Optical fiber rod and method for manufacturing optical fiber ribbon
By adjusting the Young's modulus and extraction force of the main layer of the fiber optic wire, the peeling and cracking of the bare wire and the main layer during the manufacturing process are avoided, and the gap generated by heating is repaired, which solves the problem of increased transmission loss of the fiber optic wire. It realizes efficient manufacturing of optical fiber wires and optical fiber tapes.
Patent Information
- Application Number
- CN202380032761.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-27
- Filing Date
- 2023-04-19
- Publication Date
- 2024-11-22
AI Technical Summary
During the manufacturing process of fiber optic wire, the pressure applied in the radial direction may cause peeling, gaps or cracking between the bare wire and the main layer, increasing the transmission loss of the fiber optic wire and the fiber tape.
By designing the main layer of the optical fiber wire material, it has a Young's modulus of 0.10 to 0.45MPa and a pull-out force of 0.6 to 1.2N/mm, it is ensured that there is no peeling or cracking between the bare wire part and the main layer under point load, only A void that can be eliminated by heating is generated in the main layer.
It effectively suppresses the increase in transmission loss of optical fiber wires and optical fiber tapes, ensuring the performance stability and transmission efficiency of optical fiber wires.
Smart Images

Figure CN119013240A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for manufacturing an optical fiber wire and an optical fiber ribbon.
[0002] This application claims priority based on U.S. patent application No. 63 / 335,224 filed in the United States on April 27, 2022, and its contents are incorporated herein. Background Art
[0003] Conventionally, there is known an optical fiber wire as disclosed in Japanese Patent Application Laid-Open No. 2005-189390, which includes a bare fiber portion having a core and a cladding, a main layer covering the bare fiber portion, and a sub-layer covering the main layer.
[0004] When manufacturing optical fiber wires, or when using optical fiber wires to manufacture optical fiber ribbons and optical fiber cables, there is a situation where radial pressure (lateral pressure) is applied to the optical fiber wires. For example, when the spun optical fiber wires are wound up on a bobbin, the optical fiber wires are sandwiched between the extraction belt and the capstan, or the optical fiber wires overlap each other. Therefore, a compressive force is applied to the optical fiber wires. When the above-mentioned pressure is applied to the optical fiber wires, there is a possibility that the bare wire portion is peeled off from the main layer, or that gaps or cracks are generated in the main layer. The generation of such peeling, gaps or cracks in the optical fiber wires sometimes leads to an increase in the transmission loss of the optical fiber wires and the optical fiber ribbons and optical fiber cables using the optical fiber wires.
[0005] As a result of in-depth research by the inventors of the present application, it is known that when a void is generated in the main layer, the void disappears by heating the optical fiber wire. In other words, the inventors of the present application have found that even if a void is generated in the optical fiber wire, the increase in the transmission loss of the optical fiber wire can be suppressed by heating the optical fiber wire. On the other hand, as a result of in-depth research by the inventors of the present application, it is known that when peeling occurs between the bare wire portion and the main layer, it is difficult to eliminate the peeling even if the optical fiber wire is heated. Summary of the invention
[0006] The present invention has been made in consideration of such a situation, and an object of the present invention is to provide a method for manufacturing an optical fiber wire and an optical fiber ribbon in which the transmission loss is unlikely to increase.
[0007] In order to solve the above-mentioned problems, an optical fiber wire involved in one embodiment of the present invention comprises: a bare wire portion, which has a core and a cladding and extends in an axial direction; a main layer, which covers the above-mentioned bare wire portion; and a sub-layer, which covers the above-mentioned main layer, wherein the Young's modulus of the above-mentioned main layer is in the range of 0.10 to 0.45 MPa, and the extraction force required to extract the above-mentioned bare wire portion from the above-mentioned main layer in the above-mentioned axial direction is in the range of 0.6 to 1.2 N / mm, and when a point load is applied to the above-mentioned optical fiber wire with a spherical pin with a diameter of 3 mm, a gap is generated in the above-mentioned main layer before peeling occurs between the above-mentioned bare wire portion and the above-mentioned main layer and before cracks occur in the above-mentioned main layer.
[0008] According to the above aspects of the present invention, it is possible to provide a method for manufacturing an optical fiber wire and an optical fiber ribbon in which the transmission loss is unlikely to increase. BRIEF DESCRIPTION OF THE DRAWINGS
[0009] Figure 1 It is a perspective view showing the optical fiber wire according to the present embodiment.
[0010] Figure 2 It is along Figure 1 A cross-sectional view along line II-II is shown.
[0011] Figure 3 It is along Figure 1 The cross-sectional view taken along the line III-III is a diagram for explaining peeling, voids, and cracks.
[0012] Figure 4 This is a diagram for explaining an example of a method for measuring the Young's modulus of the main layer. DETAILED DESCRIPTION
[0013] Hereinafter, the optical fiber wire 1 according to the present embodiment will be described with reference to the drawings.
[0014] like Figure 1 , 2 As shown, the optical fiber wire 1 includes a bare wire portion 30, a main layer 10, and a secondary layer 20. The line speed when spinning the optical fiber wire 1 can be, for example, in the range of 1800 to 3000 m / min.
[0015] (Direction definition)
[0016] Here, in the present embodiment, the direction parallel to the central axis O of the bare wire portion 30 is referred to as the Z direction or the axial direction Z. The cross section perpendicular to the axial direction Z is referred to as the cross section. The direction orthogonal to the central axis O of the bare wire portion 30 is referred to as the radial direction. Along the radial direction, the direction close to the central axis O is referred to as the radial inner side, and the direction away from the central axis O is referred to as the radial outer side. The direction around the central axis O viewed from the axial direction Z is referred to as the circumferential direction.
[0017] The bare wire portion 30 extends along the axial direction Z. The bare wire portion 30 has a core and a cladding. The bare wire portion 30 is formed of, for example, glass. In this case, the bare wire portion 30 is also referred to as a glass portion 30. The refractive index of the core is higher than the refractive index of the cladding. Through this structure, light is sealed in the core, and the light propagates in the bare wire portion 30 along the axial direction Z. The outer diameter of the bare wire portion 30 is, for example, about 125 μm. However, the outer diameter of the bare wire portion 30 may be less than 100 μm. Alternatively, the outer diameter of the bare wire portion 30 may be less than 80 μm.
[0018] The main layer 10 is also called the first covering layer 10. The main layer 10 extends in the axial direction Z. The main layer 10 covers the bare wire portion 30 from the radial outside. The material of the main layer 10 is, for example, a UV-curable acrylate resin. More specifically, as the material of the main layer 10, for example, various monomers, oligomers, ultraviolet curable resin compositions, reactive diluents, polymerization initiators suitable for them, and silane coupling agents that improve the adhesion with the bare wire portion can be appropriately combined, such as polyurethane (meth) acrylate, epoxy (meth) acrylate, polyester acrylate, polyether, and polyamide. The Young's modulus of the main layer 10 involved in this embodiment is in the range of 0.10 to 0.45 MPa. For example, when the outer diameter of the bare wire portion 30 is about 125 μm and the outer diameter of the sub-layer 20 is less than 200 μm, the thickness of the main layer 10 is about 11 to 22 μm (more preferably 13 to 19 μm).
[0019] The sub-layer 20 is also referred to as the second coating layer 20. The sub-layer 20 extends in the axial direction Z. The sub-layer 20 covers the main layer 10 from the radial outside. The material of the sub-layer 20 is, for example, a UV-curable acrylate resin. More specifically, as the material of the sub-layer 20, for example, a material that appropriately combines various monomers, oligomers, ultraviolet curable resin compositions, reactive diluents, and polymerization initiators suitable for them, such as polyurethane (meth) acrylate, epoxy (meth) acrylate, polyester acrylate, polyether, and polyamide, can be used. The Young's modulus of the sub-layer 20 can be, for example, in the range of 750 to 2000 MPa (more preferably 750 to 1400 MPa). The glass transition temperature of the sub-layer 20 can be, for example, in the range of 60 to 110°C (more preferably 70 to 100°C). For example, when the outer diameter of the bare wire portion 30 is about 125 μm and the outer diameter of the sub-layer 20 is 200 μm or less, the thickness of the main layer 10 is about 11 to 22 μm (more preferably 13 to 19 μm).
[0020] The main layer 10 and the bare wire portion 30 are chemically bonded. Therefore, a certain amount of force is required to extract the bare wire portion 30 from the main layer 10 in the axial direction Z. Hereinafter, in this specification, the amount of force required to extract the bare wire portion 30 from the main layer 10 in the axial direction Z is referred to as "extraction force". In more detail, the extraction force is defined as the amount of force required to extract the bare wire portion 30 in the axial direction Z from the main layer 30 having a dimension of 1 mm in the axial direction Z. In the optical fiber wire 1 involved in the present embodiment, the extraction force is in the range of 0.6 to 1.2 N / mm. The amount of the extraction force depends on the amount of chemical bonding between the bare wire portion 30 and the main layer 10. Therefore, the amount of the extraction force becomes an indicator for knowing the amount of bonding between the bare wire portion 30 and the main layer 10.
[0021] Next, the operation of the optical fiber wire 1 configured as above will be described.
[0022] When manufacturing the optical fiber wire 1, or when manufacturing an optical fiber ribbon or an optical fiber cable using the optical fiber wire 1, there is a case where radial pressure (lateral pressure) is applied to the optical fiber wire 1. For example, when the spun optical fiber wire 1 is wound up on a bobbin, the optical fiber wires 1 overlap each other, and thus compressive stress is applied to the optical fiber wire 1. In addition, in order to extract the optical fiber wire 1, when the optical fiber wire 1 is sandwiched between a substrate and a ribbon, compressive stress is also applied to the optical fiber wire 1. In the above case, the optical fiber wire 1 generates a tensile stress in a direction perpendicular to the direction in which the compressive stress acts (axial direction Z).
[0023] When the above-mentioned pressure is applied to the optical fiber wire 1, defects may occur in the main layer 10 of the optical fiber wire 1 (see Figure 3 ). These defects are caused by both the stress applied to the optical fiber wire 1 and the residual stress in the optical fiber wire 1 itself. Defects are classified into peeling, voids V, and cracks C. Peeling is a phenomenon in which the close contact between the main layer 10 and the bare wire portion 30 is partially lost. If peeling occurs, Figure 3 In this way, a gap S is generated between the main layer 10 and the bare wire portion 30. The void V and the crack C are spaces generated in the main layer 10. That is, the void V and the crack C are not in contact with the bare wire portion 30 and the sub-layer 20. Therefore, even if the void V or the crack C is generated, the adhesion between the bare wire portion 30 and the main layer 10 remains unchanged. The shape of the crack C is such that the void V is connected in the longitudinal direction Z of the optical fiber 11.
[0024] In this specification, the void V is defined as a portion where the dimension L1 in the axial direction Z of the space generated in the main layer 10 is less than or equal to 3 times the dimension L2 in the radial direction. That is, L1≤3×L2 holds true for the void V. On the other hand, the crack C is defined as a portion where the dimension L1 in the axial direction Z of the space generated in the main layer 10 is greater than 3 times the dimension L2 in the radial direction. That is, L1>3×L2 holds true for the crack C.
[0025] As described above, when lateral pressure is applied to the optical fiber wire 1, local tensile stress is generated in the main layer 10. When the tensile stress exceeds the adhesion between the bare wire portion 30 and the main layer 10, peeling occurs. On the other hand, when the stress applied to the constituent material of the main layer 10 is relieved and the microscopic space inside the main layer 10 is expanded, a void V may be formed inside the main layer 10. When excessive stress is applied and the bare wire portion 30 and the main layer 10 are firmly adhered, not only the microscopic space inside the main layer 10 is expanded, but also sometimes the bond is cut. The expansion of the microscopic space accompanied by the cut of the bond becomes a crack C. Due to the influence of residual stress, the peeling, void V, and crack C that are temporarily generated will not disappear even after the applied stress is eliminated.
[0026] The generation of peeling, voids V, or cracks C in the optical fiber wire 1 may sometimes lead to an increase in the transmission loss of the optical fiber wire 1. This is because if peeling, voids V, or cracks C are generated in the optical fiber wire 1, the main layer 10 becomes uneven, causing adverse effects such as bending of the bare wire portion 30. In particular, when the optical fiber wire 1 is cooled, the main layer 10 becomes hard and shrinks unevenly, which easily causes adverse effects such as bending of the bare wire portion 30. As a result, the transmission loss of the optical fiber wire 1 is more likely to increase.
[0027] As a result of intensive research, the inventors of the present application have found that, for the optical fiber wire 1 according to the present embodiment, when the defect generated in the main layer 10 is a void V, the void V can be eliminated by heating the optical fiber wire 1. In other words, the inventors of the present application have found that even if the void V is generated in the optical fiber wire 1 according to the present embodiment, the increase in the transmission loss of the optical fiber wire 1 can be suppressed by heating the optical fiber wire 1.
[0028] It is believed that the voids V disappear due to heating because the residual stress in the optical fiber wire 1 is relaxed by heat due to the influence of the stress applied to the main layer 10. In addition, even if the optical fiber wire 1 is cooled temporarily, the residual stress that has been relaxed will not be restored. Therefore, even if the optical fiber wire 1 is cooled, the voids V that disappeared due to heating will not be generated again.
[0029] On the other hand, the inventors of the present application have conducted intensive research and found that when peeling or cracking occurs between the bare wire portion 30 and the main layer 10, the peeling or cracking will not disappear even if the optical fiber wire 1 is heated. In other words, the inventors of the present application have found that if peeling or cracking occurs in the optical fiber wire 1, it is difficult to suppress the increase in the transmission loss of the optical fiber wire 1.
[0030] It is considered that the reason why it is difficult to eliminate the peeling is that the chemical bond between the main layer 10 and the bare wire portion 30 is cut, thereby causing the peeling. However, it is also considered that the residual stress of the main layer 10 is relaxed by heating, the deformation of the main layer 10 is eliminated, and the peeling appears to disappear. However, in the part where the peeling does not occur, the chemical bond between the main layer 10 and the bare wire portion 30 is maintained, while in the part where the peeling occurs, the chemical bond between the main layer 10 and the bare wire portion 30 is cut. Therefore, when the optical fiber wire 1 is cooled, uneven stress is generated between the main layer 10 and the bare wire portion 30, and bending is easily generated in the bare wire portion 30. Therefore, it is difficult to suppress the increase in the transmission loss of the optical fiber wire 1. It is considered that the reason why it is difficult to eliminate the crack C is that the crack C is generated along with the cutting of the chemical bond in the main layer 10.
[0031] Here, in the optical fiber wire 1 involved in this embodiment, the Young's modulus of the main layer 10 is within the above range, and the extraction force is within the above range. Since the optical fiber wire 1 has this structure, when a point load is applied to the optical fiber wire 1 with a spherical pin with a diameter of 3 mm, for example, a void V is generated in the optical fiber wire 1 before peeling and cracking C.
[0032] As described above, even if a void V is generated in the optical fiber wire 1 by applying pressure such as a point load to the optical fiber wire 1, the void V can be eliminated by heating the optical fiber wire 1. That is, even if a defect is generated in the optical fiber wire 1, the generated defect is a void V that can be repaired by heating, rather than peeling or cracking C that cannot be repaired by heating. Therefore, an increase in the transmission loss of the optical fiber wire 1 can be suppressed.
[0033] In addition, the Young's modulus of the main layer 10, the extraction force of the optical fiber wire 1, etc. can be designed so that the void V disappears at a predetermined heating temperature and heating time. For example, the Young's modulus, extraction force, etc. can be set so that the void V disappears by heating the optical fiber wire 1 at 60°C for more than 3 minutes. Alternatively, the Young's modulus, extraction force, etc. can be set so that the void V that has disappeared temporarily will not be generated again at a predetermined cooling temperature and cooling time. For example, the Young's modulus, extraction force, etc. can be set so that the void V will not be generated again even if the optical fiber wire 1 is cooled at -40°C for more than 30 minutes.
[0034] It is also possible to prepare a plurality of optical fiber wires 1 involved in the present embodiment to manufacture an optical fiber ribbon. In addition, "optical fiber ribbon" refers to a tape-shaped (ribbon-shaped) component in which a plurality of optical fiber wires 1 are arranged and integrated in a direction perpendicular to the axial direction Z. When the optical fiber wire 1 is used to manufacture an optical fiber ribbon, a coloring process and a ribbonization process are performed. The coloring process is a process of using a colorant to set a coloring layer on the optical fiber wire 1. The ribbonization process is a process of integrating a plurality of optical fiber wires 1 into a ribbon by applying a ribbonization material to a plurality of optical fiber wires 1 and heating and curing the ribbonization material. In addition, the ribbonization material may also be a plurality of connecting portions in which a plurality of optical fiber wires 1 are intermittently connected in the axial direction Z. The optical fiber ribbon in this case is a so-called intermittent fixed ribbon core wire. Alternatively, the ribbonization material may also be a coating material that covers a plurality of optical fiber wires 1 together. In addition, the optical fiber wire 1 involved in the present embodiment may also be used to manufacture an optical fiber cable. When the optical fiber wire 1 is used to manufacture an optical fiber cable, a cableization process of covering the optical fiber wire 1 (optical fiber ribbon) with an outer skin material (sheath) is performed.
[0035] In these processes, heat is applied to the optical fiber wire 1. That is, in the final use form of the optical fiber ribbon or optical fiber cable, the optical fiber wire 1 has a thermal history related to the manufacture of the optical fiber ribbon or the manufacture of the optical fiber cable. The following specifically describes the heat to which the optical fiber wire 1 is subjected during the manufacture of the optical fiber ribbon and the optical fiber cable using the optical fiber wire 1.
[0036] The colorant used in the coloring process and the tape material used in the tape process are both UV curable resins. In each of the coloring process and the tape process, after the optical fiber wire 1 is coated with UV curable resin (colorant, tape material), it is irradiated with a metal halide lamp or UV-LED light to cause a cross-linking reaction. Thus, the formation of the coloring layer or the integration (taping) of the optical fiber wire 1 is performed. Here, the temperature inside the ultraviolet lamp is usually several hundred degrees Celsius due to radiant heat. Therefore, the optical fiber wire 1 is exposed to high temperature in the ultraviolet lamp whether in the coloring process or in the tape process. In addition, the cross-linking reaction is an exothermic reaction. Therefore, during curing, the optical fiber wire 1 is wound up by the bobbin in a state where the temperature has become high.
[0037] In addition, a thermoplastic resin is used as a sheath material of the optical fiber cable. In the cable-making process, the thermoplastic resin is processed after being heated to 120° C. or higher. Therefore, the optical fiber wire 1 housed in the heated thermoplastic resin is exposed to high temperature.
[0038] Therefore, whether the optical fiber wire 1 is commercialized as an optical fiber ribbon or as an optical fiber cable, the optical fiber wire 1 is exposed to high temperature. Therefore, the optical fiber wire 1 commercialized as an optical fiber ribbon or an optical fiber cable is likely to have a thermal history of 60° C. equivalent to about 3 minutes. According to the optical fiber wire 1 involved in this embodiment, the heat in the above-mentioned processes involved in the manufacture of the optical fiber ribbon and the manufacture of the optical fiber cable can also be used to eliminate the gap V.
[0039] Example
[0040] Hereinafter, the above-mentioned embodiment will be described using specific examples. In addition, the present invention is not limited to the following examples.
[0041] A total of 16 optical fiber wires consisting of Examples 1 to 9 and Comparative Examples 1 to 7 were prepared. Examples 1 to 9 are the optical fiber wires 1 described in the above embodiment. Examples 1 to 9 and Comparative Examples 1 to 7 differ from each other in the outer diameter of the optical fiber wire, the outer diameter of the main layer, the Young's modulus of the main layer, the Young's modulus of the sub-layer, and the extraction force. Table 1 is a table summarizing Examples 1 to 9 and Comparative Examples 1 to 7. For each of Examples 1 to 9 and Comparative Examples 1 to 7, the glass transition temperature of the sub-layer is 85°C, and the line speed during spinning is 2500 m / min. The glass transition temperature was measured by measurement at 1 Hz based on dynamic viscoelasticity measurement (DMA).
[0042] 【Table 1
[0043]
[0044] The Young's modulus of the main layer was measured in the state of the optical fiber wire, that is, in the state where the main layer, the bare wire portion, and the sub-layer formed the optical fiber wire. The Young's modulus of the main layer was measured in the shear mode.
[0045] Similarly, the Young's modulus of the sub-layer was measured in the state of the optical fiber wire. The coating material was separated from the optical fiber wire and the Young's modulus of the sub-layer was measured in the tensile mode.
[0046] The extraction force is calculated based on the maximum value of the force required to extract the bare wire portion from the main layer having a dimension of 5 mm in the axial direction Z at a speed of 3 mm / min in the axial direction Z.
[0047] In addition, the Young's modulus (shear mode) of the main layer is measured more specifically by the TMA method in an environment of 25°C. Figure 4As shown, the main layer and part of the sub-layer remain and the bare wire portion is exposed. Then, the sub-layer is fixed to stretch the bare wire portion in the axial direction, and the stretching load and the displacement of the bare wire portion are measured. When the stretching load is set to F and the displacement of the bare wire portion is set to ω, the Young's modulus G of the main layer can be calculated by the following formula (1). In formula (1), rg is the radius of the bare wire portion, rp is the radius of the main layer, and L is the length of the sub-layer in the axial direction (refer to Figure 4 ).
[0048] [Formula 1]
[0049]
[0050] The following experiment was conducted on the 16 optical fiber wires listed in Table 1. That is, for each optical fiber wire, a point load was applied using a 3mm diameter spherical pin to cause a defect in the main layer. More specifically, the spherical pin was brought into contact with the secondary layer and moved radially inward at a speed of 1mm / min, and a load of 1.0 to 3.0N was applied to the secondary layer. The magnitude of the load applied by the spherical pin was appropriately adjusted within the above range in such a way that a defect was caused in the main layer without damaging the secondary layer.
[0051] In addition, defects generated in the main layer were observed and classified into peeling, voids V, and cracks C. The defects were observed by immersing each optical fiber wire in matching oil and observing the immersed optical fiber wire with a microscope. The classification results are recorded in the right column of Table 1.
[0052] The above experiments were conducted within 7 days after the optical fiber wires were spun. During the period from spinning to the start of the experiment, each optical fiber wire was stored in an environment with a temperature of 20 to 26°C and a humidity (relative humidity, RH) of 40 to 60%.
[0053] As shown in Table 1, in the optical fiber wires involved in Examples 1 to 9 (optical fiber wire 1 involved in the above embodiment), the Young's modulus of the main layer is in the range of 0.10 to 0.45 MPa, and the extraction force is in the range of 0.60 to 0.90 N / mm. Furthermore, in the optical fiber wires involved in Examples 1 to 9, the form of the defect generated is a void V. In other words, in the optical fiber wires involved in Examples 1 to 9, when the magnitude of the load by the ball pin is gradually increased, the void V is generated before the peeling and cracking C.
[0054] As described above, the void V can be eliminated by heating. Therefore, in the optical fiber wires according to Examples 1 to 9, an increase in the transmission loss of the optical fiber wire can be suppressed by heating the optical fiber wire.
[0055] The reason why crack C occurred in the optical fiber wires involved in Comparative Examples 1 and 2 is considered to be that the Young's modulus of the main layer is low. More specifically, in the optical fiber wires involved in Comparative Examples 1 and 2, the Young's modulus of the main layer is less than 0.10 MPa. When the Young's modulus of the main layer is low, the main layer is easily broken, and it is considered that crack C is easily generated.
[0056] On the contrary, in the optical fiber wires according to Examples 1 to 9, the Young's modulus of the main layer is 0.10 MPa or more, which is relatively large, and therefore it is considered that cracks C are less likely to occur. In other words, in the optical fiber wires in which the Young's modulus of the main layer is relatively large, voids V are considered to occur before cracks C.
[0057] Delamination occurred in the optical fiber wires according to Comparative Examples 3 to 7. The causes of delamination will be examined below for each comparative example.
[0058] The optical fiber wires according to Comparative Examples 3 to 5 have a smaller extraction force than the optical fiber wire 1 according to the present embodiment. More specifically, the extraction force is less than 0.6 N / mm in the optical fiber wires according to Comparative Examples 1 and 2. When the extraction force is weak, the chemical adhesion between the main layer and the bare wire portion is weak, and thus it is considered that the adhesion between the main layer and the bare wire portion is easily lost, and peeling is easily caused.
[0059] On the contrary, in the optical fiber wires involved in Examples 1 to 9, the extraction force is 0.6 N / mm or more, which is sufficiently large. Therefore, it is considered that the close contact between the main layer and the bare wire portion is not easily lost, and peeling is not easy to occur. In other words, in the optical fiber wire with a sufficiently large extraction force, it is considered that the gap V is generated before peeling. Therefore, for example, for the optical fiber wire with a extraction force of 1.2 N / mm, it is naturally expected that the gap V is generated before peeling, just like the optical fiber wires involved in Examples 1 to 9.
[0060] In the optical fiber wires involved in Comparative Examples 6 and 7, the Young's modulus of the main layer is higher than that of the optical fiber wire 1 involved in the present embodiment. More specifically, in the optical fiber wires involved in Comparative Examples 6 and 7, the Young's modulus of the main layer is higher than 0.45 MPa. When the Young's modulus of the main layer is high, the main layer is strong, and it is considered that it is not easy to cause cracks in the main layer. Therefore, it can be considered that the void V caused by the rupture of the main layer is relatively difficult to generate compared with the peeling caused by the loss of the close contact between the main layer and the bare wire part. That is, when the Young's modulus of the main layer is high, it is considered that the peeling occurs before the void V.
[0061] On the contrary, in the optical fiber wires according to Examples 1 to 9, the Young's modulus of the main layer is 0.45 MPa or less, which is relatively low, and therefore it is considered that the void V is more likely to be generated than the peeling. That is, in the optical fiber wire having a relatively low Young's modulus of the main layer, the void V is considered to be generated before the peeling.
[0062] As described above, the optical fiber wire 1 involved in the present embodiment includes: a bare wire portion 30 having a core and a cladding and extending in the axial direction Z; a main layer 10 covering the bare wire portion 30; and a sub-layer 20 covering the main layer 10, wherein the Young's modulus of the main layer 10 is in the range of 0.10 to 0.45 MPa, and the extraction force required to extract the bare wire portion 30 from the main layer 10 in the axial direction Z is in the range of 0.6 to 1.2 N / mm, and when a point load is applied to the optical fiber wire 1 with a spherical pin with a diameter of 3 mm, a void V is generated in the main layer 10 before peeling occurs between the bare wire portion 30 and the main layer 10 and before cracks C are generated in the main layer 10.
[0063] According to this structure, even if a defect is generated in the optical fiber wire 1 due to pressure, the generated defect is a void V that can be repaired by heating, rather than peeling or cracking that cannot be repaired by heating. Therefore, an increase in the transmission loss of the optical fiber wire 1 can be suppressed.
[0064] The Young's modulus of the sub-layer 20 is in the range of 750 to 2000 MPa. In this case, by setting the Young's modulus of the main layer 10 and the extraction force of the optical fiber wire 1 in the above range, it is possible to prevent peeling from occurring.
[0065] In addition, the method for manufacturing an optical fiber ribbon according to the present embodiment prepares a plurality of the above-mentioned optical fiber wires 1, applies a ribbon material to the plurality of optical fiber wires 1, and heats and cures the ribbon material, thereby integrating the plurality of optical fiber wires 1 into a ribbon shape. According to this structure, when heat is applied to the optical fiber wires 1, the space V disappears, and an optical fiber ribbon with suppressed transmission loss can be manufactured.
[0066] In addition, the technical scope of the present invention is not limited to the above-mentioned embodiment, and various modifications can be added without departing from the gist of the present invention.
[0067] For example, the optical fiber wire 1 may have more than three coating layers. That is, other coating layers may be further provided around the secondary layer (second coating layer) 20. In addition, in order to ensure the adhesion between the bare wire portion 30 and the main layer 10, an adhesive layer may be provided between the bare wire portion 30 and the main layer 10.
[0068] In addition, the components in the above-described embodiment may be appropriately replaced with known components without departing from the gist of the present invention, and the above-described embodiment and modified examples may be appropriately combined.
[0069] Description of Reference Numerals
[0070] 1…optical fiber; 10…primary layer; 20…secondary layer; 30…bare wire portion; V…gap; V1…point-shaped gap; V2…linear gap; Z…axial direction.
Claims
1. An optical fiber wire, comprising: a bare wire portion having a core and a cladding and extending in an axial direction; a main layer covering the bare wire portion; and a secondary layer covering the main layer. The optical fiber wire is characterized in that: The Young's modulus of the main layer is in the range of 0.10 to 0.45 MPa, The extraction force required to extract the bare wire portion from the main layer along the axial direction is in the range of 0.6 to 1.2 N / mm. When a point load was applied to the optical fiber wire using a spherical pin having a diameter of 3 mm, voids were generated in the main layer before peeling occurred between the bare wire portion and the main layer and before cracks occurred in the main layer.
2. The optical fiber wire according to claim 1, It is characterized in that The Young's modulus of the secondary layer is in the range of 750 to 2000 MPa.
3. The optical fiber wire according to claim 1 or 2, It is characterized in that Even if the voids are generated in the main layer due to the application of a point load, the voids disappear by heating the optical fiber wire at 60° C. for more than 3 minutes.
4. The optical fiber wire according to any one of claims 1 to 3, It is characterized in that Even if the voids are generated in the main layer due to the application of a point load, the voids disappear by heating the optical fiber wire. Even if the heated optical fiber wire is cooled at -40°C for more than 30 minutes, the voids burned by heating will not be generated again.
5. A method for manufacturing an optical fiber ribbon, It is characterized in that A plurality of optical fiber wires according to any one of claims 1 to 4 are prepared, applying a ribbon material to the plurality of optical fiber wires, The plurality of optical fiber wires are integrated into a ribbon shape by heating and curing the ribbon material.
Citation Information
Patent Citations
Fiber coatings with low pullout force
CN112074493A
Coated optical fiber
CN1378655A
Coated optical fiber