Method for subsequently improving heterojunction performance of photo-anode

By constructing heterojunction on WO3 and treating it with sodium hydroxide solution, the photocurrent and stability of WO3/BiVO4 photoanode is improved, the problem of WO3 corrosion in alkaline solution is solved, and high-efficiency and low-cost photoelectricity is achieved Improved catalytic performance.

CN119019097APending Publication Date: 2024-11-26SHENYANG UNIV
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410783222.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-18
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

WO3 is prone to corrosion in alkaline solution, causing the catalyst to lose its activity, and the recombination rate of photogenerated electrons and photogenerated holes is too fast, so it cannot quickly migrate to the surface to participate in the redox reaction, resulting in a reduction in catalytic capacity.

Method used

The heterojunction is constructed with tungsten trioxide nanosheets and bismuth vanadate, and the photocurrent is increased by sodium hydroxide solution treatment. The steps include spin-coating the WO3 seed layer on the FTO conductive glass, annealing at high temperature to form the WO3 nanosheets, and spin-coating the vanadium. Bismuth acid and surface modification in sodium hydroxide solution.

Benefits of technology

The stability and photocurrent of WO3/BiVO4 photoanode are achieved, the product thickness is uniform, the preparation method is simple and efficient, and the cost is low. It is suitable for large-scale industrial production. It is easy to handle and operate with sodium hydroxide solution, saving time and effort.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019097A_ABST
    Figure CN119019097A_ABST
Patent Text Reader

Abstract

The invention discloses a method for subsequently improving the heterojunction performance of a photo-anode. The experimental preparation method comprises the following steps: firstly, spin-coating a layer of tungsten trioxide precursor solution on FTO (Fluorine-doped Tin Oxide) conductive glass, and putting the FTO conductive glass into a muffle furnace for annealing at 500 DEG C for 2 hours; then, a WO3 nanosheet is obtained by combining a hydrothermal method; and finally, spin-coating a tungsten trioxide nanosheet with the bismuth vanadate precursor solution, and annealing the tungsten trioxide nanosheet in a muffle furnace at 450 DEG C for 2 hours to obtain the WO3 / BiVO4 photo-anode heterojunction. The obtained WO3 / BiVO4 photo-anode heterojunction is put into a sodium hydroxide solution with a certain concentration to be soaked for different times, then the WO3 / BiVO4 photo-anode heterojunction is washed clean with deionized water and aired at the room temperature, and a photo-anode subjected to sodium hydroxide follow-up treatment can be obtained; and finally, a three-electrode system is adopted to explore the photocurrent density of hydrogen production in the solution by a photoanode in subsequent treatment under the condition that the illumination is calibrated to be 1 solar intensity irradiation. The method disclosed by the invention is simple to operate, low in equipment requirement, good in repeatability and low in cost, and the photocurrent density in the system is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of metal semiconductor material preparation methods, specifically designs a preparation method for subsequently improving the performance of a photoanode heterojunction, and studies its use as a method for improving the photocurrent of photoelectrocatalytic hydrogen production. Background Art

[0002] At present, with the rapid development of society, energy consumption is increasing day by day, and the environmental problems it brings are becoming increasingly prominent. In the next few decades, global development will still be inseparable from non-renewable fossil energy such as coal and oil. With the continuous use of non-renewable energy, the world will definitely face energy shortages in the future, so it is very important to seek renewable clean energy. At present, the world is vigorously developing clean energy, such as nuclear energy, solar energy, wind energy and tidal energy. Hydrogen energy has great advantages as a secondary clean energy. Hydrogen can release a lot of energy when burned, but it will not produce other pollutants. Therefore, hydrogen energy can be used as one of the effective solutions to replace energy in the future.

[0003] Photoelectrochemical (PEC) water splitting systems provide a promising method to produce hydrogen at the semiconductor / electrolyte interface under continuous sunlight. In addition, metal oxide semiconductors play an important role in both photocatalysis and photoelectrochemical (PEC) methods due to their low cost, high abundance and easy preparation methods. Among them, WO3 is one of the most promising materials, which has a relatively high response in the visible light range. Moreover, the band gap of WO3 is small, which is 2.5eV-2.8eV. In theory, WO3 can be used as a photoanode for hydrogen evolution.

[0004] However, WO3 itself still has some defects. It is easy to corrode in alkaline solution, which makes the catalyst inactive. The main reason is that the recombination rate of photogenerated electrons and photogenerated holes generated by WO3 itself is too fast under light, so it cannot quickly migrate to the surface to participate in the redox reaction, and the concentration of photogenerated carriers is low, thus losing its catalytic ability. In order to solve this problem, choosing a suitable semiconductor with a good energy band position as a protective layer on WO3 is a necessary condition for achieving its stable and efficient water decomposition reaction. Summary of the invention

[0005] The technical problem to be solved by the present invention is a method for post-processing the photoanode heterojunction at a low cost to increase the photoanode current.

[0006] In order to solve the technical problem of the present invention, the technical solution adopted is: a method for constructing a heterojunction by combining tungsten trioxide nanosheets with bismuth vanadate and subsequent treatment to improve the photocurrent, the main steps are as follows: Step 1: Use a glass cutter to cut the FTO conductive glass into a 2cm × 1cm cuboid, place the FTO glass in a mixed solution of acetone and ethanol (volume ratio of 1:1), and ultrasonicate for 15 minutes. Then, place the FTO conductive glass in a pre-prepared mixture of hydrogen peroxide and concentrated sulfuric acid (volume ratio of 7:3) and soak for 10 minutes. Finally, take out the FTO conductive glass, rinse it with alcohol, and blow it dry with nitrogen; Step 2, prepare the tungsten trioxide precursor solution in a container with a volume of V. Dissolve 1.65 g of sodium tungstate (Na2WO4·2H2O) in 25 ml of deionized water. After adding 3 ml of concentrated hydrochloric acid (HCl), a light yellow precipitate can be observed. Then put it into the centrifuge at 5000 rpm and centrifuge for 10 minutes, then pour out the supernatant and add deionized water, which is called one centrifugation, and centrifuge it 3 times in total. Dissolve the yellow precipitate after centrifugation in 5 ml of hydrogen peroxide (H2O2), then add 10 ml of deionized water and 0.5 g of polyvinyl alcohol (PVA). After ultrasonic treatment for 30 minutes, add deionized water to dilute the solution to 30 ml and mark it as WO3 precursor solution; Step 3, spin coating the WO3 precursor solution on the dried FTO conductive glass by a spin coating method, and then annealing the FTO conductive glass in a muffle furnace to obtain the FTO conductive glass with a WO3 seed layer; Step 4, weigh 0.1g sodium tungstate (Na2WO4·2H2O) and dissolve it in 45ml deionized water. After adding 4ml concentrated hydrochloric acid (HCl) to the above solution, a light yellow precipitate is obtained. Then, 0.54g oxalic acid (H2C2O4·2H2O) is added to the above solution under magnetic stirring until the precipitate is dissolved, and then diluted to 135ml. Next, take out 30ml of the precursor solution and transfer it to a stainless steel autoclave. Then, a piece of FTO conductive glass with a WO3 seed layer is immersed in the solution and tilted on the wall of the container with the seed layer facing down. The autoclave is then sealed and placed in a forced air drying oven. After cooling to room temperature, rinse the sample with deionized water. Finally, annealing in a muffle furnace can obtain WO3 nanosheets; Step 5: First, weigh 0.173 g of bismuth nitrate pentahydrate (BiNO3·5H2O) and 0.095 g of vanadyl acetylacetonate (C 10 H 14 O5V), put it into a clean glass bottle, then add 4.46 ml acetylacetone (C5H8O2) solution and 0.54 ml glacial acetic acid (C2H4O2) and shake the glass bottle to make the solid and liquid fully mixed and contact, then ultrasonicate it at room temperature for 10 minutes. There is no precipitation in the glass bottle and the solution turns dark green, which is marked as BiVO4 precursor solution; Step 6, prepare WO3 / BiVO4 photoanode by spin coating. Take 25μl of the BiVO4 precursor solution prepared above and coat it on FTO conductive glass with WO3, and set the spin coater speed to 2000 rpm and the spin coating time to 30s. Then put the spin-coated sample on a high-temperature workbench, set the temperature to 400℃ and keep it for 2 minutes. Finally, transfer the prepared sample to a muffle furnace to obtain a WO3 / BiVO4 photoanode; Step 7, in a container with a volume of V, prepare a sodium hydroxide solution with a concentration of c1, wherein c1 is 0.5 mol / L; Step 8, immersing the WO3 / BiVO4 photoanode prepared above in a sodium hydroxide solution for different time periods for surface modification; Step 9, use the traditional three-electrode method to test the stability of the sample, with WO3 / BiVO4 photoanode as the working electrode, Pt as the counter electrode, and Ag / AgCl as the reference electrode. Perform a photocurrent test on the sample under simulated sunlight.

[0007] The uniqueness of this low-cost preparation method as a subsequent treatment of WO3 / BiVO4 photoanodes is: A WO3 seed layer was spin-coated on the FTO conductive glass to ensure that the tungsten trioxide nanosheets were successfully attached to the FTO conductive glass during the hydrothermal process.

[0008] The bismuth vanadate precursor solution is spin-coated on the tungsten trioxide nanosheets and placed in a muffle furnace for high-temperature annealing to ensure that the bismuth vanadate particles are attached to the surface of the tungsten trioxide nanosheets, giving them a heterojunction function.

[0009] The surface of WO3 / BiVO4 photoanode heterojunction was treated with sodium hydroxide solution to improve the surface chemical properties for light conversion.

[0010] The unique effects of this new method compared to existing technologies are: First, the obtained target product was characterized by scanning electron microscopy and photocurrent density curve. The results showed that the target product had a relatively uniform thickness of about 200 nm tungsten trioxide nanosheets. Secondly, the preparation method is simple and efficient, not only producing tungsten trioxide nanosheets with uniform thickness, but also having the characteristics of time saving, green environmental protection, low preparation cost and easy large-scale industrial production. The raw materials required in the preparation process are all common raw materials for industrial production, which are easy to obtain and cheap; Third, the use of sodium hydroxide solution to treat the photoanode heterojunction has the advantages of simple operation, time saving and low cost.

[0011] The technical solution adopted in this experiment to realize the above-mentioned subsequent processing of the photoanode heterojunction preparation is as follows: The bismuth vanadate precursor solution was spin-coated on the surface of the tungsten trioxide nanosheets by spin coating, and then the sample was placed on a heating table at 400°C for 2 minutes. Finally, the sample was placed in a muffle furnace for high temperature annealing at 450°C for 2 hours, and then taken out when cooled to room temperature, immersed in a sodium hydroxide solution for a period of time, and then washed with deionized water and dried at room temperature. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] The preferred embodiments of the present invention are described in further detail below in conjunction with the accompanying drawings.

[0013] Figure 1 This is the scanning electron microscope (SEM) spectrum of the tungsten trioxide sample in Example 1; Figure 2 This is a scanning electron microscope (SEM) image of a tungsten trioxide sample spin-coated with 7 layers of bismuth vanadate in Example 2; Figure 3 This is a scanning electron microscope (SEM) image of the photoanode heterojunction treated with sodium hydroxide for 30 seconds in Example 3; Figure 4 This is a scanning electron microscope (SEM) image of the photoanode heterojunction treated with sodium hydroxide for 5 minutes in Example 4; Figure 5 This is a scanning electron microscope (SEM) image of the photoanode heterojunction treated with sodium hydroxide for 10 minutes in Example 5; Figure 6 The linear sweep (LSV) photocurrent spectrum of the photoanode heterojunction treated with sodium hydroxide for 0 to 10 minutes in Examples 2 to 5. DETAILED DESCRIPTION

[0014] The technical solution adopted by the present invention for preparing the cuprous oxide nanowires is further described in detail below in conjunction with the accompanying drawings and examples.

[0015] Example 1 The specific steps of preparation are: Step 1: Use a glass cutter to cut the FTO conductive glass into a 2cm × 1cm cuboid, place the FTO glass in a mixed solution of acetone and ethanol (volume ratio of 1:1), and ultrasonicate for 15 minutes. Then, place the FTO conductive glass in a pre-prepared mixture of hydrogen peroxide and concentrated sulfuric acid (volume ratio of 7:3) and soak for 10 minutes. Finally, take out the FTO conductive glass, rinse it with alcohol, and blow it dry with nitrogen; Step 2, prepare the tungsten trioxide precursor solution in a container with a volume of V. Dissolve 1.65 g of sodium tungstate (Na2WO4·2H2O) in 25 ml of deionized water. After adding 3 ml of concentrated hydrochloric acid (HCl), a light yellow precipitate can be observed. Then put it into the centrifuge at 5000 rpm and centrifuge for 10 minutes, then pour out the supernatant and add deionized water, which is called one centrifugation, and centrifuge it 3 times in total. Dissolve the yellow precipitate after centrifugation in 5 ml of hydrogen peroxide (H2O2), then add 10 ml of deionized water and 0.5 g of polyvinyl alcohol (PVA). After ultrasonic treatment for 30 minutes, add deionized water to dilute the solution to 30 ml and mark it as WO3 precursor solution; Step 3, spin coating the WO3 precursor solution on the dried FTO conductive glass by a spin coating method, and then annealing the FTO conductive glass in a muffle furnace to obtain the FTO conductive glass with a WO3 seed layer; Step 4, weigh 0.1g sodium tungstate (Na2WO4·2H2O) and dissolve it in 45ml deionized water. After adding 4ml concentrated hydrochloric acid (HCl) to the above solution, a light yellow precipitate is obtained. Then 0.54g oxalic acid (H2C2O4·2H2O) is added to the above solution under magnetic stirring until the precipitate is dissolved, and then diluted to 135ml. Next, 30ml of the precursor solution is taken out and transferred to a stainless steel autoclave. Then a piece of FTO conductive glass with a WO3 seed layer is immersed in the solution and tilted on the container wall with the seed layer facing down. The autoclave is then sealed and placed in a blast drying oven. After cooling to room temperature, the sample is rinsed with deionized water. Finally, WO3 nanosheets are obtained by annealing in a muffle furnace.

[0016] Example 2 The specific steps of preparation are: Step 1: Use a glass cutter to cut the FTO conductive glass into a 2cm × 1cm cuboid, place the FTO glass in a mixed solution of acetone and ethanol (volume ratio of 1:1), and ultrasonicate for 15 minutes. Then, place the FTO conductive glass in a pre-prepared mixture of hydrogen peroxide and concentrated sulfuric acid (volume ratio of 7:3) and soak for 10 minutes. Finally, take out the FTO conductive glass, rinse it with alcohol, and blow it dry with nitrogen; Step 2, prepare the tungsten trioxide precursor solution in a container with a volume of V. Dissolve 1.65 g of sodium tungstate (Na2WO4·2H2O) in 25 ml of deionized water. After adding 3 ml of concentrated hydrochloric acid (HCl), a light yellow precipitate can be observed. Then put it into the centrifuge at 5000 rpm and centrifuge for 10 minutes, then pour out the supernatant and add deionized water, which is called one centrifugation, and centrifuge it 3 times in total. Dissolve the yellow precipitate after centrifugation in 5 ml of hydrogen peroxide (H2O2), then add 10 ml of deionized water and 0.5 g of polyvinyl alcohol (PVA). After ultrasonic treatment for 30 minutes, add deionized water to dilute the solution to 30 ml and mark it as WO3 precursor solution; Step 3, spin coating the WO3 precursor solution on the dried FTO conductive glass by a spin coating method, and then annealing the FTO conductive glass in a muffle furnace to obtain the FTO conductive glass with a WO3 seed layer; Step 4, weigh 0.1g sodium tungstate (Na2WO4·2H2O) and dissolve it in 45ml deionized water. After adding 4ml concentrated hydrochloric acid (HCl) to the above solution, a light yellow precipitate is obtained. Then, 0.54g oxalic acid (H2C2O4·2H2O) is added to the above solution under magnetic stirring until the precipitate is dissolved, and then diluted to 135ml. Next, 30ml of the precursor solution is taken out and transferred to a stainless steel autoclave. Then a piece of FTO conductive glass with a WO3 seed layer is immersed in the solution and tilted on the wall of the container with the seed layer facing down. The autoclave is then sealed and placed in a forced air drying oven. After cooling to room temperature, the sample is rinsed with deionized water. Finally, annealing is performed in a muffle furnace to obtain WO3 nanosheets; Step 5: First, weigh 0.173 g of bismuth nitrate pentahydrate (BiNO3·5H2O) and 0.095 g of vanadyl acetylacetonate (C 10 H 14 O5V), put it into a clean glass bottle, then add 4.46 ml acetylacetone (C5H8O2) solution and 0.54 ml glacial acetic acid (C2H4O2) and shake the glass bottle to make the solid and liquid fully mixed and contacted, then ultrasonically treat it at room temperature for 10 minutes, and then mark it as BiVO4 precursor solution; Step 6, WO3 / BiVO4 photoanode was prepared by spin coating. 25μl of the BiVO4 precursor solution prepared above was coated on FTO conductive glass with WO3, and the spin coater speed was set to 2000 rpm and the spin coating time was set to 30s. Then the spin-coated sample was placed on a high-temperature workbench, the temperature was set to 400℃, and kept for 2 minutes. This was one cycle. After 7 cycles, the prepared sample was transferred to a muffle furnace to obtain a WO3 / BiVO4 photoanode.

[0017] Example 3 The specific steps of preparation are: Step 1: Use a glass cutter to cut the FTO conductive glass into a 2cm × 1cm cuboid, place the FTO glass in a mixed solution of acetone and ethanol (volume ratio of 1:1), and ultrasonicate for 15 minutes. Then, place the FTO conductive glass in a pre-prepared mixture of hydrogen peroxide and concentrated sulfuric acid (volume ratio of 7:3) and soak for 10 minutes. Finally, take out the FTO conductive glass, rinse it with alcohol, and blow it dry with nitrogen; Step 2, prepare the tungsten trioxide precursor solution in a container with a volume of V. Dissolve 1.65 g of sodium tungstate (Na2WO4·2H2O) in 25 ml of deionized water. After adding 3 ml of concentrated hydrochloric acid (HCl), a light yellow precipitate can be observed. Then put it into the centrifuge at 5000 rpm and centrifuge for 10 minutes, then pour out the supernatant and add deionized water, which is called one centrifugation, and centrifuge it 3 times in total. Dissolve the yellow precipitate after centrifugation in 5 ml of hydrogen peroxide (H2O2), then add 10 ml of deionized water and 0.5 g of polyvinyl alcohol (PVA). After ultrasonic treatment for 30 minutes, add deionized water to dilute the solution to 30 ml and mark it as WO3 precursor solution; Step 3, spin coating the WO3 precursor solution on the dried FTO conductive glass by a spin coating method, and then annealing the FTO conductive glass in a muffle furnace to obtain the FTO conductive glass with a WO3 seed layer; Step 4, weigh 0.1g sodium tungstate (Na2WO4·2H2O) and dissolve it in 45ml deionized water. After adding 4ml concentrated hydrochloric acid (HCl) to the above solution, a light yellow precipitate is obtained. Then, 0.54g oxalic acid (H2C2O4·2H2O) is added to the above solution under magnetic stirring until the precipitate is dissolved, and then diluted to 135ml. Next, 30ml of the precursor solution is taken out and transferred to a stainless steel autoclave. Then a piece of FTO conductive glass with a WO3 seed layer is immersed in the solution and tilted on the wall of the container with the seed layer facing down. The autoclave is then sealed and placed in a forced air drying oven. After cooling to room temperature, the sample is rinsed with deionized water. Finally, annealing is performed in a muffle furnace to obtain WO3 nanosheets; Step 5: First, weigh 0.173 g of bismuth nitrate pentahydrate (BiNO3·5H2O) and 0.095 g of vanadyl acetylacetonate (C 10 H 14O5V), put it into a clean glass bottle, then add 4.46 ml acetylacetone (C5H8O2) solution and 0.54 ml glacial acetic acid (C2H4O2) and shake the glass bottle to make the solid and liquid fully mixed and contacted, then ultrasonically treat it at room temperature for 10 minutes, and then mark it as BiVO4 precursor solution; Step 6, WO3 / BiVO4 photoanode was prepared by spin coating. Take 25μl of the BiVO4 precursor solution prepared above and coat it on FTO conductive glass with WO3, and set the spin coater speed to 2000 rpm and the spin coating time to 30s. Then put the spin-coated sample on a high-temperature workbench, set the temperature to 400℃, and keep it for 2 minutes. This is one cycle. After 7 cycles, transfer the prepared sample to a muffle furnace to obtain a WO3 / BiVO4 photoanode. Step 7, in a container with a volume of V, prepare a sodium hydroxide solution with a concentration of c1, wherein c1 is 0.5 mol / L; Step 8, immersing the WO3 / BiVO4 photoanode prepared above in a sodium hydroxide solution for 30 seconds for surface modification; Step 9, use the traditional three-electrode method to test the stability of the sample, with WO3 / BiVO4 photoanode as the working electrode, Pt as the counter electrode, and Ag / AgCl as the reference electrode. Perform a photocurrent test on the sample under simulated sunlight.

[0018] Example 4 The specific steps of preparation are: Step 1: Use a glass cutter to cut the FTO conductive glass into a 2cm × 1cm cuboid, place the FTO glass in a mixed solution of acetone and ethanol (volume ratio of 1:1), and ultrasonicate for 15 minutes. Then, place the FTO conductive glass in a pre-prepared mixture of hydrogen peroxide and concentrated sulfuric acid (volume ratio of 7:3) and soak for 10 minutes. Finally, take out the FTO conductive glass, rinse it with alcohol, and blow it dry with nitrogen; Step 2, prepare the tungsten trioxide precursor solution in a container with a volume of V. Dissolve 1.65 g of sodium tungstate (Na2WO4·2H2O) in 25 ml of deionized water. After adding 3 ml of concentrated hydrochloric acid (HCl), a light yellow precipitate can be observed. Then put it into the centrifuge at 5000 rpm and centrifuge for 10 minutes, then pour out the supernatant and add deionized water, which is called one centrifugation, and centrifuge it 3 times in total. Dissolve the yellow precipitate after centrifugation in 5 ml of hydrogen peroxide (H2O2), then add 10 ml of deionized water and 0.5 g of polyvinyl alcohol (PVA). After ultrasonic treatment for 30 minutes, add deionized water to dilute the solution to 30 ml and mark it as WO3 precursor solution; Step 3, spin coating the WO3 precursor solution on the dried FTO conductive glass by a spin coating method, and then annealing the FTO conductive glass in a muffle furnace to obtain the FTO conductive glass with a WO3 seed layer; Step 4, weigh 0.1g sodium tungstate (Na2WO4·2H2O) and dissolve it in 45ml deionized water. After adding 4ml concentrated hydrochloric acid (HCl) to the above solution, a light yellow precipitate is obtained. Then, 0.54g oxalic acid (H2C2O4·2H2O) is added to the above solution under magnetic stirring until the precipitate is dissolved, and then diluted to 135ml. Next, 30ml of the precursor solution is taken out and transferred to a stainless steel autoclave. Then a piece of FTO conductive glass with a WO3 seed layer is immersed in the solution and tilted on the wall of the container with the seed layer facing down. The autoclave is then sealed and placed in a forced air drying oven. After cooling to room temperature, the sample is rinsed with deionized water. Finally, annealing is performed in a muffle furnace to obtain WO3 nanosheets; Step 5: First, weigh 0.173 g of bismuth nitrate pentahydrate (BiNO3·5H2O) and 0.095 g of vanadyl acetylacetonate (C 10 H 14 O5V), put it into a clean glass bottle, then add 4.46 ml acetylacetone (C5H8O2) solution and 0.54 ml glacial acetic acid (C2H4O2) and shake the glass bottle to make the solid and liquid fully mixed and contacted, then ultrasonically treat it at room temperature for 10 minutes, and then mark it as BiVO4 precursor solution; Step 6, WO3 / BiVO4 photoanode was prepared by spin coating. Take 25μl of the BiVO4 precursor solution prepared above and coat it on FTO conductive glass with WO3, and set the spin coater speed to 2000 rpm and the spin coating time to 30s. Then put the spin-coated sample on a high-temperature workbench, set the temperature to 400℃, and keep it for 2 minutes. This is one cycle. After 7 cycles, transfer the prepared sample to a muffle furnace to obtain a WO3 / BiVO4 photoanode. Step 7, in a container with a volume of V, prepare a sodium hydroxide solution with a concentration of c1, wherein c1 is 0.5 mol / L; Step 8, immersing the WO3 / BiVO4 photoanode prepared above in a sodium hydroxide solution for 5 minutes for surface modification; Step 9, use the traditional three-electrode method to test the stability of the sample, with WO3 / BiVO4 photoanode as the working electrode, Pt as the counter electrode, and Ag / AgCl as the reference electrode. Perform a photocurrent test on the sample under simulated sunlight.

[0019] Example 5 The specific steps of preparation are: Step 1: Use a glass cutter to cut the FTO conductive glass into a 2cm × 1cm cuboid, place the FTO glass in a mixed solution of acetone and ethanol (volume ratio of 1:1), and ultrasonicate for 15 minutes. Then, place the FTO conductive glass in a pre-prepared mixture of hydrogen peroxide and concentrated sulfuric acid (volume ratio of 7:3) and soak for 10 minutes. Finally, take out the FTO conductive glass, rinse it with alcohol, and blow it dry with nitrogen; Step 2, prepare the tungsten trioxide precursor solution in a container with a volume of V. Dissolve 1.65 g of sodium tungstate (Na2WO4·2H2O) in 25 ml of deionized water. After adding 3 ml of concentrated hydrochloric acid (HCl), a light yellow precipitate can be observed. Then put it into the centrifuge at 5000 rpm and centrifuge for 10 minutes, then pour out the supernatant and add deionized water, which is called one centrifugation, and centrifuge it 3 times in total. Dissolve the yellow precipitate after centrifugation in 5 ml of hydrogen peroxide (H2O2), then add 10 ml of deionized water and 0.5 g of polyvinyl alcohol (PVA). After ultrasonic treatment for 30 minutes, add deionized water to dilute the solution to 30 ml and mark it as WO3 precursor solution; Step 3, spin coating the WO3 precursor solution on the dried FTO conductive glass by a spin coating method, and then annealing the FTO conductive glass in a muffle furnace to obtain the FTO conductive glass with a WO3 seed layer; Step 4, weigh 0.1g sodium tungstate (Na2WO4·2H2O) and dissolve it in 45ml deionized water. After adding 4ml concentrated hydrochloric acid (HCl) to the above solution, a light yellow precipitate is obtained. Then, 0.54g oxalic acid (H2C2O4·2H2O) is added to the above solution under magnetic stirring until the precipitate is dissolved, and then diluted to 135ml. Next, 30ml of the precursor solution is taken out and transferred to a stainless steel autoclave. Then a piece of FTO conductive glass with a WO3 seed layer is immersed in the solution and tilted on the wall of the container with the seed layer facing down. The autoclave is then sealed and placed in a forced air drying oven. After cooling to room temperature, the sample is rinsed with deionized water. Finally, annealing is performed in a muffle furnace to obtain WO3 nanosheets; Step 5: First, weigh 0.173 g of bismuth nitrate pentahydrate (BiNO3·5H2O) and 0.095 g of vanadyl acetylacetonate (C 10 H 14 O5V), put it into a clean glass bottle, then add 4.46 ml acetylacetone (C5H8O2) solution and 0.54 ml glacial acetic acid (C2H4O2) and shake the glass bottle to make the solid and liquid fully mixed and contacted, then ultrasonically treat it at room temperature for 10 minutes, and then mark it as BiVO4 precursor solution; Step 6, WO3 / BiVO4 photoanode was prepared by spin coating. Take 25μl of the BiVO4 precursor solution prepared above and coat it on FTO conductive glass with WO3, and set the spin coater speed to 2000 rpm and the spin coating time to 30s. Then put the spin-coated sample on a high-temperature workbench, set the temperature to 400℃, and keep it for 2 minutes. This is one cycle. After 7 cycles, transfer the prepared sample to a muffle furnace to obtain a WO3 / BiVO4 photoanode. Step 7, in a container with a volume of V, prepare a sodium hydroxide solution with a concentration of c1, wherein c1 is 0.5 mol / L; Step 8, immersing the WO3 / BiVO4 photoanode prepared above in a sodium hydroxide solution for 10 minutes for surface modification; Step 9, use the traditional three-electrode method to test the stability of the sample, with WO3 / BiVO4 photoanode as the working electrode, Pt as the counter electrode, and Ag / AgCl as the reference electrode. Perform a photocurrent test on the sample under simulated sunlight.

[0020] Through the above five implementation examples, the heterojunction constructed by tungsten trioxide and bismuth vanadate was analyzed, and we concluded that the photocurrent of the photoanode heterojunction treated with sodium hydroxide solution was further improved, and 5 min was the optimal treatment time. The product obtained by this method has good uniformity, good controllability, simple process, low cost, and has important research value and broad application prospects.

[0021] Obviously, those skilled in the art can make various changes and modifications to the low-cost preparation method of a photoanode heterojunction of the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. A method for improving the photocurrent of a photoanode heterojunction by subsequent treatment, characterized in that The main steps are as follows: Step 1: Use a glass cutter to cut the FTO conductive glass into a 2 cm × 1 cm cuboid, put the FTO glass into a mixed solution of acetone and ethanol (volume ratio of 1:1), ultrasonicate for 15 minutes, then put the FTO conductive glass into a pre-prepared mixture of hydrogen peroxide and concentrated sulfuric acid (volume ratio of 7:3) and soak for 10 minutes, finally take out the FTO conductive glass, rinse it with alcohol, and blow it dry with nitrogen; Step 2, in a container with a volume of V, prepare a tungsten trioxide precursor solution, dissolve 1.65g sodium tungstate (Na2WO4·2H2O) in 25ml deionized water, add 3ml concentrated hydrochloric acid (HCl), and a light yellow precipitate can be observed. Then put it into a centrifuge at 5000rpm and centrifuge for 10 minutes, then pour out the supernatant, and add deionized water, which is called one centrifugation. Centrifuge 3 times in total, dissolve the yellow precipitate after centrifugation in 5ml hydrogen peroxide (H2O2), and then add 10ml deionized water and 0.5g polyvinyl alcohol (PVA). After ultrasonic treatment for 30 minutes, add deionized water to dilute the solution to 30ml, and mark it as WO3 precursor solution; Step 3, spin coating the WO3 precursor solution on the dried FTO conductive glass by a spin coating method, and then annealing the FTO conductive glass in a muffle furnace to obtain the FTO conductive glass with a WO3 seed layer; Step 4, weigh 0.1g sodium tungstate (Na2WO4·2H2O) and dissolve it in 45ml deionized water, add 4ml concentrated hydrochloric acid (HCl) to the above solution to obtain a light yellow precipitate, then add 0.54g oxalic acid (H2C2O4·2H2O) to the above solution under magnetic stirring until the precipitate is dissolved, and then dilute to 135ml, next, take out 30ml of the precursor solution and transfer it to a stainless steel autoclave, then immerse a piece of FTO conductive glass with a WO3 seed layer in the solution, and tilt it on the container wall with the seed layer facing down, then seal the autoclave and put it into a blast drying oven, after cooling to room temperature, rinse the sample with deionized water, and finally, put it into a muffle furnace for annealing to obtain WO3 nanosheets; Step 5: First, weigh 0.173 g of bismuth nitrate pentahydrate (BiNO3·5H2O) and 0.095 g of vanadium acetylacetonate (C 10 H 14 O5V), put it into a clean glass bottle, then add 4.46ml acetylacetone (C5H8O2) solution and 0.54ml glacial acetic acid (C2H4O2) and shake the glass bottle to make the solid and liquid fully mixed and contacted, then ultrasonically treat it at room temperature for 10min, and then standardize it as BiVO4 precursor solution; Step 6, WO3 / BiVO4 photoanode was prepared by spin coating. 25 μl of the BiVO4 precursor solution prepared above was coated on FTO conductive glass with WO3, and then the spin-coated sample was placed on a high-temperature workbench, the temperature was set to 400°C, and maintained for 2 minutes, and the prepared sample was transferred to a muffle furnace and cooled to room temperature to obtain a WO3 / BiVO4 photoanode; Step 7, in a container with a volume of V, prepare a sodium hydroxide solution with a concentration of c1, wherein c1 is 0.5 mol / L; Step 8, immersing the WO3 / BiVO4 photoanode prepared above in a sodium hydroxide solution for a period of time for surface modification; Step 9, use the traditional three-electrode method to test the stability of the sample, with WO3 / BiVO4 photoanode as the working electrode, Pt as the counter electrode, and Ag / AgCl as the reference electrode. Perform a photocurrent test on the sample under simulated sunlight.

2. The preparation method according to claim 1, wherein in step 1, the concentration ratio of the alcohol to acetone mixed solution is 1:1, and the volume ratio of the mixed solution of hydrogen peroxide and concentrated sulfuric acid is 7:

3.

3. The preparation method according to claim 1, wherein in step 3, the high temperature annealing temperature in the muffle furnace is 500°C, the duration is 2 hours, and the mixture is naturally cooled to room temperature.

4. The preparation method according to claim 1, wherein in step 4, the hydrothermal reaction temperature is maintained at 180°C for 8 hours, and then naturally cooled to room temperature.

5. The preparation method according to claim 1, wherein in step 4, the high temperature annealing temperature in the muffle furnace is 500°C, the duration is 2 hours, and the mixture is naturally cooled to room temperature.

6. The preparation method according to claim 1, wherein the spin coater speed is set to 2000 rpm and the spin coating time is set to 30 s.

7. The preparation method according to claim 1, wherein in step 6, the high temperature annealing temperature in the muffle furnace is 450°C, the duration is 2 hours, and the annealing is naturally cooled to room temperature.

8. preparation method according to claim 1, in step 7, the sodium hydroxide solution concentration c1 is 0.5 mol / L.

9. The preparation method according to claim 1, wherein the sodium hydroxide solution treatment time in step 8 is 30s to 10min, and the further optimized post-treatment time is 5min.

10. The preparation method according to claim 1, wherein the sunlight simulated in step 9 is AM 1.5G illumination of 1 sunlight.

Citation Information

Cited By

  • Method for monitoring intracellular NADH (Nicotinamide Adenine Dinucleotide Hormone) in real time based on nanowire coupled photoelectrochemical sensor

    CN119881044A

  • A method for real-time monitoring of intracellular NADH based on a nanowire-coupled photoelectrochemical sensor