Slag modifier and method for smelting low-TFe IF steel from semisteel

By using slag conditioners with specific compositions and particle sizes and active lime during the IF steel smelting process, the iron content in the slag is controlled, solving the problem of excessive TFe in semi-steel smelting and achieving the production of high-quality IF steel.

CN118979134APending Publication Date: 2024-11-19PANGANG GRP XICHANG STEEL & VANADIUM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411041664.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

Xichang Steel & Vanadium Company faces the problem of low carbon content and insufficient heat in the semi-steel when smelting IF steel, resulting in excessive TFe in the slag, which affects the quality of the finished steel. Moreover, existing technology is not able to effectively control the iron content in the slag.

Method used

A slag conditioner is used, whose main components are: Mal: ​​43.0-47.0%, CaO: 16.0-22.0%, SiO2≤5.0%, Al2O3: 4.0-8.0%, Na2O: 1.5-3.0%, H2O≤1.5%, S≤0.2%, with the balance being impurities. The particle size is 10-50mm. It is used in converter smelting and RH treatment. Combined with the use of active lime, it controls the alkalinity and melting point of the slag and reduces the steel-slag interface reaction.

Benefits of technology

By using slag conditioners, the rapid depletion of metallic Al in the slag is prevented, secondary oxidation of molten steel is reduced, the TFe content in the slag is controlled to be below 6%, and the quality of IF molten steel is ensured to meet the requirements of a temperature above 1640℃ and an oxygen activity of above 400ppm.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a slag modifier and a method for smelting low-TFe IF steel from semisteel. The slag modifier comprises the following chemical components in percentage by mass: 43.0-47.0% of Mal, 16.0-22.0% of CaO, less than or equal to 5.0% of SiO2, 4.0-8.0% of Al2O3, 1.5-3.0% of Na2O, less than or equal to 1.5% of H2O, less than or equal to 0.2% of S and the balance of impurities. The slag modifier is suitable for being used in IF steel production. The slag modifier can play a role in slowly releasing Al to prevent the metal Al in the slag from being used up too fast, and the argon is not opened during the slag modification of the process to prevent the molten steel and the slag surface in the steel ladle from being stirred too strongly so as to weaken the steel slag interface reaction, so that the slag modifier can be completely spread on the slag surface after the converter tapping and the molten steel surface is not exposed. And TFe in the slag is prevented from rising due to secondary oxidation after tapping.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of converter steelmaking, and in particular to a slag conditioning agent and a method for semi-steel smelting low TFe IF steel. Background Art

[0002] At present, IF steel has excellent deep drawing and forming properties, and is widely used in the manufacturing fields of automobiles, home appliances, etc., with a large market demand. With the continuous improvement of the quality requirements for steel products, this high-quality IF steel will be more popular, and it can meet the requirements of energy conservation and emission reduction and efficient use of resources, which is in line with the trend of sustainable development in the steel industry. For Xichang Steel and Vanadium Company, there are some challenges to achieve this smelting. The raw material for converter steelmaking of Xichang Steel and Vanadium Company is semi-steel after vanadium extraction. This semi-steel has a low carbon content and almost no silicon and manganese elements. The poor heat source is very unfavorable for the production of IF steel molten steel. The IF steel molten steel must be guaranteed to have a temperature of more than 1640℃ and an oxygen activity of more than 400ppm. If the oxygen activity of the steel molten steel is guaranteed to be certain, it will cause TFe in the slag to be too high, thus affecting the quality of the finished molten steel. Summary of the invention

[0003] In order to solve the problems of the prior art, the present invention provides a slag conditioning agent and a method for semi-steel smelting low TFe IF steel.

[0004] The purpose of the present invention is achieved through the following technical solutions:

[0005] A slag conditioning agent, whose main chemical components are Mal: ​​43.0-47.0%, CaO: 16.0-22.0%, SiO2≤5.0%, Al2O3: 4.0-8.0%, Na2O: 1.5-3.0%, H2O≤1.5%, S≤0.2%, and the remainder is impurities.

[0006] Furthermore, the particle size of the slag adjusting agent is 10 to 50 mm.

[0007] Furthermore, the slag conditioning agent is suitable for use in the production of IF steel.

[0008] Furthermore, the raw material for producing IF steel is semi-steel, which is molten steel after vanadium extraction and desulfurization from molten iron, contains almost no Si element, has a C content of about 3.30±0.3%, and a temperature of about 1350±30°C.

[0009] A method for semi-steeling low TFe IF steel, comprising converter smelting, RH treatment, and continuous casting;

[0010] Among them, during the converter smelting process, semi-steel is added to the converter, the oxygen activity of the tapping steel is controlled at 400-600ppm, and the tapping temperature is above 1640℃; active lime is added at the beginning of tapping, argon is turned off in the later stage of tapping, and the above-mentioned slag adjusting agent is added after tapping is completed to control the final carbon content below 5%.

[0011] Furthermore, based on the molten steel volume of 220t±10t, the amount of active lime added is 500±50kg, and the amount of slag conditioning agent added is 400-450kg.

[0012] Furthermore, when the oxygen activity is lower than 350 ppm, additional blowing is necessary.

[0013] Furthermore, after the RH treatment, the steel was tapped, slag samples were taken, and TFe was determined.

[0014] Furthermore, based on the molten steel amount of 220t±10t, when the end point C>0.04% and C>0.5%, the amount of slag adjusting agent added is 400kg, and when the end point C≤0.04, the amount of slag adjusting agent added is 450kg.

[0015] Furthermore, the low TFe is RH final slag TFe≤6%.

[0016] Beneficial effects of the present invention:

[0017] Firstly, the slag adjusting agent can be used to slowly release Al, so as to prevent the metal Al in the slag from being exhausted too quickly. Secondly, the argon is not turned on during the slag adjusting process, so as to prevent the molten steel and the slag surface in the ladle from being stirred too strongly, thereby weakening the slag interface reaction. As long as the slag adjusting agent can be spread completely on the slag surface after the converter is tapped, the molten steel surface is not exposed, and the secondary oxidation after tapping is prevented, thereby preventing the TFe in the slag from rising. The invention can control the alkalinity in the slag, increase the melting point of the slag, and reduce its fluidity by adding a certain amount of lime, thereby inhibiting the slag interface reaction during the RH treatment. DETAILED DESCRIPTION

[0018] The following non-limiting embodiments may enable a person skilled in the art to more fully understand the present invention, but are not intended to limit the present invention in any way.

[0019] Example 1

[0020] A slag conditioning agent is suitable for use in the production of IF steel. The main chemical components of the slag conditioning agent are shown in Table 1 by mass percentage.

[0021] Table 1 Main chemical composition of slag conditioning agent / %

[0022] Particle size / mm MA1, % CaO, % <![CDATA[SiO2,%]]> <![CDATA[Al2O3,%]]> <![CDATA[Na2O,%]]> <![CDATA[H2O,%]]> S,% <![CDATA[CO 2,% ]]> 10~50 45.0 19.0 3.7 6.0 3.0 0.5 0.06 22.74

[0023] Example 2

[0024] A method for producing low TFe semi-steel smelting IF steel comprises the following steps:

[0025] Semi-steel is molten steel after vanadium extraction and desulfurization. It contains almost no Si element, the C content is about 3.30±0.3%, and the temperature is about 1350℃.

[0026] The IF steel production process of RH directly from the converter is adopted, the molten steel volume is 220t, the oxygen activity of the steel is controlled at 400-600ppm, and the temperature is 1640-1680℃; 500kg of active lime is added at the beginning of steel tapping, argon is turned off in the later stage of steel tapping, and 400kg of the slag adjusting agent of Example 1 is added after the steel tapping is completed, and the end point C is controlled to be greater than 0.04%. After the RH treatment is completed, the slag sample is taken, and the average TFe in the slag can reach 4.5%.

[0027] Example 3

[0028] A method for producing low TFe semi-steel smelting IF steel comprises the following steps:

[0029] Semi-steel is molten steel after vanadium extraction and desulfurization. It contains almost no Si element, the C content is about 3.30±0.3%, and the temperature is about 1350℃.

[0030] The IF steel production process of converter direct RH is adopted, the molten steel volume is 220t, the oxygen activity of steel tapping is controlled at 400-600ppm, and the temperature is 1640-1680℃; 500kg of active lime is added at the beginning of steel tapping, argon is turned off in the later stage of steel tapping, and 450kg of slag adjusting agent of Example 1 is added after steel tapping is completed, and the end point C is controlled to be ≤0.04. After the RH treatment is completed, the slag sample is taken, and the average TFe in the slag can reach 4.5%.

Claims

1. A slag conditioning agent, characterized in that: Its chemical composition by mass percentage is Mal: ​​43.0-47.0%, CaO: 16.0-22.0%, SiO2≤5.0%, Al2O3: 4.0-8.0%, Na2O: 1.5-3.0%, H2O≤1.5%, S≤0.2%, and the remainder is impurities.

2. The slag conditioning agent according to claim 1, characterized in that: The particle size of the slag adjusting agent is 10 to 50 mm.

3. The slag conditioning agent according to claim 1, characterized in that: The slag conditioning agent is suitable for use in producing IF steel.

4. The slag conditioning agent according to claim 3, characterized in that: The raw material for producing IF steel is semi-steel.

5. The slag conditioning agent according to claim 4, characterized in that: The C content of the semi-steel is 3.30±0.3%.

6. A method for semi-steel smelting low TFe IF steel, characterized in that: Including converter smelting, RH treatment, and continuous casting; During the converter smelting process, semi-steel is added to the converter, the oxygen activity of the tapping steel is controlled at 400-600ppm, and the tapping temperature is 1640°C; active lime is added at the beginning of tapping, argon is turned off in the later stage of tapping, and the slag adjusting agent described in any one of claims 1 to 4 is added after tapping is completed to control the end point carbon to be below 5%.

7. The method according to claim 6, characterized in that Based on the molten steel volume of 220t±10t, the amount of active lime added is 500±50kg, and the amount of slag adjuster added is 400-450kg.

8. The method according to claim 6, characterized in that When the oxygen activity is lower than 350 ppm, additional blowing is required.

9. The method according to claim 6 or 7, characterized in that: Based on the molten steel amount of 220t±10t, when the end point C>0.04% and C>05%, the amount of slag adjusting agent added is 400kg, and when the end point C≤0.04, the amount of slag adjusting agent added is 450kg.

10. The method according to claim 6, characterized in that The low TFe refers to RH final slag TFe≤6%.