High-gas-retention and high-heat-conductivity tire transition layer rubber composition, mixing method thereof and all-steel truck tire

By using sheet silicate inorganic filler and recycled rubber in the all-steel tire transition layer formula, the problem of insufficient thermal conductivity and gas-retaining performance of carbon black is solved, and a rubber composition with high thermal conductivity and gas-retaining is achieved, and the tires are improved thermal balance and airtight properties.

CN119019767AActive Publication Date: 2024-11-26ZHONGCE RUBBER GRP CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411159778.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-26
Estimated Expiration
2044-08-22

AI Technical Summary

Technical Problem

The thermal conductivity and gas-retaining performance of carbon black in the existing all-steel tire transition layer formula is insufficient, making it difficult to meet the requirements of carbon reduction and performance improvement, especially in high-temperature environments with challenges in heat transfer and airtightness.

Method used

The sheet-layer silicate inorganic filler is used to replace most of the carbon black, combine recycled rubber and specific additives, and optimize the rubber composition formula through the kneading method to improve thermal conductivity and gas-saving performance.

Benefits of technology

It significantly improves the thermal conductivity and air-saving performance of the tire transition layer, reduces the air permeability and heat generation of the formula, improves the thermal balance and air tightness, and meets the high-performance needs of all-steel radial tires.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the technical field of new tire manufacturing materials, in particular to a high-gas-retention and high-heat-conductivity tire transition layer rubber composition, a mixing method thereof and an all-steel truck tire. According to the invention, the lamellar silicate inorganic filler is mainly used for replacing most of carbon black and is applied to the all-steel radial tire transition layer formula, so that the air permeability coefficient of the transition layer formula is reduced, and the air retaining performance of the tire is improved; the heat conductivity coefficient of the transition layer formula is improved, and the heat transfer efficiency in the tire is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of new materials for tire manufacturing, and in particular to a tire transition layer rubber composition with high air retention and high heat conductivity, a mixing method thereof, and an all-steel load-bearing tire. Background Art

[0002] With the development of the load-carrying market, people's research on all-steel load-carrying radial tires has become more mature, and the role of each tire component in the tire has become clearer. At present, the inner liner of the all-steel load-carrying radial tire is mainly composed of a transition layer and an airtight layer. The transition layer is to ensure the stability of the tire body, and its key performance is close to the tire body performance. The air retention performance is poor, and the tire air retention performance is mainly supported by the airtight layer. Early tests showed that the air retention performance of the inner liner was improved by 10%, which significantly improved the shoulder empty return rate of the all-steel radial tire (the cycle return rate of a certain specification of 12R after 36 months was reduced by 20%-30%). Thermal conductivity is an important indicator of tire performance, which directly affects the temperature distribution and heat transfer of the tire during driving. The thermal conductive filler in the tire formula can quickly conduct heat from the tire surface to the inside of the tire body, thereby reducing the occurrence of local overheating, improving the thermal balance ability of the tire, and enabling the tire to maintain good performance in a high temperature environment. Carbon black is the main thermal conductive filler in the current all-steel tire formula. With the introduction of carbon reduction requirements and the market's increased performance requirements for all-steel tires and demand for production efficiency, it is particularly important to improve the existing formula and enhance the thermal conductivity and air retention performance of the formula.

[0003] At present, the filler of the all-steel transition layer formula is mainly carbon black. The spherical structure of carbon element determines that its gas retention performance is significantly worse than that of inorganic fillers with lamellar structure. In addition, the thermal conductivity of carbon element is somewhat different from that of metal elements in inorganic fillers. With the requirements of carbon reduction, it is urgent to find a high gas retention and high thermal conductivity material that can replace traditional carbon black.

[0004] The applicant applied for a Chinese invention patent application (publication number: CN109134981A, publication date: 2019-01-04) to disclose a rubber composition for the tire tread of a high-performance tire, the rubber composition comprising 100 parts by weight of at least one rubber component selected from natural rubber, polyisoprene rubber, polybutadiene rubber and styrene-butadiene copolymer rubber and 0.5 to 40 parts by weight of (a) nano-scale surface conductive modified silicate, and (b) carbon black and silica, wherein the total amount of components (a) and (b) is 40 to 120 parts by weight. The patent innovatively introduces nano-scale surface conductive modified silicate, which has the same effect of reducing tire rolling resistance and improving tire wet grip as silica, while also increasing tire conductivity, so that the amount of silica can be increased within the resistance range allowed by regulations, thereby achieving the purpose of further reducing rolling resistance and improving wet grip.

[0005] The applicant applied for a Chinese invention patent application (publication number: CN115322463A, publication date: 2022-11-11) to disclose a low-heating, anti-fatigue rubber composition for producing air springs, and its preparation method and application. The rubber composition is prepared by mixing the following raw materials based on 100 parts by weight of the rubber component: 100 parts of chloroprene rubber, 20-40 parts of carbon black, 5.0-30 parts of white carbon black, 1.0-5.0 parts of silane coupling agent, 5.0-20 parts of nano-sheet silicate, and 0-0.8 parts of organic sulfur donor. The air spring of this patent has lower heat generation and better fatigue resistance.

[0006] The addition of nano-flaky silicates to the above-mentioned rubber is generally for the purpose of reducing heat generation. Lamellar materials are also added to all-steel radial tires, and are generally used in the airtight layer. The rubber material of the airtight layer is halogenated butyl rubber. For example, the Chinese invention patent application (publication number: CN115975303A, publication date: 2023-04-18) discloses an airtight layer rubber material for an all-steel radial tire, which is prepared by mixing the following components in parts by mass: 80 parts of halogenated butyl rubber, 40 parts of lamellar materials, 40 parts of carbon black, 2 parts of magnesium oxide, 2 parts of zinc oxide, 4 parts of stearic acid, 2 parts of a homogenizer, 3 parts of operating oil, 0.5 parts of sulfur, and 1.5 parts of an accelerator.

[0007] In addition, recycled rubber is one of the main products of the comprehensive utilization of waste tires and waste rubber. The application of recycled rubber not only reduces the cost of rubber products and improves economic benefits, but also plays a great role in saving rubber resources and protecting the environment. It is the embodiment of circular economy in the rubber industry. The application of recycled rubber, such as the Chinese invention patent applications applied by the applicant (CN101628994A, CN101624454A, CN101628993A, CN101628995A and CN101628992A, etc.), is generally applied to the carcass, tread, sidewall and outer protective rubber. If it is in the transition layer of the tire, it will affect the performance of the transition layer. Therefore, it is also necessary to design a suitable formula so that the recycled rubber can be used in the transition layer without affecting the performance of the transition layer. Summary of the invention

[0008] In view of the above problems, the purpose of the present invention is to provide a tire transition layer rubber composition with high air retention and high thermal conductivity, mainly using lamellar silicate inorganic filler to replace most of the carbon black, and applying it to the transition layer formula of the all-steel radial tire, thereby reducing the air permeability coefficient of the transition layer formula and improving the air retention performance of the tire; improving the thermal conductivity of the transition layer formula and improving the heat transfer efficiency in the tire.

[0009] In order to achieve the above-mentioned purpose, the present invention adopts the following technical solutions: A tire transition layer rubber composition with high air retention and high thermal conductivity, characterized in that the rubber composition is prepared by mixing the following components by mass fraction: Natural rubber: 100 parts Recycled rubber: 5-30 copies Lamellar silicate filler: 70-110 parts Carbon black: 0-15 parts Tackifying resin: 1-8 parts Meta-acetic resin: 0.3-1.2 parts Nickel salt: 0.3-1.2 parts; The D50 particle size of the lamellar silicate filler is below 1 micron, and the main components are 30-45% aluminum oxide and 35-50% silicon dioxide.

[0010] Preferably, the rubber composition is prepared by mixing the following raw materials by mass fraction: Natural rubber: 100 parts Recycled rubber: 10-20 copies Lamellar inorganic filler: 90-100 parts Carbon black: 5-10 parts Tackifying resin: 3-6 parts Meta-acetic resin: 0.5-1.0 parts Nickel salt: 0.5-1.0 part.

[0011] Preferably, the flaky inorganic filler is RC-15 flaky silicate inorganic filler provided by China Baiya Trading (Hong Kong) Co., Ltd., the main components of which are 38% aluminum oxide and 42% silicon dioxide.

[0012] Preferably, the active agent is 1-8 parts, preferably 3-6 parts; the binder is 2-6 parts, preferably 3-5 parts; the antioxidant is 0-3 parts, preferably 0.5-2 parts; the accelerator is 0.5-2 parts, preferably 1-1.5 parts; and the sulfur is 1-8 parts, preferably 3-6 parts.

[0013] Preferably, the antioxidant is selected from 0.3-0.8 parts of antioxidant 4020 and 0.8-1.5 parts of antioxidant RD; and the sulfur is selected from 3.0-4.5 parts of insoluble sulfur and 0.8-1.5 parts of 10% oil-extended sulfur.

[0014] Preferably, the reclaimed rubber is GZ-12 reclaimed rubber and GZ-16 reclaimed rubber produced by Shanxi Beihai Rubber Co., Ltd., with GZ-12 reclaimed rubber being preferred.

[0015] Preferably, the carbon black is one or more of N326, N330, N375, N550, N660 and N774, and preferably the carbon black is N326 or N375.

[0016] Preferably, the nickel salt is nickel borate; Preferably, the tackifying resin is one or more of p-tert-butyl tackifying resin, p-tert-octyl tackifying resin, acetyl tackifying resin and ethylene tackifying resin, preferably p-tert-octyl tackifying resin; Preferably, the active agent is one or more of zinc oxide and stearic acid.

[0017] Furthermore, the present invention also discloses a mixing method for the tire transition layer rubber composition with high air retention and high thermal conductivity, which comprises the following steps: 1) First-stage mixing: Rubber, carbon black and inorganic filler RC-15 are put into an internal mixer and mixed for 30 to 50 seconds at a speed of 45 to 60 rpm. The mixture is lifted and pressed every 20 to 35 seconds. When the temperature of the rubber reaches 155 to 170 °C, the rubber is discharged and the pieces are dropped. After cooling at room temperature for 8 to 12 hours, a first-stage masterbatch is obtained, which is then subjected to second-stage mixing. 2) Second stage mixing: the first stage masterbatch, inorganic filler RC-15, antioxidant and other rubber processing aids of step 1) are put into an internal mixer, mixed at a speed of 40-55 rpm, and the lump is lifted and pressed every 20-35 seconds. When the temperature of the rubber material reaches 145-160°C, the rubber is discharged and the sheets are dropped. After cooling at room temperature for 8-12 hours, the second stage masterbatch is obtained, and then final mixing is performed; 3) Final mixing: the second-stage masterbatch, vulcanizing agent and accelerator of step 2) are put into an internal mixer, mixed at a speed of 20-30 rpm, and the mixture is lifted and pressed at intervals of 20-30 seconds, 15-25 seconds and 10-20 seconds respectively. When the temperature of the rubber material reaches 100-120°C, the rubber material is discharged and the sheet is removed. After being left to cool, the transition layer rubber composition is obtained.

[0018] Furthermore, the present invention also discloses an all-steel load-bearing tire, the transition layer of which is prepared by vulcanizing the tire transition layer rubber composition with high air retention and high heat conductivity.

[0019] The present invention adopts the above-mentioned technical solution, and uses lamellar silicate inorganic filler to replace most of the carbon black, especially RC-15, which is a nano-scale natural mineral filler, and its structure is mainly lamellar silicate, which can form a space barrier effect in the free volume of rubber. The more fillers, the less corresponding rubber phase, the smaller the free volume, and the better the air retention performance of the formula. The stacking effect of inorganic fillers is used to improve the problem of the single function of the transition layer formula of the existing all-steel load-bearing radial tire, increase the barrier effect of the formula on gas, and improve the performance of the formula permeability coefficient; and RC-15 contains about 40% of aluminum oxide components, which has good thermal conductivity. After a large amount of use, it can significantly improve the thermal conductivity of the formula and the vulcanization efficiency of the tire. The present invention replaces most of the N326 carbon black in the formula with high-lamellar inorganic fillers, and the formula permeability coefficient is increased by about 20%, and the heat generation of the formula can be reduced while the thermal conductivity of the formula can be increased by more than 20%. DETAILED DESCRIPTION

[0020] The following is a clear and complete description of the technical solutions in the embodiments of the present invention in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0021] Source of raw materials: raw materials Product Description Natural Rubber (NR) Malaysia GZ-12 recycled rubber Ordinary reclaimed rubber, Shanxi Beihai Rubber Co., Ltd. RC-15 Inorganic fillers, China Baiya Trading (Hong Kong) Co., Ltd. N326 Carbon Black Commercially available Modified zinc oxide Surfactant, Jiaozuo Xingguang Additives Company SL1801 resin Para-octyl tackifying resin, Huaqi (Zhangjiagang) Co., Ltd. 4020 Antioxidant, Shandong Shengao Chemical Technology Co., Ltd. RD Antiaging agent, Shandong Shangshun Chemical Co., Ltd. SL3022B Meta-resin, Huaqi (Zhangjiagang) Co., Ltd. Nickel boroacylate Nickel salt, Yangzhou Baron Co., Ltd. OT20 Insoluble sulfur, Shandong Shangshun Chemical Co., Ltd. NS Accelerator, Kemai Chemical FA608 Adhesive, commercially available Example 1 The formula consists of the following materials in parts by weight: 100 parts of natural rubber, 16 parts of GZ-12 reclaimed rubber, 5 parts of N326 carbon black, 90 parts of RC-15, 6 parts of modified zinc oxide, 4 parts of tackifying resin (SL1801), 0.5 parts of antioxidant (4020), 1 part of antioxidant (RD), 0.8 parts of meta-acetic resin (SL3022B), 0.6 parts of nickel borate, 3.7 parts of 0T20 (insoluble sulfur), 1.1 parts of 10% oil-extended sulfur, 1.2 parts of accelerator (NS), and 4 parts of adhesive (FA608).

[0022] The mixing method comprises the following steps: 1) one-stage mixing: putting rubber, carbon black and inorganic filler RC-15 into an internal mixer and mixing for 30 to 50 seconds, mixing at a rotation speed of 45 to 60 rpm, lifting and pressing the lumps every 20 to 35 seconds, and when the temperature of the rubber material reaches 155°C to 170°C, the rubber material is discharged and flakes are dropped, and the masterbatch is obtained after being cooled at room temperature for 8 to 12 hours, and then the masterbatch is mixed in two stages; 2) Second stage mixing: the first stage masterbatch, inorganic filler RC-15, antioxidant and other rubber processing aids of step 1) are put into an internal mixer, mixed at a speed of 40-55 rpm, and the lump is lifted and pressed every 20-35 seconds. When the temperature of the rubber material reaches 145-160°C, the rubber is discharged and the sheets are dropped. After cooling at room temperature for 8-12 hours, the second stage masterbatch is obtained, and then final mixing is performed; 3) Final mixing: the second-stage masterbatch, vulcanizing agent and accelerator of step 2) are put into an internal mixer, mixed at a speed of 20-30 rpm, and the mixture is lifted and pressed at intervals of 20-30 seconds, 15-25 seconds and 10-20 seconds respectively. When the temperature of the rubber material reaches 100-120°C, the rubber material is discharged and the sheet is removed. After being left to cool, the transition layer rubber composition is obtained.

[0023] Example 2 The formula consists of the following materials in parts by weight: 100 parts of natural rubber, 16 parts of GZ-12 reclaimed rubber, 5 parts of N326 carbon black, 100 parts of RC-15, 6 parts of modified zinc oxide, 4 parts of tackifying resin (SL1801), 0.5 parts of antioxidant (4020), 1 part of antioxidant (RD), 0.8 parts of meta-acetic resin (SL3022B), 0.6 parts of nickel borate, 3.7 parts of 0T20 (insoluble sulfur), 1.1 parts of 10% oil-extended sulfur, 1.2 parts of accelerator (NS), and 4 parts of adhesive (FA608).

[0024] The mixing method is similar to that in Example 1.

[0025] Example 3 The formula consists of the following materials in parts by weight: 100 parts of natural rubber, 16 parts of GZ-12 reclaimed rubber, 5 parts of N326 carbon black, 110 parts of RC-15, 6 parts of modified zinc oxide, 4 parts of tackifying resin (SL1801), 0.5 parts of antioxidant (4020), 1 part of antioxidant (RD), 0.8 parts of meta-acetic resin (SL3022B), 0.6 parts of nickel borate, 3.7 parts of 0T20 (insoluble sulfur), 1.1 parts of 10% oil-extended sulfur, 1.2 parts of accelerator (NS), and 4 parts of adhesive (FA608).

[0026] The mixing method is similar to that in Example 1.

[0027] Example 4 The formula is composed of the following materials in parts by weight: 100 parts of natural rubber, 16 parts of GZ-12 reclaimed rubber, 10 parts of N326 carbon black, 72.5 parts of RC-15, 6 parts of modified zinc oxide, 4 parts of tackifying resin (SL1801), 0.5 parts of antioxidant (4020), 1 part of antioxidant (RD), 0.8 parts of meta-acetic resin (SL3022B), 0.6 parts of nickel borate, 3.7 parts of 0T20 (insoluble sulfur), 1.1 parts of 10% oil-extended sulfur, 1.2 parts of accelerator (NS), and 4 parts of adhesive (FA608).

[0028] The mixing method is similar to that in Example 1.

[0029] Example 5 The formula consists of the following materials in parts by weight: 100 parts of natural rubber, 16 parts of GZ-12 reclaimed rubber, 10 parts of N326 carbon black, 82.5 parts of RC-15, 6 parts of modified zinc oxide, 4 parts of tackifying resin (SL1801), 0.5 parts of antioxidant (4020), 1 part of antioxidant (RD), 0.8 parts of meta-acetic resin (SL3022B), 0.6 parts of nickel borate, 3.7 parts of 0T20 (insoluble sulfur), 1.1 parts of 10% oil-extended sulfur, 1.2 parts of accelerator (NS), and 4 parts of adhesive (FA608).

[0030] The mixing method is similar to that in Example 1.

[0031] Example 6 The formula consists of the following materials in parts by weight: 100 parts of natural rubber, 16 parts of GZ-12 reclaimed rubber, 10 parts of N326 carbon black, 92.5 parts of RC-15, 6 parts of modified zinc oxide, 4 parts of tackifying resin (SL1801), 0.5 parts of antioxidant (4020), 1 part of antioxidant (RD), 0.8 parts of meta-acetic resin (SL3022B), 0.6 parts of nickel borate, 3.7 parts of 0T20 (insoluble sulfur), 1.1 parts of 10% oil-extended sulfur, 1.2 parts of accelerator (NS), and 4 parts of adhesive (FA608).

[0032] The mixing method is similar to that in Example 1.

[0033] Example 7 The formula is composed of the following materials in parts by weight: 100 parts of natural rubber, 16 parts of GZ-12 reclaimed rubber, 120 parts of RC-15, 6 parts of modified zinc oxide, 4 parts of tackifying resin (SL1801), 0.5 parts of antioxidant (4020), 1 part of antioxidant (RD), 0.8 parts of meta-acetic resin (SL3022B), 0.6 parts of nickel borate, 3.7 parts of 0T20 (insoluble sulfur), 1.1 parts of 10% oil-extended sulfur, 1.2 parts of accelerator (NS), and 4 parts of adhesive (FA608).

[0034] The mixing method is similar to that in Example 1.

[0035] Comparative Example 1 The formula consists of the following materials in parts by weight: 100 parts of natural rubber, 16 parts of GZ-12 reclaimed rubber, 59.5 parts of N326 carbon black, 6 parts of modified zinc oxide, 4 parts of tackifying resin (SL1801), 0.5 parts of antioxidant (4020), 1 part of antioxidant (RD), 0.8 parts of meta-acetic resin (SL3022B), 0.6 parts of nickel borate, 3.7 parts of 0T20 (insoluble sulfur), 1.1 parts of 10% oil-extended sulfur, 1.2 parts of accelerator (NS), and 4 parts of adhesive (FA608).

[0036] The mixing method is similar to that in Example 1.

[0037] Comparative Example 2 The formula is composed of the following materials in parts by weight: 100 parts of natural rubber, 16 parts of GZ-12 reclaimed rubber, 44.5 parts of N326 carbon black, 15 parts of RC-15, 6 parts of modified zinc oxide, 4 parts of tackifying resin (SL1801), 0.5 parts of antioxidant (4020), 1 part of antioxidant (RD), 0.8 parts of meta-acetic resin (SL3022B), 0.6 parts of nickel borate, 3.7 parts of 0T20 (insoluble sulfur), 1.1 parts of 10% oil-extended sulfur, 1.2 parts of accelerator (NS), and 4 parts of adhesive (FA608).

[0038] The mixing method is similar to that in Example 1.

[0039] Comparative Example 3 The formula consists of the following materials in parts by weight: 100 parts of natural rubber, 16 parts of GZ-12 reclaimed rubber, 20 parts of N326 carbon black, 60 parts of RC-15, 6 parts of modified zinc oxide, 4 parts of tackifying resin (SL1801), 0.5 parts of antioxidant (4020), 1 part of antioxidant (RD), 0.8 parts of meta-acetic resin (SL3022B), 0.6 parts of nickel borate, 3.7 parts of 0T20 (insoluble sulfur), 1.1 parts of 10% oil-extended sulfur, 1.2 parts of accelerator (NS), and 4 parts of adhesive (FA608).

[0040] The mixing method is similar to that in Example 1.

[0041] According to national standards, physical property tests were performed on Examples 1-6 and Comparative Examples, respectively. Specific physical properties are shown in Table 1 below.

[0042] The Shore A hardness is measured according to GB / T 531.1-2008, the 100% elongation, 200% elongation, 300% elongation, tensile strength, elongation at break, and tensile permanent deformation are measured according to GB / T 528-2009, the air tightness is measured according to GB / T 1038-2000, and the thermal conductivity is measured according to ISO22007-2. The DMA dynamic performance test conditions are: frequency 20HZ, strain 7±2%, and temperature scanning 60°C. Table 1 Physical performance test results of Examples 1-7 and Comparative Examples 1-3: project Comparative Example 1 Comparative Example 2 Comparative Example 3 Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Example 7 Natural rubber 100 100 100 100 100 100 100 100 100 100 Recycled Rubber 16 16 16 16 16 16 16 16 16 16 N326 59.5 44.5 20 5 5 5 10 10 10 - RC-15 - 15 60 90 100 110 72.5 82.5 92.5 120 Modified zinc oxide 6 6 6 6 6 6 6 6 6 6 Tackifying resin 4 4 4 4 4 4 4 4 4 4 4020 0.5 0.5 0.5 0.5 0.5 0.5 0.5 0.5 0.5 0.5 RD 1 1 1 1 1 1 1 1 1 1 Meta-nail resin 0.8 0.8 0.8 0.8 0.8 0.8 0.8 0.8 0.8 0.8 Nickel boroacylate 0.6 0.6 0.6 0.6 0.6 0.6 0.6 0.6 0.6 0.6 0T20 3.7 3.7 3.7 3.7 3.7 3.7 3.7 3.7 3.7 3.7 Oil-filled sulfur 1.1 1.1 1.1 1.1 1.1 1.1 1.1 1.1 1.1 1.1 NS 1.2 1.2 1.2 1.2 1.2 1.2 1.2 1.2 1.2 1.2 Adhesives 4 4 4 4 4 4 4 4 4 4 Test data is shown in Table 2 Through Examples 1-3 and Comparative Examples 1-3, it can be concluded that the inorganic filler RC-15 replaces carbon black in the transition layer, and the air permeability and thermal conductivity of the transition layer formula are significantly improved, and the formula modulus is also significantly improved. Example 2 M300 is improved by 21%, the air permeability is improved by more than 15%, the thermal conductivity is improved by 20%, and the loss factor at 60°C is significantly reduced. The performance meets the requirements for the use of transition layer rubber of all-steel radial tires, and can be used as a high air retention, high thermal conductivity, and low heat generation transition layer in all-steel radial tires.

[0043] Through Examples 4-7 and Comparative Examples 1-3, it can be concluded that after using 82.5 parts of RC-15 to replace 35 parts of N326 carbon black, the modulus, air permeability and thermal conductivity of the formulation of Example 4 are significantly improved, and the performance meets the requirements for the use of airtight layer rubber of all-steel radial tires, and can be used as a high modulus, high air retention, and high thermal conductivity transition layer in the transition layer formulation of all-steel radial tires.

[0044] The above is a description of the embodiments of the present invention. Through the above description of the disclosed embodiments, professionals and technicians in the field can implement or use the present invention. Various modifications to these embodiments will be apparent to professionals and technicians in the field. The general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to these embodiments shown in this article, but will conform to the widest range consistent with the principles and novelties disclosed herein.

Claims

1. A tire transition layer rubber composition with high air retention and high thermal conductivity, characterized in that: The rubber composition is prepared by mixing the following raw materials by mass fraction: Natural rubber: 100 parts Recycled rubber: 5-30 copies Lamellar silicate filler: 70-110 parts Carbon black: 0-15 parts Tackifying resin: 1-8 parts Meta-acetic resin: 0.3-1.2 parts Nickel salt: 0.3-1.2 parts; The D50 particle size of the lamellar silicate filler is below 1 micron, and the main components are 30-45% aluminum oxide and 35-50% silicon dioxide.

2. A tire transition layer rubber composition with high air retention and high thermal conductivity according to claim 1, characterized in that: The rubber composition is prepared by mixing the following raw materials by mass fraction: Natural rubber: 100 parts Recycled rubber: 10-20 copies Lamellar silicate filler: 80-95 parts Carbon black: 5-10 parts Tackifying resin: 3-6 parts Meta-acetic resin: 0.5-1.0 parts Nickel salt: 0.5-1.0 part.

3. A tire transition layer rubber composition with high air retention and high thermal conductivity according to claim 1 or 2, characterized in that: The lamellar silicate filler is RC-15 lamellar silicate inorganic filler provided by China Baiya Trading (Hong Kong) Co., Ltd., and its composition includes 38% aluminum oxide and 42% silicon dioxide.

4. A tire transition layer rubber composition with high air retention and high thermal conductivity according to claim 1 or 2, characterized in that: The rubber composition further comprises an activator, an adhesive, an antioxidant, an accelerator and sulfur; preferably, the activator: 1-8 parts, preferably 3-6 parts; Binder: 2-6 parts, preferably 3-5 parts; Antiaging agent: 0-3 parts, preferably 0.5-2 parts; Accelerator: 0.5-2 parts, preferably 1-1.5 parts; Sulfur: 1-8 parts, preferably 3-6 parts.

5. A tire transition layer rubber composition with high air retention and high thermal conductivity according to claim 4, characterized in that: The antioxidants used are 0.3-0.8 parts of antioxidant 4020 and 0.8-1.5 parts of antioxidant RD; the sulfur used is 3.0-4.5 parts of insoluble sulfur and 0.8-1.5 parts of 10% oil-extended sulfur.

6. A tire transition layer rubber composition with high air retention and high thermal conductivity according to claim 1 or 2, characterized in that: The reclaimed rubber used is GZ-12 reclaimed rubber and GZ-16 reclaimed rubber produced by Shanxi Beihai Rubber Co., Ltd., and GZ-12 reclaimed rubber is preferred.

7. A tire transition layer rubber composition with high air retention and high thermal conductivity according to claim 1 or 2, characterized in that: The carbon black is selected from one or more of N326, N330, N375, N550, N660 and N774, and preferably the carbon black is N326 or N375.

8. A tire transition layer rubber composition with high air retention and high thermal conductivity according to claim 1 or 2, characterized in that: The nickel salt is nickel borate; And / or, the tackifying resin is one or more of p-tert-butyl tackifying resin, p-tert-octyl tackifying resin, acetyl tackifying resin and ethylene tackifying resin, preferably p-tert-octyl tackifying resin; And / or, the active agent is one or more of zinc oxide and stearic acid.

9. A mixing method for a tire transition layer rubber composition with high air retention and high thermal conductivity according to any one of claims 1 to 8, characterized in that: The method comprises the following steps: 1) First-stage mixing: Rubber, carbon black and inorganic filler RC-15 are put into an internal mixer and mixed for 30 to 50 seconds at a speed of 45 to 60 rpm. The mixture is lifted and pressed every 20 to 35 seconds. When the temperature of the rubber reaches 155 to 170 °C, the rubber is discharged and the pieces are dropped. After cooling at room temperature for 8 to 12 hours, a first-stage masterbatch is obtained, which is then subjected to second-stage mixing. 2) Second stage mixing: the first stage masterbatch, inorganic filler RC-15, antioxidant and other rubber processing aids of step 1) are put into an internal mixer, mixed at a speed of 40-55 rpm, and the lump is lifted and pressed every 20-35 seconds. When the temperature of the rubber material reaches 145-160°C, the rubber is discharged and the sheets are dropped. After cooling at room temperature for 8-12 hours, the second stage masterbatch is obtained, and then final mixing is performed; 3) Final mixing: the second-stage masterbatch, vulcanizing agent and accelerator of step 2) are put into an internal mixer, mixed at a speed of 20-30 rpm, and the mixture is lifted and pressed at intervals of 20-30 seconds, 15-25 seconds and 10-20 seconds respectively. When the temperature of the rubber material reaches 100-120°C, the rubber material is discharged and the sheet is removed. After being left to cool, the transition layer rubber composition is obtained.

10. An all-steel load-carrying tire, characterized in that: The transition layer of the tire is prepared by vulcanizing the tire transition layer rubber composition with high air retention and high thermal conductivity as described in any one of claims 1 to 8.

Citation Information

Patent Citations

  • Tire transition layer stock and preparation method thereof

    CN103834071A

  • Material and method used for producing all steel truck radical tire inner liner

    CN104761769A

  • Environment-friendly all-steel transition layer rubber and preparation method thereof

    CN113528055A

  • Rubber composition for inner liner, method of producing the rubber composition, and pneumatic tire

    JP2012233093A

  • Innerliner rubber composition for aircraft