Polarized electro-synaptic device prepared based on micro-channel confinement method and preparation method of polarized electro-synaptic device
The preparation of polarized photoelectric synaptic devices through the microchannel domain method solves the problem of incompatibility of perovskite materials and photolithography processes, realizes the orderly growth and polarization characteristics of perovskite materials, and improves the dimension and ability of object recognition The richness of observational information.
Patent Information
- Application Number
- CN202411126148.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-26
AI Technical Summary
The existing perovskite synaptic devices are not compatible with the lithography process, resulting in a large electrode area and can only capture two-dimensional imaging information, which cannot recognize multi-dimensional information of objects.
The polarized photoelectric synaptic device was prepared by microchannel domain method, by covering the microchannels on the substrate, and applying the PEA2SnI4 solution droplets on it, filling the microchannels with capillary force, and then Annealing is carried out to form a highly consistent perovskite microwire layer to achieve the orderly growth and polarization characteristics of perovskite materials.
The orderly growth and polarization characteristics of perovskite materials are achieved, the problem of incompatibility with the lithography process is avoided, electrodes of any shape and size are obtained, and the dimensions of object recognition and the richness of observable information are improved.
Smart Images

Figure CN119031730A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of semiconductor technology, and in particular relates to a polarized photoelectric synapse device prepared based on a microchannel confinement method and a preparation method thereof. Background Art
[0002] With the rapid development of science and technology and the explosive growth of information data, traditional computing systems based on the von Neumann architecture can no longer meet the growing data demand. The separation between its central processing unit and memory increases the information transmission time, which inevitably leads to additional power consumption. Inspired by the human brain system, brain-like neuromorphic computing shows great advantages in high-speed computing and ultra-low power consumption in perception, learning, memory, etc., and is expected to become one of the important solutions to the above problems. From the external stimuli captured by the senses to the inside of the brain, it is necessary to pass through a series of closely connected synaptic neurons. In order to fully simulate this complex function of the brain, it is urgent to develop an artificial synaptic device that integrates sensing and processing functions.
[0003] In recent years, perovskite has become an ideal material choice for simulating the functions of synaptic neurons due to its remarkable properties such as low toxicity, long carrier diffusion lifetime and high light absorption coefficient.
[0004] Although perovskite-based synaptic devices have made significant progress in the field of imaging, most existing studies are limited to the use of light intensity information, and fail to fully obtain multi-dimensional information such as object shape, material, and surface roughness. In order to overcome this limitation, optoelectronic synaptic devices with polarization performance have emerged. Such devices can elevate the information captured by traditional imaging systems to a higher dimension, greatly enriching the types and quantity of observable information, thereby improving the recognition accuracy of neuromorphic systems for detection targets, thereby enabling visual sensing and image recognition functions in complex environments.
[0005] Synaptic devices based on perovskite materials are sensitive to organic solvents and are not compatible with photolithography processes, so the electrode area is usually at the sub-millimeter level; research based on synaptic devices is mostly limited to the use of light intensity information, and fails to fully obtain multi-dimensional information such as object shape, material and surface roughness.
[0006] Technical issues to be solved:
[0007] 1. At present, since perovskite materials are still not compatible with photolithography processes, most devices can only be prepared using traditional masks to obtain a larger electrode area.
[0008] 2. Synaptic devices can only capture traditional two-dimensional imaging information and cannot recognize multi-dimensional information of objects. Summary of the invention
[0009] In view of this, the present invention provides a polarized photoelectric synapse device and a preparation method based on the microchannel confinement method, which can capture imaging information in more dimensions and achieve more efficient and intelligent information processing and data analysis.
[0010] The technical solution for implementing the present invention is as follows:
[0011] A polarized photoelectric synaptic device prepared based on a microchannel confinement method comprises: a substrate, an electrode layer formed on the substrate, and micrometer wires, wherein the electrode layer comprises two bases and two interdigital units, wherein the two bases are arranged opposite to each other, the two interdigital units are respectively connected to the two bases, and the interdigital fingers on the two interdigital units extend toward each other and are insulated from each other, and the two interdigital units are an asymmetric structure with different interdigital widths; the micrometer wire layer is a perovskite material, prepared based on the microchannel confinement method, and covers multiple interdigital fingers of the two interdigital units.
[0012] Furthermore, the material of the micron-wire layer of the present invention is a two-dimensional PEA2SnI4 perovskite material.
[0013] Furthermore, the preparation based on the microchannel confinement method described in the present invention is as follows: a layer of polydimethylsiloxane (PDMS) with microchannels is covered on the substrate, a PEA2SnI4 solution is drop-coated on one end of the PDMS substrate, and after the PEA2SnI4 solution fills the entire microchannel area under the action of capillary force, it is heated on an annealing table, and then the top PDMS is peeled off and annealed again.
[0014] Furthermore, the microchannel confinement method of the present invention is prepared as follows:
[0015] First, a PEA2SnI4 solution was prepared by mixing 0.14945 g of phenylethylamine iodine powder and 0.11175 g of tin iodide powder and dissolving them in a mixed solution of dimethyl sulfoxide and dimethylformamide with a mixing ratio of 1:4 and a mixing volume of 1 ml; stirring for 12 hours at room temperature to form a PEA2SnI4 solution; and placing the prepared PEA2SnI4 solution in a glove box protected by argon gas;
[0016] Secondly, a layer of polydimethylsiloxane (PDMS) with microchannels was covered on the substrate and then transferred to a glove box;
[0017] Again, the PEA2SnI4 solution was drop-coated on one end of the PDMS substrate and allowed to stand for ten minutes. The solution gradually filled the entire microchannel area under the action of capillary force.
[0018] Finally, the substrate filled with PEA2SnI4 solution was placed on an annealing table at 80 degrees Celsius for ten minutes, and then the top PDMS was peeled off and annealed again for 20 minutes.
[0019] Furthermore, the substrate of the present invention can be made of Si / SiO2 or flexible PET, and the material of the interdigital units can be gold.
[0020] Furthermore, in the present invention, the width of the interdigital fingers on the first interdigital unit is 10 micrometers, the width of the interdigital fingers on the second interdigital unit is 200 micrometers, and the distance between two adjacent interdigital fingers extending toward each other is 10 micrometers.
[0021] A method for preparing a polarized photoelectric synapse device based on a microchannel confinement method, the method comprising the following steps:
[0022] S1: Select a substrate and clean it;
[0023] S2: using photolithography technology, preparing an asymmetric electrode layer on a substrate, the electrode layer comprising two bases and two interdigital units, the two bases are arranged opposite to each other, the two interdigital units are respectively connected to the two bases, and the interdigits on the two interdigital units extend towards each other and are insulated from each other, and the interdigits on the two interdigital units have different widths;
[0024] S3: Cover the substrate with a layer of polydimethylsiloxane (PDMS) with microchannels, and drop the PEA2SnI4 solution on one end of the PDMS substrate. After the PEA2SnI4 solution fills the entire microchannel area under the action of capillary force, heat it on an annealing table, then peel off the top PDMS, and anneal it again to prepare the synaptic device.
[0025] Furthermore, the substrate of the present invention can be a Si / SiO2 or PET substrate, and the substrate can be cut into a size of 1 cm×1 cm.
[0026] Furthermore, the cleaning process of the present invention is as follows: placing the prepared substrate in acetone, ethanol and deionized water for ultrasonic cleaning for 10 minutes respectively, and then blowing it dry with high-purity nitrogen for standby use to complete the first cleaning treatment to achieve the effect of removing debris and oil stains; and placing the above-mentioned substrate in a glass culture dish and cleaning it with a plasma machine for 10 minutes to complete the second cleaning treatment, making the substrate surface more hydrophilic and helping the solution to spread to form a film, wherein the gas used for cleaning can be oxygen.
[0027] Furthermore, the specific process of step S3 of the present invention is as follows:
[0028] First, a PEA2SnI4 solution was prepared by mixing 0.14945 g of phenylethylamine iodine powder and 0.11175 g of tin iodide powder and dissolving them in a mixed solution of dimethyl sulfoxide and dimethylformamide with a mixing ratio of 1:4 and a mixing volume of 1 ml; stirring for 12 hours at room temperature to form a PEA2SnI4 solution; and placing the prepared PEA2SnI4 solution in a glove box protected by argon gas;
[0029] Secondly, a layer of polydimethylsiloxane (PDMS) with microchannels was covered on the substrate and then transferred to a glove box;
[0030] Again, the PEA2SnI4 solution was drop-coated on one end of the PDMS substrate and allowed to stand for ten minutes. The solution gradually filled the entire microchannel area under the action of capillary force.
[0031] Finally, the substrate filled with PEA2SnI4 solution was placed on an annealing table at 80 degrees Celsius for ten minutes, and then the top PDMS was peeled off and annealed again for 20 minutes.
[0032] Beneficial effects:
[0033] First, the present invention utilizes microchannel confinement to restrict the growth of perovskite materials along the direction of the micron-wire template. This restricted growth mode causes the perovskite crystals to be arranged in an orderly manner along the axis of the micron-wire, forming a highly consistent and continuous single crystal, which exhibits linearly polarized optical properties on a macro scale.
[0034] Second, the micrometer wires of the present invention are prepared by the microchannel confinement method. By directly preparing the photolithography electrodes on the substrate and then transferring the micrometer wires, the incompatibility problem between the perovskite material and the photolithography process is cleverly avoided, and horizontal photolithography electrodes of any shape and size can be obtained.
[0035] Third, the synaptic device prepared by the method of the present invention can well improve the anisotropy of the material. At different polarization angles, the device photocurrent response has obvious differences, which elevates the device's recognition of objects to a higher dimension and enriches observable information. This description constructs a synaptic device with polarization performance, which is expected to achieve the simulation of human brain neurons in complex environments, including the judgment of motion trajectories in complex environments. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0037] Figure 1 is a simplified top view of a synaptic device according to an exemplary embodiment of the present disclosure;
[0038] Figure 2 yes Figure 1 The partial photograph of the micrometer wire shown is scanned under an electron microscope;
[0039] Figure 3(a) is Figure 1FIG3( b ) is a polar coordinate diagram of the anisotropic absorption value of the micron-wire at different polarization angles when the wavelength is 647 nanometers; FIG3( b ) is a polar coordinate diagram of the anisotropic absorption value of the micron-wire at different polarization angles;
[0040] Figure 4 yes Figure 1 Schematic diagram of testing the synaptic device under different polarized light angles;
[0041] Figure 5(a) is Figure 1 The postsynaptic current curves of the synaptic device shown in FIG5( b ) are the corresponding polar coordinate diagrams of the anisotropic postsynaptic current under different polarization angles;
[0042] Figure 6 yes Figure 1 The postsynaptic current curves of the synaptic device shown are after multi-pulse stimulation at polarization angles of 0 and 90 degrees. DETAILED DESCRIPTION
[0043] The embodiments of the present invention are described in detail below with reference to the accompanying drawings.
[0044] It should be noted that the following embodiments and features in the embodiments may be combined with each other in the absence of conflict; and, based on the embodiments in the present disclosure, all other embodiments obtained by ordinary technicians in the field without making any creative work are within the scope of protection of the present disclosure.
[0045] It should be noted that various aspects of the embodiments within the scope of the appended claims are described below. It should be apparent that the aspects described herein may be embodied in a wide variety of forms, and any specific structure and / or function described herein is merely illustrative. Based on the present disclosure, it should be understood by those skilled in the art that an aspect described herein may be implemented independently of any other aspect, and two or more of these aspects may be combined in various ways. For example, any number of aspects described herein may be used to implement the device and / or practice the method. In addition, other structures and / or functionalities other than one or more of the aspects described herein may be used to implement this device and / or practice this method.
[0046] like Figure 1As shown, an embodiment of the present application is a polarized photoelectric synapse device prepared based on a microchannel confinement method, the synapse device comprising: a substrate 1, an electrode layer 2 formed on the substrate 1, and a micron wire 3, the electrode layer 2 comprising two bases and two finger units, the two bases being arranged opposite to each other, the two finger units being connected to the two bases respectively, and the fingers on the two finger units extending toward each other and insulated from each other, the two finger units being an asymmetric structure with different finger widths; the micron wire layer 3 is a perovskite material, prepared based on the microchannel confinement method, and covering multiple fingers of the two finger units.
[0047] In this embodiment, when the light beam to be measured irradiates the synaptic device, the micron wire layer generates electron-hole pairs. Under the action of the external electric field, the carriers drift, and the micron wire layer 3 is a defect state in the perovskite material that captures part of the photogenerated electrons, showing synaptic characteristics. As the illumination time increases and the light power increases, the device shows a transition from short-term plasticity to long-term plasticity. And based on the structural anisotropy of the perovskite material, by changing the direction of the linearly polarized light, the corresponding post-synaptic current value will also change accordingly, and the synaptic device shows good polarization-sensitive detection capabilities.
[0048] In this embodiment, the micron wires prepared based on the microchannel confinement method have a specific orientation and show significant linear polarization characteristics from a macroscopic perspective, indicating that the polarization synaptic device can realize object recognition in complex environments. In addition, the polarization synaptic device can not only simulate the synaptic behavior of neurons, such as excitation and inhibition, but also realize multi-state processing of signals by adjusting the polarization state, providing new possibilities for neuromorphic computing and brain-like computing.
[0049] In this embodiment, which is another embodiment of the present application, the material of the micron wire layer 3 is a two-dimensional PEA2SnI4 perovskite material, and the micron wires are obtained by crystallization through a microchannel confinement method. This preparation process is relatively simple and does not require a vacuum, high pressure or other environment. The microchannel template can be recycled, which can further reduce production costs. Figure 2 yes Figure 1 The following is a partial photo of the micrometer wire scanned under an electron microscope. Figure 2 As shown, the PEA2SnI4 microwires have high crystalline quality and can form uniform and regular microwires along the microchannel region, which is beneficial to carrier transport.
[0050] like Figure 1As shown, in another embodiment of the present application, the substrate 1 can be made of Si / SiO2 or flexible PET, and the material of the interdigital unit is gold, and the transfer and transmission of photogenerated carriers are regulated by constructing an asymmetric electrode. In detail, the electrode layer 2 includes two bases and two interdigital units, which are marked as the first base 211, the second base 212, the first interdigital unit 221 and the second interdigital unit 222. The first base 211 and the second base 212 are arranged opposite to each other, the first base 211 is integrally connected to the first interdigital unit 221, and the second base 212 is integrally connected to the second interdigital unit 222. The interdigits of the first interdigital unit 221 and the second interdigital unit 222 extend toward each other but do not extend to the bases arranged opposite to each other, and the interdigits of the first interdigital unit 221 and the second interdigital unit 222 are isolated from each other, that is, the interdigits belonging to different interdigital units are in an insulating state. In this embodiment, the PEA2SnI4 micron wire layer 3 covers multiple fingers of multiple finger units. After covering the fingers of the first finger unit 221 and the second finger unit 222, the first finger unit 221 and the second finger unit 222 that are isolated from each other are connected by micron wires, and the synaptic device forms a pattern of electrode layer 2-micron wire layer 3-electrode layer 2 (MSM).
[0051] like Figure 1 As shown, in another embodiment of the present application, the width of the fingers on the first finger unit is b1, the width of the fingers on the second finger unit is b2, and the spacing between two adjacent fingers extending toward each other is 10 microns, wherein b2:b1=20:1. In this embodiment, the width of b1 is 10 microns, and the width of b2 is 200 microns. The asymmetric finger electrodes result in differences in the contact potential barriers between the two ends of the electrode and the material. The existence of this difference can store partial charges, improve the long-term memory of the synaptic device, and facilitate the reverse erasure of the voltage. In this embodiment, the microwire is prepared by the microchannel confinement method, with a width of 5 microns and a length of up to 1.5 centimeters.
[0052] The present application embodiment provides a method for preparing a polarized photoelectric synapse device based on a microchannel confinement method, the method comprising the following steps:
[0053] S1: Select a substrate and clean it;
[0054] S2: using photolithography technology, preparing a photolithographic asymmetric electrode layer 2 on the substrate, the electrode layer 2 comprising two bases and two interdigital units, the two bases are arranged opposite to each other, the two interdigital units are respectively connected to the two bases, and the interdigits on the two interdigital units extend towards each other and are insulated from each other, and the two interdigital units are an asymmetric structure with different interdigital widths;
[0055] S3: Cover substrate 1 with a layer of polydimethylsiloxane (PDMS) with microchannels, and drop PEA2SnI4 solution on one end of the PDMS substrate. After the PEA2SnI4 solution fills the entire microchannel area under the action of capillary force, heat it on an annealing table, then peel off the top PDMS, and anneal it again for 20 minutes to prepare the synaptic device.
[0056] In the specific implementation of step S1 of this embodiment, the substrate may be a Si / SiO2 or PET substrate, and the substrate 1 is cut into a size of 1 cm×1 cm.
[0057] In the specific implementation of step S1 of this embodiment, the cleaning process is as follows: the prepared substrate 1 is sequentially placed in acetone, ethanol and deionized water for ultrasonic cleaning for 10 minutes each, and then blown dry with high-purity nitrogen for standby use to complete the first cleaning treatment to achieve the effect of removing debris and oil stains; and the above-mentioned substrate 1 is placed in a glass culture dish and cleaned with a plasma machine for 10 minutes to complete the second cleaning treatment, so that the surface of the substrate 1 is more hydrophilic, which is helpful for the solution to spread and form a film, wherein the gas used for cleaning can be oxygen.
[0058] In the specific implementation of step S2 of this embodiment, on the substrate 1 after the first cleaning process and the second cleaning process, based on the photolithography technology, the asymmetric electrode layer 2 is photoetched, and the thickness of the electrode layer is 50 nanometers. Figure 1 As shown, the process of preparing the electrode layer 2 includes photolithography of the first base 211 and the interdigital unit 221, the second base 212 and the interdigital unit 222, multiple interdigits of the two interdigital units extend toward each other and are insulated from each other, and the photolithography spacing between the interdigits is 10 microns.
[0059] The electrode layer 2 prepared by the above method has excellent conductivity, and because the electrode preparation precedes the growth of the microwires 3, the patterned electrode can be designed and the electrode size can be adjusted arbitrarily, thereby realizing large-area batch array electrode preparation.
[0060] When step S3 of this embodiment is implemented, the specific process is as follows:
[0061] First, a PEA2SnI4 solution was prepared by mixing 0.14945 g of phenylethylamine iodine powder and 0.11175 g of tin iodide powder and dissolving them in a mixed solution of dimethyl sulfoxide and dimethylformamide with a mixing ratio of 1:4 and a mixing volume of 1 ml; stirring was performed at room temperature for 12 hours to form a PEA2SnI4 solution; and the prepared PEA2SnI4 solution was placed in a glove box protected by argon gas.
[0062] Next, a layer of polydimethylsiloxane (PDMS) having microchannels is covered on the substrate 1 and then transferred to a glove box.
[0063] Again, the PEA2SnI4 solution was drop-coated on one end of the PDMS substrate and allowed to stand for ten minutes. The solution gradually filled the entire microchannel area under the action of capillary force.
[0064] Finally, the substrate filled with PEA2SnI4 solution was placed on an annealing table at 80 degrees Celsius for ten minutes, and then the top PDMS was peeled off and annealed again for 20 minutes.
[0065] The synaptic device prepared by the above method connects the insulated electrode layers 2 through the micron wire layer 3, so that the synaptic device has excellent polarization performance. When the light wavelength is 520 nanometers and the light power is 0.1 milliwatts per square centimeter, the photoelectric response of polarization angle resolution is studied, and the ratio of the maximum and minimum photocurrents (dichroic ratio) reaches 1.38, indicating that the synaptic device has good polarization-sensitive detection capabilities. Therefore, its characteristics can be further used to improve the recognition of objects and enrich observable information.
[0066] The micron wire layer 3 prepared by the above method has high crystal quality. Figure 2 As shown, it can be observed that after annealing, the microwire layer 3 has a smooth surface, low roughness, and is evenly and regularly arranged. The width of the microwire is 5 microns and the maximum length can reach 1.5 cm. This preparation process is relatively simple, does not require vacuum and high pressure environments, and the microchannel template can be recycled, which can further reduce production costs.
[0067] Figure 3(a) is Figure 1 FIG3( b ) is a polar coordinate diagram of the anisotropic absorption value of the micrometer wire at different polarization angles when the wavelength is 647 nanometers. In some embodiments, as shown in FIG3 , the absorption peak spectral curves of the micrometer wire at polarization angles of 0 and 180 degrees overlap within the tested wavelength range of 600 to 700 nanometers. Within this range, as the polarization angle changes, the peak intensity also changes accordingly. A polar coordinate diagram is drawn of the anisotropic absorption value of the micrometer wire at different polarization angles when the wavelength is 647 nanometers. A spindle-shaped polarization distribution can be intuitively seen, in which the maximum absorption peak appears at the polarization directions of 0 and 180 degrees.
[0068] Figure 4 yes Figure 1 The schematic diagram of the test of the synaptic device at different polarization angles is shown. The 520nm laser first passes through the linear polarizer to become linearly polarized light, then passes through the half-wave plate to generate a π phase difference, and finally irradiates the device surface. By adjusting the rotation angle of the half-wave plate, linearly polarized light at different polarization angles can be obtained.
[0069] Figure 5(a) is Figure 1The postsynaptic current curves of the synaptic device under different polarization angles are shown, and FIG5(b) is the corresponding polar coordinate diagram of the anisotropic postsynaptic current under different polarization angles. In some embodiments, as shown in FIG5(a), five identical illumination cycles are applied to the device, and the polarization angle is adjusted from 0 to 360 degrees, and the postsynaptic current of the device is recorded. The peak current of the fifth pulse is counted, and a polar coordinate diagram is drawn as shown in FIG5(b). When the illumination wavelength is 520 nanometers and the optical power is 0.1 milliwatts per square centimeter, the polarization-resolved photoelectric response is studied, and the ratio of the maximum and minimum photocurrents (dichroic ratio) reaches 1.38, indicating that the synaptic device has good polarization-sensitive detection capabilities.
[0070] Figure 6 yes Figure 1 The device shown shows the postsynaptic current curves of multiple pulse stimulation at 0 and 90 degree polarization angles (illumination conditions are 520 nm, optical power is 0.49 mW / cm2, and applied voltage is 0.1 V). After 30 pulses of illumination, the postsynaptic current at 0 and 90 degree polarization angles produced a difference of about 0.5 microamperes.
[0071] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the protection scope of the claims.
Claims
1. A polarized photoelectric synaptic device prepared based on a microchannel confinement method, characterized in that: include: A substrate, an electrode layer formed on the substrate, and a micrometer wire, wherein the electrode layer includes two bases and two interdigital units, wherein the two bases are arranged opposite to each other, the two interdigital units are respectively connected to the two bases, and the interdigital fingers on the two interdigital units extend toward each other and are insulated from each other, and the two interdigital units are an asymmetric structure with different interdigital widths; the micrometer wire layer is a perovskite material, prepared based on a microchannel confinement method, and covers multiple interdigital fingers of the two interdigital units.
2. According to claim 1, the polarized photoelectric synaptic device prepared based on the microchannel confinement method is characterized in that: The material of the micron line layer is a two-dimensional PEA2SnI4 perovskite material.
3. The polarized photoelectric synaptic device prepared based on the microchannel confinement method according to claim 2, characterized in that: The preparation based on the microchannel confinement method is as follows: a layer of polydimethylsiloxane (PDMS) with microchannels is covered on the substrate, a PEA2SnI4 solution is drop-coated on one end of the PDMS substrate, and after the PEA2SnI4 solution fills the entire microchannel area under the action of capillary force, it is heated on an annealing table, and then the top PDMS is peeled off and annealed again.
4. The polarized photoelectric synaptic device prepared based on the microchannel confinement method according to claim 3, characterized in that: The preparation based on the microchannel confinement method is as follows: First, a PEA2SnI4 solution was prepared by mixing 0.14945 g of phenylethylamine iodine powder and 0.11175 g of tin iodide powder and dissolving them in a mixed solution of dimethyl sulfoxide and dimethylformamide with a mixing ratio of 1:4 and a mixing volume of 1 ml; stirring for 12 hours at room temperature to form a PEA2SnI4 solution; and placing the prepared PEA2SnI4 solution in a glove box protected by argon gas; Secondly, a layer of polydimethylsiloxane (PDMS) with microchannels was covered on the substrate and then transferred to a glove box; Again, the PEA2SnI4 solution was drop-coated on one end of the PDMS substrate and allowed to stand for ten minutes. The solution gradually filled the entire microchannel area under the action of capillary force. Finally, the substrate filled with PEA2SnI4 solution was placed on an annealing table at 80 degrees Celsius for ten minutes, and then the top PDMS was peeled off and annealed again for 20 minutes.
5. The polarized photoelectric synaptic device prepared based on the microchannel confinement method according to claim 1, characterized in that: The substrate is made of Si / SiO2 or flexible PET, and the material of the interdigital units is gold.
6. The polarized photoelectric synaptic device prepared based on the microchannel confinement method according to claim 1, characterized in that: The width of the fingers on the first interdigital unit is 10 micrometers, the width of the fingers on the second interdigital unit is 200 micrometers, and the distance between two adjacent interdigits extending toward each other is 10 micrometers.
7. A method for preparing a polarized photoelectric synaptic device based on a microchannel confinement method, characterized in that: The method comprises the following steps: S1: Select a substrate and clean it; S2: using photolithography technology, preparing an asymmetric electrode layer on a substrate, the electrode layer comprising two bases and two interdigital units, the two bases are arranged opposite to each other, the two interdigital units are respectively connected to the two bases, and the interdigits on the two interdigital units extend toward each other and are insulated from each other, and the two interdigital units are an asymmetric structure with different interdigital widths; S3: Cover the substrate with a layer of polydimethylsiloxane (PDMS) with microchannels, and drop the PEA2SnI4 solution on one end of the PDMS substrate. After the PEA2SnI4 solution fills the entire microchannel area under the action of capillary force, heat it on an annealing table, then peel off the top PDMS, and anneal it again to prepare the synaptic device.
8. The method for preparing a polarized photoelectric synapse device based on a microchannel confinement method according to claim 7, characterized in that: The substrate may be a Si / SiO2 or PET substrate, and the substrate is cut into a size of 1 cm×1 cm.
9. The method for preparing a polarized photoelectric synapse device based on a microchannel confinement method according to claim 7, characterized in that: The cleaning process is as follows: placing the prepared substrate in acetone, ethanol and deionized water for ultrasonic cleaning for 10 minutes respectively, and then drying it with high-purity nitrogen gas for standby use to complete the first cleaning process to achieve the effect of removing debris and oil stains; and placing the above substrate in a glass culture dish and cleaning it with a plasma machine for 10 minutes to complete the second cleaning process to make the substrate surface more hydrophilic and help the solution spread to form a film, wherein the cleaning gas can be oxygen.
10. The method for preparing a polarized photoelectric synaptic device based on a microchannel confinement method according to claim 7, characterized in that: The specific process of step S3 is: First, a PEA2SnI4 solution was prepared by mixing 0.14945 g of phenylethylamine iodine powder and 0.11175 g of tin iodide powder and dissolving them in a mixed solution of dimethyl sulfoxide and dimethylformamide with a mixing ratio of 1:4 and a mixing volume of 1 ml; stirring for 12 hours at room temperature to form a PEA2SnI4 solution; and placing the prepared PEA2SnI4 solution in a glove box protected by argon gas; Secondly, a layer of polydimethylsiloxane (PDMS) with microchannels was covered on the substrate and then transferred to a glove box; Again, the PEA2SnI4 solution was drop-coated on one end of the PDMS substrate and allowed to stand for ten minutes. The solution gradually filled the entire microchannel area under the action of capillary force. Finally, the substrate filled with PEA2SnI4 solution was placed on an annealing table at 80 degrees Celsius for ten minutes, and then the top PDMS was peeled off and annealed again for 20 minutes.