Display, light-emitting device, quantum dot fluorescent composite film and preparation method of quantum dot fluorescent composite film
By setting a composite absorption layer of the blue light absorption layer and the microlens array on the quantum dot fluorescent layer, the problem of insufficient blue light absorption value in the prior art is solved, the luminescence uniformity and light output efficiency of the quantum dot display device are improved, and the thin film is realized Highly efficient blue light absorption.
Patent Information
- Application Number
- CN202310551341.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-16
- Publication Date
- 2024-11-22
AI Technical Summary
The existing photoluminescent color conversion films are difficult to combine small thickness and high blue light absorption values, which affects the color development effect and light output efficiency of quantum dot display devices.
A quantum dot fluorescent composite film was designed, including a quantum dot fluorescent layer and a composite absorbing layer. The composite absorbing layer consists of a blue light absorbing layer and a microlens array. The blue light absorbing layer uses curable polymers and blue light absorbing dyes. The microlenses are used. The array is made of materials such as polydimethylsiloxane. This structure allows the absorption and optical path adjustment of the blue light on the quantum dot fluorescent layer.
The blue light absorption value of the quantum dot fluorescent composite film is maintained at a high level, which improves the luminescence uniformity and light output efficiency, and reduces the thickness of the film, meeting the requirements of display devices for blue light absorption and light output efficiency.
Smart Images

Figure CN119012749A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of quantum dot display technology, and more specifically, to a display, a light-emitting device, a quantum dot fluorescent composite film and a preparation method thereof. Background Art
[0002] Quantum dots are semiconductor nanostructures that bind excitons in three spatial directions. By applying a certain electric field or light pressure to this nano-semiconductor material, they will emit light of a specific frequency, and the frequency of the emitted light will change with the size of the semiconductor. Therefore, by adjusting the size of the nano-semiconductor, the color of the light it emits can be controlled. Since this nano-semiconductor has the property of confining electrons and electron holes, which is similar to atoms or molecules in nature, it is called a quantum dot.
[0003] The construction of full-color quantum dot display devices relies on the precise patterning of red, green and blue light-emitting device units. In response to the optoelectronic application needs of quantum dots, the device technologies currently under development, such as quantum dot micro-display (QD microled Display) and quantum dot-organic electroluminescence (QD-OLED), are the most cutting-edge ways to achieve high color rendering.
[0004] According to the design requirements of device structure and optical effect, the thickness of the photoluminescent color conversion film required by the above device is generally thin, but at the same time, it is necessary to ensure that all blue light from the blue light source is absorbed by the color conversion film. However, it is difficult for existing photoluminescent color conversion films to have both a small thickness and a high blue light absorption value. Summary of the invention
[0005] The technical problem to be solved by the embodiments of the present application is to provide a photoluminescent color conversion film with a smaller thickness and a higher blue light absorption value.
[0006] In order to solve the above technical problems, the embodiment of the present application provides a quantum dot fluorescent composite film, which specifically includes:
[0007] A quantum dot fluorescent layer and a composite absorption layer are sequentially arranged from bottom to top on the substrate;
[0008] The composite absorption layer comprises a blue light absorption layer and a microlens array layer, and the blue light absorption layer is located between the quantum dot fluorescent layer and the microlens array layer.
[0009] Furthermore, the material of the blue light absorbing layer includes a curable high molecular polymer and a blue light absorbing dye.
[0010] Further, the material of the blue light absorbing layer comprises the following combination calculated by weight: 3-5 parts of the blue light absorbing dye and 95-97 parts of the curable high molecular polymer; and / or
[0011] The curable high molecular polymer material includes at least one of polyimide, epoxy resin, phenolic resin, urea-formaldehyde resin, melamine-formaldehyde resin, furan resin, silicone resin, polyester resin, polyamide resin, acrylic resin, polyurethane, vinyl resin, hydrocarbon resin or polyether resin; and / or
[0012] The blue light absorbing dye has an absorbable wavelength of 430nm-500nm; and / or
[0013] The blue light absorbing dye has an absorbable peak wavelength of 455nm-465nm; and / or
[0014] The blue light absorbing dye is at least one of Epolight 5843, Epolight 5765, Epolight 5532 or Epolight7276G.
[0015] Furthermore, the material of the microlens array layer includes at least one of polydimethylsiloxane, polymethyl methacrylate, polystyrene, polycarbonate or photoresist.
[0016] Furthermore, the microlenses on the microlens array layer are convex lenses, and the convex lens array is arranged on the blue light absorbing layer.
[0017] Furthermore, the thickness of the quantum dot fluorescent composite film is 1-10 μm.
[0018] Furthermore, the thickness of the quantum dot fluorescent layer is 6-9.8 μm, and the thickness of the blue light absorbing layer is 0.1-3.9 μm.
[0019] In order to solve the above technical problems, the present application also provides a method for preparing a quantum dot fluorescent composite film according to an embodiment, which adopts the following technical solution:
[0020] Providing a quantum dot ink solution, and placing the quantum dot ink solution on a substrate to form a quantum dot fluorescent layer;
[0021] Providing a blue light absorbing solution, and forming a blue light absorbing layer on the quantum dot fluorescent layer with the blue light absorbing solution;
[0022] A microlens array is prepared on the blue light absorbing layer, and the blue light absorbing layer and the microlens array form a composite absorbing layer to obtain a quantum dot fluorescent composite film.
[0023] Furthermore, the step of preparing a microlens array on the blue light absorbing layer specifically includes:
[0024] Providing a grid template, wherein at least one side of the grid template is provided with a grid structure;
[0025] Disposing a lens material on the blue light absorbing layer;
[0026] Attaching the grid template with the grid structure on the lens material so that the lens material fills the grid structure;
[0027] The lens material is solidified on the blue light absorbing layer, and the grid template is peeled off to form a microlens array.
[0028] Furthermore, in the step of curing the lens material on the blue light absorbing layer, the lens material includes at least one of polydimethylsiloxane solution, polymethyl methacrylate, polystyrene, polycarbonate and photoresist; and / or the curing temperature is 35-45° C., and the curing time is 2-4 hours.
[0029] Further, the polydimethylsiloxane solution includes polydimethylsiloxane and a curing agent;
[0030] wherein the curing agent is selected from at least one of an isocyanate curing agent, a diamine curing agent, a triamine curing agent or a tetramine curing agent; the isocyanate curing agent is selected from at least one of HDI isocyanate, TDI isocyanate or IPDI isocyanate; the diamine curing agent is selected from at least one of hydroxyethylethylenediamine or 1,3-propylenediamine; the triamine curing agent is selected from at least one of diethylenetriamine, triethylamine or triethanolamine; and the tetramine curing agent is selected from triethylenetetramine; and / or
[0031] The mass ratio of the polydimethylsiloxane to the curing agent is (8-10):(1-2).
[0032] Furthermore, the preparation steps of the blue light absorbing solution include:
[0033] Mixing a curable high molecular polymer material with a blue light absorbing dye to obtain the blue light absorbing solution;
[0034] The blue light absorbing solution comprises the following combination by weight: 3-5 parts of the blue light absorbing dye and 95-97 parts of the curable high molecular polymer; and / or
[0035] The curable high molecular polymer material includes at least one of polyimide, epoxy resin, phenolic resin, urea-formaldehyde resin, melamine formaldehyde resin, furan resin, silicone resin, polyester resin, polyamide resin, acrylic resin, polyurethane, vinyl resin, hydrocarbon resin, and polyether resin; and / or
[0036] The absorbable wavelength of the blue light absorbing dye is 430nm-470nm; and / or
[0037] The blue light absorbing dye has an absorbable peak wavelength of 455nm-465nm; and / or
[0038] The blue light absorbing dye is at least one of Epolight 5843, Epolight 5765, Epolight 5532 and Epolight7276G.
[0039] Furthermore, the step of disposing the blue light absorbing solution on the quantum dot fluorescent layer to form a blue light absorbing layer specifically includes:
[0040] Disposing the blue light absorbing solution on the quantum dot fluorescent layer;
[0041] Performing a first heating curing on the blue light absorbing solution;
[0042] Performing a second heating and curing on the blue light absorbing solution to obtain the blue light absorbing layer on the quantum dot fluorescent layer;
[0043] Wherein, the temperature of the first heating and curing is 100-120°C, and the heating and curing time is 20min-40min; and / or
[0044] The temperature of the second heating and curing is 140° C.-160° C., and the time of heating and curing is 50 min-70 min.
[0045] Further, the quantum dot ink solution includes quantum dot material and an organic solvent;
[0046] The quantum dot material includes one or more of silicon quantum dots, germanium quantum dots, sulfide quantum dots, selenide quantum dots, telluride quantum dots, phosphide quantum dots, arsenide quantum dots and indium copper sulfide quantum dots; and / or
[0047] The quantum dot material includes at least one of a single structure quantum dot and a core-shell structure quantum dot, and the material of the single structure quantum dot, the core material of the core-shell structure quantum dot and the shell material of the core-shell structure quantum dot are independently selected from at least one of a II-VI group compound, a IV-VI group compound, a III-V group compound and a I-III-VI group compound;
[0048] Wherein, the II-VI Group compound is selected from at least one of CdS, CdSe, CdTe, ZnS, ZnSe, ZnTe, ZnO, HgS, HgSe, HgTe, CdSeS, CdSeTe, CdSTe, ZnSeS, ZnSeTe, ZnSTe, HgSeS, HgSeTe, HgSTe, CdZnS, CdZnSe, CdZnTe, CdHgS, CdHgSe, CdHgTe, HgZnS, HgZnSe, HgZnTe, CdZnSeS, CdZnSeTe, CdZnSTe, CdHgSeS, CdHgSeTe, CdHgSTe, HgZnSeS, HgZnSeTe and HgZnSTe;
[0049] The IV-VI group compound is selected from at least one of SnS, SnSe, SnTe, PbS, PbSe, PbTe, SnSeS, SnSeTe, SnSTe, PbSeS, PbSeTe, PbSTe, SnPbS, SnPbSe, SnPbTe, SnPbSSe, SnPbSeTe and SnPbSTe;
[0050] The III-V group compound is selected from at least one of GaN, GaP, GaAs, GaSb, AlN, AlP, AlAs, AlSb, InN, InP, InAs, InSb, GaNP, GaNAs, GaNSb, GaPAs, GaPSb, AlNP, AlNAs, AlNSb, AlPAs, AlPSb, InNP, InNAs, InNSb, InPAs, InPSb, GaAlNP, GaAlNAs, GaAlNSb, GaAlPAs, GaAlPSb, GaInNP, GaInNAs, GaInNSb, GaInPAs, GaInPSb, InAlNP, InAlNAs, InAlNSb, InAlPAs or InAlPSb;
[0051] The I-III-VI group compound is selected from at least one of CuInS2, CuInSe2 and AgInS2; and / or
[0052] The organic solvent includes one or more of an alkane solvent, an alcohol solvent, an aromatic solvent and a ketone solvent;
[0053] Wherein, the alkane solvent is at least one of hexane, octane, decane and alkane; the alcohol solvent is hexylethanol; the aromatic solvent is at least one of benzene, toluene, xylene and alkylbenzene; the ketone solvent is at least one of acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, N-methylpyrrolidone and tetrahydrofuran; and / or
[0054] The quantum dot material surface is bound with a ligand, wherein the ligand comprises at least one of an acid ligand, a thiol ligand, an amine ligand and an oxide phosphine ligand;
[0055] wherein the acid ligand comprises at least one of oleic acid, decanoic acid, undecyl acid, dodecyl acid, tridecyl acid, tetradecyl acid, hexadecyl acid, octadecyl acid, undecylenic acid, dodecylenic acid, tridecylenic acid, tetradecylenic acid, pentadecylenic acid, hexadecylenic acid, heptadecenic acid and octadecylenic acid;
[0056] The thiol ligand comprises at least one of n-butyl mercaptan, 1-pentanethiol, hexyl mercaptan, 1-decyl mercaptan, benzene mercaptan, benzyl mercaptan, octadecyl mercaptan, dodecyl mercaptan and octadecyl mercaptan;
[0057] The amine ligand comprises at least one of oleylamine, n-octylamine, tributylamine, trihexylamine, triheptylamine, trioctylamine, trinonylamine, tridecylamine, nitroaniline and sulfonaniline;
[0058] The phosphine oxide ligand includes at least one of tributylphosphine, trihexylphosphine, triheptylphosphine, trioctylphosphine, trioctylphosphine oxide, trinonylphosphine and tridecylphosphine.
[0059] In order to solve the above technical problems, the embodiment of the present application further provides a light emitting device, which adopts the following technical solution:
[0060] The light-emitting device comprises a substrate and a quantum dot fluorescent composite film as provided in any of the above schemes or a quantum dot fluorescent composite film prepared by the preparation method provided in any of the above schemes, wherein a blue light-emitting unit is provided on the substrate, and the quantum dot fluorescent composite film is arranged on the blue light-emitting unit.
[0061] In order to solve the above technical problems, the embodiment of the present application further provides a display, which adopts the following technical solution:
[0062] The display comprises the light emitting device provided by the above solution.
[0063] Compared with the prior art, the embodiments of the present application have the following beneficial effects:
[0064] In the present application, a composite absorption layer composed of a blue light absorption layer and a microlens array is arranged on the quantum dot fluorescent layer. The composite absorption layer covering the quantum dot fluorescent layer absorbs excess blue light on the quantum dot fluorescent layer, thereby ensuring that the blue light absorption value of the quantum dot fluorescent composite film is maintained at a high level. The arrangement of the microlens array can also enhance the light output coupling efficiency of the quantum dot fluorescent composite film, improve the luminous uniformity and light extraction efficiency of the quantum dot device, and make the quantum dot fluorescent composite film of the present application have a smaller thickness and at the same time have a higher blue light absorption value and light extraction efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0065] In order to more clearly illustrate the scheme of the present application, a brief introduction is given below to the drawings required for use in the description of the embodiments. Obviously, the drawings described below are some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0066] Figure 1 This is a schematic diagram of the structure of a quantum dot fluorescent composite film provided by an embodiment of the present application;
[0067] Figure 2 yes Figure 1 A top view of the microlens array layer of the quantum dot fluorescent composite film;
[0068] Figure 3 yes Figure 1 A flowchart of a method for preparing a quantum dot fluorescent composite film is provided;
[0069] Figure 4 yes Figure 2 Specific method flow chart of step S300;
[0070] Figure 5 yes Figure 3 Specific method flow chart of step S310;
[0071] Figure 6 It is the fluorescence spectra of Example 1 and Comparative Example 2 of the present application.
[0072] Reference numerals:
[0073] 500, substrate; 600, quantum dot fluorescent layer; 700, blue light absorption layer; 800, microlens array layer. DETAILED DESCRIPTION
[0074] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by technicians in the technical field of this application; the terms used in the specification of the application herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" and any variations thereof in the specification and claims of this application and the above-mentioned drawings are intended to cover non-exclusive inclusions. The terms "first", "second", etc. in the specification and claims of this application or the above-mentioned drawings are used to distinguish different objects, not to describe a specific order.
[0075] Reference to "embodiment" herein means that the specific features, structures or characteristics described in conjunction with the embodiment may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein can be combined with other embodiments. The reagents used in the embodiments described herein, unless otherwise specified, are all products obtained through commercial channels.
[0076] like Figure 1 As shown, the embodiment of the present application provides a quantum dot fluorescent composite film, which includes: a quantum dot fluorescent layer 600 and a composite absorption layer arranged sequentially from bottom to top on a substrate;
[0077] The composite absorption layer includes a blue light absorption layer 700 and a microlens array layer 800 . The blue light absorption layer 700 is located between the quantum dot fluorescent layer 600 and the microlens array layer 800 .
[0078] In this embodiment, a composite absorption layer composed of a blue light absorption layer 700 and a microlens array layer 800 is arranged on the quantum dot fluorescent layer 600. The composite absorption layer covering the quantum dot fluorescent layer 600 absorbs excess blue light on the quantum dot fluorescent layer 600, thereby ensuring that the blue light absorption value of the quantum dot fluorescent composite film is maintained at a high level. The arrangement of the microlens array layer 800 can also enhance the light output coupling efficiency of the quantum dot fluorescent composite film, improve the luminous uniformity and light extraction efficiency of the quantum dot device, and make the quantum dot fluorescent composite film of the present application have a smaller thickness and at the same time have a higher blue light absorption value and light extraction efficiency.
[0079] Due to the curing shrinkage and solvent volatilization of the quantum dot ink during the drying process, the quantum dot fluorescent layer will form a "coffee ring" structure with a concave middle part on the substrate. Such an uneven film formation structure will reduce the light extraction efficiency of the quantum dot fluorescent layer, easily leak light, and cause uneven color. In this embodiment, a composite absorption layer is arranged on the quantum dot fluorescent layer 600. Through the combination of the composite absorption layer and the quantum dot fluorescent layer 600, the light extraction efficiency of the quantum dot fluorescent layer with uneven film formation can be improved, and the light extraction uniformity can be improved.
[0080] In this embodiment, the material of the blue light absorbing layer 700 includes a curable high molecular polymer and a blue light absorbing dye.
[0081] In some embodiments, the blue light absorbing dye is a yellow dye.
[0082] In some embodiments, the material of the blue light absorbing layer 700 includes the following combination by weight: 3-5 parts of blue light absorbing dye and 95-97 parts of curable high molecular polymer. Under this weight ratio range, the blue light absorption value of the blue light absorbing layer 700 can be controlled within an ideal range.
[0083] In some embodiments, the material of the blue light absorbing layer 700 may be a combination of 3 parts of a blue light absorbing dye and 97 parts of a curable high polymer. In other embodiments, the material of the blue light absorbing layer 700 may be a combination of 4 parts of a blue light absorbing dye and 96 parts of a curable high polymer. In this embodiment, the material of the blue light absorbing layer 700 is a combination of 5 parts of a blue light absorbing dye and 95 parts of a curable high polymer.
[0084] In some embodiments, the curable polymer material includes at least one of polyimide, epoxy resin, phenolic resin, urea-formaldehyde resin, melamine formaldehyde resin, furan resin, silicone resin, polyester resin, polyamide resin, acrylic resin, polyurethane, vinyl resin, hydrocarbon resin or polyether resin.
[0085] In this embodiment, the curable high molecular polymer material is polyimide. It should be noted that polyimide refers to a class of polymers containing an imide ring (-CO-NR-CO-) on the main chain. The derivatives of polyimide refer to other polymers containing an imide ring (-CO-NR-CO-) obtained by the reaction of polyimide. This embodiment uses polyimide as one of the materials of the blue light absorbing layer 700, so that the blue light absorbing layer 700 has good mechanical properties and rigidity, can effectively resist impact, and better protect the quantum dots in the quantum dot fluorescent layer 600. The blue light absorbing layer 700 with polyimide has high radiation resistance and high temperature resistance. Even under long-term illumination and heat, it will not discolor, which greatly improves the service life of the quantum dot light-emitting device.
[0086] In some embodiments, the absorbable wavelength of the blue light absorbing dye is 430nm-500nm. Specifically, the blue light absorbing dye can absorb the blue light within the absorption wavelength range emitted by the blue light emitting unit, and the blue light absorbing dye within the absorption wavelength range can have a high blue light absorption efficiency. In the photoluminescent quantum dot fluorescent layer, the green light quantum dots or the red light quantum dots are excited by the blue light emitted by the light emitting unit and emit green light or red light, but the green light or red light emitted by such a quantum dot light emitting layer is often doped with unused blue light, and the excess blue light is mixed in the green light or red light, resulting in a low purity of the light color. In this embodiment, a blue light absorbing layer containing a blue light absorbing dye is arranged on the quantum dot light emitting layer, and the blue light absorbing dye in the blue light absorbing layer can absorb blue light of a specific wavelength, and at the same time will not affect the green light or red light emitted by the quantum dot fluorescent layer, thereby obtaining green light or red light with higher purity.
[0087] In some embodiments, the maximum absorption wavelength of the blue light absorbing dye may be 430 nm, 470 nm or 500 nm.
[0088] In some embodiments, the peak absorption wavelength of the blue light absorbing dye is 455nm-465nm, specifically 455nm, 460nm, 465nm, 455nm-460nm or 460nm-465nm.
[0089] In some embodiments, the blue light absorbing dye is at least one of Epolight 5843, Epolight 5765, Epolight5532 and Epolight 7276G. Of course, in other embodiments, other yellow visible light dyes can also be selected, as long as the absorption wavelength is within the range of 430nm-500nm or the peak wavelength is within the range of 455nm-465nm.
[0090] In the embodiment, the blue light absorbing layer 700 is prepared from polyimide and blue light absorbing dye, so that the blue light absorbing layer 700 has stable and strong characteristics. The composite absorbing layer is arranged on the quantum dot fluorescent layer 600. The combination of the composite absorbing layer and the quantum dot fluorescent layer 600 can effectively block the migration of electrons, prevent the corrosion of the device, play a moisture-proof effect, effectively prevent the quantum dot fluorescent layer 600 from collapsing due to the effect of thermal stress, and effectively protect the life of the quantum dot fluorescent layer 600.
[0091] In some embodiments, the material of the microlens array layer 800 includes at least one of polydimethylsiloxane, polymethyl methacrylate, polystyrene, polycarbonate and photoresist. It can be understood that the microlens array layer 800 formed by the above-mentioned light-transmitting polymer can achieve high light transmittance of the lens and improve the light extraction efficiency.
[0092] In this embodiment, the material of the microlens array layer 800 is polydimethylsiloxane. It can be understood that the present embodiment uses polydimethylsiloxane as the material of the microlens array layer 800, so that the microlens array layer 800 can form a close and stable bonding surface with the contact interface between the polyimide of the blue light absorption layer 700, thereby improving the bonding strength between the microlens array layer 800 and the blue light absorption layer 700, and no other adhesive is required to be added, so as to ensure that the formed composite absorption layer is a whole with strong stability, effectively prevent the entry of external water and oxygen from affecting the quantum dot fluorescent layer 600 and the substrate 500, and extend the service life of the quantum dot fluorescent composite film. The microlens array layer 800 formed by the thermal curing of polydimethylsiloxane has a colorless and transparent appearance, a light transmittance of 100%, and has excellent characteristics such as heat resistance, cold resistance, and water resistance. The microlens array layer 800 is formed and covered on the blue light absorption layer 700, which can improve the luminous efficiency and life of the quantum dot fluorescent composite film.
[0093] Specifically, the thickness of the quantum dot fluorescent composite film is 1-10 μm. In some embodiments, the thickness of the quantum dot fluorescent composite film can be set to 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 7.5 μm, 8 μm, 8.5 μm, 9 μm, 9.5 μm or 10 μm. The thickness of the quantum dot fluorescent composite film within this range can meet the structural thickness requirements of existing displays.
[0094] In some embodiments, the thickness of the quantum dot fluorescent layer 600 is 6-9.8 μm, and the thickness of the blue light absorbing layer 700 is 0.1-3.9 μm. In one embodiment, when the thickness of the quantum dot fluorescent layer 600 is 6 μm, the thickness of the blue light absorbing layer 700 can be set to 0.1-3.9 μm. In some other embodiments, when the thickness of the quantum dot fluorescent layer 600 is 7 μm, the thickness of the blue light absorbing layer 700 can be set to 0.1-2.9 μm. Of course, in other embodiments, the thickness of the quantum dot fluorescent layer 600 can also be set to 8 μm or 9.8 μm, and the thickness of the blue light absorbing layer 700 can be set to 0.1-1.9 μm or 0.1 μm accordingly.
[0095] In this embodiment, the thickness of the quantum dot fluorescent layer 600 is 7 μm, and the thickness of the blue light absorbing layer 700 is 2.5 μm.
[0096] The quantum dot fluorescent layer 600 and the blue light absorption layer 700 are within the above-mentioned thickness range, which can ensure that the thickness of the quantum dot fluorescent composite film does not exceed 10μm, meets the thickness requirement, and at the same time can have a higher blue light absorption value and luminous efficiency, and can also reduce the cost of the quantum dot ink solution used to prepare the quantum dot fluorescent layer 600.
[0097] like Figure 2 As shown, the microlenses on the microlens array layer 800 are convex lenses, and the convex lens array is arranged on the blue light absorbing layer.
[0098] Specifically, the convex lenses are arranged in a rectangular array on the blue light absorbing layer, and the convex lenses are nano-sized.
[0099] The convex lenses arranged in a rectangular array are disposed on the blue light absorption layer 700, so that the light emitted by the quantum dot light emitting layer 600 can pass through the blue light absorption layer 700, and then pass through the convex lenses for optical path adjustment before being emitted. The convex lenses arranged in an array can effectively enhance the light output coupling efficiency of the quantum dot fluorescent layer 600, improve the uniformity of light emission, and greatly improve the light emission efficiency of the quantum dot fluorescent layer while ensuring that the blue light absorption value meets the requirements. The rectangular array arrangement of the convex lenses is adapted to the arrangement of the pixels on the substrate, effectively improving the display effect.
[0100] It should be noted that, since the convex lenses on the microlens array 800 are of nanometer size, the thickness of the microlens array 800 is also of nanometer size, which has little effect on the thickness of the quantum dot fluorescent composite film.
[0101] The construction of full-color quantum dot display devices relies on the precise patterning of red, green and blue light-emitting device units. According to the design requirements of the device structure and optical effects, the thickness of the photoluminescent color conversion film required by the device needs to be controlled below 10μm, while ensuring that all blue light from the blue light source is absorbed by the color conversion film. If converted into a quantitative standard, it is generally measured by the absorbance value of the blue light band (450nm), that is, the absorbance of the color conversion film to blue light (abbreviation: OD@450nm) needs to be no less than 2, so as to ensure that no less than 99% of the blue light is fully absorbed by the quantum dots, thereby ensuring full utilization of blue light, improving energy utilization, and ensuring that the color gamut and color purity of the display are high enough to achieve high-quality images.
[0102] It can be understood that the present application provides a quantum dot fluorescent layer 600 and a composite absorption layer formed by attaching a blue light absorption layer 700 and a microlens array layer 800 on the substrate, and the composite absorption layer covering the quantum dot fluorescent layer 600 absorbs the blue light emitted from the quantum dot fluorescent layer 600 without affecting the green light or red light emitted by the quantum dot fluorescent layer 600, thereby obtaining a single green light and red light, which can ensure that the quantum dot fluorescent composite film is thinner as a whole and the blue light absorption value is maintained at a high level. The provision of the microlens array layer 800 can also enhance the light output coupling efficiency of the quantum dot fluorescent composite film, improve the luminous uniformity and light extraction efficiency of the quantum dot device, so that the thickness of the quantum dot fluorescent composite film meets the requirements while having a high blue light absorption value and light extraction effect.
[0103] like Figure 3As shown, the present application embodiment provides a method for preparing the quantum dot fluorescent composite film provided in any of the above embodiments, and the method specifically includes:
[0104] S100, providing a quantum dot ink solution, and placing the quantum dot ink solution on a substrate to form a quantum dot fluorescent layer;
[0105] S200, providing a blue light absorbing solution, and placing the blue light absorbing solution on the quantum dot fluorescent layer to form a blue light absorbing layer;
[0106] S300, preparing a microlens array on the blue light absorption layer, the blue light absorption layer and the microlens array form a composite absorption layer, and obtaining a quantum dot fluorescent composite film.
[0107] The present application directly constructs a microlens array on the blue light absorbing layer, so that the interface between the blue light absorbing layer and the microlens array is closely fitted, the adhesion strength between the blue light absorbing layer and the microlens array is improved, and the structural stability of the quantum dot fluorescent composite film is ensured. The direct construction method for the microlens array saves the steps of preparing the microlens array and then attaching the microlens array, which can better adapt to the formation of a large-area microlens array and improve the preparation efficiency of the quantum dot fluorescent composite film.
[0108] In this embodiment, a blue light absorbing solution is prepared on a quantum dot fluorescent layer with uneven film formation, and then a microlens array is constructed on the blue light absorbing layer to form a composite absorption layer. Through the combination of the composite absorption layer and the quantum dot fluorescent layer, the light output efficiency of the quantum dot fluorescent layer with uneven film formation can be improved, and the light output uniformity can be improved.
[0109] In the step of providing a quantum dot ink solution in S100, the steps of preparing the quantum dot ink solution specifically include:
[0110] The quantum dot material and the organic solvent are mixed evenly by magnetic stirring to prepare a quantum dot ink solution;
[0111] The quantum dot ink solution is coated on the substrate by a solution method, and the quantum dot ink solution is solidified to form a quantum dot fluorescent layer.
[0112] Among them, in the quantum dot ink solution, the weight fraction of quantum dot material is 15-25 parts, and the weight fraction of organic solvent is 75-85 parts. Specifically, in some embodiments, in the quantum dot ink solution, the weight fraction of quantum dot material is 25 parts, and the weight fraction of organic solvent is 75 parts. In some other embodiments, in the quantum dot ink solution, the weight fraction of quantum dot material is 15 parts, and the weight fraction of organic solvent is 85 parts. In the embodiment provided in the present application, in the quantum dot ink solution, the weight fraction of quantum dot material is 20 parts, and the weight fraction of organic solvent is 80 parts.
[0113] Among them, the solution method can be a spin coating method, a printing method, an inkjet printing method, a doctor blade method, a printing method, a dip-pull method, an immersion method, a spraying method, a roll coating method, a casting method, a slit coating method, a strip coating method, and the like.
[0114] In some embodiments, the quantum dot ink solution includes a quantum dot material and an organic solvent, wherein the quantum dot material includes one or more of silicon quantum dots, germanium quantum dots, sulfide quantum dots, selenide quantum dots, telluride quantum dots, phosphide quantum dots, arsenide quantum dots, and indium copper sulfide quantum dots.
[0115] In some embodiments, the quantum dot material may also include at least one of a single structure quantum dot and a core-shell structure quantum dot, wherein the material of the single structure quantum dot, the core material of the core-shell structure quantum dot and the shell material of the core-shell structure quantum dot are independently selected from at least one of II-VI group compounds, IV-VI group compounds, III-V group compounds and I-III-VI group compounds.
[0116] Wherein, the II-VI Group compound is selected from at least one of CdS, CdSe, CdTe, ZnS, ZnSe, ZnTe, ZnO, HgS, HgSe, HgTe, CdSeS, CdSeTe, CdSTe, ZnSeS, ZnSeTe, ZnSTe, HgSeS, HgSeTe, HgSTe, CdZnS, CdZnSe, CdZnTe, CdHgS, CdHgSe, CdHgTe, HgZnS, HgZnSe, HgZnTe, CdZnSeS, CdZnSeTe, CdZnSTe, CdHgSeS, CdHgSeTe, CdHgSTe, HgZnSeS, HgZnSeTe and HgZnSTe;
[0117] The IV-VI group compound is at least one selected from SnS, SnSe, SnTe, PbS, PbSe, PbTe, SnSeS, SnSeTe, SnSTe, PbSeS, PbSeTe, PbSTe, SnPbS, SnPbSe, SnPbTe, SnPbSSe, SnPbSeTe and SnPbSTe;
[0118] The III-V compound is selected from at least one of GaN, GaP, GaAs, GaSb, AlN, AlP, AlAs, AlSb, InN, InP, InAs, InSb, GaNP, GaNAs, GaNSb, GaPAs, GaPSb, AlNP, AlNAs, AlNSb, AlPAs, AlPSb, InNP, InNAs, InNSb, InPAs, InPSb, GaAlNP, GaAlNAs, GaAlNSb, GaAlPAs, GaAlPSb, GaInNP, GaInNAs, GaInNSb, GaInPAs, GaInPSb, InAlNP, InAlNAs, InAlNSb, InAlPAs or InAlPSb;
[0119] The I-III-VI group compound is selected from at least one of CuInS2, CuInSe2 and AgInS2.
[0120] The organic solvent includes one or more of an alkane solvent, an alcohol solvent, an aromatic solvent and a ketone solvent.
[0121] Among them, the alkane solvent can be at least one of hexane, octane, decane or alkanes with higher boiling points; the alcohol solvent can be hexylethanol; the aromatic solvent can be at least one of benzene, toluene, xylene or alkylbenzenes with higher boiling points; the ketone solvent can be a mixture of one or more of acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, N-methylpyrrolidone and tetrahydrofuran.
[0122] The surface of the quantum dot material is bound with a ligand, and the ligand includes one or more of an amino group, a thiol group, a carboxyl group, and a hydroxyl group; and / or the ligand includes at least one of an acid ligand, a thiol ligand, an amine ligand, an oxygen phosphine ligand, a phosphine ligand, a phospholipid, a soft phospholipid, and polyvinyl pyridine, etc.; wherein the acid ligand includes oleic acid, decanoic acid, undecyl acid, dodecyl acid, tridecyl acid, tetradecyl acid, hexadecyl acid, octadecyl acid, undecylenic acid, dodecylenic acid, tridecylenic acid, tetradecylenic acid, pentadecylenic acid, hexadecylenic acid, heptadecenic acid, and octadecylenic acid. The thiol ligands include at least one of n-butyl mercaptan, 1-pentanethiol, hexyl mercaptan, 1-decyl mercaptan, benzenethiol, benzyl mercaptan, octadecyl mercaptan, dodecyl mercaptan and octadecyl mercaptan; the amine ligands include at least one of oleylamine, n-octylamine, tributylamine, trihexylamine, triheptylamine, trioctylamine, trinonylamine, tridecylamine, nitroaniline and sulfonaniline; the phosphine oxide ligands include at least one of tributylphosphine, trihexylphosphine, triheptylphosphine, trioctylphosphine, trioctylphosphine oxide, trinonylphosphine and tridecylphosphine.
[0123] The prior art is to add diffusion powder to the quantum dot material and then print to form a fluorescent layer. However, since the nozzle of the printing equipment of the quantum dot ink is micron-level, the nozzle diameter is generally not higher than 2 microns, and the general diffusion powder particle size is 2-8μm, and the particle size distribution is generally normal distribution, it is difficult to achieve a uniform particle size. If the diffusion powder is directly added to the quantum dot ink, the printing nozzle will be blocked. In the preparation method of the present application, the quantum dot ink solution does not need to add diffusion powder, but the quantum dot material and the organic solvent are mixed to prepare the quantum dot ink solution, avoiding the risk of the nozzle being blocked.
[0124] In S200, before providing the blue light absorbing solution, the steps of preparing the blue light absorbing solution specifically include:
[0125] The curable high molecular polymer material is mixed with the blue light absorbing dye to obtain the blue light absorbing solution.
[0126] Wherein, the curable high molecular polymer material includes at least one of polyimide, epoxy resin, phenolic resin, urea-formaldehyde resin, melamine formaldehyde resin, furan resin, silicone resin, polyester resin, polyamide resin, acrylic resin, polyurethane, vinyl resin, hydrocarbon resin, and polyether resin. It should be noted that polyimide refers to a class of polymers containing an imide ring (-CO-NR-CO-) on the main chain. The derivatives of polyimide refer to other polymers containing an imide ring (-CO-NR-CO-) obtained by the reaction of polyimide.
[0127] In this embodiment, the curable high molecular polymer material is polyimide. After thermal curing, polyimide has excellent mechanical properties and rigidity, can effectively resist impact, and better protect the quantum dots in the quantum dot fluorescent layer. Polyimide has high radiation resistance and high temperature resistance. It is not easy to change color under the long-term irradiation and thermal action of the light emitted by the quantum dot fluorescent layer, and can maintain stable high transmittance. Using polyimide as the material of the blue light absorption layer, the blue light absorption layer has high transmittance, will not absorb the green light and red light emitted by the quantum dot fluorescent layer, will not affect the light color purity of the quantum dot fluorescent layer, and has better light emission effect compared with the blue light absorption layer prepared by other resin materials.
[0128] In some other embodiments, when the curable polymer material is selected from at least one of epoxy resin, phenolic resin, urea-formaldehyde resin, melamine formaldehyde resin, furan resin, silicone resin, polyester resin, polyamide resin, acrylic resin, polyurethane, vinyl resin, hydrocarbon resin, and polyether resin, an absorption layer curing agent is added to the curable polymer material. A commercially available product containing an absorption layer curing agent can be used, or the curable polymer material is mixed with the absorption layer curing agent, and the curable polymer to which the absorption layer curing agent is added is mixed with a blue light absorbing dye to obtain a blue light absorbing solution.
[0129] Among them, the absorption layer curing agent can be selected from at least one of polythiol curing agent, isocyanate curing agent, aliphatic polyamine curing agent, alicyclic polyamine curing agent, polyamide curing agent, modified aromatic amine curing agent, tertiary amine curing agent, imidazole curing agent, boron trifluoride complex curing agent, aromatic polyamine curing agent, anhydride curing agent, resol phenolic resin curing agent, amino resin curing agent, dicyandiamide curing agent, hydrazide curing agent, tetraethyl orthosilicate curing agent or other curing agents that can affect the resin curing reaction; the type and amount of the absorption layer curing agent can be determined according to the specific type of curable polymer material and the curing conditions, and the present application does not limit this.
[0130] The blue light absorbing dye is a yellow visible light dye absorbing wavelength of 430nm-500nm.
[0131] In some embodiments, the blue light absorbing dye may be selected from one or more of Epolight 5843, Epolight 5765, Epolight 5532, or Epolight 7276G from Epolin.
[0132] The blue light absorbing solution includes the following combination calculated by weight: 3-5 parts of blue light absorbing dye and 95-97 parts of curable high molecular polymer. Under this weight ratio, after the blue light absorbing solution is cured to form a blue light absorbing layer, the blue light absorption value can be controlled within an ideal range.
[0133] Specifically, in some embodiments, the blue light absorbing solution can be a mixture of 3 parts of blue light absorbing dye and 97 parts of curable high molecular polymer. In other embodiments, the blue light absorbing solution can be a mixture of 4 parts of blue light absorbing dye and 96 parts of curable high molecular polymer. In this embodiment, the blue light absorbing solution is a mixture of 5 parts of blue light absorbing dye and 95 parts of curable high molecular polymer.
[0134] In S200, the step of disposing the blue light absorbing solution on the quantum dot fluorescent layer to form a blue light absorbing layer specifically includes:
[0135] placing a blue light absorbing solution on the quantum dot fluorescent layer;
[0136] Performing a first heating cure on the blue light absorbing solution;
[0137] The blue light absorbing solution is heated and cured for a second time to obtain a blue light absorbing layer on the quantum dot fluorescent layer.
[0138] The first heating and curing temperature is 100-120°C and the heating and curing time is 20min-40min; and / or
[0139] The temperature of the second heating curing is 140°C-160°C, and the heating curing time is 50min-70min.
[0140] In the present embodiment, a first heating-curing and a second heating-curing are performed on the blue light absorbing solution respectively by adopting a stepwise heating-curing method. The temperature of the first heating-curing is lower than that of the second heating-curing, which serves as a pre-curing for the blue light absorbing solution. Under the pre-curing effect of the first heating-curing, the heating temperature is further increased, and a second heating-curing at a higher temperature is performed. This can shorten the time required for heating-curing, improve the preparation efficiency, and avoid deformation or breakage of the blue light absorbing layer due to being at high temperature for a long time during the curing process, thereby improving the yield of the blue light absorbing layer.
[0141] In some embodiments, the temperature of the first heating and curing can be set to 100°C, and the curing time at this temperature is 40 minutes; or the temperature of the first heating and curing can be set to 120°C, and the curing time at this temperature is 20 minutes. In the embodiment provided in the present application, the temperature of the first heating and curing is 110°C, and the curing time is 30 minutes.
[0142] In some embodiments, the temperature of the second heating and curing can be set to 140°C, and the curing time at this temperature is 70 minutes; or the temperature of the second heating and curing can be set to 160°C, and the curing time at this temperature is 40 minutes. In the embodiment provided in the present application, the temperature of the second heating and curing is 150°C, and the curing time is 60 minutes.
[0143] Specifically, a solution method may be used to place a blue light absorbing solution on the quantum dot fluorescent layer.
[0144] like Figure 4 As shown, S300, the step of preparing a microlens array on the blue light absorbing layer specifically includes:
[0145] S310, providing a grid template, wherein at least one side of the grid template is provided with a grid structure;
[0146] S320, disposing a lens material on the blue light absorbing layer;
[0147] S330, attaching the side of the grid template with the grid structure to the lens material, so that the lens material fills the grid structure of the grid template;
[0148] S340, curing the lens material on the blue light absorbing layer, peeling off the grid template, and forming a microlens array.
[0149] Among them, Figure 5 As shown, in S310, before providing the grid template, the method for preparing the grid template specifically includes:
[0150] S311. Provide a shaping base plate and a motherboard with a grating structure, and attach the shaping surface of the shaping base plate to the motherboard.
[0151] S312, separating the shaping base plate and the mother plate after the first printing and pressing, so as to form a first grating structure on the shaping base plate and obtain a first template.
[0152] S313, rotate the first template so that the first grating structure on the first template is perpendicular to the grating structure on the motherboard, attach the side with the first grating structure to the motherboard again, perform a second embossing on the first template and the motherboard, separate and shape them to form a grid structure on the first template, and obtain a grid template.
[0153] Specifically, the first template may be rotated 90° or 270° to make the first grating structure on the first template perpendicular to the grating structure on the motherboard, thereby forming mutually perpendicular grating structures on the first template after the second embossing.
[0154] In this embodiment, each grid on the grid template is a centrally symmetrical pattern. Each lens on the microlens array formed by the grid template is centrally symmetrical, which can make the light emission effect of the quantum dot light-emitting device more uniform and improve the light emission efficiency.
[0155] Specifically, the shaping base plate is a polymer template, which can be polymerized from one of polymethyl methacrylate, polystyrene, and polycarbonate. The shaping base plate has at least one shaping surface, which is covered with a protective film before use. The protective film needs to be torn off before use, and then the side without the protective film is attached to the motherboard.
[0156] In some implementation modes, the above step S312 specifically includes:
[0157] Place the shaping base plate together with the mother plate in the center of the stage of the imprint instrument, and cover the shaping base plate with a protective sheet to perform the first imprinting and molding, so that the shaping base plate completely replicates the grating structure of the mother plate, and then demold the shaping base plate that is tightly attached to the mother plate, thereby forming the first grating structure on the shaping base plate and obtaining the first template.
[0158] The above step S313 specifically includes:
[0159] After rotating the first template obtained in step S312 by 90°, the side with the first grating structure is re-attached to the motherboard, and a protective sheet is covered on the top of the first template. After the stage is sent to the top of the lifting platform, the hatch is lowered to start the program for the second imprinting. After the imprinting is completed, the mold is demolded to obtain the second grating structure on the first template, thereby forming a grid structure and obtaining a grid template.
[0160] The motherboard is a silicon motherboard with a nano-sized grating structure. The protective sheet is a composite light-curing material sheet (UV sheet), a kind of ultra-high strength anti-corrosion, fire-proof and insulating protective layer. The protective sheet can protect the shaping base plate during embossing and prevent damage to the shaping base plate caused by uneven pressure during embossing.
[0161] Specifically, the lenses on the microlens array are nanometer-sized. After the shaping base plate is embossed twice horizontally and vertically by a silicon mother plate with a nanometer-sized grating structure, a grid structure is formed on the shaping surface of the shaping base plate. After solidification, a grid template with a nanometer-sized grid is formed. Through the grid template, a microlens array composed of nanometer-sized microlenses can be constructed.
[0162] The present application prepares a grid template with a nano-grid structure to realize the construction of a nano-sized microlens array, making the size of the microlens array smaller. On the one hand, it reduces the thickness of the microlens array to the quantum dot fluorescent composite film, and on the other hand, it allows more microlenses to be on a pixel point, thereby improving the luminous uniformity of the quantum dot fluorescent composite film and further improving the light output effect of the device.
[0163] It should be noted that the preparation of the grid template can be completed before preparing the quantum dot fluorescent composite film, or can be carried out at the same time as the first preparation of the quantum dot fluorescent composite film.
[0164] The grid template prepared by the present application can be used repeatedly in the subsequent large-scale preparation process of quantum dot fluorescent composite films, saving production costs and improving preparation efficiency, and can also adapt to the preparation of larger-sized quantum dot fluorescent composite films.
[0165] In the above step S340, the lens material is cured on the blue light absorbing layer by heating.
[0166] The lens material includes at least one of polydimethylsiloxane solution, polymethyl methacrylate, polystyrene, polycarbonate and photoresist.
[0167] In this embodiment, the polydimethylsiloxane solution includes polydimethylsiloxane and a curing agent, wherein the polydimethylsiloxane (PDMS) is in liquid state; and the curing agent can be selected from at least one of an isocyanate curing agent, a diamine curing agent, a triamine curing agent or a tetraamine curing agent.
[0168] In some embodiments, the curing agent is selected from at least one of an isocyanate curing agent, a diamine curing agent, a triamine curing agent or a tetramine curing agent, the isocyanate curing agent is selected from at least one of HDI isocyanate, TDI isocyanate or IPDI isocyanate, the diamine curing agent is selected from at least one of hydroxyethylethylenediamine or 1,3-propylenediamine, the triamine curing agent is selected from at least one of diethylenetriamine, triethylamine or triethanolamine, and the tetraamine curing agent is selected from triethylenetetramine.
[0169] In some embodiments, the mass ratio of polydimethylsiloxane to the curing agent is (8-10):(1-2). Specifically, the mass ratio of polydimethylsiloxane to the curing agent is 10:1.
[0170] In some embodiments, the polydimethylsiloxane and the curing agent are commercially available kit products. Specifically, the polydimethylsiloxane and the curing agent can be selected from SYLGARD 184PDMS products. This application is not limited to this.
[0171] In some embodiments, the polydimethylsiloxane solution is obtained by the following preparation method. Specifically, the steps of the preparation method include:
[0172] Polydimethylsiloxane (PDMS) and a PDMS curing agent are uniformly mixed according to a mass ratio to obtain a polydimethylsiloxane solution.
[0173] It can be understood that the present embodiment uses a polydimethylsiloxane solution to directly construct a microlens array on the blue light absorbing layer, so that the polydimethylsiloxane on the microlens array can form a tight and stable bonding surface at the contact interface of the polyimide on the blue light absorbing layer, thereby improving the bonding strength between the microlens array and the blue light absorbing layer without the need to add other adhesives, thereby saving preparation steps, the required preparation time and material costs.
[0174] In this embodiment, in step S340, the temperature condition for heating and curing the polydimethylsiloxane is 35-45° C., and the time for heating and curing the polydimethylsiloxane is 2-4 hours.
[0175] Specifically, the temperature condition for heating and curing the polydimethylsiloxane can be set to 35° C., 36° C., 37° C., 38° C., 39° C., 40° C., 41° C., 42° C., 43° C., 44° C. or 45° C. The time for heating and curing the polydimethylsiloxane can be set to 2 h, 2.5 h, 3 h or 4 h.
[0176] The present invention will be further described below in conjunction with specific embodiments:
[0177] Embodiment 1:
[0178] This embodiment provides a quantum dot fluorescent composite film, and the preparation method thereof is as follows:
[0179] (1) 20 parts of CdZnSe / ZnS quantum dot material and 80 parts of hexyl ethanol are stirred by strong magnetic force to prepare a quantum dot ink solution;
[0180] (2) On a substrate with a plurality of blue light sources, a quantum dot ink solution is printed onto pixel points of the substrate, and cured at 130° C. for 30 min to obtain a quantum dot fluorescent layer, wherein the quantum dot fluorescent layer has a thickness of 7 μm;
[0181] (3) 95 parts of polyimide and 5 parts of yellow visible light dye (Epolight 5532, maximum absorption wavelength 500 nm) were mixed evenly by strong magnetic stirring to prepare a blue light absorbing solution. The blue light absorbing solution was printed on the quantum dot fluorescent layer, and then cured at 110° C. for 30 min and then at 150° C. for 60 min to obtain a blue light absorbing layer, wherein the thickness of the blue light absorbing layer was 2.5 μm;
[0182] (4) Provide a nano-mesh template, mix polydimethylsiloxane and curing agent (diethylenetriamine) at a mass ratio of 10:1, and stir evenly to obtain a polydimethylsiloxane solution. Put the polydimethylsiloxane solution into a vacuum drying oven and evacuate it to completely expel the bubbles in the solution before taking it out. Print the polydimethylsiloxane solution on the blue light absorption layer, attach the nano-mesh side of the nano-mesh template to the polydimethylsiloxane solution printed on the blue light absorption layer, and in a vacuum drying environment, allow the polydimethylsiloxane solution to completely fill the nano-mesh. Heat at 35°C for 4 hours to completely cure the polydimethylsiloxane solution, peel off the nano-mesh template, and form a composite absorption layer with the blue light absorption layer and the microlens array to obtain a quantum dot fluorescent composite film.
[0183] Example 2
[0184] This embodiment provides a quantum dot fluorescent composite film, and the preparation method thereof is as follows:
[0185] (1) 20 parts of CdZnSe / ZnS quantum dot material and 80 parts of hexyl ethanol are stirred by strong magnetic force to prepare a quantum dot ink solution;
[0186] (2) On a substrate with a plurality of blue light sources, a quantum dot ink solution is printed onto pixel points of the substrate, and cured at 130° C. for 30 min to obtain a quantum dot fluorescent layer, wherein the quantum dot fluorescent layer has a thickness of 7 μm;
[0187] (3) 97 parts of polyimide and 3 parts of yellow visible light dye (Epolight 5532, maximum absorption wavelength 500 nm) were mixed evenly by strong magnetic stirring to prepare a blue light absorbing solution. The blue light absorbing solution was printed on the quantum dot fluorescent layer, and cured at 110° C. for 30 min and at 150° C. for 60 min to obtain a blue light absorbing layer, wherein the thickness of the blue absorbing layer was 2.5 μm;
[0188] (4) Provide a nano-mesh template, mix polydimethylsiloxane and curing agent (diethylenetriamine) in a mass ratio of 10:1, and stir evenly to obtain a polydimethylsiloxane solution. Put the polydimethylsiloxane solution into a vacuum drying oven and evacuate it to completely expel the bubbles in the solution before taking it out. Print the polydimethylsiloxane solution on the blue light absorption layer, and attach the nano-mesh side of the nano-mesh template to the polydimethylsiloxane solution printed on the blue light absorption layer. Under a vacuum drying environment, the polydimethylsiloxane solution is completely filled with the nano-mesh. Heat at 40°C for 3 hours to completely cure the polydimethylsiloxane solution, peel off the nano-mesh template, and allow the blue light absorption layer and the microlens array to adhere to form a composite absorption layer to obtain a quantum dot fluorescent composite film.
[0189] Example 3
[0190] This embodiment provides a quantum dot fluorescent composite film, and the preparation method thereof is as follows:
[0191] (1) 20 parts of CdZnSe / ZnS quantum dot material and 80 parts of hexyl ethanol are stirred by strong magnetic force to prepare a quantum dot ink solution;
[0192] (2) On a substrate with a plurality of blue light sources, a quantum dot ink solution is printed onto pixel points of the substrate, and cured at 130° C. for 30 min to obtain a quantum dot fluorescent layer, wherein the quantum dot fluorescent layer has a thickness of 7 μm;
[0193] (3) 95 parts of epoxy resin (containing benzophenone tetracarboxylic dianhydride curing agent) and 5 parts of yellow visible light dye (Epolight 5765, maximum absorption wavelength 488nm) were mixed evenly by strong magnetic stirring to prepare a blue light absorbing liquid. The blue light absorbing liquid was printed on the quantum dot fluorescent layer, cured at 100°C for 20 minutes and at 130°C for 60 minutes to obtain a blue light absorbing layer, wherein the thickness of the blue light absorbing layer was 2.7 μm;
[0194] (4) Provide a nano-mesh template, mix polydimethylsiloxane and curing agent (diethylenetriamine) in a mass ratio of 10:1, and stir evenly to obtain a polydimethylsiloxane solution. Put the polydimethylsiloxane solution into a vacuum drying oven and evacuate it to completely expel the bubbles in the solution before taking it out. Print the polydimethylsiloxane solution on the blue light absorption layer, attach the nano-mesh side of the nano-mesh template to the polydimethylsiloxane solution printed on the blue light absorption layer, and in a vacuum drying environment, allow the polydimethylsiloxane solution to completely fill the nano-mesh. Heat at 35°C for 4 hours to completely cure the polydimethylsiloxane solution, peel off the nano-mesh template, and form a composite absorption layer by adhering the blue light absorption layer and the microlens array to obtain a quantum dot fluorescent composite film.
[0195] Example 4
[0196] This embodiment provides a quantum dot fluorescent composite film, and the preparation method thereof is as follows:
[0197] (1) 20 parts of CdZnSe / ZnS quantum dot material and 80 parts of hexyl ethanol are stirred by strong magnetic force to prepare a quantum dot ink solution;
[0198] (2) On a substrate with a plurality of blue light sources, a quantum dot ink solution is printed onto pixel points of the substrate, and cured at 130° C. for 30 min to obtain a quantum dot fluorescent layer, wherein the quantum dot fluorescent layer has a thickness of 7 μm;
[0199] (3) 95 parts of acrylic resin (containing isocyanate curing agent) and 5 parts of yellow visible light dye (Epolight7276G, maximum absorption wavelength 450nm, transmittance>500nm) were mixed evenly by strong magnetic stirring to prepare a blue light absorbing liquid. The blue light absorbing liquid was printed on the quantum dot fluorescent layer and cured at 130°C for 60 minutes to obtain a blue light absorbing layer, wherein the thickness of the blue light absorbing layer was 2.5 μm;
[0200] (4) Provide a nano-mesh template, mix polydimethylsiloxane and curing agent (diethylenetriamine) at a mass ratio of 10:1, and stir evenly to obtain a polydimethylsiloxane solution. Put the polydimethylsiloxane solution into a vacuum drying oven and evacuate it to completely expel the bubbles in the solution before taking it out. Print the polydimethylsiloxane solution on the blue light absorption layer, attach the nano-mesh side of the nano-mesh template to the polydimethylsiloxane solution printed on the blue light absorption layer, and in a vacuum drying environment, allow the polydimethylsiloxane solution to completely fill the nano-mesh. Heat at 35°C for 4 hours to completely cure the polydimethylsiloxane solution, peel off the nano-mesh template, and allow the blue light absorption layer and the microlens array to adhere to form a composite absorption layer to obtain a quantum dot fluorescent composite film.
[0201] Example 5
[0202] This embodiment provides a quantum dot fluorescent composite film, and the preparation method thereof is as follows:
[0203] (1) 20 parts of CdZnSe / ZnS quantum dot material and 80 parts of hexyl ethanol are stirred by strong magnetic force to prepare a quantum dot ink solution;
[0204] (2) On a substrate with a plurality of blue light sources, a quantum dot ink solution is printed onto pixel points of the substrate, and cured at 130° C. for 30 min to obtain a quantum dot fluorescent layer, wherein the quantum dot fluorescent layer has a thickness of 7 μm;
[0205] (3) 95 parts of silicone resin (containing ethyl orthosilicate curing agent) and 5 parts of yellow visible light dye (Epolight 5843, maximum absorption wavelength 480nm) were mixed evenly by strong magnetic stirring to prepare a blue light absorbing liquid. The blue light absorbing liquid was printed on the quantum dot fluorescent layer and cured at 150°C for 80 minutes to obtain a blue light absorbing layer, wherein the thickness of the blue light absorbing layer was 2.6 μm.
[0206] (4) Provide a nano-mesh template, mix polydimethylsiloxane and curing agent (diethylenetriamine) at a mass ratio of 10:1, and stir evenly to obtain a polydimethylsiloxane solution. Put the polydimethylsiloxane solution into a vacuum drying oven and evacuate it to completely expel the bubbles in the solution before taking it out. Print the polydimethylsiloxane solution on the blue light absorption layer, attach the nano-mesh side of the nano-mesh template to the polydimethylsiloxane solution printed on the blue light absorption layer, and in a vacuum drying environment, allow the polydimethylsiloxane solution to completely fill the nano-mesh. Heat at 35°C for 4 hours to completely cure the polydimethylsiloxane solution, peel off the nano-mesh template, and allow the blue light absorption layer and the microlens array to adhere to form a composite absorption layer to obtain a quantum dot fluorescent composite film.
[0207] Comparative Example 1:
[0208] This comparative example provides a quantum dot fluorescent composite film, which is different from Example 1 in that: the quantum dot fluorescent composite film of this comparative example is not provided with a microlens array layer, and its preparation method is as follows:
[0209] (1) 20 parts of CdZnSe / ZnS quantum dot material and 80 parts of hexyl ethanol are stirred by strong magnetic force to prepare a quantum dot ink solution;
[0210] (2) On a substrate with a plurality of blue light sources, a quantum dot ink solution is printed onto pixel points of the substrate, and cured at 130° C. for 30 min to obtain a quantum dot fluorescent layer, wherein the quantum dot fluorescent layer has a thickness of 7 μm;
[0211] (3) 95 parts of polyimide and 5 parts of yellow visible light dye (Epolight 5532, maximum absorption wavelength 500 nm) were mixed evenly by strong magnetic stirring to prepare a blue light absorbing solution. The blue light absorbing solution was printed on the quantum dot fluorescent layer, and cured at 110° C. for 30 min and at 150° C. for 60 min to obtain a blue light absorbing layer, wherein the thickness of the blue absorbing layer was 2.5 μm, and a quantum dot fluorescent composite film without a microlens array layer was obtained.
[0212] Comparative Example 2:
[0213] This comparative example provides a quantum dot fluorescent layer, which is different from Example 1 in that: the quantum dot fluorescent layer of this comparative example is not provided with a composite absorption layer, and its preparation method is as follows:
[0214] (1) 20 parts of CdZnSe / ZnS quantum dot material and 80 parts of hexyl ethanol are stirred by strong magnetic force to prepare a quantum dot ink solution;
[0215] (2) On a substrate with a plurality of blue light sources, a quantum dot ink solution was printed onto pixel points of the substrate, and the solution was cured at 130° C. for 30 min to obtain a quantum dot fluorescent layer, wherein the thickness of the quantum dot fluorescent layer was 7 μm.
[0216] Functional testing:
[0217] The above-mentioned Examples 1 to 5, Comparative Example 1 and Comparative Example 2 were subjected to various performance tests, and the specific test methods are as follows:
[0218] Test 1: The absorption of 450nm blue light by the quantum dot fluorescent composite film of Example 1, the quantum dot fluorescent layer composite film without a microlens array of Comparative Example 1, and the quantum dot fluorescent layer of Comparative Example 2 was tested using an ultraviolet spectrophotometer.
[0219] Test 2: The wavelength, half-peak width and external quantum efficiency of the quantum dot fluorescent composite films of Examples 1 to 5, the quantum dot fluorescent composite film of Comparative Example 1 (without a microlens array), and the quantum dot fluorescent layer of Comparative Example 2 were tested using an integrating sphere method.
[0220] The results of test 1 and test 2 are shown in Table 1:
[0221] Table 1
[0222]
[0223] It should be noted that in Table 1, the difference between the half-width data of Examples 1 to 5, Comparative Example 1 and Comparative Example 2 is a natural error. The natural error is a normal phenomenon caused by the different order of detecting samples when the same detection equipment detects multiple samples. Those skilled in the art should not regard the natural error as the main comparison basis for judging the difference in actual light output effects between Examples 1 to 5, Comparative Example 1 and Comparative Example 2.
[0224] It can be seen from Table 1 that the quantum dot fluorescent composite film prepared in Examples 1 to 5 has a blue light absorption value (OD@450nm) greater than 2 under the condition that the total thickness does not exceed 10 μm, indicating that the quantum dot fluorescent composite film can have a higher blue light absorption ability while being thinner.
[0225] It can be seen from Table 1 that when the thickness of the quantum dot fluorescent layer is the same, Example 1 has a higher blue light absorption value than Comparative Example 2. When the thickness of the quantum dot fluorescent composite film of Example 1 does not exceed 10 μm, it can also meet the requirement of a blue light absorption value (OD@450nm) higher than 2.
[0226] Compared with Example 1 and Comparative Example 1, the quantum dot fluorescent composite film of Example 1 has a higher external quantum efficiency, which means that the luminous efficiency of Example 1 is higher and the luminescence is more uniform.
[0227] Test 3: The fluorescence spectra of the quantum dot fluorescent composite film of Example 1 and the quantum dot fluorescent layer of Comparative Example 2 were tested using a color brightness meter. The test results are as follows: Figure 6 As shown, the quantum dot fluorescent composite film of Example 1 has no blue light emission peak at 460nm, indicating that the blue light is basically absorbed by the quantum dots and converted into green light at 535nm. The quantum dot fluorescent layer of Comparative Example 2 has a blue emission peak at 460nm, indicating that part of the blue light is not absorbed by the quantum dots and is mixed with the green light emitted by the quantum dots, and the peak value at 535nm is lower than that of Example 1, indicating that the green light emission intensity at 535nm is weaker than that of Example 1. It can be seen that Example 1 adopts the preparation method of the quantum dot fluorescent composite film provided by the present application, and the prepared quantum dot fluorescent composite film can effectively improve the blue light absorption value, make the light color purity higher, and also have higher luminous efficiency.
[0228] Based on the quantum dot fluorescent composite film provided in the above embodiments, the embodiments of the present application also provide a light-emitting device, which includes a substrate and a quantum dot fluorescent composite film provided in any of the above embodiments or a quantum dot fluorescent composite film prepared by the preparation method provided in any of the above embodiments, a blue light-emitting unit is provided on the substrate, and the quantum dot fluorescent composite film is arranged on the blue light-emitting unit.
[0229] Specifically, the quantum dot fluorescent composite film is arranged on the light-emitting side of the blue light-emitting unit and completely covers the blue light-emitting unit, thereby ensuring that the quantum dot fluorescent composite film has a high blue light utilization rate and blue light absorption rate.
[0230] The embodiment of the present application further provides a display, which includes the light-emitting device provided in the above embodiment.
[0231] The display uses a light-emitting device composed of the quantum dot fluorescent composite film provided by the present application, so that the resulting display can have better light output efficiency and blue light absorption value, and the light output color is good. The microlens array can improve the uniformity of the light output, which can bring a better visual experience to the user, and can have lower power consumption, longer service life and durability.
[0232] Obviously, the embodiments described above are only some embodiments of the present application, rather than all embodiments. The preferred embodiments of the present application are given in the accompanying drawings, but they do not limit the patent scope of the present application. The present application can be implemented in many different forms. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present application more thorough and comprehensive. Although the present application is described in detail with reference to the aforementioned embodiments, for those skilled in the art, it is still possible to modify the technical solutions recorded in the aforementioned specific implementation methods, or to perform equivalent replacement of some of the technical features therein. Any equivalent structure made using the contents of the specification and drawings of this application, directly or indirectly used in other related technical fields, is similarly within the scope of patent protection of this application.
Claims
1. A quantum dot fluorescent composite film, characterized in that: include A quantum dot fluorescent layer and a composite absorption layer are sequentially arranged from bottom to top on the substrate; The composite absorption layer comprises a blue light absorption layer and a microlens array layer, and the blue light absorption layer is located between the quantum dot fluorescent layer and the microlens array layer.
2. The quantum dot fluorescent composite film according to claim 1, characterized in that: The material of the blue light absorbing layer includes a curable high molecular polymer and a blue light absorbing dye.
3. The quantum dot fluorescent composite film according to claim 2, characterized in that: The material of the blue light absorbing layer comprises the following combination calculated by weight: 3-5 parts of the blue light absorbing dye and 95-97 parts of the curable high molecular polymer; and / or The curable high molecular polymer material includes at least one of polyimide, epoxy resin, phenolic resin, urea-formaldehyde resin, melamine-formaldehyde resin, furan resin, silicone resin, polyester resin, polyamide resin, acrylic resin, polyurethane, vinyl resin, hydrocarbon resin or polyether resin; and / or The blue light absorbing dye has an absorbable wavelength of 430nm-500nm; and / or The blue light absorbing dye has an absorbable peak wavelength of 455nm-465nm; and / or The blue light absorbing dye is at least one of Epolight 5843, Epolight 5765, Epolight 5532 or Epolight7276G.
4. The quantum dot fluorescent composite film according to claim 1, characterized in that: The material of the microlens array layer includes at least one of polydimethylsiloxane, polymethyl methacrylate, polystyrene, polycarbonate or photoresist.
5. The quantum dot fluorescent composite film according to claim 1, characterized in that: The microlenses on the microlens array layer are convex lenses, and the convex lens array is arranged on the blue light absorbing layer.
6. The quantum dot fluorescent composite film according to claim 1, characterized in that: The thickness of the quantum dot fluorescent composite film is 1-10 μm.
7. The quantum dot fluorescent composite film according to claim 6, characterized in that: The thickness of the quantum dot fluorescent layer is 6-9.8 μm, and the thickness of the blue light absorbing layer is 0.1-3.9 μm.
8. A method for preparing a quantum dot fluorescent composite film, characterized in that: include: Providing a quantum dot ink solution, and placing the quantum dot ink solution on a substrate to form a quantum dot fluorescent layer; Providing a blue light absorbing solution, and disposing the blue light absorbing solution on the quantum dot fluorescent layer to form a blue light absorbing layer; A microlens array is prepared on the blue light absorbing layer, and the blue light absorbing layer and the microlens array form a composite absorbing layer to obtain a quantum dot fluorescent composite film.
9. The method for preparing a quantum dot fluorescent composite film according to claim 8, characterized in that: The step of preparing a microlens array on the blue light absorbing layer specifically includes: Providing a grid template, wherein at least one side of the grid template is provided with a grid structure; Disposing a lens material on the blue light absorbing layer; Attaching the grid template with the grid structure on the lens material so that the lens material fills the grid structure; The lens material is solidified on the blue light absorbing layer, and the grid template is peeled off to form a microlens array.
10. The method for preparing a quantum dot fluorescent composite film according to claim 9, characterized in that: In the step of curing the lens material on the blue light absorbing layer, the lens material comprises at least one of polydimethylsiloxane solution, polymethyl methacrylate, polystyrene, polycarbonate and photoresist; and / or The curing temperature is 35-45° C., and the curing time is 2-4 hours.
11. The method for preparing a quantum dot fluorescent composite film according to claim 10, characterized in that: The polydimethylsiloxane solution comprises polydimethylsiloxane and a curing agent; The curing agent is selected from at least one of an isocyanate curing agent, a diamine curing agent, a triamine curing agent or a tetraamine curing agent, Wherein, the isocyanate curing agent is selected from at least one of HDI isocyanate, TDI isocyanate or IPDI isocyanate, the diamine curing agent is selected from at least one of hydroxyethylethylenediamine or 1,3-propylenediamine, the triamine curing agent is selected from at least one of diethylenetriamine, triethylamine or triethanolamine, and the tetraamine curing agent is selected from triethylenetetramine; and / or The mass ratio of the polydimethylsiloxane to the curing agent is (8-10):(1-2).
12. The method for preparing a quantum dot fluorescent composite film according to claim 8, characterized in that: The preparation steps of the blue light absorbing solution include: Mixing a curable high molecular polymer material with a blue light absorbing dye to obtain the blue light absorbing solution; The blue light absorbing solution comprises the following combination calculated by weight: 3-5 parts of the blue light absorbing dye and 95-97 parts of the curable high molecular polymer; and / or The curable high molecular polymer material includes at least one of polyimide, epoxy resin, phenolic resin, urea-formaldehyde resin, melamine formaldehyde resin, furan resin, silicone resin, polyester resin, polyamide resin, acrylic resin, polyurethane, vinyl resin, hydrocarbon resin, and polyether resin; and / or The blue light absorbing dye has an absorbable wavelength of 430nm-500nm; and / or The blue light absorbing dye has an absorbable peak wavelength of 455nm-465nm; and / or The blue light absorbing dye is at least one of Epolight 5843, Epolight 5765, Epolight 5532 or Epolight7276G.
13. The method for preparing a quantum dot fluorescent composite film according to claim 8, characterized in that: The step of disposing the blue light absorbing solution on the quantum dot fluorescent layer to form a blue light absorbing layer specifically includes: Disposing the blue light absorbing solution on the quantum dot fluorescent layer; Performing a first heating curing on the blue light absorbing solution; Performing a second heating and curing on the blue light absorbing solution to obtain the blue light absorbing layer on the quantum dot fluorescent layer; Wherein, the temperature of the first heating and curing is 100-120°C, and the heating and curing time is 20min-40min; and / or The temperature of the second heating and curing is 140° C.-160° C., and the time of heating and curing is 50 min-70 min.
14. The method for preparing a quantum dot fluorescent composite film according to claim 8, characterized in that: The quantum dot ink solution comprises quantum dot material and an organic solvent; The quantum dot material includes at least one of a single structure quantum dot and a core-shell structure quantum dot, and the material of the single structure quantum dot, the core material of the core-shell structure quantum dot and the shell material of the core-shell structure quantum dot are independently selected from at least one of a II-VI group compound, a IV-VI group compound, a III-V group compound and a I-III-VI group compound; Wherein, the II-VI Group compound is selected from at least one of CdS, CdSe, CdTe, ZnS, ZnSe, ZnTe, ZnO, HgS, HgSe, HgTe, CdSeS, CdSeTe, CdSTe, ZnSeS, ZnSeTe, ZnSTe, HgSeS, HgSeTe, HgSTe, CdZnS, CdZnSe, CdZnTe, CdHgS, CdHgSe, CdHgTe, HgZnS, HgZnSe, HgZnTe, CdZnSeS, CdZnSeTe, CdZnSTe, CdHgSeS, CdHgSeTe, CdHgSTe, HgZnSeS, HgZnSeTe and HgZnSTe; The IV-VI group compound is selected from at least one of SnS, SnSe, SnTe, PbS, PbSe, PbTe, SnSeS, SnSeTe, SnSTe, PbSeS, PbSeTe, PbSTe, SnPbS, SnPbSe, SnPbTe, SnPbSSe, SnPbSeTe and SnPbSTe; The III-V group compound is selected from at least one of GaN, GaP, GaAs, GaSb, AlN, AlP, AlAs, AlSb, InN, InP, InAs, InSb, GaNP, GaNAs, GaNSb, GaPAs, GaPSb, AlNP, AlNAs, AlNSb, AlPAs, AlPSb, InNP, InNAs, InNSb, InPAs, InPSb, GaAlNP, GaAlNAs, GaAlNSb, GaAlPAs, GaAlPSb, GaInNP, GaInNAs, GaInNSb, GaInPAs, GaInPSb, InAlNP, InAlNAs, InAlNSb, InAlPAs or InAlPSb; The I-III-VI group compound is selected from at least one of CuInS2, CuInSe2 and AgInS2; and / or The organic solvent includes one or more of an alkane solvent, an alcohol solvent, an aromatic solvent and a ketone solvent; Wherein, the alkane solvent is at least one of hexane, octane, decane and alkane; the alcohol solvent is hexylethanol; the aromatic solvent is at least one of benzene, toluene, xylene and alkylbenzene; the ketone solvent is at least one of acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, N-methylpyrrolidone and tetrahydrofuran; and / or The quantum dot material surface is bound with a ligand, wherein the ligand comprises at least one of an acid ligand, a thiol ligand, an amine ligand and an oxide phosphine ligand; wherein the acid ligand comprises at least one of oleic acid, decanoic acid, undecyl acid, dodecyl acid, tridecyl acid, tetradecyl acid, hexadecyl acid, octadecyl acid, undecylenic acid, dodecylenic acid, tridecylenic acid, tetradecylenic acid, pentadecylenic acid, hexadecylenic acid, heptadecenic acid and octadecylenic acid; The thiol ligand comprises at least one of n-butyl mercaptan, 1-pentanethiol, hexyl mercaptan, 1-decyl mercaptan, benzene mercaptan, benzyl mercaptan, octadecyl mercaptan, dodecyl mercaptan and octadecyl mercaptan; The amine ligand comprises at least one of oleylamine, n-octylamine, tributylamine, trihexylamine, triheptylamine, trioctylamine, trinonylamine, tridecylamine, nitroaniline and sulfonaniline; The phosphine oxide ligand includes at least one of tributylphosphine, trihexylphosphine, triheptylphosphine, trioctylphosphine, trioctylphosphine oxide, trinonylphosphine and tridecylphosphine.
15. A light emitting device, characterized in that: It comprises a substrate and a quantum dot fluorescent composite film as described in any one of claims 1 to 7 or a quantum dot fluorescent composite film prepared by the preparation method as described in any one of claims 8 to 14, wherein a blue light-emitting unit is provided on the substrate, and the quantum dot fluorescent composite film is arranged on the blue light-emitting unit.
16. A display, characterized in that: Comprising the light emitting device as claimed in claim 15.