 1 As shown in , it mainly includes the following steps:
[0046] In step S110, a strong electron-donating organic substance and a strong electron-withdrawing organic substance are mixed to obtain a composite solution, wherein the composite solution contains amino groups and fluoride ions;
[0047] In step S120, anhydrous ethanol is added to the composite solution to obtain the antistatic coating material.
[0048] In some embodiments, two organic substances containing strong electron donating groups and strong electron withdrawing groups are mixed to form a composite solution, and then anhydrous ethanol is added to the composite solution to obtain a mixed solution containing strong electron donating groups and strong electron withdrawing groups after dilution, and the mixed solution is used as an antistatic coating material.
[0049] In some embodiments, when forming a composite solution, the strong electron donating organic compound and the strong electron withdrawing organic compound can be ultrasonically mixed, and the ultrasonic mixing time can be 1-10 minutes, for example, 5 minutes. Exemplarily, two organic solvents containing strong electron withdrawing groups and strong electron donating groups are mixed, and then ultrasonically mixed at room temperature for 5 minutes to form a composite solution.
[0050] Further, a certain volume of absolute ethanol is added to the composite solution, stirred and ultrasonically mixed to form an antistatic coating material. Wherein, the stirring method can be magnetic stirring, the temperature of magnetic stirring is room temperature, and the stirring time is 5-15 minutes, for example, can be 10 minutes. The time of ultrasonic mixing is 5 minutes. For example, a certain volume of absolute ethanol is added to the composite solution, magnetic stirring is 10 minutes at room temperature, and ultrasonic 5 minutes are used to form an antistatic agent with good positive and negative charge dispersibility, and the antistatic agent is an antistatic coating material.
[0051] Furthermore, when configuring the antistatic coating material, the ratio of the two organic solvents, strong electron donating organic matter and strong electron withdrawing organic matter, can be determined according to the electrostatic dissipation performance. When the ratio of positive and negative charges in the composite solution composed of the two organic solvents is 1:1, its electrostatic dissipation performance reaches the best. When the proportion of strong electron donating groups, i.e. amino groups, increases in the composite solution composed of the two organic solvents, the surface bonding force of the antistatic coating material to the base material will be improved, but it may lead to a decrease in electrostatic dissipation performance. Therefore, it is necessary to comprehensively consider the electrostatic dissipation capacity and coating stability according to the application scenario of the base material.
[0052] In some embodiments, the antistatic coating can be prepared by the following method, which specifically includes the following steps:
[0053] Step 1, prepare the base material and the covering material: first prepare a 0.5% mass fraction of ethoxy polyethyleneimine solution, the solvent is 2-methoxyethanol, add zinc acetate so that the mass of the polymer and the mass of zinc acetate is 1:14, stir for 0.5h to obtain a clear solution;
[0054] Step 2, adding the Ag nanowire solution to the above clear solution, so that the mass fraction of the Ag nanowire is 25%, the mass ratio of the polymer to the Ag nanowire is 0.01:1, and shaking evenly;
[0055] Step 3, preparation process of antistatic coating: Take a 1.7×1.7 cm glass as a substrate, spin-coat the substrate material on the cleaned glass sheet at a rotation speed of 4000 rpm, and heat at 150°C for 10 minutes after 45 seconds to obtain a substrate layer. Further spin-coat at least one layer of antistatic coating material on the substrate layer to obtain a main layer. Continue to spin-coat the cover layer solution on the main layer to obtain an antistatic coating.
[0056] A layer of antistatic coating material is spin-coated on the above-mentioned base layer at a rotation speed of 5500rpm, and heated at 150°C for 10min after 45s; if the middle layer of the antistatic coating has two layers, the rotation speed of the first layer is 5500rpm, and heated at 150°C for 3min after 45s; the rotation speed of the second layer is 7000rpm, and heated at 150°C for 15min after 45s; if the middle layer of the antistatic coating has three layers, the rotation speed of the first layer is 5500rpm, and heated at 150°C for 3min after 45s; the rotation speed of the second layer is 7000rpm, and heated at 150°C for 3min after 45s; the rotation speed of the third layer is 8000rpm, and heated at 150°C for 15min after 45s; the number of layers of the middle layer is appropriately increased according to the conductivity requirements to obtain the main layer.
[0057] The cover layer solution is continuously spin-coated on the main layer at a rotation speed of 3000 rpm, and heated at 150°C for 10 min after 45 seconds to obtain a cover layer, thereby preparing an antistatic coating. The square resistance of the antistatic coating prepared by this method is between 10Ω and 10 11 Adjustable between Ω.
[0058] In the embodiment of the present disclosure, a method for generating an antistatic coating is also provided, referring to Figure 2 As shown in , it mainly includes the following steps:
[0059] In step S210, the base material is cleaned to form a base material with a clean surface;
[0060] In step S220, the base material is processed according to the antistatic coating material to obtain a base material containing the antistatic coating material;
[0061] In step S230, the base material containing the antistatic coating material is dried to obtain an antistatic coating.
[0062] In the disclosed embodiment, the base material is treated with an antistatic coating material to obtain a base material containing the antistatic coating material, and then dried to obtain an antistatic coating. The operation process is simple, thus improving the operation efficiency.
[0063] Next, the method for producing the antistatic coating is described in detail.
[0064] In step S210 , the base material is cleaned to form a base material with a clean surface.
[0065] In the embodiment of the present disclosure, the base material may be, for example, a glass material or an organic material. According to the intrinsic properties of the material, the base material is cleaned with water or ethanol to form a base material with a clean surface.
[0066] In step S220, the base material is processed according to the antistatic coating material to obtain a base material containing the antistatic coating material.
[0067] In the embodiment of the present disclosure, when the base material with a clean surface is treated with the antistatic coating material, it can be obtained by immersion or spraying. For example, the antistatic coating material can be directly sprayed on the surface of the base material with a clean surface, or the base material with a clean surface can be immersed in the antistatic coating material.
[0068] When the substrate material with a clean surface is treated by immersion, the immersion time may be 20-30 minutes. For example, the substrate material with a clean surface may be completely immersed in the antistatic agent for 30 minutes and then taken out.
[0069] When the substrate material with a clean surface is processed by spraying, the number of spraying times can be 2-5 times, for example, can be 3 times. The number of spraying times can be determined according to the thickness of the antistatic coating as needed, and the greater the thickness, the greater the number of spraying times. It should be noted that after completing a spraying, the next spraying can be carried out after it is naturally dried. For example, the antistatic coating material is evenly sprayed on the surface of the substrate material with a clean surface, after naturally drying, the next spraying is continued, and the above operation is repeated 3 times to obtain the substrate material containing the antistatic coating material.
[0070] In step S230, the base material containing the antistatic coating material is dried to obtain an antistatic coating.
[0071] In the disclosed embodiment, the drying time for drying the base material containing the antistatic coating material is 5 min-15 min, and the drying temperature is 75° C.-85° C.
[0072] For example, the base material containing the antistatic coating material can be placed in an oven with a drying temperature of 80°C and a drying time of 10 minutes to increase the adhesion between the antistatic coating material and the surface of the base material, and finally form an antistatic coating. Of course, the drying temperature or the drying time can also be adjusted, which is determined according to actual needs.
[0073] Next, the method for producing the antistatic coating in the embodiment of the present disclosure is described in detail.
[0074] Example 1
[0075] The antistatic coating is prepared by immersion. In the process of preparing the antistatic coating, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane (APTS) is selected as a strong electron-donating organic matter, and 1H,1H,2H,2H-perfluorooctyltrimethoxysilane (FOTS) is selected as a strong electron-withdrawing organic matter. The substrate material can be organic glass.
[0076] The main steps include:
[0077] Step 1. Prepare a composite solution: weigh 1 mL of N-(2-aminoethyl)-3-aminopropyltrimethoxysilane (APTS) and 1 mL of 1H,1H,2H,2H-perfluorooctyltrimethoxysilane (FOTS), mix them at room temperature, and rapidly ultrasonically vibrate for 5 minutes to form a composite solution.
[0078] Step 2: prepare an antistatic coating material: add 20 mL of anhydrous ethanol to the prepared composite solution, stir under magnetic stirring for 10 minutes at room temperature, and then ultrasonically vibrate for 5 minutes to form an antistatic coating material.
[0079] Step 3: Pretreatment of the substrate material: Wipe a 5 cm×5 cm piece of organic glass with anhydrous ethanol until the surface is clean and free of obvious contamination, thereby obtaining a substrate material with a clean surface.
[0080] Step 4: completely immerse the wiped plexiglass in the antistatic coating material at room temperature, take it out after soaking for 30 minutes, and dry it at room temperature.
[0081] Step 5: Place the dried organic glass in an oven at 80°C for 10 minutes to form an antistatic coating.
[0082] Step 6: Use a surface resistance meter to test the surface resistance of the organic glass coated with antistatic coating.
[0083] Among them, the test results show that the double-sided resistance is 10E8Ω, so the organic glass coated with anti-static coating has good static dissipation performance.
[0084] Example 2
[0085] The antistatic coating is prepared by spraying. In the process of preparing the antistatic coating, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane (APTS) is selected as a strong electron-donating organic compound, and 1H,1H,2H,2H-perfluorooctyltrimethoxysilane (FOTS) is selected as a strong electron-withdrawing organic compound. The base material can be polydimethylsiloxane (PDMS).
[0086] The preparation of antistatic coating by spraying mainly includes the following steps:
[0087] Step 1. Prepare a composite solution: weigh 1 mL of N-(2-aminoethyl)-3-aminopropyltrimethoxysilane (APTS) and 1 mL of 1H,1H,2H,2H-perfluorooctyltrimethoxysilane (FOTS), mix them at room temperature, and rapidly ultrasonically vibrate for 5 minutes to form a composite solution.
[0088] Step 2: prepare an antistatic coating material: add 20 mL of anhydrous ethanol to the prepared composite solution, stir under magnetic stirring for 10 minutes at room temperature, and then ultrasonically vibrate for 5 minutes to form an antistatic coating material.
[0089] Step 3: Pretreatment of substrate material: Wipe 4 cm×5 cm polydimethylsiloxane (PDMS) with anhydrous ethanol until the surface is clean and free of obvious contamination, thereby obtaining a substrate material with a clean surface.
[0090] Step 4: Use polydimethylsiloxane (PDMS) as the base material, keep the distance between the manual spray pot and polydimethylsiloxane (PDMS) at 15cm-20cm, dry naturally for 3 minutes after spraying, continue spraying, dry naturally, and repeat the spraying and natural drying process.
[0091] Step 5: After the last spraying is completed and dried, the polydimethylsiloxane (PDMS) dried at room temperature is transferred to an oven at 80° C. and dried for 10 minutes to form an antistatic coating.
[0092] Step 6: Use a surface resistance meter to test the surface resistance of polydimethylsiloxane (PDMS) coated with an antistatic coating.
[0093] Among them, the test results show that the double-sided resistance can be adjusted in a wide range from 10E7Ω-10E11Ω, for example, it can be 10E8Ω, so the polydimethylsiloxane (PDMS) coated with an antistatic coating has good electrostatic dissipation performance.
[0094] Figure 3 The test results of Example 1 are schematically shown in FIG. Figure 3 As shown in, according to the immersion method in Example 1, organic glass is used as the base material, and the antistatic coating material is used to treat the base material with a clean surface represented by the organic glass to obtain a base material containing the antistatic coating material, and the base material containing the antistatic coating material is further dried to obtain an antistatic coating. The test results of the antistatic coating obtained by the immersion method are that the double-sided resistance is 10E8Ω, and its order of magnitude is within the order of magnitude range corresponding to the antistatic requirement. Therefore, the organic glass coated with the antistatic coating prepared by Example 1 has good electrostatic dissipation performance and meets the requirements.
[0095] Figure 4The test results of Example 2 are schematically shown. Figure 4 As shown in, according to the spraying method in Example 2, polydimethylsiloxane (PDMS) is used as the base material, and the antistatic coating material is used to treat the base material with a clean surface represented by polydimethylsiloxane (PDMS) to obtain a base material containing the antistatic coating material, and the base material containing the antistatic coating material is further dried to obtain an antistatic coating. The test result of the antistatic coating obtained by spraying is that the double-sided resistance is 10E10, which can be adjusted in a wide range of 10E7Ω-10E11Ω, and its order of magnitude is within the order of magnitude range corresponding to the antistatic demand. Therefore, the polydimethylsiloxane (PDMS) coated with the antistatic coating prepared by Example 2 has good electrostatic dissipation performance and meets the preparation requirements.
[0096] In the disclosed embodiment, when configuring the antistatic coating material, using an organic substance containing a strong electron-withdrawing group and a strong electron-donating group as a substrate for balancing the charge, the electrostatic dissipation requirements of the antistatic coating material can be met. The strong electron-donating organic substance contains amino groups, and the strong electron-withdrawing organic substance contains fluorine ions. When configuring the antistatic coating material, by controlling the ratio of amino groups and fluorine ions in these two components, an equal number of positive and negative charges can be obtained, thereby achieving an effect of zero overall charge, to meet the electrostatic dissipation requirements of the antistatic coating material. In addition, the silane present in the two components makes it have a strong chemical bond to many base materials, increases the bonding force of the antistatic coating material and the base material, so that the antistatic coating formed can be closely adhered to a variety of base materials, so that the electrostatic coating has a great improvement in the universality of the material, can be applied to various types of base materials, improves universality, and increases the scope of application. By configuring the antistatic coating material containing a strong electron-donating group and a strong electron-withdrawing group, the antistatic coating material can be coated on any type of base material, that is, an antistatic coating with excellent material universality is obtained. At the same time, the number of positive and negative charges in the mixed solution can be adjusted so that the ratio of positive and negative charges is 1:1, and the electrostatic dissipation properties of the antistatic coating material can be further adjusted according to the ratio of positive and negative charges, so that the antistatic coating material can meet different application scenarios.
[0097] In the embodiments of the present disclosure, chemical components with strong electron-donating and electron-withdrawing functions are introduced into the antistatic coating material. By adjusting the ratio of the two components to adjust the surface potential of the coating surface, the excess charge can be completely eliminated in the coating area. The preparation method of the antistatic coating provided in the related art greatly limits the choice of the shape of the substrate material. The antistatic coating provided in the embodiments of the present disclosure can be obtained only by immersion, which eliminates the limitation of the required surface shape, and the antistatic coating can be made into a curved surface that is difficult to achieve with the original electrostatic coating. Moreover, this coating has good transparency, which increases the scope of application.
[0098] In this exemplary embodiment, a device is also provided. The device may have the above antistatic coating, such as a mobile phone, a tablet computer, a laptop computer, a smart bracelet, a smart watch, a smart helmet, smart glasses, a vehicle, a robot, and any type of industrial equipment, etc., as long as it can contain the antistatic coating or can contain the above antistatic coating material, and this exemplary embodiment does not specifically limit this.
[0099] In addition, the above-mentioned figures are only schematic illustrations of the processes included in the method according to the exemplary embodiments of the present disclosure, and are not intended to be limiting. It is easy to understand that the processes shown in the above-mentioned figures do not indicate or limit the time sequence of these processes. In addition, it is also easy to understand that these processes can be performed synchronously or asynchronously, for example, in multiple modules.
[0100] Those skilled in the art will readily appreciate other embodiments of the present disclosure after considering the specification and practicing the invention disclosed herein. This application is intended to cover any modification, use or adaptation of the present disclosure, which follows the general principles of the present disclosure and includes common knowledge or customary techniques in the art that are not disclosed in the present disclosure. The specification and examples are intended to be exemplary only, and the true scope and spirit of the present disclosure are indicated by the appended claims.
[0101] It should be understood that the present disclosure is not limited to the exact structures that have been described above and shown in the drawings, and that various modifications and changes may be made without departing from the scope thereof. The scope of the present disclosure is limited only by the appended claims.
Claims
1. An antistatic coating material, It is characterized in that The components of the antistatic coating material include: strong electron-donating organic matter, strong electron-absorbing organic matter and anhydrous ethanol; The strong electron-donating organic matter contains amino groups, and the strong electron-withdrawing organic matter contains fluorine ions.
2. The antistatic coating material according to claim 1, It is characterized in that The strong electron donating organic matter includes one or more of N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, diethylenetriaminopropyltrimethoxysilane, N-aminoethyl-3-aminopropyltriethoxysilane, and N-methyl-3-aminopropyltrimethoxysilane.
3. The antistatic coating material according to claim 1, It is characterized in that The strong electron-withdrawing organic matter includes one or more of trimethoxy (1H, 1H, 2H, 2H-tridecafluorooctyl) silane, 1H, 1H, 2H, 2H-perfluorodecyl triethoxy silane, trimethoxy (1H, 1H, 2H, 2H-heptadecafluorodecyl) silane, trimethoxy (1H, 1H, 2H, 2H-nonafluorohexyl) silane, triethoxy-1H, 1H, 2H, 2H-tridecafluorooctyl silane, and 1H, 1H, 2H, 2H-perfluorododecyl triethoxy silane.
4. The antistatic coating material according to claim 1, It is characterized in that The molar percentage of the strong electron donating organic matter to the strong electron withdrawing organic matter is determined according to the ratio of positive charge to negative charge in the composite solution, and the composite solution includes the strong electron donating organic matter and the strong electron withdrawing organic matter.
5. The antistatic coating material according to claim 1, It is characterized in that The molar percentage of the strong electron-donating organic matter and the strong electron-withdrawing organic matter is adjusted according to the bonding force between the antistatic coating material and the base material.
6. A method for preparing an antistatic coating material, It is characterized in that The antistatic coating material is the antistatic coating material according to any one of claims 1 to 5, and the preparation method of the antistatic coating material comprises: Mixing a strong electron-donating organic substance and a strong electron-withdrawing organic substance to obtain a composite solution, wherein the composite solution contains amino groups and fluoride ions; Anhydrous ethanol is added to the composite solution to obtain the antistatic coating material. 7.An antistatic coating, It is characterized in that The antistatic coating material is prepared according to any one of claims 1 to 5.
8. A method for producing an antistatic coating, for preparing the antistatic coating as claimed in claim 7, It is characterized in that include: Cleaning the base material to form a base material with a clean surface; The base material is processed according to the antistatic coating material according to any one of claims 1 to 5 to obtain a base material containing the antistatic coating material; The base material containing the antistatic coating material is dried to obtain an antistatic coating.
9. The method for producing the antistatic coating according to claim 8, It is characterized in that The base material containing the antistatic coating material is obtained by immersion or spraying.
10. The method for producing an antistatic coating according to claim 9, It is characterized in that The soaking duration of the soaking method is 30-50 minutes, and the spraying times of the spraying method is 3-10 times.
Citation Information
Cited By
Coating composition, antistatic protective coating and preparation method
CN119307180A