Low heat conduction component for bubble type heat insulation material and bubble type heat insulation material
By using the low thermal conductivity components of bubble-type thermal insulation materials in extreme temperature differences, the problem of difficulty in insulation in the existing technology is solved, and effective thermal insulation and resistance in scenarios such as the North and South Pole, high altitude areas and Mars is achieved. Pressure, reducing material weight and transportation costs.
Patent Information
- Application Number
- CN202411047981.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-22
AI Technical Summary
Existing thermal insulation materials are difficult to effectively insulate heat in extreme temperature differences, especially in scenarios such as the Arctic and South Pole, high altitude areas and Mars, which cannot meet the needs of daytime heat absorption and night insulation.
Using bubble-type thermal insulation materials, low thermal conductivity components include bubble substrates such as trans-1-chloro-3,3,3-trifluoropropylene, 1,1,1,3,3-pentafluoropropane and 1 -Fluoro-1,1-dichloroethane, combined with helium, hexafluoroethane and perfluoro-n-pentane, forms bubbles with low thermal conductivity and compressive resistance through low thermal conductivity and boiling point characteristics in the gaseous state. structure.
Maintain good thermal insulation performance in extreme temperature differences, reduce the risk of solidification of bubble structures, ensure bubble stability and thermal insulation, and reduce material weight and transportation costs.
Smart Images

Figure BDA0004974043890000141 
Figure BDA0004974043890000151 
Figure BDA0004974043890000161
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of thermal insulation materials, in particular to a low thermal conductivity component for a bubble-type thermal insulation material and a bubble-type thermal insulation material. Background Art
[0002] Thermal insulation foam materials mainly include EPS polystyrene insulation board, foamed ceramic insulation board, polystyrene foam insulation board, polyurethane insulation material, Class A fireproof foamed cement insulation board, etc. These materials have their own characteristics and are suitable for different application scenarios. Their common goal is to reduce energy loss and achieve energy conservation and emission reduction. These thermal insulation foam materials are widely used in many fields such as building exterior wall insulation, fire isolation belts, storage tanks, ventilation ducts, etc., which can improve energy efficiency by reducing heat transfer, improve indoor environment, and reduce maintenance and use costs. However, their application environment is mostly under atmospheric pressure, and the temperature fluctuates greatly with the seasons. The temperature difference in a short period of time (for example, one day) is small (mostly a few degrees or more than ten degrees).
[0003] However, in certain cases, such as the North and South Poles and high altitude areas, the temperature difference between day and night is large. The temperature difference between day and night on the moon can reach hundreds of degrees (during the day, the temperature of the lunar surface where the sunlight shines vertically is as high as 127°C; at night, its surface temperature can drop to -183°C). The temperature difference between day and night on Mars is more than 100 degrees (the daytime temperature on Mars is around 27°C, and around -133°C at night when there is no sunlight, and the temperature difference between day and night is close to 150°C), and the pressure is often less than or much less than atmospheric pressure.
[0004] Based on the above situation, in order to adapt to the huge changes in temperature in a short period of time, it is necessary to enable buildings under such environmental conditions to absorb heat during the day and keep warm at night, so as to meet higher constant temperature requirements.
[0005] However, the materials provided by the related technology are difficult to meet the low thermal conductivity and heat preservation requirements of the above environment. Summary of the invention
[0006] The object of the present invention is to provide a low thermal conductivity component for bubble type thermal insulation material and a bubble type thermal insulation material, wherein the low thermal conductivity component for bubble type thermal insulation material has a low thermal conductivity coefficient and good thermal insulation performance; the bubble type thermal insulation material having the low thermal conductivity component for bubble type thermal insulation material not only has a low thermal conductivity coefficient and good thermal insulation performance, but also can utilize the low thermal conductivity component for bubble type thermal insulation material to maintain the compression resistance of the bubble wall material.
[0007] The present invention is achieved in that:
[0008] In a first aspect, the present invention provides a low thermal conductivity component for a bubble-type thermal insulation material, comprising: a bubble substrate, helium, hexafluoroethane and perfluoro-n-pentane; the bubble substrate comprises at least one of trans-1-chloro-3,3,3-trifluoropropene, 1,1,1,3,3-pentafluoropropane and 1-fluoro-1,1-dichloroethane; wherein,
[0009] In the case where the bubble substrate contains only trans-1-chloro-3,3,3-trifluoropropene, the low thermal conductivity component for the bubble type thermal insulation material includes, by mass percentage:
[0010] 46-70% trans-1-chloro-3,3,3-trifluoropropene;
[0011] 10-20% helium;
[0012] 15-25% hexafluoroethane;
[0013] 1-10% perfluoropentane.
[0014] In an alternative embodiment, when the bubble substrate contains only 1,1,1,3,3-pentafluoropropane and 1-fluoro-1,1-dichloroethane,
[0015] The low thermal conductivity components used in bubble-type thermal insulation materials include, by mass percentage:
[0016] 46-70% of 1,1,1,3,3-pentafluoropropane and 1-fluoro-1,1-dichloroethane;
[0017] 10-20% helium;
[0018] 15-25% hexafluoroethane;
[0019] 1-10% perfluoropentane.
[0020] In an alternative embodiment, when the bubble substrate includes at least one of 1,1,1,3,3-pentafluoropropane and 1-fluoro-1,1-dichloroethane, and trans-1-chloro-3,3,3-trifluoropropene,
[0021] The low thermal conductivity components used in bubble-type thermal insulation materials include, by mass percentage:
[0022] 46-70% of the bubble substrate, wherein 1,1,1,3,3-pentafluoropropane accounts for 1-10% of the total mass of the low thermal conductivity components for the bubble-type thermal insulation material, and / or 1-fluoro-1,1-dichloroethane accounts for 1-10% of the total mass of the low thermal conductivity components for the bubble-type thermal insulation material;
[0023] 10-20% helium;
[0024] 15-25% hexafluoroethane;
[0025] 1-10% perfluoropentane.
[0026] In an alternative embodiment, the mass of at least one of 1,1,1,3,3-pentafluoropropane and 1-fluoro-1,1-dichloroethane is 10-20% of the mass of trans-1-chloro-3,3,3-trifluoropropene.
[0027] In an optional embodiment, the low thermal conductivity component for the bubble-type thermal insulation material further comprises, by mass percentage, at least one of 1-10% sulfur hexafluoride and 1-10% perfluoro-n-butane.
[0028] In a second aspect, the present invention provides a bubble-type thermal insulation material, which is prepared by using a low thermal conductivity component and a bubble wall material of the bubble-type thermal insulation material of any of the aforementioned embodiments; wherein the components of the bubble wall material include, by mass percentage:
[0029] 9-59.95% sodium lauryl sulfate;
[0030] 9-26% sodium alkylbenzene sulfonate;
[0031] 9-26% fatty acid polyoxyethylene ether;
[0032] 20-35% hexadecyltrimethylammonium bromide;
[0033] 0.05-0.1% graphene.
[0034] In an optional embodiment, the bubble-type heat insulation material has bubble walls formed by bubble wall materials, and the bubble-type heat insulation material is filled with low thermal conductivity components in the bubbles; wherein,
[0035] The bubble wall thickness is 0.1-1g / m 2 .
[0036] In an alternative embodiment, the diameter of the gas bubbles is 1-10 mm.
[0037] In an optional embodiment, the method for preparing the bubble-type heat insulating material comprises: using a gaseous bubble-type heat insulating material with a low thermal conductivity component to form bubbles in a bubble wall material in a blowing manner;
[0038] The gas phase thermal conductivity of the low thermal conductivity component used in the gaseous bubble type thermal insulation material is lower than 15mw / m·k.
[0039] In an optional embodiment, a film is further included, which encloses a filling space, and a gaseous bubble-type thermal insulation material is used with a low thermal conductivity component to blow bubbles so that the bubble wall material forms bubbles and fills the filling space.
[0040] The present invention includes the following beneficial effects:
[0041] The gas phase thermal conductivity coefficients of the bubble substrate (any one of trans-1-chloro-3,3,3-trifluoropropene, 1,1,1,3,3-pentafluoropropane and 1-fluoro-1,1-dichloroethane) in the low thermal conductivity component for the bubble type thermal insulation material of the present invention, as well as hexafluoroethane and perfluoro-n-pentane are very low, which is conducive to providing the thermal insulation performance of the low thermal conductivity component for the bubble type thermal insulation material; moreover, the bubble substrate (trans-1-chloro-3,3,3-trifluoropropene, 1,1,1,3,3-pentafluoropropane and 1-fluoro-1,1-dichloroethane) Any one of the three ethyl chloride) and perfluoropentane also have a lower saturated liquid phase thermal conductivity, which makes the bubble-type thermal insulation material with low thermal conductivity components more conducive to environments with large temperature differences (the temperature range can be -133℃-27℃, for example: the temperature on Mars is around 27℃ during daylight hours, and around -133℃ at night when there is no sunlight. The temperature difference between day and night is close to 150℃, with a large temperature difference and an average temperature of -55℃.), which can reduce the adverse effects on thermal insulation performance when the bubble substrate and perfluoropentane become liquid, thereby ensuring good thermal insulation.
[0042] It should be noted that the density of perfluoropentane is relatively high. Controlling its weight within 1-10% is beneficial to reducing costs on the one hand, and on the other hand, it can avoid increasing the weight of the low thermal conductivity component used in the entire bubble-type thermal insulation material, which is beneficial to achieving lightweight.
[0043] The bubble-type heat-insulating material of the present invention is prepared from the low thermal conductivity component for the bubble-type heat-insulating material and the bubble wall material; wherein, the bubble base material in the low thermal conductivity component for the bubble-type heat-insulating material (under low pressure 700Pa conditions, any one of trans-1-chloro-3,3,3-trifluoropropene (boiling point -67.89°C), 1,1,1,3,3-pentafluoropropane (boiling point -67.27°C) and 1-fluoro-1,1-dichloroethane (boiling point -60.14°C)) has a boiling point temperature close to the average temperature of Mars (-55°C), a gas-liquid transition temperature in the middle, a high latent heat of vaporization, more heat required for gas-liquid change, which can slow down the gas-liquid phase change process, and is more favorable under conditions of large temperature difference It can mitigate the pressure fluctuations caused by the gas-liquid changes of components in the bubbles formed by filling the bubble-type thermal insulation materials with low thermal conductivity components, which is beneficial to maintaining the stability of the bubbles. The extremely low freezing point under low pressure (lower than or close to the lowest temperature on Mars) can also prevent the substance from becoming a solidified state or reduce the time it takes for the substance to become a solidified state, which is beneficial to maintaining the stability of the bubbles. The bubble substrate also has the characteristic of low density when it is in liquid state. During the gas-liquid conversion process in an environment with a large temperature difference, the low-density liquid (low density means that the bubble substrate has a lower density than other thermal conductive components when they are in the same liquid state) can reduce the influence of the liquid substance on the bubble structure, thereby ensuring the stability of the bubbles formed by filling the bubble-type thermal insulation materials with low thermal conductivity components.
[0044] The helium in the low thermal conductivity component of the bubble type thermal insulation material is always maintained in a gaseous state under low pressure (the low pressure can be 700Pa, for example: the atmosphere of Mars is composed of CO2 (95.3%), N2 (2.7%), argon (1.6%), oxygen (0.15%), and water vapor (0.03%). The atmospheric pressure in most areas is 7 millibars (lower than the earth's air pressure, the gas is thin, the gas density is less than 1% of the earth, and its low pressure is about 700Pa). Its low density characteristic is conducive to reducing weight and reducing transportation costs, and maintaining helium in The mass percentage of the low thermal conductivity component in the entire bubble-type thermal insulation material is 10-20%, which can ensure that the gas phase composition inside the bubbles formed by filling the bubble-type thermal insulation material with the low thermal conductivity component maintains a certain pressure when a phase change occurs under a large temperature difference, thereby ensuring the stability of the bubbles; moreover, the helium phase change temperature difference range is large (much larger than the ambient temperature change range of Mars, etc.), which can always ensure that it is in a gas state, and then reliably utilize helium to improve the stability of the bubbles formed by filling the bubble-type thermal insulation material with the low thermal conductivity component.
[0045] Hexafluoroethane in the low thermal conductivity component of the bubble type thermal insulation material is conducive to bubble formation. It always maintains a gaseous state under low pressure (700Pa), and its low density characteristic is also conducive to reducing weight and reducing transportation costs. Although the density of hexafluoroethane is slightly higher than that of helium, the thermal conductivity of hexafluoroethane is low. Maintaining the mass percentage of hexafluoroethane in the low thermal conductivity component of the entire bubble type thermal insulation material at 15-25% can ensure that the gas phase composition inside the bubble formed by filling the low thermal conductivity component of the bubble type thermal insulation material maintains a certain pressure when a phase change occurs under a large temperature difference, thereby ensuring the stability of the bubble. At the same time, it has a low thermal conductivity, which is conducive to maintaining the excellent thermal insulation performance of the bubble type thermal insulation material.
[0046] Perfluoropentane is compounded with other components to facilitate the formation of bubbles; the boiling point of perfluoropentane (-59.01°C) is closer to the average temperature of Mars (-55°C), the gas-liquid transition temperature is in the middle, and it has a higher boiling point than other components, so that perfluoropentane can realize the process of gas-liquid phase change of each raw material component at different temperatures with bubble substrates, helium and hexafluoroethane having different boiling points, that is, the bubble substrate, helium, hexafluoroethane and perfluoropentane in the low thermal conductivity component for bubble-type thermal insulation materials have different boiling points, so gas-liquid phase change can be realized at different temperatures, so that the low thermal conductivity component for bubble-type thermal insulation materials used to fill the bubbles is not easy to directly change from gas phase to liquid phase at the same time at a certain temperature. In other words, under conditions of large temperature differences, it is more conducive to slowing down the pressure fluctuations caused by the gas-liquid changes of each raw material component in the bubbles formed by filling the bubble-type thermal insulation material with the low thermal conductivity component, and is conducive to maintaining the stability of the bubbles; moreover, perfluoropentane has an extremely low freezing point under low pressure (lower than the lowest temperature on Mars), therefore, perfluoropentane is at most converted into a liquid phase at low temperatures, and will not solidify into a solid state, so as to ensure that the bubbles formed by filling the bubble-type thermal insulation material with the low thermal conductivity component can maintain at least the presence of a liquid phase in the bubbles at extremely low temperatures, which is conducive to reducing the adverse effects of the solidification of the substance in the low thermal conductivity component of the bubble-type thermal insulation material on the bubbles formed by the filling, and is conducive to maintaining the stability of the bubbles.
[0047] Sodium lauryl sulfate (anionic surfactant) and hexadecyl trimethyl ammonium bromide (cationic surfactant) in the bubble wall material of the bubble-type thermal insulation material form a compound of anionic surfactant and cationic surfactant to obtain a high-surface-active surfactant suitable for the rapid formation of bubbles by composite gas; the compound of sodium lauryl sulfate and hexadecyl trimethyl ammonium bromide also has a solubilizing effect, and the two have good mutual solubility; the addition of hexadecyl trimethyl ammonium bromide cationic surfactant also enhances the activity of the surfactant. By adding sodium alkylbenzene sulfonate anionic surfactant, the proportion of anionic surfactant can be increased, and the problems such as surfactant deposition caused by the similar amount of cationic and anionic surfactants can be reduced, which is conducive to improving the stability of bubbles formed by the bubble wall material, that is, the bubbles are not easy to break. Fatty acid polyoxyethylene ether is a non-ionic surfactant, which is a long-chain polyether. The addition of fatty acid polyoxyethylene ether can achieve the addition of macromolecules, increase the mutual solubility of surfactants, and improve the stability under cationic and anionic surfactants, thereby improving the bubble wall stability of bubbles formed by the bubble wall material. The addition of graphene can enhance the toughness of the bubble wall material and make it difficult to break bubbles. DETAILED DESCRIPTION
[0048] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0049] The present invention provides a bubble-type thermal insulation material, which can be used to fill in components such as walls and container shells; the bubble-type thermal insulation material is prepared from a low thermal conductivity component A and a bubble wall material B for the bubble-type thermal insulation material.
[0050] The low thermal conductivity component A for bubble-type thermal insulation materials includes, by mass percentage:
[0051] 46-70% trans-1-chloro-3,3,3-trifluoropropene, for example: 46%, 50%, 53%, 55%, 57%, 60%, 64%, 66%, 70%, etc., not specifically limited here;
[0052] 10-20% helium, for example: 10%, 12%, 15%, 17%, 20%, etc., not specifically limited here;
[0053] 15-25% hexafluoroethane, for example: 15%, 17%, 20%, 22%, 25%, etc., not specifically limited here;
[0054] 1-10% of perfluoro-n-pentane, for example: 1%, 2%, 4%, 5%, 7%, 10%, etc., which is not specifically limited herein.
[0055] The cell wall material B component includes, by mass percentage:
[0056] 34.9-59.95% sodium lauryl sulfate, for example: 34.9%, 35%, 37%, 40%, 43%, 45%, 47%, 50%, 53%, 55%, 57%, 59.95%, etc., not specifically limited here;
[0057] 9-26% sodium alkylbenzene sulfonate, for example: 9%, 10%, 12%, 15%, 17%, 20%, 22%, 24%, 26%, etc., not specifically limited here;
[0058] 9-26% fatty acid polyoxyethylene ether, for example: 9%, 10%, 12%, 15%, 17%, 20%, 22%, 24%, 26%, etc., not specifically limited here;
[0059] 20-35% hexadecyltrimethylammonium bromide, for example: 20%, 22%, 24%, 26%, 30%, 32%, 35%, etc., not specifically limited here;
[0060] 0.05-0.1% graphene, for example: 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, 0.1%, etc., which is not specifically limited here.
[0061] The gas phase thermal conductivity coefficients of the bubble matrix (trans-1-chloro-3,3,3-trifluoropropene), hexafluoroethane and perfluoro-n-pentane in the low thermal conductivity component for bubble type thermal insulation materials are very low, which is conducive to providing the thermal insulation and thermal insulation performance of the low thermal conductivity component for bubble type thermal insulation materials; moreover, trans-1-chloro-3,3,3-trifluoropropene and perfluoro-n-pentane also have a relatively low saturated liquid phase thermal conductivity coefficient, which also makes the low thermal conductivity component for bubble type thermal insulation materials more conducive to an environment with a large temperature difference, and can reduce the adverse effects on the thermal insulation performance when the bubble matrix and perfluoro-n-pentane become liquid, thereby ensuring good thermal insulation.
[0062] Since helium has a relatively high gas phase thermal conductivity (for example, the gas phase thermal conductivity of helium is 154.5 mw / m·k (23°C, 700 Pa)), which is more than ten times the thermal conductivity of other component gases, its proportion is no more than 20%. If the proportion is too high, it will have an adverse effect on the thermal insulation performance.
[0063] It should be noted that the density of perfluoropentane is relatively high. Controlling its weight within 1-10% is beneficial to reducing costs on the one hand, and on the other hand, it can avoid increasing the weight of the low thermal conductivity component used in the entire bubble-type thermal insulation material, which is beneficial to achieving lightweight.
[0064] It should also be noted that when the ambient temperature is lower than the boiling point of the gas, the gas will be liquefied, and the gas with low thermal conductivity will become a liquid with high thermal conductivity, which will affect the thermal insulation performance and cause the thermal insulation to deteriorate; therefore, by using trans-1-chloro-3,3,3-trifluoropropene and perfluoropentane with lower saturated liquid phase thermal conductivity, when trans-1-chloro-3,3,3-trifluoropropene and perfluoropentane themselves are converted into liquid, it can also ensure that the low thermal conductivity component used in the bubble-type thermal insulation material still has good thermal insulation and heat insulation performance as a whole.
[0065] The trans-1-chloro-3,3,3-trifluoropropene in the low thermal conductivity component of the bubble-type thermal insulation material has a low density, which is conducive to lightweighting to reduce transportation costs, and its liquid density under low pressure is low (for example: 1471.58kg / m 3 (pressure 700Pa, temperature -70℃), in the process of gas-liquid transition under the environment of large temperature difference, the low density of liquid can reduce the influence of liquid-like substances on the bubble structure, thereby improving the stability of the bubble; trans-1-chloro-3,3,3-trifluoropropene (under low pressure condition 700Pa, boiling point -67.89℃) has a boiling point close to the average temperature of Mars (-55℃), a gas-liquid transition temperature in the middle, a high latent heat of vaporization, and more heat required for gas-liquid change, which can slow down the gas-liquid phase change process and is more conducive to reducing the temperature difference under the condition of large temperature difference. The pressure fluctuations caused by the gas-liquid changes of the components in the bubbles formed by the bubble-type thermal insulation material filled with low thermal conductivity components are slowed down, which is beneficial to maintaining the stability of the bubbles. The extremely low freezing point under low pressure (close to the lowest temperature on Mars) can also reduce the time it takes for the substance to become solidified, which is beneficial to maintaining the stability of the bubbles. The bubble substrate also has the characteristic of low density. During the gas-liquid conversion process in an environment with a large temperature difference, the low-density liquid can reduce the influence of the liquid substance on the bubble structure, thereby ensuring the stability of the bubbles formed by the bubble-type thermal insulation material filled with low thermal conductivity components.
[0066] The helium in the low thermal conductivity component of the bubble-type thermal insulation material is always maintained in a gaseous state under low pressure (700Pa). Its low density characteristic is conducive to reducing the weight of the component and reducing transportation costs. Maintaining the mass percentage of helium at 10-20% can ensure that when the gas phase composition inside the bubbles formed by filling the low thermal conductivity component of the bubble-type thermal insulation material undergoes a phase change under a large temperature difference, a certain pressure is maintained, thereby ensuring the stability of the bubbles; moreover, the helium has a large temperature difference range for phase change, which can ensure that it is always in a gaseous state, and then reliably utilize helium to improve the stability of the bubbles formed by filling the low thermal conductivity component of the bubble-type thermal insulation material.
[0067] Hexafluoroethane in the low thermal conductivity component of the bubble-type thermal insulation material is conducive to bubble formation. It always maintains a gaseous state under low pressure (700Pa), and its low density is also conducive to reducing weight and reducing transportation costs. Although the density of hexafluoroethane is slightly higher than that of helium, the thermal conductivity of hexafluoroethane is low. Maintaining the mass percentage of hexafluoroethane at 15-25% can ensure that the gas phase composition inside the bubble formed by the low thermal conductivity component of the bubble-type thermal insulation material undergoes a phase change under a large temperature difference, thereby maintaining a certain pressure to ensure the stability of the bubble. Hexafluoroethane can be used to adjust the mass of the entire bubble-type thermal insulation material as needed, that is, the mass of the entire bubble-type thermal insulation material can be adjusted by increasing or decreasing the amount of hexafluoroethane.
[0068] Perfluoropentane is compounded with other components to facilitate the formation of bubbles; the boiling point of perfluoropentane (-59.01°C under low pressure conditions of 700Pa) is closer to the average temperature of Mars (-55°C), the gas-liquid transition temperature is in the middle, and it has a higher boiling point than other components, so that perfluoropentane can realize the process of gas-liquid phase change of each raw material component at different temperatures with bubble substrates, helium and hexafluoroethane having different boiling points, that is, the bubble substrate, helium, hexafluoroethane and perfluoropentane in the low thermal conductivity component for bubble-type thermal insulation materials have different boiling points, so gas-liquid phase change can be realized at different temperatures, so that the low thermal conductivity component for bubble-type thermal insulation materials used to fill bubbles is not easy to directly freeze at a certain temperature. At the same time, it changes from gas phase to liquid phase, that is, under the condition of large temperature difference, it is more conducive to slowing down the pressure fluctuation caused by the gas-liquid change of each raw material component in the bubbles formed by filling the bubble-type thermal insulation material with low thermal conductivity components, and is conducive to maintaining the stability of the bubbles; moreover, perfluoropentane has an extremely low freezing point under low pressure (lower than the lowest temperature on Mars). Therefore, perfluoropentane can at most change into liquid phase at low temperature, and will not solidify into solid state, so as to ensure that the bubbles formed by filling the bubble-type thermal insulation material with low thermal conductivity components can maintain at least the liquid phase in the bubbles at extremely low temperature, which is conducive to reducing the adverse effect of the solidification of the substance in the low thermal conductivity component of the bubble-type thermal insulation material on the bubbles formed by filling, and is conducive to maintaining the stability of the bubbles.
[0069] The bubble wall material of the bubble-type thermal insulation material has super strong foaming ability; among them, sodium lauryl sulfate (anionic surfactant) and hexadecyl trimethyl ammonium bromide (cationic surfactant) form a compound of anionic surfactant and cationic surfactant to obtain a high surface active surfactant suitable for rapid formation of bubbles by composite gas; sodium lauryl sulfate and hexadecyl trimethyl ammonium bromide compound also have a solubilizing effect, and the two have good mutual solubility. The addition of hexadecyl trimethyl ammonium bromide cationic surfactant also enhances the activity of the surfactant. By adding sodium alkylbenzene sulfonate anionic surfactant, the proportion of anionic surfactant can be increased, and the problems such as surfactant deposition caused by the similar amount of cationic and anionic surfactants can be reduced, which is conducive to improving the bubble wall stability of the bubbles formed by the bubble wall material, that is, the bubbles are not easy to break. Fatty acid polyoxyethylene ether is a non-ionic surfactant, which is a long-chain polyether. The addition of fatty acid polyoxyethylene ether can achieve the addition of macromolecules, increase the mutual solubility of surfactants, and improve the stability under cationic and anionic surfactants, thereby improving the bubble wall stability of the bubbles formed by the bubble wall material. The addition of graphene can enhance the toughness of the bubble wall material and make it difficult to break bubbles.
[0070] In some embodiments, at least one of 1,1,1,3,3-pentafluoropropane and 1-fluoro-1,1-dichloroethane may be used to completely or partially replace trans-1-chloro-3,3,3-trifluoropropene as the bubble substrate.
[0071] Exemplarily, in one embodiment, 1,1,1,3,3-pentafluoropropane and 1-fluoro-1,1-dichloroethane are used to completely replace trans-1-chloro-3,3,3-trifluoropropene, that is, the bubble matrix contains only 1,1,1,3,3-pentafluoropropane and 1-fluoro-1,1-dichloroethane. In this case, the low thermal conductivity component of the bubble-type thermal insulation material includes, by mass percentage: a total of 46-70% of 1,1,1,3,3-pentafluoropropane and 1-fluoro-1,1-dichloroethane; 10-20% of helium; 15-25% of hexafluoroethane; and 1-10% of perfluoro-n-pentane. Optionally, the mass ratio of 1,1,1,3,3-pentafluoropropane and 1-fluoro-1,1-dichloroethane can be selected as needed, including but not limited to (1-10): (1-10), and illustratively can be selected as needed: 1:1, 1:2, 2:1, 1:3, 3:1, 1:4, 4:1, 1:5, 5:1, 1:6, 6:1, 1:7, 7:1, 1:8, 8:1, 1:9, 9:1, 1:10, 10:1, etc., which are not specifically limited here.
[0072] In another embodiment, at least one of 1,1,1,3,3-pentafluoropropane and 1-fluoro-1,1-dichloroethane is used to partially replace trans-1-chloro-3,3,3-trifluoropropene, that is, the bubble matrix includes at least one of 1,1,1,3,3-pentafluoropropane and 1-fluoro-1,1-dichloroethane, and trans-1-chloro-3,3,3-trifluoropropene; in this case, the low thermal conductivity component for the bubble type thermal insulation material includes, by mass percentage, 46-70% of the bubble matrix, wherein 1,1 , 1,3,3-pentafluoropropane accounts for 1-10% (for example: 1%, 2%, 4%, 5%, 7%, 10%, etc., not specifically limited herein) of the total mass of the low thermal conductivity components used in bubble type thermal insulation materials, and / or, 1-fluoro-1,1-dichloroethane accounts for 1-10% (for example: 1%, 2%, 4%, 5%, 7%, 10%, etc., not specifically limited herein) of the total mass of the low thermal conductivity components used in bubble type thermal insulation materials; 10-20% of helium; 15-25% of hexafluoroethane; 1-10% of perfluoropentane.
[0073] In a preferred embodiment, the mass of at least one of 1,1,1,3,3-pentafluoropropane and 1-fluoro-1,1-dichloroethane is 10-20% (for example, 10%, 12%, 14%, 15%, 17%, 20%, etc., not specifically limited herein) of the mass of trans-1-chloro-3,3,3-trifluoropropene; wherein, when 1,1,1,3,3-pentafluoropropane and 1-fluoro-1,1-dichloroethane are both used to replace part of trans-1-chloro-3,3,3-trifluoropropene, the mass ratio of 1,1,1,3,3-pentafluoropropane to 1-fluoro-1,1-dichloroethane can be selected as needed, including but not limited to (1 to 10): (1 to 10).
[0074] The main physical properties of these two components, 1,1,1,3,3-pentafluoropropane (HFC-245fa) and 1-fluoro-1,1-dichloroethane (R141b), are similar to those of trans-1-chloro-3,3,3-trifluoropropene (LBA), and therefore, they can replace trans-1-chloro-3,3,3-trifluoropropene (LBA).
[0075] Moreover, 1,1,1,3,3-pentafluoropropane (HFC-245fa, boiling point -67.27°C under low pressure condition 700Pa), 1-fluoro-1,1-dichloroethane (R141b, boiling point -60.14°C under low pressure condition 700Pa) and trans-1-chloro-3,3,3-trifluoropropene LBA (boiling point -67.89°C under low pressure condition 700Pa) have different boiling points, that is, 1,1,1,3,3-pentafluoropropane, 1-fluoro-1,1-dichloroethane and trans-1-chloro-3,3,3-trifluoropropene can realize gas-liquid phase transition process at different temperatures. In the embodiment where the three components of 1,1,3,3-pentafluoropropane, 1-fluoro-1,1-dichloroethane and trans-1-chloro-3,3,3-trifluoropropene jointly constitute the bubble substrate, the three components of 1,1,1,3,3-pentafluoropropane, 1-fluoro-1,1-dichloroethane and trans-1-chloro-3,3,3-trifluoropropene can realize gas-liquid phase change at different temperatures, instead of changing from gas phase to liquid phase at the same time at a certain temperature, that is, under the condition of large temperature difference, it is more conducive to slowing down the pressure fluctuation caused by the gas-liquid changes of each component in the bubbles formed by filling the bubble-type thermal insulation material with low thermal conductivity components, which is beneficial to maintaining the stability of the bubbles.
[0076] Optionally, in some embodiments, the low thermal conductivity component for the bubble-type thermal insulation material further comprises, by mass percentage: 1-10% (for example, 1%, 2%, 4%, 5%, 7%, 10%, etc., not specifically limited herein) of sulfur hexafluoride (SF6) and 1-10% (for example, 1%, 2%, 4%, 5%, 7%, 10%, etc., not specifically limited herein) of perfluoro-n-butane (C4F10 ) at least one of the two. On the one hand, the above components can ensure low gas phase thermal conductivity. On the other hand, sulfur hexafluoride (under low pressure conditions of 700Pa, boiling point is -49.99°C) and perfluoro-n-butane (under low pressure conditions of 700Pa, boiling point is -81.77°C) have different boiling points, that is, sulfur hexafluoride and perfluoro-n-butane have different temperatures for transformation into gas state. By further adding at least one of sulfur hexafluoride and perfluoro-n-butane, it can be further ensured that each component of the low thermal conductivity component for bubble-type thermal insulation material can realize the phase change process of gas-liquid transformation at different temperatures, and will not change from gas phase to liquid phase at the same time at a certain temperature, and thus it is more conducive to slowing down the pressure fluctuation caused by the change of the low thermal conductivity component for bubble-type thermal insulation material in the bubble under the condition of large temperature difference, and is conducive to maintaining the stability of the bubble.
[0077] The bubble-type thermal insulation material disclosed herein has bubble walls formed of bubble wall materials, and the bubbles are filled with low thermal conductivity components.
[0078] Optionally, the preparation of bubble-type thermal insulation materials can adopt the principle of blowing bubbles to prepare bubble-type materials; specifically, the preparation method of bubble-type thermal insulation materials includes: using a gaseous bubble-type thermal insulation material with a low thermal conductivity component to blow bubbles to form bubbles in the bubble wall material; the bubble wall has high toughness, high strength, and is not easy to break, and the thin outer wall of the bubble wall material contains a gas with low gas phase thermal conductivity (that is, the gaseous bubble-type thermal insulation material with a low thermal conductivity component), and the gas phase thermal conductivity of the gaseous bubble-type thermal insulation material with a low thermal conductivity component is lower than 15mw / m·k, ensuring that the bubble-type thermal insulation material has good thermal insulation performance.
[0079] Among them, the low thermal conductivity component used in the bubble type thermal insulation material can maintain a certain pressure in the bubble, so that the bubble can be stably maintained under conditions of low pressure and large temperature difference, and the bubble has a higher resistance to deformation, which is more conducive to the use of the bubble type thermal insulation material as a thermal insulation material. The low thermal conductivity component used in the bubble type thermal insulation material has a low thermal conductivity coefficient and low density. In addition to being able to be used as a thermal insulation material, it is also beneficial to reduce the transportation cost of the material and has more economic value.
[0080] Optionally, the bubble wall thickness is 0.1-1 g / m 2 , for example: 0.1g / m 2 , 0.2g / m 2 , 0.4g / m 2 , 0.6g / m 2 , 0.8g / m 2 , 0.9g / m 2 , 1g / m 2Optimizing the thickness of the bubble wall can ensure that the bubble wall has sufficient toughness so that the bubble is not easily broken under the external pressure.
[0081] It should be noted that the unit of bubble wall thickness is "gram per square meter" (g / m 2 ), specifically refers to the surface density of the material, that is, the mass of the material per unit area, which is used to describe the relationship between the thickness and weight of the material, and is used to characterize the strength and durability of the material; among them, the surface density is a measure of the mass of the material over a certain area. The formula for calculating the surface density is: total mass of the material (g) ÷ area (square meters). Using "grams per square meter" as the unit can easily compare the performance and cost of bubble films of different thicknesses or different materials. For example, a thicker bubble film may have a higher surface density, which means that it has a greater mass per unit area and may provide better protection.
[0082] Optionally, the diameter of the bubble is 1-10 mm, for example, 1 mm, 2 mm, 3 mm, 5 mm, 7 mm, 9 mm, 10 mm, etc., which is not specifically limited here. Controlling the diameter of the bubble is conducive to improving its toughness, so that the bubble is not easily broken under the action of external pressure.
[0083] Optionally, the bubble-type heat insulation material further includes a film, which encloses a filling space, and the gaseous bubble-type heat insulation material uses a low thermal conductivity component to blow bubbles to form bubbles in the bubble wall material and fill the filling space. In this way, multiple bubbles can be formed in the filling space, and the multiple bubbles are closely arranged due to a certain pressure, and the bubbles contain a gas with low gas phase thermal conductivity, thereby having a good heat preservation and insulation effect.
[0084] In an environment with large temperature differences, for example, the temperature change ratio on Mars in one day is close to 150°C. The low thermal conductivity component of the bubble-type thermal insulation material is composed of multiple components with different boiling points, which can better adapt to the large temperature difference span. In addition, the components with different boiling points can make the bubbles formed by the low thermal conductivity components of the bubble-type thermal insulation material have slow pressure changes at different temperatures, which is conducive to maintaining the stability of the bubbles and maintaining a low thermal conductivity coefficient at the same time, ensuring good thermal insulation and heat preservation effects.
[0085] The thermal insulation performance of the low thermal conductivity component of the bubble-type thermal insulation material and its supporting and stabilizing effect on the bubble wall come from the properties of each component itself. The properties of each component are shown in Table 1 below.
[0086] Table 1 Various material states of low thermal conductivity components that can constitute bubble-type thermal insulation materials
[0087]
[0088]
[0089] He and C2F6 are difficult to liquefy into liquids because their boiling points are lower than the lowest temperature of the Martian environment, so they are shown as lacking data in liquid state in Table 1; and SF6 is also difficult to liquefy into liquid state because its critical temperature and critical pressure are relatively low. It exists in gaseous state even if the temperature is lower than its boiling point, so it is also shown as lacking data in liquid state in Table 1.
[0090] Regarding the data on latent heat of vaporization in Table 1, since the gas pressure condition of the data in Table 1 is fixed at 700Pa, and the latent heat of vaporization belongs to the saturated state, that is, the physical property under the equilibrium condition of the liquid phase and the gas phase, the saturation temperature corresponding to the gas pressure condition of 700Pa is the boiling point temperature of the corresponding gas.
[0091] The boiling point temperatures in Table 1 are the lowest temperatures at which each component can maintain a gaseous state under pressure conditions similar to the Martian environment for 700 years.
[0092] In Table 1, 23℃ is close to the highest temperature of the Martian environment; -123℃ is close to the lowest temperature of Mars.
[0093] It should be noted that the data in Table 1 are derived from the calculation results of the REPROP model, which is used as a prediction of the material properties in the low-pressure 700Pa state.
[0094] REFPROP stands for "Reference Fluid Thermodynamic and Transport Properties Database", which is a fluid thermodynamic and transport properties database. It is widely used in simulation and engineering calculations to query the thermodynamic and transport property parameters of various substances, such as temperature, pressure, density, enthalpy, etc. REFPROP's models and functions are very powerful and can provide high-precision thermophysical property calculations for selected pure fluids and their mixtures, with the goal of bringing uncertainty close to the level of basic experimental data.
[0095] Because the ambient air pressure on Mars is much lower than the atmospheric pressure on Earth, the boiling point and freezing point of substances decrease accordingly as the atmospheric pressure decreases. Therefore, under standard conditions, it is difficult for materials with a freezing point of tens or even hundreds of degrees below zero to form a solid state in the Martian environment. Therefore, the Martian ambient air pressure conditions (700Pa) were used as the calculation conditions for the first time to develop the above table data.
[0096] Solidification data calculation method:
[0097] Known data (in C5F 12 For example)
[0098] 1.C5F12 Freezing point under standard atmospheric pressure: -119°C (154.15K);
[0099] 2. Gas constant R: 8.314 J / (mol·K);
[0100] 3. Solidification enthalpy ΔH sub :Assumed to be 20000 J / mol.
[0101] Clausius-Clapeyron equation:
[0102]
[0103] Substitute data
[0104] P1=101325Pa
[0105] P2=700Pa
[0106] T1=154.15K
[0107] R = 8.314 J / (mol cdot pK)
[0108] ΔH sub ≈20000 J / mol
[0109] Calculation steps
[0110] 1. Calculate the natural logarithm of the pressure ratio:
[0111]
[0112] 2. Substitute into the Clausius-Clapeyron equation and solve the equation:
[0113]
[0114] 3. Calculate the coefficients on the right:
[0115] 4. Substitute and solve:
[0116]
[0117] 5. Simplify and solve:
[0118]
[0119] 6. Calculation
[0120]
[0121] 7. Find T2:
[0122]
[0123] Convert it to Celsius: 116.68K-273.15≈-156.47℃
[0124] in conclusion
[0125] Under the condition of 0.0007MPa (700Pa), C5F 12 The freezing point of C5F is about -156.47℃. This estimate shows that at this temperature and pressure, 12 If you need to calculate other substances, you can recalculate them according to the new pressure value.
[0126] Calculate the freezing point of each component in turn at 700 Pa. Due to limitations in data and detail, assumed values will be used for estimation.
[0127] 1.HFC-245fa (1,1,1,3,3-pentafluoropropane)
[0128] Freezing point at standard atmospheric pressure: -103.3°C (169.85K);
[0129] Assuming solidification enthalpy ΔH sub :20000J / mol;
[0130] Pressure: 101325Pa (standard) -> 700Pa;
[0131] Gas constant R: 8.314 J / (mol-K).
[0132] 2. HCFC-141b (1,1-dichloro-1-fluoroethane)
[0133] Freezing point at standard atmospheric pressure: -103.5°C (169.65K);
[0134] Assuming solidification enthalpy ΔH sub :18000J / mol;
[0135] Pressure: 101325Pa->700Pa.
[0136] 3. LBA (trans-1-chloro-3,3,3-trifluoropropene)
[0137] Freezing point under standard atmospheric pressure: -19°C (254.15K);
[0138] Assuming solidification enthalpy ΔH sub :18000J / mol;
[0139] Pressure: 101325Pa->700Pa.
[0140] 4. He (helium)
[0141] Freezing point at standard atmospheric pressure: -272.2°C (0.95K);
[0142] Assuming solidification enthalpy ΔH sub :100 J / mol (very small, because helium requires very low temperatures to solidify);
[0143] Pressure: 101325Pa->700Pa.
[0144] 5.C2F6 (hexafluoroethane)
[0145] Freezing point under standard atmospheric pressure: -100°C (173.15K);
[0146] Assuming solidification enthalpy ΔH sub :15000J / mol;
[0147] Pressure: 101325Pa->700Pa.
[0148] 6.SF6 (sulfur hexafluoride)
[0149] Freezing point at standard atmospheric pressure: -50.8°C (222,35K);
[0150] Assuming solidification enthalpy ΔH sub :25000J / mol;
[0151] Pressure: 101325Pa->700Pa.
[0152] 7.C4F 10 (Perfluorobutane)
[0153] Freezing point at standard atmospheric pressure: -184.7°C (88.45K);
[0154] Assuming solidification enthalpy ΔH sub :20000J / mol;
[0155] Pressure: 101325Pa->700Pa.
[0156] 8.C5F 12 (Perfluoropentane)
[0157] Freezing point at standard atmospheric pressure: -119°C (154.15K);
[0158] Assuming solidification enthalpy ΔH sub :20000J / mol;
[0159] Pressure: 101325Pa->700Pa.
[0160] Recalculate
[0161] Since Python is needed for the calculations and it involves calculations for multiple compounds, a Python script can be written to automatically calculate the freezing points of various components, assuming that all the above ΔH sub and R. Next, perform this calculation. Here are the estimated freezing points of various components at 700 Pa:
[0162] 1.HFC-245fa: -147.45℃.
[0163] 2.HCFC-141b: -151.09℃.
[0164] 3.LBA(R-1233zd(E)):-112.70℃.
[0165] 4.He (helium): -272.47℃.
[0166] 5.C2F6(hexafluoroethane):-155.96℃.
[0167] 6.SF6 (sulfur hexafluoride): -110.6℃
[0168] 7.C4F 10 (Perfluorobutane): -198.38℃.
[0169] 8.C5F 12 (Perfluoropentane): -156.47°C.
[0170] The above results show that at 700 Pa, the freezing points of most components are below -133 °C, indicating that most components are already in solid state under the above conditions. These calculations are based on the standard freezing enthalpy and temperature of various compounds, and are estimated using the Clausius-Clapeyron equation.
[0171] The present invention is further described in detail below in conjunction with embodiments.
[0172] Example 1
[0173] A bubble-type heat insulation material is prepared from a low thermal conductivity component A for bubble-type heat insulation material and a bubble wall material B, that is, the bubble wall material B is filled with the low thermal conductivity component A for bubble-type heat insulation material to form bubbles, that is, the bubble wall material B contains bubbles of the low thermal conductivity component A for bubble-type heat insulation material, and the bubbles are filled in the filling space of the film. The bubble wall thickness of the bubble is 0.1g / m2 , diameter is 1mm.
[0174] The low thermal conductivity component A for the bubble type thermal insulation material comprises, by mass percentage, 70% of trans-1-chloro-3,3,3-trifluoropropene; 10% of helium; 15% of hexafluoroethane; and 5% of perfluoro-n-pentane.
[0175] The components of the cell wall material B include, by mass percentage: 59.95% sodium lauryl sulfate; 9% sodium alkylbenzene sulfonate; 9% fatty acid polyoxyethylene ether; 22% hexadecyltrimethylammonium bromide; and 0.05% graphene.
[0176] Example 2
[0177] A bubble-type heat insulation material is prepared from a low thermal conductivity component A for bubble-type heat insulation material and a bubble wall material B, that is, the bubble wall material B is filled with the low thermal conductivity component A for bubble-type heat insulation material to form bubbles, that is, the bubble wall material B contains bubbles of the low thermal conductivity component A for bubble-type heat insulation material. The bubble wall thickness is 1g / m 2 , diameter is 10mm.
[0178] The low thermal conductivity component A for the bubble type thermal insulation material comprises, by mass percentage, 46% of trans-1-chloro-3,3,3-trifluoropropene; 20% of helium; 25% of hexafluoroethane; and 9% of perfluoro-n-pentane.
[0179] The components of the cell wall material B include, by mass percentage: 34.9% sodium lauryl sulfate; 24% sodium alkylbenzene sulfonate; 21% fatty acid polyoxyethylene ether; 20% hexadecyltrimethylammonium bromide; and 0.1% graphene.
[0180] Example 3
[0181] A bubble-type heat insulation material is prepared from a low thermal conductivity component A for bubble-type heat insulation material and a bubble wall material B, that is, the bubble wall material B is filled with the low thermal conductivity component A for bubble-type heat insulation material to form bubbles, that is, the bubble wall material B contains bubbles of the low thermal conductivity component A for bubble-type heat insulation material. The bubble wall thickness is 0.5g / m 2 , diameter is 7mm.
[0182] The low thermal conductivity component A for the bubble type thermal insulation material comprises, by weight percentage, 55% of trans-1-chloro-3,3,3-trifluoropropene; 15% of helium; 20% of hexafluoroethane; and 10% of perfluoro-n-pentane.
[0183] The components of the cell wall material B include, by mass percentage: 44.93% sodium lauryl sulfate; 10% sodium alkylbenzene sulfonate; 10% fatty acid polyoxyethylene ether; 35% hexadecyltrimethylammonium bromide; and 0.07% graphene.
[0184] Example 4
[0185] A bubble-type heat insulation material is prepared from a low thermal conductivity component A for bubble-type heat insulation material and a bubble wall material B, that is, the bubble wall material B is filled with the low thermal conductivity component A for bubble-type heat insulation material to form bubbles, that is, the bubble wall material B contains bubbles of the low thermal conductivity component A for bubble-type heat insulation material. The bubble wall thickness is 0.2g / m 2 , diameter is 3mm.
[0186] The low thermal conductivity component A for the bubble type thermal insulation material includes, by mass percentage, 35% of 1,1,1,3,3-pentafluoropropane; 35% of 1-fluoro-1,1-dichloroethane; 11% of helium; 17% of hexafluoroethane; and 2% of perfluoro-n-pentane.
[0187] The components of the cell wall material B include, by mass percentage: 37.94% sodium lauryl sulfate; 26% sodium alkylbenzene sulfonate; 16% fatty acid polyoxyethylene ether; 20% hexadecyltrimethylammonium bromide; and 0.06% graphene.
[0188] Example 5
[0189] A bubble-type heat insulation material is prepared from a low thermal conductivity component A for bubble-type heat insulation material and a bubble wall material B, that is, the bubble wall material B is filled with the low thermal conductivity component A for bubble-type heat insulation material to form bubbles, that is, the bubble wall material B contains bubbles of the low thermal conductivity component A for bubble-type heat insulation material. The bubble wall thickness is 0.8g / m 2 , diameter is 6mm.
[0190] The low thermal conductivity component A for bubble-type thermal insulation materials includes, by mass percentage:
[0191] 10% 1,1,1,3,3-pentafluoropropane; 10% 1-fluoro-1,1-dichloroethane; 50% trans-1-chloro-3,3,3-trifluoropropene; 10% helium; 15% hexafluoroethane; 5% perfluoropentane.
[0192] The components of the cell wall material B include, by mass percentage: 39.94% sodium lauryl sulfate; 14% sodium alkylbenzene sulfonate; 26% fatty acid polyoxyethylene ether; 20% hexadecyltrimethylammonium bromide; and 0.06% graphene.
[0193] Example 6
[0194] A bubble-type heat insulation material is prepared from a low thermal conductivity component A for bubble-type heat insulation material and a bubble wall material B, that is, the bubble wall material B is filled with the low thermal conductivity component A for bubble-type heat insulation material to form bubbles, that is, the bubble wall material B contains bubbles of the low thermal conductivity component A for bubble-type heat insulation material. The bubble wall thickness is 0.9g / m 2 , diameter is 7mm.
[0195] The low thermal conductivity component A for the bubble type thermal insulation material includes, by mass percentage, 1% of 1,1,1,3,3-pentafluoropropane; 1% of 1-fluoro-1,1-dichloroethane; 68% of trans-1-chloro-3,3,3-trifluoropropene; 10% of helium; 15% of hexafluoroethane; and 5% of perfluoro-n-pentane.
[0196] The components of the cell wall material B include, by mass percentage: 45.91% sodium lauryl sulfate; 14% sodium alkylbenzene sulfonate; 20% fatty acid polyoxyethylene ether; 20% hexadecyltrimethylammonium bromide; and 0.09% graphene.
[0197] Example 7
[0198] A bubble-type heat insulation material is prepared from a low thermal conductivity component A for bubble-type heat insulation material and a bubble wall material B, that is, the bubble wall material B is filled with the low thermal conductivity component A for bubble-type heat insulation material to form bubbles, that is, the bubble wall material B contains bubbles of the low thermal conductivity component A for bubble-type heat insulation material. The bubble wall thickness is 0.2g / m 2 , diameter is 4mm.
[0199] The low thermal conductivity component A for the bubble type thermal insulation material comprises, by mass percentage, 5% of 1,1,1,3,3-pentafluoropropane; 65% of trans-1-chloro-3,3,3-trifluoropropene; 10% of helium; 15% of hexafluoroethane; and 5% of perfluoro-n-pentane.
[0200] The components of the cell wall material B include, by mass percentage: 39.94% sodium lauryl sulfate; 14% sodium alkylbenzene sulfonate; 26% fatty acid polyoxyethylene ether; 20% hexadecyltrimethylammonium bromide; and 0.06% graphene.
[0201] Example 8
[0202] A bubble-type heat insulation material is prepared from a low thermal conductivity component A for bubble-type heat insulation material and a bubble wall material B, that is, the bubble wall material B is filled with the low thermal conductivity component A for bubble-type heat insulation material to form bubbles, that is, the bubble wall material B contains bubbles of the low thermal conductivity component A for bubble-type heat insulation material. The bubble wall thickness is 0.1 g / m 2, diameter is 2mm.
[0203] The low thermal conductivity component A for the bubble type thermal insulation material includes, by mass percentage, 6% of 1-fluoro-1,1-dichloroethane; 64% of trans-1-chloro-3,3,3-trifluoropropene; 10% of helium; 15% of hexafluoroethane; and 5% of perfluoro-n-pentane.
[0204] The components of the cell wall material B include, by mass percentage: 39.94% sodium lauryl sulfate; 14% sodium alkylbenzene sulfonate; 26% fatty acid polyoxyethylene ether; 20% hexadecyltrimethylammonium bromide; and 0.06% graphene.
[0205] Example 9
[0206] A bubble-type heat insulation material is prepared from a low thermal conductivity component A for bubble-type heat insulation material and a bubble wall material B, that is, the bubble wall material B is filled with the low thermal conductivity component A for bubble-type heat insulation material to form bubbles, that is, the bubble wall material B contains bubbles of the low thermal conductivity component A for bubble-type heat insulation material. The bubble wall thickness is 0.2g / m 2 , diameter is 3mm.
[0207] The low thermal conductivity component A for the bubble type thermal insulation material comprises, by mass percentage, 6.36% of 1,1,1,3,3-pentafluoropropane; 63.64% of trans-1-chloro-3,3,3-trifluoropropene; 10% of helium; 15% of hexafluoroethane; and 5% of perfluoro-n-pentane.
[0208] The components of the cell wall material B include, by mass percentage: 39.94% sodium lauryl sulfate; 14% sodium alkylbenzene sulfonate; 26% fatty acid polyoxyethylene ether; 20% hexadecyltrimethylammonium bromide; and 0.06% graphene.
[0209] Example 10
[0210] A bubble-type heat insulation material is prepared from a low thermal conductivity component A for bubble-type heat insulation material and a bubble wall material B, that is, the bubble wall material B is filled with the low thermal conductivity component A for bubble-type heat insulation material to form bubbles, that is, the bubble wall material B contains bubbles of the low thermal conductivity component A for bubble-type heat insulation material. The bubble wall thickness is 0.1 g / m 2 , diameter is 5mm.
[0211] The low thermal conductivity component A for the bubble type thermal insulation material includes, by mass percentage, 1.2% of 1-fluoro-1,1-dichloroethane; 68.8% of trans-1-chloro-3,3,3-trifluoropropylene; 10% of helium; 15% of hexafluoroethane; and 5% of perfluoro-n-pentane.
[0212] The components of the cell wall material B include, by mass percentage: 39.94% sodium lauryl sulfate; 14% sodium alkylbenzene sulfonate; 26% fatty acid polyoxyethylene ether; 20% hexadecyltrimethylammonium bromide; and 0.06% graphene.
[0213] Embodiment 11
[0214] A bubble-type heat insulation material is prepared from a low thermal conductivity component A for bubble-type heat insulation material and a bubble wall material B, that is, the bubble wall material B is filled with the low thermal conductivity component A for bubble-type heat insulation material to form bubbles, that is, the bubble wall material B contains bubbles of the low thermal conductivity component A for bubble-type heat insulation material. The bubble wall thickness is 0.3g / m 2 , diameter is 2mm.
[0215] The low thermal conductivity component A for bubble-type thermal insulation material includes, by mass percentage, 3.36% of 1,1,1,3,3-pentafluoropropane; 3% of 1-fluoro-1,1-dichloroethane; 63.64% of trans-1-chloro-3,3,3-trifluoropropene; 10% of helium; 15% of hexafluoroethane; and 5% of perfluoro-n-pentane.
[0216] The components of the cell wall material B include, by mass percentage: 39.94% sodium lauryl sulfate; 14% sodium alkylbenzene sulfonate; 26% fatty acid polyoxyethylene ether; 20% hexadecyltrimethylammonium bromide; and 0.06% graphene.
[0217] Example 12
[0218] A bubble-type heat insulation material is prepared from a low thermal conductivity component A for bubble-type heat insulation material and a bubble wall material B, that is, the bubble wall material B is filled with the low thermal conductivity component A for bubble-type heat insulation material to form bubbles, that is, the bubble wall material B contains bubbles of the low thermal conductivity component A for bubble-type heat insulation material. The bubble wall thickness is 0.5g / m 2 , diameter is 1mm.
[0219] The low thermal conductivity component A for the bubble type thermal insulation material includes, by mass percentage, 50% of trans-1-chloro-3,3,3-trifluoropropene; 10% of sulfur hexafluoride; 10% of perfluoro-n-butane, 10% of helium; 15% of hexafluoroethane; and 5% of perfluoro-n-pentane.
[0220] The components of the cell wall material B include, by mass percentage: 59.95% sodium lauryl sulfate; 9% sodium alkylbenzene sulfonate; 9% fatty acid polyoxyethylene ether; 22% hexadecyltrimethylammonium bromide; and 0.05% graphene.
[0221] Example 13
[0222] A bubble-type heat insulation material is prepared from a low thermal conductivity component A for bubble-type heat insulation material and a bubble wall material B, that is, the bubble wall material B is filled with the low thermal conductivity component A for bubble-type heat insulation material to form bubbles, that is, the bubble wall material B contains bubbles of the low thermal conductivity component A for bubble-type heat insulation material. The bubble wall thickness is 0.3g / m 2 , diameter is 6mm.
[0223] The low thermal conductivity component A for the bubble type thermal insulation material includes, by mass percentage, 68% of trans-1-chloro-3,3,3-trifluoropropylene; 1% of sulfur hexafluoride; 1% of perfluoro-n-butane; 10% of helium; 15% of hexafluoroethane; and 5% of perfluoro-n-pentane.
[0224] The components of the cell wall material B include, by mass percentage: 59.95% sodium lauryl sulfate; 9% sodium alkylbenzene sulfonate; 9% fatty acid polyoxyethylene ether; 22% hexadecyltrimethylammonium bromide; and 0.05% graphene.
[0225] Embodiment 14
[0226] A bubble-type heat insulation material is prepared from a low thermal conductivity component A for bubble-type heat insulation material and a bubble wall material B, that is, the bubble wall material B is filled with the low thermal conductivity component A for bubble-type heat insulation material to form bubbles, that is, the bubble wall material B contains bubbles of the low thermal conductivity component A for bubble-type heat insulation material. The bubble wall thickness is 0.1 g / m 2 , diameter is 1.5mm.
[0227] The low thermal conductivity component A for the bubble type thermal insulation material comprises, by mass percentage, 65% of trans-1-chloro-3,3,3-trifluoropropene; 5% of sulfur hexafluoride; 10% of helium; 15% of hexafluoroethane; and 5% of perfluoro-n-pentane.
[0228] The components of the cell wall material B include, by mass percentage: 59.95% sodium lauryl sulfate; 9% sodium alkylbenzene sulfonate; 9% fatty acid polyoxyethylene ether; 22% hexadecyltrimethylammonium bromide; and 0.05% graphene.
[0229] Embodiment 15
[0230] A bubble-type heat insulation material is prepared from a low thermal conductivity component A for bubble-type heat insulation material and a bubble wall material B, that is, the bubble wall material B is filled with the low thermal conductivity component A for bubble-type heat insulation material to form bubbles, that is, the bubble wall material B contains bubbles of the low thermal conductivity component A for bubble-type heat insulation material. The bubble wall thickness is 0.35g / m 2 , diameter is 6.5mm.
[0231] The low thermal conductivity component A for the bubble type thermal insulation material comprises, by mass percentage, 63% of trans-1-chloro-3,3,3-trifluoropropene; 7% of perfluoro-n-butane; 10% of helium; 15% of hexafluoroethane; and 5% of perfluoro-n-pentane.
[0232] The components of the cell wall material B include, by mass percentage: 59.95% sodium lauryl sulfate; 9% sodium alkylbenzene sulfonate; 9% fatty acid polyoxyethylene ether; 22% hexadecyltrimethylammonium bromide; and 0.05% graphene.
[0233] In summary, the low thermal conductivity component for the bubble type thermal insulation material of the present invention has a low thermal conductivity coefficient and good thermal insulation properties; the bubble type thermal insulation material having the low thermal conductivity component for the bubble type thermal insulation material not only has a low thermal conductivity coefficient and good thermal insulation properties, but also can utilize the low thermal conductivity component for the bubble type thermal insulation material to maintain the compression resistance of the bubble wall material.
[0234] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A low thermal conductivity component for bubble-type thermal insulation materials, It is characterized in that include: Bubble substrate, helium, hexafluoroethane and perfluoropentane; the bubble substrate includes at least one of trans-1-chloro-3,3,3-trifluoropropene, 1,1,1,3,3-pentafluoropropane and 1-fluoro-1,1-dichloroethane; wherein, In the case where the bubble substrate contains only trans-1-chloro-3,3,3-trifluoropropene, the low thermal conductivity component for the bubble-type thermal insulation material includes, by mass percentage: 46-70% of said trans-1-chloro-3,3,3-trifluoropropene; 10-20% of said helium; 15-25% of said hexafluoroethane; 1-10% of said perfluoro-n-pentane.
2. The low thermal conductivity component for the bubble-type thermal insulation material according to claim 1, It is characterized in that In the case where the bubble substrate contains only the 1,1,1,3,3-pentafluoropropane and the 1-fluoro-1,1-dichloroethane, The low thermal conductivity component for the bubble-type thermal insulation material includes, by mass percentage: 46-70% of the total amount of said 1,1,1,3,3-pentafluoropropane and said 1-fluoro-1,1-dichloroethane; 10-20% of said helium; 15-25% of said hexafluoroethane; 1-10% of said perfluoro-n-pentane.
3. The low thermal conductivity component for the bubble-type thermal insulation material according to claim 1, It is characterized in that In the case where the bubble substrate includes at least one of the 1,1,1,3,3-pentafluoropropane and the 1-fluoro-1,1-dichloroethane, and the trans-1-chloro-3,3,3-trifluoropropene, The low thermal conductivity component for the bubble-type thermal insulation material includes, by mass percentage: 46-70% of the bubble substrate, wherein the 1,1,1,3,3-pentafluoropropane accounts for 1-10% of the total mass of the low thermal conductivity components for the bubble-type thermal insulation material, and / or the 1-fluoro-1,1-dichloroethane accounts for 1-10% of the total mass of the low thermal conductivity components for the bubble-type thermal insulation material; 10-20% of said helium; 15-25% of said hexafluoroethane; 1-10% of said perfluoro-n-pentane.
4. The low thermal conductivity component for the bubble-type thermal insulation material according to claim 3, It is characterized in that The mass of at least one of the 1,1,1,3,3-pentafluoropropane and the 1-fluoro-1,1-dichloroethane is 10-20% of the mass of the trans-1-chloro-3,3,3-trifluoropropene.
5. The low thermal conductivity component for the bubble-type thermal insulation material according to any one of claims 1 to 4, It is characterized in that The low thermal conductivity component for the bubble-type heat insulation material further comprises, by mass percentage, at least one of 1-10% of sulfur hexafluoride and 1-10% of perfluoro-n-butane.
6. A bubble type thermal insulation material, It is characterized in that It is prepared from the low thermal conductivity component and bubble wall material of the bubble-type thermal insulation material described in any one of claims 1 to 5; wherein the components of the bubble wall material include, by mass percentage: 34.9-59.95% of sodium lauryl sulfate; 9-26% of sodium alkylbenzene sulfonate; 9-26% of fatty acid polyoxyethylene ether; 20-35% of hexadecyltrimethylammonium bromide; and 0.05-0.1% of graphene.
7. The bubble-type heat-insulating material according to claim 6, It is characterized in that The bubble-type heat insulation material has bubble walls formed by the bubble wall material, and the bubble-type heat insulation material is filled with low thermal conductivity components in the bubbles; wherein, The bubble wall thickness of the bubble is 0.1-1g / m 2 .
8. The bubble-type heat-insulating material according to claim 7, It is characterized in that The diameter of the bubbles is 1-10 mm.
9. The bubble-type heat-insulating material according to claim 7, It is characterized in that The preparation method of the bubble-type heat-insulating material comprises: using the gaseous bubble-type heat-insulating material with a low thermal conductivity component to blow bubbles so that the bubble wall material forms the bubbles; The gas phase thermal conductivity of the low thermal conductivity component for the gaseous bubble-type thermal insulation material is lower than 15 mw / m·k.
10. The bubble-type heat-insulating material according to any one of claims 6 to 8, It is characterized in that It also includes a film, which encloses a filling space, and uses the gaseous bubble-type thermal insulation material with a low thermal conductivity component to blow bubbles so that the bubble wall material forms bubbles and fills the filling space.
Citation Information
Patent Citations
Cavity filled insulation pack
CA2247782A1
Heat-insulating profile and water heater
CN108506645A
Phase change microcapsule composite material as well as preparation method and application thereof
CN115595123A