CsI (T1) crystal coating treatment method and application of CsI (T1) crystal coating treatment method in n / gamma ray detection

Through CsI(Tl) crystal coating treatment, the detection efficiency of neutron detectors is improved by utilizing the neutron absorption characteristics of 6Li and 10B, and the problems of high cost and low efficiency of existing detectors are solved, and efficient n/γ is achieved Radiation detection and multifunctional applications.

CN118996612APending Publication Date: 2024-11-22HEFEI UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411091910.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Existing neutron detectors are costly and inefficient, especially the 3He gas resources are tight. Traditional semiconductor detectors are weak in domestic research and have not been commercialized, making it difficult to meet the needs of efficient neutron detection.

Method used

The CsI(T1) crystal coating treatment method is used to prepare CsI(T1) heterojunction crystal thin films by using the large neutron absorption cross-section characteristics of 6Li and 10B to improve the detection efficiency of the detector.

Benefits of technology

It significantly improves the detection efficiency of neutron detectors, reduces production costs, and realizes efficient n/γ ray detection. It is suitable for multifunctional applications and portable detectors, adapting to the needs of modern technology development.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996612A_ABST
    Figure CN118996612A_ABST
Patent Text Reader

Abstract

The invention discloses a CsI (T1) crystal coating treatment method and application of the CsI (T1) crystal coating treatment method in n / gamma ray detection. The nuclide scintillator is used for processing CsI (T1), high detection efficiency can be achieved, and the material is used as a scintillator detector probe, so that the efficiency of a detector can be remarkably improved. By applying the embodiment, people can clearly observe that more neutron signals with relatively high PSD values can be obviously detected by a material subjected to film coating treatment. Compared with other processes, the manufacturing cost is low, and the process is mature.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of n / gamma ray detection, and in particular relates to a CsI (Tl) crystal coating processing method and an application thereof in n / gamma ray detection. Background Art

[0002] The discovery of neutrons is a milestone in the history of physics. It reveals the internal structure of the atomic nucleus and opens the door to human research on nuclear energy. With the development of nuclear technology, the application of neutrons has expanded to all walks of life. Neutrons are widely used in agriculture, medical industry and other fields. Neutron detection technology also occupies an important position in aerospace, mineral resource detection and nuclear reaction detection. With the development of science and technology and society, countries around the world have unanimously attached great importance to energy issues. Energy is the driving force for the development of all aspects of modern countries. Research on neutron detectors with nuclear radiation detection capabilities is crucial. Currently, neutron detectors on the market can be divided into three categories: gas detectors, scintillator detectors, and semiconductor detectors. At present, traditional neutron detectors mainly use high pressure 3 He detector. 3 He neutron detectors are the most widely used in the market due to their high detection efficiency, strong radiation resistance and excellent performance. Although they have disadvantages such as large size and slow response speed, they are the most widely used in the market. As more countries invest in research on them, 3 As He gas resources become increasingly scarce, its price has skyrocketed, and the cost of neutron detectors has also risen. Scintillator neutron detectors have gradually replaced neutron detectors due to their unique advantages such as high detection efficiency, strong time resolution, good n / γ discrimination, easy large-scale production and low price. 3 He is used in many neutron instruments. Semiconductor detectors have been studied a lot abroad, but China started late, the research is weak, and has not been commercialized. Summary of the invention

[0003] The object of the present invention is to provide a CsI (Tl) crystal coating treatment method and its application in n / γ ray detection. 6 Li and 10 B The scintillator CsI (Tl) crystal is coated with a film to improve the detection efficiency of the detector due to its large neutron absorption cross section.

[0004] The CsI(Tl) crystal coating treatment method of the present invention adopts a high vacuum vapor phase thermal evaporation deposition technology, comprising the following steps:

[0005] Step 1: Preparation of CsI(Tl) seed layer

[0006] First, place the clean substrate on a fixed bracket above the evaporation tungsten boat, and control the vertical distance between the evaporation tungsten boat and the substrate to be 10-15 cm; under the protection of inert gas, place the CsI (Tl) sample in the clean evaporation tungsten boat, open the vacuum chamber valve to evacuate, and wait until the vacuum degree is reduced to 5.0×10 -4 -5.0×10 -5 Pa, the evaporation of CsI(Tl) powder begins; when the thickness of the seed layer reaches 6-8 nanometers, the evaporation ends and the evaporation power is turned off.

[0007] Step 2: Preparation of CsI(Tl) thin film layer

[0008] Wait until the vacuum degree reaches (1.0-5.0)×10 -5 When the evaporation power is turned on, evaporation is started to obtain a CsI(Tl) film layer with a thickness of 0.01 to 50 microns. The evaporation power is turned off and vacuum is continued.

[0009] Step 3: Preparation of B or Li containing crystalline thin film layer

[0010] Enable another containing LiF or BI 3 The tungsten boat for evaporation of powder is used to reduce the vacuum to (5.0-8.0)×10 -6 Pa, start the evaporation power supply, and evaporate to obtain a crystalline film layer containing B or Li with a thickness of 0.01 to 30 microns; then, turn off the evaporation power supply, wait for the system to cool for 1-2 hours, then take out the sample, and finally obtain a CsI(Tl) heterojunction crystalline film.

[0011] In step 1, the rotation speed of the substrate is controlled at 5-8 rpm, the prefabrication temperature is 120-150°C, and the evaporation rate is controlled at 0.2-0.5 angstroms / second. The substrate can be a FTO substrate or a glass substrate. The glass substrate includes a window glass on a photoelectric conversion device (SiPM, PMT, MPPC, etc.).

[0012] In step 2, the rotation speed of the substrate is 10-15 rpm, the prefabrication temperature is 150-200°C, the evaporation rate is controlled at 0.5-1.0 Å / s in the initial stage, and after 5 minutes of evaporation, the evaporation rate is adjusted to 3-10 Å / s until the evaporation power is turned off after the evaporation is completed.

[0013] In step 3, the rotation speed of the substrate is 3-5 rpm, the prefabrication temperature is 200-250°C, the evaporation rate is controlled at 0.3-0.5 Å / s in the initial stage, and after 10 minutes of evaporation, the evaporation rate is adjusted to 5-15 Å / s until the evaporation power is turned off after the evaporation is completed.

[0014] During the thermal evaporation deposition process, the inert gas is nitrogen, argon, etc.

[0015] The CsI heterojunction film is composed of FTO or glass substrate, CsI (Tl) crystalline film layer, and crystalline film layer containing B or Li in sequence from bottom to top, or FTO or glass substrate, TiO 2 The invention comprises a thin film layer, a CsI (Tl) crystalline thin film layer, and a crystalline thin film layer containing B or Li. The CsI (Tl) crystalline thin film is composed of large-sized crystal particles, with high density and controllable orientation. (The CsI (Tl) crystals on the FTO substrate mainly protrude in the 200 crystal direction, while the CsI (Tl) crystals prepared on the glass substrate mainly protrude in the 110 crystal direction)

[0016] The thickness of the seed layer in the present invention is 6-8 nanometers, the thickness of the CsI (Tl) film is 0.01-50 micrometers, and the thickness of LiF is 0.01-30 micrometers.

[0017] The CsI(Tl) crystalline thin film may be replaced by a NaI(Tl) crystalline thin film.

[0018] The application of the CsI(Tl) heterojunction crystalline film prepared by the present invention in n / gamma ray detection.

[0019] Specifically, the probe crystal material of the scintillator detector is prepared by using the CsI (Tl) heterojunction crystal film.

[0020] The idea of ​​the present invention is 6 Li and 10 Materials such as B have a large neutron absorption cross section, and neutrons react with them to produce photons. Using the above-mentioned nuclide scintillator to process CsI (Tl) can achieve a very high detection efficiency. Using this material as a scintillator detector probe can significantly improve the efficiency of the detector. Through the application examples, we can clearly observe that the material with a coating treatment can significantly detect more neutron signals with higher PSD values. Compared with other processes, the production cost is low and the process is mature.

[0021] 6 Li and 10Materials such as B have a large neutron absorption cross section, and neutrons react with them to produce photons. Using the above-mentioned nuclide scintillator to treat CsI (Tl) can achieve a very high detection efficiency. At present, the preparation process of crystal films is divided into three categories: physical vapor deposition and chemical vapor deposition. Compared with chemical vapor deposition, the physical vapor deposition method has the following characteristics: (1) The preparation steps and principles are simple. (2) The raw materials only need to be vaporized through a physical process, no chemical reaction is involved, and no impurities are introduced. (3) The air pressure environment is relatively low. The lower air pressure environment can reduce the scattering effect of other gas molecules on the gas phase atoms of the raw materials. Physical vapor deposition is divided into three common processes: evaporation, sputtering, and ion plating. The temperature of sputtering and ion plating is too high and will destroy the crystal structure. The deposition rate of the evaporation method is fast, and the resulting crystal film has a high purity. The present invention adopts a vacuum hot plating process to prepare CsI (Tl) crystals, and a crystalline film layer containing B or Li is plated on the CsI (Tl) film layer.

[0022] Our research group develops detectors based on two conventional materials: Li-containing materials and crystals. After functional coating of Li-containing materials, CsI (Tl) detectors can not only detect n / γ rays, but also combine other technologies, such as imaging technology and spectroscopy technology, to achieve multifunctional applications. In addition, with the advancement of science and technology, detectors are becoming more and more miniaturized and portable. Highly integrated and highly sensitive portable n / γ-ray detectors are more in line with the usage habits of modern humans and can be more flexibly applied to various scenarios, such as laboratories, medical treatment, safety testing and other fields. Meet the huge demand in the field of marine monitoring and ensure marine safety. The emergence of extreme weather in recent years has put forward more stringent requirements on the operating environment of detectors. The development of portable detectors can not only meet environmental requirements, but also be combined with high-tech drones, 5G technology, etc., to better adapt to future developments and changes. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a 500nm scanning electron microscope image of CsI(Tl) crystal on FTO substrate.

[0024] Figure 2 This is the XRD image of CsI(Tl) crystal on FTO substrate.

[0025] Figure 3 This is the XRD pattern of CsI(Tl) on glass substrate.

[0026] Figure 4 FTO / TiO 2 Scanning electron microscope image of / CsI / LiF crystal.

[0027] Figure 5 FTO / TiO 2 Scanning electron microscope top view of / CsI / LiF crystal.

[0028] Figure 6 Schematic diagram of the prepared CsI(Tl) crystal structure.

[0029] Figure 7 FTO / TiO 2 Power spectral density diagram of / CsI crystal structure detector.

[0030] Figure 8 FTO / TiO 2 Power spectral density diagram of the / CsI / LiF crystal structure detector. DETAILED DESCRIPTION

[0031] The present invention is further described in detail below with reference to the accompanying drawings and specific implementation examples.

[0032] The following examples use FTO substrate and glass substrate as substrates for preparing CsI(Tl) crystals, respectively, and provide scanning electron microscope images and XRD images of the final samples.

[0033] Example 1: Preparation of CsI(Tl) crystalline thin film on FTO conductive glass substrate

[0034] 1. Cleaning of FTO conductive glass

[0035] FTO substrate cleaning: put it in acetone and use ultrasonic machine to sonicate for 15 minutes. After the acetone sonication is completed, put it in isopropanol and sonicate for 15 minutes. After the isopropanol sonication is completed, use deionized water to sonicate for 15 minutes. After the sonication is completed, put it in a drying oven for standby use.

[0036] 2. Cleaning of coating chamber and evaporation source

[0037] Cleaning and drying of the coating room: Use anhydrous ethanol for wiping. Before coating, it needs to be vacuumed three times to ensure the cleanliness and dryness of the coating room.

[0038] The experiment used a tungsten boat as the resistive evaporation source of Li and CsI.

[0039] The molybdenum boat needs to be cleaned and dried before the experiment.

[0040] Cleaning of evaporation source: rinse the tungsten boat with hydrochloric acid, then put it in acetone and use ultrasonic machine to sonicate for 15 minutes. After the acetone ultrasonication is completed, put it in isopropanol ultrasonication for 15 minutes. After the isopropanol ultrasonication is completed, use deionized water to sonicate for 15 minutes. After the ultrasonication is completed, put it in a drying oven for standby use.

[0041] The tungsten boat should not be exposed to air for too long after it is taken out of the drying box. It should be used quickly and quickly.

[0042] 3. Preparation of CsI(Tl) crystals

[0043] First, place the aluminum probe shell on a fixed bracket above the evaporation groove, and control the vertical distance between the shell bottom and the evaporation groove to be 10 cm. Then place the CsI (Tl) sample in a clean evaporation groove protected by an inert gas (e.g., nitrogen, argon), open the vacuum chamber valve to evacuate, and wait until the vacuum degree drops to 5.0×10 -4 -5.0×10 -5 CsI(Tl) powder was evaporated at 1.50 rpm. The rotation speed of the FTO substrate was ensured to be 5-8 rpm, the prefabrication temperature was 120°C, the evaporation rate was controlled at 0.2 angstroms / second, the thickness of the seed layer was controlled at 6 nanometers, and the evaporation power supply was turned off after the evaporation was completed.

[0044] Wait until the vacuum degree reaches 10 -5 Pa, the evaporation power supply was turned on to start evaporation. The rotation speed of the aluminum probe shell was ensured to be 10 rpm, the prefabrication temperature was 150°C, the evaporation rate was controlled at 0.5 angstroms / second in the initial stage, and after 5 minutes of evaporation, the evaporation rate was adjusted to 3 angstroms / second until the evaporation power supply was turned off after the evaporation was completed to obtain a 500-nanometer-thick CsI(Tl) film layer, while continuing to evacuate the vacuum.

[0045] 4. CsI(Tl) crystal characterization

[0046] Scanning electron microscope image of CsI(Tl) crystal on FTO substrate Figure 1 As shown, the XRD pattern of CsI(Tl) crystal is as follows Figure 2 shown.

[0047] Example 2: Preparation of CsI(Tl) crystalline thin film on glass substrate

[0048] 1. Cleaning of glass substrate

[0049] Glass substrate cleaning: put it in acetone and use ultrasonic machine to sonicate for 15 minutes. After the acetone sonication is completed, put it in isopropanol and sonicate for 15 minutes. After the isopropanol sonication is completed, use deionized water to sonicate for 15 minutes. After the sonication is completed, put it in a drying oven for standby use.

[0050] 2. Preparation of CsI(Tl) crystals

[0051] Cleaning the coating chamber and rinsing the tungsten boat: Same as Example 1.

[0052] First, place the aluminum probe shell on a fixed bracket above the evaporation groove, and control the vertical distance between the bottom of the shell and the evaporation groove to be 13 cm. Then, place the CsI (Tl) sample in a clean evaporation groove protected by an inert gas (e.g., nitrogen, argon), open the vacuum chamber valve to evacuate, and wait until the vacuum degree drops to 10-5 CsI(Tl) powder was evaporated at 0.0400 Pa. A glass substrate was used, the substrate rotation speed was 7 rpm, the prefabrication temperature was 150°C, the evaporation rate was controlled at 0.5 angstroms / second, the thickness of the seed layer was controlled at 8 nanometers, and the evaporation power was turned off after the evaporation was completed.

[0053] The vacuum degree reaches 5.0×10 -5 Pa, the evaporation power supply was turned on to start evaporation. The rotation speed of the aluminum probe shell was 15 rpm, the prefabrication temperature was 200 °C, the evaporation rate was controlled at 1.0 angstroms / second in the initial stage, and after 5 minutes of evaporation, the evaporation rate was adjusted to 5.0 angstroms / second until the evaporation power supply was turned off after the evaporation was completed, and a 600-nanometer-thick CsI(Tl) film layer was obtained, and vacuum was continued.

[0054] 3. CsI(Tl) crystal characterization

[0055] The XRD pattern of CsI(Tl) crystal on glass substrate is shown in Figure 2 , Figure 3 , Figure 4 shown.

[0056] Example 3: TiO 2 Preparation of CsI(Tl) / LiF Heterojunction Thin Films on Thin Film Substrates

[0057] 1. Cleaning of FTO conductive glass

[0058] The glass substrate was ultrasonically cleaned with acetone, isopropanol and ultrapure water for 5 minutes respectively to obtain a clean glass substrate, which was dried and used for later use.

[0059] 2. TiO 2 Preparation of thin film substrate

[0060] Anhydrous ethanol, n-butyl titanate, and glacial acetic acid were mixed in a volume ratio of 20:5:0.5 to prepare a uniform, colorless TiO 2 Then, TiO 2 The sol precursor solution was spin-coated on a clean FTO conductive glass (2500 rpm, 30 s) to obtain TiO 2 Sol-gel film; TiO 2 After the sol film was stored in a moisturizer with a relative humidity of 50% at room temperature for 12 hours, it was placed in a muffle furnace with an air atmosphere, and the temperature of the muffle furnace was raised to 550°C at a heating rate of 1°C / min and maintained at this temperature for 30 minutes to perform TiO 2 Sintering of the sol film; after sintering, the muffle furnace was cooled to room temperature at a rate of 1°C / min to obtain TiO 2 Thin film substrate (abbreviated as FTO / TiO 2 film).

[0061] 3. Preparation of CsI(Tl) crystals

[0062] Cleaning of evaporation source: rinse the tungsten boat with hydrochloric acid, then put it in acetone and use ultrasonic machine to sonicate for 15 minutes. After the acetone ultrasonication is completed, put it in isopropanol ultrasonication for 15 minutes. After the isopropanol ultrasonication is completed, use deionized water to sonicate for 15 minutes. After the ultrasonication is completed, put it in a drying oven for standby use.

[0063] The tungsten boat should not be exposed to air for too long after it is taken out of the drying box. It should be used quickly and quickly.

[0064] First, place the aluminum probe shell on a fixed bracket above the evaporation groove, and control the vertical distance between the bottom of the shell and the evaporation groove to be 10 cm. Then, place the CsI(Tl) sample in a clean evaporation groove protected by an inert gas (e.g., nitrogen, argon), open the vacuum chamber valve to evacuate, and wait until the vacuum degree drops to 5.0×10 -4 -5.0×10 -5 CsI(Tl) powder was evaporated at 1.50 rpm. The rotation speed of the FTO substrate was ensured to be 5-8 rpm, the prefabrication temperature was 120°C, the evaporation rate was controlled at 0.2 angstroms / second, the thickness of the seed layer was controlled at 6 nanometers, and the evaporation power supply was turned off after the evaporation was completed.

[0065] Wait until the vacuum degree reaches 10 -5 Pa, the evaporation power supply was turned on to start evaporation. The rotation speed of the aluminum probe shell was ensured to be 10 rpm, the prefabrication temperature was 150°C, the evaporation rate was controlled at 0.5 angstroms / second in the initial stage, and after 5 minutes of evaporation, the evaporation rate was adjusted to 3 angstroms / second until the evaporation was completed and the evaporation power supply was turned off to obtain a 3.96 μm thick CsI (Tl) film layer, while continuing to evacuate.

[0066] 4. LiF crystal preparation

[0067] The evaporation tungsten boat containing LiF powder was started and the vacuum was reduced to 5.0×10 -6 Pa, start the evaporation power supply. Among them, ensure that the rotation speed of the aluminum probe shell is 3 rpm, the prefabrication temperature is 200°C, the evaporation rate is controlled at 0.3 angstroms / second in the initial stage, and after 10 minutes of evaporation, adjust the evaporation rate to 5 angstroms / second until the evaporation power supply is turned off after the evaporation is completed, and a 0.22 micron thick Li-containing crystalline film is obtained. At this point, turn off the evaporation power supply, wait for the system to cool for 1 hour, then take out the sample, and finally obtain the CsI (Tl, Li) crystalline film as the scintillator probe crystal material.

[0068] Figure 7 and Figure 8 FTO / TiO 2 / CsI crystal, FTO / TiO 2 / CsI / LiF crystal is used as the scintillator detector probe material. By comparison, it can be found that FTO / TiO 2 / CsI / LiF crystal structure can detect more neutron signals, which is significantly better than FTO / TiO 2 / CsI crystal structure.

Claims

1. A CsI(Tl) crystal coating treatment method, characterized in that The steps include: Step 1: Preparation of CsI(Tl) seed layer First, place the clean substrate on a fixed bracket above the evaporation tungsten boat, and control the vertical distance between the evaporation tungsten boat and the substrate to be 10-15 cm; under the protection of inert gas, place the CsI (Tl) sample in the clean evaporation tungsten boat, open the vacuum chamber valve to evacuate, and wait until the vacuum degree is reduced to 5.0×10 -4 -5.0×10 -5 Pa, the CsI(Tl) powder was evaporated to obtain a CsI(Tl) seed layer; Step 2: Preparation of CsI(Tl) thin film layer Wait until the vacuum degree reaches (1.0-5.0)×10 -5 When Pa, the evaporation power supply is turned on to start evaporation, and a CsI(Tl) thin film layer is obtained; Step 3: Preparation of B or Li containing crystalline thin film layer Start another tungsten evaporation boat containing LiF or BI3 powder and wait until the vacuum degree drops to (5.0-8.0)×10 -6 Pa, start the evaporation power supply, and evaporate to obtain a crystalline thin film layer containing B or Li; at this point, turn off the evaporation power supply, wait for the system to cool down for 1-2 hours, then take out the sample, and finally obtain a CsI(Tl) heterojunction crystalline thin film.

2. The method according to claim 1, characterized in that: In step 1, the rotation speed of the substrate is controlled at 5-8 rpm, the prefabrication temperature is 120-150° C., and the evaporation rate is controlled at 0.2-0.5 angstroms / second.

3. The method according to claim 2, characterized in that: In step 1, when the thickness of the seed layer reaches 6-8 nanometers, the evaporation is completed and the evaporation power supply is turned off.

4. The method according to claim 1, characterized in that: In step 2, the rotation speed of the substrate is 10-15 rpm, the prefabrication temperature is 150-200°C, the evaporation rate is controlled at 0.5-1.0 Å / s in the initial stage, and after 5 minutes of evaporation, the evaporation rate is adjusted to 3-10 Å / s until the evaporation power is turned off after the evaporation is completed.

5. The method according to claim 4, characterized in that: In step 2, when the thickness of the CsI(Tl) thin film layer reaches 0.01 to 50 μm, the evaporation power supply is turned off and vacuuming is continued.

6. The method according to claim 1, characterized in that: In step 3, the rotation speed of the substrate is 3-5 rpm, the prefabrication temperature is 200-250°C, the evaporation rate is controlled at 0.3-0.5 Å / s in the initial stage, and after 10 minutes of evaporation, the evaporation rate is adjusted to 5-15 Å / s until the evaporation power is turned off after the evaporation is completed.

7. The method according to claim 6, characterized in that: In step 3, the thickness of the crystalline thin film layer containing B or Li is 0.01 to 30 microns.

8. Application of the CsI(Tl) heterojunction crystalline thin film prepared according to any one of claims 1 to 7 in n / γ-ray detection.

9. The use according to claim 8, characterized in that: The probe crystal material of the scintillator detector is prepared by using the CsI(Tl) heterojunction crystal film.