Large-size photocuring 3D printing ceramic and preparation method thereof
By adopting the dual processes of photocuring and thermal curing in large-size ceramic printing, combining anhydride curing agent and thermal conducting agent, the problems of uneven ceramic curing and cracking in traditional technology are solved, and efficient sintering and stable ceramic components are achieved, satisfying the The mechanical properties and thermal stability requirements of large-sized ceramics.
Patent Information
- Application Number
- CN202411248732.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-09-06
AI Technical Summary
When preparing large-size ceramic components, traditional three-dimensional photocuring technology causes uneven internal and external curing due to the limitation of light source penetration force and curing depth, which affects mechanical properties and thermal stability. The high exothermic characteristics during thermal curing increase the risk of cracking, making it difficult to Meet the requirements of precision engineering.
The large-size photocuring 3D printed ceramic consisting of ceramic powder, photosensitive resin monomer, epoxy-anhydride prepolymer, thermal conductor, dispersant, thermal initiator and photoinitiator are adopted. Through the dual process of photocuring and thermal curing, Combining an appropriate amount of anhydride curing agent and curing accelerator, optimize the heat distribution and crosslinking reaction to achieve thorough curing and efficient sintering of the blank.
It significantly enhances the internal bonding strength and thermal stability of large-sized ceramic blanks, reduces the risk of cracking, improves production efficiency, overall strength and sintering stability of finished products, and can stably print large-sized ceramic components to meet high density and Rapid forming demand.
Smart Images

Figure CN119019157A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a 3D printing ceramic and a preparation method thereof. Background Art
[0002] Traditional stereolithography technology faces many challenges in the preparation of large-scale ceramic components. The limited penetration of the light source and the curing depth lead to uneven curing inside and outside the component, which affects the mechanical properties and thermal stability of the material and limits its application in high-performance applications. In addition, insufficient resin curing and deformation and cracking during the drying process further damage the integrity and reliability of the material, making it difficult for the components to meet the strict standards of precision engineering. Therefore, it is urgent to develop new technologies to solve these problems.
[0003] As a key step in strengthening ceramic green bodies, secondary curing promotes further cross-linking of the resin through additional ultraviolet irradiation or other curing treatments, significantly improving the physical properties of the model and ensuring the reliability of the post-processing process. However, when the UV curing box currently used performs secondary curing on the green body, due to the limitation of ultraviolet light penetration, the internal curing of the green body is insufficient, and cracking or even breaking is prone to occur during the subsequent debinding and sintering process, reducing the yield rate. Although thermal curing can promote further curing of the resin, the huge heat generated may cause stress concentration, which has an adverse effect on the subsequent debinding and sintering process and may increase the risk of green body cracking. In particular, the cationic catalytic polymerization and cationic ring-opening polymerization mechanism of thermal curing epoxy resin, the ester exchange reaction between esters and alcohols, and the addition polymerization reaction of isocyanates and alcohols, the high exothermic characteristics of these reaction processes lead to obvious local heat release, resulting in uneven heating and easy generation of large thermal stress, which limits the application of thermal curing reactions in photocurable printing materials. Summary of the invention
[0004] The present invention aims to solve the problems of lower mechanical properties and thermal stability caused by incomplete curing of large-sized green bodies in the existing stereolithography technology, and deformation and cracking caused by internal and external temperature differences, and further provide a large-sized photocurable 3D printed ceramic and a preparation method thereof.
[0005] A large-size light-cured 3D printing ceramic is prepared by 72.25 to 86.75 parts of ceramic powder, 0.5 to 5 parts of reinforcing phase powder, 10 to 20 parts of photosensitive resin monomer, 0.5 to 2.5 parts of epoxy-anhydride prepolymer, 0.1 to 1 part of thermal conductor, 8 to 15 parts of dispersant, 0.1 to 0.5 parts of thermal initiator and 0.1 to 0.5 parts of photoinitiator in parts by mass;
[0006] The epoxy-acid anhydride prepolymer is prepared from 75 to 95 parts of aliphatic epoxide, 5 to 25 parts of acid anhydride curing agent and 0.05 to 0.25 parts of curing accelerator in parts by mass.
[0007] A method for preparing large-size light-cured 3D printed ceramics is carried out according to the following steps:
[0008] 1. Preparation of epoxy-anhydride prepolymer:
[0009] Weigh 75 to 95 parts of aliphatic epoxide, 5 to 25 parts of anhydride curing agent and 0.05 to 0.25 parts of curing accelerator by weight and stir and mix them evenly to obtain an epoxy-anhydride prepolymer;
[0010] 2. Preparation of ceramic photosensitive slurry:
[0011] Weigh 72.25 to 86.75 parts of ceramic powder, 0.5 to 5 parts of reinforcing phase powder, 10 to 20 parts of photosensitive resin monomer, 0.5 to 2.5 parts of epoxy-anhydride prepolymer, 0.1 to 1 part of thermal conductor, 8 to 15 parts of dispersant, 0.1 to 0.5 parts of thermal initiator and 0.1 to 0.5 parts of photoinitiator by mass, then stir and mix 72.25 to 86.75 parts of ceramic powder, 0.5 to 5 parts of reinforcing phase powder, 10 to 20 parts of photosensitive resin monomer, 0.5 to 2.5 parts of epoxy-anhydride prepolymer and 0.1 to 1 part of thermal conductor, then add 8 to 15 parts of dispersant and continue stirring, add 0.1 to 0.5 parts of thermal initiator and 0.1 to 0.5 parts of photoinitiator after stirring, and vacuum degassing and stirring to obtain ceramic photosensitive slurry;
[0012] 3. Large size model printing:
[0013] Pour the ceramic photosensitive slurry into the slurry tank, export the printing file according to the model slicing software, and use the light-curing printer to print layer by layer to obtain the ceramic blank;
[0014] 4. Post-processing of green body:
[0015] The ceramic green body is photocured for 2h to 3h by using UV light with a power of 50W to 100W and a wavelength of 355nm to 405nm, and then thermally cured for 3h to 5h at a temperature of 100℃ to 150℃ to obtain a dried ceramic green body. The dried ceramic green body is heated to 380℃ to 400℃ in an air atmosphere, and the binder is removed for 3h to 4h in an air atmosphere at a temperature of 380℃ to 400℃, and then heated to 500℃ to 550℃ in an air atmosphere, and Under the conditions of an air atmosphere and a temperature of 500°C to 550°C, debinding is carried out for 3h to 4h, and then the temperature is raised to 1000°C to 1200°C in an air atmosphere, and sintered for 3h to 5h in an air atmosphere and a temperature of 1000°C to 1200°C, and then the temperature is raised to 1500°C to 1650°C in an air atmosphere, and sintered for 3h to 5h in an air atmosphere and a temperature of 1500°C to 1650°C, and finally cooled with the furnace, thus completing a method for preparing large-size light-curing 3D printed ceramics.
[0016] The beneficial effects of the present invention are:
[0017] (a) By introducing an appropriate amount of anhydride curing agent and accelerator, the present invention achieves complete cross-linking of the unreacted small molecule resin in the photocurable printed body by thermal curing, thereby significantly enhancing the internal bonding strength of the large-sized ceramic body. This improvement ensures the complete curing of the small molecule monomer in the body and effectively reduces the risk of cracking during the drying process.
[0018] (b) The thermal conductivity of the printed body is optimized by using the excellent thermal conductivity of the thermal conductive agent, which achieves uniform heat transfer inside and outside the body. This temperature balance strategy effectively improves the heat transfer and heat dissipation performance of the printed body, helps to alleviate the thermal stress caused by the temperature gradient, prevents the cracking of large-sized bodies during the curing process, and improves thermal stability.
[0019] (c) The photothermal dual curing system composed of epoxy-anhydride is adopted. The present invention realizes the rapid photocuring shaping and thermal curing strengthening of the green body. The dual slow curing effect of photothermal and thermal and thermal balance mechanism are utilized to not only improve the production efficiency, but also significantly improve the overall strength of the green body, improve the forming and sintering stability of large-sized ceramic parts, effectively inhibit the generation of cracks, and meet the preparation requirements of large-sized and thick-walled ceramic green bodies.
[0020] (d) The 3D printing technology of the present invention can stably print large-sized ceramic green bodies with a size of up to 200 mm and a wall thickness of up to 36 mm. Through the entire process of drying, debinding and sintering, high-stability large-sized ceramic preparation is achieved, and rapid green body forming and high density are achieved.
[0021] Instruction Manual
[0022] Figure 1 The surface macro crack image of the large-scale photocurable 3D printed ceramic prepared in the comparative experiment 1;
[0023] Figure 2 This is a SEM image of the end of the crack propagation during the drying process of the ceramic body after drying described in step 4 of comparative experiment 2;
[0024] Figure 3 TG-DSC graphs of large-size photocurable 3D printed ceramics prepared in Example 5 and Comparative Experiment 3;
[0025] Figure 4 This is a schematic diagram of the structure of a large-size photocurable 3D printed ceramic prepared in Example 1;
[0026] Figure 5 This is a physical picture of the large-scale photocurable 3D printed ceramic prepared in Example 1. DETAILED DESCRIPTION
[0027] Specific implementation method 1: This implementation method is a large-size light-cured 3D printed ceramic, which is prepared by 72.25 to 86.75 parts of ceramic powder, 0.5 to 5 parts of reinforcing phase powder, 10 to 20 parts of photosensitive resin monomer, 0.5 to 2.5 parts of epoxy-anhydride prepolymer, 0.1 to 1 part of thermal conductor, 8 to 15 parts of dispersant, 0.1 to 0.5 parts of thermal initiator and 0.1 to 0.5 parts of photoinitiator in parts by mass;
[0028] The epoxy-acid anhydride prepolymer is prepared from 75 to 95 parts of aliphatic epoxide, 5 to 25 parts of acid anhydride curing agent and 0.05 to 0.25 parts of curing accelerator in parts by mass.
[0029] The beneficial effects of this embodiment are:
[0030] (a) By introducing an appropriate amount of anhydride curing agent and accelerator, the present invention achieves complete cross-linking of the unreacted small molecule resin in the photocurable printed body by thermal curing, thereby significantly enhancing the internal bonding strength of the large-sized ceramic body. This improvement ensures the complete curing of the small molecule monomer in the body and effectively reduces the risk of cracking during the drying process.
[0031] (b) The thermal conductivity of the printed body is optimized by using the excellent thermal conductivity of the thermal conductive agent, which achieves uniform heat transfer inside and outside the body. This temperature balance strategy effectively improves the heat transfer and heat dissipation performance of the printed body, helps to alleviate the thermal stress caused by the temperature gradient, prevents the cracking of large-sized bodies during the curing process, and improves thermal stability.
[0032] (c) The photothermal dual curing system composed of epoxy-anhydride is adopted. The present invention realizes the rapid photocuring shaping and thermal curing strengthening of the green body. The dual slow curing effect of photothermal and thermal and thermal balance mechanism are utilized to not only improve the production efficiency, but also significantly improve the overall strength of the green body, improve the forming and sintering stability of large-sized ceramic parts, effectively inhibit the generation of cracks, and meet the preparation requirements of large-sized and thick-walled ceramic green bodies.
[0033] (d) The 3D printing technology of the present invention can stably print large-sized ceramic green bodies with a size of up to 200 mm and a wall thickness of up to 36 mm. Through the entire process of drying, debinding and sintering, high-stability large-sized ceramic preparation is achieved, and rapid green body forming and high density are achieved.
[0034] Specific implementation method 2: This implementation method is different from specific implementation method 1 in that: the ceramic powder is one or more of zirconium oxide, aluminum oxide, silicon oxide, magnesium oxide, yttrium oxide, silicon nitride, boron nitride, aluminum nitride, aluminum carbide and chromium oxide; the reinforcing phase powder is one or more of calcium oxide, lanthanum oxide, cerium oxide and zinc oxide; the photosensitive resin monomer is one or more of 1,6-hexanediol diacrylate, tripropylene glycol diacrylate, trimethylolpropane triacrylate, polydipentaerythritol hexaacrylate and pentaerythritol tetraacrylate; the thermal conductor is graphite, carbon fiber The dispersant is one or more of BYK180, BYK190 and BYK163; the thermal initiator is one or more of azobisisobutyronitrile, potassium persulfate, sodium persulfate, ammonium persulfate, dodecyl peroxide, diisopropylbenzene peroxide and 1,1-di(tert-amylperoxy)cyclohexane; the photoinitiator is one or more of phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide and 2-hydroxy-2-methyl-1-phenyl-1-propanone. The others are the same as the first embodiment.
[0035] Specific implementation method three: This implementation method is different from specific implementation method one or two in that: the aliphatic epoxide is one or more of bis(3,3,5-trimethylcyclohexyl)phthalate, 3,4-epoxycyclohexanecarboxylic acid methyl ester, 3-cyclohexenecarboxylic acid methyl ester, methyl p-hydroxybenzoate and 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate; the acid anhydride curing agent is hexahydrophthalic anhydride, nadic anhydride, 4-methyltetrahydrophthalic anhydride, bicyclo[2.2.2]oct-7-ene-2,3,5,6-tetracarboxylic dianhydride, cyclobutanetetracarboxylic acid One or more of dianhydride, 3-methyltetrahydrophthalic anhydride, 4-methylhexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylendophthalic anhydride, methylhexahydrophthalic anhydride, tetrahydrophthalic anhydride, 4-methyltetrahydrophthalic anhydride, 3,3'-dithiodipropionic anhydride and hexahydro-4-methylphthalic anhydride are mixed; the curing accelerator is one or more of benzyldimethylamine, 2-hydroxybenzylaniline, 3-(3-hydroxyphenyl)-1,1-dimethylurea, resorcinol, o-cresol, ferric acetylacetonate, zinc acetylacetonate, boron trifluoride ether complex, 4-dimethylaminopyridine and 2-ethyl-4-methylimidazole. The rest is the same as the first or second embodiment.
[0036] Specific embodiment 4: This embodiment is a method for preparing large-size light-cured 3D printed ceramics, which is carried out according to the following steps:
[0037] 1. Preparation of epoxy-anhydride prepolymer:
[0038] Weigh 75 to 95 parts of aliphatic epoxide, 5 to 25 parts of anhydride curing agent and 0.05 to 0.25 parts of curing accelerator by weight and stir and mix them evenly to obtain an epoxy-anhydride prepolymer;
[0039] 2. Preparation of ceramic photosensitive slurry:
[0040] Weigh 72.25 to 86.75 parts of ceramic powder, 0.5 to 5 parts of reinforcing phase powder, 10 to 20 parts of photosensitive resin monomer, 0.5 to 2.5 parts of epoxy-anhydride prepolymer, 0.1 to 1 part of thermal conductor, 8 to 15 parts of dispersant, 0.1 to 0.5 parts of thermal initiator and 0.1 to 0.5 parts of photoinitiator by mass, then stir and mix 72.25 to 86.75 parts of ceramic powder, 0.5 to 5 parts of reinforcing phase powder, 10 to 20 parts of photosensitive resin monomer, 0.5 to 2.5 parts of epoxy-anhydride prepolymer and 0.1 to 1 part of thermal conductor, then add 8 to 15 parts of dispersant and continue stirring, add 0.1 to 0.5 parts of thermal initiator and 0.1 to 0.5 parts of photoinitiator after stirring, and vacuum degassing and stirring to obtain ceramic photosensitive slurry;
[0041] 3. Large size model printing:
[0042] Pour the ceramic photosensitive slurry into the slurry tank, export the printing file according to the model slicing software, and use the light-curing printer to print layer by layer to obtain the ceramic blank;
[0043] 4. Post-processing of green body:
[0044] The ceramic green body is photocured for 2h to 3h by using UV light with a power of 50W to 100W and a wavelength of 355nm to 405nm, and then thermally cured for 3h to 5h at a temperature of 100℃ to 150℃ to obtain a dried ceramic green body. The dried ceramic green body is heated to 380℃ to 400℃ in an air atmosphere, and the binder is removed for 3h to 4h in an air atmosphere at a temperature of 380℃ to 400℃, and then heated to 500℃ to 550℃ in an air atmosphere, and Under the conditions of an air atmosphere and a temperature of 500°C to 550°C, debinding is carried out for 3h to 4h, and then the temperature is raised to 1000°C to 1200°C in an air atmosphere, and sintered for 3h to 5h in an air atmosphere and a temperature of 1000°C to 1200°C, and then the temperature is raised to 1500°C to 1650°C in an air atmosphere, and sintered for 3h to 5h in an air atmosphere and a temperature of 1500°C to 1650°C, and finally cooled with the furnace, thus completing a method for preparing large-size light-curing 3D printed ceramics.
[0045] Specific embodiment 5: This embodiment differs from specific embodiment 4 in that: in step 1, the mixture is stirred and mixed for 10 min to 60 min at a temperature of 10° C. to 20° C. and a rotation speed of 400 r / min to 800 r / min. The rest is the same as specific embodiment 4.
[0046] Specific embodiment 6: This embodiment is different from the specific embodiment 4 or 5 in that: in step 2, 72.25 to 86.75 parts of ceramic powder, 0.5 to 5 parts of reinforcing phase powder, 10 to 20 parts of photosensitive resin monomer, 0.5 to 2.5 parts of epoxy-anhydride prepolymer and 0.1 to 1 part of thermal conductive agent are stirred and mixed for 10 to 30 minutes at a temperature of 20 to 60 degrees Celsius and a rotation speed of 800 to 1500 r / min, and then 8 to 15 parts of dispersant are added, and stirring is continued for 30 to 60 minutes at a temperature of 20 to 60 degrees Celsius and a rotation speed of 800 to 1500 r / min. The rest is the same as the specific embodiment 4 or 5.
[0047] Specific embodiment 7: This embodiment differs from Specific embodiments 4 to 6 in that: in step 2, vacuum degassing and stirring are performed for 30 min to 60 min under the conditions of vacuum degree of 0.01 MPa to 0.09 MPa, temperature of 20°C to 60°C and rotation speed of 800 r / min to 1500 r / min. The rest is the same as Specific embodiments 4 to 6.
[0048] Specific embodiment 8: This embodiment differs from specific embodiments 4 to 7 in that: in step 3, a light-curing printer is used to print layer by layer at a wavelength of 355 nm and an exposure power of 100 mW to 1000 mW, and the thickness of each layer is 30 μm to 300 μm. The rest is the same as specific embodiments 4 to 7.
[0049] Specific embodiment 9: This embodiment is different from specific embodiments 4 to 8 in that: in step 4, the dried ceramic body is heated to 380°C to 400°C in an air atmosphere and a heating rate of 80°C / h to 100°C / h, and the binder is removed for 3h to 4h in an air atmosphere and a temperature of 380°C to 400°C, and then the temperature is raised to 500°C to 550°C in an air atmosphere and a heating rate of 20°C / h to 60°C / h, and the binder is removed for 3h to 4h in an air atmosphere and a temperature of 500°C to 550°C. The rest is the same as specific embodiments 4 to 8.
[0050] Specific embodiment 10: This embodiment differs from specific embodiments 4 to 9 in that: in step 4, the temperature is raised to 1000°C to 1200°C in an air atmosphere at a heating rate of 200°C / h to 240°C / h, and sintered for 3h to 5h in an air atmosphere at a temperature of 1000°C to 1200°C, and then the temperature is raised to 1500°C to 1650°C in an air atmosphere at a heating rate of 60°C / h to 120°C / h, and sintered for 3h to 5h in an air atmosphere at a temperature of 1500°C to 1650°C. The rest is the same as specific embodiments 4 to 9.
[0051] The following examples are used to verify the beneficial effects of the present invention:
[0052] Embodiment 1:
[0053] A method for preparing large-size light-cured 3D printed ceramics is carried out according to the following steps:
[0054] 1. Preparation of epoxy-anhydride prepolymer:
[0055] Weigh 75 parts of aliphatic epoxide, 25 parts of anhydride curing agent and 0.25 parts of curing accelerator by mass, stir and mix for 10 minutes at a temperature of 20° C. and a magnetic stirring speed of 800 r / min to obtain an epoxy-anhydride prepolymer;
[0056] The aliphatic epoxide is 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexylcarboxylate; the acid anhydride curing agent is hexahydro-4-methylphthalic anhydride; the curing accelerator is 4-dimethylaminopyridine;
[0057] 2. Preparation of ceramic photosensitive slurry:
[0058] Weigh 86.75 parts of ceramic powder, 0.5 parts of reinforcing phase powder, 10 parts of photosensitive resin monomer, 2.5 parts of epoxy-anhydride prepolymer, 0.25 parts of thermal conductor, 8 parts of dispersant, 0.5 parts of thermal initiator and 0.5 parts of photoinitiator by mass, then stir and mix 86.75 parts of ceramic powder, 0.5 parts of reinforcing phase powder, 10 parts of photosensitive resin monomer, 2.5 parts of epoxy-anhydride prepolymer and 0.25 parts of thermal conductor for 30 minutes at a temperature of 20°C and a rotation speed of 800r / min, then add 8 parts of dispersant, continue stirring for 30 minutes at a temperature of 20°C and a rotation speed of 800r / min, add 0.5 parts of thermal initiator and 0.5 parts of photoinitiator after stirring, and vacuum degas and stir for 30 minutes at a vacuum degree of 0.05MPa, a temperature of 20°C and a rotation speed of 800r / min to obtain a ceramic photosensitive slurry;
[0059] The ceramic powder is aluminum oxide powder with an average particle size of 1 μm; the reinforcing phase powder is zinc oxide powder with an average particle size of 1 μm; the photosensitive resin monomer is 1,6-hexanediol diacrylate; the thermal conductor is graphene; the dispersant is BYK180; the thermal initiator is 1,1-di(tert-amylperoxy)cyclohexane; and the photoinitiator is phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide;
[0060] 3. Large size model printing:
[0061] Pour the ceramic photosensitive slurry into the slurry tank, export the printing file according to the model slicing software, and use the SLA light-curing printer to print layer by layer at a wavelength of 355nm and an exposure power of 500mW, and the printing thickness of each layer is 100μm to obtain a ceramic blank;
[0062] 4. Post-processing of green body:
[0063] The ceramic green body was photocured for 2 hours using UV light with a power of 50 W and a wavelength of 355 nm, and then thermally cured for 3 hours at a temperature of 130 ° C to obtain a dried ceramic body. The dried ceramic body was heated to 400 ° C in an air atmosphere and a heating rate of 100 ° C / h, and debinded for 4 hours in an air atmosphere and a temperature of 400 ° C, and then heated to 550 ° C in an air atmosphere and a heating rate of 50 ° C / h, and debinded for 4 hours in an air atmosphere and a temperature of 550 ° C, and then heated to 1000 ° C in an air atmosphere and a heating rate of 240 ° C / h, and sintered for 5 hours in an air atmosphere and a temperature of 1000 ° C, and then heated to 1600 ° C in an air atmosphere and a heating rate of 60 ° C / h, and sintered for 5 hours in an air atmosphere and a temperature of 1600 ° C, and finally cooled with the furnace to obtain large-size light-cured 3D printed ceramics.
[0064] The epoxy-anhydride prepolymer prepared in step 1 is stored in a refrigerated environment at 6° C.;
[0065] During printing in step 3, the UV light machine scans the point projection layer by layer, and the ceramic slurry polymerizes;
[0066] The large-size photocurable 3D printed ceramics prepared in step 4 are in the shape of special triangular structure ceramic parts with a total size of 200 mm × 214 mm × 35 mm and a wall thickness of 36.64 mm.
[0067] Embodiment 2: This embodiment is different from Embodiment 1 in that the amount of the anhydride curing agent in step 1 is 5 parts. The rest is the same as Embodiment 1.
[0068] Embodiment 3: This embodiment is different from Embodiment 1 in that the curing accelerator in step 1 is zinc acetylacetonate. The rest is the same as Embodiment 1.
[0069] Embodiment 4: This embodiment is different from Embodiment 1 in that the thermal conductive agent in step 2 is 0.1 parts. The rest is the same as Embodiment 1.
[0070] Embodiment 5: This embodiment is different from Embodiment 1 in that the thermal conductive agent in step 2 is 1 part. The rest is the same as Embodiment 1.
[0071] Comparative Experiment 1: This embodiment is different from Embodiment 1 in that the anhydride curing agent is omitted in Step 1. The rest is the same as Embodiment 1.
[0072] Comparative Experiment 2: This embodiment is different from the embodiment 1 in that the curing accelerator is omitted in step 1. The rest is the same as the embodiment 1.
[0073] Comparative Experiment 3: This embodiment is different from the embodiment 1 in that the thermal conductive agent is omitted in step 2. The rest is the same as the embodiment 1.
[0074] Table 1
[0075]
[0076] “-” in the table: The comparative experimental green bodies all cracked to varying degrees during the drying process. The cracking of the ceramic green bodies after drying in step 4 was not conducive to the test of linear shrinkage and density.
[0077] Examples 1 and 2 used 25 and 5 parts of anhydride curing agent, respectively. Compared with comparative experiment 1 (without using anhydride curing agent), the use of an appropriate amount of anhydride curing agent can significantly promote the ring-opening reaction of epoxy groups in epoxy resin, form intermediates, and further form a hardened network structure through cross-linking, which can effectively promote the bonding force between layers and avoid the generation of a large number of cross-layer cracks. This process effectively improves the strength and stability of the green body, laying a solid foundation for the subsequent debinding and sintering steps. Figure 1 The surface macro crack image of the large-scale photocurable 3D printed ceramics prepared for comparison experiment 1.
[0078] Example 3 uses zinc acetylacetonate as a curing accelerator. According to the data in the table, the selected curing accelerator can effectively promote the complete curing of the epoxy-anhydride prepolymer in the green body during the heat treatment process, which is beneficial to the debinding and sintering of the green body, but the ceramic linear shrinkage and density are worse than those of Example 1. Figure 2 As shown ( Figure 2 (SEM image of the end of the crack propagation during the drying process of the dried ceramic body described in step 4 of comparative experiment 2) The body in comparative experiment 2 without the addition of a curing accelerator cannot achieve the same degree of complete curing of the internal resin, causing the ceramic body to crack during the drying process, manifesting as interlayer cracks, which is not conducive to the stability of the ceramic body and affects its mechanical properties after sintering.
[0079] In Examples 4 and 5, 0.1 and 1 parts of graphene were introduced as thermal conductors, respectively. The data in the table show that, compared with Example 1, only when the addition amount of graphene was 0.25 parts, the internal curing degree of the material was significantly improved, which promoted the uniformity of heat distribution during the thermal curing process of the ceramic body, thereby greatly improving the mechanical properties of the ceramic. Figure 3 As shown, Figure 3TG-DSC graphs of large-scale photocurable 3D printed ceramics prepared in Example 5 and Comparative Experiment 3; Compared with Comparative Experiment 3 (without using thermal conductive agent), the addition of an appropriate amount of thermal conductive agent in Example 5 significantly increases the efficiency of thermal conductive curing of the system, balances the difference in internal and external thermal stress, and reduces the risk of cracking of the green body caused by rapid volatilization of small molecular resins in the green body. At the same time, its high thermal conductivity characteristics optimize the heat flow distribution and ensure the temperature uniformity of the green body during the curing process, thereby improving the overall quality and reliability of the finished product. At the same time, the problem of temperature difference between the inside and outside of the material is solved, greatly improving the stability of large-scale printed ceramic green bodies.
[0080] Figure 1 The surface macro cracks of large-scale photocurable 3D printed ceramics prepared in the first comparative experiment; it can be seen from the figure that the cross-linking density of the epoxy polymer will be significantly limited without the anhydride curing agent, which greatly reduces the degree of curing of the green body. This insufficient curing action leads to a weakening of the interlayer bonding force, and then during the thermal curing stage, due to the volatilization of the small molecule resin, stress concentration occurs inside the green body, causing the macroscopic expansion of interlayer cracks. These cracks not only damage the integrity of the material, but also further evolve into cross-layer cracks, posing a serious threat to the mechanical properties and structural stability of the material.
[0081] Figure 2 This is a SEM image of the end of the crack propagation during the drying process of the ceramic green body after drying described in step 4 of comparative experiment 2; it can be seen from the figure that the ceramic powder particles are tightly wrapped by the photosensitive resin, and the observed crack end morphology is mainly manifested as micron-level cracks, which are attributed to the accumulation of internal stress during the green body drying stage, which eventually exceeds the bonding strength of the polymer. Since no curing accelerator was used in comparative experiment 2, the green body contained incompletely cured small molecule resins, and the rapid volatilization of small molecules during high-temperature heat treatment caused excessive local compressive stress. This shows the importance of curing accelerators in the green body molding preparation process, and the necessity of controlling the release of volatile substances during heat treatment to avoid crack formation caused by stress concentration.
[0082] Figure 3TG-DSC diagram of large-size photocurable 3D printed ceramics prepared in Example 5 and Comparative Experiment 3. As can be seen from the figure, by comparing the thermal curing process of samples with and without thermal conductive agent in the temperature range of 0°C to 300°C, the significant difference in mass change between the two is revealed. According to the thermogravimetric analysis (TG) curve, it is shown that the sample with thermal conductive agent added has a slower mass decrease, a reduced volatilization amount, and good thermal stability when the temperature rises. On the contrary, the sample without thermal conductive agent has a faster mass decrease in the same temperature range, a higher volatilization amount, and a mass decrease rate that is too fast can easily lead to cracking of the green body. The analysis results of differential scanning calorimetry (DSC) further confirm the importance of thermal conductive agent. The sample without thermal conductive agent fails to effectively absorb and transfer heat during the thermal curing process, resulting in the failure of the small molecule resin inside to complete the curing reaction in time, which is another key factor causing the green body to crack.
[0083] Figure 4 This is a schematic diagram of the structure of a large-size photocurable 3D printed ceramic prepared in Example 1; Figure 5 This is a physical picture of the large-scale photocurable 3D printed ceramic prepared in Example 1. As can be seen from the figure, the large-scale ceramic printed structure printed by photocuring has a unique triangular structure, with a total size of 200mm×214mm×35mm and a wall thickness of 36.64mm. The 3D printed ceramic treated with a thermal conductive agent in the photothermal curing system has a smooth surface, a complete structure, and no obvious cracks.
Claims
1. A large-size photocurable 3D printed ceramic, characterized in that It is prepared from 72.25 to 86.75 parts of ceramic powder, 0.5 to 5 parts of reinforcing phase powder, 10 to 20 parts of photosensitive resin monomer, 0.5 to 2.5 parts of epoxy-anhydride prepolymer, 0.1 to 1 part of thermal conductor, 8 to 15 parts of dispersant, 0.1 to 0.5 parts of thermal initiator and 0.1 to 0.5 parts of photoinitiator by weight. The epoxy-acid anhydride prepolymer is prepared from 75 to 95 parts of aliphatic epoxide, 5 to 25 parts of acid anhydride curing agent and 0.05 to 0.25 parts of curing accelerator in parts by mass.
2. A large-size photocurable 3D printed ceramic according to claim 1, characterized in that The ceramic powder is one or more of zirconium oxide, aluminum oxide, silicon oxide, magnesium oxide, yttrium oxide, silicon nitride, boron nitride, aluminum nitride, aluminum carbide and chromium oxide; the reinforcing phase powder is one or more of calcium oxide, lanthanum oxide, cerium oxide and zinc oxide; the photosensitive resin monomer is one or more of 1,6-hexanediol diacrylate, tripropylene glycol diacrylate, trimethylolpropane triacrylate, polydipentaerythritol hexaacrylate and pentaerythritol tetraacrylate; the thermal conductor is one or more of graphite, carbon fiber, carbon nanotube and graphene. The invention relates to a method for preparing the present invention and the method for preparing the present invention. The method comprises the following steps: the step of preparing the present invention comprises: preparing the present invention by using the following methods: azobisisobutyronitrile, potassium persulfate, sodium persulfate, ammonium persulfate, dodecyl peroxide, diisopropylbenzene peroxide and 1,1-di(tert-amylperoxy)cyclohexane; the step of preparing the present invention comprises the following steps: a) preparing the present invention by using the following methods: b) preparing the present invention by using the following methods: c) preparing the present invention by using the following methods: e) preparing the present invention by using the following methods: e) preparing the present invention by using the following methods:
3. A large-size photocurable 3D printed ceramic according to claim 1, characterized in that The aliphatic epoxide is one or a mixture of bis(3,3,5-trimethylcyclohexyl)phthalate, 3,4-epoxycyclohexanecarboxylic acid methyl ester, 3-cyclohexenecarboxylic acid methyl ester, methyl p-hydroxybenzoate and 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexylcarboxylate; the acid anhydride curing agent is hexahydrophthalic anhydride, nadic anhydride, 4-methyltetrahydrophthalic anhydride, bicyclo[2.2.2]oct-7-ene-2,3,5,6-tetracarboxylic dianhydride, cyclobutanetetracarboxylic dianhydride, 3-methyltetrahydrophthalic anhydride, 4-methyl The curing accelerator is one or a mixture of hexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylendophthalic anhydride, methylhexahydrophthalic anhydride, tetrahydrophthalic anhydride, 4-methyltetrahydrophthalic anhydride, 3,3'-dithiodipropionic anhydride and hexahydro-4-methylphthalic anhydride; the curing accelerator is one or a mixture of benzyldimethylamine, 2-hydroxybenzylaniline, 3-(3-hydroxyphenyl)-1,1-dimethylurea, resorcinol, o-cresol, ferric acetylacetonate, zinc acetylacetonate, boron trifluoride ether complex, 4-dimethylaminopyridine and 2-ethyl-4-methylimidazole.
4. A method for preparing large-size photocurable 3D printed ceramics according to claim 1, characterized in that It is carried out in the following steps:
1. Preparation of epoxy-anhydride prepolymer: Weigh 75 to 95 parts of aliphatic epoxide, 5 to 25 parts of anhydride curing agent and 0.05 to 0.25 parts of curing accelerator by weight and stir and mix them evenly to obtain an epoxy-anhydride prepolymer; 2. Preparation of ceramic photosensitive slurry: Weigh 72.25 to 86.75 parts of ceramic powder, 0.5 to 5 parts of reinforcing phase powder, 10 to 20 parts of photosensitive resin monomer, 0.5 to 2.5 parts of epoxy-anhydride prepolymer, 0.1 to 1 part of thermal conductor, 8 to 15 parts of dispersant, 0.1 to 0.5 parts of thermal initiator and 0.1 to 0.5 parts of photoinitiator by mass, then stir and mix 72.25 to 86.75 parts of ceramic powder, 0.5 to 5 parts of reinforcing phase powder, 10 to 20 parts of photosensitive resin monomer, 0.5 to 2.5 parts of epoxy-anhydride prepolymer and 0.1 to 1 part of thermal conductor, then add 8 to 15 parts of dispersant and continue stirring, add 0.1 to 0.5 parts of thermal initiator and 0.1 to 0.5 parts of photoinitiator after stirring, and vacuum degassing and stirring to obtain ceramic photosensitive slurry; 3. Large size model printing: Pour the ceramic photosensitive slurry into the slurry tank, export the printing file according to the model slicing software, and use the light-curing printer to print layer by layer to obtain the ceramic blank; 4. Post-processing of green body: The ceramic green body is photocured for 2h to 3h by using UV light with a power of 50W to 100W and a wavelength of 355nm to 405nm, and then thermally cured for 3h to 5h at a temperature of 100℃ to 150℃ to obtain a dried ceramic green body. The dried ceramic green body is heated to 380℃ to 400℃ in an air atmosphere, and the binder is removed for 3h to 4h in an air atmosphere at a temperature of 380℃ to 400℃, and then heated to 500℃ to 550℃ in an air atmosphere, and Under the conditions of an air atmosphere and a temperature of 500°C to 550°C, debinding is carried out for 3h to 4h, and then the temperature is raised to 1000°C to 1200°C in an air atmosphere, and sintered for 3h to 5h in an air atmosphere and a temperature of 1000°C to 1200°C, and then the temperature is raised to 1500°C to 1650°C in an air atmosphere, and sintered for 3h to 5h in an air atmosphere and a temperature of 1500°C to 1650°C, and finally cooled with the furnace, thus completing a method for preparing large-size light-curing 3D printed ceramics.
5. The method for preparing large-size photocurable 3D printed ceramics according to claim 4, characterized in that In step 1, the mixture is stirred and mixed for 10 min to 60 min at a temperature of 10° C. to 20° C. and a rotation speed of 400 r / min to 800 r / min.
6. The method for preparing large-size photocurable 3D printed ceramics according to claim 4, characterized in that In step 2, 72.25 to 86.75 parts of ceramic powder, 0.5 to 5 parts of reinforcing phase powder, 10 to 20 parts of photosensitive resin monomer, 0.5 to 2.5 parts of epoxy-anhydride prepolymer and 0.1 to 1 part of thermal conductor are stirred and mixed for 10 to 30 minutes at a temperature of 20 to 60 degrees Celsius and a rotation speed of 800 to 1500 r / min, and then 8 to 15 parts of dispersant are added. Stirring is continued for 30 to 60 minutes at a temperature of 20 to 60 degrees Celsius and a rotation speed of 800 to 1500 r / min.
7. The method for preparing large-size photocurable 3D printed ceramics according to claim 4, characterized in that In step 2, vacuum degassing and stirring are performed for 30 min to 60 min under the conditions of vacuum degree of 0.01 MPa to 0.09 MPa, temperature of 20° C. to 60° C. and rotation speed of 800 r / min to 1500 r / min.
8. The method for preparing large-size photocurable 3D printed ceramics according to claim 4, characterized in that In step 3, a photocuring printer is used to print layer by layer at a wavelength of 355 nm and an exposure power of 100 mW to 1000 mW, and the printing thickness of each layer is 30 μm to 300 μm.
9. The method for preparing large-size photocurable 3D printed ceramics according to claim 4, characterized in that In step 4, the dried ceramic body is heated to 380°C to 400°C in an air atmosphere at a heating rate of 80°C / h to 100°C / h, and the binder is removed for 3h to 4h in an air atmosphere at a temperature of 380°C to 400°C. Then, the temperature is increased to 500°C to 550°C in an air atmosphere at a heating rate of 20°C / h to 60°C / h, and the binder is removed for 3h to 4h in an air atmosphere at a temperature of 500°C to 550°C.
10. The method for preparing large-size photocurable 3D printed ceramics according to claim 4, characterized in that In step 4, the temperature is increased to 1000°C to 1200°C in an air atmosphere at a heating rate of 200°C / h to 240°C / h, and sintered for 3h to 5h in an air atmosphere at a temperature of 1000°C to 1200°C. Then, the temperature is increased to 1500°C to 1650°C in an air atmosphere at a heating rate of 60°C / h to 120°C / h, and sintered for 3h to 5h in an air atmosphere at a temperature of 1500°C to 1650°C.
Citation Information
Patent Citations
Ceramic slurry preparation and 3D (three dimensional) printing light curing molding method
CN106810215A
Monomer formulations and methods for 3D printing of preceramic polymers
CN110023378A
UV / near-infrared light dual-trigger-cured thiol-ene system and preparation method thereof
CN110563950A
Compositions, methods, and articles involving in situ crosslinking of polyamides during additive manufacturing
CN114539765A
Curing agent composition for epoxy resin and epoxy resin composition containing the same
JP2005075915A
Cited By
Complex coupling field six-axis robot multi-material additive manufacturing system and using method thereof
CN119748598A
Additive manufacturing high-precision collapsible ceramic shell
CN120984815A
Additive manufacturing of high precision fugitive ceramic shells
CN120984815B
ZnO-based voltage-sensitive semiconductor ceramic and preparation method and application thereof